Tin-based perovskite thin films, methods of making, applications, and thin film transistors

By using a single saturated carbide ring ammonium ion additive, the fabrication process of tin-based perovskite thin films was simplified, solving the problems of complexity and poor repeatability in existing technologies, and realizing high-quality thin films and thin-film transistors with good stability.

CN123165012APending Publication Date: 2026-11-24JILIN UNIVERSITY
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202611655925.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-26
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing methods for preparing tin-based perovskite thin films are complex and have poor reproducibility. Furthermore, the use of various organic ammonium salt additives leads to a decline in electrical performance and a narrow process window. The antisolvent drop-addition process is difficult to achieve large-area preparation and industrialization.

Method used

Tin-based perovskite films were prepared by spin coating and annealing using a single saturated carbocyclic ammonium ion additive, eliminating the need for anti-solvent processing, promoting polycrystalline film crystallization and improving repeatability.

Benefits of technology

The prepared tin-based perovskite thin film has low defect density and a smooth surface, which significantly improves the mobility and electrical cycling stability of thin film transistors, with a mobility retention rate of over 90%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123165012A_ABST
    Figure CN123165012A_ABST
Patent Text Reader

Abstract

This invention relates to the field of organic-inorganic hybrid semiconductor materials and thin-film transistors, specifically providing a tin-based perovskite thin film, its preparation method, and its applications. The preparation method includes the following steps: dissolving saturated carbocyclic ammonium iodide, formamidinium iodide (FAI), stannous iodide (SnI2), and stannous fluoride (SnF2) in a mixed solvent according to a stoichiometric ratio, and stirring at room temperature to obtain a precursor solution; the saturated carbocyclic ammonium cation in the saturated carbocyclic ammonium iodide is a cation with a saturated carbocyclic ammonium group directly connected to an ammonium group or a cation with an ammonium group connected via a C1-C3 alkyl group; depositing the precursor solution onto a substrate by spin coating to form a wet film; and annealing the wet film to obtain the perovskite thin film. The tin-based perovskite thin film has the advantages of high crystallinity and low defect density, which significantly improves the carrier mobility and operating stability of its thin-film transistor devices, and helps to promote the development and industrial application of perovskite thin-film transistors.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of organic-inorganic hybrid semiconductor materials and thin-film transistors, specifically providing a tin-based perovskite thin film, its preparation method, applications, and a thin-film transistor. Background Technology

[0002] Organic and inorganic metal halide perovskites have attracted widespread attention in recent years due to their excellent photoelectric properties, such as in solar cells, light-emitting diodes, photodetectors, and thin-film transistors. Sn-based perovskites are promising candidate materials, not only because of their environmentally friendly characteristics, but also because of their low effective mass, strong intrinsic charge transport properties, and low exciton binding energy. Therefore, tin-based perovskites have been extensively developed.

[0003] However, due to the strong p-type self-doping induced by natural Sn vacancies, Sn 2+ It is easily oxidized to Sn 4+ Furthermore, the rapid crystallization rate of Sn-based perovskites can lead to a decline in film quality, making the preparation of stable tin-based perovskite films a challenge. To address this issue, several effective strategies have been developed, including composition engineering, surface passivation, and solvent engineering.

[0004] Introducing bulk organic ammonium salts into perovskites is an effective method to improve film quality. As a bulky cation, the bulk organic ammonium cation causes the three-dimensional octahedral layers of perovskites to split, thereby forming a two-dimensional phase. The specific literature, High-Mobility and Bias-Stable Field-Effect Transistors Based on Lead-Free Formamidinium Tin Iodide Perovskites (published in ACS Energy Letters, Vol. 8, No. 10, 2023, pp. 4496–4505), shows that these two-dimensional phases can delay the crystallization of the three-dimensional phase and act as templates to induce film growth, thereby regulating film orientation and effectively reducing the defect density of the film.

[0005] In previous technologies, such as the patent "A method for preparing a quasi-two-dimensional perovskite thin film and its application in a transistor" (Chinese Invention Patent, Publication No.: CN120500248A, Publication Date: 2025.08.15) and the literature "Elucidation of the Formation Mechanism of Highly Oriented Multiphase Ruddlesden" PopperPerovskite Solar Cells (Published in ACS Energy Letters, Volume 6, Issue 1, 2021, Page 249) (260) Large-volume organic ammonium salts are commonly used to improve the quality of perovskite films, but this brings the following problems: First, a large amount of organic ammonium salt needs to be added, and the incorporation of a large amount of organic matter will reduce the electrical performance of the film. Second, studies have found that most organic ammonium salts tend to accumulate at the bottom of the film during film formation. This bottom enrichment has limited effect on the overall crystallization of perovskite and, on the other hand, acts as a trap, adversely affecting the conductive channel at the bottom of the transistor. Third, this method often requires the synergistic effect of different types of organic ammonium salts, necessitating precise control of the ratio between components, resulting in a narrow process window and increasing the difficulty and cost of the process. Fourth, existing preparation methods usually employ anti-solvent drop-addition processes (such as adding anti-solvents such as chlorobenzene or diethyl ether during spin coating) to induce rapid nucleation of perovskite. The anti-solvent drop-addition process has extremely strict requirements on parameters such as operating time, drop volume, and drop position, resulting in poor process repeatability and hindering large-area preparation and industrial applications. Summary of the Invention

[0006] In view of this, the present invention aims to provide a tin-based perovskite thin film, its preparation method, application, and thin-film transistor; specifically, addressing the current situation of complex processes and poor repeatability, the tin-based perovskite thin film preparation method provided by the present invention utilizes saturated carbocyclic ammonium salt as a single-component additive, which not only simplifies the process but also avoids the use of anti-solvent processes, thereby improving the repeatability of thin film and device preparation. The resulting polycrystalline tin-based perovskite thin film is smooth and dense, and its thin-film transistor device performance is significantly improved.

[0007] To achieve the above objectives, the technical solution created by this invention is implemented as follows: This invention provides a method for preparing a tin-based perovskite thin film, the method comprising the following steps: S1. Saturated carbocyclic amine iodide, formamidinium iodide (FAI), stannous iodide (SnI2) and stannous fluoride (SnF2) are dissolved in a mixed solvent in stoichiometric ratio and stirred at room temperature to obtain a precursor solution; S2. The precursor solution is deposited on the substrate by spin coating to form a wet film; the wet film is annealed to obtain a perovskite thin film.

[0008] Furthermore, the saturated carbocyclic ammonium iodide includes a saturated carbocyclic ammonium cation, wherein the saturated carbocyclic ammonium cation is a cation in which a saturated carbocyclic ring is directly linked to an ammonium group or a cation in which an ammonium group is linked via a C1-C3 alkyl group; the general chemical formula of the saturated carbocyclic ammonium cation is R. x -Cm H 2m-1-x -C n H 2n -NH3 + In this denominator, R represents a substituent, x represents the number of substituents, m represents the number of first carbon atoms, and n represents the number of second carbon atoms; R is independently selected from one or more of hydrogen, fluorine, or trifluoromethyl; x is an integer from 0 to 2; m is an integer from 3 to 6; and n is an integer from 0 to 3; the saturated carbocyclic ammonium cation does not contain aromatic ring structures or straight-chain aliphatic hydrocarbon structures.

[0009] Furthermore, the saturated carbocyclic ammonium cation is selected from cyclohexylammonium (CyHA). + Cyclohexylmethylammonium (CyHMA) + Cyclohexylethylammonium (CyHEA) + 4,4-Difluorocyclohexylmethylammonium (DFCHMA) + 4-Trifluoromethylcyclohexylammonium CF3CHA + Cypentylammonium (CyPentA) + Cyclobutylammonium (CyBA) + Or cyclopropylammonium CyPA + At least one of them.

[0010] Furthermore, the stoichiometric ratio of the saturated carbocyclic ammonium iodide, the formamidinium iodide (FAI), the stannous iodide (SnI2), and the stannous fluoride (SnF2) is (0.01~0.12):1:1:0.1; the molar concentration of the saturated carbocyclic ammonium iodide is 1%~12% of the molar concentration of the stannous iodide (SnI2); and the concentration of the stannous iodide (SnI2) in the precursor solution ranges from 0.2 mol / L to 0.4 mol / L.

[0011] Furthermore, the mixed solvent includes N,N-dimethylformamide (DMF) and dimethyl sulfoxide (DMSO), the volume ratio of N,N-dimethylformamide (DMF) to dimethyl sulfoxide (DMSO) is in the range of (5:1) to (3:1), the stirring time at room temperature is 10 h to 14 h, the substrate is a Si / SiO2 substrate, a glass substrate or a flexible polymer substrate, and the annealing temperature range is 60 °C to 70 °C.

[0012] The present invention also provides a tin-based perovskite thin film, which is prepared by the above-described method for preparing tin-based perovskite thin films of the present invention.

[0013] Furthermore, the thickness of the tin-based perovskite film is 10 nm to 100 nm.

[0014] The present invention also provides an application of the tin-based perovskite thin film described above, wherein the tin-based perovskite thin film is applied in a thin-film transistor, and the perovskite thin film serves as a semiconductor layer in the thin-film transistor.

[0015] Furthermore, the thin-film transistor is a bottom-gate top contact structure, a bottom-gate bottom contact structure, a top-gate bottom contact structure, or a top-gate top contact structure.

[0016] The present invention also provides a thin film transistor, including a gate, a dielectric layer, a semiconductor layer, a source, and a drain, wherein the semiconductor layer of the thin film transistor includes the tin-based perovskite thin film described above in the present invention; the thin film transistor retains a mobility of ≥90% after 50 electrical cycle tests.

[0017] Compared with the prior art, the present invention can achieve the following beneficial effects: (1) Using a single saturated carbocyclic ammonium ion additive can promote the crystallization of polycrystalline thin films and eliminate the process step of adding antisolvent: During the crystallization of perovskite, saturated carbocyclic ammonium ions can be evenly distributed in the perovskite wet film and play a role in promoting the crystallization of perovskite. This eliminates the operation step of adding antisolvent, and the prepared film has a low defect density and improves the repeatability of different product batches.

[0018] (2) Significantly improved grain orientation in the film: By adding saturated carbocyclic organic ammonium ion additives, XRD test showed that the grain orientation in the film was significantly improved. The prepared film surface was smooth and flat, the grains were closely connected, the coverage was increased, and it had a high degree of crystallinity.

[0019] (3) The two-dimensional phase is uniformly distributed in the perovskite film: the PL ratio of the two-dimensional phase / three-dimensional phase at the top and bottom of the film is approximately the same under different additive concentrations, indicating that the phase distribution of the perovskite film is uniform, avoiding the phase separation problem caused by using multiple additives, and the operation is simple.

[0020] (4) The performance and stability of thin film transistor devices are significantly improved: the perovskite thin film transistors prepared by the method of the present invention exhibit high field-effect mobility and high electrical cycling stability; compared with the traditional PEAI additive scheme, the mobility of the thin film transistors prepared by this scheme is 14 times that of the traditional PEAI additive scheme, and the retention rate after 50 cycles is improved by more than 15%. Attached Figure Description

[0021] The accompanying drawings, which form part of this invention, are used to provide a further understanding of the invention. The illustrative embodiments and descriptions of the invention are used to explain the invention and do not constitute an undue limitation of the invention. In the drawings: Figure 1 A schematic diagram of the bottom-gate top-contact thin-film transistor structure in a specific embodiment of the present invention; Figure 2 X-ray diffraction patterns of tin-based perovskite thin films prepared in Examples 1, 2 and Comparative Example 1 of this invention; Figure 3 Fluorescence spectra of tin-based perovskite thin films prepared in Example 2 and Comparative Example 2 of this invention; Figure 4 Atomic force microscopy images of the tin-based perovskite thin films prepared in Examples 1, 3 and 4 of this invention; Figure 5 Cyclic test curves of bottom-gate top-contact thin-film transistors prepared from the tin-based perovskite thin film obtained in Comparative Example 3 were created for this invention. Figure 6 Transfer curves of bottom-gate top-contact thin-film transistors prepared from the tin-based perovskite thin films obtained in Examples 5 and 6 of this invention; Figure 7 Cyclic test curve of the bottom-gate top-contact thin-film transistor prepared from the tin-based perovskite thin film obtained in Example 7 of this invention; Figure 8 X-ray diffraction patterns of tin-based perovskite thin films prepared in Examples 8 and 9 of this invention; Figure 9 An atomic force microscope image of the tin-based perovskite thin film prepared in Example 10 of this invention; Figure 10 Transfer curve of a bottom-gate top-contact thin-film transistor prepared from the tin-based perovskite thin film obtained in Example 10 of this invention; Figure 11 Cyclic test curve of the bottom gate top contact thin film transistor prepared from the tin-based perovskite thin film obtained in Example 10 of the present invention; Figure 12 Transfer curve of a bottom-gate top-contact thin-film transistor prepared from the tin-based perovskite thin film obtained in Example 13 of this invention; Figure 13 Transfer curve of a bottom-gate top-contact thin-film transistor prepared from the tin-based perovskite thin film obtained in Example 16 of this invention; Figure 14 An atomic force microscope image of the tin-based perovskite thin film prepared in Example 17 of this invention; Figure 15 Transfer curve of a bottom-gate top-contact thin-film transistor prepared from the tin-based perovskite thin film obtained in Example 18 of this invention; Figure 16 The transfer curve of the bottom gate top contact thin film transistor prepared from the tin-based perovskite thin film obtained in Example 20 of this invention.

[0022] Figure label: Gate 1, dielectric layer 2, active semiconductor layer 3, source and drain 4. Detailed Implementation

[0023] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to the accompanying drawings and specific embodiments. It should be understood that the specific embodiments described herein are merely illustrative of the invention and do not constitute a limitation thereof.

[0024] It should be noted that, unless otherwise specified, the embodiments and features described in the present invention can be combined with each other.

[0025] In the description of this invention, it should be understood that the terms "first," "second," etc., are used for descriptive purposes only and should not be construed as indicating or implying relative importance or implicitly specifying the number of indicated technical features. Therefore, a feature defined with "first," "second," etc., may explicitly or implicitly include one or more of that feature. In the description of this invention, unless otherwise stated, "a plurality of" means two or more.

[0026] This invention provides a tin-based perovskite thin film, the preparation method of which includes the following steps: S1. Saturated carbocyclic amine iodide, formamidinium iodide (FAI), stannous iodide (SnI2) and stannous fluoride (SnF2) are dissolved in a mixed solvent in stoichiometric ratio and stirred at room temperature to obtain a precursor solution; In a specific embodiment, the saturated carbocyclic ammonium iodide includes a saturated carbocyclic ammonium cation, which is a cation in which a saturated carbocyclic ammonium ring is directly connected to an ammonium group or a cation in which an ammonium group is connected via a C1-C3 alkyl group; specifically, it is a cation in which a saturated carbocyclic ammonium ring with different substituents or without substituents is directly connected to an ammonium group or a cation in which an ammonium group is connected via a C1-C3 alkyl group; the general chemical formula of the saturated carbocyclic ammonium cation is R. x -C m H 2m-1-x -C n H 2n -NH3 + In this formula, R represents a substituent, x represents the number of substituents, m represents the number of the first carbon atom (i.e., the number of the first carbon atom in the general chemical formula), and n represents the number of the second carbon atom (i.e., the number of the second carbon atom in the general chemical formula); R is independently selected from one or more of hydrogen, fluorine, or trifluoromethyl; x is an integer from 0 to 2; m is an integer from 3 to 6; and n is an integer from 0 to 3; the saturated carbocyclic ammonium cation does not contain aromatic ring structures or straight-chain aliphatic hydrocarbon structures.

[0027] In a further preferred embodiment, the saturated carbocyclic ammonium iodide is selected from at least one of cyclohexylammonium iodide, cyclohexylmethylammonium iodide, cyclohexylethylammonium iodide, 4,4-difluorocyclohexylmethylammonium iodide, 4-trifluoromethylcyclohexylammonium iodide, cyclopentylammonium iodide, cyclobutylammonium iodide, or cyclopropylammonium iodide. The organic cations contained in these organic ammonium salts can precipitate uniformly during perovskite crystallization, thus better promoting crystallization and improving film quality. Specifically, as shown in Table 1, the saturated carbocyclic ammonium cation is selected from cyclohexylammonium (CyHA). + Cyclohexylmethylammonium (CyHMA) + Cyclohexylethylammonium (CyHEA) + 4,4-Difluorocyclohexylmethylammonium (DFCHMA) + 4-Trifluoromethylcyclohexylammonium CF3CHA + Cypentylammonium (CyPentA) + Cyclobutylammonium (CyBA) + Or cyclopropylammonium CyPA + At least one of them.

[0028] Table 1

[0029] In a specific embodiment, the stoichiometric ratio of the saturated carbocyclic ammonium iodide, the formamidinium iodide (FAI), the stannous iodide (SnI2), and the stannous fluoride (SnF2) is (0.01~0.12):1:1:0.1; the molar concentration of the saturated carbocyclic ammonium iodide is 1%~12% of the molar concentration of the stannous iodide (SnI2); and the concentration of the stannous iodide (SnI2) in the precursor solution ranges from 0.2 mol / L to 0.4 mol / L.

[0030] The mixed solvent includes N,N-dimethylformamide (DMF) and dimethyl sulfoxide (DMSO), and the volume ratio of N,N-dimethylformamide (DMF) to dimethyl sulfoxide (DMSO) is in the range of (5:1) to (3:1); the stirring time at room temperature is 10 h to 14 h.

[0031] S2. The precursor solution is deposited onto a substrate by spin coating to form a wet film; the wet film is then annealed to obtain a perovskite thin film. Specifically, the substrate is a Si / SiO2 substrate, a glass substrate, or a flexible polymer substrate; the annealing temperature range is 60℃~70℃.

[0032] Under these preferred conditions, the tin-based perovskite film prepared by spin coating has high crystallinity and a flat and dense grain arrangement.

[0033] The method for preparing tin-based perovskite thin films provided in this invention regulates the crystallization of perovskite thin films by introducing different saturated carbocyclic ammonium cation additives. During spin coating, saturated carbocyclic ammonium ions can be uniformly dispersed in the wet perovskite film, and can effectively promote crystallization during annealing. The resulting tin-based perovskite thin films have the advantages of high crystallinity and low defect density, which significantly improves the carrier mobility and operating stability of their thin-film transistor devices, and helps to promote the development and industrial application of perovskite thin-film transistors.

[0034] The method for preparing tin-based perovskite thin films provided in the specific embodiments of the present invention has the following advantages: First, it eliminates the process of adding antisolvent, as the harsh process of adding antisolvent reduces the yield of the prepared devices. Adding additives to the precursor solution is beneficial to the uniformity of device performance. Second, it improves the efficiency of the additives. This uniform dispersion characteristic allows the additives to better contact the perovskite octahedral layer, enabling the production of smooth and full polycrystalline perovskite thin films by adding only a small amount of saturated carbocyclic ammonium salt. Third, the method is simple. Adding a single organic ammonium salt additive to the precursor solution is simple, efficient, and easy to implement.

[0035] In a specific embodiment of the present invention, a tin-based perovskite thin film is also provided, which is prepared by the above-described method for preparing tin-based perovskite thin films. The thickness of the tin-based perovskite thin film ranges from 10 nm to 100 nm, and more preferably from 60 to 80 nm. Using this thickness range as a semiconductor layer is more conducive to carrier transport. Specifically, in the tin-based perovskite thin film, PL spectroscopy detection of the upper and lower surfaces shows that the intensity ratio of the two-dimensional phase characteristic peak (~690 nm) to the three-dimensional phase characteristic peak (~875 nm) is 0.8 to 1.2 on the upper and lower surfaces, indicating that the two-dimensional phase is uniformly distributed in the upper and lower layers of the film.

[0036] In a specific embodiment of the present invention, an application of the tin-based perovskite thin film described above is also provided. The tin-based perovskite thin film is applied in a thin-film transistor, where the perovskite thin film serves as the semiconductor layer of the thin-film transistor. Specifically, the thin-film transistor is a bottom-gate-top contact structure, a bottom-gate-bottom contact structure, a top-gate-bottom contact structure, or a top-gate-top contact structure.

[0037] In a specific embodiment of the present invention, a thin-film transistor is also provided, comprising: the semiconductor layer of the thin-film transistor comprising the tin-based perovskite thin film of the present invention described above; silicon (Si) can be used as the gate, silicon dioxide (SiO2) as the dielectric layer, and gold electrode (Au) as the source and drain; the thin-film transistor retains a mobility of ≥90% after 50 electrical cycle tests.

[0038] The invention will now be described in detail with reference to the accompanying drawings and embodiments.

[0039] Example 1 In this embodiment, cyclohexylmethylammonium (CyHMA) is used. + In this embodiment, the saturated carbocyclic ammonium iodide used to prepare the tin-based perovskite thin film is cyclohexylmethylammonium iodide (CyHMAI), and the saturated carbocyclic ammonium cation is cyclohexylmethylammonium (CyHMA). + .

[0040] Step (1) Preparation of precursor solution: CyHMAI, FAI, SnI2, and SnF2 were dissolved in a mixed solvent of DMF / DMSO (volume ratio 4:1) at a stoichiometric ratio of 0.12:1:1:0.1 and stirred at room temperature for 12 h to prepare a 0.25 mol / L precursor solution. + The concentration was 12%.

[0041] Step (2) Thin film preparation: The above precursor solutions are deposited on the Si / SiO2 substrate by spin coating to form a wet film, and then annealed to obtain a tin-based perovskite thin film.

[0042] Example 2 The difference from Example 1 is that the stoichiometric ratio of CyHMAI, FAI, SnI2, and SnF2 is 0.06:1:1:0.1, resulting in a precursor solution. The precursor solution contains CyHMAI... + The concentration was 6%.

[0043] Example 3 The difference from Example 1 is that the stoichiometric ratio of CyHMAI, FAI, SnI2, and SnF2 is 0.08:1:1:0.1, resulting in a precursor solution. The precursor solution contains CyHMAI... + The concentration was 8%.

[0044] Example 4 The difference from Example 1 is that the stoichiometric ratio of CyHMAI, FAI, SnI2, and SnF2 is 0.04:1:1:0.1, resulting in a precursor solution. The precursor solution contains CyHMAI... + The concentration was 4%.

[0045] Comparative Example 1 PEAI, FAI, SnI2, and SnF2 were dissolved in a DMF / DMSO mixture (volume ratio 4:1) at a stoichiometric ratio of 0.06:1:1:0.1 and stirred at room temperature for 12 h to prepare a 0.25 mol / L precursor solution. The precursor solution contained PEA...+ The concentration was 6%; tin-based perovskite films were prepared using the same method as in Example 1.

[0046] Comparative Example 2 The difference from Comparative Example 1 is that the stoichiometric ratio of PEAI, FAI, SnI2, and SnF2 is 0.12:1:1:0.1, resulting in a precursor solution. The precursor solution contains PEA... + The concentration was 12%.

[0047] The thicknesses of the tin-based perovskite films prepared in Examples 1, 2, 3, 4, Comparative Example 1, and Comparative Example 2 were 71 nm, 68 nm, 73 nm, 70 nm, 66 nm, and 74 nm, respectively.

[0048] The X-ray diffraction patterns of the tin-based perovskite films prepared in Examples 1, 2, and Comparative Example 1 are shown below. Figure 2 As shown in the figure, it can be seen that in CyHMA + Under the influence of the above, the tin-based perovskite films prepared in Examples 1 and 2 will eventually form a three-dimensional phase (2 ≈13.9 / 27.8) and two-dimensional phases with n=2 (2 (≈3.9), although this method cannot avoid introducing a small amount of two-dimensional phase, the peak intensity of the three-dimensional phase is significantly improved compared with Comparative Example 1, indicating that CyHMA + Compared to PEA + It has a more effective effect in promoting crystallization.

[0049] The fluorescence spectra of the tin-based perovskite films prepared in Example 2 and Comparative Example 2, emitted from above and below, are shown in the figures. Figure 3 As shown in the figure, the peaks near 405 nm and 810 nm correspond to the excitation source, the peak near 690 nm represents the two-dimensional phase (n=2), and the peak near 875 nm represents the three-dimensional phase. In Comparative Example 2, the film with 12% PEAI added mainly exhibits a low-dimensional phase distributed in the lower layer. In contrast, the film with 12% CyHMA added in Example 2... + In the thin film, a two-dimensional phase with n=2 was detected in both the upper and lower layers. The intensity ratio of the characteristic peaks of the two-dimensional phase to those of the three-dimensional phase was 1:0.9 on the upper and lower surfaces of the film. This indicates that CyHMA crystallized during the crystallization process. + The film is relatively uniformly distributed in both the upper and lower layers, and can play a role in inducing the crystallization of three-dimensional phases.

[0050] The surface morphologies of the tin-based perovskite films prepared in Examples 1, 3, and 4 are as follows: Figure 4As shown in the figure, dense films with smooth surfaces were obtained at different concentrations in the tin-based perovskite films prepared in different embodiments. With decreasing proportions of saturated carbocyclic ammonium ions, the grain diameter tended to increase, and the grain density decreased. However, even at a concentration of 4%, tight connections between grains were still observed. This indicates that in the preparation method of the tin-based perovskite film provided in the embodiments of the present invention, CyHMA... + The addition of CyHMAI promotes the crystallization of thin films. This promoting effect gradually weakens as the addition ratio decreases. After adding CyHMAI, the tight connection between grains ensures the transport of charge carriers between grains.

[0051] Example 5 like Figure 1 The diagram shown is a schematic representation of the thin-film transistor structure in this embodiment, wherein heavily doped silicon (Si(p)) is used. ++ The gate electrode is SiO2, the dielectric layer is SiO2, the active semiconductor layer is the tin-based perovskite thin film prepared in Example 1, and Au is used as the source and drain electrode. Specifically, gold (Au) electrodes are deposited using a mask through vacuum evaporation to serve as the source and drain electrode 4, thereby obtaining... Figure 1 The thin-film transistor shown has a bottom-gate top-contact structure.

[0052] Example 6 The difference from Example 5 is that the tin-based perovskite thin film prepared in Example 4 is used as the active semiconductor layer 3.

[0053] Example 7 The difference from Example 5 is that the tin-based perovskite thin film prepared in Example 2 is used as the active semiconductor layer 3.

[0054] Comparative Example 3 The difference from Example 5 is that the tin-based perovskite thin film prepared in Comparative Example 1 is used as the active semiconductor layer 3.

[0055] like Figure 5 The figure shows the cycle test curves of the thin-film transistor corresponding to Comparative Example 3. It can be seen from the figure that the mobility of the first curve is 1.5 cm⁻¹. 2 v -1 s -1 The cycle retention rate (50th test migration rate / first test migration rate) was 73%.

[0056] like Figure 6 The figure shows the transfer curves of the thin-film transistors corresponding to Examples 5 and 6. It can be seen from the figure that the field-effect mobility reaches 22 cm⁻¹ at a concentration of 4%. 2 v -1 s -1This result demonstrates that CyHMA at low concentrations... + The induced crystallization behavior that it still possesses is beneficial for manufacturing high-performance semiconductor layer materials.

[0057] like Figure 7 The figure shows the cycling test curves of the thin-film transistor corresponding to Example 7. It can be seen from the figure that the mobility of the first curve is 21 cm⁻¹. 2 v -1 s -1 The 50-cycle test demonstrates that this thin-film transistor exhibits excellent operational stability, with a cycle retention rate of 91.5%. In comparison, CyHMA... + This effectively improves the operational stability of perovskite thin-film transistors.

[0058] Example 8 In this embodiment, cyclohexylethylammonium (CyHEA) is used. + In this embodiment, the saturated carbocyclic ammonium iodide used is cyclohexylethylammonium (CyHEAI), and the saturated carbocyclic ammonium cation is cyclohexylethylammonium (CyHEA). + .

[0059] Step (1) Preparation of precursor solution: CyHEAI, FAI, SnI2, and SnF2 were dissolved in a mixed solvent of DMF / DMSO (volume ratio 4:1) at a stoichiometric ratio of 0.12:1:1:0.1 to prepare a 0.2 mol / L precursor solution. + The concentration was 12%.

[0060] Step (2) Thin film preparation: The above precursor solutions are deposited on the Si / SiO2 substrate by spin coating to form a wet film, and then annealed to obtain a tin-based perovskite thin film.

[0061] Example 9 The difference from Example 1 is that the stoichiometric ratio of CyHEAI, FAI, SnI2, and SnF2 is 0.06:1:1:0.1, resulting in a precursor solution. The precursor solution contains CyHEAI... + The concentration was 6%.

[0062] Example 10 The difference from Example 1 is that the stoichiometric ratio of CyHEAI, FAI, SnI2, and SnF2 is 0.08:1:1:0.1, resulting in a precursor solution. The precursor solution contains CyHEAI... + The concentration was 8%.

[0063] The thicknesses of the tin-based perovskite films prepared in Examples 8, 9, and 10 were 72 nm, 67 nm, and 70 nm, respectively.

[0064] The X-ray diffraction patterns of the tin-based perovskite films prepared in Examples 8 and 9 are shown below. Figure 8 As shown in the figure, it can be seen that in CyHEA + Under the influence of the above, the tin-based perovskite films prepared in Examples 8 and 9 will eventually form a two-dimensional phase with n=2 (2 ≈3.9) and three-dimensional phase (2 (≈13.9 / 27.8), although this method introduces a small amount of two-dimensional phase, the high intensity of the three-dimensional peaks indicates the good crystal quality of the three-dimensional phase.

[0065] An atomic force microscope image of the tin-based perovskite thin film prepared in Example 10 is shown below. Figure 9 As shown in the figure, a dense film with small intergranular gaps was obtained at this concentration, indicating that CyHEA... + It has the effect of inducing the crystallization of tin-based perovskites; Figure 10 The figure shows the transfer curve of the bottom-gate top-contact thin-film transistor prepared from the tin-based perovskite thin film obtained in Example 10. It can be seen from the figure that in CyHEA... + Under the influence of [the specific technology / mechanism], the field-effect mobility of the perovskite thin-film transistor corresponding to Example 10 is 6.8 cm⁻¹. 2 v -1 s -1 ; Figure 11 The figure shows the cycling test curves of the bottom-gate top-contact thin-film transistor prepared from the tin-based perovskite thin film obtained in Example 10. As can be seen from the figure, the 50-cycle test indicates that it has excellent working stability.

[0066] Example 11 The difference from Example 5 is that the tin-based perovskite thin film prepared in Example 10 is used as the active semiconductor layer 3.

[0067] Example 12 In this embodiment, cyclohexylammonium (CyHA) is used. + In this embodiment, the saturated carbocyclic ammonium iodide used is cyclohexylammonium iodide (CyHAI), and the saturated carbocyclic ammonium cation is cyclohexylammonium (CyHA). + .

[0068] Step (1) Preparation of precursor solution: CyHAI, FAI, SnI2, and SnF2 were dissolved in a mixed solvent of DMF / DMSO (volume ratio 4:1) at a stoichiometric ratio of 0.12:1:1:0.1 and stirred at room temperature for 12 h to prepare a 0.25 mol / L precursor solution. + The concentration was 12%.

[0069] Step (2) Thin film preparation: The above precursor solution is deposited on a Si / SiO2 substrate by spin coating to form a wet film, and then annealed to obtain a tin-based perovskite thin film.

[0070] Example 13 The difference from Example 12 is that the stoichiometric ratio of CyHAI, FAI, SnI2, and SnF2 is 0.04:1:1:0.1, resulting in a precursor solution. The precursor solution contains CyHAI... + The concentration was 4%.

[0071] The thicknesses of the tin-based perovskite films prepared in Examples 12 and 13 were 66 nm and 69 nm, respectively.

[0072] Example 14 The difference from Example 5 is that the tin-based perovskite thin film prepared in Example 13 is used as the active semiconductor layer 3.

[0073] The transfer curve of the effect transistor corresponding to Example 13 is as follows: Figure 12 As shown in the figure, it can be seen that in CyHA + Under the influence of [the specific effect], the field-effect mobility of the perovskite thin-film transistor is 3.2 cm⁻¹. 2 v -1 s -1 .

[0074] Example 15 In this embodiment, 4,4-difluorocyclohexylmethylammonium (DFCHMA) is used. + The preparation of tin-based perovskite thin films was controlled by specific parameters. In this example, the saturated carbocyclic ammonium iodide used was 4,4-difluorocyclohexylmethylammonium iodide (DFCHMAI), and the saturated carbocyclic ammonium cation included was 4,4-difluorocyclohexylmethylammonium (DFCHMAI). + .

[0075] Step (1) Preparation of precursor solution: DFCHMAI, FAI, SnI2, and SnF2 were dissolved in a mixed solvent of DMF / DMSO (volume ratio 4:1) at a stoichiometric ratio of 0.06:1:1:0.1 and stirred at room temperature for 12 h to prepare a 0.3 mol / L precursor solution.+ The concentration was 6%.

[0076] Step (2) Thin film preparation: The above precursor solutions are deposited on the Si / SiO2 substrate by spin coating to form a wet film, and then annealed to obtain a tin-based perovskite thin film.

[0077] The thickness of the tin-based perovskite film prepared in Example 15 was 72 nm.

[0078] Example 16 The difference from Example 5 is that the tin-based perovskite thin film prepared in Example 15 is used as the active semiconductor layer 3.

[0079] The transfer curve of the thin-film transistor corresponding to Example 16 is as follows: Figure 13 As shown in the figure, its field-effect mobility reaches 21.2 cm⁻¹. 2 v -1 s -1 This indicates that DFCHMA + It promotes the crystallization of tin-based perovskite thin films, which is beneficial to the fabrication of perovskite thin film transistors.

[0080] Example 17 In this embodiment, cyclopentylammonium (CyPentA) is used. + In this embodiment, the saturated carbocyclic ammonium iodide used is cyclopentylammonium iodide (CyPentAI), and the saturated carbocyclic ammonium cation is cyclopentylammonium (CyPentA). + .

[0081] Step (1) Preparation of precursor solution: CyPentAI, FAI, SnI2, and SnF2 were dissolved in a mixed solvent of DMF / DMSO (volume ratio 4:1) at a stoichiometric ratio of 0.12:1:1:0.1 and stirred at room temperature for 12 h to prepare a 0.25 mol / L precursor solution. + The concentration was 12%.

[0082] Step (2) Thin film preparation: The above precursor solutions are deposited on the Si / SiO2 substrate by spin coating to form a wet film, and then annealed to obtain a tin-based perovskite thin film.

[0083] The thickness of the tin-based perovskite film prepared in Example 17 is 68 nm.

[0084] The surface morphology of the tin-based perovskite thin film prepared in Example 17 is as follows: Figure 14 As shown in the figure, CyPentA +It can also promote the formation of dense films, but the grain height varies considerably.

[0085] Example 18 The difference from Example 5 is that the tin-based perovskite thin film prepared in Example 17 is used as the active semiconductor layer 3.

[0086] The transfer curve of the perovskite thin-film transistor corresponding to Example 18 is as follows: Figure 15 As shown in the figure, the mobility of this perovskite thin-film transistor is 8.3 cm⁻¹. 2 v -1 s -1 .

[0087] Example 19 In this embodiment, cyclopropylammonium (CyPA) is used. + In this embodiment, the saturated carbocyclic ammonium iodide used is cyclopropylammonium iodide (CyPI), and the saturated carbocyclic ammonium cation is cyclopropylammonium (CyPA). + .

[0088] Step (1) Preparation of precursor solution: CyPI, FAI, SnI2, and SnF2 were dissolved in a mixed solvent of DMF / DMSO (volume ratio 4:1) at a stoichiometric ratio of 0.08:1:1:0.1 and stirred at room temperature for 12 h to prepare a 0.4 mol / L precursor solution. + The concentration is 8%.

[0089] Step (2) Thin film preparation: The above precursor solutions are deposited on the Si / SiO2 substrate by spin coating to form a wet film, and then annealed to obtain a tin-based perovskite thin film.

[0090] The thickness of the tin-based perovskite film prepared in Example 19 is 73 nm.

[0091] Example 20 The difference from Example 5 is that the tin-based perovskite thin film prepared in Example 19 is used as the active semiconductor layer 3.

[0092] The transfer curve of the perovskite thin-film transistor corresponding to Example 20 is as follows: Figure 16 As shown in the figure, the mobility of this perovskite thin-film transistor is 4.5 cm⁻¹. 2 v -1 s -1 .

[0093] The test results of the above embodiments and comparative examples fully demonstrate that the tin-based perovskite thin film prepared by the special preparation method of the present invention has the advantages of high crystallinity and low defect density, which significantly improves the carrier mobility and working stability of its thin film transistor device, and helps to promote the development and industrial application of perovskite thin film transistors.

[0094] It is understood that the above description is only a preferred embodiment of the present invention and does not constitute a limitation on the scope of protection of the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.

Claims

1. A method for preparing a tin-based perovskite thin film, characterized in that: The method for preparing the tin-based perovskite thin film includes the following steps: S1. Saturated carbocyclic amine iodide, formamidinium iodide (FAI), stannous iodide (SnI2) and stannous fluoride (SnF2) are dissolved in a mixed solvent in stoichiometric ratio and stirred at room temperature to obtain a precursor solution; S2. The precursor solution is deposited onto a substrate by spin coating to form a wet film; The wet film is annealed to obtain a perovskite thin film.

2. The method for preparing tin-based perovskite thin films according to claim 1, characterized in that: Saturated carbocyclic ammonium iodides include saturated carbocyclic ammonium cations, wherein the saturated carbocyclic ammonium cation is a cation in which a saturated carbocyclic ring is directly linked to an ammonium group or a cation in which an ammonium group is linked via a C1-C3 alkyl group; the general chemical formula of the saturated carbocyclic ammonium cation is R. x -C m H 2m-1-x -C n H 2n -NH3 + In this denominator, R represents a substituent, x represents the number of substituents, m represents the number of first carbon atoms, and n represents the number of second carbon atoms; R is independently selected from one or more of hydrogen, fluorine, or trifluoromethyl; x is an integer from 0 to 2; m is an integer from 3 to 6; and n is an integer from 0 to 3; the saturated carbocyclic ammonium cation does not contain aromatic ring structures or straight-chain aliphatic hydrocarbon structures.

3. The method for preparing tin-based perovskite thin films according to claim 2, characterized in that: The saturated carbocyclic ammonium cation is selected from cyclohexylammonium (CyHA). + Cyclohexylmethylammonium (CyHMA) + Cyclohexylethylammonium (CyHEA) + 4,4-Difluorocyclohexylmethylammonium (DFCHMA) + 4-Trifluoromethylcyclohexylammonium CF3CHA + Cypentylammonium (CyPentA) + Cyclobutylammonium (CyBA) + Or cyclopropylammonium CyPA + At least one of them.

4. The method for preparing tin-based perovskite thin films according to claim 1, characterized in that: The stoichiometric ratio of the saturated carbocyclic ammonium iodide, the formamidinium iodide (FAI), the stannous iodide (SnI2), and the stannous fluoride (SnF2) is (0.01~0.12):1:1:0.1; the molar concentration of the saturated carbocyclic ammonium iodide is 1%~12% of the molar concentration of the stannous iodide (SnI2); and the concentration of the stannous iodide (SnI2) in the precursor solution ranges from 0.2 mol / L to 0.4 mol / L.

5. The method for preparing tin-based perovskite thin films according to claim 1, characterized in that: The mixed solvent includes N,N-dimethylformamide (DMF) and dimethyl sulfoxide (DMSO), wherein the volume ratio of N,N-dimethylformamide (DMF) to dimethyl sulfoxide (DMSO) is in the range of (5:1) to (3:1); the stirring time at room temperature is 10 h to 14 h; the substrate is a Si / SiO2 substrate, a glass substrate, or a flexible polymer substrate; and the annealing temperature range is 60 °C to 70 °C.

6. A tin-based perovskite thin film, characterized in that: The tin-based perovskite thin film is prepared by the method for preparing tin-based perovskite thin films according to any one of claims 1 to 5.

7. The tin-based perovskite thin film according to claim 6, characterized in that: The thickness of the tin-based perovskite film is 10 nm to 100 nm.

8. An application of a tin-based perovskite thin film according to any one of claims 6 or 7, characterized in that: The tin-based perovskite film is used in a thin-film transistor, whereby the perovskite film serves as the semiconductor layer in the thin-film transistor.

9. The application of the tin-based perovskite thin film according to claim 8, characterized in that: The thin-film transistor is a bottom-gate-top contact structure, a bottom-gate-bottom contact structure, a top-gate-bottom contact structure, or a top-gate-top contact structure.

10. A thin-film transistor, comprising a gate, a dielectric layer, a semiconductor layer, a source, and a drain, characterized in that: The semiconductor layer of the thin-film transistor comprises the tin-based perovskite thin film as described in any one of claims 6 or 7; the thin-film transistor retains a mobility of ≥90% after 50 electrical cycle tests.

Citation Information

Patent Citations

  • Preparation method of quasi-two-dimensional perovskite thin film and application of quasi-two-dimensional perovskite thin film in transistor

    CN120500248A