Semiconductor layer comprising doped tin oxide

By doping a tin oxide semiconductor layer and annealing it in a synthesis gas, the problem of increased electron carriers in the tin oxide semiconductor layer during synthesis gas annealing was solved, thereby improving the current control capability and overall performance of the transistor.

CN123165033APending Publication Date: 2026-11-24ASM IP HLDG BV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202610678531.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2025-05-21
Filing Date
2026-05-18
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

During annealing in a syngas process, hydrogen bonds with oxygen in tin oxide semiconductor layers, leading to an increase in the number of electron carriers. This makes it difficult for the gate to effectively control the current, affecting its performance as a transistor channel material.

Method used

By doping a tin oxide semiconductor layer with elements such as Zr, Hf, Ge, La, Si, Nb, and Ta, and combining this with vapor deposition technology, a doped tin oxide semiconductor layer is formed on the substrate surface, and then annealed in a synthesis gas to form the gate dielectric and conductive contacts.

Benefits of technology

The conduction band characteristics of the tin oxide semiconductor layer were improved, the gate's ability to control current was enhanced, and the overall performance of the transistor was improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123165033A_ABST
    Figure CN123165033A_ABST
Patent Text Reader

Abstract

The present disclosure relates to a method of depositing a semiconductor layer comprising doped tin oxide, a method for manufacturing a semiconductor structure comprising a semiconductor layer comprising doped tin oxide, and a structure comprising a semiconductor layer comprising doped tin oxide.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for depositing a semiconductor layer comprising doped tin oxide, a method for manufacturing a semiconductor structure comprising a semiconductor layer comprising doped tin oxide, and a structure comprising a semiconductor layer comprising doped tin oxide. Background Technology

[0002] Tin oxide (SnO2) is a semiconductor. Because the reduction / oxidation potential (ε(+ / -)) of hydrogen is within the conduction band of tin oxide, when tin oxide undergoes syngas annealing, hydrogen in the syngas bonds with oxygen in the tin oxide. As a result, hydrogen acts as an electron donor, increasing the number of electron carriers in the tin oxide. This makes tin oxide unsuitable as a channel material in transistors because the gate cannot effectively control the current within it. Summary of the Invention

[0003] This synopsis is provided to introduce some concepts in a simplified form. These concepts are further described in detail in the following detailed description of exemplary embodiments of this disclosure. This synopsis is not intended to require the identification of key or essential features of the claimed subject matter, nor is it intended to limit the scope of the claimed subject matter.

[0004] To improve the properties of tin oxide-containing semiconductor layers during synthesis gas annealing, this disclosure proposes doping the semiconductor layer with one or more elements, resulting in an increase in the minimum conduction band value of the semiconductor layer. These one or more elements may be Zr, Hf, Ge, La, Si, Nb, and / or Ta.

[0005] In one aspect, the method according to this disclosure is a method for depositing a semiconductor layer comprising tin oxide, the method comprising:

[0006] A substrate with a surface is provided in the reaction chamber;

[0007] Perform multiple deposition cycles, each cycle including:

[0008] (a) A first gaseous precursor is supplied to the reaction chamber to contact the surface, the first precursor containing a first chemical element, the first chemical element being Sn;

[0009] (b) Providing a gaseous second precursor to the reaction chamber for contact with the surface, the second precursor comprising a second chemical element selected from Zr, Hf, Ge, La, Si, Nb, and Ta; and

[0010] (c) A gaseous first reactant is supplied to the reaction chamber to contact the surface, the first reactant containing a third chemical element, which is O.

[0011] In some examples, each deposition cycle includes a single-step (a) and a single-step (b) step.

[0012] In some examples, in at least some loops, steps (a), (b), and (c) are performed in the following order: step (a), step (b), and step (c).

[0013] In some examples, the surface comprises a semiconductor material or a dielectric material.

[0014] In some examples, in the semiconductor layer, the ratio of the number of atoms N2 of the second chemical element to the number of atoms N1 of the first chemical element is between 1% and 50% (0.01≤N2 / N1≤0.50).

[0015] In some examples, the semiconductor layer includes a planar portion with a length of at least 10 nm.

[0016] In some examples, the semiconductor layer has a thickness between 0.5 nm and 10 nm.

[0017] In some examples, the first precursor is selected from SnCl4, SnBr4, SnI4, Sn(NMe2)4, Sn(NEtMe)4, Sn(NEt2)4, Sn(dmap)2, Sn(dmamp)2, Sn(dmamb)2, Sn(OtBu)4, Sn(OtPn)4, Sn(OAm)4, Sn(acac)2, Sn(N(SiMe3)2)2, Sn(tbba), SnMe4, SnEt4, SnHBu3, Sn(iPr2FMD)2, Sn(DMP)4.

[0018] In some embodiments, the second chemical element is Zr, and the second precursor is selected from ZrCl4, ZrI4, Zr(NMe2)4, Zr(NEtMe)4, Zr(NEt2)4, Zr(thd)4, Zr(OiPr)4, Zr(OtBu)4, ZrCp(NMe2)3, Zr(MeCp)(NMe2)3, Zr(EtCp)(NMe2)3, ZrCp(NEt2)3, Zr(MeCp)(NEt2)3, Zr(EtCp)(NEt2)3, ZrCp(NEtMe)3, Zr(MeCp)(NEtMe)3, Zr(EtCp)(NEtMe)3, Zr Cp2Cl2, ZrCp2Me2, ZrCp2(OMe)2, ZrCp2Me(OMe), ZrCp2(NMe2)2, Zr(MeCp)2Cl2, Zr(MeCp)2Me2, Zr(MeCp)2(OMe)2, Zr(MeCp)2Me(OMe), Zr( MeCp)2(NMe2)2, Zr(EtCp)2Cl2, Zr(EtCp)2Me2, Zr(EtCp)2(OMe)2, Zr(EtCp)2Me(OMe), Zr(EtCp)2(NMe2)2, ZrNp4 and ZrCp(tBu2DAD)(OiPr).

[0019] In some examples, the first reactant is selected from H2O, H2O2, O2, O3, N2O, NO, NO2, oxygen plasma, N-oxide, N-oxygen compound, metal alkoxide or alcohol oxidant.

[0020] In some examples, step (a) lasts at least twice as long as step (b).

[0021] In some examples, the method includes a purging step between each of steps (a), (b), and (c).

[0022] In one aspect, the method according to this disclosure is a method for manufacturing a semiconductor structure including a semiconductor layer comprising tin oxide, the method comprising:

[0023] Semiconductor layers are deposited through the following methods:

[0024] A substrate with a surface is provided in the reaction chamber;

[0025] Perform multiple deposition cycles, each cycle including:

[0026] (a) A first gaseous precursor is supplied to the reaction chamber to contact the surface, the first precursor containing a first chemical element, the first chemical element being Sn;

[0027] (b) Providing a gaseous second precursor to the reaction chamber for contact with the surface, the second precursor comprising a second chemical element selected from Zr, Hf, Ge, La, Si, Nb, and Ta; and

[0028] (c) A gaseous first reactant is supplied to the reaction chamber to contact the surface, the first reactant containing a third chemical element, the third chemical element being O;

[0029] A dielectric layer is formed to form the gate dielectric; and

[0030] Conductive contacts are formed to form gate contacts;

[0031] The method includes annealing in a synthesis gas containing hydrogen.

[0032] In some examples, the semiconductor layer forms the transistor channel.

[0033] In some examples, annealing is performed at temperatures between 300°C and 500°C.

[0034] In some examples, annealing lasts between 30 minutes and 4 hours.

[0035] In some examples, the semiconductor structure includes or is included in the following: memory, dynamic random access memory (DRAM), three-dimensional dynamic random access memory, charge-coupled device memory, gain unit memory, sensor, processor, controller, logic circuit, image sensor, transistor, horizontal transistor, vertical transistor, and transistor built on top of a silicon wafer and separated from the silicon wafer by at least one electrical isolation layer.

[0036] In one aspect, the structure according to this disclosure is a structure comprising a substrate having a surface and a semiconductor layer deposited on the surface, the semiconductor layer comprising:

[0037] The first chemical element, Sn;

[0038] The second chemical element is selected from Zr, Hf, Ge, La, Si, Nb, and Ta; and

[0039] The third chemical element is O;

[0040] In the semiconductor layer,

[0041] The ratio of the number of atoms of the second chemical element N2 to the number of atoms of the first chemical element N1 is between 1% and 50% (0.01 ≤ N2 / N1 ≤ 0.50), and

[0042] The ratio of the number of atoms of the third chemical element N3 to the number of atoms of the first and second chemical elements (N1+N2) is between 1.0 and 4.0 (1.0≤N3 / (N1+N2)≤4.0).

[0043] In some examples, the semiconductor layer includes a planar portion with a length of at least 10 nm.

[0044] In some examples, the semiconductor layer includes a channel portion, a source portion, and a drain portion, with the source and drain portions having a higher dopant concentration than the channel portion. Attached Figure Description

[0045] These and other aspects of this disclosure will be explained in more detail by way of examples and with reference to the accompanying drawings, wherein:

[0046] Figure 1a A method according to an exemplary embodiment of the present disclosure is shown.

[0047] Figure 1b A method according to an exemplary embodiment of the present disclosure is shown.

[0048] Figure 2 A method according to an exemplary embodiment of the present disclosure is shown.

[0049] Figure 3 An exemplary structure according to an exemplary embodiment of the present disclosure is shown.

[0050] Figure 4 An exemplary structure according to an exemplary embodiment of the present disclosure is shown.

[0051] Figure 5 An exemplary structure according to an exemplary embodiment of the present disclosure is shown.

[0052] Figure 6 An exemplary structure according to an exemplary embodiment of the present disclosure is shown.

[0053] Figure 7 A reactor system according to another exemplary embodiment of the present disclosure is shown. Detailed Implementation

[0054] The invention will be described with reference to specific embodiments and certain accompanying drawings, but is not limited thereto. The described drawings are illustrative only and not restrictive. In the drawings, for illustrative purposes, the dimensions of some elements may be exaggerated and not drawn to scale.

[0055] Furthermore, the terms first, second, third, etc., used in the specification and claims are used to distinguish similar elements and are not necessarily used to describe a sequence or chronological order. These terms are interchangeable where appropriate, and embodiments of this disclosure may differ from other sequences of operation described or shown herein.

[0056] Furthermore, while the various embodiments are referred to as "preferred," they should be construed as exemplary ways of implementing this disclosure and not as limiting the scope of this disclosure.

[0057] The term "comprising" as used in the claims should not be construed as limited to the elements or steps listed thereafter; it does not exclude other elements or steps. It should be interpreted as specifying the presence of the mentioned features, integers, steps, or components, but does not exclude the presence or addition of one or more other features, integers, steps, or components, or groups thereof. Therefore, the scope of the expression "a device comprising A and B" should not be limited to a device consisting solely of components A and B, but rather, relative to this disclosure, the device is defined solely by the listed components A and B, and further, the claims should be interpreted as including equivalents of those components.

[0058] As used herein, the term "atomic layer deposition" (ALD) can refer to a vapor deposition method in which deposition cycles, preferably multiple consecutive cycles, are performed in a processing chamber. Typically, during each cycle, a precursor is chemisorbed onto the deposition surface (e.g., a substrate surface or a previously deposited lower layer surface, such as material from a previous ALD cycle), forming a monolayer or sub-monolayer that is not readily reactive with another precursor (i.e., a self-limiting reaction). Subsequently, if desired, a reactant (e.g., another precursor or reactive gas) can be introduced into the processing chamber to convert the chemisorbed precursor into the desired material on the deposition surface. Typically, this reactant is capable of further reacting with the precursor. Furthermore, a purging step can be used during each cycle to remove excess precursor from the processing chamber and / or excess reactant and / or reaction byproducts from the processing chamber after the conversion of the chemisorbed precursor. Furthermore, as used herein, the term “atomic layer deposition” is also intended to include processes specified by related terms such as “chemical vapor deposition,” “atomic layer epitaxy” (ALE), molecular beam epitaxy (MBE), gas-source MBE or organometallic MBE, and chemical beam epitaxy when performed with alternating pulses of a precursor composition, a reactive gas, and a purge gas (e.g., an inert carrier gas).

[0059] As used herein, the term “chemical vapor deposition” can refer to any method in which a substrate is exposed to one or more volatile precursors that react and / or decompose on the substrate surface to produce the desired deposition.

[0060] The terms “cyclic deposition process” and “cyclic deposition process” can refer to the sequential introduction of precursors (and / or reactants) into a reaction chamber to deposit a layer on a substrate, and include processing techniques such as atomic layer deposition (ALD), cyclic chemical vapor deposition (cyclic CVD), and hybrid cyclic deposition processes that include ALD and cyclic CVD components.

[0061] As used herein, "structure" can be or includes a substrate as described herein. A structure can include one or more layers covering the substrate, such as one or more layers formed according to the methods described herein. Device portions and interconnects can be or include structures.

[0062] As used herein, "semiconductor structure" can be any structure that includes semiconductor layers. It can include, for example, transistors, memory, or sensors. It can be built on a semiconductor wafer, such as a silicon wafer.

[0063] Within the framework of this document, deposits “on” a surface can be deposits covering a surface, located below a surface (e.g., if the surface is the bottom surface of a suspended structure), and / or laterally contacting a surface (e.g., if the surface includes the side surfaces of a vertical structure).

[0064] In this disclosure, "gas" can include materials that are gaseous at ambient temperature and pressure (NTP), evaporated solids, and / or evaporated liquids, and may consist of a single gas or a mixture of gases, depending on the circumstances. Gases other than process gases, i.e., gases not introduced through gas distribution components, other gas distribution devices, etc., can be used, for example, to seal the reaction space, and may include sealing gases, such as rare gases. In some cases, the term "precursor" can refer to a compound that participates in a chemical reaction to produce another compound, particularly a compound constituting the membrane matrix or the membrane backbone; the term "reactant" is used interchangeably with the term "precursor." The term "inert gas" can refer to a gas that does not participate in a chemical reaction and / or does not become part of the membrane matrix to a perceptible extent. Exemplary inert gases include helium, argon, and any combination thereof. In some cases, inert gases may include nitrogen and / or hydrogen.

[0065] As used herein, the term "substrate" can refer to any one or more underlying materials that can be used to form or on which devices, circuits, or films are formed. A substrate may comprise a bulk material, such as silicon (e.g., single-crystal silicon), other group IV materials (e.g., germanium), or other semiconductor materials (e.g., group II-VI or III-V semiconductor materials), and may comprise one or more layers overlying or underlying the bulk material. Furthermore, the substrate may include various features, such as recesses, protrusions, etc., formed within or on at least a portion of the substrate layers. For example, a substrate may comprise a bulk semiconductor material and an insulating or dielectric material layer covering at least a portion of the bulk semiconductor material.

[0066] As used herein, the terms “film” and / or “layer” can refer to any continuous or discontinuous structure and material, such as materials deposited by the methods disclosed herein. For example, films and / or layers can include two-dimensional materials, three-dimensional materials, nanoparticles, or even partial or complete molecular layers or partial or complete atomic layers or atomic and / or molecular clusters. Films or layers can include materials or layers with pinholes, which can be at least partially continuous.

[0067] Now turn to the attached image. Figure 1a A method 100 according to an exemplary embodiment of the present disclosure is illustrated. Method 100 can be used, for example, to form a semiconductor layer 210 (such as...). Figures 3 to 6 The structure is shown. Semiconductor layer 210 can be used in devices, such as those described herein. However, unless otherwise stated, the method is not limited to such applications. Semiconductor layer 210 comprises doped tin oxide, preferably such that semiconductor layer 210 is n-doped.

[0068] During step 105, a substrate 10 (such as...) is provided in the reaction chamber. Figure 3 and Figure 4 (As shown). The reaction chamber used during step 105 may be or include a reaction chamber of a chemical vapor deposition reactor system configured to perform a cyclic deposition process. The reaction chamber may be a standalone reaction chamber or part of a cluster of tools.

[0069] Step 105 may include heating the substrate to the desired deposition temperature within the reaction chamber. In some embodiments of this disclosure, step 105 includes heating the substrate to a temperature below 800°C. For example, in some embodiments of this disclosure, heating the substrate to the deposition temperature may include heating the substrate to a temperature between about 20°C and about 800°C.

[0070] In addition to controlling the temperature of the substrate, the pressure inside the reaction chamber can also be adjusted. For example, in some embodiments of this disclosure, the pressure inside the reaction chamber during step 105 may be less than 760 Torr or between 0.2 Torr and 760 Torr.

[0071] Steps 110, 120, and 130 are repeated in multiple deposition cycles 101 to deposit a semiconductor layer 210 onto the surface of the substrate 10 using a cyclic deposition process. The surface of the substrate may, for example, comprise a semiconductor material or a dielectric material. As described above, the cyclic deposition process may include a cyclic CVD, ALD, or hybrid cyclic CVD / ALD process. For example, in some embodiments, the growth rate of a particular ALD process may be lower than that of a CVD process. One way to increase the growth rate is to operate at a deposition temperature higher than that typically used in ALD processes, resulting in some portions of the chemical vapor deposition process, but still utilizing the sequential introduction of reactants. Such a process may be referred to as cyclic CVD. In some embodiments, a cyclic CVD process may include introducing two or more reactants into a reaction chamber, wherein there may be overlapping time periods between the two or more reactants in the reaction chamber, resulting in a deposited ALD component and a deposited CVD component. This is referred to as a hybrid process.

[0072] According to another example, the cyclic deposition process may include (a) pulsed and / or flowed gaseous first precursor (step 110) and / or (b) pulsed and / or flowed gaseous second precursor (step 120) and / or (c) pulsed and / or flowed gaseous first reactant (step 130) into the reaction chamber. Each cycle 101 includes at least one step (a), at least one step (b), and at least one step (c). Within cycle 101, the pulsed and / or flowed first precursor (step 110) and / or second precursor (step 120) and / or first reactant (step 130) may be sequential, simultaneous, and / or repeated, and the claimed subject matter is not limited in this respect. Therefore, any order of steps (a), (b), and (c) is possible. A possible order is step (a), then step (b), then step (c).

[0073] In an exemplary embodiment, each deposition cycle 101 includes a single step (a) and a single step (b). The deposition cycle 101 may include other steps, such as providing a third gaseous precursor to the reaction chamber to contact the surface, the third precursor not containing Sn, In, Zr, Hf, Ge, La, Si, Nb, or Ta. The cycle 101 may also include a step of providing a second gaseous reactant to the reaction chamber to contact the surface, the second reactant containing or not containing O.

[0074] Steps (a), (b), and (c) may have similar or different durations. For example, step (a) may be longer than step (b), preferably at least twice as long, more preferably at least five times as long, and even more preferably at least ten times as long. The duration of each of steps (a), (b), and (c) may be greater than or equal to 0.1 seconds, greater than or equal to 60 seconds, or between about 0.1 and 60 seconds.

[0075] As part of multiple deposition cycles 101, the reaction chamber can be purged with a vacuum and / or inert gas to, for example, mitigate gas-phase reactions between reactants and achieve self-saturating surface reactions—e.g., in the case of ALD. Alternatively or additionally, the substrate can be moved to contact the first and second gas-phase reactants, respectively. Excess chemicals and reaction byproducts (if any) can be removed from the substrate surface or the reaction chamber, for example, by purging the reaction space or by moving the substrate and then contacting the substrate with the next reactive chemical. Figure 1b As shown, the reaction chamber can be purged with a first purge 115 between the provision of the first precursor 110 and the provision of the second precursor 120; a second purge 125 between the provision of the second precursor 120 and the provision of the first reactant 130; and a third purge 135 at the end of the deposition cycle 101. Preferably, any precursors and any reactants in the reaction chamber are purged after each step that produces the deposition.

[0076] In an exemplary embodiment, each cycle 101 includes step (d) of providing a second reactant in gaseous phase to the reaction chamber to contact the surface, the second reactant being different from the first reactant and containing a third chemical element.

[0077] The first precursor includes a first chemical element, which is tin (Sn). The second precursor includes a second chemical element selected from zirconium (Zr), hafnium (Hf), germanium (Ge), lanthanum (La), silicon (Si), niobium (Nb), and tantalum (Ta). The first reactant includes a third chemical element, which is oxygen (O).

[0078] Based on, for example, the desired thickness of the semiconductor layer, deposition cycle 101 can be repeated once or multiple times. For example, if the thickness of the semiconductor layer is less than that required for a particular application, steps (a), (b), and (c) can be repeated once or multiple times. Once the semiconductor layer has been deposited to the desired thickness, further processes can be performed on the substrate to form device structures and / or devices.

[0079] In some embodiments, in / on structures with an aspect ratio (height / width) greater than about 2, greater than about 5, greater than about 10, greater than about 25, greater than about 50, greater than about 100, or between about 10 and 100 or between about 5 and about 25, the step coverage of the semiconductor layer is equal to or greater than about 50%, or greater than about 80%, or greater than about 90%, or about 95%, or about 98%, or about 99% or greater.

[0080] The growth rate of the semiconductor layer can be relatively low—for example, less than 3 angstroms / cycle, between about 0.2 and 3 angstroms / cycle, or from about 0.1 to about 1 angstrom / cycle. A relatively low growth rate can facilitate the desired precision in film thickness and / or film thickness uniformity. Even if not completely closed, the semiconductor layer can still possess its semiconductor properties because its total thickness can be less than one angstrom. Therefore, in the case of such thin layers, low growth rate and high precision can be advantageous.

[0081] In one example, semiconductor layer 210 may include impurities such as halides, hydrogen and / or oxygen, in amounts individually or in combination less than 10 atomic%, 5 atomic%, less than 1 atomic%, less than 0.2 atomic%, less than 0.1 atomic%, or less than 0.05 atoms.

[0082] The thickness of semiconductor layer 210 can vary depending on the application. For example, the desired or predetermined thickness of semiconductor layer 210 can be less than 10 nm or about 0.05 nm to about 10 nm, or about 0.06 nm to about 5 nm, or about 0.07 nm to about 5 nm, or about 0.08 nm to about 4 nm, or about 0.09 nm to about 3 nm, or about 0.1 nm to about 2 nm. In one example, semiconductor layer 210 can be relatively thin, which may be desirable for many applications. In some cases, the thickness of semiconductor layer 210 can be greater than 2 nm—for example, when semiconductor layer 210 is used as a barrier layer or liner.

[0083] Alternatively, the semiconductor layer 210 can be formed as a continuous film—for example, using method 100—with a thickness of <5 nm, <4 nm, <3 nm, <2 nm, <1.5 nm, <1.2 nm, <1.0 nm, or <0.9 nm. The semiconductor layer 210 can be relatively smooth, with relatively low grain boundary formation.

[0084] In an embodiment, the semiconductor layer 210 includes a planar portion 280. The planar portion 280 is defined by two parallel planar surfaces 281, which are separated by a thickness 285. If the semiconductor layer 210 is formed on a wafer, the two parallel planar surfaces 281 may be parallel to the wafer, and the thickness 285 may be perpendicular to the wafer. In a preferred embodiment, the planar portion has a length 282 of at least 10 nm. The length 282 is a straight line and is measured in a direction parallel to the two parallel planar surfaces 281. The planar portion 280 and the planar surfaces 281 are... Figure 3 , Figure 4 and Figure 6 As can be seen, the thickness is 285. Figure 3 As can be seen, and the length is 282. Figure 6 As can be seen, within the framework of this disclosure, the curved surfaces of nanoparticles are not considered planar.

[0085] In an embodiment, semiconductor layer 210 comprises a first chemical element (which is Sn), a second chemical element (which is any one of Zr, Hf, Ge, La, Si, Nb, and Ta), and a third chemical element (which is O) to form tin oxide doped with the second chemical element. Preferably, the ratio of the number of atoms N2 of the second chemical element to the number of atoms N1 of the first chemical element is less than 50% (N2 / N1≤0.50), more preferably between 1% and 50% (0.01≤N2 / N1≤0.50), and even more preferably between 3% and 40% (0.03≤N2 / N1≤0.40). Preferably, the ratio of the number of atoms N3 of the third chemical element to the number of atoms (N1+N2) of the first and second chemical elements is between 1.0 and 4.0 (1.0≤N3 / (N1+N2)≤4.0). A possible material for semiconductor layer 210 is stoichiometric zirconium-doped tin oxide, which can be written as Sn. 1–x Zr x O2 (where 0.01 ≤ x ≤ 0.40, preferably 0.03 ≤ x ≤ 0.30). However, within the scope of this disclosure, non-stoichiometric doped tin oxide is also possible.

[0086] In an embodiment, such as Figure 2 As shown, in addition to steps 105, 110, 120 and 130 already described above, method 102 according to this disclosure also includes forming a dielectric layer 220 (e.g., Figures 3 to 6 Step 140 (as shown), step 150 (annealing in a synthesis gas containing a mixture of hydrogen and nitrogen), and step 160 (forming conductive contacts 230) Figure 3 , Figure 4 and Figure 6 (As shown).

[0087] Method 102 is particularly suitable for manufacturing semiconductor structures, such as semiconductor structures including transistors. The semiconductor structure may be or may include any or a portion of: memory, dynamic random access memory (DRAM), three-dimensional dynamic random access memory, charge-coupled device memory, gain unit memory, sensor, processor, controller, logic circuit, image sensor, display, touchscreen, solar cell, flexible electronic device, transistor, horizontal transistor, vertical transistor, and transistor constructed above a silicon wafer and separated from the silicon wafer by at least one electrically insulating layer.

[0088] In this embodiment, semiconductor layer 210 forms the channel of the transistor, dielectric layer 220 forms the gate dielectric, and conductive contact 230 forms the gate contact. Synthesis gas annealing helps passivate defects and improve the electrical properties of the gate dielectric, thereby ensuring better overall device performance. Dielectric layer 220 may contact semiconductor layer 210, or at least one layer may exist between semiconductor layer 210 and dielectric layer 220. Dielectric layer 220 and conductive contact 230 may be formed before or after deposition of semiconductor layer 210. Without departing from the scope of this disclosure, steps 140, 160, and the plurality of deposition cycles 101 may be performed in any order to obtain any stack of layers 210, 220, 230. Furthermore, each of steps 140, 150, 160, and the plurality of deposition cycles 101 may be performed several times during the fabrication of the semiconductor structure. Synthesis gas annealing 150 may be performed at any time after at least one deposition of semiconductor layer 210.

[0089] Syngas annealing 150 is preferably carried out at a temperature of at least 300°C, more preferably between 300°C and 500°C. Syngas annealing 150 is preferably carried out for at least 30 minutes, more preferably between 30 minutes and 4 hours.

[0090] In embodiments, the first precursor and / or the second precursor comprises one or more of the following ligands:

[0091] • Cyclopentadienyl ligands, examples of which include cyclopentadienyl (Cp), methylcyclopentadienyl (MeCp), ethylcyclopentadienyl (EtCp), isopropylcyclopentadienyl (iPrCp), tert-butylcyclopentadienyl (tBuCp), trimethylsilylcyclopentadienyl (TMSCp), and pentamethylcyclopentadienyl 1,2,4-triisopropylcyclopentadienyl (iPr3Cp) and 1,2,4-tritert-butylcyclopentadienyl (tBu3Cp);

[0092] • Acylamino ligands, examples of which include dimethylamino (NMe2), diethylamino (NEt2), ethylmethylamino (NEtMe), diisopropylamino (NiPr2), disec-butylamino (NsBu2), ethylamino (NHEt), tert-butylamino (NHtBu), N,N'-di-tert-butyl-butane-2,3-diacylamino (tbba) and bis(trimethylsilyl)amino (N(SiMe3)2);

[0093] • Imino-type ligands, examples of which include ethylimino (NEt), isopropylimino (NiPr), isobutylimino (NiBu), tert-butylimino (NtBu) and tert-pentylimino (NtPn);

[0094] • Onanyl ligands, examples of which include N,N'-diethylacetamidine (Et2AMD), N,N'-diisopropylacetamidine (iPr2AMD), N,N'-diisopropylmethylamidine (iPr2FMD), N,N'-di-tert-butylacetamidine (tBu2AMD) and N,N'-di-tert-butylmethylamidine (tBu2FMD);

[0095] • Halogenated ligands, examples of which include fluorine (F), chlorine (Cl), bromine (Br), and iodine (I);

[0096] • Alkyl ligands, examples of which include methyl (Me), ethyl (Et), isopropyl (iPr), n-butyl (Bu), tert-butyl (tBu), isobutyl (iBu), neopentyl (Np), and dimethylaminopropyl (DMP);

[0097] • Alkoxide ligands, examples of which include methanol (OMe), ethanol (OEt), isopropoxide (OiPr), tert-butanol (OtBu), tert-amylol (OtPn), 2-methyl-1-butanol (OAm), 2-dimethylaminoethanol (dmae), 1-methoxy-2-methyl-2-propanol (mmp), 1-dimethylamino-2-propanol (dmap), 1-dimethylamino-2-methyl-2-propanol (dmamp), 1-ethylmethylamino-2-methyl-2-propanol (emamp), 1-diethylamino-2-methyl-2-propanol (deamp), 1-dimethylamino-2-methyl-2-butanol (dmamb), 1-ethylmethylamino-2-methyl-2-butanol (emamb), and 1-diethylamino-2-methyl-2-butanol (deamb);

[0098] • Diketone ligands, examples of which include acetylacetonate (acac), 2,2,6,6-tetramethylheptane-3,5-diketone (thd), and 1,1,1,5,5,5-hexafluoropentane-2,5-diketone (hfac);

[0099] • Diazabutadiene-type ligands, examples of which include 1,4-di-tert-butyl-1,4-diaza-1,3-butadiene (tBu2DAD), 1,4-diisopropyl-1,4-diaza-1,3-butadiene (iPr2DAD), 1,4-di-sec-butyl-1,4-diaza-1,3-butadiene (sBu2DAD) and 1,4-di-tert-pentyl-1,4-diaza-1,3-butadiene (tPn2DAD).

[0100] In the embodiments, the first precursor is selected from SnCl4, SnBr4, SnI4, Sn(NMe2)4, Sn(NEtMe)4, Sn(NEt2)4, Sn(dmap)2, Sn(dmamp)2, Sn(dmamb)2, Sn(OtBu)4, Sn(OtPn)4, Sn(OAm)4, Sn(acac)2, Sn(N(SiMe3)2)2, Sn(tbba), SnMe4, SnEt4, SnHBu3, Sn(iPr2FMD)2, and Sn(DMP)4. The first precursor may comprise one or more of a metal halide precursor and a metal-organic precursor.

[0101] In the embodiments, the second precursor is at least one of the following: Zr precursor, Hf precursor, Ge precursor, La precursor, Si precursor, Nb precursor, and Ta precursor.

[0102] In some embodiments, the Zr precursor is selected from ZrCl4, ZrI4, Zr(NMe2)4, Zr(NEtMe)4, Zr(NEt2)4, Zr(thd)4, Zr(OiPr)4, Zr(OtBu)4, ZrCp(NMe2)3, Zr(MeCp)(NMe2)3, Zr(EtCp)(NMe2)3, ZrCp(NEt2)3, Zr(MeCp)(NEt2)3, Zr(EtCp)(NEt2)3, ZrCp(NEtMe)3, Zr(MeCp)(NEtMe)3, Zr(EtCp)(NEtMe)3, ZrCp2Cl 2. ZrCp2Me2, ZrCp2(OMe)2, ZrCp2Me(OMe), ZrCp2(NMe2)2, Zr(MeCp)2Cl2, Zr(MeCp)2Me2, Zr(MeCp)2(OMe)2, Zr(MeCp)2Me(OMe), Zr(Me Cp)2(NMe2)2, Zr(EtCp)2Cl2, Zr(EtCp)2Me2, Zr(EtCp)2(OMe)2, Zr(EtCp)2Me(OMe), Zr(EtCp)2(NMe2)2, ZrNp4 and ZrCp(tBu2DAD)(OiPr).

[0103] In some embodiments, the Hf precursor is selected from HfCl4, HfI4, Hf(NMe2)4, Hf(NEtMe)4, Hf(NEt2)4, Hf(thd)4, Hf(OiPr)4, Hf(OtBu)4, Hf(BH4)4, HfCp(NMe2)3, Hf(MeCp)(NMe2)3, Hf(EtCp)(NMe2)3, HfCp(NEt2)3, Hf(MeCp)(NEt2)3, Hf(EtCp)(NEt2)3, HfCp(NEtMe)3, Hf(MeCp)(NEtMe)3, Hf(EtCp)(NEtMe)3, HfCp2Cl2, HfCp2Me2, and HfCp2(OMe). 2. HfCp2Me(OMe), HfCp2(NMe2)2, Hf(MeCp)2Cl2, Hf(MeCp)2Me2, Hf(MeCp)2(OMe)2, Hf(MeCp)2Me(OMe), Hf(MeCp)2(NMe2)2, Hf(EtCp)2Cl2, Hf(EtCp)2Me2 , Hf(EtCp)2(OMe)2, Hf(EtCp)2Me(OMe), Hf(EtCp)2(NMe2)2, Hf(MeCp)2(mmp)Me, Hf(OtBu)2(mmp)2, Hf(iPr2FMD)2(NMe2)2, HfNp4, Hf(dmap)4 and Hf(mmp)4.

[0104] In some embodiments, the Ge precursor is selected from GeCl4, GeHCl3, Ge2H6, Ge(NMe2)4, Ge(OEt)4, Ge(OBu)4, GeCl2(dioxane), Ge(tbba), Ge(NMe2)2(tbba), Ge(N(SiMe3)2)2, GeHBu3, and GeCl(thd).

[0105] In some embodiments, the La precursor is selected from LaCp3, La(MeCp)3, La(EtCp)3, La(iPrCp)3, La(tBuCp)3, La(TMSCp)3, La(thd)3, La(N(SiMe3)2)3, La(iPr2FMD)3, La(tBu2FMD)3, La(sBu2FMD)3, La(tPn2FMD)3, La(iPr2AMD)3, La(tBu2AMD)3, La(sBu2AMD)3, La(tPn2AMD)3, LaCp2(iPr2AMD, LaCp2(tBu2AMD), LaCp2(iPr2FMD), LaCp2(tBu2FMD), La(MeCp)2(iPr2AMD ... )2(tBu2AMD), La(MeCp)2(iPr2FMD), La(MeCp)2(tBu2FMD), La(EtCp)2(iPr2AMD), La (EtCp)2(tBu2AMD), La(EtCp)2(iPr2FMD), La(EtCp)2(tBu2FMD), La(iPrCp)2(iPr2AM) D), La(iPrCp)2(tBu2AMD), La(iPrCp)2(iPr2FMD), La(iPrCp)2(tBu2FMD), La(tBuCp )2(iPr2AMD), La(tBuCp)2(tBu2AMD), La(tBuCp)2(iPr2FMD) and La(tBuCp)2(tBu2FMD).

[0106] In some embodiments, the Si precursor is selected from SiH4, Si2H6, Si3H8, SiCl4, SiH2Cl2, SiCl2Me2, SiHCl3, Si2Cl6, Si2HCl5, Si2H3Cl3, Si2H5Cl, Si3Cl8, SiBr4, SiI4, SiH2I2, Si(NMe2)4, SiH(NMe2)3, SiH2(NHtBu)2, SiH2(NEt2)2, Si2(NHEt)6, Si(OMe)4, Si(OEt)4, SiH2Et2, N(SiH3)3, SiH3(NiPr2), SiH3(NsBu2), Si(NCO)4, Si(OtBu)3OH, Si(OtPn)3OH, Si(NMe2)3SiH3, SiH2(NiPr)SiH2(NiPr), and N(SiMe3)(SiHMeNMe2)2.

[0107] In some embodiments, the Nb precursor is selected from NbF5, NbCl5, NbBr5, NbI5, Nb(NMe2)5, Nb(NEt2)5, Nb(NEtMe)5, Nb(NtBu)(NMe2)3, Nb(NtBu)(NEt2)3, Nb(NtBu)(NEtMe)3, Nb(NiPr)(NEtMe)3, Nb(NtPn)(NMe2)3, Nb(OEt)5, Nb(NtBu)(NEtMe)3, and Nb(NtBu)(NEt2)2(Cp).

[0108] In some embodiments, the Ta precursor is selected from TaF5, TaCl5, TaBr5, TaI5, Ta(NMe2)5, Ta(NEt2)5, Ta(NEtMe)5, Ta(NtBu)(NMe2)3, Ta(NtBu)(NEt2)3, Ta(NtBu)(NEtMe)3 , Ta(NiPr)(NEtMe)3, Ta(NtPn)(NMe2)3, Ta(OEt)5, Ta(OEt)4(dmae), TaNp3Cl2, Ta(NtBu)Cl3, Ta(NtPn)Cl3 and Ta(NtBu)(iPr2AMD)2(NMe2).

[0109] In some embodiments, the first reactant is selected from H2O, H2O2, O2, O3, N2O, NO, NO2, oxygen plasma, N-oxide, N-oxy compound, metal alkoxide, or alcohol-based oxidant. In some embodiments, the second reactant is selected from H2O, H2O2, O2, O3, N2O, NO, NO2, oxygen plasma, N-oxide, N-oxy compound, metal alkoxide, or alcohol-based oxidant. Alcohol oxidants may be selected from methanol, ethanol, n-propanol, isopropanol, n-butanol, sec-butanol, isobutanol, and tert-butanol. N-oxides may be selected from optionally substituted pyridine N-oxides, amine N-oxides, imine N-oxides, nitrile N-oxides, and azo N-oxides. N-oxy compounds may be organic free radicals containing a NO• group, also known as N-oxy radicals or nitrocellulose radicals, wherein unpaired electrons are delocalized on nitrogen and oxygen atoms.

[0110] Figure 3A semiconductor structure 2 including a semiconductor layer 210 is shown according to an embodiment of the present disclosure. The semiconductor layer 210 is located on a substrate 10 including a silicon wafer 200. The semiconductor layer 210 includes a source portion 211, a drain portion 212, and a channel portion 213, such that the source portion 211 and the drain portion 212 have a higher doping concentration than the channel portion 213. The semiconductor layer 210 includes a planar portion 280. The planar portion 280 is defined by two parallel planar surfaces 281 separated by a thickness 285. Although illustrated as a horizontal structure, the structures and devices according to the examples of the present invention may include vertical and / or three-dimensional structures and devices, such as FinFET devices.

[0111] Figure 4 A CCD structure 3 including a semiconductor layer 210 according to an embodiment of the present disclosure is shown. The semiconductor layer 210 is located on a substrate 10, which includes a silicon wafer 200, a first bottom dielectric layer 240 (e.g., Al2O3), and a second bottom dielectric layer 250 (e.g., SiO2). A dielectric layer 220 is present above the semiconductor layer 210 and has conductive contacts 230 for a gate.

[0112] Figure 5 A 3D DRAM structure 4 including a semiconductor layer 210 according to an embodiment of the present disclosure is shown. The semiconductor layer 210 includes a source portion 211 and a drain portion 212. It is vertically located between two dielectric layers 220 forming a gate dielectric layer. The drain portion 212 is connected to a bit line 310, and the dielectric layers 220 are in contact with word lines 320. The source portion 211 is in contact with a first capacitor plate 331, which is separated from a second capacitor plate 332 by a capacitor dielectric 340. Another dielectric 350 is present between the word line 320 and the first capacitor plate 331.

[0113] Figure 6 A semiconductor structure 5, including a semiconductor layer 210, according to an embodiment of the present disclosure is shown. The semiconductor structure 5 includes a dielectric layer 220, conductive contacts 230 for a gate, and electrodes 270. A planar portion 280 and its length 282 of at least 10 nm are also visible in this figure.

[0114] Figure 7 A system 6 according to another exemplary embodiment of the present disclosure is shown. System 6 can be used to perform the methods described herein and / or form structural or device portions as described herein.

[0115] In the example shown, system 6 includes one or more reaction chambers 450, a first precursor gas source 410, a second precursor gas source 420, a reactant gas source 430, a purge gas source 440, an exhaust source 470, and a controller 460. The reaction chamber 450 may include any suitable reaction chamber, such as an ALD or CVD reaction chamber.

[0116] The first precursor gas source 310 may include a container and one or more first precursors as described herein—either alone or mixed with one or more carrier gases (e.g., inert gases). The second precursor gas source 320 may include a container and one or more second precursors as described herein—either alone or mixed with one or more carrier gases (e.g., inert gases). The reactant gas source 330 may include a container and one or more first reactants as described herein—either alone or mixed with one or more carrier gases. The purge gas source 440 may include one or more inert gases as described herein. Although four gas sources 410, 420, 430, and 440 are shown, system 6 may include any suitable number of gas sources. Gas sources 410, 420, 430, and 440 may be connected to reaction chamber 450 via lines 415, 425, 435, and 445, each of which may include a flow controller, valve, heater, etc.

[0117] The exhaust source 470 may include one or more vacuum pumps.

[0118] Controller 460 includes electronic circuitry and software to selectively operate valves, manifolds, heaters, pumps, and other components included in system 6. Such circuitry and components operate to introduce precursors, reactants, and purge gases from corresponding sources 410, 420, 430, and 440. Controller 460 can control the timing of gas pulse sequences, the temperature of the substrate and / or reaction chamber, the pressure within the reaction chamber, and various other operations to provide appropriate operation of system 6. Controller 460 may include control software to electrically or pneumatically control valves to control the inflow and outflow of precursors, reactants, and purge gases from reaction chamber 450. Controller 460 may include modules, such as software or hardware components like FPGAs or ASICs, to perform certain tasks. Modules may advantageously be configured to reside on addressable storage media of the control system and configured to perform one or more processes.

[0119] Other configurations of System 6 are possible, including different numbers and types of precursor and reactant sources, as well as purge gas sources. Furthermore, it should be understood that numerous arrangements of valves, conduits, precursor sources, and purge gas sources exist to achieve the objective of selectively supplying gases to the reaction chamber 450. Additionally, for the sake of illustration and simplicity, many components have been omitted, and these components may include, for example, various valves, manifolds, purifiers, heaters, containers, vents, and / or bypasses.

[0120] During the operation of reactor system 6, substrate 10 of a semiconductor wafer is transferred from, for example, a substrate processing system to reaction chamber 450. Once the substrate is transferred to reaction chamber 450, one or more gases (e.g., precursors, reactants, carrier gases, and / or purge gases) from gas sources 410, 420, 430, 440 are introduced into reaction chamber 450.

[0121] The exemplary embodiments described above do not limit the scope of this disclosure, as these embodiments are merely examples of embodiments of this disclosure, the scope of which is defined by the appended claims and their legal equivalents. Any equivalent embodiments are intended to fall within the scope of this disclosure. In fact, various modifications to this disclosure, such as alternative useful combinations of the described elements, will become apparent to those skilled in the art from the description, in addition to those shown and described herein. These modifications and embodiments are also intended to fall within the scope of the appended claims. Although exemplary examples of this disclosure have been set forth herein, it should be understood that this disclosure is not limited thereto. Various modifications, variations, and enhancements may be made to the systems and methods described herein without departing from the spirit and scope of this disclosure.

[0122] The subject matter of this disclosure includes all novel and non-obvious combinations and sub-combinations of the various systems, components and configurations disclosed herein, as well as other features, functions, actions and / or properties, and any and all equivalents thereof.

Claims

1. A method for depositing a semiconductor layer comprising tin oxide, the method comprising: A substrate with a surface is provided in the reaction chamber; Perform multiple deposition cycles, each cycle including: (a) A first gaseous precursor is supplied to the reaction chamber to contact the surface, the first precursor containing a first chemical element, the first chemical element being Sn; (b) Providing a gaseous second precursor to the reaction chamber for contact with the surface, the second precursor comprising a second chemical element selected from Zr, Hf, Ge, La, Si, Nb, and Ta; and (c) A gaseous first reactant is supplied to the reaction chamber to contact the surface, the first reactant containing a third chemical element, which is O.

2. The method according to claim 1, wherein, Each deposition cycle includes a single step (a) and a single step (b).

3. The method according to claim 1 or 2, wherein, In at least some loops, steps (a), (b), and (c) are performed in the following order: step (a), step (b), and step (c).

4. The method according to any one of the preceding claims, wherein, The surface may be a semiconductor material or a dielectric material.

5. The method according to any one of the preceding claims, wherein, In the semiconductor layer, the ratio of the number of atoms N2 of the second chemical element to the number of atoms N1 of the first chemical element is between 1% and 50% (0.01≤N2 / N1≤0.50).

6. The method according to any one of the preceding claims, wherein, The semiconductor layer includes a planar portion having a length of at least 10 nm.

7. The method according to any one of the preceding claims, wherein, The semiconductor layer has a thickness between 0.5 nm and 10 nm.

8. The method according to any one of the preceding claims, wherein, The first precursor is selected from SnCl4, SnBr4, SnI4, Sn(NMe2)4, Sn(NEtMe)4, Sn(NEt2)4, Sn(dmap)2, Sn(dmamp)2, Sn(dmamb)2, Sn(OtBu)4, Sn(OtPn)4, Sn(OAm)4, Sn(acac)2, Sn(N(SiMe3)2)2, Sn(tbba), SnMe4, SnEt4, SnHBu3, Sn(iPr2FMD)2, Sn(DMP)4.

9. The method according to any one of the preceding claims, wherein, The second chemical element is Zr, and the second precursor is selected from ZrCl4, ZrI4, Zr(NMe2)4, Zr(NEtMe)4, Zr(NEt2)4, Zr(thd)4, Zr(OiPr)4, Zr(OtBu)4, ZrCp(NMe2)3, Zr(MeCp)(NMe2)3, Zr(EtCp)(NMe2)3, ZrCp(NEt2)3, Zr(MeCp)(NEt2)3, Zr(EtCp)(NEt2)3, ZrCp(NEtMe)3, Zr(MeCp)(NEtMe)3, Zr(EtCp)(NEtMe)3, ZrC p2Cl2, ZrCp2Me2, ZrCp2(OMe)2, ZrCp2Me(OMe), ZrCp2(NMe2)2, Zr(MeCp)2Cl2, Zr(MeCp)2Me2, Zr(MeCp)2(OMe)2, Zr(MeCp)2Me(OMe), Zr( MeCp)2(NMe2)2, Zr(EtCp)2Cl2, Zr(EtCp)2Me2, Zr(EtCp)2(OMe)2, Zr(EtCp)2Me(OMe), Zr(EtCp)2(NMe2)2, ZrNp4 and ZrCp(tBu2DAD)(OiPr).

10. The method according to any one of the preceding claims, wherein, The first reactant is selected from H2O, H2O2, O2, O3, N2O, NO, NO2, oxygen plasma, N-oxide, N-oxygen compound, metal alkoxide or alcohol oxidant.

11. The method according to any one of the preceding claims, wherein, Step (a) is at least twice as long as step (b).

12. The method according to any one of the preceding claims, comprising a purging step between each of steps (a), (b), and (c).

13. A method for manufacturing a semiconductor structure including a semiconductor layer comprising tin oxide, the method comprising: Semiconductor layers are deposited through the following methods: A substrate with a surface is provided in the reaction chamber; Perform multiple deposition cycles, each cycle including: (a) A first gaseous precursor is supplied to the reaction chamber to contact the surface, the first precursor containing a first chemical element, the first chemical element being Sn; (b) Providing a gaseous second precursor to the reaction chamber for contact with the surface, the second precursor comprising a second chemical element selected from Zr, Hf, Ge, La, Si, Nb, and Ta; and (c) A gaseous first reactant is supplied to the reaction chamber to contact the surface, the first reactant containing a third chemical element, the third chemical element being O; A dielectric layer is formed to form the gate dielectric; and Conductive contacts are formed to form gate contacts; The method includes annealing in a synthesis gas containing hydrogen.

14. The method according to claim 13, wherein, The semiconductor layer forms a transistor channel.

15. The method according to claim 13 or 14, wherein, The annealing is performed at a temperature between 300°C and 500°C.

16. The method according to any one of claims 13 to 15, wherein, The annealing process lasts between 30 minutes and 4 hours.

17. The method according to any one of claims 13 to 16, wherein, The semiconductor structure includes or is included in the following: memory, dynamic random access memory (DRAM), three-dimensional dynamic random access memory, charge-coupled device memory, gain unit memory, sensor, processor, controller, logic circuit, image sensor, transistor, horizontal transistor, vertical transistor, and transistor constructed above a silicon wafer and separated from the silicon wafer by at least one electrical isolation layer.

18. A structure comprising a substrate having a surface and a semiconductor layer deposited on the surface, the semiconductor layer comprising: The first chemical element, Sn; The second chemical element is selected from Zr, Hf, Ge, La, Si, Nb, and Ta; as well as The third chemical element is O; In the semiconductor layer, The ratio of the number of atoms of the second chemical element N2 to the number of atoms of the first chemical element N1 is between 1% and 50% (0.01 ≤ N2 / N1 ≤ 0.50), and The ratio of the number of atoms of the third chemical element N3 to the number of atoms of the first and second chemical elements (N1+N2) is between 1.0 and 4.0 (1.0≤N3 / (N1+N2)≤4.0).

19. The structure according to claim 18, wherein, The semiconductor layer includes a planar portion having a length of at least 10 nm.

20. The structure according to claim 18 or 19, wherein, The semiconductor layer includes a channel portion, a source portion, and a drain portion, wherein the source portion and the drain portion have a higher dopant concentration than the channel portion.