Semiconductor processing method
By forming insulating layers with different step coverage in semiconductor devices and using plasma deposition technology to control pressure and power, the problems of RC delay and structural deformation in semiconductor devices have been solved, thereby improving device performance.
Patent Information
- Application Number
- CN202611223794.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2020-09-25
- Filing Date
- 2021-09-22
- Publication Date
- 2026-11-24
AI Technical Summary
As semiconductor device manufacturing processes become more refined, the spacing between cells narrows, leading to RC delay and deterioration of device response time caused by parasitic capacitance, which is difficult to effectively solve with existing technologies.
By forming insulating layers with different step coverage on a patterned structure, selective thin film deposition is achieved by controlling the pressure and power of the reaction space using plasma deposition technology, and air gaps are formed to reduce the dielectric constant between electrodes.
It effectively reduces the RC delay between electrodes, prevents structural deformation, and improves the response time and reliability of the device.
Smart Images

Figure CN123165083A_ABST
Abstract
Description
[0001] This application is a divisional application of Chinese invention patent application filed on September 22, 2021 (application number: 202111105605.3, applicant: ASM IP Private Holdings Limited, invention title: semiconductor processing method). Technical Field
[0002] One or more embodiments relate to a substrate processing method, and more specifically, to a substrate processing method for forming air gaps within gaps between patterned structures. Background Technology
[0003] In the manufacturing of semiconductor devices such as DRAM, as the process becomes more refined, the spacing between cells becomes narrower. As a result, resistive-capacitive (RC) delay caused by parasitic capacitance between cells and the resulting degradation in device response time occur.
[0004] To address this issue, a process has been considered to form an air gap between the electrodes as a gap-filling material to reduce the dielectric constant of the buried material in the region between the electrodes. This air-gap process not only prevents RC delay due to the low dielectric constant but also prevents structural deformation problems that may arise due to the shrinkage of the gap-filling dielectric material, such as film rupture and contact misalignment.
[0005] Air gap processes are used in various fields other than DRAM devices to obtain low dielectric constants. For example, Korean Patent Publication No. 10-2010-0037212 discloses a process for forming an air gap in an insulating film disposed on a photodiode. Summary of the Invention
[0006] One or more embodiments include a structure in which a film with a very low step coverage is deposited by utilizing the overhang properties of the film, thereby forming a void in the lower part of the gap structure and crosslinking the film in the upper part of the gap structure.
[0007] One or more embodiments include an optional thin film deposition method that minimizes the thin film deposition rate at the bottom of the gap structure and increases the thin film deposition rate at the top of the gap structure to maximize the effectiveness of the air gap process.
[0008] Additional aspects will be set forth in part in the description which follows, and in part will be obvious from the description, or may be learned by practicing the embodiments shown in this disclosure.
[0009] According to one or more embodiments, a substrate processing method includes: forming a first insulating layer having a first step overlay on a patterned structure including a first protrusion and a second protrusion; and forming a second insulating layer having a second step overlay lower than the first step overlay on the first insulating layer, wherein an air gap can be formed between the first protrusion and the second protrusion by repeatedly forming the second insulating layer.
[0010] According to an example of a substrate processing method, during the formation of a first insulating layer, the pressure in the reaction space is maintained at a first pressure value, and the plasma power is set to a first power value; and during the formation of a second insulating layer, the pressure in the reaction space is maintained at a second pressure value greater than the first pressure value, and the plasma power can be set to a second power value less than the first power value.
[0011] According to another example of the substrate processing method, during the formation of the second insulating layer, the mean free path of the gas supplied to the reaction space is reduced by a second pressure value, causing the gas to concentrate on the upper part of the first and second protrusions.
[0012] According to another example of the substrate processing method, during the formation of the second insulating layer, the amount of ions generated in the reaction space is reduced by the second power value, thereby reducing the ion density, and the ions can be concentrated on the upper part of the first and second protrusions.
[0013] According to another example of the substrate processing method, during the formation of the first insulating layer, the pressure in the reaction space can be maintained at about 5 Torr to about 11 Torr, and during the formation of the second insulating layer, the pressure in the reaction space can be maintained at about 11 Torr to about 15 Torr.
[0014] According to another example of the substrate processing method, during the formation of the first insulating layer, the power of the plasma can be set to about 500W to about 1500W, and during the formation of the second insulating layer, the power of the plasma can be set to about 100W to about 400W.
[0015] According to another example of the substrate processing method, the substrate processing method further includes removing byproducts remaining between the first protrusion and the second protrusion, and the removal of byproducts can be performed while the second insulating layer is being repeatedly formed.
[0016] According to another example of the substrate processing method, during the removal of byproducts, an etching material with etching selectivity for the second insulating layer can be used.
[0017] According to another example of the substrate processing method, forming the first insulating layer may include: forming a first silicon molecular layer on the first and second protrusions by supplying a first silicon-containing source gas; purging the first silicon-containing source gas; supplying a first reactive gas that is reactive with the first silicon molecular layer; and purging the first reactive gas.
[0018] According to another example of the substrate processing method, forming the second insulating layer may include: forming a second silicon molecular layer on the first insulating layer by supplying a second silicon-containing source gas; purging the second silicon-containing source gas; supplying a second reactive gas that is reactive with the second silicon molecular layer; and purging the second reactive gas.
[0019] According to another example of the substrate processing method, the substrate processing method may further include applying a first hydrogen plasma to the first protrusion and the second protrusion before forming the second silicon molecular layer, wherein a hydrogen-rich insulating layer including hydrogen (H) end-capped sites can be formed by the first hydrogen plasma.
[0020] According to another example of the substrate processing method, a hydrogen monolayer can be formed by performing a purging process between applying a first hydrogen plasma and forming a second silicon molecular layer.
[0021] According to another example of the substrate processing method, during the application of the first hydrogen plasma, the pressure in the reaction space can be maintained at about 11 Torr to about 15 Torr, and the power of the plasma can be set at about 100 W to about 400 W. Due to this pressure and power, more hydrogen end-capping sites can be formed in the upper part of the first protrusion and the lower part of the second protrusion than in the lower part.
[0022] According to another example of the substrate processing method, the second silicon-containing source gas is reactive with the hydrogen-sealed end sites, thereby allowing the second silicon molecular layer to be formed in greater quantities on the upper part of the first protrusion than on the lower part of the second protrusion.
[0023] According to another example of the substrate processing method, a second hydrogen plasma is applied during the supply of the second reactive gas, and due to the application of the second hydrogen plasma, the hydrogen content of the second insulating layer may increase, and the etch resistance of the second insulating layer may decrease.
[0024] According to another example of the substrate processing method, the substrate processing method may further include planarizing the upper surface of the second insulating layer, wherein planarization can be performed using isotropic etching of the second insulating layer with reduced etch resistance.
[0025] According to another example of the substrate processing method, the substrate processing method may further include planarizing the upper surface of the second insulating layer, wherein planarization can be performed by a chemical mechanical polishing (CMP) process for the second insulating layer.
[0026] According to one or more embodiments, a substrate processing method includes depositing an insulating layer on a patterned structure having a first protrusion and a second protrusion to form an air gap between the patterned structure and the insulating layer, wherein the air gap can be formed between the first protrusion and the second protrusion by maintaining a pressure in the reaction space such that the mean free path of the gas supplied to the reaction space is reduced, and by setting the power of the plasma such that the amount of ions generated in the reaction space is reduced.
[0027] According to one or more embodiments, a substrate processing method may include: depositing an insulating layer having a step coverage of about 60% or less on a patterned structure by setting the power of a plasma to about 100W to about 400W and applying the power for about 0.1 seconds to about 1 second, thereby forming an air gap between the patterned structure and the insulating layer.
[0028] According to an example of a substrate processing method, when an insulating layer is deposited on a patterned structure, the pressure in the reaction space can be maintained at about 10 Torr to about 15 Torr. Attached Figure Description
[0029] The above and other aspects, features and advantages of certain embodiments of the present disclosure will become more apparent from the following description taken in conjunction with the accompanying drawings, in which: Figure 1 This is a flowchart of a substrate processing method according to an embodiment; Figure 2 This is a flowchart of a substrate processing method according to an embodiment; Figure 3 and 4 This is a view illustrating a substrate processing method according to an embodiment; Figure 5 and 6 This is a view illustrating a substrate processing method according to an embodiment; Figure 7 and 8 As an example of other embodiments Figure 3 and 4 Modified embodiments of the above embodiments; and Figure 9 and 10 This is a view showing the step coverage (S / C) characteristics of the SiN film on the side surface compared to the top surface (side / top) of the patterned structure, according to an embodiment, based on RF voltage and process pressure. Detailed Implementation
[0030] Reference will now be made in detail to embodiments, examples of which are shown in the accompanying drawings, wherein the same reference numerals always refer to the same elements. In this respect, the embodiments may take different forms and should not be construed as limited to the description set forth herein. Therefore, the embodiments are described below only with reference to the accompanying drawings to explain various aspects of this specification. As used herein, the term "and / or" includes any and all combinations of one or more of the associated listed items. Expressions such as "at least one of" preceding a list of elements modify the entire list of elements, rather than a single element in the list.
[0031] In the following description, one or more embodiments will be described more fully with reference to the accompanying drawings.
[0032] In this respect, this embodiment may take different forms and should not be construed as limited to the description set forth herein. Rather, these embodiments are provided so that this disclosure will be thorough and complete, and will fully convey the scope of this disclosure to those skilled in the art.
[0033] The terminology used herein is for the purpose of describing particular embodiments and not for the purpose of limiting this disclosure. As used herein, the singular forms “a,” “an,” and “the” are intended to include the plural forms as well, unless the context clearly indicates otherwise. It will be further understood that the terms “comprising,” “including,” and / or variations thereof as used herein specify the presence of the stated feature, integer, step, process, component, part, and / or group thereof, but do not exclude the presence or addition of one or more other features, integers, steps, processes, components, parts, and / or groups thereof. As used herein, the term “and / or” includes any and all combinations of one or more of the associated listed items.
[0034] It should be understood that although the terms first, second, etc., can be used to describe various components, parts, regions, layers, and / or portions, these components, parts, regions, layers, and / or portions should not be limited by these terms. These terms do not indicate any order, quantity, or importance, but are only used to distinguish the various parts, regions, layers, and / or portions. Therefore, without departing from the teachings of the embodiments, the first component, part, region, layer, or portion discussed below may be referred to as the second component, part, region, layer, or portion.
[0035] In this disclosure, "gas" can include evaporated solids and / or liquids, and can include a single gas or a mixture of gases. In this disclosure, the process gas introduced into the reaction chamber via the nozzle can include precursor gases and additive gases. Precursor gases and additive gases can typically be introduced as a mixed gas or can be introduced separately into the reaction space. Precursor gases can be introduced together with a carrier gas, such as an inert gas. Additive gases can include diluent gases, such as reactant gases and inert gases. Reactant gases and diluent gases can be introduced into the reaction space either mixedly or separately. Precursors can include two or more precursors, and reactant gases can include two or more reactant gases. Precursors can be gases chemisorbed onto the substrate and typically contain metalloid or metallic elements constituting the main structure of the dielectric film matrix, and the reactant gas used for deposition can be a gas that reacts with the precursor chemisorbed onto the substrate when excited to immobilize an atomic layer or monolayer onto the substrate. The term "chemisorbed" can refer to chemically saturated adsorption. Gases other than the process gas, i.e., gases not introduced via the nozzle, can be used to seal the reaction space, and can include sealing gases, such as inert gases. In some embodiments, the term "film" may refer to a layer that extends continuously in a direction perpendicular to the thickness direction, substantially without pinholes covering the entire target or associated surface, or may refer to a layer that simply covers the target or associated surface. In some embodiments, the term "layer" may refer to a structure formed on a surface having any thickness, or a synonym for a film, or a non-film structure. A film or layer may include discrete single films or layers or multiple films or layers having certain properties, and the boundaries between adjacent films or layers may be clear or unclear, and may be defined based on physical, chemical and / or other properties, formation process or sequence, and / or the function or purpose of adjacent films or layers.
[0036] In this disclosure, the expression "containing Si-N bonds" can be described as characterized in that one or more Si-N bonds have a backbone consisting essentially of one or more Si-N bonds and / or have substituents consisting essentially of one or more Si-N bonds. The silicon nitride layer can be a dielectric layer containing Si-N bonds and can include a silicon nitride layer (SiN) and a silicon oxynitride layer (SiON).
[0037] In this disclosure, the term "same material" should be interpreted as meaning that the main components (composition) are the same. For example, when both the first layer and the second layer are silicon nitride layers and are formed of the same material, the first layer may be selected from the group consisting of Si2N, SiN, Si3N4 and Si2N3, and the second layer may also be selected from the group above, but its specific film quality may differ from that of the first layer.
[0038] Furthermore, in this disclosure, any two variables can constitute an operational range of variables, based on an operational range that can be determined based on routine work, and any indicated range can include or exclude terminal locations. Additionally, the value of any indicated variable can refer to an exact value or an approximate value (whether or not they are indicated as “about”), can include equivalents, and can refer to an average, median, representative value, multi-value, etc.
[0039] In disclosures that do not specify conditions and / or structures, those skilled in the art can readily provide such conditions and / or structures based on the disclosure as routine experiments. In all described embodiments, any component used in the embodiments may be replaced by any of its equivalents for intended purposes, including those explicitly, necessary, or substantially described herein; furthermore, this disclosure can be similarly applied to devices and methods.
[0040] In the following description, embodiments of the present disclosure will be illustrated with reference to the accompanying drawings. In the drawings, variations in the illustrated shapes may be expected as a result of, for example, manufacturing techniques and / or tolerances. Therefore, embodiments of the present disclosure should not be construed as limited to specific shapes within the areas shown herein, but may include, for example, shape deviations resulting from the manufacturing process.
[0041] Figure 1 This is a flowchart of a substrate processing method according to an embodiment.
[0042] refer to Figure 1 In operation S100, a substrate with a patterned structure is prepared. For example, the substrate may be loaded into the reaction space of a substrate processing apparatus. The substrate may be a semiconductor substrate and may include, for example, any of silicon, silicon-on-insulator, silicon-on-sapphire, germanium, silicon-germanium, and gallium arsenide.
[0043] The patterned structure is a non-planar structure and can be a stepped structure including an upper surface, a lower surface, and a side surface connecting the upper and lower surfaces. For example, the patterned structure may include a plurality of protrusions defined by a plurality of recesses. The patterned structure can be used to form an active region or to form a gate pattern. For example, the patterned structure may include a first protrusion and a second protrusion, and each of the first and second protrusions may include a gate electrode. When the patterned structure is used to implement flash memory, each of the first and second protrusions may also include a tunnel insulating layer.
[0044] In operation S200, when preparing the substrate, a first insulating layer can be formed on the patterned structure. The first insulating layer can be formed to have a first step coverage. For example, the first step coverage of the first insulating layer can be 90% or higher. That is, operation S200 for forming the first insulating layer can be performed such that a conformal thin film is deposited on the patterned structure.
[0045] The operation S200 of forming the first insulating layer may include supplying a first source gas and supplying a first reaction gas. Furthermore, during the operation S200 of forming the first insulating layer, a thin film deposition process using plasma can be used. For example, at least one of plasma atomic layer deposition (PEALD), plasma chemical vapor deposition (PECVD), pulsed plasma chemical vapor deposition (pulsed PECVD), and cyclic pulsed PECVD can be used.
[0046] For example, the first insulating layer may include silicon oxide, silicon nitride, or a combination thereof. In this case, the operation S200 of forming the first insulating layer may include: forming a first silicon molecular layer on the first and second protrusions by supplying a first silicon-containing source gas on the patterned structure; purging the first silicon-containing source gas; supplying a first reactive gas (e.g., oxygen and / or nitrogen) that is reactive with the first silicon molecular layer; and purging the first reactive gas.
[0047] At least one process parameter can be adjusted to deposit a conformal thin film during the operation S200 of forming the first insulating layer. For example, the gas pressure in the reaction space can be reduced to increase the mean free path of the gas supplied to the patterned structure of the substrate in the reaction space, so that the pressure in the reaction space can be maintained at a first pressure value (e.g., 5 Torr to 11 Torr). Furthermore, the power of the plasma supplied to the reaction space can be increased to increase the amount of ions generated in the reaction space to increase the ion density, so that the plasma power can be set to a first power value (e.g., 500 W to 1500 W).
[0048] In operation S300, after forming a first insulating layer on the patterned structure, a second insulating layer can be formed on the first insulating layer. The second insulating layer can be formed with a second step coverage that is lower than that of the first step coverage. For example, the second step coverage of the second insulating layer can be 60% or lower. By forming a second insulating layer with a low step coverage, a gap can be formed between the first and second insulating layers. Because air is usually contained in the gap, the gap is also called an air gap.
[0049] The operation S300 of forming the second insulating layer may include supplying a second source gas and a second reactant gas. Furthermore, during the operation S300 of forming the second insulating layer, a thin film deposition process using plasma can be used. For example, at least one of PEALD, PECVD, pulsed PECVD, and cyclic pulsed PECVD can be used.
[0050] For example, the second insulating layer may include silicon oxide, silicon nitride, or a combination thereof. In this case, the operation S300 of forming the second insulating layer may include: forming a second silicon molecular layer on the first insulating layer by supplying a second silicon-containing source gas on a patterned structure; purging the second silicon-containing source gas; supplying a second reactive gas (e.g., oxygen and / or nitrogen) that is reactive with the second silicon molecular layer; and purging the second reactive gas.
[0051] At least one process parameter can be adjusted to deposit a lower-step cover film during the operation S300 of forming the second insulating layer. For example, the gas pressure in the reaction space can be increased, thereby reducing the mean free path of the gas supplied to the patterned structure of the substrate in the reaction space, so that the pressure in the reaction space can be maintained at a second pressure value (e.g., 11 Torr to 15 Torr). Furthermore, the power of the plasma supplied to the reaction space can be reduced, thereby reducing the amount of ions generated in the reaction space to lower the ion density; therefore, the plasma power can be set to a second power value (e.g., 100 W to 400 W).
[0052] In other words, during the operation S300 of forming the second insulating layer, the pressure in the reaction space can be maintained at a second pressure value greater than the first pressure value during the formation of the first insulating layer, and the plasma power can be set to a second power value less than the first power value during the formation of the insulating layer. Due to this relatively high pressure, the gas concentrates on the upper part of the first and second protrusions due to the low mean free path, and the ion density decreases due to the low power, causing ions to concentrate on the upper part of the first and second protrusions. Therefore, a second insulating layer with a low step coverage can be formed on the first insulating layer.
[0053] In operation S400, after the second insulating layer is formed, it can be determined whether an air gap is formed between the first and second insulating layers and between the first and second protrusions. If no air gap is formed, operation S300 of forming the second insulating layer is repeated. The formation of the second insulating layer can be repeated a certain number of times until an air gap is formed. That is, by repeating operation S300 of forming the second insulating layer, an air gap can be formed between the first and second protrusions.
[0054] The first and second protrusions of the patterned structure can be arranged apart from each other with narrow gaps in the nanometer unit (e.g., 10 nm gaps). When the second insulating layer covering the lower step is deposited on the patterned structure due to this narrow-gap arrangement, the second insulating layer can be formed in large quantities in the upper part of the region between the first and second protrusions, while the second insulating layer can be formed in relatively small quantities in the lower part of the region between the first and second protrusions.
[0055] Therefore, by repeating the operation S300 of forming the second insulating layer, a structure (crosslinking) in which the deposited second insulating layers are interconnected is formed in the upper part of the region between the first and second protrusions, while a void is formed in the lower part of the region between the first and second protrusions. By maintaining the pressure in the reaction space to reduce the mean free path of the gas supplied to the reaction space and / or by setting the plasma power to reduce the amount of ions generated in the reaction space, an air gap formed by the void inside the gap between the protrusions can be formed.
[0056] Subsequently, when an air gap is determined to form, operation S500, planarizing the upper surface of the second insulating layer, can be performed. This planarization can be performed by using a chemical mechanical polishing (CMP) process on the second insulating layer. In another embodiment, isotropic etching can be used to perform planarization. In the case of isotropic etching, because the planarization rate is lower than that of CMP, the etch resistance of the second insulating layer can be additionally reduced to increase the speed. This will... Figure 2 A more detailed description is provided below.
[0057] although Figure 1 Not shown, but in some embodiments, the substrate processing method may further include removing byproducts remaining between the first and second protrusions. In this case, the first insulating layer may perform the function of protecting the patterned structure while removing byproducts. The removal of byproducts will... Figure 2 A more detailed description is provided below.
[0058] Figure 2 This is a view of a substrate processing method according to an embodiment. The substrate processing method according to the embodiment may be a variation of the substrate processing method according to the above embodiment. In the following, the embodiments will not be described again.
[0059] refer to Figure 2 The substrate processing method may include an operation S200 of forming a first insulating layer, an operation S300 of forming a second insulating layer, an operation S400 of determining whether an air gap is formed, and an operation S450 of removing by-products.
[0060] As described above, the operation S200 of forming the first insulating layer can be performed using a thin-film deposition process employing plasma. For example, the first insulating layer can be silicon nitride, and in this case, a silicon-containing gas can be used as the first silicon source gas. Furthermore, a nitrogen-containing gas can be used as the first reactant gas. In another example, the first insulating layer can be silicon oxide, and in this case, a silicon-containing gas can be used as the first silicon source gas. Furthermore, an oxygen-containing gas can be used as the first reactant gas.
[0061] To form the first insulating layer, a first cycle can be performed multiple times, including operation S210 of forming the first silicon molecular layer by supplying a first silicon source gas and operation S220 of supplying a first reactant gas under a first plasma atmosphere. In operations S230 and S240, this first cycle can be repeated a certain number of times (i.e., until X becomes M), and then operation S300 of forming the second insulating layer can be performed.
[0062] Similar to operation S200, which forms the first insulating layer, operation S300, which forms the second insulating layer, may include a second cycle comprising operation S320, which forms the second silicon molecular layer by supplying a second silicon source gas, and operation S330, which supplies a second reactant gas under a second plasma atmosphere. The second silicon source gas and the second reactant gas may be the same as or different from the first silicon source gas and the first reactant gas, respectively. The second insulating layer may be the same as the first insulating layer. For example, when the first insulating layer is silicon nitride, the second insulating layer may also be silicon nitride.
[0063] In some embodiments, prior to the operation S320 of supplying a second silicon source gas to form a second silicon molecular layer, an operation S310 of applying a first hydrogen plasma to the first and second protrusions may be performed. By applying the first hydrogen plasma, hydrogen (H) end-capping sites can be formed on the first insulating layer of the first and second protrusions. That is, by applying the first hydrogen plasma, the first insulating layer (and the lower second insulating layer formed in the previous second cycle) can be transformed into a hydrogen-rich insulating layer.
[0064] During operation S310, when the first hydrogen plasma is applied, the process conditions can be adjusted such that more hydrogen ions are formed in the upper part of the first and second protrusions than in the lower part of the first and second protrusions. For example, the pressure in the reaction space can be maintained at 11 Torr to 15 Torr, thereby reducing the mean free path of the hydrogen gas supplied to the reaction space, and the plasma power can be set to 100 W to 400 W, thereby reducing the amount of hydrogen ions generated in the reaction space. Due to the aforementioned pressure and power conditions, more H-terminal sites can be formed in the upper part of the first and second protrusions compared to the lower part of the first and second protrusions.
[0065] After the operation S310 of applying the first hydrogen plasma, the operation S320 of supplying the second silicon-containing source gas can be performed. Because the H-terminal sites serve as bonding sites for reaction with the second silicon-containing source gas, the second silicon molecular layer can be formed in greater quantities on the upper part of the first and second protrusions than on the lower part of the first and second protrusions. In an alternative embodiment, the operation S310 of applying the first hydrogen plasma and the operation S320 of supplying the second silicon-containing source gas can be performed simultaneously (see [link to documentation]). Figure 7 ).
[0066] In alternative embodiments, although Figure 2The process is not shown, but purging (not shown) can be performed between operation S310, which applies the first hydrogen plasma, and operation S320, which supplies the second silicon-containing source gas. A hydrogen monolayer can be formed by purging on the first insulating layer and the lower second insulating layer formed by the previous second cycle (e.g., cycle Y-1, if a new second insulating layer is formed during cycle Y). Furthermore, hydrogen gas remaining inside the gap can be removed by purging.
[0067] After operation S320, which involves supplying a second silicon source gas to form a second silicon molecular layer, operation S330, which involves supplying a second reactive gas, is performed. In some embodiments, a second hydrogen plasma may be applied during operation S330, which involves supplying the second reactive gas. Due to the application of the second hydrogen plasma, the hydrogen content of the second insulating layer may increase, resulting in a possible decrease in the etch resistance of the second insulating layer. The second insulating layer with reduced etch resistance may be adapted to be planarized by isotropic etching, such as wet etching.
[0068] To form the second insulating layer, a second cycle can be performed multiple times, including operation S320 of forming the second silicon molecular layer by supplying a second silicon source gas and operation S330 of supplying a second reactant gas under a second plasma atmosphere. In operations S340 and S350, this second cycle can be repeated a certain number of times (i.e., until Y becomes N), after which operation S400 can be performed to determine whether an air gap has been formed.
[0069] The operations S200 for forming the first insulating layer and S300 for forming the second insulating layer can be common because an insulating layer containing Si-N bonds is formed. In this case, in some embodiments, operations S200 for forming the first insulating layer and S300 for forming the second insulating layer can be performed in situ in the same reactor. However, the detailed process parameters for forming the insulating layer containing Si-N bonds may differ. For example, as described above, the pressure of the reaction space and the power of the plasma can be set differently to form insulating layers with different step coverage.
[0070] As another example, in some embodiments, different types of gases can be supplied during operations S200 (forming the first insulating layer) and S300 (forming the second insulating layer). More specifically, during operation S300 (forming the second insulating layer), a material with a relatively high hydrogen content can be used as the second silicon source gas. Furthermore, a nitrogen source with a high hydrogen content or containing hydrogen can be used as the second reactant gas. In other words, the hydrogen content of the second silicon source gas and the second reactant gas used in operation S300 (forming the second insulating layer) can be higher than the hydrogen content of the first silicon source gas and the first reactant gas used in operation S200 (forming the first insulating layer).
[0071] Due to the difference in hydrogen content, a first insulating layer (i.e., a first silicon nitride layer) with a first step coverage and a second insulating layer (i.e., a second silicon nitride layer) with a second step coverage below the first step can have different densities and wet etch rates (WER). As a specific example, by supplying a second reactive gas including NH3 contained in the second reactive gas during operation S300 to form the second insulating layer, a larger amount of hydrogen can be incorporated into the second insulating layer. Therefore, the second insulating layer can have a relatively small number of Si-N bonds, and thus, the second insulating layer can have high WER and low etch resistance.
[0072] Return to reference Figure 2 The operation S400, which determines whether an air gap has been formed, is executed. This operation may include determining whether the air gap forming cycle, which includes the operation S300 of forming the second insulating layer and the operation S450 of removing by-products, has been executed a certain number of times. In other words, the air gap forming cycle, including the operation S300 of forming the second insulating layer and the operation S450 of removing by-products, may be repeated a certain number of times, after which planarization may be performed.
[0073] When no air gap is formed under the second insulating layer (i.e., when the second insulating layers on the first protrusion and the second insulating layers on the second protrusion are not connected to each other), the operation S300 of forming the second insulating layer is performed again. In an alternative embodiment, before performing the operation S300 of forming the second insulating layer, the operation S450 of removing byproducts remaining between the first and second protrusions of the patterned structure can be performed. That is, the removal of byproducts can be performed while repeating the operation S300 of forming the second insulating layer.
[0074] Due to the narrow gap between the first and second protrusions and the deposition of a second insulating layer with a low-step cover, byproducts may remain between the first and second protrusions. For example, at least one of the second silicon source gas, second silicon molecules separated from or suspended and bonded to the second silicon molecular layer formed on the inner surface of the gap between the first and second protrusions, molecular fragments containing the second silicon, and the second reactant gas may remain between the first and second protrusions, and this byproduct may not be removed even after purging following the supply of the second reactant gas.
[0075] Therefore, isotropic etching can be used to remove byproducts. For example, wet etching can be performed during byproduct removal using an etchant that is selective for etching the second insulating layer. By isotropic etching, such as wet etching, byproducts remaining inside the gaps of the patterned structure after purging can be removed.
[0076] In operation S400, which determines whether an air gap is formed, if an air gap is formed under the second insulating layer (i.e., when the second insulating layers on the first protrusion and the second insulating layers on the second protrusion are connected to each other), operation S500, which plans the second insulating layer, can be performed as a subsequent operation. Planarization can be performed using CMP on the second insulating layer. In some other embodiments, planarization can be performed using isotropic etching of the second insulating layer with reduced etch resistance (i.e., increased WER). As described above, in operation S330, a second hydrogen plasma can be applied to form a second insulating layer with reduced etch resistance.
[0077] Despite Figure 1 and 2 In some embodiments, the second insulating layer is formed after the first insulating layer is formed; however, in other embodiments, the second insulating layer may be formed on the patterned structure without forming the first insulating layer. That is, an insulating layer with low step coverage (e.g., 60% or less step coverage) may be deposited on the patterned structure having first and second protrusions to create an air gap between the patterned structure and the insulating layer.
[0078] In this case, as described above, the plasma power can be set to a relatively low level (e.g., 100W to 400W) to form an insulating layer with a low-step coverage, and this power can be applied for a short time (0.1 seconds to 1 second). Furthermore, when the insulating layer is deposited on the patterned structure, the pressure in the reaction space can be kept relatively high (e.g., 10 Torr to 15 Torr), thereby reducing the mean free path of the gas supplied to the reaction space.
[0079] As described above, according to the embodiments, air gaps can be formed in the gaps between patterned structures by performing selective deposition on the patterned structures. More specifically, selective deposition on the patterned structures and the formation of air gaps within the gaps can be more easily achieved by adjusting the amount of process pressure and applied RF power.
[0080] Figure 3 and 4 This is a view of a substrate processing method according to an embodiment. The substrate processing method according to the embodiment may be a variation of the substrate processing method according to the above embodiment. In the following, the embodiments will not be described again.
[0081] This disclosure presents a processing method for forming air gaps in gaps. More specifically, a two-step plasma process is proposed as a method for selectively controlling the thin film deposition rate between gap structures.
[0082] Plasma ion flux distribution based on interstitial structure depth is highly dependent on process pressure. When the process pressure is sufficiently low, the number of collisions between ions and gas is relatively small, resulting in a longer mean free path (MFP) for the ions, which are distributed to the lower part of the interstitial structure. However, at high process pressures, the number of collisions between ions and gas is relatively high, resulting in a shorter MFP for the ions, which are concentrated primarily in the upper part of the interstitial structure. Furthermore, this phenomenon is more pronounced with the applied RF power. In other words, when high RF power is applied, a large amount of ions are generated, resulting in a high ion density, and thus ions may reach the bottom of the interstitial structure. Conversely, when low RF power is applied, a relatively small amount of ions are generated, resulting in a low ion density, and thus ions are mainly distributed in the upper part of the interstitial structure. Therefore, selectively adjusting the membrane quality in the upper part of the interstitial structure requires an appropriate combination of process pressure and applied RF power. For example, under low process pressure and high RF power, the membrane forms on the inner surface of the interstitial structure, while under high process pressure and low applied RF power, the membrane mainly forms on the upper surface of the interstitial structure.
[0083] refer to Figure 3 The detailed description of each operation is as follows.
[0084] 1. First Step (Step 1): Depositing a thin film 1 on the patterned structure including the gaps. In this embodiment, a SiN film is uniformly deposited. Deposition is performed by plasma atomic layer deposition (PEALD) or pulsed PECVD, or a combination thereof, supplying a silicon-containing source gas and an activated nitrogen-containing reactive gas. In this step, high RF power is applied at a low process pressure to supply the activated nitrogen reactive gas 2 (N2 plasma flux) to the inner surface and bottom of the gap structure. The film deposited in this step serves as a protective film to protect the patterned structure from the etch material during the gap etching performed between steps three and four, which will be described later.
[0085] 2. Second step (Step 2): Si source gas is supplied to the SiN film deposited on the patterned structure to form a silicon (Si) source molecular layer. In the second step, a Si source monolayer can be formed by supplying Si source gas and then further adding a purging step.
[0086] 3. Third step (step 3): A SiN film is formed by providing an activated nitrogen-containing reactive gas to a patterned structure in which a Si source molecular layer is formed. This step is performed at low RF power and high process pressure, such that the activated nitrogen reactive gas 2' flows primarily in the upper part of the patterned structure, thus selectively depositing the SiN film on the upper part of the patterned structure compared to the interior of the patterned structure. Steps 2 and 3 are repeated multiple times. In another embodiment, a purging step is added between steps 2 and 3 and after step 3, thereby selectively depositing the SiN film on the upper part of the patterned structure by plasma atomic layer deposition.
[0087] 4. Fourth step (step 4): By repeating steps 2 and 3, the SiN films formed on the upper part of the patterned structure are connected to each other to form voids 3 therein. After this step, a film 4 of a certain thickness can be further removed from the patterned structure in a CMP step.
[0088] When steps two and three are repeated by performing an additional etching process between steps three and four, the reaction byproducts accumulated in the gap space 3 between the patterned structures can be removed. Because the SiN film (i.e., the SiN film as a protective film) is uniformly formed on the gap surface in the first step, damage to the patterned structure by the etching material can be prevented.
[0089] refer to Figure 4 Steps T1 to T4 correspond to Figure 3 The first step, and represents the step of uniformly depositing a SiN film on a patterned structure. This step is repeated M times. Steps T5 to T8 correspond to... Figure 3 The second and third steps describe the selective deposition of a SiN film on top of the patterned structure. This step is repeated N times. Figure 4 As shown, Figure 3 The first step is called the conformal deposition step. Figure 3 The second and third steps are called selective deposition steps. The conformal deposition and selective deposition steps can be performed in one reactor in an in-situ continuous process or in another reactor in an ex-situ process. During an ex-situ process, after performing a conformal deposition step in one reactor, the substrate can be transferred to another reactor to perform a selective deposition step.
[0090] according to Figure 3 and 4 The disclosed embodiments have the technical effect of promoting selective deposition on patterned structures by controlling the amount of applied RF power and process pressure.
[0091] Figure 5 and 6This is a view of a substrate processing method according to an embodiment; the substrate processing method according to the embodiment may be a variation of the substrate processing method according to the above embodiment. In the following, the embodiments will not be described again.
[0092] because Figure 5 The first step shown corresponds to Figure 3 The first step is not described in this article. Figure 5 The second to fifth steps are described in detail below.
[0093] 1. Second Step (Step 2): In the second step, after forming a SiN thin film on the gap surface in the first step, hydrogen plasma is applied. In this step, a hydrogen-rich (H) film is formed on the upper part of the patterned structure by performing the process under a low RF applied voltage and a high process pressure, primarily forming a hydrogen plasma flux of 13 on the upper part of the patterned structure. The H-rich film acts as H-termining sites, and the H-termining sites are highly reactive with the silicon-containing source gas, thus becoming binding sites. In another embodiment, a hydrogen monolayer can be formed by adding a purging step after the second step.
[0094] 2. Third step (Step 3): Supplying silicon source gas. As mentioned in Step 2, the silicon source gas chemically reacts with the H-terminal sites formed in the upper part of the patterned structure to form a silicon layer. In another embodiment, a Si monolayer can be formed by adding a purging step after Step 3.
[0095] 3. Fourth step (step 4): A SiN film is formed by chemically reacting activated nitrogen reactive gas with the silicon layer on top of the patterned structure. In this step, the SiN film is formed on top of the patterned structure by applying a low RF voltage and a high process pressure, primarily forming a nitrogen plasma flux 2' on top of the patterned structure.
[0096] 4. Fifth step (step 5): Steps 2, 3, and 4 are repeated multiple times. Through repetition, the SiN films formed on the top of the patterned structure are interconnected to form voids 3 therein. After this step, a film 4 of a certain thickness is formed. Figure 3 The membrane 4) in the fourth step can be removed from the patterned structure in the CMP step.
[0097] 5. Additional Step: When repeating steps three and four, an additional etching process is performed between steps four and five to remove reaction byproducts deposited in the interstitial space 3. Because the SiN film is uniformly formed on the interstitial surface in the first step, damage to the patterned structure by the etching material can be prevented. Furthermore, after step five, a portion of the film deposited on the upper part of the interstitial space can be removed using a CMP process (see [link to CMP process]). Figure 3 Step 4 in the process.
[0098] Figure 6 It shows Figure 5 The process sequence of the embodiment.
[0099] refer to Figure 6 Steps T1 to T4 correspond to Figure 5 The first step, and represents the step of uniformly depositing a SiN film on a patterned structure. This step is repeated M times. Steps T5 to T9 correspond to... Figure 5 The second to fourth steps describe the formation of H-rich and Si-rich regions on the upper part of the patterned structure and the selective deposition of SiN films in the corresponding regions. This step is repeated N times. Figure 6 As shown, Figure 5 The first step is called the conformal deposition step. Figure 5 The second to fourth steps are called selective deposition steps. Conformal deposition and selective deposition steps can be performed in one reactor in an in-situ continuous process, or in another reactor in an ex-situ process. During an ex-situ process, after performing a conformal deposition step in one reactor, the substrate can be transferred to another reactor to perform a selective deposition step. Figure 6 In the selective deposition step, a hydrogen monolayer can be formed on the upper part of the patterned structure by adding a purging step T6 after the hydrogen supply step T5. Furthermore, a Si monolayer can be formed on the upper part of the patterned structure by adding a purging step T8 after the silicon-containing gas supply step T7.
[0100] Simultaneously, during step T5, the nitrogen supply can be stopped. Nitrogen can be continuously supplied during the conformal deposition and selective deposition steps as a reactive purge gas (see [link to relevant documentation]). Figure 4 In other words, nitrogen can be used as a purge gas when no plasma is applied, and it can be activated when plasma is applied for the formation of a nitride film. Conversely, in Figure 6 In one embodiment, the supply of a reactive purge gas, such as nitrogen, is stopped during step T5, and by stopping the supply of the reactive purge gas, hydrogen can more easily reach the patterned structure. Therefore, there is a technical effect that further promotes the formation of H-terminal sites on the patterned structure that react with the silicon source.
[0101] according to Figures 5 to 6 The disclosed technical effect of the embodiments can promote selective deposition in the upper part of the patterned structure by controlling the process pressure and the applied RF power, and by forming an H-rich layer that is highly reactive with the silicon source gas in the upper part of the patterned structure. Figure 7 and 8 As an example of other embodiments Figure 5 and 6 Modified embodiments of the above embodiments.
[0102] refer to Figure 7 In an alternative embodiment, in step T5, the silicon source and hydrogen mixture can be supplied and activated together. That is, they can be performed simultaneously. Figure 5 The second step involves applying hydrogen plasma, and the third step involves supplying a silicon source. In the above... Figure 6 In the embodiments, when applying ( Figure 6 After the T5 hydrogen plasma, the silicon source is supplied ( Figure 6 (T7 in the middle), but Figure 7 In this embodiment, both a silicon source and hydrogen plasma can be supplied simultaneously. Therefore, there is a technical advantage that can further improve substrate processing speed and yield.
[0103] refer to Figure 8 In an alternative embodiment, in step T7, a mixed gas of nitrogen and hydrogen is supplied and activated together in the selective deposition step. Hydrogen is a process variable affecting the wet etch resistance of the film. When the hydrogen content is high, the film's etch resistance decreases, and when the hydrogen content is low, the film's etch resistance increases. Therefore, this technique has the effect of controlling the etch resistance of the SiN film deposited on the top of the patterned structure and improving its adaptability to subsequent processes. For example, when in Figure 5 When removing the patterned upper structure after the fourth step, the etching process can be performed more precisely by wet etching instead of CMP.
[0104] In another embodiment, when in Figure 5 When the etching process is performed between the fourth and fifth steps to remove the reaction byproducts accumulated in the gap space 3, there is a technical effect of promoting the removal of reaction byproducts by controlling the etching of the film in the upper part of the patterned structure.
[0105] Table 1 below shows the results based on Figures 3 to 6 The test conditions for the embodiments.
[0106] Table 1
[0107] In one embodiment, the Si-containing gas as the first reactant gas may include at least one of the following: TSA, (SiH3)3N; DSO, (SiH3)2; DSMA, (SiH3)2NMe; DSEA, (SiH3)2NEt; DSIPA, (SiH3)2N(iPr); DSTBA, (SiH3)2N(tBu); DEAS, SiH3NEt2; DTBAS, SiH3N(tBu)2; BDEAS, SiH2(NEt2)2; BDMAS, SiH2(NMe2)2; BTBAS, SiH2(NHtBu)2; BITS, SiH2(NHSiMe3)2; DIPAS, SiH3N(iPr)2; TEOS, Si(OEt)4; SiCl4; HCD, Si2Cl6; 3DMAS, SiH(N(Me)2)3; BEMAS, SiH2[N(Et)(Me)]2; AHEAD, Si2(NHEt)6; TEAS, Si(NHEt)4; Si3H8; DCS, SiH2Cl2; SiHI3 and SiH2I2, or derivatives thereof or mixtures thereof. The nitrogen-containing gas as the second reactant may include at least one of the following: N2, NH3, NH4. + N2O or NO2 or mixtures thereof.
[0108] Figure 9 and 10 This is a view showing the step coverage (S / C) characteristics of the SiN film on the side surface compared to the top surface (side / top) of the patterned structure, according to an embodiment, based on RF voltage and process pressure.
[0109] like Figure 9 As shown, it can be seen that the lower the applied RF power and the shorter the application time, the lower the S / C ratio of the SiN film on the patterned structure. Furthermore, as... Figure 10 As shown, the lower the applied RF power and the higher the process pressure, the lower the S / C ratio of the SiN film on the patterned structure. This means that when the applied RF power is small and the process pressure is high, the deposition on the inner surface of the gap decreases, thus making it easier to form an air gap structure.
[0110] It should be understood that the embodiments described herein are to be considered descriptive only and not for limiting purposes. The description of features or aspects within each embodiment should generally be considered applicable to other similar features or aspects in other embodiments. While one or more embodiments have been described with reference to the accompanying drawings, those skilled in the art will understand that various changes in form and detail may be made without departing from the spirit and scope of this disclosure as defined by the appended claims.
Claims
1. A substrate processing method, comprising: An insulating layer is deposited on a patterned structure having a first protrusion and a second protrusion to form an air gap between the patterned structure and the insulating layer. The pressure in the reaction space is maintained to reduce the mean free path of the gas supplied to the reaction space, and the power of the plasma is set to reduce the amount of ions generated in the reaction space, thus forming an air gap between the first protrusion and the second protrusion.
2. The substrate processing method according to claim 1, wherein, When the insulating layer is deposited on the patterned structure, the pressure in the reaction space is maintained at about 10 Torr to about 15 Torr.
3. The substrate processing method according to claim 1, further comprising forming a first insulating layer, wherein a second insulating layer is formed on the first insulating layer.
4. The substrate processing method according to claim 3, wherein the step coverage of the second insulating layer is lower than that of the first insulating layer.
5. The substrate processing method according to claim 3, wherein the hydrogen content of the second silicon-containing source gas and the second reactive gas used for depositing the second insulating layer is higher than the hydrogen content of the first silicon-containing source gas and the first reactive gas used for forming the first insulating layer.
6. The substrate processing method according to claim 1, comprising forming an air gap between the first protrusion and the second protrusion by depositing an insulating layer.
7. The substrate processing method according to claim 1, comprising removing byproducts between the first protrusion and the second protrusion.
8. The substrate processing method according to claim 7, wherein, Byproducts are removed while depositing the insulating layer.
9. The substrate processing method according to claim 7, wherein, Byproducts include at least one of the following: source gas, molecules separated from or suspended and bonded to the inner surface of the gap formed between the first and second protrusions, molecular fragments containing source gas, or reactant gas.
10. The substrate processing method according to claim 7, wherein, During the removal of byproducts, an etching material with etching selectivity for the second insulating layer is used.
11. The substrate processing method according to claim 7, wherein, Forming the first insulating layer includes: A first silicon molecular layer is formed on the first and second protrusions by supplying a first silicon-containing source gas; Purge the first silicon-containing source gas; Supply a first reactive gas that is reactive with the first silicon molecular layer; and Purge the first reaction gas.
12. The substrate processing method according to claim 11, wherein, Depositing the second insulating layer includes: A second silicon molecular layer is formed on the first insulating layer by supplying a second silicon-containing source gas; Purge the second silicon-containing source gas; Supply a second reactive gas that is reactive with the second silicon molecular layer; and Purge the second reaction gas.
13. The substrate processing method according to claim 1, further comprising: Before depositing the insulating layer, a first hydrogen plasma is applied to the first and second protrusions.
14. The substrate processing method according to claim 13, wherein, A hydrogen-rich insulating layer, including hydrogen-sealed sites, is formed using a first hydrogen plasma.
15. The substrate processing method according to claim 14, wherein, A hydrogen monolayer is formed by performing a purging step between the application of a first hydrogen plasma and the formation of a second silicon molecular layer.
16. The substrate processing method according to claim 14, wherein, During the application of the first hydrogen plasma, the pressure in the reaction space is maintained between 11 Torr and 15 Torr.
17. The substrate processing method according to claim 16, wherein, During the application of the first hydrogen plasma, the plasma power is set between approximately 100 W and approximately 400 W.
18. A substrate processing method, comprising: An air gap is formed between the patterned structure and the insulating layer by setting the plasma power to 100W to 400W and applying the power for 0.1 seconds to 1 second to deposit an insulating layer with 60% or less step coverage on the patterned structure.
19. The substrate processing method according to claim 18, wherein, When the insulating layer is deposited on the patterned structure, the pressure in the reaction space is maintained at 10 to 15 Torr.
20. The substrate processing method according to claim 18, wherein, Byproducts are removed while air gaps are formed.
Citation Information
Patent Citations
Semiconductor device and fabricating method thereof
KR1020100037212A