A lightweight high-toughness bismuth telluride thermoelectric device and a preparation method and application thereof
By introducing an octahedral lattice pyrolytic carbon framework and a bismuth telluride thermoelectric thin film into the bismuth telluride thermoelectric device, the problems of easy cracking and interface failure of the bismuth telluride thin film are solved, and a lightweight, high-strength, high-toughness and high-reliability thermoelectric conversion effect is achieved.
Patent Information
- Application Number
- CN202611394700.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-09
- Publication Date
- 2026-11-24
AI Technical Summary
Existing bismuth telluride thin-film thermoelectric devices are prone to thin-film cracking, interface peeling, electrode breakage, encapsulation failure, and output attenuation during use, making it difficult to meet the comprehensive requirements of flexible wearable devices for lightweight, high reliability, and long-term mechanical stability.
An octahedral lattice pyrolytic carbon skeleton is used as a support. The pyrolytic carbon skeleton is formed by photopolymerization 3D printing and tube furnace pyrolysis. Then, bismuth telluride thermoelectric thin film and silver paste electrode are deposited on it. Lightweight, high-strength and tough bismuth telluride thermoelectric device is prepared by combining magnetron sputtering process.
This technology enables lightweight devices, improves mechanical reliability and thermoelectric output stability, enhances the strength and toughness of materials, allows for stress distribution in multiple directions, and improves thermoelectric conversion efficiency and electrical connection continuity.
Smart Images

Figure CN123165017A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of thermoelectric device technology, and in particular to a lightweight, high-strength, and tough bismuth telluride thermoelectric device, its preparation method, and its application. Background Technology
[0002] With the rapid development of the Internet of Things, flexible electronics, biomedical monitoring, and wearable devices, the market demand for lightweight, self-powered micro-power supplies is becoming increasingly urgent. Thermoelectric devices, based on the Seebeck effect, can directly convert heat energy into electrical energy. They require no moving parts, have a compact structure, and high reliability. They can utilize human body heat or ambient waste heat to power low-power electronic devices, and have broad application prospects in wearable energy devices and micro-sensing systems.
[0003] Bismuth telluride (Bi₂Te₃) and its alloys are among the most widely used thermoelectric materials due to their excellent thermoelectric properties near room temperature. Existing flexible thermoelectric devices typically employ a method of depositing a bismuth telluride-based thin film onto the surface of a flexible substrate to achieve adhesion to curved heat sources. However, bismuth telluride is a brittle layered semiconductor material with limited tensile and bending resistance. During repeated bending, compression, or thermal cycling, it is prone to cracking, peeling, and interface failure, leading to significant performance degradation in the device. Therefore, simply improving the thermoelectric properties of the material is insufficient to meet the comprehensive requirements of lightweight, high reliability, and long-term mechanical stability for flexible wearable devices.
[0004] In recent years, lattice structures have attracted widespread attention due to their mechanical advantages such as ultra-lightweight, high specific strength, and high specific stiffness. Among them, octahedral lattice structures achieve efficient multi-directional load-bearing through a spatial truss network, maintaining good structural stability at extremely low densities. Compared with traditional planar or thin-film structures, octahedral lattice structures can not only significantly reduce the overall weight of devices but also provide continuous and uniform mechanical support for the thermoelectric functional layers covering their surfaces, effectively reducing local stress concentration and thus improving the overall mechanical reliability of the device. However, existing research on octahedral lattice structures mainly focuses on lightweight load-bearing and energy absorption, while research on their structural-functional integration with high-performance thermoelectric materials remains relatively limited.
[0005] On the other hand, polymer lattice frameworks, after controlled inert atmosphere heat treatment, can form pyrolytic carbon frameworks containing carbonized components and incompletely pyrolyzed components. This process, while largely maintaining the original lattice topology, can significantly improve the stiffness and thermal stability of the framework members and retain certain variation limits, thus combining load-bearing capacity and structural toughness. However, existing technologies have not integrated this pyrolytic carbon lattice framework with bismuth telluride thermoelectric thin films to address the device challenges posed by the easy cracking and interface failure of bismuth telluride thin films.
[0006] In summary, there is an urgent need in this field to construct a thermoelectric device that balances lightweight design, mechanical strength, and thermoelectric output stability. Summary of the Invention
[0007] In view of this, the present invention proposes a lightweight, high-strength and tough bismuth telluride thermoelectric device, its preparation method and application, to solve the problems of thin film cracking, interface peeling, electrode breakage, encapsulation failure and output attenuation that are prone to occur in existing bismuth telluride thin film thermoelectric devices during use.
[0008] The technical solution of the present invention is implemented as follows: In the first aspect, the present invention provides a lightweight, high-strength and tough bismuth telluride thermoelectric device, comprising an octahedral lattice pyrolytic carbon skeleton, a bismuth telluride thermoelectric thin film, a silver paste electrode, a wire and a substrate; The bismuth telluride thermoelectric thin film is deposited on the surface of an octahedral lattice pyrolytic carbon framework. An octahedral lattice pyrolytic carbon framework loaded with the bismuth telluride thermoelectric thin film is fixed to and electrically connected to the substrate via silver paste electrodes. The wire is electrically connected to the silver paste electrode.
[0009] The thermoelectric device has a peak compressive strength of 35 MPa to 45 MPa and a specific strength of 98 MPa·cm. 3 ·g -1 ~113 MPa·cm 3 ·g -1 The specific energy absorption is 15 J·g -1 ~ 18 J·g -1 At a temperature difference of 30 K, the maximum output power is 1.2~1.6 nW.
[0010] Based on the above technical solutions, the preferred method for preparing the octahedral lattice pyrolytic carbon skeleton is as follows: using photosensitive toughening resin as the printing material, an octahedral lattice resin skeleton is prepared by photopolymerization 3D printing technology; after printing, the printed octahedral lattice structure is removed, immersed in alcohol, and then cleaned with an ultrasonic cleaner to remove excess residual resin, followed by curing with an ultraviolet irradiation instrument for 5 minutes; the printed structure is placed in a tube furnace, and after the air in the tube is purged with a vacuum pump, high-purity argon gas is slowly introduced for heat treatment (vacuuming for 5 minutes each time, and introducing high-purity argon gas until the gas pressure in the tube reaches 0.8 standard atmospheres each time, for a total of 3 times), to obtain an octahedral lattice pyrolytic carbon skeleton containing carbonized components and incompletely pyrolyzed components.
[0011] In the above scheme, preferably, during printing, the thickness of each normal layer is 0.02 mm, the exposure time of each layer is 1.8 s, the waiting time before lifting is 4 s, and the waiting time after lifting is 10 s; the bottom layer has 5 layers, the exposure time is 30 s, the bottom lamp-off time is 20 s, the waiting time before lifting the bottom is 5 s, and the waiting time after lifting the bottom is 15 s; the Z-axis lifting height is 8 mm, and the lifting speed and the descent speed are both 0.8 mm / s.
[0012] Based on the above technical solution, preferably, the octahedral lattice resin skeleton is formed by connecting multiple octahedral lattice unit cells in a periodic array along the X, Y, and Z directions; the octahedral lattice unit cell includes several rods and spatial nodes connecting the rods, and the rods form a three-dimensional truss load-bearing network through the spatial nodes; the length, width, and height of the octahedral lattice unit cell are all L, where L is 1.5 mm, the diameter d of the rods is 0.188 mm ~ 0.375 mm, and d / L is 0.125 ~ 0.25.
[0013] Based on the above technical solutions, preferably, the heat treatment temperature is 250 ℃~500 ℃, the heat treatment time is 0.5 h~8 h, and the heating rate is 1 ℃ / min~10 ℃ / min.
[0014] Based on the above technical solutions, preferably, the substrate is a 3D printed substrate, and the substrate material is one or more combinations of tough resin, ultra-tough resin or rigid resin; the material of the wire is copper.
[0015] Secondly, the present invention also provides a method for preparing a lightweight, high-strength, and tough bismuth telluride thermoelectric device, comprising the following steps: S1, a bismuth telluride thermoelectric thin film layer is deposited on the surface of the octahedral lattice pyrolytic carbon skeleton using magnetron sputtering. S2, using silver paste to connect the octahedral lattice pyrolytic carbon skeleton that has been coated to the 3D printed substrate, and curing to form a silver paste electrode connected to the bismuth telluride thermoelectric thin film layer; S3, connect the wires to the silver paste electrode to obtain the thermoelectric device.
[0016] Based on the above technical solution, preferably, in step S1, after the pyrolysis of the octahedral lattice structure is completed, it is placed on the substrate and then loaded into the sputtering cavity. A thin film is grown using a co-sputtering method with a tellurium-bismuth alloy target and a tellurium elemental target. The tellurium-bismuth alloy target is connected to a DC power supply, and the tellurium elemental target is connected to an RF power supply. The target-substrate spacing and sputtering angle are adjusted, and the mechanical pump and molecular pump evacuate the cavity to 5 × 10⁻⁶. -4 After the pressure drops below Pa, high-purity argon gas is introduced and a bias voltage of 800 V is applied. The pulse duty cycle is set to 80%, and the substrate is cleaned using ionized argon ions.
[0017] After the substrate cleaning is complete, turn on the RF power supply and DC power supply, along with the corresponding power baffle, for 5-10 minutes of pre-sputtering. After pre-sputtering, sequentially turn on the substrate disk rotation and substrate baffle to begin the actual sputtering. After each sputtering period, turn off the RF power supply, DC power supply, corresponding power baffle, and substrate baffle, and stop sputtering for a period of time. Repeat this sputtering process using intermittent sputtering until the sputtering requirements are met.
[0018] Based on the above technical solution, preferably, the RF power supply power is 40 W, the DC power supply power is 10 W, the working gas pressure is 3 Pa, the argon flow rate is 85 sccm ~ 90 sccm, the sputtering temperature is 20 ~ 30 ℃, the sputtering bias voltage is 0 V ~ 200 V, and the substrate stage rotation speed is 10 ~ 20 rpm; the deposition is performed by intermittent sputtering, with each sputtering time being 15 mins and the interval time being 10 mins ~ 30 mins, and the thickness of the deposited bismuth telluride thermoelectric thin film layer is 0.1 μm ~ 2 μm.
[0019] Based on the above technical solutions, preferably, the curing temperature of the silver paste is 80~120 ℃ and the curing time is 0.5 h~1 h.
[0020] Based on the above technical solutions, preferably, after sputtering, the substrate is placed in the cavity and kept in a vacuum state for 0.5 h to 1 h.
[0021] Thirdly, the present invention also provides the application of the above-mentioned bismuth telluride thermoelectric device in wearable electronics and micro self-powered systems.
[0022] The bismuth telluride thermoelectric device, its preparation method, and its application disclosed in this invention have the following advantages over the prior art: (1) In terms of the fabrication process, this invention uses a process route that combines photopolymerization three-dimensional lattice structure printing, tube furnace pyrolysis, and magnetron sputtering coating with a substrate (3D printed substrate) to fabricate bismuth telluride thermoelectric devices with octahedral lattice structures. This process first uses photopolymerization three-dimensional printing technology to construct octahedral lattice structures with periodic spatial topological features, which can achieve precise control of lattice unit cell size, rod diameter, porosity, structural period, and overall shape. This avoids the problem that traditional processing methods are difficult to use to fabricate complex three-dimensional microstructures, and has the advantages of high design freedom, high forming accuracy, and strong structural customizability.
[0023] Subsequently, the long-chain organic compounds in the photocurable resin undergo carbonization transformation through tube furnace pyrolysis, forming a pyrolytic carbon lattice framework while largely maintaining the overall octahedral lattice topology. The carbonization shrinkage and structural densification during pyrolysis improve the strength, stiffness, and thermal stability of the rod itself; the resulting pyrolytic carbon structure also exhibits good chemical stability, which helps to address the low strength and poor temperature resistance of the original polymer framework. Therefore, the tube furnace pyrolysis process can transform the polymer template obtained from 3D printing into a pyrolytic carbon framework with load-bearing capacity and functional support.
[0024] Furthermore, this invention employs magnetron sputtering to deposit a bismuth telluride thermoelectric functional layer on the surface of a pyrolytic carbon octahedral lattice framework. Magnetron sputtering offers advantages such as relatively low deposition temperature, controllable film thickness, good film density, and high process repeatability, making it suitable for constructing bismuth telluride-based thermoelectric thin films on the surface of a pyrolytic carbon lattice framework. By adjusting the sputtering power, sputtering pressure, time, and target composition, the thickness, composition, and microstructure of the bismuth telluride film can be controlled, thereby endowing the lattice framework with thermoelectric conversion functionality.
[0025] In summary, this invention organically combines complex three-dimensional structure forming, pyrolytic carbon framework reinforcement, and bismuth telluride thermoelectric functional layer deposition. All important components are manufactured using 3D printing technology, achieving synergy between structural design and functional material preparation. This process not only enables the fabrication of three-dimensional octahedral lattice thermoelectric devices that are difficult to obtain using traditional planar processes, but also improves the structural stability, mechanical reliability, and thermoelectric functional integration capabilities of the devices while maintaining lightweight and high specific surface area characteristics.
[0026] (2) In terms of mechanical properties, compared with traditional thin film devices, during the pyrolysis process, the long-chain organic matter in the photocurable resin undergoes dehydrogenation, deoxygenation, aromatization and cross-linking rearrangement, generating amorphous carbon and graphitic sp. 2 Carbon structure and a small amount of sp 3 The cross-linked pyrolytic carbon phase. Because this invention employs partial pyrolysis, certain amorphous carbon structures, defect structures, and localized residual organic networks are retained within the material, making the members less prone to instantaneous brittle fracture under load. Simultaneously, the octahedral lattice structure itself absorbs external loads through member bending, node rotation, local buckling, and progressive deformation of elements, resulting in a certain degree of structural plasticity and deformation limit in the macroscopic structure. Therefore, the enhanced plasticity in this invention primarily stems from the buffering effect of the locally residual organic network and the gradual deformation capability of the lattice structure.
[0027] Furthermore, from the perspective of strength enhancement, the long polymer chains undergo carbonization shrinkage and structural densification during pyrolysis, reducing the free volume within the rods and enhancing the continuity of the carbon skeleton, thereby improving the material's elastic modulus, compressive strength, and load-bearing capacity. The carbon phase formed after pyrolysis possesses high stiffness and thermal stability, significantly improving the problems of low strength, poor heat resistance, and easy creep of the original photocurable resin. Simultaneously, the octahedral lattice is a typical three-dimensional truss-type load-bearing structure, with rods interconnected through spatial nodes, enabling the transfer and dispersion of external loads along multiple directions throughout the lattice network, reducing stress concentration in individual rods or localized areas. Especially under compressive or bending loads, the octahedral lattice structure can improve the overall structural stiffness through the synergistic load-bearing capacity of multiple rods, thus endowing the device with high specific strength and structural stability.
[0028] Meanwhile, from the perspective of the reasons for the improved toughness, the three-dimensional lattice framework after pyrolysis and carbonization can form a multi-level energy dissipation mechanism under external force. The heterogeneous carbon structure, microporous structure, and carbonization gradient formed by partial pyrolysis are conducive to interface debonding, frictional energy dissipation, and crack bridging during crack propagation, thereby improving the material's damage tolerance and fracture toughness.
[0029] In summary, this invention achieves simultaneous optimization of material composition and structural topology through collaborative design. The pyrolytic carbon phase generated by partial pyrolysis improves the strength and thermal stability of the rod body, while the octahedral lattice structure enhances the overall load-bearing efficiency and variation limit. The amorphous carbon structure, node connections, and three-dimensional topological network jointly enhance crack resistance and energy dissipation capabilities. Therefore, this pyrolytic carbon octahedral lattice structure can achieve a synergistic improvement in strength, plasticity, and toughness while maintaining lightweight characteristics, providing a stable three-dimensional mechanical support framework for the subsequent construction of high-strength, high-toughness, lightweight bismuth telluride thermoelectric devices.
[0030] (3) Regarding thermoelectric performance, this invention deposits a bismuth telluride thermoelectric functional layer on the surface of an octahedral lattice framework, which can increase the effective working area of the thermoelectric film within the same projected area. The three-dimensional lattice structure facilitates the formation of more sufficient heat flow transmission paths in the thickness and spatial directions of the device, thereby improving the utilization rate of temperature difference. The pyrolytic carbon framework provides structural support, which can improve the electrical continuity of the bismuth telluride film and reduce the impact of film cracking or local detachment on the overall electrical transmission. At the same time, the octahedral lattice framework can disperse external stress and reduce the damage to the brittle bismuth telluride film during bending, compression, or thermal cycling. Therefore, this device can improve output stability and service reliability while maintaining the thermoelectric conversion capability of bismuth telluride. Attached Figure Description
[0031] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0032] Figure 1 This is a process flow diagram for the fabrication of the bismuth telluride thermoelectric device of the present invention; Figure 2 The following figures show the equipment used in the preparation process of this invention: a) Photopolymerization 3D printer, b) Tube furnace, c) Magnetron sputtering equipment, and d) Mechanical property testing equipment. Figure 3 The diagram shows the unit cell model of the lattice structure used in Embodiment 1, Comparative Example 1 and Comparative Example 4 of the present invention. Figure a shows the octahedral lattice structure unit cell, Figure b shows the bcc lattice structure unit cell, and Figure c shows the fcc lattice structure unit cell. Figure 4 These are physical images of the octahedral lattice pyrolytic carbon skeletons of Embodiment 1, Comparative Example 1, and Comparative Example 4 of the present invention. Figure 5 This is a schematic diagram of the device assembly of the present invention; Figure 6 Figure a shows the assembled physical diagram of the bismuth telluride thermoelectric device of Embodiment 1 of the present invention. Figure a is a schematic diagram of the structure after packaging, and Figure b is an internal view of it. Figure 7 The diagram shows the specific strength and specific energy absorption of the octahedral structure of this invention at different d / L ratios; Figure 8 Figure a shows the performance test results of Examples 1-3 and Comparative Examples 1-6. Figure b shows the compressive stress-strain curve and the comparison of specific strength and specific energy absorption of different lattice structures. Figure 9 The output voltage and output power curves and output power comparison diagrams of the thermoelectric devices of Example 1 and Comparative Example 4 under different temperature differences are shown in Figure a. Figure a shows the output voltage and power curve of Example 1, Figure b shows the output voltage and power curve of Comparative Example 4, and Figure c shows the comparison of their maximum output power at different temperatures. Figure 10 Figure 1 shows the lightweight performance of the bismuth telluride thermoelectric device according to Embodiment 1 of the present invention. Figure 1a shows the device carrying a 3 kg weight, Figure 2b is a magnified view of a part of the device, and Figure 3c shows the lightweight performance. Figure 11 This is a test diagram of the output stability of the bismuth telluride thermoelectric device in Embodiment 1 of the present invention; Figure 12 This is a schematic diagram illustrating the application scenario of the bismuth telluride thermoelectric device in Embodiment 1 of the present invention. Detailed Implementation
[0033] The technical solutions of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, and not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.
[0034] In this invention, the 3D printing substrate is made of photosensitive toughness resin. Both the 3D printing substrate and the octahedral lattice resin framework are printed using photopolymerization 3D printing equipment. A substrate model is constructed using 3D modeling software. The substrate is 23mm long and wide, and 6mm high. A groove measuring 15mm long, 15mm wide, and 3mm deep is cut in the center of the substrate to accommodate the octahedral lattice pyrolytic carbon framework. After printing, residual resin is cleaned using an ultrasonic cleaner, and no secondary UV post-curing treatment is performed, thus preserving the toughness of the photosensitive toughness resin.
[0035] Example 1
[0036] This embodiment provides a lightweight, high-strength, and tough bismuth telluride thermoelectric device with an octahedral lattice structure, its fabrication method, and its application, specifically following these steps: (1) Construct the basic octahedral lattice unit cell structure using 3D modeling software (see Figure 3 (Figure a) The structure has a length, width, and height of 1.5 mm and a rod diameter of 0.3 mm. It was then expanded to a 4 × 4 × 4 lattice structure, with each octahedral lattice containing 64 basic structures. (2) Photosensitive toughness resin was selected as the material and printed using a photopolymer 3D printer. Each layer was 0.02 mm thick and the exposure time for each layer was 1.8 s. After printing, the printed octahedral lattice structure was removed, immersed in alcohol, and then cleaned with an ultrasonic cleaner to remove excess residual resin. Afterward, it was cured for 5 mins by ultraviolet irradiation. (3) Use a tube furnace to prepare pyrolytic carbon. Place the printed structure into the tube furnace, use a vacuum pump to remove the air in the tube, and slowly introduce high-purity argon. Set the heating rate to 3 ℃ / min. After reaching 350 ℃, keep it at that temperature for 4 hours, and then let it cool naturally to room temperature. (4) After the pyrolysis is completed, the octahedral lattice structure is placed on the substrate and then installed into the sputtering chamber. The thin film is grown by co-sputtering. The tellurium-bismuth alloy target is fixed on the DC power supply, and the tellurium elemental target is fixed on the RF power supply. The distance between the target and the substrate and the sputtering angle are adjusted. The mechanical pump and the molecular pump evacuate the vacuum in the chamber to 5 × 10⁻⁶ m³ / s. -4 After the pressure drops below Pa, high-purity argon gas is introduced and a bias voltage of 800 V is applied. The pulse duty cycle is set to 80%, and the substrate is cleaned using ionized argon ions. (5) After cleaning, adjust the argon flow rate to 85 sccm~90 sccm (in order to stabilize the gas pressure at 3 Pa, the argon flow rate will fluctuate slightly between 85 and 90, but the overall flow rate is 90). The working gas pressure is fixed at 3 Pa, the substrate rotation speed is set to 15 rpm, the sputtering temperature is set to 25 ℃, the RF power supply power is set to 40 W, the DC power supply power is set to 10 W, the sputtering bias voltage is set to 50 V, and the pulse duty cycle is set to 80%. Every 15 mins of sputtering, the RF and DC power supplies need to be turned off for 15 mins. Repeat this intermittent sputtering process 4 times to prevent the substrate temperature from rising due to continuous sputtering. At the same time, intermittent sputtering can allow the atoms on the film surface to fully relax, which is more conducive to the growth of the film. (6) After sputtering is complete, turn off the RF and DC power supplies, place the film in the high vacuum environment of the cavity for more than 30 mins and then take it out; (7) The octahedral lattice structure with the coating completed is connected to the 3D printing substrate using silver paste and cured at 100 °C for 1 h to allow the solvent in the silver paste to evaporate. Then, wires are soldered to the silver paste.
[0037] Example 2
[0038] The only difference between this embodiment and embodiment 1 is that in step (3), the heat preservation time is 2 hours, and the rest is the same as in embodiment 1.
[0039] Example 3
[0040] The only difference between this embodiment and embodiment 1 is that in step (3), the heat preservation time is 3 hours, and the rest is the same as in embodiment 1.
[0041] Example 4
[0042] This embodiment provides a lightweight, high-strength, and tough bismuth telluride thermoelectric device with an octahedral lattice structure, its fabrication method, and its application, specifically following these steps: (1)~(2) Same as Example 1; (3) Use a tube furnace to prepare pyrolytic carbon. Place the printed structure into the tube furnace, use a vacuum pump to remove the air in the tube, and slowly introduce high-purity argon. Set the heating rate to 1 ℃ / min. After reaching 250 ℃, keep it at that temperature for 8 h, and then let it cool naturally to room temperature. (4) Same as Example 1; (5) After cleaning, adjust the argon flow rate to 85 sccm~90 sccm (in order to stabilize the gas pressure at 3 Pa, the argon flow rate will fluctuate slightly between 85 and 90, but the overall flow rate is 90). The working gas pressure is fixed at 3 Pa, the substrate rotation speed is set to 10 rpm, the sputtering temperature is set to 20 ℃, the RF power supply power is set to 30 W, the DC power supply power is set to 5 W, the sputtering bias voltage is set to 30 V, and the pulse duty cycle is set to 80%. Every 15 mins of sputtering, the RF and DC power supplies need to be turned off for 30 mins. Repeat this intermittent sputtering process 4 times to prevent the substrate temperature from rising due to continuous sputtering. At the same time, intermittent sputtering can allow the atoms on the film surface to fully relax, which is more conducive to the growth of the film. (6) Same as Example 1; (7) The octahedral lattice structure with the coating completed is connected to the 3D printing substrate using silver paste and cured at 80 °C for 40 mins to allow the solvent in the silver paste to evaporate. Then, wires are soldered to the silver paste.
[0043] Example 5
[0044] This embodiment provides a lightweight, high-strength, and tough bismuth telluride thermoelectric device with an octahedral lattice structure, its fabrication method, and its application, specifically following these steps: (1)~(2) Same as Example 1; (3) Use a tube furnace to prepare pyrolytic carbon. Place the printed structure into the tube furnace, use a vacuum pump to remove the air in the tube, and slowly introduce high-purity argon gas. Set the heating rate to 10 ℃ / min. After reaching 500 ℃, keep it at that temperature for 0.5 h, and then let it cool naturally to room temperature. (4) Same as Example 1; (5) After cleaning, adjust the argon flow rate to 85 sccm~90 sccm (in order to stabilize the gas pressure at 3 Pa, the argon flow rate will fluctuate slightly between 85 and 90, but the overall flow rate is 90). The working gas pressure is fixed at 3 Pa, the substrate rotation speed is set to 20 rpm, the sputtering temperature is set to 30 ℃, the RF power supply power is set to 50 W, the DC power supply power is set to 15 W, the sputtering bias voltage is set to 150 V, and the pulse duty cycle is set to 80%. Every 15 mins of sputtering, the RF and DC power supplies need to be turned off for 10 mins. Repeat this intermittent sputtering process 4 times to prevent the substrate temperature from rising due to continuous sputtering. At the same time, intermittent sputtering can allow the atoms on the film surface to fully relax, which is more conducive to the growth of the film. (6) Same as Example 1; (7) The octahedral lattice structure with the coating completed is connected to the 3D printing substrate using silver paste and cured at 120 °C for 0.5 h to allow the solvent in the silver paste to evaporate. Then, wires are soldered to the silver paste.
[0045] Example 6
[0046] The only difference between this embodiment and Embodiment 1 is the rod diameter. The d / L ratio is adjusted to 0.125, 0.149, 0.175, 0.227, and 0.250 by changing the rod diameter. All other aspects are the same as in Embodiment 1. The results are shown in [link to Embodiment 1]. Figure 7 .
[0047] from Figure 7 The influence of octahedral lattice geometry on mechanical properties can be observed. While keeping the unit cell size constant (L = 1.5 mm), the d / L ratio was adjusted by changing the rod diameter. The results show that both specific strength and specific energy absorption exhibit a pattern of first increasing and then decreasing with increasing d / L, reaching their maximum values at d / L = 0.20 (Example 1), with specific strengths and specific energy absorptions of approximately 116 MPa·g. -1 ·cm 3 and 16 J·g -1 .
[0048] The reason is that a smaller rod diameter leads to insufficient rod stiffness, making it prone to local buckling during compression, thus limiting load-bearing capacity and energy absorption. As the rod diameter increases, the axial load-bearing capacity of the rod increases, and the stress distribution becomes more uniform, resulting in higher specific strength and specific energy absorption. However, when the rod diameter increases further, the relative density of the lattice increases, and the load-bearing efficiency per unit mass decreases, causing both properties to decline. Therefore, d / L=0.20 is the preferred geometric parameter for the octahedral lattice, which can achieve the best comprehensive mechanical properties while ensuring lightweight design. This provides a basis for the selection of octahedral lattice structure parameters in this invention, and this unit cell size and rod diameter are used in both the embodiments and comparative examples.
[0049] Comparative Example 1 The only difference between this comparative example and Example 1 is that the lattice unit cell structure constructed in step (1) is based on the bcc lattice unit cell structure (see Example 1). Figure 3 (See Figure b in the example), the rest of the content is the same as in Example 1.
[0050] Comparative Example 2 The only difference between this comparative example and comparative example 1 is that in step (3), the heat preservation time is 2 h, and the rest of the contents are the same as comparative example 1.
[0051] Comparative Example 3 The only difference between this comparative example and comparative example 1 is that in step (3), the heat preservation time is 3 h, and the rest is the same as comparative example 1.
[0052] Comparative Example 4 The only difference between this comparative example and Example 1 is that the lattice unit cell structure constructed in step (1) is based on the fcc lattice unit cell structure (see Figure 3(See Figure c in the original text), the rest of the content is the same as in Example 1.
[0053] Comparative Example 5 The only difference between this comparative example and comparative example 4 is that in step (3), the heat preservation time is 2 h, and the rest is the same as comparative example 4.
[0054] Comparative Example 6 The only difference between this comparative example and comparative example 4 is that in step (3), the heat preservation time is 3 h, and the rest is the same as comparative example 4.
[0055] from Figure 8 As can be seen, different lattice configurations and pyrolysis times have a significant impact on the compressive performance of the thermoelectric device. Under a compression loading rate of 2 μm / s, the peak load values for Examples 1, 2, and 3 were 43.79 MPa, 42.89 MPa, and 40.00 MPa, respectively, with an average of 42.22 MPa; the peak load values for Comparative Examples 1–3 were 8.31 MPa, 8.25 MPa, and 7.75 MPa, respectively, with an average of 8.10 MPa; and the peak load values for Comparative Examples 4–6 were 19.78 MPa, 16.38 MPa, and 15.75 MPa, respectively, with an average of 17.30 MPa. The average peak compressive strength of the Example group was approximately 5.2 times that of Comparative Examples 1–3 and 2.4 times that of Comparative Examples 4–6. The specific strength of Examples 1–3 was 113.0 MPa·cm⁻¹. 3 ·g -1 110.2 MPa·cm 3 ·g -1 and 98.4 MPa·cm 3 ·g -1 The average value is 107.2 MPa·cm. 3 ·g -1 These figures are approximately 1.9 times and 2.0 times the average values of the two comparative examples, respectively. The specific energy absorbed in Examples 1-3 are 15.8 J·g. -1 16.0 J·g -1 and 17.8 J·g -1 The average value is 16.5 J·g -1 It is close to the overall value of Comparative Examples 1-3, and about 2.0 times the average value of Comparative Examples 4-6. Figure 8 As shown in Figure a, the example group still exhibits certain stress fluctuations and sustained load-bearing capacity after reaching peak stress, indicating that the octahedral lattice structure can delay overall failure through stepwise buckling failure of the members. Therefore, the octahedral lattice structure used in this invention can achieve a balance between high peak compressive strength, specific strength, and energy absorption capacity.
[0056] from Figure 9As can be seen, as the temperature difference increases from 10 K to 30 K, the open-circuit voltage, output current, and maximum output power of the thermoelectric devices in Example 1 and Comparative Example 4 gradually increase, indicating that the prepared thermoelectric devices can continuously convert thermal energy into electrical energy under different temperature differences. The maximum output power of the thermoelectric device in Example 1 at temperature differences of 10 K, 20 K, and 30 K is approximately 0.06 nW, 0.58 nW, and 1.52 nW, respectively, while the corresponding maximum output power of the thermoelectric device in Comparative Example 4 is approximately 0.03 nW, 0.22 nW, and 0.55 nW, respectively. At a temperature difference of 30 K, the maximum output power of the thermoelectric device in Example 1 is approximately 2.7 times that of Comparative Example 4. The thermoelectric device in Example 1 has a larger effective output power range under the same temperature difference, indicating that the bismuth telluride thermoelectric thin film, silver paste electrode, and external wires on the surface of the octahedral lattice framework can form a more continuous electrical transport path, which is beneficial for reducing the equivalent internal resistance of the device and improving the output power under load matching conditions.
[0057] from Figure 10 As can be seen, the octahedral lattice bismuth telluride thermoelectric device prepared in Example 1 of this invention maintains its integrity when bearing a 3kg weight, with no obvious breakage or overall instability observed, indicating that the device has good structural load-bearing capacity. Furthermore, the device can be placed on soft carrier surfaces such as flower petals, visually demonstrating its low mass. The above results are consistent with... Figure 8 The high specific strength shown corroborates each other, indicating that the three-dimensional octahedral lattice structure can form an effective spatial load-bearing network with less material, maintaining high structural stability while reducing device mass, which is beneficial for reducing the additional load of the device on the wearable carrier.
[0058] from Figure 11 As can be seen from the results, the octahedral lattice bismuth telluride thermoelectric device prepared in Example 1 of this invention maintained a relatively stable output voltage of approximately 2.8 mV during a continuous test of about 700 s. The voltage fluctuated slightly at the beginning of the test, then gradually stabilized. No continuous attenuation, abrupt zeroing, or significant drift was observed throughout the test. This result indicates that under continuous temperature difference, the octahedral lattice framework, bismuth telluride thermoelectric film, silver paste electrode, and external wires can maintain a relatively stable thermo-electric coupling relationship and electrical connection state. The device exhibits good thermoelectric response stability and can provide a stable millivolt-level voltage output for low-power energy management, energy storage, and micro-sensing circuits.
[0059] from Figure 12As can be seen, the octahedral lattice bismuth telluride thermoelectric device prepared in this invention can be attached to the surface of the human body, generating electrical energy by utilizing the temperature difference between the human body and the external environment. With the appropriate connecting circuitry, the device can enable a mobile phone to enter a slow charging state, demonstrating the feasibility of the energy transfer link between human body heat harvesting, thermoelectric conversion, and terminal electrical energy input. This experiment primarily verifies the device's ability to collect low-grade heat energy and transfer electrical energy to an external terminal.
[0060] Literature comparison This study compared several existing methods with those reported in the prior art from four perspectives: preparation method, preparation temperature, structure, and mechanical properties. The relevant literature and patent reports are as follows: Reference 1: Feng et al., "Microalloyed medium-entropy alloy composite nanolattices with ultrahigh toughness and cyclability", which prepared octahedral polymer nanolattices by two-photon lithography and deposited CoCrNiTi using magnetron co-sputtering. 0.1 The medium-entropy alloy thin film, with an alloy shell approximately 30 nm thick, dissipates energy through surface wrinkling and plastic deformation, while the elastic polymer core facilitates structural recovery, allowing the lattice to maintain good structural integrity even under cyclic compressive strain exceeding 50%. This research primarily focuses on improving the toughness and cyclic stability of the nanolattice through the synergistic effect of the metal shell and polymer core, classifying it as a purely mechanical metamaterial without thermoelectric conversion capabilities. This invention utilizes a partially pyrolytic carbon octahedral lattice as a load-bearing framework, depositing a bismuth telluride thermoelectric thin film on its surface, and further integrating silver paste electrodes and a 3D-printed substrate to achieve integrated mechanical support, thermoelectric conversion, and device assembly.
[0061] Reference 2: Karthikeyan et al., "Three dimensional architected thermoelectric devices with high toughness and power conversion efficiency," fabricated a 4×4×4 face-centered cubic lattice using DLP 3D printing. After partial carbonization, p-type Sb₂Te₃ and n-type Bi₂Te₃ thin films were deposited by thermal evaporation, and assembled into a series thermoelectric device using Ni electrodes, Ag-Sn solder paste, and a ceramic plate. This device exhibited over 50% compressive deformation capacity, approximately 30 J / g specific energy absorption, and approximately 10% conversion efficiency under the influence of rod bending deformation. However, this invention employs an octahedral lattice configuration, where rod compression dominates under pressure. The film composition is controlled by Bi₂Te₃ / Te magnetron co-sputtering, and low-temperature bonding with the 3D-printed substrate is achieved using silver paste to avoid the thermal impact of Ag-Sn soldering and 220 °C assembly annealing on the brittle bismuth telluride film and interface. This invention primarily targets stable energy harvesting under relatively small temperature differences, such as human body heat and low-grade waste heat. Therefore, there are significant differences between the two in terms of lattice topology, thin film preparation, electrode connection and target application.
[0062] Reference 3: Surjadi et al., "Lightweight, ultra-tough, 3D-architected hybridcarbon microlattices," fabricated face-centered cubic microlattices using photopolymerization 3D printing and partial carbonization processes. The optimized lattice strength increased by more than 100 times, and it did not show significant fracture under compressive strain exceeding 50%, with a maximum specific energy absorption of 60 J / g. This research mainly focused on mechanical load-bearing and energy absorption, without involving thermoelectric functions. This invention further employs an octahedral lattice framework and integrates a bismuth telluride thermoelectric thin film, silver paste electrodes, and a 3D-printed substrate to achieve a high-strength and tough structure with thermoelectric conversion functionality.
[0063] Compared with the prior art, the technical effects of the present invention include the following: In terms of fabrication technology, existing bismuth telluride thermoelectric devices are mostly fabricated using methods such as planar thin-film deposition, bulk cutting and assembly, or flexible substrate transfer, which makes it difficult to obtain complex three-dimensional lattice structures, and there is a lack of effective synergy between structural forming and functional layer fabrication. This invention employs a process route combining photopolymerization 3D printing, tube furnace pyrolysis, and magnetron sputtering deposition. First, high-precision forming of an octahedral lattice structure is achieved through photopolymerization 3D printing. Then, the polymer lattice is transformed into a pyrolytic carbon framework through pyrolysis. Finally, a bismuth telluride thermoelectric functional layer is deposited on the framework surface by magnetron sputtering. This method organically combines the fabrication of complex three-dimensional structures, carbon-based framework reinforcement, and thermoelectric functional layer construction, offering advantages such as a clear process route, strong structural designability, controllable functional layer thickness, and a high degree of structural-functional integration.
[0064] Structurally, existing flexible thermoelectric devices are mostly planar, thin-film, or simple support structures, relying mainly on flexible substrates to buffer external deformation, making it difficult to simultaneously achieve lightweight, three-dimensional load-bearing capacity, and high effective working area. This invention introduces an octahedral lattice structure as the three-dimensional support framework for the thermoelectric device. This structure, composed of periodic rods and nodes, features lightweight, high specific surface area, and multi-directional load-bearing capacity. Compared to traditional planar thermoelectric devices, the octahedral lattice structure not only provides continuous support for the bismuth telluride functional layer but also increases the effective deposition area and spatial distribution range of the thermoelectric thin film, thereby realizing the transformation from planar thermoelectric structures to three-dimensional integrated structural and functional thermoelectric devices.
[0065] In terms of mechanical properties, existing bismuth telluride-based thermoelectric thin films generally suffer from high brittleness, weak bending resistance, and susceptibility to cracking during service, limiting their application in flexible wearable devices and complex curved surface heat sources. This invention supports and reinforces the bismuth telluride thermoelectric layer using an octahedral lattice framework. The pyrolytic carbon framework possesses high strength, stiffness, and thermal stability, while the octahedral lattice structure reduces stress concentration through synergistic load-bearing by rods, stress dispersion at nodes, and localized progressive deformation. When the device is subjected to bending, compression, or impact loads, the three-dimensional lattice framework dissipates energy through rod bending, node rotation, local buckling, and crack deflection, thereby improving the device's strength, toughness, and damage tolerance, and reducing cracking and failure of the bismuth telluride functional layer.
[0066] In terms of thermoelectric performance, existing planar thin-film thermoelectric devices are limited by the film area, temperature difference in the thickness direction, and electrical transport stability. Their actual output performance is easily affected by temperature difference attenuation, film cracking, and interface failure. This invention deposits a bismuth telluride thermoelectric functional layer on the surface of a three-dimensional octahedral lattice framework. This increases the effective working area of the thermoelectric film within the same projected area and creates richer spatial heat flow transport paths, which is beneficial for improving heat capture capability and temperature difference utilization. Simultaneously, the pyrolytic carbon framework provides a certain degree of continuous support, improving the electrical connection stability of the bismuth telluride film in complex structures and reducing the impact of local cracking or detachment on the overall electrical transport path. Therefore, this structure is beneficial for improving the stability of the device's output power and its long-term service reliability.
[0067] In terms of connection and assembly, this invention uses silver paste to connect the lattice thermoelectric units, wires, and the 3D printed substrate. Compared with high-temperature welding, silver paste has a lower curing temperature, which can reduce the thermal impact of the connection process on the bismuth telluride thermoelectric thin film; the 3D printed substrate can be designed according to the size, arrangement, and wire position of the thermoelectric units.
[0068] In summary, this invention achieves a unified approach to fabrication process, structural configuration, mechanical properties, and thermoelectric functionality through a synergistic design of an octahedral lattice structure, a pyrolytic carbon-reinforced framework, a bismuth telluride thermoelectric functional layer, and a silver paste-connected 3D-printed substrate. This device maintains the thermoelectric conversion capability of bismuth telluride while improving structural load-bearing capacity and output stability, making it suitable for applications such as flexible wearable energy devices, power supply for micro-sensors, and energy harvesting from complex curved surface heat sources.
[0069] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A lightweight, high-strength, and tough bismuth telluride thermoelectric device, characterized in that: It includes an octahedral lattice pyrolytic carbon framework, bismuth telluride thermoelectric thin film, silver paste electrode, wires and substrate; The bismuth telluride thermoelectric thin film is deposited on the surface of an octahedral lattice pyrolytic carbon framework. An octahedral lattice pyrolytic carbon framework loaded with the bismuth telluride thermoelectric thin film is fixed to and electrically connected to the substrate via silver paste electrodes. The wire is electrically connected to the silver paste electrode.
2. The lightweight, high-strength, and tough bismuth telluride thermoelectric device as described in claim 1, characterized in that: The method for preparing the octahedral lattice pyrolytic carbon skeleton is as follows: using photosensitive toughening resin as the printing material, an octahedral lattice resin skeleton is prepared by photopolymerization 3D printing technology, and then the octahedral lattice resin skeleton is heat-treated under an inert atmosphere to obtain an octahedral lattice pyrolytic carbon skeleton.
3. The lightweight, high-strength, and tough bismuth telluride thermoelectric device as described in claim 2, characterized in that: The octahedral lattice resin skeleton is formed by connecting multiple octahedral lattice unit cells in a periodic array along the X, Y, and Z directions. Each octahedral lattice unit cell includes several rods and spatial nodes connecting the rods. The rods form a three-dimensional truss load-bearing network through the spatial nodes. The length, width, and height of each octahedral lattice unit cell are all L, where L is 1.5 mm. The diameter d of each rod is 0.188 mm to 0.375 mm, and the d / L ratio is 0.125 to 0.
25.
4. The lightweight, high-strength, and tough bismuth telluride thermoelectric device as described in claim 2, characterized in that: The heat treatment temperature is 250 ℃~500 ℃, the heat treatment time is 0.5 h~8 h, the heating rate is 1 ℃ / min~10 ℃ / min, and the inert atmosphere is argon.
5. A method for preparing a lightweight, high-strength, and tough bismuth telluride thermoelectric device as described in any one of claims 1-4, characterized in that: Includes the following steps: S1, a bismuth telluride thermoelectric thin film layer is deposited on the surface of the octahedral lattice pyrolytic carbon skeleton using magnetron sputtering. S2, using silver paste to connect the octahedral lattice pyrolytic carbon skeleton that has been coated to the substrate, and curing it to form a silver paste electrode connected to the bismuth telluride thermoelectric thin film layer; S3, connect the wires to the silver paste electrode to obtain the thermoelectric device.
6. The method for fabricating a lightweight, high-strength, and tough bismuth telluride thermoelectric device as described in claim 5, characterized in that: In step S1, magnetron co-sputtering is performed using a tellurium-bismuth alloy target and a tellurium elemental target, wherein the tellurium-bismuth alloy target is connected to a DC power supply and the tellurium elemental target is connected to an RF power supply.
7. The method for fabricating a lightweight, high-strength, and tough bismuth telluride thermoelectric device as described in claim 5, characterized in that: The RF power supply has a power of 30~50 W, the DC power supply has a power of 5~15 W, the working gas pressure is 3 Pa, the argon flow rate is 85 sccm~90 sccm, the sputtering temperature is 20~30 ℃, the sputtering bias voltage is 0 V~200 V, and the substrate stage rotation speed is 10~20 rpm. Deposition is performed by intermittent sputtering, with each sputtering time being 15 mins and the interval time being 10 mins~30 mins. The thickness of the bismuth telluride thermoelectric thin film layer formed by deposition is 0.1 μm~2 μm.
8. The method for preparing a lightweight, high-strength, and tough bismuth telluride thermoelectric device as described in claim 5, characterized in that: The curing temperature of the silver paste is 80~120 ℃, and the curing time is 0.5 h~1 h.
9. The method for fabricating a lightweight, high-strength, and tough bismuth telluride thermoelectric device as described in claim 5, characterized in that: The cavity vacuum was evacuated to 5×10 before sputtering. -4 The octahedral lattice pyrolytic carbon framework is cleaned with argon ions below Pa.
10. The application of a lightweight, high-strength, and tough bismuth telluride thermoelectric device as described in any one of claims 1-4 in wearable electronics and micro self-powered systems.