Method for forming a metal film in a feature

By combining a cyclic deposition and etching process with plasma-enhanced atomic layer deposition (PEAD) technology using pulsed metal precursors and plasma power, the void problem in metal film deposition in narrow features of semiconductor devices was solved, achieving void-free metal film filling and improving conductivity.

CN123165035APending Publication Date: 2026-11-24ASM IP HLDG BV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202610688424.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2025-05-22
Filing Date
2026-05-19
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing technologies struggle to effectively deposit metal films within narrow features of semiconductor devices, resulting in voids or incomplete filling, which increases resistivity.

Method used

A cyclic deposition and etching process is employed in a reaction chamber, combining pulsed metal precursors, reduction reactants, and plasma power to form a metal layer at low temperatures using plasma-enhanced atomic layer deposition (PEALD). The same metal precursor is used for precise control during etching, and the cycle is repeated to fill the feature.

Benefits of technology

This technology enables the formation of void-free metal films in the features of semiconductor devices at low temperatures, improving filling efficiency and conductivity while reducing defects in the metal films.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123165035A_ABST
    Figure CN123165035A_ABST
Patent Text Reader

Abstract

A method for forming a metal film in one or more features on the surface of a substrate is disclosed. An exemplary method includes providing a substrate in a reaction chamber, performing a first deposition cycle, performing an etching cycle, and performing a second deposition cycle. The same metal precursor can be used in the etching cycle and the second deposition cycle.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This disclosure generally relates to methods and apparatus for forming a metal film in one or more features on a substrate, and to structures including a metal film in one or more features. Such methods, apparatus, and structures can be used to form electronic devices. Background Technology

[0002] The scaling of semiconductor devices has led to significant improvements in the speed and density of integrated circuits. However, the scaling of semiconductor devices has also presented challenges. As semiconductor devices are scaled down, features on the substrate surface (such as trenches, gaps, etc.) become narrower. Depositing metal films into features has proven difficult. Using conventional deposition techniques, voids may form in the deposited metal film, or the metal film may not completely fill the feature. The formation of voids or the lack of complete filling can lead to an increase in the resistivity of the metal film. Therefore, there is a need for improved metal films in features and improved, efficient methods for forming void-free metal films in features.

[0003] Any discussion set forth in this section (including discussions of problems and solutions) is included in this disclosure and is for the purpose of providing background to this disclosure only. Such discussion should not be construed as an admission that any or all information was known at the time of making this invention or otherwise constitutes prior art. Summary of the Invention

[0004] This synopsis is provided to introduce some concepts in a simplified form. These concepts are further described in detail in the following detailed description of exemplary embodiments of this disclosure. This synopsis is not intended to require the identification of key or essential features of the claimed subject matter, nor is it intended to limit the scope of the claimed subject matter.

[0005] The various examples described herein relate to methods for forming a metal film in one or more features on the surface of a substrate. As set forth below, the methods described herein can be used to manufacture electronic devices, such as semiconductor devices.

[0006] According to one or more embodiments, a method is provided for forming a metal film in one or more features on a substrate surface. An exemplary method includes providing a substrate in a reaction chamber, performing a first deposition cycle, performing an etching cycle, performing a second deposition cycle, and optionally repeating the etching cycle and the second deposition cycle. The exemplary method can be performed at relatively low temperatures (e.g., below about 500°C). The exemplary method can be performed in a single reaction chamber. The exemplary method can use the same precursor in one or more of the deposition and etching cycles. The exemplary method can fill one or more features with a metal film (e.g., completely or substantially completely). The exemplary method can form a metal film (e.g., substantially) free of voids or gaps.

[0007] Performing a first deposition process may include pulsed first metallic precursor, pulsed reduction reactant, and applying first plasma (e.g., RF) power to a reaction chamber to generate a first plasma. Applying the first plasma (e.g., RF) power may occur during the pulsed reduction reactant step. The first deposition process may be a cyclic deposition process, such as a plasma-enhanced atomic layer deposition process. The first deposition process may produce a first layer. The first layer may be metallic or a metallic layer.

[0008] Performing an etching cycle may include providing a second metal precursor and applying second plasma (e.g., RF) power to the reaction chamber to generate a second plasma. Applying the second plasma (e.g., RF) power may occur during the step of providing the second metal precursor. The application of the second plasma (e.g., RF) power may have a duration between about 10 seconds and about 300 seconds, or between about 60 seconds and about 120 seconds. The second metal precursor provided during the etching cycle may include the same metal as the first metal precursor pulsed during the first deposition cycle, or may be or include the same precursor as the first metal precursor pulsed during the first deposition cycle. The etching cycle may remove a portion of the first layer.

[0009] Performing a second deposition process may include pulsed second metallic precursors, pulsed reduction reactants, and the application of third plasma (e.g., RF) power to the reaction chamber to generate a third plasma. The application of third plasma (e.g., RF) power may occur during the pulsed reduction reactant step. The second deposition process may be a cyclic deposition process, such as plasma-enhanced atomic layer deposition. The second deposition process may produce a second layer. The second layer may be metallic or a metallic layer.

[0010] According to another example of this disclosure, a device may be formed and / or include the structure described herein using the methods described herein.

[0011] According to yet another exemplary embodiment of this disclosure, a system is provided for performing the methods described herein and / or for forming structures as described herein.

[0012] These and other embodiments will become apparent to those skilled in the art from the following detailed description of certain embodiments with reference to the accompanying drawings; the invention is not limited to any particular embodiment disclosed. Attached Figure Description

[0013] Figure 1 A method for forming a film in one or more features according to one or more embodiments of the present disclosure is shown;

[0014] Figure 2 A method for performing a first deposition cycle according to one or more embodiments of the present disclosure is shown;

[0015] Figure 3 The timing of a deposition cycle according to one or more embodiments of the present disclosure is shown;

[0016] Figure 4 A method for performing an etching cycle according to one or more embodiments of the present disclosure is shown;

[0017] Figure 5 A method for performing a second deposition cycle according to one or more embodiments of the present disclosure is shown;

[0018] Figure 6 An example of a substrate processing apparatus according to one or more examples of this disclosure is shown;

[0019] Figure 7 Examples of structures that can form part of a device according to one or more examples of this disclosure are shown; and

[0020] Figure 8 Examples of structures that can be formed based on one or more examples of this disclosure are shown.

[0021] It should be understood that the elements in the accompanying drawings are shown for simplicity and clarity and are not necessarily drawn to scale. For example, the dimensions of some elements may be exaggerated relative to other elements to aid in understanding the embodiments shown in this disclosure. Detailed Implementation

[0022] The following description of exemplary embodiments of the methods, structures, apparatuses, and systems is merely illustrative and for purposes of explanation only; the following description is not intended to necessarily limit the scope of this disclosure or the claims. Furthermore, the description of multiple embodiments having the described features is not intended to exclude other embodiments having additional features or other embodiments including different combinations of the described features. For example, various embodiments are set forth as exemplary embodiments and may be recited in the dependent claims. Unless otherwise stated, exemplary embodiments or components thereof may be combined or may be applied separately from each other.

[0023] As used herein, the term “and / or” includes any and all combinations of one or more of the associated listed items. Unless otherwise stated, expressions such as “at least one of…” modify the entire column of elements when following an element in the column, and not necessarily any individual element in that column.

[0024] As used in this article, the singular forms “a,” “one,” and “the” are intended to include both singular and plural forms, unless the context otherwise requires.

[0025] As used herein, the term "substrate" can refer to any one or more underlying materials that can be used to form or on which devices, circuits, or films are formed. A substrate may comprise a bulk material, such as silicon (e.g., single-crystal silicon), other group IV materials (e.g., germanium), or compound semiconductor materials (e.g., group III-V or II-VI semiconductors), and may comprise one or more layers overlaid or under the bulk material. For example, a substrate may comprise silicon or silicon-germanium. In some cases, a substrate may comprise an oxide (e.g., silicon oxide).

[0026] The terms "precursor" and "reactant" can refer to molecules or compounds that participate in the chemical reaction that produces a layer or deposited material. A precursor typically comprises a portion that is at least partially bound to the layer. This resulting portion can be deposited on a substrate to form a film as disclosed herein. A reactant can be a compound bound to the layer or a compound not significantly bound to the resulting layer. In some cases, the term reactant is used interchangeably with the term precursor.

[0027] As used herein, “metallic precursor” includes gases or materials that can be converted into a gaseous state and can be represented by a chemical formula comprising one or more metals.

[0028] In some embodiments, "film" refers to a layer extending in a direction perpendicular to the thickness direction. In some embodiments, "layer" refers to a material of a certain thickness formed on a surface, and can be synonymous with a film or non-film structure. A film or layer may consist of discrete single films or layers or multiple films or layers having certain properties, and the boundaries between adjacent films or layers may or may not be clear, and may or may not be based on the physical, chemical and / or any other properties, formation process or sequence and / or function or purpose of adjacent films or layers. A layer or film may be continuous or discontinuous. Furthermore, a single film or layer may be formed using one or more deposition cycles.

[0029] As used herein, the term "purge" can refer to the process of supplying an inert or substantially inert gas to a reaction chamber between two potentially interacting gas pulses. For example, a purging process using, for instance, an inert gas (e.g., a rare gas) can be provided between a precursor pulse and a reactant pulse to reduce gas-phase interactions between the precursor and reactant that might otherwise occur. It should be understood that purging can be temporally or spatially, or both. For example, in the case of temporal purging, purging steps can be used, for instance, in a temporal sequence of supplying a precursor to the reaction chamber, supplying a purge gas to the reaction chamber, and supplying a reactant or another precursor to the reaction chamber, wherein the substrate on which the deposited layer is located remains stationary. In the case of spatial purging, the purging step can take the form of moving the substrate from (e.g., continuously) a first position where the precursor is supplied via a purge gas curtain to (e.g., continuously) a second position where the reactant or other precursor is supplied.

[0030] As used herein, the term "structure" can refer to a device structure that is partially or fully fabricated. For example, a structure can be a substrate or a substrate having one or more layers and / or features formed thereon.

[0031] As used in this article, the term “covering” can refer to a membrane (e.g., directly) on top of another membrane.

[0032] As used herein, the term "cyclic deposition process" or "cyclic deposition process" can refer to a vapor phase deposition process in which deposition cycles (typically multiple consecutive deposition cycles) are performed in a processing chamber. Cyclic deposition processes can include, for example, cyclic chemical vapor deposition (CCVD) and / or atomic layer deposition (ALD) processes.

[0033] In this disclosure, any two numbers of a variable may constitute a feasible range of the variable, and any range indicated may include or exclude endpoints. Furthermore, any value of the indicated variable (whether or not it is indicated by “about”) may refer to an exact value or an approximate value and include equivalents, and may refer to an average, median, representative value, multi-value, etc. For example, the value of a variable may include + / -20%, or + / -10%, or + / -5%, or + / -1%, or + / -0% of the value of the listed variable. Additionally, in this disclosure, the terms “comprising,” “including,” “consisting of,” and “having” may independently mean “generally or broadly comprising,” “including,” “substantially constitutes,” or “consisting of” in some embodiments. The meaning of any definition in this disclosure does not necessarily exclude the common and customary meaning in some embodiments.

[0034] The carrier gas and / or inert gas may co-flow in any step or sub-step of any method described herein (e.g., continuously). For example, the carrier gas and / or inert gas may be one or more of helium, argon, or nitrogen in any combination.

[0035] The various steps of the methods described herein can be performed in a single reaction chamber or in multiple reaction chambers (e.g., the reaction chamber for clustered tools). In some embodiments, the method can be performed in a single reaction space. In some embodiments, one or more steps or sub-steps of the methods described herein can be performed in different reaction spaces and / or different reaction chambers.

[0036] Figure 1 A method 100 for forming a film according to an exemplary embodiment of the present disclosure is shown. The method 100 includes providing a substrate including one or more features in a reaction chamber (step 110), performing a first deposition cycle (step 120), performing an etching cycle (step 130), performing a second deposition cycle (step 140), and optionally repeating the steps of performing the etching cycle and performing the second deposition cycle (cycle 150).

[0037] During step 110, a substrate is provided into the reaction space within the reaction chamber. According to examples of this disclosure, the reaction chamber may form part of a chemical vapor deposition reactor, such as a chemical vapor deposition (CVD) reactor, an atomic layer deposition (ALD) reactor, etc. In some embodiments, method 100 is performed only in a single reaction space within the reaction chamber.

[0038] One or more features on the substrate surface may be gaps, trenches, etc. One or more features may have an aspect ratio greater than 1 or greater than 10, or between about 5 and about 25. One or more features may have a depth greater than 10 nm or greater than 30 nm, or between about 10 nm and 100 nm. Alternatively or additionally, one or more features may have a width between about 5 nm and about 100 nm, or between about 10 nm and about 50 nm.

[0039] During step 110, the substrate may be brought to a desired temperature and / or the reaction space may be brought to a desired pressure, such as a temperature and / or pressure suitable for subsequent steps. For example, the temperature within the reaction space (e.g., the temperature of the substrate, substrate support, or ambient temperature) may be between about 0°C and about 500°C, or between about 300°C and about 450°C, or between about 350°C and 425°C. The pressure within the reaction space may be less than 760 Torr, or between about 1 Torr and 100 Torr, or between about 1 Torr and about 20 Torr, or between about 3 Torr and 10 Torr. In some embodiments, throughout method 100, the temperature within the reaction space is between about 0°C and about 500°C, or between about 300°C and about 450°C, or between about 350°C and 425°C.

[0040] Method 100 continues to perform a first deposition cycle (step 120). In some embodiments, the first deposition cycle is a cyclic deposition process, such as a plasma-enhanced cyclic deposition process. In some embodiments, the first deposition cycle forms a first layer. In some embodiments, the first layer comprises a metal or a metallic layer. In some embodiments, the first layer comprises one or more transition metals. In some embodiments, the first layer comprises one or more Group 4-8 metals. In some embodiments, the first layer comprises one or more Group 6 metals. In some embodiments, the first layer comprises (e.g., metallic) molybdenum. In some embodiments, the first layer is a conformal layer.

[0041] Figure 2 It shows the applicable Figure 1Method 200 of step 120. Method 200 includes pulsating a first metal precursor (step 210), pulsating a reduction reactant (step 220), applying first plasma (e.g., RF) power (step 230), optionally performing a purge (step 240), and optionally repeating these steps one or more times (loop 250). In some cases, steps 210-230 are performed in the order of 210, 220, and 230. Each step 210-240 of method 200 may be performed one or more times before proceeding to the next step. In some embodiments, a purge (e.g., purge 240) is performed after any or all of steps 210-230 of pulsating the first metal precursor 210, pulsating the reduction reactant 220, and applying the first plasma (e.g., RF) power 230. In some embodiments, applying the first plasma (e.g., RF) power 230 at least partially overlaps with pulsating the reduction reactant 220. In some embodiments, applying the first plasma (e.g., RF) power 230 occurs after starting pulsating the reduction reactant 220. In some embodiments, the application of the first plasma (e.g., RF) power 230 occurs after the start pulse reduction reactant 220 and before the end pulse reduction reactant 220.

[0042] In some embodiments, the first metal precursor comprises one or more transition metals. In some embodiments, the first metal precursor comprises one or more Group 4-8 metals. In some embodiments, the first metal precursor comprises one or more of Mo, Vn, Ti, Nb, and Zr. In some embodiments, the first metal precursor comprises a halide, a halide oxide, or an organometallic compound. For example, the first metal precursor may be or include one or more of MoCl5, MoO2Cl2, MoOCl4, VCl4, TiCl4, NbCl5, or ZrCl4. During step 210, the first metal precursor is adsorbed (e.g., chemisorbed) onto the surface of one or more features to form adsorbed (e.g., chemisorbed) material on the surface of one or more features.

[0043] In some embodiments, the reducing reactant comprises any compound capable of reacting (and / or reducing) an adsorbed (e.g., chemisorbed) substance to form a metallic layer. In some embodiments, the reducing reactant comprises hydrogen. In some embodiments, the reducing reactant comprises hydrogen (H2), ammonia (NH3), or hydrazine. For example, the reducing reactant is or contains hydrogen (H2) or an activated substance of hydrogen, such as a hydrogen radical.

[0044] In some embodiments, the pulsed first metal precursor includes supplying the first metal precursor into the reaction chamber at a flow rate of about 0.5 slm to about 6 slm. In some embodiments, the pulsed reduction reactant includes supplying the reduction reactant into the reaction chamber at a flow rate of about 1 slm to about 30 slm.

[0045] In some embodiments, the first plasma (e.g., RF) power is between about 150 W and 1200 W, or between about 300 W and 1000 W, or between about 500 W and 800 W. In some embodiments, the first plasma (e.g., RF) power includes pulsed RF power. In some embodiments, the first plasma (e.g., RF) power has a frequency between 40 kHz and 2.45 GHz, or about 13.56 MHz. In some embodiments, applying the first plasma (e.g., RF) power 230 forms the first plasma (e.g., from a gas containing a reducing reactant and optionally an inert gas). In some embodiments, the first plasma forms an activating substance (e.g., a free radical) of the reducing reactant. In some embodiments, the reducing reactant (e.g., the activating substance of the reducing reactant) reacts with a substance adsorbed (or chemisorbed) by the first metal precursor to form a metallic layer on one or more characteristic surfaces.

[0046] In some embodiments, the steps of method 200 are repeated (optionally cycle 250) to increase the thickness of the first layer. In some embodiments, the thickness of the first layer is between about 3 angstroms and about 30 angstroms, or between about 5 angstroms and about 20 angstroms, or between about 7 angstroms and about 15 angstroms.

[0047] In some embodiments, method 100 may form a first layer such that the width of an opening in one or more features is smaller than the width of one or more features below the opening. Figure 8 A structure 800, which may form part of a deposition cycle according to one or more examples of the present disclosure, is shown. Structure 800 includes a substrate 810 and a first layer 830, the substrate 810 including one or more features 820. After the first layer 830 is formed, the width of an opening 840 in the one or more features 820 may be smaller than the width 850 of the one or more features below the opening.

[0048] Figure 3 The timing of a deposition cycle according to one or more embodiments of the present disclosure is shown. Figure 3 The timing sequence applicable to the first deposition cycle and / or the second deposition cycle described below is shown. Figure 3 In step t1, the process includes flowing a metal precursor. t1 may correspond to pulsed first metal precursor (step 210). t2 includes a purging step, wherein excess metal precursor is removed from the reaction chamber. t2 may correspond to optional purging step 240. t3 includes providing reduction reactants and applying RF power. t3 may correspond to pulsed reduction reactants 220 and applying first plasma (e.g., RF) power 230. t4 includes a purging step, wherein excess reduction reactants are removed from the reaction chamber. t4 may correspond to optional purging step 240.

[0049] In some embodiments, the duration of the RF on-time in a deposition cycle is between about 1 second and about 3.5 seconds. In some embodiments, the total RF on-time in one or more first deposition cycles is from about 20 seconds to about 200 seconds. In some embodiments, the purging step has a duration of from about 0.3 seconds to about 3 seconds.

[0050] Back Figure 1 Method 100 continues with an etching cycle (step 130). The etching cycle may remove a portion of the first layer formed in the first deposition cycle. In some embodiments, the etching cycle is anisotropic. For example, the etching cycle may remove more of the first layer formed at the openings of one or more features than the first layer formed below the openings of one or more features.

[0051] Figure 4 It shows the applicable Figure 1 Method 400 of step 130. Method 400 includes providing a second metal precursor (step 410), optionally providing an inert gas (step 420), applying a second plasma (e.g., RF) power (step 430), and optionally performing a purging (step 440). Each step 410-440 of method 400 may be performed once or more before proceeding to the next step. In some embodiments, purging, such as purging 440, is performed after any or all of steps 410-420. In some embodiments, applying the second plasma (e.g., RF) power 430 at least partially overlaps with providing the second metal precursor 410. In some embodiments, applying the second plasma (e.g., RF) power occurs after the start of providing the second metal precursor 410. In some embodiments, applying the second plasma (e.g., RF) power 430 occurs after the start of providing the second metal precursor 410 and before the end of providing the second metal precursor 410.

[0052] In some embodiments, the second metal precursor comprises one or more transition metals. In some embodiments, the first metal precursor comprises one or more Group 4-8 metals. In some embodiments, the second metal precursor comprises one or more of Mo, Vn, Ti, Nb, and Zr. In some embodiments, the second metal precursor comprises one or more transition metals identical to the first metal precursor. In some embodiments, the second metal precursor comprises a halide or halide oxide. For example, the second metal precursor may be or include one or more of MoCl5, MoO2Cl2, MoOCl4, VCl4, TiCl4, NbCl5, or ZrCl4. In some embodiments, the second metal precursor may be identical to the first metal precursor. In some embodiments, the second metal precursor is provided to the reaction chamber at a flow rate of about 0.5 slm to about 6 slm.

[0053] In some embodiments, the inert gas provided during step 420 includes argon.

[0054] In some embodiments, the second plasma (e.g., RF) power is between 20W and 300W, or between about 50W and about 150W. In some embodiments, the second plasma (e.g., RF) power includes pulsed RF power. In some embodiments, the second plasma (e.g., RF) power has a frequency between 40kHz and 2.45GHz, or about 13.56MHz. In some embodiments, the application of the second plasma (e.g., RF) power (step 430) has a duration between about 10 seconds and 300 seconds, or between about 40 seconds and 150 seconds, or between about 60 seconds and 120 seconds. The duration of the application of the second RF power (step 430) will affect the etching amount of the first layer.

[0055] In some embodiments, a second RF power 430 is applied to form a second plasma (e.g., from a gas containing a second metal precursor). In some embodiments, the second plasma forms an activating material (e.g., free radicals and / or ions) of the second metal precursor. In some embodiments, the activating material of the second metal precursor may include an activated (e.g., free radicals and / or ions) halide material. The activating material of the second metal precursor may react with the first layer to form a gaseous material, which may subsequently be removed. Advantageously, using the second metal precursor during an etching cycle results in no additional type of transition metal being added to the first layer. Advantageously, in embodiments where the first and second metal precursors are the same, the etching cycle and the first deposition cycle may use the same metal precursor. In embodiments where the first and second metal precursors are the same, the ratio of the RF on-time in one or more first deposition cycles to the RF on-time in one or more etching cycles preceding the second deposition cycle may be between about 2:1 and 1:2.

[0056] Back Figure 1 Method 100 continues to perform a second deposition cycle (step 140). In some embodiments, the second deposition cycle is a cyclic deposition process. The second deposition cycle may be a plasma-enhanced cyclic deposition process. In some embodiments, the second deposition cycle uses the same metal precursor as the etching cycle. In some embodiments, the second deposition cycle uses the same metal precursor and / or the same reactants as the first deposition cycle. In some embodiments, the second deposition cycle is (e.g., essentially) the same as the first deposition cycle.

[0057] In some embodiments, a second deposition cycle forms a second layer. The second deposition cycle may form the second layer directly on the first layer. In some embodiments, the second layer includes a metallic layer. In some embodiments, the second layer contains one or more transition metals. In some embodiments, the second layer contains one or more Group 4-8 metals. In some embodiments, the second layer contains one or more Group 6 metals. In some embodiments, the second layer contains (e.g., metallic) molybdenum. In some embodiments, the second layer is a conformal layer.

[0058] Figure 5 It shows the applicable Figure 1 Method 500 of step 140 in the method includes pulsed second metal precursor (step 510), pulsed reduction reactant (step 520), application of third plasma (e.g., RF) power (step 530), optionally performing purging (step 540), and optionally repeating these steps one or more times (loop 550). In some cases, steps 510-530 are performed in the order of 510, 520, and 530. Each step 510-540 of method 500 may be performed one or more times before proceeding to the next step. In some embodiments, purging (e.g., purging 540) is performed after any or all of steps 510-530 of pulsed second metal precursor 510, pulsed reduction reactant 520, and application of third plasma (e.g., RF) power 530. In some embodiments, application of third plasma (e.g., RF) power 530 at least partially overlaps with pulsed reduction reactant 520. In some embodiments, application of third plasma (e.g., RF) power 530 occurs after the start of pulsed reduction reactant 520. In some embodiments, the application of third plasma (e.g., RF) power 530 occurs after the start pulse reduction reactant 520 and before the end pulse reduction reactant 520.

[0059] During step 510, a second metal precursor is adsorbed (e.g., chemisorbed) onto the first layer to form an adsorbed (e.g., chemisorbed) substance on the surface of the first layer.

[0060] In some embodiments, the reducing reactant comprises any compound capable of reacting (and / or reducing) a substance adsorbed (or chemisorbed) from the second metal precursor to form a metallic layer. In some embodiments, the reducing reactant comprises hydrogen. For example, the reducing reactant is or contains hydrogen (H2) or an activated substance of hydrogen, such as a hydrogen radical.

[0061] In some embodiments, the pulsed second metal precursor includes supplying the second metal precursor into the reaction chamber at a flow rate of about 0.5 slm to about 6 slm. In some embodiments, the pulsed reduction reactant includes supplying the reduction reactant into the reaction chamber at a flow rate of about 1 slm to about 30 slm.

[0062] In some embodiments, the third plasma (e.g., RF) power is between about 150 W and 1200 W, or between about 300 W and 1000 W, or between about 500 W and 800 W. In some embodiments, the third plasma (e.g., RF) power is greater than the second plasma (e.g., RF) power. In some embodiments, the third plasma (e.g., RF) power includes pulsed RF power. In some embodiments, the third plasma (e.g., RF) power has a frequency between 40 kHz and 2.45 GHz, or about 13.56 MHz. In some embodiments, the third plasma (e.g., RF) power 530 is applied (e.g., from a gas containing reducing reactants) to form the third plasma. In some embodiments, the third plasma forms an activating substance (e.g., free radicals and / or ions) of the reducing reactants. In some embodiments, the reducing reactants (e.g., the activating substance of the reducing reactants) react with a substance adsorbed (e.g., chemisorbed) on the second metal precursor to form a metallic layer on the first layer (e.g., directly).

[0063] Back Figure 1 Method 100 may optionally continue (loop 150) by repeating the steps of etching cycle 130 and performing a second deposition cycle 140. Loop 150 may continue until one or more features are filled with a metal film (wherein the metal film comprises a first layer and a second layer). In some embodiments, the metal film (e.g., a base) has no voids.

[0064] Advantageously, using a second metal precursor during the etching cycle and the second deposition cycle results in no additional type of transition metal being added to the second layer. Advantageously, in embodiments where the first and second metal precursors are the same, the same metal precursor can be used for the etching cycle, the first deposition cycle, and the second deposition cycle.

[0065] Figure 6 An example of a substrate processing apparatus 600 according to one or more examples of this disclosure is shown. Apparatus 600 can be used to perform the methods described herein and / or form structural or device portions as described herein.

[0066] In the example shown, device 600 includes one or more reaction chambers 602, a first metal gas precursor source 604, a reduction reactant source 606, a second metal precursor source 608, an inert gas source 610, an exhaust source 622, and a controller 612.

[0067] Reaction chamber 602 may include any suitable reaction chamber, such as an atomic layer deposition (ALD) or chemical vapor deposition (CVD) reaction chamber.

[0068] The first metal gas precursor source 604 may include a container and one or more precursors containing a metal (e.g., the first metal precursor described herein) – alone or mixed with one or more carrier gases (e.g., inert gases). The reduction reactant source 606 may include a container and one or more reactants as described herein (e.g., reduction reactants) – alone or mixed with one or more carrier gases (e.g., inert gases). The second metal precursor source 608 may include a container and one and / or more precursors containing a metal as described herein (e.g., the second metal precursor described herein) – alone or mixed with one or more carrier gases (e.g., inert gases). The inert gas source 610 may include a container and one or more inert gases as described herein. Although four gas sources 604-610 are shown, the apparatus 600 may include any suitable number of gas sources. Gas sources 604-610 may be coupled to the reaction chamber 602 via lines 614-620, each of which may include a flow controller, valve, heater, etc.

[0069] The exhaust source 622 may include one or more vacuum pumps.

[0070] Controller 612 includes electronic circuitry and software to selectively operate valves, manifolds, heaters, pumps, and other components included in apparatus 600. Such circuitry and components operate to introduce precursors, reactants, and gases from respective sources 604-610. Controller 612 can control the timing of gas pulse sequences, the temperature of the substrate and / or reaction chamber, the pressure within the reaction chamber, and various other operations to provide appropriate operation of apparatus 600. Controller 612 may include control software to electrically or pneumatically control valves to control the inflow and outflow of precursors, reactants, and purge gases from reaction chamber 602. Controller 612 may include modules, such as software or hardware components like FPGAs or ASICs, to perform certain tasks. Modules may advantageously be configured to reside on addressable storage media of the control system and configured to perform one or more processes or methods as described herein.

[0071] Other configurations of the apparatus 600 are possible, including different numbers and types of precursor and reactant sources, as well as purge gas sources. Furthermore, it should be understood that numerous arrangements of valves, conduits, precursor sources, and purge gas sources exist to achieve the objective of selectively supplying gases to the reaction chamber 602. Additionally, for the sake of illustrative purposes and for simplicity, many components have been omitted, and these components may include, for example, various valves, manifolds, purifiers, heaters, containers, vents, and / or bypasses.

[0072] During operation of the apparatus 600, a substrate, such as a semiconductor wafer (not shown), is transferred from, for example, a substrate transport system to a reaction chamber 602. Once the substrate is transferred to the reaction chamber 602, one or more gases (e.g., precursors, reactants, carrier gases, and / or purge gases) from gas sources 604-610 are introduced into the reaction chamber 602.

[0073] Figure 7 The structure / partial view of a device 700 according to another example of the invention is shown. The device or structure 700 includes a substrate 710 comprising one or more features 720, and a metal film 730 in the one or more features 720. In some embodiments, the substrate 710 comprises a semiconductor, such as silicon or silicon-germanium. In some embodiments, the one or more features include gaps, trenches, etc., as described herein. In some embodiments, the metal film 730 comprises one or more transition metals. In some embodiments, a first layer comprises one or more transition metals. In some embodiments, the metal film 730 comprises one or more Group 4-8 metals. In some embodiments, the metal film 730 comprises one or more Group 6 metals. In some embodiments, the metal film 730 comprises molybdenum. In some embodiments, the metal film 730 is a metallic film. In some embodiments, the metal film 730 contains less than about 5 atomic% of impurities, or less than about 3 atomic% of impurities, such as carbon, oxygen, nitrogen, or other nonmetals.

[0074] The exemplary embodiments described above do not limit the scope of the invention, as these embodiments are merely examples of embodiments of the invention, the scope of which is defined by the appended claims and their legal equivalents. Any equivalent embodiments are intended to fall within the scope of the invention. In fact, various modifications to this disclosure, such as alternative useful combinations of the described elements, in addition to those shown and described herein, will become apparent to those skilled in the art from the description. These modifications and embodiments are also intended to fall within the scope of the appended claims.

Claims

1. A method for forming a metal film in one or more features on the surface of a substrate, the method comprising: A substrate is provided in the reaction chamber, the substrate comprising one or more features; Perform a first deposition cycle, wherein the first deposition cycle includes: The pulsed first metal precursor comprises one or more of a metal halide or a metal halide oxide. Pulse reduction reactants, and A first plasma is generated during the pulsed reduction reaction step; Execute an etching cycle, wherein the etching cycle includes: A second metal precursor is provided to the reaction chamber, and A second plasma is generated during the step of providing the second metallic precursor; and After the etching cycle is performed, a second deposition cycle is performed, wherein the second deposition cycle includes a pulsed second metal precursor.

2. The method according to claim 1, wherein, The first metallic precursor includes molybdenum.

3. The method according to claim 1, wherein, The first deposition cycle includes a plasma-enhanced atomic layer deposition process.

4. The method according to claim 1, wherein, The temperature of the reaction chamber is 400°C or lower during the method.

5. The method according to claim 1, wherein, The first metal precursor includes one or more of MoCl5, MoOCl4, and MoO2Cl2.

6. The method according to claim 1, wherein, The reducing reactants include hydrogen (H2).

7. The method according to claim 1, wherein, The duration of generating the second plasma is between approximately 10 seconds and 300 seconds.

8. The method according to claim 1, wherein, The duration of generating the second plasma is between approximately 60 and 120 seconds.

9. The method according to claim 1, wherein, The etching cycle also includes supplying argon gas to the reaction chamber during the step of supplying the second metal precursor to the reaction chamber.

10. The method of claim 1, further comprising repeating the second deposition cycle and the etching cycle once or more.

11. The method according to claim 1, wherein, The metal film is metallic.

12. The method according to claim 1, wherein, The first deposition cycle forms a first layer, and the etching cycle removes a portion of the first layer.

13. The method according to claim 1, wherein, The method is carried out in a single reaction space.

14. The method according to claim 1, wherein, The first metal precursor, the second metal precursor, the reduction reactant, and the optional inert gas are the only gases supplied to the reaction chamber during the method.

15. The method according to claim 1, wherein, No plasma is generated during the step of pulsing the first metallic precursor.

16. A method for forming a metal film, the method comprising: Provide a substrate in the reaction chamber; Depositing a first layer, wherein depositing the first layer includes providing a first metal precursor; Etching a portion of the first layer, wherein etching the first layer includes providing a second metallic precursor; and A second layer is deposited on the first layer, wherein depositing the second layer includes providing a second metal precursor. The second metal precursor includes one or more of metal halides or metal halide oxides.

17. The method according to claim 16, wherein, Etching the first layer involves generating plasma.

18. The method according to claim 16, wherein, Depositing the first layer involves generating plasma.

19. The method of claim 16, wherein, The second metal precursor includes one or more of MoCl5, MoOCl4, and MoO2Cl2.

20. The method of claim 16, wherein, The deposition of the first layer includes a cyclic vapor deposition process.