Wafer defect traceability detection method
By performing two scans of the wafer surface with different sensitivities and epitaxial layer growth, combined with data analysis, latent defects were accurately located, solving the problem of misjudgment of latent defects and improving the quality and yield of semiconductor structures.
Patent Information
- Application Number
- CN202611443399.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-17
- Publication Date
- 2026-11-24
AI Technical Summary
In semiconductor manufacturing, latent defects are difficult to identify before thin film deposition, leading to them being misjudged as defects generated during the thin film deposition process after deposition, which misleads the identification of the defect source and increases costs.
By employing two scanning methods with different sensitivities, combined with epitaxial layer growth, and by eliminating interference terms, common defect results are screened out, and latent defects are accurately located.
This enabled precise tracing of defects, established directions for improvement, and enhanced the quality and yield of semiconductor structures.
Smart Images

Figure CN123165079A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of semiconductor technology, and more specifically to a method for tracing and detecting wafer defects. Background Technology
[0002] In semiconductor manufacturing, performing multiple thin-film deposition processes on the wafer surface is a crucial step in wafer structure fabrication and functional layer formation. Before deposition, the wafer surface contains various minute, latent defects that are difficult to detect during pre-deposition inspections. However, after deposition, these latent defects are encapsulated by the film, increasing in size and becoming easier to identify. Because these defects are only discovered after deposition, they are easily misjudged as originating during the deposition process, misleading the identification of the defect source and causing subsequent defect remediation efforts to be misguided, increasing costs in terms of manpower and equipment. Summary of the Invention
[0003] This invention proposes a method for tracing the source of wafer defects. By using the method provided by this invention, defects can be accurately traced to their source, so as to identify the direction of defect improvement and thus accurately improve the quality of semiconductor structure.
[0004] To address the aforementioned technical problems, this invention provides a method for tracing and detecting wafer defects, comprising at least the following steps: A first wafer is provided, the surface of which has original defects, including explicit defects and implicit defects; A first scan is performed on the surface of the first wafer to obtain a first defect scan result, which includes the explicit defects. A second scan is performed on the surface of the first wafer to obtain a second defect scan result, which includes the original defect and interference items. The first defect scan result is excluded from the second defect scan result to obtain the third defect scan result; After growing an epitaxial layer on the surface of the first wafer, the epitaxial layer is subjected to the first scan to obtain a fourth defect scan result, which includes the original defect and the epitaxial defect; and The common defect scan results that are repeated in the third defect scan results and the fourth defect scan results are filtered out, and the latent defect is located based on the common defect scan results.
[0005] In one embodiment of the present invention, the defect scanning results of the first scan and the second scan include a defect distribution location map and a feature value of each defect, wherein the feature value includes at least one of grayscale, energy and size.
[0006] In one embodiment of the present invention, after obtaining the common defect scanning results, the latent defect is located according to the common defect distribution location map in the common defect scanning results.
[0007] In one embodiment of the present invention, after obtaining the common defect scanning results, defect detection is performed on a second wafer from the same batch as the first wafer, which includes at least the following steps: The first data sample of the grayscale feature value in the public defect scanning results is statistically analyzed, and the mean x1 and standard deviation S1 of the first data sample are obtained. Data outside the range [x1-3S1, x1+3S1] in the first data sample is excluded to obtain the first correction sample; Data samples within the confidence interval of the first correction sample are selected to obtain a first standard sample. Based on the upper and lower limits of the first standard sample, a grayscale standard for judging the latent defect is determined. Repeat the steps of statistical analysis, elimination, and screening of the energy characteristic value and the size characteristic value to obtain the energy standard and size standard for judging the latent defect.
[0008] In one embodiment of the present invention, after obtaining the grayscale standard, the energy standard and the size standard, the surface of the second wafer is scanned for the first time to obtain the fifth defect scan result and locate the visible defects on the surface of the second wafer.
[0009] In one embodiment of the present invention, after locating the visible defects on the surface of the second wafer, it is also necessary to locate the hidden defects on the surface of the second wafer, which includes at least the following steps: The second scan is performed on the surface of the second wafer to obtain the sixth defect scan result; and Based on the grayscale standard, the energy standard, and the size standard, the target defect results in the sixth defect scan results are selected, and based on the target defect results, the latent defects on the surface of the second wafer are located.
[0010] In one embodiment of the present invention, when locating latent defects on the surface of the second wafer, target feature values that simultaneously meet the grayscale standard, the energy standard, and the size standard are selected from the sixth defect scanning results, and the position of the target defect corresponding to the target feature value is located in the defect distribution location map of the sixth defect scanning results, thereby completing the location of latent defects on the surface of the second wafer.
[0011] In one embodiment of the present invention, the sensitivity of the first scan is lower than the sensitivity of the second scan.
[0012] In one embodiment of the present invention, the method for the first scan and the second scan is a bright-field scanning method.
[0013] In one embodiment of the present invention, in the first scan, the pixel size is 0.8μm-2.0μm and the light transmission ratio of the light source aperture is 50%-70%; in the second scan, the pixel size is 0.2μm-0.7μm and the light transmission ratio of the light source aperture is 20%-45%.
[0014] In summary, this invention proposes a method for tracing the source of wafer defects. By improving the existing method, the unexpected technical effect of this application is the ability to accurately trace the source of defects, thereby confirming the direction for defect improvement and precisely improving the quality of the semiconductor structure. Furthermore, the wafer defect tracing method proposed in this invention can comprehensively detect defects on the wafer surface, rigorously screening out defective products and improving the yield rate. Attached Figure Description
[0015] To more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings used in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0016] Figure 1 This is a flowchart of the wafer defect tracing and detection method of the present invention.
[0017] Figure 2 This is a schematic diagram of the defect distribution locations in the first defect scan result.
[0018] Figure 3 for Figure 2 The electron microscope schematic diagram of the corresponding dominant defect.
[0019] Figure 4 This is a schematic diagram of the defect distribution locations in the second defect scan results.
[0020] Figure 5 for Figure 4 The electron microscope diagram corresponding to the latent defect is shown in the image.
[0021] Figure 6 This is a schematic diagram of the defect distribution locations in the third defect scan results.
[0022] Figure 7 for Figure 6 Electron micrograph of the corresponding interference term.
[0023] Figure 8 This is a schematic diagram of the defect distribution locations in the fourth defect scan results.
[0024] Figure 9 for Figure 8 A schematic diagram of an electron microscope corresponding to an epitaxial defect.
[0025] Figure 10 This is a schematic diagram showing the location of defects in the common defect scan results.
[0026] Label Explanation: 10. First wafer; 11. Dominant defect; 12. Latent defect; 13. Interference term; 14. Epitaxial defect. Detailed Implementation
[0027] The following specific examples illustrate the implementation of the present invention. Those skilled in the art can easily understand other advantages and effects of the present invention from the content disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and various details in this specification can also be modified or changed based on different viewpoints and applications without departing from the spirit of the present invention.
[0028] It should be understood that the invention can be embodied in various forms and should not be construed as being limited to the embodiments set forth herein. Rather, providing these embodiments will make the disclosure thorough and complete, and will fully convey the scope of the invention to those skilled in the art.
[0029] The technical solution of the present invention will be further described in detail below with reference to the embodiments. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0030] Please see Figures 1 to 10 As shown, this invention provides a method for tracing the source of wafer defects, which can accurately trace the source of defects to identify the direction of defect improvement and thus accurately improve the quality of semiconductor structures. The method includes steps S11-S16.
[0031] Step S11: Provide a first wafer 10, the surface of the first wafer 10 having original defects, including explicit defects 11 and implicit defects 12.
[0032] Step S12: Perform a first scan on the surface of the first wafer 10 to obtain the first defect scan result, which includes the explicit defect 11.
[0033] Step S13: Perform a second scan on the surface of the first wafer 10 to obtain the second defect scan result, which includes the original defect and interference item 13.
[0034] Step S14: Exclude the first defect scan result from the second defect scan result to obtain the third defect scan result.
[0035] Step S15: After growing an epitaxial layer on the surface of the first wafer 10, the epitaxial layer is scanned for the first time to obtain the fourth defect scan result, which includes the original defect and the epitaxial defect 14.
[0036] Step S16: Filter out the common defect scan results that are repeated in the third defect scan results and the fourth defect scan results, and locate the latent defect 12 based on the common defect scan results.
[0037] Please see Figure 1 As shown, in one embodiment of the present invention, in step S11, the surface of the first wafer 10 has original defects formed by the manufacturing process. These original defects can be classified into two categories according to their identifiability: explicit defects 11 and latent defects 12. Explicit defects 11 are characterized by significant differences in wafer surface morphology or optical features, and can be directly identified and captured using conventional scanning methods. Latent defects 12 are characterized by weak wafer surface features or insignificant differences in morphology, making them difficult to detect directly using conventional scanning methods. High-sensitivity scanning methods are required for effective identification. However, high-sensitivity scanning methods easily detect many interference items 13, thus making it impossible to accurately distinguish latent defects 12. These interference items 13 originate from weak background signals such as optical and circuit noise of the detection equipment, environmental micro-vibrations, and electromagnetic interference. These weak background signals are amplified in high-sensitivity scanning methods, thus enabling their detection.
[0038] Please see Figures 1 to 2As shown, in one embodiment of the present invention, after obtaining the first wafer 10, in step S12, the surface of the first wafer 10 is scanned for the first time to obtain a first defect scanning result. The first scan, for example, employs a bright-field scanning method, and this method is performed, for example, on a bright-field scanning machine. Specifically, in the first scan, for example, a coaxial vertical bright-field illumination method is used to perform a full-area defect scan detection on the surface of the first wafer 10. The wavelength of the light source is, for example, 450nm-650nm, the pixel size is, for example, 0.8μm-2.0μm, the light transmission ratio of the light source aperture is, for example, 50%-70%, the scanning speed is, for example, 200mm / s-350mm / s, the grayscale threshold is, for example, 80-140, the energy relative to the substrate reflected energy threshold is, for example, 25%-40%, and the defect equivalent diameter threshold is, for example, 0.5μm-1.5μm. By controlling the scanning parameters, the sensitivity level of the first scan can be controlled at a medium sensitivity level, specifically, level 3-4, thereby enabling the detection of visible defects 11 on the surface of the first wafer 10 and obtaining a first defect scan result including the visible defects 11. The first defect scan result includes, for example, a defect distribution map of the visible defects 11 and characteristic values of each defect. Characteristic values include, for example, at least one of grayscale, energy, and size, with the size being, for example, the equivalent diameter of the defect. Furthermore, based on the defect distribution map of the visible defects 11, each visible defect 11 on the surface of the first wafer 10 can be characterized using scanning electron microscopy, thereby enabling the classification of the type of each visible defect 11 to comprehensively understand its characteristics. The characterization of the visible defects 11 under the electron microscope is as follows: Figure 3 As shown.
[0039] Please see Figures 1 to 7As shown, in one embodiment of the present invention, after obtaining the first defect scanning result, in step S13, the surface of the first wafer 10 is scanned a second time to obtain the second defect scanning result. The second scan, for example, employs a bright-field scanning method, and this method is performed, for example, on a bright-field scanning machine. Specifically, in the second scan, for example, a coaxial vertical bright-field illumination method is used to perform a full-area defect scan on the surface of the first wafer 10. The wavelength of the light source is, for example, 400nm-550nm, the pixel size is, for example, 0.2μm-0.7μm, the light transmission ratio of the light source aperture is, for example, 20%-45%, the scanning speed is, for example, 50mm / s-180mm / s, the grayscale threshold is, for example, 30-75, the energy relative to the substrate reflection energy threshold is, for example, 10%-23%, and the defect equivalent diameter threshold is, for example, 0.2μm-0.45μm. Compared to the first scan, the second scan, by reducing scanning parameters such as pixel size and the light transmission ratio of the light source aperture, can control the sensitivity level of the second scan to a high level, specifically ≥5 levels. This allows for the simultaneous detection of both explicit defects 11 and latent defects 12 on the surface of the first wafer 10, obtaining the second defect scanning results for the original defects. The characterization of latent defect 12 under an electron microscope is as follows: Figure 5 As shown. The second defect scan result includes, for example, a defect distribution map of the original defect and feature values for each defect. Feature values include, for example, at least one of grayscale, energy, and size, with size being, for example, the equivalent diameter of the defect. However, due to the high sensitivity of the second scan, not only the original defect can be detected in the second defect scan result, but also many interference items 13. The presence of interference items 13 makes it impossible to accurately obtain the original defect based on the second defect scan result. It should be noted that interference items 13 include regions or feature structures with grayscale values similar to the defect, as well as interference signals that are misjudged. For example, weak background signals such as optical and circuit noise of the detection equipment, environmental micro-vibrations, and electromagnetic interference are amplified in high-sensitivity scanning methods, thus being detected and identified by the machine as defects. However, the actual scanned corresponding location, such as... Figure 7 As shown, Figure 7 The defect structure corresponding to the defect signal does not exist in the image, indicating that this is a false alarm. The area of a wafer is millions of times larger than that of a single defect structure; therefore, manually checking each defect individually using electron microscopy images to eliminate interference item 13 is time-consuming and laborious. However, this invention, through multiple scans and scans based on epitaxial layer deposition, can eliminate the influence of interference item 13 without verifying the authenticity of each individual item.
[0040] Please see Figures 1 to 6As shown, in one embodiment of the present invention, after obtaining the second defect scanning result, in step S14, the first defect scanning result in the second defect scanning result is excluded to obtain the third defect scanning result. Specifically, the defect distribution location map of the original defect in the second defect scanning result is compared with the defect distribution location map of the explicit defect 11 in the first defect scanning result. The defect distribution location of the explicit defect 11 is deleted from the defect distribution location map of the original defect, and the defect distribution location maps of the latent defect 12 and interference item 13 are obtained. The feature value of each location is then calculated to obtain the third defect scanning result. The third defect scanning result includes the defect distribution location maps of the latent defect 12 and interference item 13, and the feature value of each location in the defect distribution location maps.
[0041] Please see Figures 1 to 6 As shown, in one embodiment of the present invention, after obtaining the third defect scanning result, in step S15, an epitaxial layer is grown on the surface of the first wafer 10. The epitaxial layer is formed by methods such as low-pressure chemical vapor deposition, plasma-enhanced chemical vapor deposition, rapid thermal chemical vapor deposition, or molecular beam epitaxy. The epitaxial layer is, for example, a homoepitaxial layer or a heteroepitaxial layer.
[0042] Please see Figures 1 to 8 As shown, in one embodiment of the present invention, after the epitaxial layer is formed, in step S15, a first scan is performed on the epitaxial layer to obtain a fourth defect scan result. The fourth defect scan result includes a defect distribution location map and a feature value for each defect. The feature value includes at least one of grayscale, energy, and size, and the size is, for example, the equivalent diameter of the defect. The method and parameters of the first scan are detailed in step S12 above and will not be elaborated here. Since the latent defect 12 is not significant, it cannot be identified by the first scan in step S11. However, as the epitaxial layer grows, the latent defect 12 becomes more obvious as it is covered by the epitaxial layer. Therefore, the latent defect 12 can be identified in the fourth defect scan result obtained by the first scan in step S15. Therefore, in the fourth defect scan result, the defects include the latent defect 12, as well as the obvious explicit defect 11 that was relatively obvious before the epitaxial layer grew, and the epitaxial defect 14 generated during the epitaxial process. The characterization of the epitaxial defect 14 under an electron microscope is as follows. Figure 9 As shown.
[0043] Please see Figures 1 to 10 As shown, in one embodiment of the present invention, after obtaining the fourth defect scanning result, in step S16, the defect distribution location maps in the fourth defect scanning result and the third defect scanning result are compared, the duplicate common defect distribution locations are filtered out, and the feature value of each common defect in the common defect distribution location is counted, thereby obtaining the common defect scanning result.
[0044] Please see Figures 1 to 10 As shown, in one embodiment of the present invention, after obtaining the common defect scanning results, in step S16, the latent defects 12 on the surface of the first wafer 10 can be located according to the distribution location of the common defects, so as to accurately trace the source of the latent defects 12, so as to confirm the direction of defect improvement, thereby accurately improving the quality of the semiconductor structure.
[0045] Please see Figures 1 to 10 As shown, in one embodiment of the present invention, after obtaining the common defect scanning results, in step S16, latent defects on the surfaces of other wafers in the same batch as the first wafer 10 are located based on the characteristic values of the common defects. Specifically, taking the second wafer as an example, the location process is described in detail. The second wafer and the first wafer 10 belong to the same batch and are fabricated under the same process technology. The positions and characteristic values of defects on the surfaces of the two wafers are common. Therefore, latent defects on the second wafer can be located and identified based on the information of the latent defects 12 on the first wafer 10. The location of latent defects on the surface of the second wafer includes at least steps S161-S165.
[0046] Step S161: Statistically analyze the first data sample of grayscale feature values in the public defect scanning results, and obtain the mean x1 and standard deviation S1 of the first data sample.
[0047] Step S162: Remove data outside the range [x1-3S1, x1+3S1] from the first data sample to obtain the first correction sample.
[0048] Step S163: Select data samples that are within the confidence interval in the first calibration sample to obtain the first standard sample, and determine the gray scale standard for judging latent defects based on the upper and lower limits of the first standard sample.
[0049] Step S164: Repeat the steps of statistical analysis, elimination, and screening of energy characteristic values and size characteristic values to obtain energy standards and size standards for judging latent defects.
[0050] Step S165: Perform a first scan on the surface of the second wafer to obtain the fifth defect scan result, and use it to locate the visible defects on the surface of the second wafer.
[0051] Step S166: Perform a second scan on the surface of the second wafer to obtain the sixth defect scan result.
[0052] Step S167: Based on the grayscale standard, energy standard and size standard, select the target defect results in the sixth defect scan results, and locate the latent defects on the second wafer surface based on the target defect results.
[0053] In one embodiment of the present invention, in step S161, the grayscale feature value of each defect is selected from the common defect scanning results, and a first data sample of grayscale feature values is constructed. Then the mean x1 and standard deviation S1 of the first data sample are calculated.
[0054] In one embodiment of the present invention, the mean x1 and standard deviation S1 of the first data sample are obtained. In step S162, data in the first data sample outside the range [x1-3S1, x1+3S1] are excluded to obtain a first corrected sample, thereby eliminating outliers and occasional values in the first data sample. Simultaneously, in step S163, data samples within the confidence interval of the first corrected sample are selected to obtain a first standard sample. The confidence level of the confidence interval is, for example, 90%-95%. In this embodiment, the selection process is described using a confidence level of 95% as an example. Specifically, data samples within the range [x2-1.96×(S2 / ...] are selected from the first corrected sample... ),x2+1.96×(S2 / Using data within the range of )], construct the first standard sample, where n is the number of data points in the first calibration sample. x2 is the mean of the first corrected sample, and S2 is the standard deviation of the first corrected sample.
[0055] In one embodiment of the present invention, after obtaining the first standard sample, in step S163, a grayscale standard for judging latent defects is determined based on the upper and lower limits of the first standard sample. Specifically, the maximum and minimum values of the grayscale feature values in the first standard sample are compared and selected, and the interval between the two is used as the grayscale standard for judging latent defects.
[0056] In one embodiment of the present invention, after obtaining the grayscale standard, in step S164, the energy feature values are repeatedly subjected to statistical, exclusion, and screening steps to obtain the energy standard for judging latent defects. Then, the size feature values are repeatedly subjected to statistical, exclusion, and screening steps to obtain the size standard for judging latent defects. The statistical, exclusion, and screening process is detailed in steps S161-S163 and will not be elaborated further here.
[0057] In one embodiment of the present invention, after obtaining the grayscale standard, energy standard, and size standard, in step S165, the surface of the second wafer is scanned for the first time to obtain the fifth defect scan result. The method and parameters of the first scan are detailed in step S12 above and will not be elaborated further here. The fifth defect scan result includes a defect distribution map of visible defects on the surface of the second wafer and the characteristic value of each defect, etc., so that the location of visible defects on the surface of the second wafer and the characteristic value of the visible defects can be determined based on the fifth defect scan result.
[0058] In one embodiment of the present invention, after identifying a visible defect on the surface of the second wafer, in step S166, a second scan is performed on the surface of the second wafer to obtain a sixth defect scan result. The method and parameters of the second scan are detailed in step S13 above and will not be elaborated further here. The sixth defect scan result includes a defect distribution location map and characteristic values of each defect, etc. The defects include visible defects, latent defects, and interference terms on the surface of the second wafer.
[0059] In one embodiment of the present invention, after obtaining the sixth defect scanning result, in step S167, target feature values that simultaneously meet the grayscale standard, energy standard, and size standard are selected from the feature values of the defects in the sixth defect scanning result. The location of the target defect corresponding to the target feature value is then located in the defect distribution location map, thus completing the location of the latent defects on the second wafer surface. Through step S16, not only can explicit defects on the second wafer surface be identified, but also latent defects can be identified, thereby enabling comprehensive inspection of wafer surface defects to strictly screen out defective products and improve the yield rate. Furthermore, by locating latent defects from three dimensions—grayscale, energy, and size—step S167 improves the accuracy of latent defect identification.
[0060] In summary, this invention proposes a method for tracing the origin of wafer defects. By employing two scanning methods with different sensitivities to detect defects on the wafer surface, it enables precise tracing of defects, avoiding misleading the source of defects and facilitating the identification of defect improvement directions, thereby accurately improving the quality of the semiconductor structure. Furthermore, the wafer defect tracing and detection method proposed in this invention can comprehensively detect both explicit and implicit defects on the wafer surface, rigorously screening out defective products and improving the yield rate.
[0061] The above description is merely a preferred embodiment of this application and an explanation of the technical principles used. Those skilled in the art should understand that the scope of the invention involved in this application is not limited to the technical solutions formed by a specific combination of the above-mentioned technical features, but should also cover other technical solutions formed by any combination of the above-mentioned technical features or their equivalent features without departing from the inventive concept. For example, technical solutions formed by replacing the above-mentioned features with technical features with similar functions disclosed in this application (but not limited to) each other.
[0062] Apart from the technical features described in the specification, the other technical features are known to those skilled in the art. To highlight the innovative features of this invention, the other technical features will not be described in detail here.
Claims
1. A method for tracing and detecting wafer defects, characterized in that, At least the following steps are included: A first wafer is provided, the surface of which has original defects, including explicit defects and implicit defects; The surface of the first wafer is scanned for the first time with a first sensitivity to obtain a first defect scan result, which includes the explicit defect. The surface of the first wafer is scanned a second time with a second sensitivity to obtain a second defect scan result, which includes the original defect and interference items. The first defect scan result is excluded from the second defect scan result to obtain the third defect scan result; After growing an epitaxial layer on the surface of the first wafer, the epitaxial layer is scanned for the first time with the first sensitivity to obtain a fourth defect scan result. The fourth defect scan result includes the original defect and the epitaxial defect, wherein the first scan of the epitaxial layer and the first scan of the first wafer use the same scanning parameters; and The common defect scan results that are repeated in the third defect scan results and the fourth defect scan results are filtered out, and the latent defect is located based on the common defect scan results.
2. The traceability detection method according to claim 1, characterized in that, The defect scanning results of the first and second scans include a defect distribution location map and feature values for each defect, wherein the feature values include at least one of grayscale, energy, and size.
3. The traceability detection method according to claim 2, characterized in that, After obtaining the common defect scanning results, the latent defects are located according to the common defect distribution map in the common defect scanning results.
4. The traceability detection method according to claim 2, characterized in that, After obtaining the common defect scanning results, defect detection is performed on the second wafer from the same batch as the first wafer, including at least the following steps: The first data sample of the grayscale feature value in the public defect scanning results is statistically analyzed, and the mean x1 and standard deviation S1 of the first data sample are obtained. Data outside the range [x1-3S1, x1+3S1] in the first data sample is excluded to obtain the first correction sample; Data samples within the confidence interval of the first correction sample are selected to obtain a first standard sample. Based on the upper and lower limits of the first standard sample, a grayscale standard for judging the latent defect is determined. Repeat the steps of statistical analysis, elimination, and screening of the energy characteristic values and the size characteristic values to obtain the energy standard and size standard for judging the latent defects; Specifically, after obtaining the grayscale standard, the energy standard, and the size standard, the surface of the second wafer is scanned for the first time to obtain the fifth defect scan result and locate the visible defects on the surface of the second wafer. After locating the visible defects on the surface of the second wafer, locating the hidden defects on the surface of the second wafer includes at least the following steps: The second scan is performed on the surface of the second wafer to obtain the sixth defect scan result; and Based on the grayscale standard, the energy standard, and the size standard, the target defect results in the sixth defect scan results are selected, and based on the target defect results, the latent defects on the surface of the second wafer are located. Specifically, when locating latent defects on the surface of the second wafer, target feature values that simultaneously meet the grayscale standard, the energy standard, and the size standard are selected from the sixth defect scan results. The location of the target defect corresponding to the target feature value is then located in the defect distribution location map of the sixth defect scan results, thus completing the location of latent defects on the surface of the second wafer.
5. The traceability detection method according to claim 1, characterized in that, The first sensitivity is lower than the second sensitivity.
6. The traceability detection method according to claim 1, characterized in that, The method used for the first and second scans is bright-field scanning.
7. The traceability detection method according to claim 6, characterized in that, In the first scan, the pixel size is 0.8μm-2.0μm, and the light transmission ratio of the light source aperture is 50%-70%; in the second scan, the pixel size is 0.2μm-0.7μm, and the light transmission ratio of the light source aperture is 20%-45%.