Quantum dot infrared photodetector, preparation method and application thereof
By using a Fabry-Perot microcavity design with a dielectric-metal-dielectric stacked electrode structure, the problem of mutual constraint between light absorption efficiency and carrier extraction in short-wave infrared quantum dot photodetectors is solved, achieving a balance between high external quantum efficiency and microsecond-level response speed, which is suitable for silicon-based CMOS integration.
Patent Information
- Application Number
- CN202611335560.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-31
- Publication Date
- 2026-11-24
AI Technical Summary
Existing short-wave infrared quantum dot photodetectors, while maintaining high infrared light absorption, suffer from excessively long carrier transport distances. Traditional transparent electrodes exhibit parasitic losses in the short-wave infrared region and are difficult to integrate with silicon-based CMOS back-end processes, thus failing to achieve a balance between high external quantum efficiency and microsecond-level response speed.
A dielectric-metal-dielectric (DMD) stacked electrode structure is designed as an asymmetric Fabry-Perot microcavity. Together with the top and bottom electrodes, a standing wave optical field is formed and localized within the thin quantum dot absorption layer. Combined with a low-temperature fabrication method, optical matching and electrical performance optimization are achieved.
Achieving efficient light absorption and short carrier transport within a thin quantum dot absorption layer, increasing the external quantum efficiency to 64.5%, achieving a response speed in the microsecond range, compatibility with silicon-based CMOS integration, and reducing fabrication costs.
Smart Images

Figure CN123164931A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of heterogeneous integration technology of semiconductor optoelectronic devices and special imaging chips. It relates to a quantum dot infrared photodetector, its preparation method and application. Specifically, it relates to a silicon-based quantum dot (CQD) infrared photodetector based on dielectric-metal-dielectric (DMD) stacked electrodes, its preparation method and its application in a silicon-based monolithically integrated short-wave infrared (SWIR) focal plane array (FPA) imaging and spectral acquisition system. Background Technology
[0002] Short-wave infrared (SWIR, typically referring to electromagnetic waves with wavelengths between 1000 nm and 2500 nm) imaging and detection technology has extremely important application value in fields such as night vision, weather monitoring, semiconductor defect detection, LiDAR receivers, and autonomous driving machine vision. Currently, commercially available SWIR image sensors mainly rely on epitaxially grown bulk inorganic compound semiconductor materials such as indium gallium arsenide (InGaAs) or mercury cadmium telluride (HgCdTe). However, the crystal growth process of these traditional materials requires stringent lattice matching conditions, resulting in extremely complex and costly manufacturing processes. Furthermore, it is difficult to achieve large-area, high-density monolithic wafer-level integration with standard silicon-based complementary metal-oxide-semiconductor (CMOS) readout integrated circuits (ROICs). The commonly used in-bump flip-chip bonding process faces bottlenecks such as limited pixel pitch, low yield, and extremely high cost of high-resolution pixelation, severely restricting the widespread adoption of SWIR focal plane arrays in the consumer market.
[0003] Colloidal quantum dots (CQDs), especially lead sulfide (PbS) quantum dots, are considered ideal active light-absorbing materials for next-generation infrared image sensors due to their characteristics such as broadband and continuously tunable bandgap in the infrared band caused by quantum confinement effect, extremely high optical absorption coefficient, low-cost large-area coating via room-temperature solution methods, and compatibility with standard silicon-based CMOS back-end low-temperature (BEOL) processes. However, traditional colloidal quantum dot photodetectors have long faced an intrinsic contradiction in their physical mechanism: photon absorption versus charge collection. To ensure sufficient effective light absorption at short-wave infrared operating wavelengths such as 1550 nm, the physical thickness of the quantum dot absorption layer typically needs to reach hundreds of nanometers (e.g., above 500 nm). However, due to the low intrinsic mobility of charge carriers in colloidal quantum dot films, their diffusion length is only about 100 nm to 200 nm, far less than the physical thickness required for high absorbance. This severe thickness mismatch leads to a large number of photogenerated carriers undergoing nonradiative recombination before reaching the collecting electrode, significantly reducing the device's external quantum efficiency (EQE) and increasing dark current. Furthermore, the thicker quantum dot absorption layer weakens the device's built-in electric field, resulting in excessively long carrier drift times and severely limiting the device's photoelectric response speed.
[0004] In recent years, researchers have attempted to alleviate these contradictions through optical engineering. For example, the paper "Resonantcavity-enhanced colloidal quantum-dot dual-band infrared photodetectors" integrates colloidal quantum dot dual-band infrared detectors with a Fabry-Perot resonator, achieving a bias-switchable spectral response in the short-wave infrared and mid-wave infrared ranges. Another example is the paper "Short-wave infrared colloidal QDsphotodetector with nanosecond response times enabled by ultrathin absorber layers," which shortens carrier transport time by using ultrathin quantum dot absorber layers, achieving a record-breaking response speed of 4 ns. Furthermore, it utilizes a Fabry-Perot cavity to achieve a 2.5-fold increase in light absorption, reaching an external quantum efficiency of 42% and a carrier extraction efficiency of 98% at 1330 nm. In 2025, similar research further achieved a 3.4-fold increase in absorption and a 97% carrier extraction efficiency on a flexible device using an FP cavity.
[0005] However, the research focus of the above-mentioned schemes is mainly on achieving dual-band spectral modulation using FP microcavities, improving response speed by thinning the absorption layer, or enhancing light absorption in flexible devices. No effective solution has yet been proposed for the parasitic absorption problem of the transparent top electrode in the short-wave infrared band in silicon-based top-incident quantum dot detectors. Furthermore, existing schemes do not perform joint optical matching of the transparent top electrode, the bottom high-reflectivity metal electrode, and the quantum dot absorption layer around the 1550 nm operating wavelength. This makes it difficult to simultaneously achieve localization of the standing-wave optical field, efficient light absorption, and a short carrier transport distance within a relatively thin quantum dot absorption layer. It also does not fully consider the monolithic integration requirements compatible with silicon-based CMOS back-end processes.
[0006] On the other hand, in conventional stacked detector structures, standard transparent conductive oxides (TCOs) such as indium tin oxide (ITO) are widely used as the top electrode on the light incident side. However, ITO films exhibit significant parasitic absorption in the short-wave infrared region due to the plasmon resonance characteristics of free carriers, causing a sharp deterioration in their transmittance in the short-wave infrared band. This forces the device to rely on thickening the quantum dot absorption layer to compensate for the loss of incident light intensity, thereby further exacerbating the aforementioned physical contradiction between charge extraction efficiency and light absorption thickness.
[0007] Therefore, how to shorten the carrier transport distance while maintaining high infrared light absorption, and at the same time take into account the conductivity of the top electrode, the light transmittance of the target band, and the low-temperature back-end integration of silicon-based CMOS, is a technical problem that needs to be solved in the field of short-wave infrared quantum dot image sensors. Summary of the Invention
[0008] The purpose of this invention is to overcome the shortcomings of existing quantum dot photodetectors, such as the mutual constraint between photon absorption efficiency and carrier extraction, severe parasitic losses of traditional transparent electrodes in the short-wave infrared region, and the inability to achieve both high external quantum efficiency and microsecond-level response speed. This invention provides a quantum dot infrared photodetector, its fabrication method, and its applications.
[0009] This invention introduces an optically precisely matched multilayer electrode (DMD) into the top electrode design of the infrared detector. This electrode effectively suppresses reflection of the ultrathin metal film in the short-wave infrared band while avoiding parasitic losses due to ITO as the top electrode, thus constructing an infrared optical window with high transmittance. Simultaneously, the DMD top electrode works in conjunction with the bottom reflective electrode to form a significant Fabry-Perot resonance enhancement at the target wavelength within the thin quantum dot absorption layer. This physically reshapes the spatial electromagnetic field distribution within the quantum dot absorption layer, thereby achieving superior short-wave infrared (1550 nm) external quantum efficiency and microsecond-level ultra-fast charge extraction response within the thin quantum dot absorption layer.
[0010] To achieve the above objectives, the present invention adopts the following technical solution:
[0011] In a first aspect, the present invention provides a quantum dot infrared photodetector, comprising, from bottom to top:
[0012] Base;
[0013] The bottom electrode is disposed on the substrate;
[0014] An edge overlay layer, disposed on a portion of the upper surface of the bottom electrode, is used to define the active region of the pixel;
[0015] A first charge transport layer continuously covers the exposed area of the bottom electrode and the surface of the edge covering layer;
[0016] A quantum dot absorption layer is disposed on top of the first charge transport layer;
[0017] A second charge transport layer is disposed on the quantum dot absorption layer;
[0018] The top electrode is disposed on the second charge transport layer. The top electrode adopts a dielectric-metal-dielectric three-layer stacked structure. The three-layer stacked structure consists of an inner dielectric layer, an ultrathin metal-based conductive layer, and an outer dielectric layer from bottom to top.
[0019] The bottom electrode is a reflective electrode, and the top electrode and the bottom electrode together form a Fabry-Perot microcavity. The thicknesses of the inner dielectric layer, the ultrathin metal-based conductive layer and the outer dielectric layer are optically matched so that the resonant wavelength of the Fabry-Perot microcavity is located in the short-wave infrared band.
[0020] The inner dielectric layer also serves as an interface modification layer.
[0021] Wherein, the first charge transport layer is an electron transport layer and the second charge transport layer is a hole transport layer, and the interface modification layer is an anode modification layer; or, the first charge transport layer is a hole transport layer and the second charge transport layer is an electron transport layer, and the interface modification layer is a cathode modification layer.
[0022] Preferably, the substrate is a single-crystal silicon substrate containing thermally oxidized silicon dioxide, and the bottom electrode is disposed on the thermally oxidized silicon dioxide layer; or, the substrate is a silicon wafer with integrated complementary metal-oxide-semiconductor (CMOS) readout circuitry, and the bottom electrode is directly fabricated and electrically connected to the pixel electrical contact pad on the top layer of the single-crystal silicon substrate.
[0023] Preferably, the material of the bottom electrode is selected from at least one of aluminum, titanium, gold, silver, titanium nitride, nickel, and tungsten, and the thickness is 50 to 200 nm.
[0024] Preferably, the edge covering layer is selected from at least one of silicon dioxide, silicon nitride, or aluminum oxide, and has a thickness of 30–200 nm.
[0025] Preferably, the material of the electron transport layer is selected from one of indium gallium zinc oxide (IGZO), zinc oxide (ZnO), titanium dioxide (TiO2), tin dioxide (SnO2), zinc tin oxide (ZTO), indium zinc oxide (IZO), PCBM, or C60, and the thickness is 5-25 nm.
[0026] Preferably, the quantum dot absorption layer is a near-infrared quantum dot absorption layer with a thickness of 100–250 nm; the quantum dot absorption layer is selected from PbS quantum dots, PbSe quantum dots, or HgTe quantum dots.
[0027] Preferably, the material of the hole transport layer is selected from at least one of 1,2-ethylenedithiol (EDT) treated lead sulfide quantum dots with a 900 nm absorption peak, 3-mercaptopropionic acid (MPA) treated lead sulfide quantum dots, nickel oxide (NiOx), cuprous thiocyanate (CuSCN), polyaniline (PANI), polytriarylamine (PTAA), Spiro-OMeTAD, Poly-TPD, TFB, or CBP; more preferably, the hole transport layer is 1,2-ethylenedithiol (EDT) treated PbS quantum dots.
[0028] Preferably, the inner dielectric layer is molybdenum oxide (MoO). x It is one of the following: vanadium oxide (V2O5), tungsten oxide (WO3), nickel oxide (NiOx), and copper oxide (CuO).
[0029] Preferably, the ultrathin metal-based conductive layer is composed of at least one of a single elemental metal, a metal alloy, or a metal compound with metallic conductive properties. The single elemental metal is selected from at least one of silver, gold, aluminum, copper, titanium, vanadium, iron, chromium, nickel, cobalt, molybdenum, tungsten, or tantalum; the metal compound includes at least one of titanium nitride, zirconium nitride, hafnium nitride, tantalum nitride, vanadium nitride, niobium nitride, molybdenum nitride, or tungsten nitride, and the thickness of the ultrathin metal-based conductive layer is 5–20 nm.
[0030] Furthermore, the ultrathin metal-based conductive layer also includes a wetting layer, a nucleation layer or a diffusion barrier layer located below or above it, wherein the material of the wetting layer, nucleation layer or diffusion barrier layer is selected from titanium, chromium, nickel-chromium, molybdenum, tantalum or a combination thereof, and the thickness is 0.5 to 5 nm.
[0031] Preferably, the outer dielectric layer is a dielectric material with low optical loss in the target short-wave infrared band, selected from at least one of molybdenum oxide (MoOx), tungsten oxide (WO3), bismuth oxide (Bi2O3), hafnium oxide (HfO2), zirconium oxide (ZrO2), tantalum oxide (Ta2O5), niobium oxide (Nb2O5), titanium oxide (TiO2), aluminum oxide (Al2O3), and silicon dioxide (SiO2), with a thickness of 30–250 nm.
[0032] Preferably, the light incident side of the outer dielectric layer is adjacent to an air, vacuum, or gas environment, or is provided with a transparent optical covering structure, wherein the transparent optical covering structure includes at least one of an inorganic dielectric protective film, an organic polymer encapsulation layer, a transparent adhesive layer, a transparent cover plate, and combinations thereof.
[0033] Secondly, the present invention provides a method for preparing the above-mentioned quantum dot infrared photodetector, comprising the following steps:
[0034] Step S1: Prepare a bottom electrode on the substrate using thermal evaporation or sputtering processes, and pattern the bottom electrode using lift-off, dry etching, or wet etching processes.
[0035] Step S2: An edge capping layer is prepared on the patterned bottom electrode using sputtering, chemical vapor deposition or atomic layer deposition processes, and a portion of the upper surface of the bottom electrode is etched to expose the active region of the pixel.
[0036] Step S3: A first charge transport layer is continuously deposited on the exposed area of the bottom electrode and the surface of the edge capping layer using thermal evaporation, sputtering or atomic layer deposition processes;
[0037] Step S4: Prepare a quantum dot absorption layer on the first charge transport layer using spin coating, inkjet printing, or printing processes;
[0038] Step S5: Prepare a second charge transport layer on the quantum dot absorption layer using spin coating, inkjet printing, thermal evaporation, sputtering or printing processes;
[0039] Step S6: Prepare an inner dielectric layer on the second charge transport layer using thermal evaporation, sputtering, or atomic layer deposition processes;
[0040] Step S7: Prepare an ultrathin metal-based conductive layer on the inner dielectric layer using thermal evaporation or sputtering processes;
[0041] Step S8: Prepare an outer dielectric layer on an ultrathin metal-based conductive layer using thermal evaporation, electron beam evaporation, sputtering, chemical vapor deposition, or atomic layer deposition processes.
[0042] Step S9: Package the quantum dot infrared photodetector to obtain the quantum dot infrared photodetector.
[0043] Preferably, a transparent optical cover structure is formed on the light incident side of the outer dielectric layer before or during encapsulation, or a transparent cover plate is disposed on the outer dielectric layer using a transparent adhesive layer.
[0044] Thirdly, the present invention provides the application of the above-mentioned quantum dot infrared photodetector in the fabrication of high-performance silicon-based monolithic integrated short-wave infrared photodetectors, high-pixel image sensors, and high-resolution focal plane imaging arrays.
[0045] Compared with the prior art, the beneficial effects of the present invention are as follows:
[0046] (1) This invention performs joint optical matching on the thickness of each dielectric layer of the DMD, the thickness of the ultrathin metal substrate conductive layer, and the thickness of the quantum dot absorption layer around the 1550 nm operating wavelength, so that the top DMD simultaneously serves as a low-loss infrared incident window and a semi-reflective front mirror, forming an asymmetric microcavity with the bottom high-reflectivity metal electrode. This design localizes the standing wave antinodes of the 1550 nm incident light after reflection from the upper and lower interfaces mainly within the PbS quantum dot absorption layer with a thickness of only 175-185 nm, thereby achieving efficient light absorption in the target wavelength band without relying on a thick quantum dot absorption layer. Comparative experiments show that, under the same thin absorption layer conditions, the theoretical quantum efficiency of the device using the ITO top electrode is only 36%, while the theoretical quantum efficiency of the DMD structure device of this invention can reach 64.5%, an improvement of about 79%; the measured external quantum efficiency is increased from 39.82% for the ITO device to 58.57% for the DMD device. The effect of this technology does not come from the simple replacement of the ITO electrode with the DMD electrode, but from the synergistic gain generated by the combined matching of the top DMD, the bottom reflective electrode and the thickness of the absorption layer.
[0047] (2) This invention replaces the traditional ITO transparent electrode with a DMD electrode, which fundamentally eliminates the incident light loss caused by the plasma resonance absorption of ITO free carriers in the short-wave infrared band. It uses the destructive interference effect of the dielectric-metal-dielectric three-layer structure to suppress the reflection of the ultrathin metal film in the short-wave infrared band, while avoiding the inherent infrared parasitic absorption of ITO and maximizing the infrared photon flux entering the quantum dot absorption layer.
[0048] (3) This invention utilizes the optical field localization effect of an asymmetric Fabry-Perot microcavity to achieve efficient light absorption with an absorption layer thickness of only 175 nm (within a comparable range for carrier diffusion length), thereby significantly shortening the transmission distance of photogenerated carriers. This effect relies on the synergistic effect of the thin absorption layer shortening the carrier path and the microcavity enhancement compensating for light absorption loss: if there is only a thin absorption layer without microcavity enhancement, the light absorption is insufficient; if there is microcavity enhancement but the absorption layer is too thick, carrier extraction is limited.
[0049] (4) All functional layers of this invention are fabricated at low temperatures, avoiding damage to the underlying silicon-based CMOS readout circuit or the completed device layer caused by high-temperature processes. At the same time, the ultra-thin metal-based conductive layer in the DMD can meet the electrical requirements of the electrodes without the need for thick metal or high-temperature annealing treatment. Compared with traditional sputtering ITO or high-temperature annealing processes, this effectively reduces plasma damage and thermal budget. Attached Figure Description
[0050] The accompanying drawings in this application all illustrate an upright configuration (i.e., the first charge transport layer is an electron transport layer and the second charge transport layer is a hole transport layer) as an example embodiment. However, those skilled in the art should understand that the optical and electrical gain mechanisms are also applicable to the inverted configuration.
[0051] Figure 1 A schematic diagram of the quantum dot infrared photodetector provided in this application;
[0052] Figure 2 This is a schematic diagram of the structure of the quantum dot infrared photodetector provided in Embodiment 1 of this application;
[0053] Figure 3 The simulation and actual absorption of 1550 nm wavelength infrared light by the quantum dot infrared photodetector provided in Embodiment 1 of this application and the quantum dot photodetector with the same device structure and ITO top electrode are compared with the relationship between the thickness of the quantum dot absorption layer.
[0054] Figure 4 This is the internal electric field intensity distribution of Embodiment 1 of this application under FDTD optical simulation.
[0055] Figure 5 This is the current density measured in light and dark states in Embodiment 1 of this application.
[0056] Figure 6 The response curve of Example 1 of this application under pulsed infrared light at a wavelength of 1550 nm is shown. Detailed Implementation
[0057] The technical solutions of this application will now be clearly and completely described with reference to the accompanying drawings. Obviously, the described embodiments are only some, not all, of the embodiments of this application. Based on the embodiments of this application, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this application.
[0058] Example 1
[0059] This embodiment provides a method for fabricating a quantum dot infrared photodetector, and the fabricated detector structure is as follows. Figure 2 As shown, from bottom to top, they include:
[0060] The bottom electrode is made of at least one of aluminum, titanium, gold, silver, titanium nitride, nickel, and tungsten, and has a thickness of 50–200 nm; in this embodiment, aluminum is used, and the thickness is 50 nm.
[0061] An edge covering layer, wherein the edge covering layer is selected from at least one of silicon dioxide, silicon nitride compound or aluminum oxide, and has a thickness of 50 to 200 nm; in this embodiment, silicon dioxide is used, and the thickness is 50 nm.
[0062] A first charge transport layer covers the exposed area and edge covering layer of the bottom electrode. Figure 1 In the upright configuration shown, the first charge transport layer is an electron transport layer, which is at least one of indium gallium zinc oxide (IGZO), zinc oxide (ZnO), titanium dioxide (TiO2), tin dioxide (SnO2), zinc tin oxide (ZTO), indium zinc oxide (IZO), PCBM, or C60, with a thickness of 5–25 nm; in this embodiment, indium gallium zinc oxide (IGZO) is used, with a thickness of 15 nm;
[0063] A quantum dot absorption layer is disposed on the first charge transport layer; the quantum dot absorption layer is selected from quantum dot absorption layers with near-infrared absorption spectra, and has a thickness of 100-250 nm; the quantum dot absorption layer is selected from lead sulfide (PbS) quantum dots, lead selenide (PbSe) quantum dots, or mercury telluride (HgTe) quantum dots; in this embodiment, PbS quantum dots with an absorption peak of 1550 nm and a thickness of 175 nm are used;
[0064] A second charge transport layer is disposed above the quantum dot absorption layer; Figure 1 In the upright configuration shown, the second charge transport layer is a hole transport layer, which is composed of 1,2-ethylenedithiol (EDT) treated PbS quantum dots, 3-mercaptopropionic acid (MPA) treated PbS quantum dots, and nickel oxide (NiOx).
[0065] At least one of cuprous thiocyanate (CuSCN), polyaniline (PANI), polytriarylamine (PTAA), Spiro-OMeTAD, Poly-TPD, TFB, or CBP; in this embodiment, PbS quantum dots treated with EDT are used, with an absorption peak of 900 nm and a thickness of 20 nm.
[0066] An inner dielectric layer is disposed above the second charge transport layer; the inner dielectric layer is molybdenum oxide (MoO). x Vanadium oxide (V₂O₅), tungsten oxide (WO₃), nickel oxide (NiO) x One of the following: copper oxide (CuO); in this embodiment, MoO is used. x The thickness is 15 nm;
[0067] The ultrathin metal-based conductive layer is composed of at least one of a single metal, a metal alloy, or a metal compound with metallic conductivity. The single metal is selected from at least one of silver, gold, aluminum, copper, titanium, vanadium, iron, chromium, nickel, cobalt, molybdenum, tungsten, or tantalum; the metal compound includes at least one of titanium nitride, zirconium nitride, hafnium nitride, tantalum nitride, vanadium nitride, niobium nitride, molybdenum nitride, or tungsten nitride. The thickness of the ultrathin metal-based conductive layer is 5–20 nm. Preferably, the ultrathin metal-based conductive layer further includes a wetting layer, a nucleation layer, or a diffusion barrier layer located below or above it. The material of the wetting layer, nucleation layer, or diffusion barrier layer is selected from titanium, chromium, nickel-chromium, molybdenum, tantalum, or combinations thereof, and the thickness is 0.5–5 nm. In this embodiment, silver is used, with a thickness of 18 nm.
[0068] An outer dielectric layer is disposed on top of the ultrathin metal-based conductive layer; the outer dielectric layer is a dielectric material with low optical loss in the target short-wave infrared band, selected from molybdenum oxide (MoO). x At least one of the following: tungsten oxide (WO3), bismuth oxide (Bi2O3), hafnium oxide (HfO2), zirconium oxide (ZrO2), tantalum oxide (Ta2O5), niobium oxide (Nb2O5), titanium oxide (TiO2), aluminum oxide (Al2O3), and silicon dioxide (SiO2), with a thickness of 30–250 nm; this embodiment uses MoO. x The thickness is 160 nm.
[0069] In other embodiments, an inorganic dielectric protective film, an organic polymer encapsulation layer, a transparent adhesive layer, or a transparent cover plate may also be provided on the light incident side of the outer dielectric layer, and the materials and thicknesses of the stacked top electrode and the quantum dot absorption layer are jointly optically matched according to the optical characteristics of the adjacent optical environment on the light incident side.
[0070] The present invention also provides a method for fabricating the above-mentioned quantum dot infrared photodetector, including the steps of fabricating a bottom electrode, fabricating an edge capping layer, fabricating an electron transport layer, fabricating a quantum dot absorption layer, fabricating a hole transport layer, fabricating an inner dielectric layer, fabricating an ultrathin metal-based conductive layer, and fabricating an outer dielectric layer.
[0071] Specifically as follows:
[0072] (1) A Si substrate covered with 200 nm thermally oxidized SiO2, which has undergone a rigorous cleaning process, is selected and placed in a vacuum with a degree better than 10 -6 In the Torr cavity, a dense aluminum film with a thickness of 50 nm is deposited at a rate of 1 Å / s using magnetron sputtering as the bottom electrode.
[0073] (2) Spin-coating 5350 photoresist onto the surface of the aluminum thin film. Expose the pixel area using a photolithography system, and expose the pixel area after development. Place it in an aluminum etchant to remove the parts not covered by the photoresist, and then remove the photoresist in acetone solvent to finally obtain the patterned bottom electrode.
[0074] (3) A 50 nm SiO2 layer was deposited on the bottom electrode surface at 130 °C using chemical vapor deposition. The pixel area was exposed using a photolithography system and then developed to expose the pixel area. The pixel area was then etched using plasma dry etching to expose the bottom electrode as the active area of the pixel.
[0075] (4) Using vacuum thermal evaporation or magnetron sputtering, an indium gallium zinc oxide (IGZO) layer is deposited on the edge isolation layer and the exposed bottom electrode surface to obtain a 15 nm thick IGZO film.
[0076] (5) A quantum dot absorption layer was prepared using a spin-coating method combined with a liquid-phase ligand exchange process. The I1550 ion of the quantum dot absorption layer was then applied. - ,Br - The ligand PbS quantum dot ink was spin-coated at 2500 rpm for 30 s to obtain a 175 nm quantum dot film, which was then annealed at 80 °C for 10 minutes under nitrogen atmosphere.
[0077] (6) On the surface of the quantum dot absorption layer, a quantum dot hole transport layer is prepared by spin coating combined with solid ligand exchange process. The oleic acid ligand PbS quantum dots with an absorption peak of 900 nm are dissolved in n-octane to obtain an ink of 25 mg / mL. The ink is deposited on the surface of the absorption layer by spin coating at a speed of 3000 rpm for 30 s. A 0.01% concentration of 1,2-ethylenedithiol (EDT) acetonitrile solution is added dropwise for solid ligand exchange. After standing for 30 s, the solution is dried by spin coating at a speed of 2500 rpm and the excess ligand is washed away to obtain a 20 nm film with optimized thickness. The film is annealed at 80 °C for 10 minutes under nitrogen atmosphere.
[0078] (7) Transfer the completed spin-coated semi-finished device to a vacuum thermal evaporation equipment, and heat it at a temperature better than 10°C. -4 Under Torr's vacuum environment, a uniform 15 nm thick layer of molybdenum oxide (MoO) was deposited on the surface of the 900 nm PbS quantum dot layer at an evaporation rate of 0.1 Å / s. x A thin film is deposited as the inner dielectric layer; a 18 nm thick silver film is deposited in the cooling chamber at a rate of 2 Å / s as an ultrathin metal-based conductive layer; a 160 nm thick molybdenum oxide (MoO) film is deposited in the cooling chamber at a rate of 1 Å / s. x A thin film serves as the outer dielectric layer.
[0079] Optical simulation tests were performed on the aforementioned quantum dot infrared photodetector using FDTD Lumerical software.
[0080] like Figure 3 As shown, by changing the thickness of different quantum dot absorption layers, the theoretical quantum efficiency of the quantum dot infrared photodetector of Embodiment 1 of the present invention and the quantum dot photodetector with the same device structure and ITO top electrode were compared. Near the thinner 185 nm quantum dot absorption layer, the theoretical quantum efficiency increased from 36% of the ITO top electrode quantum dot photodiode detector to 64.5% of the dielectric-metal-dielectric stacked electrode detector, an increase of about 79%. Figure 4 The internal electric field intensity distribution in the FDTD optical simulation at the thickness of Example 1 is shown. After passing through the Fabry-Perot microcavity interference effect generated by the dielectric-metal-dielectric stacked electrode, the light intensity is concentrated in the quantum dot absorption layer, which explains the absorption enhancement of the dielectric-metal-dielectric stacked electrode detector.
[0081] like Figure 3As shown, measurements were taken of the detector prepared in Example 1. The quantum efficiency of the detector with a dielectric-metal-dielectric stack electrode and a 175 nm quantum dot absorption layer was 58.57%, compared with 39.82% for the actual ITO top electrode detector. The quantum efficiency was improved by 47%, which effectively proved the absorption enhancement caused by the Fabry-Perot microcavity interference effect generated by the dielectric-metal-dielectric stack electrode in the silicon-based quantum dot photodetector with a thinner quantum dot absorption layer. Figure 5 The dark current of the detector in Example 1 is shown at 7.9 mW / cm². 2 The photocurrent under 1550 nm wavelength light has a responsivity of 0.732 A / W at -1 V and a quantum efficiency of 58.57%. Figure 6 The photoresponse curve of the detector in Example 1 is shown, with a rising edge of 1.8 μs and a falling edge of 2.8 μs.
[0082] Specifically, the quantum dot infrared photodetector fabricated in this embodiment of the invention establishes an ideal and efficient optical control mechanism and charge extraction channel in the infrared target band. This structure successfully overcomes the physical bottleneck of traditional devices being unable to simultaneously achieve high infrared absorption and extremely fast response, realizing a highly efficient fusion of high external quantum efficiency (58.57%) and microsecond-level ultrafast response time (2.8 μs) at 1550 nm, and the fabrication temperature is fully compatible with low-temperature semiconductor back-end integration processes. This provides a silicon-based CMOS monolithic integration technology path for the commercial upgrade of low-cost, high-performance, high-resolution short-wave infrared focal plane imaging technology and multi-channel portable spectrometers.
[0083] The above embodiments are merely illustrative of the technical solutions of the present invention and are not intended to limit it. Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some of the technical features; and these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the present invention. All simple variations, equivalent substitutions, or conventional optimizations derived from the concept of the present invention fall within the protection scope of the present invention.
Claims
1. A quantum dot infrared photodetector, comprising, from bottom to top: Base; The bottom electrode is disposed on the substrate; An edge overlay layer, disposed on a portion of the upper surface of the bottom electrode, is used to define the active region of the pixel; A first charge transport layer continuously covers the exposed area of the bottom electrode and the surface of the edge covering layer; A quantum dot absorption layer is disposed on top of the first charge transport layer; A second charge transport layer is disposed on the quantum dot absorption layer; Its features are, The detector also includes a top electrode disposed on the second charge transport layer. The top electrode adopts a three-layer stacked structure of dielectric-metal-based conductive layer-dielectric. The three-layer stacked structure consists of an inner dielectric layer, an ultrathin metal-based conductive layer, and an outer dielectric layer from bottom to top. The ultrathin metal-based conductive layer is formed of at least one of elemental metal, metal alloy, or metal compound with metallic conductivity. The bottom electrode is a reflective electrode, and the top electrode and the bottom electrode together form an asymmetric Fabry-Perot microcavity; The thicknesses of the inner dielectric layer, the ultrathin metal-based conductive layer, the outer dielectric layer, and the quantum dot absorption layer are combined optically matched, and the optical characteristics of the adjacent optical environment on the light incident side of the outer dielectric layer are taken into account, so that the Fabry-Perot microcavity will localize the standing wave antinode within the quantum dot absorption layer at the resonant wavelength in the short-wave infrared band.
2. The quantum dot infrared photodetector according to claim 1, characterized in that, The substrate is a single-crystal silicon substrate containing a thermally oxidized silicon dioxide layer, and the bottom electrode is disposed on the thermally oxidized silicon dioxide layer; or, the substrate is a silicon wafer with an integrated complementary metal-oxide-semiconductor readout circuit, and the bottom electrode is directly fabricated and electrically connected to the pixel electrical contact pad on the top layer of the single-crystal silicon substrate or the readout circuit.
3. The quantum dot infrared photodetector according to claim 1, characterized in that, The bottom electrode is a highly reflective metal electrode, the material of which is selected from at least one of aluminum, titanium, gold, silver, titanium nitride, nickel, and tungsten, and the thickness is 50 to 200 nm. The edge covering layer is made of at least one of silicon dioxide, silicon nitride, or aluminum oxide, and has a thickness of 30 nm to 200 nm.
4. The quantum dot infrared photodetector according to claim 1, characterized in that, The inner dielectric layer also serves as an interface modification layer. When the first charge transport layer is an electron transport layer and the second charge transport layer is a hole transport layer, the inner dielectric layer is an anode modification layer; when the first charge transport layer is a hole transport layer and the second charge transport layer is an electron transport layer, the inner dielectric layer is a cathode modification layer.
5. The quantum dot infrared photodetector according to claim 1, characterized in that, The electron transport layer is made of one of the following materials: indium gallium zinc oxide, zinc oxide, titanium dioxide, tin dioxide, zinc tin oxide, indium zinc oxide, PCBM, or C60, and has a thickness of 5–25 nm. The material of the quantum dot absorption layer is selected from one of lead sulfide quantum dots, lead selenide quantum dots, or mercury telluride quantum dots, and the thickness is 100-250 nm. The material of the hole transport layer is selected from at least one of 1,2-ethylenedithiol treated lead sulfide quantum dots, 3-mercaptopropionic acid treated lead sulfide quantum dots, nickel oxide, cuprous thiocyanate, polyaniline, polytriarylamine, Spiro-OMeTAD, Poly-TPD, TFB, or CBP. The material of the inner dielectric layer is selected from one of molybdenum oxide, vanadium oxide, tungsten oxide, nickel oxide, and copper oxide, and the thickness is 5 to 30 nm. The material of the ultrathin metal-based conductive layer is selected from at least one of silver, gold, aluminum, copper, titanium, vanadium, iron, chromium, nickel, cobalt, molybdenum, tungsten, tantalum and their alloys; or selected from at least one of metal nitrides with metallic conductive properties. The metal nitride includes at least one of titanium nitride, zirconium nitride, hafnium nitride, tantalum nitride, vanadium nitride, niobium nitride, molybdenum nitride, or tungsten nitride; The thickness of the ultrathin metal-based conductive layer is 5–20 nm; The outer dielectric layer material is a dielectric material with low optical loss in the short-wave infrared band, selected from at least one of molybdenum oxide, tungsten oxide, bismuth oxide, hafnium oxide, zirconium oxide, tantalum oxide, niobium oxide, titanium oxide, aluminum oxide, silicon dioxide, and silicon nitride, with a thickness of 30–250 nm.
6. The quantum dot infrared photodetector according to claim 1, characterized in that, The light incident side of the outer dielectric layer is adjacent to an air, vacuum, or gas environment, or is provided with a transparent optical covering structure; The transparent optical cover structure includes at least one of an inorganic dielectric protective film, an organic polymer encapsulation layer, a transparent adhesive layer, a transparent cover plate, and combinations thereof; The transparent optical covering structure is directly disposed on the surface of the outer dielectric layer, or is disposed at an interval from the outer dielectric layer, forming an air, inert gas, or vacuum gap between them.
7. The quantum dot infrared photodetector according to claim 6, characterized in that, The ultrathin metal-based conductive layer further includes a wetting layer, a nucleation layer, or a diffusion barrier layer located below or above it. The material of the wetting layer, nucleation layer, or diffusion barrier layer is selected from titanium, chromium, nickel-chromium, molybdenum, tantalum, or a combination thereof, and the thickness is 0.5–5 nm.
8. A method for fabricating a quantum dot infrared photodetector as described in any one of claims 1-7, characterized in that, Includes the following steps: Step S1: Prepare a bottom electrode on the substrate using thermal evaporation or sputtering processes, and pattern the bottom electrode using lift-off, dry etching, or wet etching processes. Step S2: An edge capping layer is prepared on the patterned bottom electrode using sputtering, chemical vapor deposition or atomic layer deposition processes, and a portion of the upper surface of the bottom electrode is etched to expose the active region of the pixel. Step S3: A first charge transport layer is continuously deposited on the exposed area of the bottom electrode and the surface of the edge capping layer using thermal evaporation, sputtering or atomic layer deposition processes; Step S4: Prepare a quantum dot absorption layer on the first charge transport layer using spin coating, inkjet printing, or printing processes; Step S5: Prepare a second charge transport layer on the quantum dot absorption layer using spin coating, inkjet printing, thermal evaporation, sputtering or printing processes; Step S6: Prepare an inner dielectric layer on the second charge transport layer using thermal evaporation, sputtering, or atomic layer deposition processes; Step S7: Prepare an ultrathin metal-based conductive layer on the inner dielectric layer using thermal evaporation or sputtering processes; Step S8: Prepare an outer dielectric layer on the ultrathin metal substrate conductive layer using thermal evaporation, electron beam evaporation, sputtering, chemical vapor deposition, or atomic layer deposition processes. Step S9: Package the quantum dot infrared photodetector.
9. The preparation method according to claim 8, characterized in that, Before or during encapsulation, a transparent optical cover structure is formed on the light incident side of the outer dielectric layer, or a transparent adhesive layer is used to place a transparent cover plate on the outer dielectric layer.
10. The application of the quantum dot infrared photodetector as described in any one of claims 1-7 in the fabrication of a silicon-based monolithic integrated short-wave infrared focal plane array imaging chip, a high-pixel short-wave infrared image sensor, or a short-wave infrared spectral acquisition system.