Perovskite thin film and preparation method thereof, and perovskite solar cell
By introducing FACl as a functional additive into perovskite films through vapor deposition, and combining component compensation, diffusion kinetics regulation, and crystallization optimization, the problems of component imbalance and disordered crystallization in vapor deposition were solved, achieving efficient preparation of perovskite films and synergistic improvement of device performance.
Patent Information
- Application Number
- CN202611424450.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-14
- Publication Date
- 2026-11-24
AI Technical Summary
Existing vapor deposition methods for preparing perovskite thin films suffer from problems such as precursor deposition rate mismatch, compositional imbalance, disordered crystallization, high defect density, and insufficient device stability, failing to meet the requirements for large-area mass production and long-term stability.
An organic salt layer, a functional additive layer, and an inorganic salt layer are deposited on a substrate using a layer-by-layer sequential thermal evaporation process, followed by annealing. FACl is used as a functional additive to regulate composition, diffusion kinetics, and crystallization, thereby improving film quality and device performance stability.
By controlling the composition of the perovskite film with FAC1, the crystal quality is improved, the grain size is increased, the number of grain boundaries is reduced, the defect state density is decreased, and the photoelectric conversion efficiency of the device is increased from 19.20% to 22.06%.
Smart Images

Figure CN123165013A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of perovskite solar cell technology, specifically to a perovskite thin film and its preparation method, and a perovskite solar cell. Background Technology
[0002] Perovskite solar cells, with their excellent photoelectric performance and low manufacturing cost, have become an important development direction for next-generation photovoltaic technology. The main methods for preparing perovskite thin films include solution methods and vacuum evaporation methods. Solution methods require organic solvents, which leads to problems such as solvent residue, uneven film thickness, and poor batch-to-batch repeatability, making it difficult to meet the demands of large-area mass production. Vacuum evaporation methods, on the other hand, offer advantages such as solvent-free production, high film uniformity, large-area fabrication capability, and good batch stability. They are well-suited for industrial-scale vacuum processes and are currently one of the most commercially viable perovskite solar cell fabrication technologies.
[0003] However, conventional vapor deposition processes still have the following defects: (1) When multiple precursors are co-deposited, due to the significant differences in saturated vapor pressure, volatilization temperature, and sublimation rate of different precursors, it is difficult to accurately match the deposition rate of multi-source precursors. This can easily lead to compositional imbalance problems such as iodine vacancies, lead enrichment, and organic component deficiency in the formed perovskite film, which increases the defect state density of the film, intensifies non-radiative recombination, reduces open-circuit voltage and photoelectric conversion efficiency, and causes large performance differences between batches; (2) Vapor deposition is a pure physical deposition process, lacking solvent-assisted mild crystallization control methods. The precursor molecules nucleate quickly on the substrate surface, and the grain growth is disordered. The resulting films generally have problems such as small grains, dense grain boundaries, insufficient density, and large surface roughness, which not only hinders carrier transport but also easily becomes a permeation channel for water vapor and oxygen, weakening the environmental stability of the film; (3) The bulk phase and the upper phase of the vapor-deposited film are not uniform. The lower interface has a large number of uncoordinated metal ions, halogen vacancies and other defects. The existing process lacks effective passivation methods for vapor deposition systems, resulting in prominent interface recombination loss and poor energy level matching, which restricts the further improvement of device performance. (4) Perovskite materials themselves are photothermal sensitive. Under continuous light and high temperature working conditions, ion migration, organic component volatilization and crystal phase transformation are easy to occur. The thin film prepared by conventional vapor deposition process is due to uneven composition, many grain boundary defects and loose structure. It cannot effectively suppress photoinduced ion migration and thermal structural collapse. The device is prone to rapid efficiency decay and performance degradation during long-term operation. Most of the existing control technology is designed for solution system and cannot be adapted to vacuum solventless vapor deposition process. There are problems such as poor control effect, low compatibility and easy introduction of impurity defects. It cannot fundamentally solve the industry bottleneck that the efficiency and stability of vapor-deposited perovskite batteries are difficult to improve in a coordinated manner.
[0004] Therefore, there is an urgent need to provide a perovskite thin film preparation method that is compatible with vapor phase evaporation processes, can precisely control the thin film composition, crystallization behavior and defect state, and simultaneously improve the optoelectronic performance and long-term stability of devices. Summary of the Invention
[0005] The purpose of this application is to provide a perovskite thin film, a method for preparing the same, and a perovskite solar cell.
[0006] The embodiments of this application can be implemented through the following technical solutions: A method for preparing a perovskite thin film includes the following steps: placing a substrate in a vacuum evaporation equipment, depositing an organic salt layer, a functional additive layer, and an inorganic salt layer on the substrate using a layer-by-layer sequential thermal evaporation process, and performing an annealing treatment after the evaporation is completed to obtain a perovskite thin film. The organic salt layer is made of FAI, the inorganic salt layer is made of CsI and PbI2, and the functional additive layer is made of FACl. The evaporation sequence is selected from any of the following: a) First, the functional additive layer is vapor-deposited, then the organic salt layer is vapor-deposited, and finally the inorganic salt layer is vapor-deposited. b) First, the organic salt layer is vapor-deposited, then the functional additive layer is vapor-deposited, and finally the inorganic salt layer is vapor-deposited. c) First, the organic salt layer is deposited by vapor deposition, then the inorganic salt layer is deposited by vapor deposition, and finally the functional additive layer is deposited by vapor deposition.
[0007] Furthermore, CsI and PbI2 in the inorganic salt layer are deposited simultaneously using a co-evaporation method.
[0008] Furthermore, the evaporation sequence is as follows: first, the organic salt layer is evaporated; then, the functional additive layer is evaporated; and finally, the inorganic salt layer is evaporated.
[0009] Furthermore, the evaporation rate of the functional additive layer is 0.2~5 Å / s, and the evaporation time is 5~30 min.
[0010] Furthermore, the annealing temperature is 110~170℃, and the annealing time is 5~30min.
[0011] Furthermore, the organic salt layer has a film thickness of 500 nm, the inorganic salt layer has a film thickness of 500 nm; and / or, the functional additive layer has a film thickness of 5~300 nm.
[0012] Furthermore, the composition of the perovskite thin film is FA. 1-x Cs x PbI3, of which .
[0013] Furthermore, the vacuum degree of the thermal evaporation is less than... .
[0014] A perovskite thin film, said perovskite thin film being prepared by the method described in any one of the preceding claims.
[0015] A perovskite solar cell includes a transparent conductive substrate, a hole transport layer, a perovskite layer, an electron transport layer, a hole blocking layer, and a back electrode, which are stacked sequentially from bottom to top; the perovskite layer is the perovskite thin film described above.
[0016] The perovskite thin film and its preparation method, as well as the perovskite solar cell provided in this application embodiment, have at least the following beneficial effects: This application introduces FACl as a functional additive during the vapor deposition of perovskite thin films. Utilizing the vapor-depositability of FACl, it combines multiple mechanisms such as component compensation, diffusion kinetics regulation, crystallization optimization, and interfacial grain boundary passivation. Without altering the main crystalline phase of the perovskite, it achieves improved film quality and synergistic enhancement of device photoelectric performance and photothermal stability. After FACl regulation, the component segregation problem of the perovskite precursor is effectively alleviated, and the elemental composition of the film is more uniform. Simultaneously, the crystallinity of the perovskite film is significantly improved, with increased grain size, reduced grain boundary number, increased film density, and effectively reduced defect state density. The device's photoelectric conversion efficiency increases from 19.20% without the additive to 22.06%.
[0017] The perovskite thin film preparation process of this application is fully compatible with existing vacuum thermal evaporation equipment. It requires no hardware modification and no introduction of any solvent. It can be achieved simply by adjusting the FACl evaporation sequence and its process parameters. It is simple to operate, highly repeatable, and suitable for promotion and application in the preparation of large-area perovskite devices. Attached Figure Description
[0018] Figure 1 This is a comparison chart of the photoelectric conversion efficiency of devices obtained under different precursor evaporation stacking sequences in the embodiments of this application; Figure 2 This is a comparison chart of the photoelectric conversion efficiency of devices obtained under different FACl evaporation times in the embodiments of this application; Figure 3 This is a comparison chart of the photoelectric conversion efficiency of devices obtained at different FACl evaporation rates in the embodiments of this application; Figure 4 This is a comparison chart of the photoelectric conversion efficiency of devices obtained under different annealing times of perovskite thin films in the embodiments of this application; Figure 5 This is a comparison chart of the photoelectric conversion efficiency of devices obtained at different perovskite thin film annealing temperatures according to the embodiments of this application. Detailed Implementation
[0019] The present application will now be further described based on preferred embodiments and with reference to the accompanying drawings.
[0020] In the description of the embodiments of this application, it should be noted that if the terms "upper", "lower", "inner", "outer" or other terms indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings, or the orientation or positional relationship that the product of this application is usually placed in during use, they are only for the convenience of describing this application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation, and therefore should not be construed as a limitation of this application.
[0021] The vocabulary used in this specification is for illustrative purposes and is not intended to limit the scope of this application. It should also be noted that, unless otherwise expressly specified and limited, the terms "set," "connected," and "linked" should be interpreted broadly. For example, they can refer to a fixed connection, a detachable connection, or an integral connection; they can refer to a mechanical connection, a direct connection, or an indirect connection via an intermediate medium; or they can refer to the internal communication between two components. Those skilled in the art will understand the specific meaning of these terms in this application.
[0022] Unless otherwise specified, the experimental methods used in the embodiments of this application are all conventional methods, and the materials and reagents used are all commercially available unless otherwise specified.
[0023] As described in the background section, existing vapor deposition methods for preparing perovskite thin films suffer from problems such as precursor deposition rate mismatch, compositional imbalance, disordered crystallization, high defect density, and insufficient device stability. To address these issues, this application provides a method for preparing perovskite thin films, comprising the following steps: placing a substrate in a vacuum evaporation apparatus, depositing an organic salt layer, a functional additive layer, and an inorganic salt layer on the substrate using a layer-by-layer sequential thermal evaporation process, and performing annealing treatment after evaporation to obtain the perovskite thin film. The organic salt layer is made of formamidinium hydroiodide (FAI), the inorganic salt layer is made of lead iodide (PbI2) and cesium iodide (CsI), and the functional additive layer is made of formamidinium hydrochloride (FACl). The vapor deposition sequence can be selected from any of the following three: first vapor deposition of the FAI layer, then vapor deposition of the FAI layer, and finally vapor deposition of the inorganic salt layer; first vapor deposition of the FAI layer, then vapor deposition of the FAI layer, and finally vapor deposition of the inorganic salt layer; or first vapor deposition of the FAI layer, then vapor deposition of the inorganic salt layer, and finally vapor deposition of the FAI layer.
[0024] Among them, FACl, due to its suitable sublimation temperature, can be heated and sublimated in a vacuum evaporation environment and deposited in the gaseous form simultaneously with precursors such as FAI, CsI, and PbI2 into the interior of the perovskite precursor film. This compensates for the organic and halogen components in the system, improves the elemental composition of the film, alleviates the component segregation caused by the mismatch of multi-source evaporation rates, and reduces the generation of defects such as halogen vacancies and lead-related intrinsic defects from the source. During the film deposition and subsequent annealing solid-phase reaction, chloride ions with small ionic radii can play a kinetic role in solid lubrication, acting as diffusion balls and reducing the halogen content of large-size FAI precursor films. + The solid-state diffusion barrier between organic cations and the Pb-I precursor promotes the full solid-state reaction, driving the precursor to transform into the perovskite main phase and reducing unreacted impurities. Simultaneously, the lubricating effect of chloride ions alleviates the excessively rapid nucleation behavior caused by the rapid accumulation of precursor molecules, reducing the nucleation rate and providing kinetic conditions for grain growth. This increases grain size, reduces the number of grain boundaries, improves film density and surface smoothness, and reduces the obstruction of carrier transport by grain boundaries and the penetration channels for water vapor and oxygen into the film. Furthermore, most chloride ions generated by the decomposition of FACl do not embed within the perovskite lattice but tend to segregate and accumulate at grain boundaries and the upper and lower interfaces of the film due to lattice thermodynamic repulsion. These chloride ions can coordinate with uncoordinated lead ions, halogen vacancies, and other deep-level defect sites, achieving in-situ defect passivation, eliminating a large number of nonradiative recombination centers, reducing the defect state density and nonradiative recombination loss of the film, and suppressing ion migration and crystal structure degradation under illumination and thermal stress conditions. This simultaneously improves the optoelectronic performance and long-term stability of the device.
[0025] Specifically, the substrate is first cleaned and surface-treated, and then sent into a high-vacuum evaporation chamber. During the evaporation process, a quartz crystal oscillating thickness gauge (QCM) placed next to the substrate can be used to monitor the evaporation rate and deposition thickness of each material in real time to ensure that the deposition thickness and rate of each layer are accurately controllable. After the evaporation is completed, the deposited multilayer precursor film is annealed to cause solid-state reactions between the precursor layers and transform them into perovskite phase.
[0026] In some specific embodiments, the substrate includes a transparent conductive substrate, such as an ITO conductive glass substrate or an FTO conductive glass substrate, which can be subjected to multi-step ultrasonic cleaning with deionized water, ethanol, and isopropanol in sequence to fully remove oil, dust and impurities from the substrate surface. After drying, UV-ozone or plasma surface treatment is performed to improve the cleanliness and wettability of the substrate surface. In some optional embodiments, a hole transport layer can also be formed on the surface of the transparent conductive substrate before evaporating the perovskite precursor.
[0027] In some preferred embodiments, PbI2 and CsI in the inorganic salt layer are deposited simultaneously by co-evaporation. Co-evaporation allows CsI and PbI2 to be fully mixed and uniformly incorporated into the film during the deposition process, which is beneficial for obtaining a perovskite precursor film with uniform elemental distribution, thereby forming a perovskite crystal with uniform composition after annealing.
[0028] Furthermore, the thermal evaporation is performed under high vacuum conditions, with a vacuum level of less than 5 × 10⁻⁶. -4 Pa. A higher vacuum level helps reduce the interference of residual gas in the vapor deposition chamber on the deposition process, ensuring that each precursor sublimates and deposits into a film at a stable rate, thereby improving the uniformity and repeatability of the film formation.
[0029] In some preferred embodiments, the evaporation sequence is as follows: first, the FAI layer is evaporated; then, the FACl layer is evaporated; and finally, the CsI and PbI2 layers are co-evaporated, that is, the FACl functional additive layer is placed between the FAI layer and the inorganic salt layer.
[0030] Furthermore, the evaporation rate of the FACl layer is 0.2~5 Å / s, for example, it can be any value among 0.2 Å / s, 0.5 Å / s, 1 Å / s, 2 Å / s, 3 Å / s, 4 Å / s, 5 Å / s, or a range of any two of these values.
[0031] Furthermore, the evaporation time for the FACl layer is 5 to 30 minutes, for example, any value among 5 min, 10 min, 15 min, 20 min, 25 min, and 30 min, or a range of any two of these values.
[0032] Furthermore, the vapor-deposited thin film of the FAC1 layer is 5~300 nm, for example, it can be any value among 5 nm, 10 nm, 15 nm, 20 nm, 25 nm, 30 nm, 45 nm, 60 nm, 75 nm, 90 nm, 180 nm, and 300 nm, or a range of values composed of any two of these values.
[0033] Furthermore, the annealing temperature is 110~170℃, for example, it can be any value among 110℃, 120℃, 130℃, 140℃, 150℃, 160℃, and 170℃, or a range of any two of these values.
[0034] Furthermore, the annealing time is 5 to 30 minutes, for example, it can be any value among 5 min, 10 min, 15 min, 20 min, 25 min, and 30 min, or a range of any two of these values.
[0035] Furthermore, the composition of the perovskite thin film is FA. 1-x Cs x PbI3, of which By adjusting the ratio of the vapor deposition thickness of the FAI layer to the CsI+PbI2 layer, the composition of the A-site cations in the perovskite film can be flexibly adjusted. For example, in some specific embodiments, the vapor deposition thickness of the FAI layer is 500 nm, and the vapor deposition thickness of the CsI and PbI2 co-deposited layer is 500 nm. Converting the vapor deposition thickness of each precursor layer to a molar ratio, it can be seen that the molar ratio of FAI, CsI, and PbI2 is approximately 0.95:0.05:1. The composition of the perovskite film obtained after annealing is FAI+PbI2 ... 0.95 Cs 0.05 PbI3.
[0036] This application also provides a perovskite thin film, which is prepared by any of the preparation methods described above.
[0037] This application also provides a perovskite solar cell, comprising a transparent conductive substrate, a hole transport layer, a perovskite layer, an electron transport layer, a hole blocking layer, and a back electrode stacked sequentially from bottom to top; The transparent conductive substrate can be made of ITO conductive glass or FTO conductive glass to ensure good light transmittance and conductivity. Before use, it is ultrasonically cleaned sequentially with deionized water, acetone and anhydrous ethanol, dried with nitrogen, and then treated with UV-ozone or plasma to improve surface cleanliness and wettability.
[0038] A hole transport layer is disposed on a transparent conductive substrate to extract photogenerated holes and block electrons. The hole transport layer is a self-assembled monolayer (SAM), and the specific material can be (4-(7H-dibenzo[c,g]carbazole-7-yl)butyl)phosphonic acid (4PADCB). Further, the SAM layer is prepared by spin-coating: 4PADCB is dissolved in anhydrous ethanol to form a solution, which is then spin-coated onto the surface of the transparent conductive substrate, followed by annealing at 100°C for 10 min to obtain a uniform and dense SAM layer. It is understood that the specific spin-coating speed and time can be adjusted according to actual needs, and no specific limitations are imposed here.
[0039] The perovskite layer is disposed on the hole transport layer and is prepared by vacuum evaporation. Its composition is FA. 1- x Cs x For PbI3, the specific steps can be referred to the aforementioned method for preparing perovskite thin films, and will not be repeated here.
[0040] An electron transport layer is disposed on the perovskite layer to extract photogenerated electrons and block holes; specifically, the material of the electron transport layer is C.60 In some preferred embodiments, it is prepared by vacuum evaporation, with an evaporation rate of 0.20 Å / s.
[0041] A hole blocking layer is disposed on the electron transport layer to block holes from migrating toward the cathode and reduce interfacial recombination losses. Specifically, the hole blocking layer is made of BCP (Bathocuproine). In some preferred embodiments, it is prepared by vacuum evaporation at a rate of 0.10 Å / s.
[0042] The back electrode is disposed on the hole blocking layer for collecting charge carriers; specifically, the material of the back electrode is at least one of Cu, Ag or Au, preferably Cu; in some preferred embodiments, it is prepared by vacuum evaporation, with an evaporation rate of 0.50 Å / s and a thickness of 100 nm.
[0043] In some preferred embodiments, except for the hole transport layer which is prepared by spin coating, the perovskite layer, electron transport layer, hole blocking layer and back electrode of the above-mentioned perovskite solar cell are all prepared by vacuum evaporation, so that the entire device process is well compatible with the evaporation process of the perovskite layer and avoids the damage of solvent to the perovskite layer.
[0044] It is understood that the materials and preparation methods of the above layers are merely examples, and those skilled in the art can make adjustments according to actual needs, as long as the corresponding functions of each layer can be achieved.
[0045] The present application will now be described in detail with reference to specific embodiments.
[0046] In the following embodiments and comparative examples, except for the explicitly specified variations, the remaining steps and parameters are the same as in Example 1. The performance testing conditions for the devices obtained in each embodiment and comparative example are uniformly as follows: AM1.5G standard spectrum, irradiance of 100 mW / cm², ambient temperature of 25℃, and JV curves are tested using an AAA-grade solar simulator and a high-precision digital source meter. The test conditions are: starting voltage of 1.2 V, ending voltage of -0.02 V, step voltage of 0.02 V, and clamping current of 150 mA. The open-circuit voltage (VOC), short-circuit current density (JSC), fill factor (FF), and photoelectric conversion efficiency (PCE) of the devices are statistically analyzed. At least 10 devices are prepared for each group, and the average value is taken.
[0047] <Example 1> This embodiment provides a method for fabricating a perovskite solar cell, the device structure of which is ITO / SAM / perovskite / C 60 / BCP / Cu, the specific steps are as follows: Step 1, Substrate pretreatment: Select an ITO conductive glass substrate and perform multi-step ultrasonic cleaning with deionized water, ethanol and isopropanol in sequence to fully remove oil, dust and impurities from the substrate surface. After drying, perform UV-ozone or plasma surface treatment on the substrate to improve the cleanliness and wettability of the ITO surface, providing good substrate conditions for the uniform growth of the subsequent SAM layer. Step 2, Preparation of SAM hole transport layer: 4PADCB self-assembled monolayer (SAM) is prepared on the surface of the treated ITO conductive substrate. The film is formed by spin coating and then annealed at 100 °C for 10 min to obtain a uniform, dense, and energy-level matched SAM hole transport layer. Step 3, vapor phase evaporation to prepare the perovskite layer: The substrate with the prepared SAM layer is placed into a vacuum evaporation apparatus, and the vapor phase evaporation is carried out at a vacuum degree of less than 5 × 10⁻⁶. -4 Under high vacuum conditions of Pa, perovskite precursor films were prepared using a layer-by-layer sequential thermal evaporation process: FAI powder was placed in an independent quartz crucible, and the evaporation rate and film thickness were monitored in real time using a quartz crystal oscillating thickness gauge (QCM) placed next to the substrate. The FAI layer was deposited at a rate of 3 Å / s to a thickness of 500 nm (approximately 28 min). Subsequently, a functional additive layer of FACl was deposited at a rate of 0.5 Å / s for 10 min, resulting in a FACl layer thickness of approximately 30 nm. Finally, CsI and PbI2 were co-evaporated at a rate of 3 Å / s, with a total co-evaporation layer thickness of 500 nm (approximately 28 min). After evaporation, the deposited multilayer precursor film was annealed under atmospheric conditions at a temperature of 150 ℃ for 10 min, with the relative humidity controlled at 20%–30%. Converting the evaporation thickness of each precursor layer to a molar ratio, the resulting film after annealing had a composition of FA... 0.95 Cs 0.05 PbI3 perovskite thin films; Step 4, Preparation of the electron transport layer: After the perovskite layer has cooled naturally to room temperature, C is deposited on the surface of the perovskite layer in a high-vacuum evaporation equipment at a evaporation rate of 0.20 Å / s. 60 As an electron transport layer; Step 5, Prepare the hole blocking layer: In C 60 On the surface of the layer, a BCP layer is deposited at a evaporation rate of 0.10 Å / s as a hole blocking layer; Step 6, fabrication of the back electrode: A Cu layer with a thickness of 100 nm is thermally deposited on the surface of the BCP layer at a evaporation rate of 0.50 Å / s to serve as the back electrode, thus completing the fabrication of the perovskite solar cell.
[0048] <Example 2> The difference from Example 1 is that the evaporation sequence of the perovskite precursor in step 3 is different: first, the FACl functional additive layer is evaporated at a rate of 0.5 Å / s (duration 10 min, thickness 30 nm), then the FAI layer is evaporated at a rate of 3 Å / s to 500 nm, and finally CsI and PbI2 are co-evaporated at a rate of 3 Å / s to a total thickness of 500 nm, that is, the FACl layer is located at the bottom layer; the remaining steps and parameters are the same as in Example 1.
[0049] <Example 3> The difference from Example 1 is that the evaporation sequence of the perovskite precursor in step 3 is different: first, the FAI layer is evaporated to 500 nm at a rate of 3 Å / s, then CsI and PbI2 are co-evaporated to a total thickness of 500 nm at a rate of 3 Å / s, and finally the FACl functional additive layer is evaporated at a rate of 0.5 Å / s (duration 10 min, thickness 30 nm), that is, the FACl layer is located on the top layer; the remaining steps and parameters are the same as in Example 1.
[0050] <Comparative Example 1> The difference from Example 1 is that the FAI layer is not deposited during the perovskite precursor evaporation process in step 3: the FAI layer is first deposited at a rate of 3 Å / s to 500 nm, and then CsI and PbI2 are co-evaporated at a rate of 3 Å / s to a total thickness of 500 nm; the remaining steps and parameters are the same as in Example 1.
[0051] <Comparative Example 2> The difference from Example 1 is that in step 3, the FACl layer is not deposited during the vapor deposition process of the perovskite precursor and the vapor deposition order is reversed: first, CsI and PbI2 are co-evaporated at a rate of 3 Å / s to a total thickness of 500 nm, and then the FACl layer is deposited at a rate of 3 Å / s to 500 nm; the remaining steps and parameters are the same as in Example 1.
[0052] The device performance of Examples 1-3 and Comparative Examples 1 and 2 is shown in Table 1 and... Figure 1 As shown.
[0053] Table 1. Effect of different precursor deposition stacking sequences on device PCE <Examples 4~8> The only difference between Examples 4 to 8 and Example 1 is the evaporation time of the FACl functional additive layer in step 3: the evaporation times of FACl in Examples 4, 5, 6, 7 and 8 are 5 min, 15 min, 20 min, 25 min and 30 min respectively (the evaporation rate is 0.5 Å / s). The other steps and parameters are the same as in Example 1.
[0054] The device performance of the FACl evaporation time series experiments is shown in Table 2 and Figure 2 As shown.
[0055] Table 2 Effect of FACl deposition time on device PCE <Examples 9~Examples 12> The only difference between Examples 9 to 12 and Example 1 is the evaporation rate of the FACl functional additive layer: the FACl evaporation rates of Examples 9, 10, 11 and 12 are 0.2 Å / s, 1 Å / s, 3 Å / s and 5 Å / s respectively (evaporation time is 10 min for all), and the other steps and parameters are the same as those of Example 1.
[0056] The device performance of the FACl evaporation rate series experiments is shown in Table 3 and Figure 3 As shown.
[0057] Table 3. Effect of FACl deposition rate on device PCE <Examples 13~17> The only difference between Examples 13 to 17 and Example 1 is the holding time for the perovskite film annealing treatment in step 3: the annealing times for Examples 13, 14, 15, 16, and 17 are 5 min, 15 min, 20 min, 25 min, and 30 min, respectively (the annealing temperature is 150 ℃). The other steps and parameters are the same as those for Example 1.
[0058] The device performance of the annealing time series experiments is shown in Table 4 and Figure 4 As shown.
[0059] Table 4. Effect of annealing time on device PCE <Examples 18~20> The only difference between Examples 18-20 and Example 1 is the annealing temperature of the perovskite film in step 3: the annealing temperatures of Examples 18, 19 and 20 are 110 ℃, 130 ℃ and 170 ℃ respectively (annealing time is 10 min for all of them), and the other steps and parameters are the same as those of Example 1.
[0060] The device performance of the annealing temperature series experiments is shown in Table 5 and Figure 5 As shown.
[0061] Table 5. Effect of annealing temperature on device PCE The specific embodiments of this application have been described in detail above. For those skilled in the art, several improvements and modifications can be made to this application without departing from the principle of this application, and these improvements and modifications also fall within the protection scope of the claims of this application.
Claims
1. A method for preparing a perovskite thin film, characterized in that, Includes the following steps: The substrate is placed in a vacuum evaporation equipment, and an organic salt layer, a functional additive layer, and an inorganic salt layer are deposited on the substrate using a sequential thermal evaporation process. After the evaporation is completed, an annealing treatment is performed to obtain a perovskite thin film. The organic salt layer is made of FAI, the inorganic salt layer is made of CsI and PbI2, and the functional additive layer is made of FACl. The evaporation sequence is selected from any of the following: a) First, the functional additive layer is vapor-deposited, then the organic salt layer is vapor-deposited, and finally the inorganic salt layer is vapor-deposited. b) First, the organic salt layer is vapor-deposited, then the functional additive layer is vapor-deposited, and finally the inorganic salt layer is vapor-deposited. c) First, the organic salt layer is deposited by vapor deposition, then the inorganic salt layer is deposited by vapor deposition, and finally the functional additive layer is deposited by vapor deposition.
2. The preparation method according to claim 1, characterized in that, The inorganic salt layer contains CsI and PbI2 deposited simultaneously using a co-evaporation method.
3. The preparation method according to claim 2, characterized in that, The vapor deposition sequence is as follows: first, the organic salt layer is vapor deposited; then, the functional additive layer is vapor deposited; and finally, the inorganic salt layer is vapor deposited.
4. The preparation method according to claim 3, characterized in that, The vapor deposition rate of the functional additive layer is 0.2~5 Å / s, and the vapor deposition time is 5~30 min.
5. The preparation method according to claim 3, characterized in that, The annealing temperature is 110~170℃, and the annealing time is 5~30min.
6. The preparation method according to claim 1, characterized in that, The organic salt layer has a film thickness of 500 nm, and the inorganic salt layer has a film thickness of 500 nm. And / or, the film thickness of the functional additive layer is 5~300nm.
7. The preparation method according to claim 1, characterized in that, The perovskite thin film has a composition of FA. 1-x Cs x PbI3, of which .
8. The preparation method according to claim 1, characterized in that, The vacuum degree of the thermal evaporation is less than .
9. A perovskite thin film, characterized in that, The perovskite thin film is prepared by the preparation method according to any one of claims 1 to 8.
10. A perovskite solar cell, characterized in that, The perovskite solar cell comprises, from bottom to top, a transparent conductive substrate, a hole transport layer, a perovskite layer, an electron transport layer, a hole blocking layer, and a back electrode, which are stacked sequentially; the perovskite layer is the perovskite thin film as described in claim 9.