Laser scribing method for perovskite photovoltaic cells, perovskite photovoltaic cells
By employing a multi-stage laser scanning method, the problem of damage and residue in the transparent conductive layer during the P2 scribing of perovskite photovoltaic cells was solved, achieving efficient electrode connection and improved cell performance.
Patent Information
- Application Number
- CN202611422982.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-14
- Publication Date
- 2026-11-24
AI Technical Summary
In existing technologies, perovskite photovoltaic cells are prone to breakdown of the transparent conductive bottom electrode layer or have residual markings when the P2 line is scribed, which affects current transmission efficiency and module performance.
A multi-stage laser scanning method is adopted. First, a high-energy-density laser is used to remove the second charge transport layer, the perovskite layer, and the main part of the first charge transport layer. Then, a lower-energy-density laser is used to clean the bottom of the tank, ensuring that the bottom of the tank is located between the first charge transport layer and the transparent conductive layer, thus avoiding damage to the transparent conductive layer.
This improves the electrical connection reliability of perovskite photovoltaic cells, reduces contact resistance and leakage risk, and enhances the consistency and yield of large-area processing.
Smart Images

Figure CN123165014A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the technical field of perovskite solar cell manufacturing, and more particularly to a laser scribing method and perovskite photovoltaic cells. Background Technology
[0002] Perovskite photovoltaic modules involve three key scribing processes. The purpose of scribing line P2 is to cut through the hole transport layer, perovskite layer, and electron transport layer, exposing a transparent conductive film layer to provide a channel for connecting the positive and negative electrodes of adjacent sub-cells. After the hole transport layer, perovskite layer, and electron transport layer are fabricated, these functional layers are scribed using laser equipment to expose the transparent conductive film layer. This allows the positive and negative electrodes of the sub-cells to be interconnected during the subsequent electrode deposition process, achieving series connection of the sub-cells.
[0003] If the P2 scribing does not completely remove the functional layer, it may increase contact resistance and affect current transmission efficiency; while excessive scribing may damage the transparent conductive film layer, which will also have an adverse effect on the component performance. Summary of the Invention
[0004] In order to solve the technical problems of easy breakdown of transparent conductive bottom electrode layer or residual scribing when performing P2 scribing in the prior art, the present invention proposes a laser scribing method and a perovskite photovoltaic cell.
[0005] The first aspect of this invention provides a laser scribing method for perovskite photovoltaic cells, comprising: S1. Provide a photovoltaic cell semi-finished product, the photovoltaic cell semi-finished product comprising a transparent conductive layer, a first charge transport layer, a perovskite layer and a second charge transport layer stacked sequentially; S2. Perform laser scanning on the photovoltaic cell semi-finished product to form a P2 groove in the photovoltaic cell semi-finished product. The P2 groove passes through at least a portion of the second charge transport layer, the perovskite layer and the first charge transport layer. S3. Perform laser scanning on the bottom of the P2 groove; Wherein, the laser energy density in step S3 is less than the laser energy density in step S2, and after step S3, the bottom of the P2 trench is located at the interface between the first charge transport layer and the transparent conductive layer.
[0006] As an optional technical solution, a laser energy density of 0.1-2.0 J / cm² is used. 2 The laser scans the bottom of the P2 groove.
[0007] As an optional technical solution, a laser energy density of 3.0-6.0 J / cm² is used. 2The laser scans at least a portion of the second charge transport layer, the perovskite layer, and the first charge transport layer.
[0008] As an optional technical solution, the photovoltaic cell semi-finished product further includes a buffer layer formed on the surface of the second charge transport layer. Before step S2, the following steps are performed: S101. Perform laser scanning on the buffer layer to form an initial groove in the buffer layer; The laser energy density in step S101 is less than the laser energy density in step S2.
[0009] As an optional technical solution, a laser energy density of 1.0-2.5 J / cm² is used. 2 The laser scans the buffer layer.
[0010] As an optional technical solution, in step S101, the initial groove extends through at least 50% of the thickness of the buffer layer.
[0011] As an optional technical solution, in step S2, the P2 trench penetrates at least 90% of the thickness of the first charge transport layer.
[0012] As an optional technical solution, the laser used in the P2 slot is a picosecond green light with a wavelength of 515–532 nm, and the laser spot is a flat-top spot.
[0013] As an optional technical solution, negative pressure dust removal can be performed simultaneously during laser scanning.
[0014] A second aspect of the present invention provides a perovskite photovoltaic cell, comprising a transparent conductive layer, a first charge transport layer, a perovskite layer, and a second charge transport layer stacked sequentially. The P2 groove of the perovskite photovoltaic cell is processed using the laser scribing method for perovskite photovoltaic cells described above. One of the first charge transport layer and the second charge transport layer is a hole transport layer, and the other is an electron transport layer.
[0015] Compared with the prior art, the present invention has at least the following beneficial effects: This invention employs a relatively high energy density laser to perform the main removal tasks of the second charge transport layer, the perovskite layer, and the first charge transport layer, thus shortening the production time; and employs a relatively low energy density laser to complete the bottom cleaning of the tank, so that the bottom of the P2 tank terminates at the interface between the first charge transport layer and the transparent conductive layer, removing residues and avoiding damage to the transparent conductive layer.
[0016] When a photovoltaic cell semi-finished product includes a buffer layer, the buffer layer is first scribed with a laser of lower energy density, and then the second charge transport layer, the perovskite layer, and at least a portion of the first charge transport layer are scribed with a laser of higher energy density. This avoids the problem of tin elements penetrating into the second charge transport layer and even the perovskite layer when the higher energy density laser acts on the buffer layer (e.g., SnOx), thus reducing the risk of cross-contamination.
[0017] Picosecond green lasers with wavelengths of 515-532nm are used. This wavelength band can be effectively absorbed by the perovskite layer and various functional layers. The picosecond-level pulse width allows the material to be removed before the heat is fully diffused. Combined with the flat-topped spot obtained by shaping, the energy distribution at the center and edge of the spot is uniform, avoiding the problems of over-etching at the center and edge residue of the Gaussian beam. The resulting P2 groove has a flat bottom, steep sidewalls, and a small heat-affected zone.
[0018] Negative pressure dust removal is performed simultaneously during laser scanning, which reduces the redeposition of particles and debris generated during scribing in the P2 tank. Combined with bottom cleaning, this further improves the cleanliness of the tank bottom.
[0019] In the perovskite photovoltaic cells produced, the bottom of the P2 cell is clean and the transparent conductive layer is intact. The subsequent series connection between the deposited top electrode and the transparent conductive layer has high reliability, low contact resistance, low leakage risk, and good consistency and high yield in large-area processing. Attached Figure Description
[0020] The present invention will now be described in detail with reference to the embodiments and accompanying drawings, wherein: Figure 1 This is a main flowchart of an embodiment of the present invention.
[0021] Figure 2 This is a schematic diagram of the P2 groove structure according to an embodiment of the present invention.
[0022] Figure 3 This is a schematic diagram of a battery structure according to an embodiment of the present invention.
[0023] 1. Substrate; 2. Transparent conductive layer; 3. First charge transport layer; 4. Perovskite layer; 5. Second charge transport layer; 6. Buffer layer; 7. Top electrode; 8. P2 trench. Detailed Implementation
[0024] To make the technical problems to be solved, the technical solutions, and the beneficial effects of the present invention clearer, the present invention will be further described in detail below with reference to the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.
[0025] Therefore, a feature pointed out in this specification is used to describe one feature of one embodiment of the invention, and does not imply that every embodiment of the invention must have the described feature. Furthermore, it should be noted that this specification describes many features. Although certain features may be combined to illustrate possible system designs, these features may also be used in other combinations not explicitly stated. Therefore, unless otherwise stated, the described combinations are not intended to be limiting.
[0026] like Figure 1 As shown, this embodiment provides a laser scribing method, including: S1. Provide photovoltaic cell semi-finished product, which includes a transparent conductive layer 2, a first charge transport layer 3, a perovskite layer 4 and a second charge transport layer 5 stacked in sequence.
[0027] In this embodiment, the photovoltaic cell semi-finished product includes a substrate 1, a transparent conductive layer 2, a first charge transport layer 3, a perovskite layer 4 and a second charge transport layer 5 arranged sequentially. In some embodiments, a buffer layer 6 formed on the surface of the second charge transport layer 5 is also included.
[0028] Before laser scanning ablation, the surface of the photovoltaic cell semi-finished product can be cleaned, for example, by using non-contact dust removal methods such as nitrogen purging or clean airflow purging, to remove particulate contaminants attached to the surface, thereby reducing local ablation and film peeling caused by particle heat absorption during laser scribing.
[0029] One of the first charge transport layer 3 and the second charge transport layer 5 is a hole transport layer, and the other is an electron transport layer.
[0030] S2. Perform laser scanning on the photovoltaic cell semi-finished product to form a P2 groove 8, which passes through at least a portion of the second charge transport layer 5, the perovskite layer 4, and the first charge transport layer 3.
[0031] Step S2 employs a relatively high-energy-density laser to perform the main material ablation and removal task. The higher energy-density laser ablation speed is faster, shortening production time. The specific scanning path is planned according to the sub-cell pattern, maintaining basic parallelism to the P1 line with a preset spacing. After step S2, the P2 groove 8 has penetrated the second charge transport layer 5 and the perovskite layer 4. In some embodiments, the P2 groove 8 only penetrates a portion of the first charge transport layer 3, for example, only 90% of the thickness of the first charge transport layer 3. There is still 10% of the first charge transport layer 3 material between the bottom of the P2 groove 8 and the transparent conductive layer 2. The transparent conductive layer 2 is not directly ablated by the relatively high-energy-density laser, reducing damage. In other embodiments, the P2 groove 8 completely penetrates the first charge transport layer 3, and the bottom of the P2 groove 8 is located at the interface between the first charge transport layer 3 and the transparent conductive layer 2.
[0032] S3. Perform laser scanning on the bottom of slot 8 in P2.
[0033] In step S3, the laser energy density is less than that in step S2. After step S3, the bottom of P2 groove 8 is located at the interface between the first charge transport layer 3 and the transparent conductive layer 2.
[0034] When the P2 trench 8 penetrates only a portion of the first charge transport layer 3, for example, only 90% of the thickness of the first charge transport layer 3, and there is still 10% of the first charge transport layer 3 material between the bottom of the P2 trench 8 and the transparent conductive layer 2, if the top electrode 7 is directly deposited in the P2 trench 8, the top electrode 7 and the transparent conductive layer 2 will be blocked by the remaining 10% of the first charge transport layer 3 material, making electrical connection impossible. Therefore, it is necessary to perform laser scanning on the bottom of the P2 trench 8 so that the bottom of the P2 trench 8 is located at the interface between the first charge transport layer 3 and the transparent conductive layer 2, ensuring electrical connection between the top electrode 7 and the transparent conductive layer 2. Since the laser energy density in step S3 is less than that in step S2, a relatively gentle cleaning scan is performed on the bottom of the trench. On the one hand, this removes the residue generated in step S2 and the remaining first charge transport layer 3 material from the bottom of the trench. On the other hand, since the laser energy density in step S3 is less than that in step S2, the laser will not cause breakdown, ablation, or significant roughening of the transparent conductive layer 2 while removing the material.
[0035] In some other embodiments, the P2 groove 8 in step S2 completely penetrates the first charge transport layer 3. After step S2, the bottom of the P2 groove 8 is located at the interface between the first charge transport layer 3 and the transparent conductive layer 2. At this time, although there is a risk of damage to the transparent conductive layer 2, the damage to the transparent conductive layer 2 can be reduced by lowering the laser energy density. That is, step S2 uses a relatively low laser energy density to completely penetrate the first charge transport layer 3. At this time, ablation residues still remain on the surface of the transparent conductive layer 2. These ablation residues still have a negative effect on the electrical connection between the top electrode 7 and the transparent conductive layer 2. Therefore, it is still necessary to remove the ablation residues in step S3 to reduce the contact resistance between the top electrode 7 and the transparent conductive layer 2 and reduce the risks of leakage and decreased reliability.
[0036] When step S3 is performed, the ablation residues adhering to both sides of the P2 groove 8 are also ablated and removed.
[0037] In this embodiment, a relatively high energy density laser is used to perform the main removal tasks of the second charge transport layer 5, the perovskite layer 4, and the first charge transport layer 3, which shortens the production time; a relatively low energy density laser is used to complete the bottom cleaning of the tank, so that the bottom of the P2 tank 8 terminates at the interface between the first charge transport layer 3 and the transparent conductive layer 2, removing residues and avoiding damage to the transparent conductive layer 2.
[0038] The terms "relatively high energy density laser" and "relatively low energy density laser" refer to the comparison of laser energy in steps S2 and S3.
[0039] In summary, this embodiment employs a multi-stage scanning ablation method that combines relatively high-energy-density coarse ablation with relatively low-energy-density fine cleaning. The higher-energy-density laser is responsible for quickly removing most of the film material, while the lower-energy-density laser is responsible for the final scanning to protect the transparent conductive layer 2. This avoids the dilemma of damaging the transparent conductive layer 2 when a single-energy ablation is performed, or failing to ablate or leaving residue when the energy is too low.
[0040] In step S2, the same laser energy density can be used for scanning and ablation throughout the process, or different laser energy densities can be used for scanning and ablation. When different laser energy densities are used for scanning and ablation, the lowest or lower laser energy density does not need to be higher than the laser energy density in step S3.
[0041] Optionally, a laser energy density of 0.1-2.0 J / cm² can be used. 2 The laser scans the bottom of slot 8 in P2.
[0042] Preferably, a laser energy density of 0.5-1.0 J / cm² is used. 2 The laser scans the bottom of slot 8 in P2.
[0043] Optionally, when scanning the bottom of P2 slot 8, the laser pulse overlap rate is 80%-99.9%.
[0044] Preferably, when scanning the bottom of P2 slot 8, the laser pulse overlap rate is 90%-99.9%.
[0045] Optionally, a laser energy density of 3.0-6.0 J / cm² can be used. 2 The laser scans at least a portion of the second charge transport layer 5, the perovskite layer 4, and the first charge transport layer 3.
[0046] Preferably, a laser energy density of 4.0-5.5 J / cm² is used. 2 The laser scans at least a portion of the second charge transport layer 5, the perovskite layer 4, and the first charge transport layer 3.
[0047] Optionally, when scanning at least a portion of the second charge transport layer 5, the perovskite layer 4, and the first charge transport layer 3, the laser pulse overlap rate is 80%-99.9%.
[0048] Optionally, when scanning at least a portion of the second charge transport layer 5, the perovskite layer 4, and the first charge transport layer 3, the laser pulse overlap rate is 90%-99.9%.
[0049] Optionally, the photovoltaic cell semi-finished product also includes a buffer layer 6 formed on the surface of the second charge transport layer 5. Before step S2, the following steps are performed: S101, Perform laser scanning on the buffer layer 6 to form an initial groove in the buffer layer 6; the laser energy density in step S101 is less than the laser energy density in step S2.
[0050] The buffer layer 6 is used to protect the second charge transport layer 5 and prevent negative effects on the second charge transport layer 5 during the fabrication of the top electrode 7. At the same time, the buffer layer 6 also plays a role in energy level regulation, leakage current suppression, ion diffusion blocking, and improving electrode contact.
[0051] The materials of buffer layer 6, charge transport layer, and perovskite layer 4 are different. For example, buffer layer 6 is made of tin oxide, while charge transport layer is made of NiOx or C60.
[0052] First, a low-energy-density laser is used to ablate the buffer layer 6, and then a high-energy-density laser is used to ablate the second charge transport layer 5, the perovskite layer 4, and the first charge transport layer 3. This reduces the risk of tin cross-penetration while ensuring the etching speed.
[0053] Optionally, a laser energy density of 1.0-2.5 J / cm² can be used. 2The laser scans the buffer layer 6.
[0054] Optionally, in step S101, the initial groove extends through at least 50% of the thickness of the buffer layer 6.
[0055] Preferably, in step S101, the initial groove penetrates at least 90% of the thickness of the buffer layer 6, for example, the initial groove penetrates 90%, 95%, or even 100% of the thickness of the buffer layer 6.
[0056] In step S101, when the initial trench does not completely penetrate the buffer layer 6, in step S2, the laser first completely ablates the remaining thickness of the buffer layer 6, and then sequentially ablates the second charge transport layer 5, the perovskite layer 4, and the first charge transport layer 3. Although there is a situation where the tin element of the remaining thickness of the buffer layer 6 penetrates into other film layers, since at least half of the buffer layer 6 has been ablated and removed in step S101, the tin content that has penetrated into other film layers can be reduced.
[0057] Optionally, in step S2, the P2 trench 8 extends through at least 90% of the thickness of the first charge transport layer 3.
[0058] Optionally, the laser used for slot P2 is a picosecond green light with a wavelength of 515–532 nm, and the laser spot is a flat-top spot.
[0059] In one embodiment, a picosecond green laser is shaped using a shaping device to obtain a circular or rectangular flat-topped spot. The shaping device can be a diffractive optical element (DOE), an aspherical shaping lens group, or any other optical device capable of converting the Gaussian beam output from the laser into a flat-topped beam. The energy uniformity of the flat-topped spot can be greater than or equal to 90%. Unlike the bell-shaped distribution of Gaussian spots, which have "excessive energy at the center and insufficient energy at the edges," the energy in the central and edge regions of the flat-topped spot is essentially the same. This avoids the problems of over-etching at the center of the spot, potentially even penetrating the transparent conductive layer 2, and insufficient energy at the edge leading to material residue. It can form P2 grooves 8 with flat bottoms, steep sidewalls, and consistent width. Circular flat-topped spots are suitable for single-channel or multi-channel overlapping scanning, while rectangular flat-topped spots are suitable for forming P2 grooves 8 with steeper edges and more controllable linewidth. Before processing, the size and energy uniformity of the flat-topped spot can be calibrated using a beam analyzer to confirm that it meets the process requirements.
[0060] Optionally, negative pressure dust removal can be performed simultaneously during laser scanning.
[0061] Negative pressure dust removal can be achieved by installing a negative pressure dust removal device near the laser processing head or on one side of the processing area. This device is used to remove plasma, particles, debris, and fumes generated during the scribing process, reducing the redeposition of scribing residue in the P2 tank 8. The negative pressure dust removal device can be continuously activated at each scribing stage, or the adsorption intensity can be adjusted according to the process stage. For example, the adsorption intensity can be increased during the stage of removing the main functional layer to promptly remove the large amount of debris generated.
[0062] The laser scribing method of the present invention can be implemented by a laser scribing system. This laser scribing system includes a laser, a shaping device, a scanning processing unit, a positioning and focusing unit, a negative pressure dust removal unit, and a control unit. The laser is used to output picosecond green laser light with a wavelength of 515-532nm; the shaping device is set in the output optical path of the laser to shape the Gaussian beam output by the laser into a flat-top beam; the scanning processing unit is used to scan the flat-top beam along the planned P2 scribing path, and it may include a collimating beam expanding unit, a scanning galvanometer, an F-theta field lens and a motion platform. Through the cooperation of the scanning galvanometer and the motion platform, both high-speed scribing and large-area substrate processing are taken into account; the positioning and focusing unit is used to identify the P1 scribing, substrate edge or alignment mark, and generate or correct the P2 scribing path accordingly, and detect the surface height of the perovskite solar cell semi-finished product to adjust the laser focus position, compensate for the warping of the perovskite solar cell semi-finished product or the undulation of the flexible substrate, and avoid local over-scribing or local residue; the negative pressure dust removal unit is used to remove particles, debris and dust during the scribing process; the control unit is connected to the laser, the scanning processing unit, the positioning and focusing unit and the negative pressure dust removal unit respectively, and is configured to execute the laser scribing method of this embodiment according to a preset process program.
[0063] In one embodiment, the width of the P2 slot 8 is 10-80 μm, and the spacing between two adjacent P2 slots 8 is 5-30 μm. The width of the P2 slot 8 can be controlled by the size of the flat-top spot, the number of scanning tracks, and the track spacing. For a wider P2 slot 8, it can be formed by overlapping multiple parallel scans. In this case, the spacing between two adjacent P2 slots 8 (i.e., the scribing slot segments formed by adjacent scanning tracks) is 5-30 μm. If the spacing is too large, there will be un-scribbed gaps between adjacent scribing slot segments; if the spacing is too small, the adjacent scribing slot segments will overlap excessively, increasing the number of pulses per unit area and increasing heat input. Controlling the spacing between 5-30 μm ensures that adjacent scribing slot segments overlap sufficiently without leaving un-scribbed gaps, while avoiding repeated heat input caused by excessive overlap. In a specific embodiment, a circular flat-top spot with a diameter of 40 μm and a track spacing of 15 μm are used for multi-track overlapping scans to form a P2 slot 8 with a width of approximately 65 μm.
[0064] After P2 scribing is completed, post-processing and quality inspection can be performed on the scribed area. Post-processing may include nitrogen purging or clean, dry gas purging to remove particles, debris, and volatile decomposition products from and around the P2 groove 8. Quality inspection may include at least one of the following: optical microscopy, scanning electron microscopy, laser confocal microscopy, four-probe testing, and electrical performance testing: optical microscopy and scanning electron microscopy are used to observe the smoothness of the groove edge, sidewall morphology, particle residue, and carbonization; laser confocal microscopy is used to detect the groove width, depth, bottom smoothness, and heat-affected zone width; four-probe testing is used to detect the conductivity continuity of the transparent conductive layer 2 after P2 scribing; electrical performance testing is used to evaluate the series resistance, parallel resistance, fill factor, and leakage risk of subsequent devices.
[0065] In one specific embodiment, the P2 line of a glass-based single-junction perovskite solar cell is used as an example.
[0066] Provide a photovoltaic cell semi-finished product with P1 marking completed but top electrode 7 not yet deposited. The photovoltaic cell semi-finished product includes, from bottom to top, a glass substrate, an FTO transparent conductive layer, a NiOx hole transport layer, a SAMs modification layer, a perovskite layer 4, a 2D passivation layer, a C60 electron transport layer and a SnOx buffer layer.
[0067] A green picosecond laser with a wavelength of 532 nm, a pulse width of 8 ps, and a repetition frequency of 800 kHz is used to form a circular flat-topped spot with a diameter of 40 μm and an energy uniformity of 92% after DOE shaping. The P1 line is visually positioned using a positioning and focusing unit, and the path for the P2 line is planned. Step S101 uses a laser with an energy density of 2.0 J / cm² and a pulse overlap rate of 95% to remove the SnOx buffer layer. Step S2 uses a laser with an energy density of 5.4 J / cm² and a pulse overlap rate of 95% to remove most of the C60 electron transport layer, 2D passivation layer, perovskite layer 4, SAMs modification layer, and the main body of the NiOx hole transport layer. Step S3 uses a laser with an energy density of 0.80 J / cm² and a pulse overlap rate of 95% to clean the bottom of the trench, removing residual NiOx hole transport layer and SAMs modification layer material, exposing the FTO transparent conductive layer. The scanning speed was 2000 mm / s, the track spacing was 15 μm, and the number of scans was 2. Negative pressure dust removal was activated simultaneously during the scribing process, and nitrogen purging was performed after scribing. Testing revealed that the width of P2 groove 8 was approximately 65 μm, the scribing depth was approximately 580 nm, the FTO transparent conductive layer remained intact with good conductivity continuity, no obvious functional layer residue was found within the groove, and no obvious carbonization, microcracks, or recast layer were observed at the groove edges.
[0068] The electrical performance of the perovskite solar cell obtained in this embodiment was compared with that of the perovskite solar cell obtained by scribing the P2 line using a Gaussian beam. The specific electrical performance data are shown in the table below. The fill factor of the present invention is improved by more than 2% compared with that of the Gaussian beam.
[0069]
[0070] The table above compares the glass-based single-junction perovskite solar cell of this embodiment with the glass-based single-junction perovskite solar cell with a Gaussian beam. In one specific embodiment, taking the P2 scribing of a flexible perovskite solar cell as an example, a photovoltaic cell semi-finished product with P1 scribing completed but without the top electrode 7 deposited is provided. This semi-finished product comprises, from bottom to top, a PET flexible substrate, an ITO transparent conductive layer, a NiOx hole transport layer, a SAMs modification layer, a perovskite layer 4, a C60 electron transport layer, and a SnOx buffer layer. A green picosecond laser with a wavelength of 532 nm, a pulse width of 8 ps, and a repetition frequency of 400 kHz is used to shape a circular flat-topped spot with a diameter of 25 μm and an energy uniformity of 93%. Step S101 uses a laser with an energy density of 1.07 J / cm² and a laser pulse overlap rate of 95%; step S2 uses a laser with an energy density of 4.4 J / cm² and a laser pulse overlap rate of 95%; step S3 uses a laser with an energy density of 0.53 J / cm² and a laser pulse overlap rate of 95% to clean the bottom of the groove, exposing the ITO transparent conductive layer. The scanning speed was 1800 mm / s, the scanning track spacing was 15 μm, and the number of scans was 2. Negative pressure dust removal was activated simultaneously during the scribing process. Because the flexible substrate and the ITO transparent conductive layer are more sensitive to thermal shock, the laser energy density and repetition frequency in each step of this embodiment are lower than those in the glass-based embodiment, which helps reduce flexible substrate warping, ITO cracking, and film peeling. Testing showed that the ITO transparent conductive layer remained intact, and the scribing grooves showed no obvious residue, carbonization, or cracks.
[0071] The electrical performance of the perovskite solar cell obtained in this embodiment was compared with that of the perovskite solar cell obtained by scribing the P2 line using a Gaussian beam. The specific electrical performance data are shown in the table below. The fill factor of the present invention is improved by more than 2% compared with that of the Gaussian beam.
[0072]
[0073] The table above compares the flexible perovskite solar cell of this embodiment with the flexible perovskite solar cell using a Gaussian beam. In other embodiments, the buffer layer 6 can be omitted. In this case, step S2 directly uses a high-energy-density laser to complete the etching of at least a portion of the second charge transport layer 5, the perovskite layer 4, and the first charge transport layer 3 in one step. The material of the buffer layer 6 is not limited to SnOx; it can be flexibly selected from materials such as IZO, AZO, ZnO, and TiOx, depending on the cell structure, the transport layer system, and the subsequent top electrode 7 process. In other embodiments, the laser scribing method of the present invention is also applicable to the P2 scribing of perovskite sub-cells in perovskite / silicon tandem cells. By controlling the energy in stages, the influence of laser heat input on the tandem interface and the underlying silicon cell structure is reduced, meeting the P2 scribing requirements of narrow dead zones and low damage in high-efficiency tandem cells. The specific materials, layer thickness, laser parameters, and detection results in the above embodiments can be adjusted according to different battery structures. As long as a multi-stage scanning etching method of "high energy density laser etching to a position close to the transparent conductive layer 2 and low energy density laser etching to the surface of the transparent conductive layer 2" is used, so that the bottom of the P2 groove 8 is finally located at the interface between the first charge transport layer 3 and the transparent conductive layer 2, it falls within the technical concept scope of this invention.
[0074] This embodiment also provides a perovskite photovoltaic cell, which includes a photovoltaic cell semi-finished product. The photovoltaic cell semi-finished product is processed by the laser scribing method described above. One of the first charge transport layer 3 and the second charge transport layer 5 is a hole transport layer, and the other of the two is an electron transport layer.
[0075] like Figure 2 As shown, the photovoltaic cell semi-finished product completes the scribing process for P2 slot 8, as follows. Figure 3 As shown, the photovoltaic cell semi-finished product completes the preparation process of the top electrode 7.
[0076] The photovoltaic cell semi-finished product includes a substrate 1, a transparent conductive layer 2, a first charge transport layer 3, a perovskite layer 4, a second charge transport layer 5, a buffer layer 6, and a top electrode 7 arranged sequentially. A portion of the top electrode 7 fills the P2 groove 8 and connects it to the transparent conductive layer 2.
[0077] It should be noted that the directional terms such as "upper" and "lower" used in this invention are relative to the stacking direction shown in the accompanying drawings. They are only used to clearly describe the relative positional relationship between the film layers and do not impose any restrictions on the orientation of the photovoltaic cell semi-finished product in actual use, processing, or testing. In this invention, "first charge transport layer" and "second charge transport layer" are only used to distinguish the charge transport layers located on both sides of the perovskite layer, and the charge carrier types of the two can be interchanged. "Photovoltaic cell semi-finished product" refers to a semi-finished part that has not yet had its top electrode (back electrode) deposited. Unless otherwise specified, its "surface," "bottom of the tank," etc., all refer to the laser incident side.
[0078] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A laser scribing method for perovskite photovoltaic cells, characterized in that, include: Step S1: Provide a photovoltaic cell semi-finished product, which includes a transparent conductive layer, a first charge transport layer, a perovskite layer and a second charge transport layer stacked sequentially. Step S2: Perform laser scanning on the photovoltaic cell semi-finished product to form a P2 groove in the photovoltaic cell semi-finished product. The P2 groove passes through at least a portion of the second charge transport layer, the perovskite layer, and the first charge transport layer. Step S3: Perform laser scanning on the bottom of the P2 groove; Wherein, the laser energy density in step S3 is less than the laser energy density in step S2, and after step S3, the bottom of the P2 trench is located at the interface between the first charge transport layer and the transparent conductive layer.
2. The laser scribing method for perovskite photovoltaic cells according to claim 1, characterized in that, The laser energy density used is 0.1-2.0 J / cm². 2 The laser scans the bottom of the P2 groove.
3. The laser scribing method for perovskite photovoltaic cells according to claim 1, characterized in that, The laser energy density used is 3.0-6.0 J / cm². 2 The laser scans at least a portion of the second charge transport layer, the perovskite layer, and the first charge transport layer.
4. The laser scribing method for perovskite photovoltaic cells according to claim 1, characterized in that, The photovoltaic cell semi-finished product also includes a buffer layer formed on the surface of the second charge transport layer. Before step S2, the following steps are performed: Step S101: Perform laser scanning on the buffer layer to form an initial groove in the buffer layer; The laser energy density in step S101 is less than the laser energy density in step S2.
5. The laser scribing method for perovskite photovoltaic cells according to claim 4, characterized in that, The laser energy density used is 1.0-2.5 J / cm². 2 The laser scans the buffer layer.
6. The laser scribing method for perovskite photovoltaic cells according to claim 4 or 5, characterized in that, In step S101, the initial groove extends through at least 50% of the thickness of the buffer layer.
7. The laser scribing method for perovskite photovoltaic cells according to claim 1, characterized in that, In step S2, the P2 trench extends through at least 90% of the thickness of the first charge transport layer.
8. The laser scribing method for perovskite photovoltaic cells according to claim 1, characterized in that, The laser used in the P2 slot is a picosecond green light with a wavelength of 515–532 nm and a flat-top laser spot.
9. The laser scribing method for perovskite photovoltaic cells according to claim 1, characterized in that, During laser scanning, negative pressure dust removal is performed simultaneously.
10. A perovskite photovoltaic cell, characterized in that, The perovskite photovoltaic cell comprises a transparent conductive layer, a first charge transport layer, a perovskite layer, and a second charge transport layer stacked sequentially. The P2 groove of the perovskite photovoltaic cell is processed by the laser scribing method for perovskite photovoltaic cells as described in any one of claims 1-9. One of the first charge transport layer and the second charge transport layer is a hole transport layer, and the other is an electron transport layer.