Wafer photolithography pressure point de-bonding method and system for controlling npn bipolar transistor beta drift

By combining plasma dry and wet methods for photoresist removal, along with centrifugal drying under PTFE basket and nitrogen protection, the problem of photoresist residue interfering with the β parameter after photolithography and etching was solved, achieving high cleanliness and parameter stability on the wafer surface.

CN123165040APending Publication Date: 2026-11-24XIAN MICROELECTRONICS TECH INST
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611277261.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-21
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing technologies cannot completely remove photoresist and modified residues generated by plasma after photolithography etching of NPN bipolar transistors. This results in impurities on the wafer surface interfering with the precise control of the β parameter, affecting product yield and parameter consistency.

Method used

The process involves initial plasma dry stripping, followed by secondary wet stripping with a stripping solution. This is followed by rinsing with a rinsing solution, rapid flushing and replacement cleaning, and centrifugal drying to gradually remove photoresist residues and impurities from the wafer surface. A PTFE basket and handle are used to prevent metal ion contamination, and nitrogen is used for centrifugal drying.

Benefits of technology

It improves the cleanliness of the wafer surface, suppresses β drift, improves the consistency of device parameters and yield, and reduces surface state disturbances caused by organic residues and particulate impurities.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123165040A_ABST
    Figure CN123165040A_ABST
Patent Text Reader

Abstract

The application belongs to the technical field of bipolar transistors, and discloses a wafer photoetching point pressing degumming method and system for controlling NPN bipolar transistor beta drift, which comprises the following steps: placing a wafer with a photoresist mask in a reaction cavity of a plasma etching machine to remove photoresist on the wafer surface; after being taken out from the plasma etching machine, the wafer is immersed in a stripping liquid for secondary degumming to remove the remaining photoresist on the wafer surface and photoresist residues modified by plasma; after being taken out from the stripping liquid, the wafer is immersed in a rinsing liquid to remove the residual stripping liquid attached to the wafer surface; the wafer cleaned by the rinsing liquid is transferred to a fast-draining water tank, and the wafer surface is subjected to displacement cleaning by using a fast-draining water method to remove the residual rinsing liquid and particulate impurities on the wafer surface; and the wafer cleaned by water flushing is subjected to centrifugal spin-drying treatment to remove free water on the wafer surface, thereby inhibiting abnormal drift of the NPN bipolar transistor forward current transmission ratio beta and reducing the beta value change amplitude before and after photoetching point pressing.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of bipolar transistor technology and relates to a method and system for removing photoresist from wafer photolithography points to control the β drift of NPN bipolar transistors. Background Technology

[0002] In the field of NPN bipolar transistors (NPN transistors) for discrete semiconductor devices, hFE (forward current transfer ratio, also known as β) is a parameter that measures the current amplification capability of the device. During chip wafer fabrication, controlling the β doubling state is a primary factor that needs to be controlled in the manufacturing process. Its stability directly determines whether the chip parameters can meet the specifications after fabrication. Therefore, the β doubling state must be controlled during the manufacturing process.

[0003] In NPN bipolar transistor manufacturing, after the aluminum interconnect is formed, one or more passivation layers need to be deposited on the surface to protect the device's stability. Then, photolithography is used to etch the passivation layer to form pressure points for subsequent bonding wires. Photolithography requires photoresist as a mask, and the photoresist must be completely removed after etching. However, existing photoresist removal methods struggle to completely remove the photoresist and modified residues generated by plasma after photolithography etching of the passivation layer. This results in residual impurities on the wafer surface interfering with the precise control of the subsequent β-doubling state, causing device β parameter drift and affecting product yield and parameter consistency. Summary of the Invention

[0004] To address the shortcomings of existing technologies, the present invention aims to provide a method and system for removing photoresist from wafer photolithography embossed points to control the β drift of NPN bipolar transistors.

[0005] To achieve the above objectives, the present invention adopts the following technical solution: This invention provides a method for removing photoresist from photolithographic foci on wafers to control β-drift of NPN bipolar transistors, comprising the following steps: placing a wafer with a photoresist mask in the reaction chamber of a plasma etching machine to remove the photoresist from the wafer surface; removing the photoresist-removed wafer from the plasma etching machine and immersing it in a stripping solution for a second photoresist removal to remove remaining photoresist and plasma-modified photoresist residue from the wafer surface; removing the second-removed wafer from the stripping solution and immersing it in a rinsing solution to remove residual stripping solution adhering to the wafer surface; transferring the rinsed wafer to a rapid rinsing tank and using a rapid rinsing method to replace and clean the wafer surface to remove residual rinsing solution and particulate impurities; and centrifuging the rinsed wafer to remove free water from the wafer surface.

[0006] Furthermore, the wafer is placed in the reaction chamber of the plasma etching machine, including: the wafer is placed on a 25-slot quartz boat in the plasma etching machine, the spacing between two adjacent slots of the quartz boat is set to 19.68±0.3 mm, and the slot width of the quartz boat is 1.19±0.05 mm.

[0007] Furthermore, the removal of photoresist from the wafer surface is performed using a Q240 plasma device; if the thickness of the photoresist on the wafer surface is 2.0 μm, the radio frequency power of the plasma device is 700±50 W, the oxygen flow rate in the reaction chamber is 300±10 sccm, the removal time is 30 min, and 2 / 3 to 3 / 4 of the photoresist thickness is removed.

[0008] Furthermore, after the photoresist-removed wafer is removed from the plasma etching machine, it is placed in a PTFE basket, and the PTFE basket carrying the wafer is placed into the quartz acid tank of the cleaning machine using a PTFE handle.

[0009] Furthermore, the stripping solution in the quartz acid tank is SN-01 type stripping solution, the temperature of the stripping solution is 100±10℃, and the immersion time of the polytetrafluoroethylene basket carrying the wafer is 30 min.

[0010] Furthermore, after the wafers that have undergone secondary desizing are removed from the stripping solution, the PTFE baskets carrying the wafers are removed from the quartz acid bath using PTFE handles. After being suspended for 10 seconds, the baskets are placed in a methanol rinsing solution and washed for 1 minute. The temperature of the methanol rinsing solution is 22±5 ℃.

[0011] Furthermore, the wafers cleaned with methanol rinsing solution and the polytetrafluoroethylene baskets are placed in a quick-drain rinsing tank for circulating cleaning.

[0012] Furthermore, the cleaned wafers and polytetrafluoroethylene baskets are placed in a centrifugal dryer for centrifugal drying at a speed of 2000 rpm for 10 minutes.

[0013] Furthermore, when the wafer and the polytetrafluoroethylene basket are centrifuged and dried in the centrifuge, nitrogen gas is introduced into the centrifuge.

[0014] This invention also provides a wafer photoresist removal and cleaning system for controlling the β drift of NPN bipolar transistors, comprising: a first photoresist removal module for placing a wafer with a photoresist mask in the reaction chamber of a plasma etching machine to remove the photoresist from the wafer surface; a second photoresist removal module for immersing the wafer, after photoresist removal from the plasma etching machine, in a stripping solution for secondary photoresist removal to remove remaining photoresist and plasma-modified photoresist residues from the wafer surface; an immersion module for immersing the wafer, after secondary photoresist removal, in a rinsing solution to remove residual stripping solution adhering to the wafer surface; a cleaning module for transferring the rinsed wafer to a rapid flushing tank and using a rapid flushing method to replace and clean the wafer surface, removing residual rinsing solution and particulate impurities; and a centrifugal drying module for centrifuging the rinsed wafer to remove free water from the wafer surface.

[0015] Compared with the prior art, the present invention has the following beneficial technical effects: This invention discloses a wafer photoresist removal method for controlling β drift in NPN bipolar transistors. The method employs a plasma dry removal process to initially remove most of the photoresist from the wafer surface. A second wet removal process using a stripping solution removes residual photoresist and plasma-modified residues. Finally, the wafer is immersed in a rinsing solution, subjected to rapid flushing and centrifugal drying to gradually remove residual stripping solution, rinsing solution, solid particles, and free moisture adhering to the wafer surface. This improves the cleanliness of the wafer surface, avoids surface state disturbances caused by organic residues and particulate impurities after photolithography of the passivation layer, suppresses abnormal drift in the forward current transfer ratio (β) of the NPN bipolar transistor, reduces the variation in β value before and after photolithography, improves parameter consistency between wafers, and increases device yield.

[0016] The spacing between adjacent slots in the quartz boat is 19.68±0.3mm, and the width of a single slot is 1.19±0.05mm. This ensures the flow and distribution of oxygen plasma between wafers within the reaction chamber, while avoiding differences in photoresist removal rates caused by mutual obstruction or spacing between wafers during plasma bombardment. This reduces the dispersion of β parameters caused by local differences in photoresist residue at the source.

[0017] After being cleaned with methanol rinsing solution, the wafers are placed together with a polytetrafluoroethylene basket in a fast-drain rinsing tank for circulating cleaning. The shear force and instantaneous dilution effect of the water flow are used to dynamically replace the wafer surface, removing residual methanol rinsing solution and any solid particulate impurities that may be attached to the wafer surface. This reduces the level of wafer surface contamination without introducing additional chemical reagents, reduces the risk of residues becoming surface recombination centers or charge traps, and suppresses β drift after photolithography.

[0018] The PTFE basket is immersed in SN-01 stripping solution at 100±10℃ for 30 minutes. During the immersion and cleaning process, the stripping solution penetrates into the photoresist film, causing swelling, rupture and dissolution. The thin layer of photoresist remaining after plasma ashing, along with the hard shell layer on the sidewall, is peeled off from the wafer surface, allowing the photoresist residue to be suspended in the liquid or settle to the bottom of the tank. The use of PTFE baskets and handles avoids metal ion contamination. At the same time, the corrosion resistance and low adsorption of PTFE ensure the purity of the stripping solution and does not introduce new impurities.

[0019] The PTFE basket carrying the wafer is lifted out of the quartz acid tank using a PTFE handle and suspended above the tank for 10 seconds to allow the stripping liquid adhering to the basket and wafer surface to drip back into the tank under gravity, reducing the contamination of the rinsing solution by the stripping liquid.

[0020] During the centrifugal drying process, nitrogen gas is continuously introduced into the cavity of the CXS series centrifuge of the 45th Institute. The nitrogen gas forms a positive pressure protective atmosphere in the cavity, which on the one hand removes air and moisture from the cavity, prevents the wafer surface from coming into contact with oxygen during the drying process to form a natural oxide layer, and inhibits the oxidation and discoloration of aluminum pressure points; on the other hand, it accelerates the evaporation of moisture and improves the drying efficiency. Attached Figure Description

[0021] Figure 1 This is a flowchart of a wafer photolithography point removal method for controlling β drift of an NPN bipolar transistor according to the present invention. Detailed Implementation

[0022] To enable those skilled in the art to better understand the present invention, the technical solutions of the present invention will be clearly and completely described below with reference to the accompanying drawings of the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort should fall within the scope of protection of the present invention.

[0023] Example 1 This invention discloses a method for removing resist from wafer photolithography marks to control β drift of NPN bipolar transistors, such as... Figure 1As shown, the process includes the following steps: placing a wafer with a photoresist mask in the reaction chamber of a plasma etching machine to remove the photoresist from the wafer surface; removing the photoresist-removed wafer from the plasma etching machine and immersing it in a stripping solution for a second photoresist removal to remove any remaining photoresist and plasma-modified photoresist residue from the wafer surface; removing the second photoresist-removed wafer from the stripping solution and immersing it in a rinsing solution to remove residual stripping solution from the wafer surface; transferring the rinsed wafer to a rapid rinsing tank and using a rapid rinsing method to replace and clean the wafer surface, removing residual rinsing solution and particulate impurities; and centrifuging the rinsed wafer to remove free water from the wafer surface.

[0024] The initial photoresist thickness on the wafer surface is 2.0 μm. Wafers with photoresist masks are first removed and then placed one by one into the corresponding slots of a 25-slot quartz boat in the plasma etching machine, using a horizontal insertion method. The slot spacing between adjacent slots in the quartz boat is 19.68 ± 0.3 mm, and the slot width of a single slot is 1.19 ± 0.05 mm. This ensures the flow and distribution of oxygen plasma within the reaction chamber between wafers while avoiding differences in photoresist removal rates caused by mutual obstruction or spacing during plasma bombardment. This reduces the dispersion of the β parameter caused by localized differences in photoresist residue at the source.

[0025] The quartz boat and wafer are fed into the reaction chamber of the Q240 plasma equipment, the chamber door is closed, and a vacuum is created. The Q240 plasma equipment is used to perform the initial resist removal process, providing controllable radio frequency glow discharge to generate high-concentration oxygen plasma.

[0026] For a wafer with a photoresist thickness of 2.0 μm, an RF power of 700 ± 50 W is applied, and oxygen is introduced into the reaction chamber at a flow rate of 300 ± 10 sccm. A uniform oxygen plasma region is formed within the reaction chamber. Oxygen free radicals react with the hydrocarbon polymers in the photoresist, generating volatile products such as CO, CO2, and H2O. The photoresist stripping time is 30 minutes, allowing the photoresist on the wafer surface to be gradually oxidized and stripped. Ultimately, 2 / 3 to 3 / 4 of the initial photoresist thickness is removed, meaning the 2.0 μm photoresist thickness is reduced to 0.5 μm to 0.67 μm within 30 minutes. This oxidative decomposition of organic contaminants on the wafer surface reduces the risk of residual impurities interfering with β-drift.

[0027] This method removes most of the photoresist, shortening the process time, while retaining a thin layer of photoresist to avoid excessive exposure of the underlying passivation layer and aluminum metal by the plasma, and to prevent potential physical damage or charge accumulation. Simultaneously, the retained photoresist is more easily swollen and stripped in the stripping solution. The plasma only modifies the surface colloid, while the underlying colloid remains incompletely hardened, making it easier to remove completely.

[0028] The quartz boat is then removed from the reaction chamber. After the wafers have cooled to room temperature, they are individually removed from the quartz boat using a vacuum pen or tweezers and placed inside a PTFE basket. This basket can vertically support multiple wafers while keeping them isolated from each other. The PTFE basket is moved using a PTFE handle, first suspending the basket containing the wafers above the quartz acid tank of the Naura H63 series cleaning machine. The quartz acid tank contains SN-01 stripping solution, a mixture of organic amines and polar solvents that dissolves and swells photoresist. The temperature of the stripping solution is 100±10℃, which accelerates the dissolution and stripping process of the photoresist. The PTFE basket is then immersed in the 100±10℃ SN-01 stripping solution, ensuring the liquid completely submerges all wafers, for a cleaning time of 30 minutes. During the immersion cleaning process, the stripping solution interacts with the residual photoresist on the wafer surface, as well as the photoresist residue after plasma modification: the stripping solution penetrates into the photoresist film, causing swelling, rupture, and dissolution, peeling off the thin layer of photoresist remaining after plasma ashing, along with the hard shell layer on the sidewalls, from the wafer surface, leaving the photoresist residue suspended in the liquid or settling to the bottom of the tank. The use of PTFE baskets and handles avoids metal ion contamination, while the corrosion resistance and low adsorption properties of PTFE ensure the purity of the stripping solution, preventing the introduction of new impurities.

[0029] If residues remain on the wafer surface, they will carbonize or decompose during high-temperature processes, releasing charged particles or impurities, causing surface state changes, and consequently leading to uncontrollable drift of the β parameter. Immersion in SN-01 stripping solution at 100±10℃ for 30 minutes completely dissolves and removes residual photoresist, reducing the residual level of organic contaminants on the wafer surface.

[0030] After the second stripping process, the PTFE basket carrying the wafer is lifted from the quartz acid tank using a PTFE handle and suspended above the tank for 10 seconds to allow the stripping solution adhering to the basket and wafer surface to drip back into the tank under gravity, reducing contamination of the rinsing solution. After 10 seconds of suspension, the basket is placed entirely into a quartz or PTFE tank containing methanol rinsing solution. The methanol rinsing solution is at a temperature of 22±5℃. The basket is fully immersed in the methanol rinsing solution. Methanol, as a polar solvent, is miscible with the residual stripping solution components adhering to the wafer surface. Through diffusion and convection, the high-viscosity stripping solution residue is displaced and diluted from the wafer surface into the methanol. The rinsing time is 1 minute, replacing most of the residual stripping solution.

[0031] Methanol rinsing can quickly and efficiently remove residual stripping solution from the wafer surface, preventing the formation of difficult-to-remove films or crystals on the wafer surface after the stripping solution dries. These films can cause poor soldering or increase contact resistance during wire bonding, and trapped charges can affect the electric field distribution, leading to deterioration of β characteristics. A temperature of 22±5℃ avoids the stress caused by excessively high temperatures leading to rapid methanol evaporation and rapid heating / cooling on the wafer surface, while also avoiding the decrease in cleaning efficiency caused by excessively low temperatures.

[0032] After being rinsed with methanol, the wafers and polytetrafluoroethylene baskets are directly transferred to the Quick Displacement Rinse-Drain (QDR) tank. The QDR is a device that dynamically replaces and cleans the wafer surface by rapidly injecting and draining ultrapure water. Using the QDR mode, the wafer surface is replaced and cleaned. During operation, the basket carrying the wafer is placed on a fixed support in the QDR tank. After the liquid level rises and submerges the wafer, the water is drained through the bottom quick-drain valve. In this embodiment, 10 consecutive rinsing cycles are required.

[0033] The shear force of each injection and evacuation of water effectively removes residual methanol rinsing solution and attached fine solid particles, such as photoresist residue and dust, from the wafer surface and basket. Rapid rinsing, relying on the physical impact and instantaneous dilution effect of the water flow, reduces chemical residues and particulate contamination on the wafer surface without introducing any chemical reagents or causing secondary pollution. Ten cycles of rapid rinsing thoroughly remove the trace amounts of stripping solution and methanol rinsing solution remaining on the wafer surface, while also removing particulate impurities. This prevents these impurities from becoming leakage paths or stress concentration points during subsequent baking or packaging processes, ensuring the stability of the device surface condition.

[0034] In this embodiment, a rapid flushing process with 10 cycles is used, and the specific number of cycles can be adjusted adaptively according to actual production needs.

[0035] After rinsing, the wafers are removed from the PTFE basket and placed into the rotor of the CXS series centrifugal dryer from the 45th Research Institute. The CXS series centrifugal dryer utilizes centrifugal force to remove free moisture from the wafer surface. The dryer operates at 2000 rpm, with a single centrifugal cycle lasting 10 minutes. During the rotor's initial acceleration to 2000 rpm and subsequent constant rotation, moisture on the wafer surface and in the basket is thrown against the chamber wall by centrifugal force and drains through the drain outlet. Throughout the centrifugal drying process, nitrogen gas is continuously introduced into the chamber of the CXS series centrifugal dryer. The nitrogen creates a positive pressure protective atmosphere within the chamber, both to expel air and moisture, preventing the wafer surface from contacting oxygen during drying and forming a natural oxide layer, thus inhibiting oxidation and discoloration of the aluminum pressure points; and to accelerate moisture evaporation, improving drying efficiency.

[0036] Centrifugal drying removes free moisture from the wafer surface quickly and without leaving watermarks, avoiding the formation of water marks and stains during slow drying. Water marks can dissolve residual impurities and leave contaminants after evaporation, affecting the quality of the bonding area, leading to insufficient bond strength or changes in contact resistance, and consequently causing β parameter shifts. Under nitrogen atmosphere, the wafer is dried while protecting the metal contact surfaces from oxidation, maintaining electrical contact characteristics.

[0037] In summary, by eliminating surface state instability caused by organic contaminants and particles, the influence on the surface recombination rate of minority carriers is avoided, ensuring that the current gain β of the NPN bipolar transistor remains stable in subsequent processes and tests without abnormal drift.

[0038] The experiment was conducted on the NPN transistor 2N2222A, and the comparative data are shown in Table 1.

[0039] Table 1. Comparison data from tests on the 2N2222A NPN transistor.

[0040] Comparative tests were conducted on NPN transistors of model 2N2222A under different conditions within the same batch. Twelve wafers from the same batch were selected for the tests. Wafers #1 to #6 were not subjected to the wafer photolithography-based resist removal method, while wafers #7 to #12 were subjected to the wafer photolithography-based resist removal method. The forward current transfer ratio β of all samples was measured at three positions—the upper, middle, and lower points—before and after photolithography-based resist removal. The test conditions were Vce = 10V and Ic = 150mA. The comparative data are shown in Table 1.

[0041] Samples 1 through 6 showed an increase in β value after photolithography etching, with a maximum increase of 33. Multiple test points showed increases exceeding 15, and the β change amplitude varied significantly between different locations within the same wafer. For example, in sample 2, the β value increased from 134 to 167 at the top, 132 to 158 at the middle, and 138 to 166 at the bottom, indicating uneven β drift in this group of wafers after photolithography etching of the passivation layer, and poor parameter consistency before and after photolithography etching.

[0042] For samples #7 to #12, the β values ​​showed only minor changes after photolithography pressing, with the variation at each test point controlled within 5, and most changes between 1 and 3. The β values ​​at the top, middle, and bottom points within the same wafer tended to be consistent, and inter-wafer differences were significantly reduced. For example, for sample #7, the β value at the top point changed from 130 to 133, at the middle point from 130 to 135, and at the bottom point from 132 to 135; for sample #12, the β value at the top point changed from 134 to 135, at the middle point from 131 to 134, and at the bottom point from 130 to 133. This indicates that the residue on the wafer surface was removed, avoiding surface state disturbances caused by residual photoresist and plasma modification products, suppressing the uncontrollable increase in β values ​​after photolithography pressing, and improving the consistency and stability of device parameters.

[0043] The wafer was treated with a Q240 plasma scanner at 700±50W power and 300±10sccm oxygen flow for 30 min, removing 2 / 3 to 3 / 4 of the photoresist thickness. This removed most of the photoresist bulk while avoiding damage to the underlying passivation layer and aluminum metal. The wafer was then immersed in SN-01 stripping solution at 100±10℃ for 30 min to dissolve and remove residual photoresist and plasma-modified residues. It was then rinsed with methanol at 22±5℃ for 1 min to remove residual stripping solution adhering to the wafer surface. Ten cycles of rapid flushing were performed to remove methanol and solid particulate impurities. Finally, the wafer was centrifuged at 2000 rpm under nitrogen protection for 10 min to obtain a clean and dry wafer surface. This process reduced organic contamination and particulate residue on the wafer surface, decreased surface recombination centers, and thus prevented abnormal drift of the β parameter after photolithography.

[0044] In summary, the wafer photolithography point-based resist removal method can reduce the β drift amplitude while ensuring resist removal.

[0045] Example 2 The present invention provides a wafer de-adhesion cleaning system for controlling the β drift of NPN bipolar transistors, comprising a first de-adhesion module, a second de-adhesion module, an immersion module, a cleaning module, and a spin-drying module.

[0046] The first photoresist removal module: Places the wafer with the photoresist mask inside the reaction chamber of the plasma etching machine to remove the photoresist from the wafer surface. The second photoresist removal module: After removing the photoresist-removed wafer from the plasma etching machine, immerses it in a stripping solution for a second photoresist removal, removing any remaining photoresist and plasma-modified photoresist residue from the wafer surface. The immersion module: After the second photoresist removal, removes the wafer from the stripping solution and immerses it in a rinsing solution to remove residual stripping solution from the wafer surface. The cleaning module: Transfers the rinsed wafer to a rapid-drain rinsing tank and uses a rapid-drain rinsing method to replace and clean the wafer surface, removing residual rinsing solution and particulate impurities. The spin-drying module: Centrifuges the rinsed wafer to remove free water from the wafer surface.

[0047] The wafer resist removal and cleaning system for controlling the β drift of NPN bipolar transistors of the present invention can achieve the same method steps as the above method, so it will not be described again.

[0048] The above embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit it. Although the present invention has been described in detail with reference to preferred embodiments, those skilled in the art should understand that modifications or equivalent substitutions can be made to the technical solutions of the present invention without departing from the spirit and scope of the present invention, and all such modifications or substitutions should be covered within the scope of the claims of the present invention. The technologies, shapes, and structures not described in detail in this invention are all well-known technologies. Any equivalent structural or procedural transformations made based on the content of this specification and drawings, or direct or indirect applications in other related technical fields, are similarly included within the patent protection scope of this invention.

[0049] It should be noted that the terms "first," "second," etc., in the specification, claims, and accompanying drawings of this invention are used to distinguish similar objects and are not necessarily used to describe a specific order or sequence. It should be understood that such data can be interchanged where appropriate so that the embodiments of the invention described herein can be implemented in orders other than those illustrated or described herein. Furthermore, the terms "comprising" and "having," and any variations thereof, are intended to cover a non-exclusive inclusion; for example, a process, method, system, product, or apparatus that comprises a series of steps or units is not necessarily limited to those steps or units explicitly listed, but may include other steps or units not explicitly listed or inherent to such processes, methods, products, or apparatus.

Claims

1. A method for removing resist from wafer photolithography marks to control β drift of NPN bipolar transistors, characterized in that, Includes the following steps: The wafer with the photoresist mask is placed in the reaction chamber of the plasma etching machine to remove the photoresist from the wafer surface; After the photoresist-removed wafer is removed from the plasma etching machine, it is immersed in the stripping solution for a second photoresist removal to remove the remaining photoresist on the wafer surface and the photoresist residue after plasma modification. After the wafers undergoing secondary desizing are removed from the stripping solution, they are immersed in rinsing solution to remove residual stripping solution adhering to the wafer surface. After rinsing with the rinsing solution, the wafers are transferred to a quick-drain rinsing tank. The quick-drain rinsing method is used to replace and clean the wafer surface, removing residual rinsing solution and particulate impurities. After rinsing with water, the wafers are centrifuged to remove free moisture from their surface.

2. The wafer photolithography point removal method for controlling β drift of NPN bipolar transistors according to claim 1, characterized in that, The wafer is placed in the reaction chamber of the plasma etching machine, including: The wafer is placed on a 25-slot quartz boat inside a plasma etching machine. The spacing between two adjacent slots on the quartz boat is set to 19.68±0.3 mm, and the slot width of the quartz boat is 1.19±0.05 mm.

3. The wafer photolithography point removal method for controlling β drift of NPN bipolar transistors according to claim 2, characterized in that: The removal of photoresist from the wafer surface was performed using a Q240 plasma equipment. If the thickness of the photoresist on the wafer surface is 2.0 μm, the radio frequency power of the plasma equipment is 700±50 W, the oxygen flow rate in the reaction chamber is 300±10 sccm, the photoresist removal time is 30 min, and 2 / 3 to 3 / 4 of the photoresist thickness is removed.

4. The wafer photolithography point removal method for controlling β drift of NPN bipolar transistors according to claim 1, characterized in that: After the photoresist-removed wafer is removed from the plasma etching machine, it is placed in a PTFE basket and then placed into the quartz acid tank of the cleaning machine using a PTFE handle.

5. The wafer photolithography point removal method for controlling β drift of NPN bipolar transistors according to claim 4, characterized in that: The stripping solution in the quartz acid tank is SN-01 type stripping solution, the temperature of the stripping solution is 100±10℃, and the immersion time of the polytetrafluoroethylene basket carrying the wafer is 30 min.

6. The wafer photolithography point removal method for controlling β drift of NPN bipolar transistors according to claim 5, characterized in that: After the wafers undergoing secondary desizing are removed from the stripping solution, the PTFE baskets carrying the wafers are taken out of the quartz acid bath using PTFE handles. After being suspended for 10 seconds, the wafers are placed in a methanol rinsing solution at a temperature of 22±5 ℃ for 1 minute.

7. The wafer photolithography point removal method for controlling β drift of NPN bipolar transistors according to claim 6, characterized in that: The wafers cleaned with methanol rinsing solution and the polytetrafluoroethylene baskets are placed in a quick-drain rinsing tank for circulating cleaning.

8. The wafer photolithography point removal method for controlling β drift of NPN bipolar transistors according to claim 7, characterized in that: After the wafers are cleaned, they are placed in a PTFE basket and centrifuged in a spin dryer at a speed of 2000 rpm for 10 minutes.

9. The wafer photolithography point removal method for controlling β drift of NPN bipolar transistors according to claim 8, characterized in that: When the wafer and the polytetrafluoroethylene basket are centrifuged and dried in the centrifuge, nitrogen gas is introduced into the centrifuge.

10. A wafer resist removal and cleaning system for controlling β drift of NPN bipolar transistors, characterized in that: First photoresist removal module: used to place the wafer with the photoresist mask into the reaction chamber of the plasma etching machine and remove the photoresist from the wafer surface; The second photoresist removal module is used to remove the photoresist-removed wafer from the plasma etching machine and immerse it in the stripping solution for a second photoresist removal, removing the remaining photoresist on the wafer surface and the photoresist residue after plasma modification. Immersion module: Used to remove the wafers after secondary desizing from the stripping solution and immerse them in rinsing solution to remove residual stripping solution adhering to the wafer surface; Cleaning module: Used to transfer the wafers after rinsing with rinsing solution to the quick-drain rinsing tank, and use the quick-drain rinsing method to replace and clean the wafer surface to remove residual rinsing solution and particulate impurities. Spin-drying module: Used to centrifuge and spin-dry the wafers after rinsing to remove free moisture from the wafer surface.