A hole transport material for driving buried interface strengthening and perovskite solar cell and preparation method thereof

By constructing a co-self-assembly layer, phosphonic acid groups are used to enhance interfacial bonding, and Lewis acid-base coordination and steric hindrance are used to regulate perovskite grain growth. This solves the problems of uneven interfacial coverage, insufficient anchoring force, and weak crystallization control of traditional hole transport layer materials in perovskite solar cells, thereby improving photoelectric conversion efficiency and reliability.

CN123164933APending Publication Date: 2026-11-24ZHEJIANG UNIV OF TECH +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611108183.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-07-24
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Traditional hole transport layer materials in perovskite solar cells suffer from uneven interface coverage, insufficient anchoring force, and weak crystallization control, resulting in high interface defect state density and aggravated energy level mismatch, which affects the photoelectric conversion efficiency and long-term operational reliability of the device.

Method used

A co-self-assembled layer was constructed using a first self-assembled molecule and a second self-assembled molecule with a molar ratio of 1:(1~9) as a hole transport layer. The interfacial bonding strength was enhanced by phosphonic acid groups, defects were passivated by Lewis acid-base coordination, and carbazole rings provided steric hindrance to regulate perovskite grain growth.

Benefits of technology

It improves the uniformity of the molecular arrangement at the interface, reduces non-radiative recombination loss, promotes the formation of large-grain, low-defect-density perovskite thin films, and enhances the photoelectric conversion efficiency and structural integrity of the device.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123164933A_ABST
    Figure CN123164933A_ABST
Patent Text Reader

Abstract

This invention belongs to the field of solar cell technology, and relates to a hole transport material for driving buried interface enhancement, a perovskite solar cell, and a method for its fabrication. This invention constructs a high-precision, ordered hole transport system on an ITO surface by co-self-assembling TMeO-PA with two phosphonic acid groups, a trimethoxybenzene ring, and a carbazole ring with 4PADCB containing a single phosphonic acid group. This system drives multiple synergistic effects, including enhanced chemical bonding, optimized energy level arrangement, passivation of interface defects, and crystal template guidance. This comprehensively enhances the buried interface in terms of mechanical bonding, charge extraction efficiency, non-radiative recombination suppression, and residual stress release, ultimately endowing the perovskite solar cell with excellent photoelectric performance and long-term operational stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of solar cell technology, and relates to a hole transport material for driving buried interface strengthening, a perovskite solar cell, and a method for preparing the same. Background Technology

[0002] Perovskite solar cells, with their unique advantages of low-temperature solution processing, high power-to-weight ratio, and ultra-thin and flexible design, have shown broad application prospects in portable energy, flexible electronics, and building-integrated photovoltaics. In recent years, with the continuous development of perovskite composition engineering, interface passivation technology, and device structure optimization, laboratory-certified photoelectric conversion efficiencies have exceeded 26%, gradually approaching the theoretical limit.

[0003] However, traditional hole transport layer materials face severe challenges in real-world operating environments. While hole transport materials, represented by self-assembled monolayers (SAMs), possess advantages such as ultrathinness and low-temperature solution processing capabilities, they exhibit the following prominent problems during device fabrication and operation: First, SAMs are prone to spontaneous molecular aggregation on the substrate surface, leading to uneven interface coverage and the formation of localized conductive dead zones. Second, the bonding force between the anchoring groups of a single molecular system and the substrate is limited, resulting in insufficient interfacial anchoring points. Under thermal or optical stress, molecular desorption easily occurs, leading to interface degradation. Third, traditional SAM molecules have a weak template-guiding effect on perovskite crystallization, failing to effectively control the nucleation and growth behavior of perovskite grains, easily inducing increased defect state density at the buried interface, exacerbated energy level mismatch, and accumulation of residual tensile strain. These problems severely restrict the photoelectric conversion efficiency and long-term operational reliability of devices.

[0004] Current research has attempted to improve the performance of SAM molecules by introducing multiple anchoring groups or functional end groups through molecular structure design. However, a single molecule often struggles to simultaneously meet multiple requirements such as strong anchoring, energy level matching, defect passivation, and crystallization regulation. Therefore, exploring perovskite photovoltaic technology based on molecular engineering methods to achieve buried interface strengthening and crystallization regulation has become a key breakthrough for overcoming its efficiency-stability constraints and promoting industrial applications. Summary of the Invention

[0005] The purpose of this invention is to address the aforementioned problems in the existing technology by proposing a perovskite solar cell based on high-precision molecular assembly to drive the enhancement of the buried interface. By constructing a multifunctional co-self-assembled layer as a hole transport layer, chemical passivation, energy level optimization, crystal template guidance, and mechanical anchoring enhancement of the buried interface are achieved.

[0006] One objective of this invention is achieved through the following technical solution: A hole transport material for driving the reinforcement of buried interfaces, the raw materials of which include a first self-assembled molecule and a second self-assembled molecule in a molar ratio of 1:(1~9); The first self-assembled molecule is 9-(3,4,5-trimethoxyphenyl)-9H-carbazole-2,7-diphosphonic acid TMeO-PA. The second self-assembled molecule is [4-(7H-dibenzocarbazole-7-yl)butyl]phosphonic acid 4PADCB; The structural formulas of the first self-assembled molecule and the second self-assembled molecule are shown in Equation (1) and Equation (2) respectively: .

[0007] The second objective of this invention is achieved through the following technical solution: A perovskite solar cell comprises, from bottom to top: a conductive substrate layer, a hole transport layer, a perovskite light-absorbing layer, an electron transport layer, an interface control layer, and a metal electrode layer. The hole transport layer is a co-self-assembly layer, and the raw materials of the co-self-assembly layer include a first self-assembly molecule and a second self-assembly molecule in a molar ratio of 1:(1~9). The first self-assembled molecule is TMeO-PA, and the second self-assembled molecule is 4PADCB. Their structural formulas are shown in Equation (1) and Equation (2) respectively: .

[0008] The first self-assembled molecule used in this invention has two phosphonic acid groups, a trimethoxybenzene ring, and a carbazole ring. The two phosphonic acid groups (-PO(OH)2) provide two binding sites that coordinate with the conductive substrate ITO surface, significantly enhancing the interfacial bonding strength, inhibiting spontaneous molecular aggregation, and forming a continuous and uniform highly conductive pathway. The electron-donating methoxy group in the trimethoxybenzene ring passivates the uncoordinated Pb at the perovskite buried interface through Lewis acid-base coordination. 2+ The defects reduce non-radiative recombination losses; the large-volume cross-configuration of the carbazole ring and trimethoxyphenyl introduces steric hindrance.

[0009] Preferably, the molar ratio of the first self-assembled molecule to the second self-assembled molecule is 1:(2~4).

[0010] Further preferably, the molar ratio of the first self-assembled molecule to the second self-assembled molecule is 1:3.

[0011] Preferably, the second self-assembled molecule can also be other carbazolylphosphonic acid self-assembled molecules, selected from [2-(9H-carbazol-9-yl)ethyl]phosphonic acid (2PACz), [4-(9H-carbazol-9-yl)butyl]phosphonic acid (4PACz), [2-(3,6-dimethoxy-9H-carbazol-9-yl)ethyl]phosphonic acid (MeO-2PACz), and [4-(3,11-dimethoxy-7H-dibenzocarbazol-7-yl)butyl]phosphonic acid (MeO-4P). One or more of the following: ADBC), [2,7-dimethoxy-9H-carbazole-9-yl)methyl]phosphonic acid (DC-PA), [2-(4-(bis(4-methoxyphenyl)amino)phenyl)-1-cyanovinyl]phosphonic acid (MPA-CPA), [4-(3,6-dimethyl-9H-carbazole-9-yl)butyl]phosphonic acid (Me-4PACz), and [2-(3,6-dimethoxy-9H-carbazole-9-yl)butyl]phosphonic acid (MeO-4PACz).

[0012] Preferably, the thickness of the conductive substrate layer is 800~1500nm.

[0013] Preferably, the conductive substrate is an indium tin oxide / polyethylene naphthalate composite conductive substrate PEN / ITO, wherein the sheet resistance of ITO is 15Ω.

[0014] Preferably, the thickness of the hole transport layer is 5~50nm.

[0015] Further preferably, the thickness of the hole transport layer is 10~30nm.

[0016] More preferably, the thickness of the hole transport layer is 15~25nm.

[0017] Preferably, the hole transport layer is prepared by dissolving the first self-assembled molecule and the second self-assembled molecule in an organic solvent, followed by spin coating and annealing.

[0018] Preferably, the thickness of the perovskite light-absorbing layer is 300~800 nm.

[0019] Further preferably, the thickness of the perovskite light-absorbing layer is 400~600nm.

[0020] Preferably, the perovskite light-absorbing layer comprises a perovskite material; The perovskite material has ABX3 crystals, wherein A is selected from formamidinium cation FA. + methylammonium cation MA + Cesium ions (Cs) + Rubidium ion Rb + One or more of them, where B is selected from lead ions (Pb). 2+ Tin ions (Sn)2+ One or more of them, where X is selected from chloride ions (Cl). - Bromide ions (Br) - Iodide ions - thiocyanate ions (SCN) - One or more of them.

[0021] Further preferably, the perovskite material is FA. 1-x-y MA x Cs y Pb(I 1-z Br z )3 or Cs 1-x (FA 1-y MA y ) x Pb(I 1- z Br z )3, where 0 < x < 1, 0 < y < 1, 0 ≤ z < 1.

[0022] Further preferably, the perovskite material is FA. 0.85 MA 0.15 Cs 0.05 PbI3 or Cs 0.05 (FA 0.96 MA 0.04 ) 0.95 Pb(I 0.95 Br 0.05 3.

[0023] Further preferably, the perovskite material is Cs. 0.05 (FA 0.96 MA 0.04 ) 0.95 Pb(I 0.95 Br 0.05 3.

[0024] Preferably, the thickness of the electron transport layer is 10~30nm.

[0025] Preferably, the material of the electron transport layer is selected from C. 60 One or more of (6,6)-phenyl-C61-butyrate methyl ester (PCBM) and poly(3-hexylthiophene) (P3HT).

[0026] Preferably, the thickness of the interface control layer is 1~20nm.

[0027] Preferably, the material of the interface regulation layer is 2,9-dimethyl-4,7-diphenyl-1,10-phenanthroline (BCP).

[0028] Preferably, the thickness of the metal electrode layer is 50~150nm.

[0029] Preferably, the metal in the metal electrode layer is selected from one or more of Ag, Al, Au and Cu.

[0030] The third objective of this invention is achieved through the following technical solution: A method for fabricating a perovskite solar cell includes the following steps: (1) Pretreatment of the conductive substrate layer; (2) Dissolve the first self-assembled molecule and the second self-assembled molecule with a molar ratio of 1:(1~9) in an organic solvent to obtain a co-self-assembled solution, spin-coat it onto the surface of the conductive substrate layer in step (1), and anneal it to obtain a hole transport layer. (3) Spin-coat the perovskite precursor solution onto the surface of the hole transport layer in step (2), add antisolvent during the spin-coating process, and anneal to obtain the perovskite light absorption layer; (4) Vacuum evaporation deposition is performed on the surface of the perovskite light-absorbing layer in step (3) to obtain the electron transport layer; (5) Vacuum evaporation deposition is performed on the surface of the electron transport layer in step (4) to obtain the interface control layer; (6) Vacuum evaporation deposition is performed on the surface of the interface control layer in step (5) to obtain a metal electrode layer.

[0031] Preferably, in step (1), the pretreatment includes: wiping the indium tin oxide / polyethylene naphthalate composite conductive substrate in sequence, drying it with nitrogen, and cleaning it with ultraviolet light.

[0032] Further preferably, the power of the ultraviolet light irradiation cleaning is 100~200W, and the time is 15~60min.

[0033] More preferably, the ultraviolet light irradiation cleaning has a power of 150W and a time of 30min.

[0034] Preferably, in step (2), the organic solvent is selected from one or more of ethanol, methanol, and isopropanol.

[0035] Further preferably, the organic solvent is anhydrous ethanol.

[0036] Preferably, in step (2), the concentration of the co-self-assembly solution is 0.1~1.5 mg / mL.

[0037] More preferably, the concentration of the co-self-assembly solution is 0.3~1.0 mg / mL.

[0038] More preferably, the concentration of the co-self-assembly solution is 0.5~0.9 mg / mL.

[0039] Preferably, in step (2), the spin coating speed is 1000~5000 rpm and the time is 10~60s.

[0040] Further preferably, the spin coating speed is 2000~4000 rpm and the spin coating time is 20~40 s.

[0041] Preferably, in step (2), the annealing temperature is 80~120℃ and the annealing time is 5~30min.

[0042] Further preferably, the annealing temperature is 90~110℃ and the annealing time is 8~15min.

[0043] Preferably, in step (3), the method for preparing the perovskite light absorption layer includes: spin-coating a perovskite precursor solution with a concentration of 0.5~3.0 mol / L onto the surface of the hole transport layer, adding an anti-solvent during the spin-coating process, and then annealing.

[0044] Further preferably, the perovskite precursor solution is FA. 0.85 MA 0.15 Cs 0.05 PbI3 or Cs 0.05 (FA 0.96 MA 0.04 ) 0.95 Pb(I 0.95 Br 0.05 3.

[0045] Further preferably, the concentration of the perovskite precursor solution is 1.0~2.0 mol / L.

[0046] More preferably, the concentration of the perovskite precursor solution is 1.5~1.8 mol / L.

[0047] Further preferably, the spin coating speed is 2000~8000 rpm and the time is 10~120s.

[0048] More preferably, the spin coating speed is 3000~5000 rpm and the time is 20~40s.

[0049] Further preferably, the antisolvent is added dropwise 1-20 seconds after the spin coating begins.

[0050] More preferably, the amount of antisolvent added is 100~1000μL.

[0051] More preferably, the antisolvent is one or more of anhydrous diethyl ether, chlorobenzene, and toluene.

[0052] More preferably, the antisolvent is anhydrous diethyl ether.

[0053] Further preferably, the annealing temperature is 80~120℃ and the annealing time is 10~60min.

[0054] More preferably, the annealing temperature is 90~110℃ and the annealing time is 20~40min.

[0055] Preferably, in step (4), the vacuum evaporation deposition process has a vacuum degree < 1 × 10⁻⁶. -2 Pa, evaporation rate is 0.1~0.5 angstroms / second.

[0056] Preferably, in step (5), the vacuum evaporation deposition process has a vacuum degree < 1 × 10⁻⁶. -2 Pa, evaporation rate is 0.1~0.5 angstroms / second.

[0057] Preferably, in step (6), the vacuum evaporation deposition process has a vacuum degree < 1 × 10⁻⁶. -2 Pa, evaporation rate is 0.1~0.5 angstroms / second.

[0058] Preferably, in step (6), the method for preparing the metal electrode layer can also be selected from one or more of vapor deposition, electron beam evaporation deposition, photoresist etching, and laser direct writing.

[0059] Compared with the prior art, the present invention has the following beneficial effects: 1. The hole transport layer of the present invention, through the synergistic effect of the phosphonic acid anchoring groups of 4PADCB and TMeO-PA, significantly enhances the chemical bonding strength between the hole transport layer and the conductive substrate, suppresses the spontaneous aggregation tendency of molecules on the substrate surface, improves the uniformity of the interface molecular arrangement, and transforms the surface current distribution from discrete island-shaped conductive regions to continuous and uniform highly conductive pathways, effectively avoiding the adverse effects of local conductive dead zones on hole extraction efficiency.

[0060] 2. The electron-donating substituents in the first self-assembled molecule of this invention enhance the overall HOMO energy level through an inductive effect, optimize the energy level arrangement between the hole transport layer and the perovskite light absorption layer, and significantly reduce the hole extraction barrier; simultaneously, the methoxy oxygen atom interacts with the uncoordinated Pb in the perovskite layer. 2+ Lewis acid-base coordination between ions effectively passivates defect states at the buried interface, reduces nonradiative recombination centers at the interface, and lowers nonradiative recombination losses.

[0061] 3. The hole transport layer of the present invention provides a uniform template interface for the nucleation and growth of perovskite crystals. The steric hindrance of the first self-assembled molecule and the weak interaction between the perovskite precursor regulate the nucleation density and orientation growth of the grains, promote the formation of large-grained, low-defect-density perovskite films, effectively release the residual tensile strain at the buried interface, transform the normal stress state into a compressive stress state, which is beneficial to suppress the initiation and propagation of cracks at grain boundaries, reduce the formation of interface microcracks, and improve the structural integrity of the film.

[0062] 4. This invention adopts a blending self-assembly strategy, which mixes two self-assembly molecules with different functional characteristics in a certain proportion and then forms a co-self-assembly layer on the substrate surface through a one-step spin coating and annealing process. It does not require a complicated multi-step chemical synthesis route, has good process scalability and material universality, and is suitable for large-area device fabrication and industrial application. Attached Figure Description

[0063] Figure 1 This is a schematic diagram of the perovskite solar cell structure of the present invention.

[0064] Figure 2 This is a comparison chart of the current-voltage curves of the perovskite solar cells in Example 1 and Comparative Example 1 of the present invention.

[0065] Figure 3 The diagram shows the energy levels of the perovskite solar cells of Example 1(b) and Comparative Example 1(a) of the present invention.

[0066] Figure 4 The atomic force scanning probe microscopy spectra of the perovskite solar cells of Example 1(b) and Comparative Example 1(a) of the present invention are shown. Detailed Implementation

[0067] The technical solution of the present invention will be further described and illustrated below through specific embodiments. It should be understood that the specific embodiments described herein are only for the purpose of helping to understand the present invention and are not intended to limit the scope of the present invention.

[0068] Unless otherwise specified, the raw materials used in the embodiments of the present invention are all commonly used in the art, and the methods used in the embodiments are all conventional methods in the art.

[0069] The raw materials used in this article include: The structure of TMeO-PA is shown in equation (1) below: 4PADCB, CAS No.: 2882156-63-8; its structural formula is shown in equation (2) below: The structure of CA-PA is shown in equation (3) below: MeO-PA, the structural formula is shown in equation (4) below: .

[0070] In this paper, the conductive substrate is an indium tin oxide / polyethylene naphthalate composite conductive substrate PEN / ITO, with an ITO sheet resistance of 15Ω and dimensions of 1.96cm × 1.96cm.

[0071] In this article, Cs 0.05 (FA 0.96 MA 0.04 ) 0.95 Pb(I 0.95 Br 0.05 The raw materials for the perovskite precursor solution include formamidinium iodide (FAI), methyl ammonium iodide (MAI), cesium iodide (CsI), lead iodide (PbI2) and lead bromide (PbBr2), and the solvent is a mixture of N,N-dimethylformamide (DMF) and dimethyl sulfoxide (DMSO).

[0072] In this paper, the tests included: under simulated AM1.5 sunlight conditions (light intensity of 100 mW / cm²). 2 The current-voltage curve (JV) of the perovskite solar cell device was tested by reverse scanning from 1.5V to 0.5V at a scan rate of 20mV / s.

[0073] Example 1

[0074] In this embodiment, the perovskite solar cell comprises, from bottom to top: a conductive substrate layer (approximately 1100 nm thick), a hole transport layer (TMeO-PA and 4PADCB in a molar ratio of 25:75, approximately 20 nm thick), and a perovskite light-absorbing layer (Cs). 0.05 (FA 0.96 MA 0.04 ) 0.95 Pb(I 0.95 Br 0.05 )3, thickness approximately 500nm), C 60 The electron transport layer (approximately 25 nm thick), the BCP interface control layer (approximately 6 nm thick), and the Ag metal electrode layer (approximately 100 nm thick) are all constructed.

[0075] Includes the following steps: (1) After wiping PEN / ITO clean, blow it dry with nitrogen gas, and then clean it by ultraviolet light for 30 minutes to obtain a conductive substrate layer.

[0076] (2) Preparation of hole transport layer: TMeO-PA and 4PADCB were dissolved in anhydrous ethanol at a molar ratio of 25:75 to prepare a co-self-assembly solution with a concentration of 0.8 mg / mL. The solution was dropped onto the surface of the conductive substrate ITO, spin-coated at 3000 rpm for 30 s, and annealed at 100 °C for 10 min to obtain the hole transport layer.

[0077] (3) Preparation of perovskite light-absorbing layer: Prepare Cs with a concentration of 1.67 mol / L. 0.05 (FA 0.96 MA 0.04 ) 0.95 Pb(I 0.95 Br 0.05 3. The perovskite precursor solution was dropped onto the surface of the hole transport layer and spin-coated at 4000 rpm for 30 s. 15 s after the start of spin-coating, 600 μL of anhydrous diethyl ether (DE) was dropped onto the perovskite wet film for anti-solvent treatment. Then, it was annealed at 100 °C for 30 min to obtain the perovskite light absorption layer.

[0078] (4) Preparation of the electron transport layer: The sample from step (3) is placed in a vacuum evaporation coating apparatus, and the vacuum degree reaches 9×10 -3 After Pa, C was deposited at an evaporation rate of 0.2 Å / s. 60 Thus, the electron transport layer is obtained.

[0079] (5) Preparation of the interface control layer: The sample from step (4) is placed in a vacuum evaporation coating device, and the vacuum degree reaches 9×10 -3 After Pa, BCP was deposited at an evaporation rate of 0.2 Å / s to obtain the interface control layer.

[0080] (6) Preparation of the metal electrode layer: The sample from step (5) is placed in a vacuum evaporation coating apparatus, and the vacuum degree reaches 9×10⁻⁶. -3 After Pa, metallic Ag was deposited at an evaporation rate of 2 Å / s to obtain an Ag metal electrode layer.

[0081] Based on the above steps, a perovskite solar cell with an effective area of ​​0.06 cm² was obtained. 2 .

[0082] A schematic diagram of the perovskite solar cell in this embodiment is shown below. Figure 1 .

[0083] The performance of the perovskite solar cell in this embodiment was tested, and the results are shown in Table 1.

[0084] Example 2

[0085] In this embodiment, the perovskite solar cell comprises, from bottom to top: a conductive substrate layer (approximately 1100 nm thick), a hole transport layer (TMeO-PA and 4PADCB in a molar ratio of 10:90, approximately 20 nm thick), and a perovskite light-absorbing layer (Cs). 0.05 (FA 0.96 MA 0.04 ) 0.95 Pb(I 0.95 Br 0.05 )3, thickness approximately 500nm), C 60 The electron transport layer (approximately 25 nm thick), the BCP interface control layer (approximately 6 nm thick), and the Ag metal electrode layer (approximately 100 nm thick) are all constructed.

[0086] Includes the following steps: (1) Same as step (1) in Example 1.

[0087] (2) Follow the steps (2) of Example 1, except that the molar ratio of TMeO-PA to 4PADCB is 10:90.

[0088] (3) Same as step (3) in Example 1.

[0089] (4) Same as step (4) in Example 1.

[0090] (5) Same as step (5) in Example 1.

[0091] (6) Same as step (6) in Example 1.

[0092] Based on the above steps, a perovskite solar cell with an effective area of ​​0.06 cm² was obtained. 2 .

[0093] The performance of the perovskite solar cell in this embodiment was tested, and the results are shown in Table 1.

[0094] Example 3 In this embodiment, the perovskite solar cell comprises, from bottom to top: a conductive substrate layer (approximately 1100 nm thick), a hole transport layer (TMeO-PA and 4PADCB molar ratio of 20:80, approximately 20 nm thick), and a perovskite light-absorbing layer (Cs). 0.05 (FA 0.96 MA 0.04 ) 0.95 Pb(I 0.95 Br 0.05 )3, thickness approximately 500nm), C 60 The electron transport layer (approximately 25 nm thick), the BCP interface control layer (approximately 6 nm thick), and the Ag metal electrode layer (approximately 100 nm thick) are all constructed.

[0095] Includes the following steps: (1) Same as step (1) in Example 1.

[0096] (2) Follow the steps (2) of Example 1, except that the molar ratio of TMeO-PA to 4PADCB is 20:80.

[0097] (3) Same as step (3) in Example 1.

[0098] (4) Same as step (4) in Example 1.

[0099] (5) Same as step (5) in Example 1.

[0100] (6) Same as step (6) in Example 1.

[0101] Based on the above steps, a perovskite solar cell with an effective area of ​​0.06 cm² was obtained. 2 .

[0102] The performance of the perovskite solar cell in this embodiment was tested, and the results are shown in Table 1.

[0103] Example 4

[0104] In this embodiment, the perovskite solar cell comprises, from bottom to top: a conductive substrate layer (approximately 1100 nm thick), a hole transport layer (TMeO-PA and 4PADCB in a molar ratio of 30:70, approximately 20 nm thick), and a perovskite light-absorbing layer (Cs). 0.05 (FA 0.96 MA 0.04 ) 0.95 Pb(I 0.95 Br 0.05 )3, thickness approximately 500nm), C 60 The electron transport layer (approximately 25 nm thick), the BCP interface control layer (approximately 6 nm thick), and the Ag metal electrode layer (approximately 100 nm thick) are all constructed.

[0105] Includes the following steps: (1) Same as step (1) in Example 1.

[0106] (2) Follow the steps (2) of Example 1, except that the molar ratio of TMeO-PA to 4PADCB is 30:70.

[0107] (3) Same as step (3) in Example 1.

[0108] (4) Same as step (4) in Example 1.

[0109] (5) Same as step (5) in Example 1.

[0110] (6) Same as step (6) in Example 1.

[0111] Based on the above steps, a perovskite solar cell with an effective area of ​​0.06 cm² was obtained. 2 .

[0112] The performance of the perovskite solar cell in this embodiment was tested, and the results are shown in Table 1.

[0113] Example 5

[0114] In this embodiment, the perovskite solar cell comprises, from bottom to top: a conductive substrate layer (approximately 1100 nm thick), a hole transport layer (TMeO-PA and 4PADCB in a molar ratio of 40:60, approximately 20 nm thick), and a perovskite light-absorbing layer (Cs). 0.05 (FA 0.96 MA 0.04 ) 0.95 Pb(I 0.95 Br 0.05 )3, thickness approximately 500nm), C 60 The electron transport layer (approximately 25 nm thick), the BCP interface control layer (approximately 6 nm thick), and the Ag metal electrode layer (approximately 100 nm thick) are all constructed.

[0115] Includes the following steps: (1) Same as step (1) in Example 1.

[0116] (2) Follow the steps (2) of Example 1, except that the molar ratio of TMeO-PA to 4PADCB is 40:60.

[0117] (3) Same as step (3) in Example 1.

[0118] (4) Same as step (4) in Example 1.

[0119] (5) Same as step (5) in Example 1.

[0120] (6) Same as step (6) in Example 1.

[0121] Based on the above steps, a perovskite solar cell with an effective area of ​​0.06 cm² was obtained. 2 .

[0122] The performance of the perovskite solar cell in this embodiment was tested, and the results are shown in Table 1.

[0123] Example 6

[0124] In this embodiment, the perovskite solar cell comprises, from bottom to top: a conductive substrate layer (approximately 1100 nm thick), a hole transport layer (TMeO-PA and 4PADCB in a molar ratio of 50:50, approximately 20 nm thick), and a perovskite light-absorbing layer (Cs). 0.05 (FA 0.96 MA 0.04 ) 0.95 Pb(I 0.95 Br 0.05 )3, thickness approximately 500nm), C 60 The electron transport layer (approximately 25 nm thick), the BCP interface control layer (approximately 6 nm thick), and the Ag metal electrode layer (approximately 100 nm thick) are all constructed.

[0125] Includes the following steps: (1) Same as step (1) in Example 1.

[0126] (2) Follow the steps (2) of Example 1, except that the molar ratio of TMeO-PA to 4PADCB is 50:50.

[0127] (3) Same as step (3) in Example 1.

[0128] (4) Same as step (4) in Example 1.

[0129] (5) Same as step (5) in Example 1.

[0130] (6) Same as step (6) in Example 1.

[0131] Based on the above steps, a perovskite solar cell with an effective area of ​​0.06 cm² was obtained. 2 .

[0132] The performance of the perovskite solar cell in this embodiment was tested, and the results are shown in Table 1.

[0133] Example 7

[0134] In this embodiment, the perovskite solar cell comprises, from bottom to top: a conductive substrate layer (approximately 1100 nm thick), a hole transport layer (TMeO-PA and 4PADCB molar ratio of 25:75, approximately 20 nm thick), and a perovskite light-absorbing layer (FA). 0.85 MA 0.15 Cs 0.05 PbI3 (approximately 500 nm thick), C 60 The electron transport layer (approximately 25 nm thick), the BCP interface control layer (approximately 6 nm thick), and the Ag metal electrode layer (approximately 100 nm thick) are all constructed.

[0135] Includes the following steps: (1) Same as step (1) in Example 1.

[0136] (2) Same as step (2) in Example 1.

[0137] (3) Follow the steps (2) of Example 1, except that the perovskite precursor solution is FA. 0.85 MA 0.15 Cs 0.05 PbI3.

[0138] (4) Same as step (4) in Example 1.

[0139] (5) Same as step (5) in Example 1.

[0140] (6) Same as step (6) in Example 1.

[0141] Based on the above steps, a perovskite solar cell with an effective area of ​​0.06 cm² was obtained. 2 .

[0142] The performance of the perovskite solar cells in this comparative example was tested, and the results are shown in Table 1.

[0143] Comparative Example 1 In this comparative example, the perovskite solar cell, from bottom to top, includes: a conductive substrate layer (approximately 1100 nm thick), a hole transport layer (only 4PADCB, without TMeO-PA, approximately 20 nm thick), and a perovskite light-absorbing layer (Cs). 0.05 (FA 0.96 MA 0.04 ) 0.95 Pb(I 0.95 Br 0.05 )3, thickness approximately 500nm), C 60 The electron transport layer (approximately 25 nm thick), the BCP interface control layer (approximately 6 nm thick), and the Ag metal electrode layer (approximately 100 nm thick) are all constructed.

[0144] Includes the following steps: (1) Same as step (1) in Example 1.

[0145] (2) Preparation of hole transport layer: 4PADCB was dissolved in anhydrous ethanol to prepare a self-assembled solution with a concentration of 0.8 mg / mL. The solution was dropped onto the surface of the conductive substrate ITO, spin-coated at 3000 rpm for 30 s, and then annealed at 100 °C for 10 min to obtain the hole transport layer.

[0146] (3) Same as step (3) in Example 1.

[0147] (4) Same as step (4) in Example 1.

[0148] (5) Same as step (5) in Example 1.

[0149] (6) Same as step (6) in Example 1.

[0150] Based on the above steps, a perovskite solar cell with an effective area of ​​0.06 cm² was obtained. 2 .

[0151] The performance of the perovskite solar cells in this comparative example was tested, and the results are shown in Table 1.

[0152] Comparative Example 2 In this comparative example, the perovskite solar cell, from bottom to top, includes: a conductive substrate layer (approximately 1100 nm thick), a hole transport layer (only TMeO-PA, without 4PADCB, approximately 20 nm thick), and a perovskite light-absorbing layer (Cs). 0.05 (FA 0.96 MA 0.04 ) 0.95 Pb(I 0.95 Br 0.05 )3, thickness approximately 500nm), C 60 The electron transport layer (approximately 25 nm thick), the BCP interface control layer (approximately 6 nm thick), and the Ag metal electrode layer (approximately 100 nm thick) are all constructed.

[0153] Includes the following steps: (1) Same as step (1) in Example 1.

[0154] (2) Preparation of hole transport layer: TMeO-PA was dissolved in anhydrous ethanol to prepare a self-assembly solution with a concentration of 0.8 mg / mL. The solution was dropped onto the surface of the conductive substrate ITO, spin-coated at 3000 rpm for 30 s, and then annealed at 100 °C for 10 min to obtain the hole transport layer.

[0155] (3) Same as step (3) in Example 1.

[0156] (4) Same as step (4) in Example 1.

[0157] (5) Same as step (5) in Example 1.

[0158] (6) Same as step (6) in Example 1.

[0159] Based on the above steps, a perovskite solar cell with an effective area of ​​0.06 cm² was obtained. 2 .

[0160] The performance of the perovskite solar cells in this comparative example was tested, and the results are shown in Table 1.

[0161] Comparative Example 3 In this comparative example, the perovskite solar cell, from bottom to top, includes: a conductive substrate layer (approximately 1100 nm thick), a hole transport layer (only TMeO-PA, without 4PADCB, approximately 20 nm thick), and a perovskite light-absorbing layer (FA). 0.85 MA 0.15 Cs 0.05 PbI3 (approximately 500 nm thick), C 60 The electron transport layer (approximately 25 nm thick), the BCP interface control layer (approximately 6 nm thick), and the Ag metal electrode layer (approximately 100 nm thick) are all constructed.

[0162] Includes the following steps: (1) Same as step (1) in Example 1.

[0163] (2) Same as step (2) in Comparative Example 2.

[0164] (3) Follow the steps (2) of Example 1, except that the perovskite precursor solution is FA. 0.85 MA 0.15 Cs 0.05 PbI3.

[0165] (4) Same as step (4) in Example 1.

[0166] (5) Same as step (5) in Example 1.

[0167] (6) Same as step (6) in Example 1.

[0168] Based on the above steps, a perovskite solar cell with an effective area of ​​0.06 cm² was obtained. 2 .

[0169] The performance of the perovskite solar cells in this comparative example was tested, and the results are shown in Table 1.

[0170] Comparative Example 4 In this comparative example, the perovskite solar cell, from bottom to top, includes: a conductive substrate layer (approximately 1100 nm thick), a hole transport layer (CA-PA and 4PADCB molar ratio of 25:75, approximately 20 nm thick), and a perovskite light-absorbing layer (Cs). 0.05 (FA 0.96 MA 0.04 ) 0.95 Pb(I 0.95 Br 0.05 )3, thickness approximately 500nm), C 60 The electron transport layer (approximately 25 nm thick), the BCP interface control layer (approximately 6 nm thick), and the Ag metal electrode layer (approximately 100 nm thick) are all constructed.

[0171] Includes the following steps: (1) Same as step (1) in Example 1.

[0172] (2) Preparation of hole transport layer: CA-PA and 4PADCB were dissolved in anhydrous ethanol at a molar ratio of 25:75 to prepare a self-assembled solution with a concentration of 0.8 mg / mL. The solution was dropped onto the surface of the conductive substrate ITO, spin-coated at 3000 rpm for 30 s, and then annealed at 100 °C for 10 min to obtain the hole transport layer.

[0173] (3) Same as step (3) in Example 1.

[0174] (4) Same as step (4) in Example 1.

[0175] (5) Same as step (5) in Example 1.

[0176] (6) Same as step (6) in Example 1.

[0177] Based on the above steps, a perovskite solar cell with an effective area of ​​0.06 cm² was obtained. 2 .

[0178] The performance of the perovskite solar cells in this comparative example was tested, and the results are shown in Table 1.

[0179] Comparative Example 5 In this comparative example, the perovskite solar cell, from bottom to top, includes: a conductive substrate layer (approximately 1100 nm thick), a hole transport layer (MeO-PA and 4PADCB molar ratio of 25:75, approximately 20 nm thick), and a perovskite light-absorbing layer (Cs). 0.05 (FA 0.96 MA 0.04 ) 0.95 Pb(I 0.95 Br 0.05 )3, thickness approximately 500nm), C 60 The electron transport layer (approximately 25 nm thick), the BCP interface control layer (approximately 6 nm thick), and the Ag metal electrode layer (approximately 100 nm thick) are all constructed.

[0180] Includes the following steps: (1) Same as step (1) in Example 1.

[0181] (2) Preparation of hole transport layer: MeO-PA and 4PADCB were dissolved in anhydrous ethanol at a molar ratio of 25:75 to prepare a self-assembled solution with a concentration of 0.8 mg / mL. The solution was dropped onto the surface of the conductive substrate ITO, spin-coated at 3000 rpm for 30 s, and then annealed at 100 °C for 10 min to obtain the hole transport layer.

[0182] (3) Same as step (3) in Example 1.

[0183] (4) Same as step (4) in Example 1.

[0184] (5) Same as step (5) in Example 1.

[0185] (6) Same as step (6) in Example 1.

[0186] Based on the above steps, a perovskite solar cell with an effective area of ​​0.06 cm² was obtained. 2 .

[0187] The performance of the perovskite solar cells in this comparative example was tested, and the results are shown in Table 1.

[0188] Table 1. Performance Test Table of Perovskite Solar Cells

[0189] According to Table 1 and Figures 2-4 It is known that the present invention employs TMeO-PA and 4PADCB co-self-assembly to form a uniform and dense co-self-assembled layer on the substrate surface through intermolecular synergistic effects. 4PADCB provides strong anchoring and deep HOMO energy levels, while TMeO-PA provides phosphonic acid anchoring, electron-donating methoxy groups, and steric hindrance. The two complement each other to achieve synergistic effects of interface strengthening, energy level optimization, defect passivation, and crystallization regulation, which significantly improves the photoelectric conversion efficiency of the device.

[0190] Comparative Example 1 uses only 4PADCB as the hole transport layer. Since single molecules are prone to spontaneous aggregation on the ITO surface, the interface coverage is uneven, forming local conductive dead zones. At the same time, the lack of functional end groups of second self-assembled molecules results in weak interface defect passivation ability and crystal template effect. Figure 3 In Comparative Example 1, the perovskite solar cell exhibits lower band bending, creating an energy barrier that hinders hole extraction. Conversely, the perovskite solar cell based on TMeO-PA in Example 1 shows upper band bending at the interface, with an energy shift of only 0.73 eV, which greatly promotes interface hole transfer. Figure 4 In Comparative Example 1, the RMS of the perovskite light-absorbing layer film was 25.5 nm, while in Example 1, the RMS was 16.4 nm, indicating a significant decrease in surface roughness. This demonstrates that the buried interface modified by TMeO-PA makes the perovskite light-absorbing layer film smoother and more even, effectively reducing the roughness of the perovskite film.

[0191] Comparative Examples 2 and 3 used only TMeO-PA as the hole transport layer. Although TMeO-PA has two phosphonic acid anchoring groups and a carbazole ring, it lacks the deep HOMO energy level and extended conjugated core provided by 4PADCB, thus limiting the hole extraction efficiency. Comparative Example 4 used CA-PA (without methoxy substitution), and Comparative Example 5 used MeO-PA (with monomethoxy substitution), both of which had weaker electron-donating effects and defect passivation capabilities.

[0192] In summary, this invention constructs a high-precision, ordered co-self-assembled hole transport system on an ITO surface by blending TMeO-PA molecules containing two phosphonic acid anchoring groups, electron-donating methoxy groups, and steric hindrance with 4PADCB molecules containing a single phosphonic acid group and then performing a one-step spin-coating annealing process. The synergistic multi-point anchoring of the two / single phosphonic acids strengthens interfacial bonding and inhibits molecular aggregation to form a continuous, highly conductive pathway. Simultaneously, the methoxy group optimizes the energy level arrangement and passivates Pb. 2+ Defects are reduced to lower the hole extraction barrier and nonradiative recombination loss, while the steric hindrance effect provides a uniform template for perovskite crystallization, promotes large grain growth, and converts residual tensile strain into compressive stress to improve film integrity. This simple and universal blending strategy drives the comprehensive enhancement of the buried interface in terms of mechanical bonding, charge extraction, defect suppression, and stress release, ultimately endowing perovskite solar cells with excellent photoelectric performance and long-term operational stability.

[0193] All aspects, embodiments, and features of this invention should be considered illustrative in all respects and not limiting of the invention; the scope of the invention is defined only by the claims. Other embodiments, modifications, and uses will become apparent to those skilled in the art without departing from the spirit and scope of the invention as claimed.

[0194] In the preparation method of this invention, the order of the steps is not limited to the listed order. For those skilled in the art, variations in the order of the steps without creative effort are also within the scope of protection of this invention. Furthermore, two or more steps or actions can be performed simultaneously.

[0195] Finally, it should be noted that the specific embodiments described herein are merely illustrative examples of the invention and are not intended to limit the implementation of the invention. Those skilled in the art can make various modifications or additions to the described specific embodiments or use similar methods to replace them; it is neither necessary nor possible to exemplify all embodiments here. However, these obvious variations or modifications derived from the essential spirit of the invention still fall within the scope of protection of the invention, and interpreting them as any additional limitation would contradict the spirit of the invention.

Claims

1. A hole transport material for driving the strengthening of buried interfaces, characterized in that, Its raw materials include a first self-assembled molecule and a second self-assembled molecule in a molar ratio of 1:(1~9); The first self-assembled molecule is 9-(3,4,5-trimethoxyphenyl)-9H-carbazole-2,7-diphosphonic acid. The second self-assembled molecule is [4-(7H-dibenzocarbazole-7-yl)butyl]phosphonic acid; The structural formulas of the first self-assembled molecule and the second self-assembled molecule are shown in Equation (1) and Equation (2) respectively: 。 2. A perovskite solar cell, characterized in that, From bottom to top, it includes: a conductive substrate layer, a hole transport layer, a perovskite light absorption layer, an electron transport layer, an interface modulation layer, and a metal electrode layer. The hole transport layer is a co-self-assembly layer, and the raw materials of the co-self-assembly layer include a first self-assembly molecule and a second self-assembly molecule in a molar ratio of 1:(1~9). The structural formulas of the first self-assembled molecule and the second self-assembled molecule are shown in Equation (1) and Equation (2) respectively: 。 3. The perovskite solar cell according to claim 2, characterized in that, The conductive substrate layer is an indium tin oxide / polyethylene naphthalate composite conductive substrate PEN / ITO.

4. The perovskite solar cell according to claim 2, characterized in that, The perovskite light-absorbing layer comprises a perovskite material; The perovskite material has ABX3 crystals, wherein A is selected from formamidinium cation FA. + methylammonium cation MA + Cesium ions (Cs) + Rubidium ion Rb + One or more of them, where B is selected from lead ions (Pb). 2+ Tin ions (Sn) 2+ One or more of them, where X is selected from chloride ions (Cl). - Bromide ions (Br) - Iodide ions - thiocyanate ions (SCN) - One or more of them.

5. The perovskite solar cell according to claim 2, characterized in that, The material of the electron transport layer is selected from C. 60 The material of the interface control layer is 2,9-dimethyl-4,7-diphenyl-1,10-phenanthroline; the metal in the metal electrode layer is selected from one or more of Ag, Al, Au and Cu.

6. A method for preparing a perovskite solar cell as described in claim 2, characterized in that, Includes the following steps: (1) Pretreatment of the conductive substrate layer; (2) Dissolve the first self-assembled molecule and the second self-assembled molecule with a molar ratio of 1:(1~9) in an organic solvent to obtain a co-self-assembled solution, spin-coat it onto the surface of the conductive substrate layer in step (1), and anneal it to obtain a hole transport layer. (3) Spin-coat the perovskite precursor solution onto the surface of the hole transport layer in step (2), add antisolvent during the spin-coating process, and anneal to obtain the perovskite light absorption layer; (4) Vacuum evaporation deposition is performed on the surface of the perovskite light-absorbing layer in step (3) to obtain the electron transport layer; (5) Vacuum evaporation deposition is performed on the surface of the electron transport layer in step (4) to obtain the interface control layer; (6) Vacuum evaporation deposition is performed on the surface of the interface control layer in step (5) to obtain a metal electrode layer.

7. The method for preparing a perovskite solar cell according to claim 6, characterized in that, In step (1), the pretreatment includes: wiping the indium tin oxide / polyethylene naphthalate composite conductive substrate in sequence, drying it with nitrogen, and cleaning it with ultraviolet light.

8. The method for preparing a perovskite solar cell according to claim 6, characterized in that, In step (2), the concentration of the co-self-assembly solution is 0.1~1.5 mg / mL; The spin coating speed is 1000~5000 rpm, and the time is 10~60s; The annealing temperature is 80~120℃, and the annealing time is 5~30min.

9. The method for preparing a perovskite solar cell according to claim 6, characterized in that, In step (3), the preparation method of the perovskite light absorption layer includes: spin-coating a perovskite precursor solution with a concentration of 0.5~3.0 mol / L onto the surface of the hole transport layer, adding an anti-solvent during the spin-coating process, and then annealing; The spin coating speed is 2000~8000 rpm, and the time is 10~120s; The antisolvent is added dropwise 1-20 seconds after the start of spin coating; The antisolvent is one or more of anhydrous diethyl ether, chlorobenzene, and toluene; The annealing temperature is 80~120℃, and the annealing time is 10~60min.

10. The method for preparing a perovskite solar cell according to claim 6, characterized in that, In steps (4-6), the vacuum evaporation deposition process has a vacuum degree < 1×10⁻⁶. -2 Pa, evaporation rate is 0.1~0.5 angstroms / second.