Preparation method of pyroelectric chip low-thermal-conductivity structure and application thereof

By combining photolithography and acid etching to prepare Cr/Au metal protective layers and suspended structures, the low thermal conductivity problem of ultrathin pyroelectric chips was solved, enabling efficient mass production and performance improvement.

CN123165019APending Publication Date: 2026-11-24KUNMING INST OF PHYSICS
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611345676.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-01
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing technologies lack methods for fabricating low thermal conductivity structures compatible with ultrathin (<25μm) pyroelectric chips, which limits the performance improvement of pyroelectric infrared detectors.

Method used

A Cr/Au metal layer was prepared as a protective layer using photolithography masking, and a suspended low thermal conductivity structure was formed by etching a glass substrate with acid solution. The acid etching process was controlled by acetone solution cleaning and magnetic stirring, resulting in a low thermal conductivity structure that is easy to operate and has a high yield.

Benefits of technology

Mass production of ultrathin pyroelectric chips has been achieved, reducing thermal conductivity and improving performance. The specific detectivity of the 15μm thick chip is increased by 10 times, which is 42% higher than that of the self-supporting chip, and the yield is greater than 90%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123165019A_ABST
    Figure CN123165019A_ABST
Patent Text Reader

Abstract

This invention discloses a method for fabricating a low thermal conductivity structure for a pyroelectric chip and its application, belonging to the field of infrared detection technology. The fabrication method includes: (1) preparing a specific pattern on a surface-treated glass substrate using photolithography; (2) preparing a Cr / Au metal layer on the glass surface using magnetron sputtering; (3) ultrasonically cleaning the glass with acetone solution to remove part of the Cr / Au metal layer, leaving a Cr / Au metal layer with a specific pattern as a protective layer; (4) etching the glass with an acid solution to form a suspended low thermal conductivity structure under the pyroelectric chip. The low thermal conductivity structure prepared by this invention can effectively support the mass production of ultrathin (<25μm) pyroelectric chips, reducing the thickness of the pyroelectric chip to 15μm. Compared with a 15μm pyroelectric chip with a glass substrate, the performance is improved by 10 times, and compared with a self-supporting 25μm pyroelectric chip, the performance is improved by 42%, showing significant application prospects in the field of pyroelectric devices.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of infrared detection technology, and more specifically, relates to a method for preparing a pyroelectric chip with low thermal conductivity and its application. Background Technology

[0002] A pyroelectric infrared detector is a sensor that uses the pyroelectric effect to detect infrared radiation. The pyroelectric effect refers to the phenomenon that certain materials generate electrical charges or voltages when their temperature changes. This effect mainly occurs in materials with polar crystal structures (such as lithium tantalate, lead zirconate titanate, and barium strontium titanate). When their temperature changes, the electric dipoles inside the crystal rearrange, leading to charge accumulation on the material surface and generating an electrical response to the radiation signal. Because the signal of a pyroelectric infrared detector originates from temperature changes and responds across the entire spectrum, it is widely used in security, automation, medical, and environmental monitoring fields.

[0003] To meet the application requirements of pyroelectric infrared detectors in high-precision detection fields, improving the performance of pyroelectric devices is crucial. The specific detectivity of pyroelectric infrared detectors is inversely proportional to both the thickness of the pyroelectric material and the thermal conductivity of the chip. Therefore, to improve the performance of pyroelectric devices, it is necessary to minimize the thickness of the pyroelectric chip while simultaneously reducing its thermal conductivity.

[0004] Several solutions for reducing the thermal conductivity of pyroelectric detectors have been proposed in existing technologies. For example, one solution uses a bridge-type suspended structure, utilizing the directional etching characteristics of silicon to create a window behind the detector element, using air to prevent heat diffusion; however, its biggest drawback is poor mechanical strength. Air gap structures create air gaps by etching silicon nitride or phosphosilicate glass under the bottom electrode of the detector element to prevent heat flow, but this requires multiple etching or photolithography processes and suffers from lateral etching problems. Microbridge structures utilize MEMS technology to fabricate silicon nitride thin film "microbridges" on silicon wafers, but the process is complex and difficult. Another solution uses porous SiO2 as an insulating layer, but the sol-gel method is complex, with poor repeatability and stability. Furthermore, some solutions reduce thermal conductivity by setting alternating layers of SiO2 and TiO2 nanoarrays in the insulating support structure, or by using a support pillar array combined with a sacrificial layer to form a suspended self-supporting structure. Still other solutions employ a suspended membrane structure with a four-sided fixed substrate, introducing insulating and heat-insulating materials between the suspended membrane and the supporting substrate to reduce thermal conductivity.

[0005] Because air has very low thermal conductivity, most pyroelectric chips currently employ a self-supporting design (without a substrate) to reduce thermal conductivity. However, as the thickness of pyroelectric chips decreases (<25μm), self-supporting chips become extremely prone to breakage, significantly reducing chip yield and making them unsuitable for mass production. Therefore, the maximum application thickness of currently mass-produced pyroelectric chips is greater than 25μm, which limits further improvements in the performance of pyroelectric infrared detectors.

[0006] In summary, the existing technology lacks a method for fabricating low thermal conductivity structures compatible with ultrathin (<25μm) pyroelectric chips. Summary of the Invention

[0007] In view of the above-mentioned defects or improvement needs of the existing technology, the present invention provides a method for preparing a low thermal conductivity structure of pyroelectric chip, which aims to be compatible with the mass production of ultrathin (<25μm) pyroelectric chips, thereby further improving the performance limit of pyroelectric infrared detectors.

[0008] A method for fabricating a low thermal conductivity structure for a pyroelectric chip includes the following steps:

[0009] (1) Provide a glass substrate and perform surface treatment on the glass substrate;

[0010] (2) A photoresist pattern is formed on a surface-treated glass substrate using a photomask method;

[0011] (3) A Cr / Au metal layer was prepared on the glass surface using magnetron sputtering;

[0012] (4) Use acetone solution to ultrasonically clean the glass, peel off part of the Cr / Au metal layer, leaving a Cr / Au metal layer with a specific pattern. This metal layer serves as a protective layer in the subsequent acid etching step.

[0013] (5) Use an acid solution to etch the glass to form a suspended low thermal conductivity structure in the glass substrate below the protective layer.

[0014] Preferably, the glass substrate mentioned in step (1) is one of quartz glass, borosilicate glass, or soda-lime glass, and preferably borosilicate glass with a thickness of 300 μm. Borosilicate glass has good mechanical properties and is easily corroded by strong acid solutions, which makes the subsequent etching preparation of low thermal conductivity structures simple and efficient.

[0015] Preferably, the surface treatment in step (1) is argon plasma surface cleaning with a power of 100-300W and a treatment time of 100-300s. This treatment can enhance the interfacial adhesion between the metal layer and the glass, making it less likely to fall off during acid corrosion and providing better protection.

[0016] Preferably, the thickness of the Cr / Au metal layer in step (2) should be at least greater than 500 nm.

[0017] Preferably, the acid solution in step (4) includes one or more combinations of nitric acid, hydrofluoric acid, and hydrochloric acid, and is preferably a nitric acid solution with a concentration of 30 wt%.

[0018] This invention also protects a low thermal conductivity structure for a pyroelectric chip, which is prepared according to the preparation method described above.

[0019] The present invention also protects the application of the low thermal conductivity structure prepared above, the application including as a low thermal conductivity substrate for pyroelectric chips prepared from different materials.

[0020] The beneficial effects of this invention are:

[0021] (1) The present invention uses photolithography mask method to prepare Cr / Au metal protective layer. This protective layer is easy to pattern, customize and mass-produce, and has a good protective effect during acid etching.

[0022] (2) The present invention uses acid solution to etch glass substrate to form a suspended low thermal conductivity structure. This method is easy to operate and prepare, and the yield is greater than 90%.

[0023] (3) The low thermal conductivity structure prepared by the present invention can be effectively compatible with the preparation of ultrathin (<25μm) pyroelectric chips, and can reduce the thickness of pyroelectric chips to 15μm. Compared with 15μm pyroelectric chips with glass substrates, the performance is improved by 10 times, and compared with 25μm pyroelectric chips with self-supporting structure, the performance is improved by 42%. Attached Figure Description

[0024] Figure 1 This is a schematic diagram of the low thermal conductivity pyroelectric chip in this invention. In the figure: 1—PZT pyroelectric chip; 2—glass substrate; 3—suspended structure formed after the glass substrate is etched.

[0025] Figure 2 The frequency-specific detectivity performance curves of the 15μm low thermal conductivity pyroelectric chip, the 15μm glass substrate pyroelectric chip, and the 25μm self-supporting pyroelectric chip prepared in this invention are shown.

[0026] Figure 3 This is a photograph of the low thermal conductivity structure after corrosion in this invention. The gold-colored Cr / Au metal protective layer around the holes can be seen in the figure. Detailed Implementation

[0027] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the invention. Furthermore, the technical features involved in the various embodiments of this invention described below can be combined with each other as long as they do not conflict with each other.

[0028] Example 1

[0029] A method for fabricating a low thermal conductivity structure for a pyroelectric chip includes the following steps:

[0030] (1) Use acetone and ethanol solution to ultrasonically clean the glass substrate for 15 min each, and then use an argon plasma surface cleaner to perform surface treatment on the glass substrate. The power is 300W and the treatment time is 200s.

[0031] (2) Spin-coat photoresist onto the surface of a glass substrate and cure at 90°C for 5 min. The photoresist thickness is approximately 1 μm. Expose the substrate to a photolithography machine using a mask for 18 s and then develop the photoresist to obtain a specific pattern.

[0032] (3) A Cr / Au metal layer was prepared on the glass surface by magnetron sputtering. The thickness of the Cr / Au metal layer was 700 nm.

[0033] In the Cr / Au metal layer, the Cr layer serves as an adhesion layer with a thickness of 50-100 nm; the Au layer serves as an anti-corrosion protective layer with a thickness of 600-650 nm. The thickness ratio of the Cr and Au layers can be adjusted according to specific corrosion conditions to ensure that the protective layer does not peel off or dissolve during acid corrosion.

[0034] (4) Use acetone solution to ultrasonically clean the glass for 5 minutes, peel off part of the Cr / Au metal layer, leaving the Cr / Au metal layer with a specific pattern, and then rinse the glass substrate surface with acetone and alcohol solution respectively, and blow dry with nitrogen.

[0035] (5) The borosilicate glass substrate was etched using a 30wt% nitric acid solution. During the etching process, the nitric acid solution was kept at a temperature of 25°C, and magnetic stirring was used to maintain the flow of the nitric acid solution. In addition, every 10 minutes during the etching process, the reactants deposited in the holes were rinsed off with water to ensure that the bottom of the holes was in contact with the nitric acid, thereby increasing the aperture ratio of the holes and reducing the side-drilling effect of the acid solution. After etching, the glass substrate was rinsed with deionized water, acetone, and alcohol, respectively, and dried with nitrogen to complete the fabrication of the low thermal conductivity structure of the pyroelectric chip.

[0036] In the low thermal conductivity structure prepared in this embodiment, the suspended region formed by etching the glass substrate is rectangular, with its length and width matching the size of the photosensitive area of ​​the pyroelectric chip. The depth of the suspended region (i.e., the thickness of the glass removed by etching) is 200-280 μm, and the thickness of the remaining glass substrate is 20-100 μm. The size and depth of the suspended region can be adjusted by controlling the size of the mask pattern and the acid etching time.

[0037] The structure of a low thermal conductivity pyroelectric chip is as follows: Figure 1 As shown, the top layer is a chip of PZT pyroelectric material, bonded to the glass substrate surface using optical adhesive. The chip thickness is 15 μm. Directly below the pyroelectric chip is the low thermal conductivity structure prepared in this invention, as shown in the physical diagram. Figure 3 As shown.

[0038] Comparative Example 1

[0039] The difference between this embodiment and Embodiment 1 is that the method of the present invention is not used to prepare the low thermal conductivity structure of the pyroelectric chip; that is, the pyroelectric chip is placed on a solid glass substrate with a chip thickness of 15 μm.

[0040] Comparative Example 2

[0041] In this embodiment, the pyroelectric chip is fabricated using a self-supporting method, without any substrate underneath, and the chip thickness is 25 μm. This chip thickness represents the limit in the fabrication of self-supporting chips; when the thickness is less than 25 μm, it is extremely prone to breakage and has little significance in mass production.

[0042] Performance Testing and Comparison

[0043] The pyroelectric chips prepared in the above three embodiments were assembled into devices (with identical circuits), and signal-noise tests were performed on them respectively. Then, the specific detectivity of each device was calculated. For example... Figure 2 As shown, the maximum specific detectivity of the pyroelectric chip on a 15μm glass substrate is 3.9×10⁻⁶. 8 The maximum specific detectivity of the 15μm low thermal conductivity pyroelectric chip is as high as 4.0×10⁻¹ cm·Hz¹ / ²·W⁻¹. 9 The performance is improved by 10 times, achieving a resolution of cm·Hz¹ / ²·W⁻¹. Furthermore, compared to a 25μm self-supporting pyroelectric chip, its maximum specific detectivity is 2.8×10⁻¹. 8 The performance of the 15μm low thermal conductivity pyroelectric chip was improved by 42%, increasing the performance ceiling of PZT pyroelectric chips. The comparison of the above three embodiments effectively demonstrates that the low thermal conductivity structure prepared in this invention has a significant effect on improving the performance of pyroelectric devices and has important application prospects in pyroelectric devices.

[0044] Tests showed that the thermal conductivity of the low thermal conductivity pyroelectric chip prepared in this embodiment was reduced by about 90% compared with that of a pyroelectric chip with a glass substrate of the same thickness. The air gap in the suspended structure effectively blocked the heat conduction path from the pyroelectric chip to the glass substrate, thereby significantly reducing the overall thermal conductivity of the chip.

[0045] Those skilled in the art will readily understand that the above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.

Claims

1. A method for fabricating a low thermal conductivity structure for a pyroelectric chip, characterized in that, Includes the following steps: (1) Provide a glass substrate and perform surface treatment on the glass substrate; (2) A photoresist pattern is formed on a surface-treated glass substrate using a photomask method; (3) A Cr / Au metal layer is deposited on the surface of the glass substrate by magnetron sputtering; (4) Use acetone solution to strip the Cr / Au metal layer on the photoresist pattern, and retain the Cr / Au metal layer that is complementary to the photoresist pattern as a protective layer. (5) The glass substrate is etched with an acid solution to form a suspended structure in the glass substrate below the protective layer.

2. The method according to claim 1, characterized in that, The surface treatment is argon plasma surface cleaning with a power of 100-300W and a processing time of 100-300s.

3. The method according to claim 1, characterized in that, The total thickness of the Cr / Au metal layer is greater than 500 nm.

4. The method according to claim 3, characterized in that, The thickness of the Cr layer in the Cr / Au metal layer is 50-100 nm, and the thickness of the Au layer is 600-650 nm.

5. The method according to claim 1, characterized in that, The acid solution is a nitric acid solution with a mass concentration of 30%.

6. The method according to claim 1, characterized in that, In step (5), the corrosion is carried out at 25°C and the acid solution is kept flowing by magnetic stirring.

7. The method according to claim 6, characterized in that, During the corrosion process, the corrosion pores are flushed with water every 10 minutes to remove the deposited reactants.

8. The method according to claim 1, characterized in that, The suspended structure is used to support pyroelectric chips with a thickness of less than 25 μm.

9. A low thermal conductivity structure for a pyroelectric chip, characterized in that, Prepared by the method described in any one of claims 1 to 8.

10. The application of the low thermal conductivity structure of the pyroelectric chip according to claim 9 in the fabrication of a pyroelectric infrared detector.