金属互连结构及其形成方法
By introducing a first barrier layer with different barrier capabilities into the copper interconnect structure and doping barrier atoms in the interface region to form a compound, the copper diffusion problem is solved, and the electromigration lifetime and device stability are improved.
Patent Information
- Application Number
- CN202510653971.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-05-20
- Publication Date
- 2026-11-24
AI Technical Summary
The problem of copper diffusion in existing copper interconnect processes has not been effectively solved, affecting the reliability and performance of interconnect structures.
A first barrier layer with different barrier capabilities is introduced between the dielectric layer and the copper conductive layer. The first and second barrier atoms are doped in the interface region to form a compound to enhance the barrier effect. The diffusion capability of the barrier layer is improved by combining the annealing treatment.
This improves the electromigration lifetime of the metal interconnect structure, reduces the increase in contact resistance, and enhances the stability of device performance.
Smart Images

Figure CN123165089A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of semiconductor manufacturing, and in particular to a metal interconnect structure and a method for forming the same. Background Technology
[0002] Metal interconnect structures are indispensable in semiconductor devices, used to interconnect active regions, transistors, or different metal lines to achieve signal transmission and control. Therefore, the formation of metal interconnect structures during semiconductor manufacturing has a significant impact on the performance of semiconductor devices and the cost of semiconductor manufacturing.
[0003] The increased device density and reduced feature linewidth in very large-scale integrated circuits (VLSI) lead to a continuous increase in RC coupling between interconnects, resulting in signal transmission delay, increased power consumption, and increased noise. To address these issues, copper has replaced aluminum as the mainstream interconnect metal material in VLSI manufacturing. Replacing traditional SiO2 interlayer insulating dielectrics with low-k and ultra-low-k dielectric materials has also become a viable option.
[0004] Because etching copper is extremely difficult, copper interconnects are fabricated using embedded processes. These embedded processes primarily include the deposition of interlayer insulating media, etching of vias and trenches within the interlayer insulating media, deposition of metal barrier layers and seed layers, copper electroplating, and chemical mechanical polishing. In copper interconnects, reliability is a critical issue, primarily involving electromigration, stress migration, and breakdown characteristics. A key factor affecting reliability is the diffusion of copper impurities into the low-dielectric-constant interlayer insulating media.
[0005] Therefore, the copper diffusion problem, which is common in copper interconnect processes, still needs further improvement. Summary of the Invention
[0006] The technical problem solved by this invention is to provide a metal interconnect structure and a method for forming the same, so as to improve the performance of the metal interconnect structure.
[0007] To address the aforementioned technical problems, the present invention provides a metal interconnect structure, comprising: a substrate, the substrate including a base and a dielectric layer located on the surface of the base, the dielectric layer having an opening that exposes the surface of the base; a first barrier layer located on the sidewalls and bottom of the opening, a seed layer located on the surface of the first barrier layer, and a first conductive layer located on the surface of the seed layer, wherein the region of the first barrier layer adjacent to the dielectric layer has a first blocking capability for the diffusion of metal ions within the first conductive layer, and the first blocking capability is greater than the blocking capability of other regions of the first barrier layer for the diffusion of metal ions within the first conductive layer.
[0008] Optionally, the first barrier layer includes an interface region and a main region, with the region adjacent to the dielectric layer being the interface region and the other regions of the first barrier layer being the main region; the interface region is doped with first barrier atoms.
[0009] Optionally, the thickness of the interface region ranges from 1 nm to 2 nm; the thickness of the first barrier layer ranges from 3 nm to 10 nm.
[0010] Optionally, the first barrier atom includes oxygen atoms; the proportion of the first barrier atom in the interface region ranges from 10 at% to 20 at%; the material of the first barrier layer includes titanium nitride or titanium nitride.
[0011] Optionally, the interface region is further doped with a second barrier atom, and the first barrier atom and the second barrier atom are combined to form a compound; the second barrier atom includes manganese atoms or aluminum atoms; the proportion of the second barrier atom in the interface region ranges from 1 at% to 5 at%.
[0012] Optionally, it may also include: an adhesive layer located between the first barrier layer and the seed crystal layer; the material of the adhesive layer includes one or more of tank, titanium and cobalt.
[0013] Optionally, it further includes: a second barrier layer located on top of the first conductive layer; the material of the second barrier layer includes a cobalt metal compound, wherein the cobalt metal compound includes a copper-cobalt compound.
[0014] Optionally, the top of the first conductive layer is lower than or flush with the top surface of the dielectric layer.
[0015] Optionally, the material of the dielectric layer includes a low-K dielectric material, which includes one or more of silicon carbonitride, silicon carbon oxycarbide, and silicon hydroxide; the oxygen content in the dielectric layer is less than or equal to 10 at.
[0016] Accordingly, the technical solution of the present invention also provides a method for forming a metal interconnect structure, comprising: providing a substrate, the substrate including a base and a dielectric layer located on the surface of the base, the dielectric layer having an opening, the bottom of the opening exposing the surface of the base; forming a barrier material layer on the sidewalls and bottom of the opening and on the surface of the dielectric layer; forming a seed material layer on the surface of the barrier material layer; forming a metal material layer on the surface of the seed material layer, wherein the region adjacent to the barrier material layer and the dielectric layer has an initial first barrier capability for the diffusion of metal ions within the metal material layer, the initial first barrier capability being greater than the barrier capability of other regions of the barrier material layer for the diffusion of metal ions within the metal material layer; planarizing the metal material layer, the seed material layer, and the barrier material layer until the surface of the dielectric layer is exposed; forming a first conductive layer with the metal material layer; forming a seed layer with the seed material layer; forming a first barrier layer with the barrier material layer, wherein the region adjacent to the first barrier layer and the dielectric layer has a first barrier capability for the diffusion of metal ions within the first conductive layer, the first barrier capability being greater than the barrier capability of other regions of the first barrier layer for the diffusion of metal ions within the first conductive layer.
[0017] Optionally, the barrier material layer includes an initial interface region and an initial host region, with the region adjacent to the dielectric layer being the initial interface region and other regions of the barrier material layer being the initial host region; the initial interface region is doped with first barrier atoms; the first barrier layer includes an interface region and a host region, with the initial interface forming the interface region and the initial host region forming the host region.
[0018] Optionally, the method for forming the barrier material layer includes: placing the substrate in a barrier layer deposition chamber; introducing a first reactive gas and a second reactive gas into the barrier layer deposition chamber, and forming the initial interface region using a first physical vapor deposition process, wherein the second reactive gas is used to provide the first barrier atoms, and the ratio of the flow rate of the first reactive gas to the flow rate of the second reactive gas is in the range of 1% to 5%; stopping the introduction of the second reactive gas while maintaining the introduction of the first reactive gas, and forming the initial host region on the initial interface region using a second physical vapor deposition process.
[0019] Optionally, the process parameters of the first physical vapor deposition process include: the target material includes tank or titanium, the first reaction gas includes nitrogen, the second reaction gas includes oxygen, the flow rate of nitrogen is in the range of 10 sccm to 30 sccm, the flow rate of oxygen is in the range of 0.1 sccm to 1.4 sccm, the DC power supply power is in the range of 5000W to 20000W, and the process time is in the range of 2s to 4s.
[0020] Optionally, the process parameters of the second physical vapor deposition process include: the target material includes tan or titanium, the first reaction gas includes nitrogen, the nitrogen gas flow rate is 10 sccm to 30 sccm, the DC power supply power range is 5000W to 20000W, and the process time range is 1s to 6s.
[0021] Optionally, the first physical vapor deposition process includes an ionization physical vapor deposition process; the second physical vapor deposition process includes an ionization physical vapor deposition process.
[0022] Optionally, the process further includes: forming an adhesive material layer on the surface of the barrier material layer, wherein the seed crystal material layer is formed on the surface of the adhesive material layer; the planarization process further includes: forming an adhesive layer with the adhesive material layer; the material of the adhesive layer includes one or more of tank, titanium and cobalt.
[0023] Optionally, the process for forming the adhesive material layer includes a third physical vapor deposition process or an atomic layer deposition process; the third physical vapor deposition process includes a self-ionizing physical vapor deposition process.
[0024] Optionally, the method for forming the adhesive material layer includes: forming a first sub-adhesive material layer on the surface of the barrier material layer using the third physical vapor deposition process; after forming the first sub-adhesive material layer, transferring or partially transferring the first sub-adhesive material layer deposited at the bottom of the opening to the sidewall of the opening using a first backsputtering process; and after the first backsputtering process, continuing to use the third physical vapor deposition process to form a second sub-adhesive material layer on the surface of the first sub-adhesive material layer, with the first sub-adhesive material layer and the second sub-adhesive material layer constituting the adhesive material layer.
[0025] Optionally, the process parameters of the third physical vapor deposition process include: the target material includes tan, the DC power supply power range is 5000W to 20000W, and the deposition time is 2s to 8s; the process parameters of the first anti-sputtering process include: the RF power supply power range is 400W to 1000W, and the process time is 2s to 8s.
[0026] Optionally, the seed crystal material layer is doped with a second barrier atom; after the metal material layer is formed and before the planarization process, the process further includes: annealing the barrier material layer and the seed crystal material layer to allow the second barrier atom to diffuse into the initial interface region and combine with the first barrier atom to form a compound, thereby improving the initial first barrier capability.
[0027] Optionally, the annealing process parameters include: annealing temperature of 300℃ to 350℃ and annealing time of 5min to 10min.
[0028] Optionally, the seed crystal material layer formation process includes a fourth physical vapor deposition process; the fourth physical vapor deposition process includes a self-ionization physical vapor deposition process.
[0029] Optionally, the process parameters of the fourth physical vapor deposition process include: the seed target material includes a first metal, the first metal is doped with a second barrier atom, the proportion of the second barrier atom in the seed target material is in the range of 0.2at% to 1.0at, and the power of the DC power supply is in the range of 20000W to 50000W; the first metal includes copper, and the second barrier atom includes aluminum or manganese.
[0030] Optionally, the method for forming the seed crystal material layer further includes: after the fourth physical vapor deposition process, a second reverse sputtering process is used to deposit the seed crystal material layer at the bottom of the opening to the sidewall of the opening.
[0031] Optionally, the process parameters of the second anti-sputtering process include: the power range of the RF power supply is 600W to 1500W.
[0032] Optionally, the material of the metal layer includes copper; the formation process of the metal layer includes an electrochemical plating process; the electrochemical plating process parameters include: an accelerator concentration range of 6 mL / L to 10 mL / L, an inhibitor concentration range of 1 mL / L to 5 mL / L, and a leveling agent concentration range of 2 mL / L to 6 mL / L.
[0033] Optionally, after forming the first conductive layer, the method further includes: forming a second barrier layer on the surface of the first conductive layer using a chemical vapor deposition process; the material of the second barrier layer includes a cobalt compound, wherein the cobalt compound includes a copper-cobalt compound.
[0034] Compared with the prior art, the technical solution of the embodiments of the present invention has the following beneficial effects:
[0035] In the method for forming a metal interconnect structure provided by the technical solution of the present invention, the region adjacent to the first barrier layer and the dielectric layer in the final obtained metal interconnect structure has a first blocking ability to prevent the diffusion of metal ions in the first conductive layer. The first blocking ability is greater than the blocking ability of other regions of the first barrier layer to prevent the diffusion of metal ions in the first conductive layer. The region adjacent to the first barrier layer and the dielectric layer improves the blocking ability of the first barrier layer to prevent the diffusion of metal ions, which is beneficial to improving the electromigration lifetime of the metal interconnect structure. At the same time, it is beneficial to control the thickness of the first barrier layer, reduce the increase in contact resistance caused by the increase in thickness, and improve the overall stability of device performance.
[0036] Furthermore, the seed crystal material layer is doped with a second barrier atom. After the metal material layer is formed and before the planarization process, the barrier material layer and the seed crystal material layer are annealed to allow the second barrier atom to diffuse into the initial interface region and combine with the first barrier atom to form a compound, thereby improving the initial first barrier capability. This further enhances the barrier capability of the first barrier layer against the diffusion of metal ions, which is beneficial for improving the electromigration lifetime of the metal interconnect structure. At the same time, it is beneficial for controlling the thickness of the first barrier layer, reducing the increase in contact resistance caused by the increase in thickness, and overall improving the stability of device performance.
[0037] In the metal interconnect structure provided by the present invention, the region adjacent to the first barrier layer and the dielectric layer has a first blocking capability for the diffusion of metal ions in the first conductive layer. The first blocking capability is greater than the blocking capability of other regions of the first barrier layer for the diffusion of metal ions in the first conductive layer. The region adjacent to the first barrier layer and the dielectric layer improves the blocking capability of the first barrier layer for the diffusion of metal ions, which is beneficial to improving the electromigration lifetime of the metal interconnect structure. At the same time, it is beneficial to control the thickness of the first barrier layer, reduce the increase in contact resistance caused by the increase in thickness, and improve the overall stability of device performance.
[0038] Furthermore, the interface region is defined as the area adjacent to the first barrier layer and the dielectric layer. The interface region is also doped with second barrier atoms, and the first barrier atoms and the second barrier atoms combine to form a compound. This further enhances the barrier ability of the first barrier layer to block the diffusion of metal ions, which is beneficial to improving the electromigration lifetime of the metal interconnect structure. At the same time, it is beneficial to control the thickness of the first barrier layer, reduce the increase in contact resistance caused by the increase in thickness, and improve the overall stability of device performance. Attached Figure Description
[0039] Figures 1 to 2 This is a cross-sectional schematic diagram of the formation process of a metal interconnect structure;
[0040] Figures 3 to 13 This is a cross-sectional schematic diagram of the metal interconnect structure formation process according to an embodiment of the present invention. Detailed Implementation
[0041] It should be noted that the terms "surface" and "on" in this specification are used to describe the relative spatial position and are not limited to whether there is direct contact.
[0042] As described in the background section, existing copper interconnect processes require further improvement. This will now be analyzed and explained in conjunction with specific embodiments.
[0043] Figures 1 to 2This is a cross-sectional schematic diagram of the formation process of a metal interconnect structure.
[0044] Please refer to Figure 1 A substrate 100 is provided, the substrate 100 having a first conductive layer 101 therein and exposing the top surface of the first conductive layer 101; an etch stop layer 102 and a dielectric layer 103 located on the surface of the etch stop layer 102 are formed on the substrate 101; the dielectric layer 103 and the etch stop layer 102 are etched, and a trench 104 is formed in the dielectric layer 103 and the etch stop layer 102, the trench 104 exposing the surface of the first conductive layer 101.
[0045] Please refer to Figure 2 A barrier layer 105, a seed crystal layer 106 on the surface of the barrier layer 105, and a second conductive layer 107 on the surface of the seed crystal layer 106 are formed in the trench 104.
[0046] In the metal interconnect structure formed by the above method, the second conductive layer 107 is made of copper, and the barrier layer 105 is made of TaN / Ta, used to block the diffusion of copper ions from the second conductive layer 107 to the dielectric layer 103. To improve the reliability of the back-end copper interconnect, the thickness of the barrier layer 105 is usually increased to enhance its anti-diffusion capability. However, this method leads to an increase in the contact resistance of the metal interconnect structure, which cannot meet the performance requirements of advanced technology nodes.
[0047] To address the aforementioned problems, this invention provides a metal interconnect structure and its formation method. The first barrier layer, in a region adjacent to the dielectric layer, possesses a first blocking capability against the diffusion of metal ions within the first conductive layer. This first blocking capability is greater than the blocking capability of other regions of the first barrier layer against the diffusion of metal ions within the first conductive layer. The improved barrier capability against metal ion diffusion by the region adjacent to the dielectric layer enhances the electromigration lifetime of the metal interconnect structure. Furthermore, it allows for better control of the thickness of the first barrier layer, reducing the increase in contact resistance due to increased thickness, and overall improving the stability of device performance.
[0048] To make the above-mentioned objectives, features and beneficial effects of the present invention more apparent and understandable, specific embodiments of the present invention will be described in detail below with reference to the accompanying drawings.
[0049] Figures 3 to 13 This is a cross-sectional schematic diagram of the metal interconnect structure formation process according to an embodiment of the present invention.
[0050] Please refer to Figure 3A substrate 20 is provided, the substrate 20 including a base 200 and a dielectric layer 201 located on the surface of the base 200, the dielectric layer 201 having an opening 202 the bottom of which exposes the surface of the base 200.
[0051] The opening 202 is used to form a first conductive layer. A device structure (such as a transistor) may be formed in the substrate 200. The first conductive layer is used to electrically connect with the device structure. Alternatively, the substrate 200 has metal interconnects that connect the device structure. The second conductive layer is the uppermost metal interconnect. The first conductive layer is used to electrically connect with the second conductive layer.
[0052] In this embodiment, the depth of the opening 202 is 500±9nm and the width is 200±2nm. In other embodiments, the size of the opening may not be limited.
[0053] In this embodiment, the metal interconnect structure is used to form a 40nm process automotive chip; in other embodiments, it may not be limited to this.
[0054] In this embodiment, the substrate 200 has a second conductive layer 203, and the bottom of the opening 202 exposes the surface of the second conductive layer 203.
[0055] The material of the second conductive layer 203 includes a metal, such as copper, tungsten, or cobalt. In this embodiment, the material of the second conductive layer 203 is copper.
[0056] The dielectric layer 201 is made of a low-k dielectric material, which includes one or more of silicon carbonitride, silicon carbide, and silicon hydroxide. The low-k dielectric material refers to a material with a dielectric constant (K value) of 3 or less, which helps to reduce signal transmission delays caused by the reduction of feature size in integrated circuits.
[0057] In this embodiment, the dielectric layer 201 is made of silicon oxycarbonate (Si-CO).
[0058] The oxygen content in the dielectric layer 201 is less than or equal to 10 at%. Due to the low oxygen content, the dielectric constant of the dielectric layer 201 is low.
[0059] In this embodiment, an etch stop layer 204 is further provided between the dielectric layer 201 and the substrate 200, and the opening 202 is located within the etch stop layer 204.
[0060] In this embodiment, the opening 202 includes a groove (not shown in the figure) and a through hole (not shown in the figure) located at the bottom of the groove. The groove and the through hole are interconnected. The groove has a first projection on the surface of the substrate 200, and the through hole has a second projection on the surface of the substrate 200. The second projection is located within the range of the first projection.
[0061] In this embodiment, before forming the barrier material layer, the substrate 20 is placed in a vacuum chamber and its surface is pre-cleaned. For example, during the surface pre-cleaning process, the substrate 20 can be heated to 300°C to improve the cleanliness of the surface of the dielectric layer 201 and the sidewalls and bottom of the opening 202, thereby reducing the contact resistance between the second conductive layer 203 and the subsequently formed first conductive layer.
[0062] Please refer to Figure 4 and Figure 5 , Figure 5 for Figure 4 The enlarged view of the area indicated by the dashed box shows that a barrier material layer 205 is formed on the sidewall and bottom of the opening 202 and on the surface of the medium layer 201.
[0063] In this embodiment, the barrier material layer 205 includes an initial interface region i and an initial main body region ii. The area adjacent to the medium layer 201 of the barrier material layer 205 is the initial interface region i, and the other areas of the barrier material layer 205 are the initial main body region ii.
[0064] In this embodiment, the initial interface region i is doped with a first barrier atom a1. The first barrier atom a1 is used to improve the barrier material layer 205's ability to block the diffusion of metal ions within the subsequently formed metal material layer.
[0065] The initial interface region i is adjacent to the dielectric layer 201, specifically referring to the initial interface region i located at the interface between the dielectric layer 201 and the barrier material layer 205.
[0066] The initial interface region i has a thickness ranging from 1 nm to 2 nm. The barrier material layer 205 is used to form a first barrier layer, wherein the initial interface region i is used to form an interface region, and the initial host region ii is used to form a host region.
[0067] The thickness of the barrier material layer 205 ranges from 3 nm to 10 nm. The barrier material layer 205 is used to form the first barrier layer. The purpose of selecting this thickness range is to avoid it being too thin to be effective, and to avoid it being too thick to increase the metal wiring capacitance, which in turn increases the transmission delay (RC delay) in the metal interconnect process.
[0068] In this embodiment, the thickness of the barrier material layer 205 is 4 nm.
[0069] The method for forming the barrier material layer 205 includes: placing the substrate 20 in a barrier layer deposition chamber (not shown in the figure); introducing a first reactive gas and a second reactive gas into the barrier layer deposition chamber, and forming the initial interface region i using a first physical vapor deposition process, wherein the second reactive gas is used to provide the first barrier atoms a1, and the ratio of the flow rate of the first reactive gas to the flow rate of the second reactive gas is in the range of 1% to 5%; stopping the introduction of the second reactive gas while maintaining the introduction of the first reactive gas, and forming the initial host region on the initial interface region using a second physical vapor deposition process.
[0070] In this embodiment, the first reactant gas is nitrogen, and the second reactant gas is oxygen. More optimally, in the first physical vapor deposition process, the ratio of nitrogen to oxygen is 1:96.
[0071] The process parameters of the first physical vapor deposition process include: the target material includes tan or titanium, the first reactant gas includes nitrogen, the second reactant gas includes oxygen, the flow rate of nitrogen ranges from 10 sccm to 30 sccm, the flow rate of oxygen ranges from 0.1 sccm to 1.4 sccm, the DC power supply ranges from 5000W to 20000W, and the process time ranges from 2s to 4s.
[0072] In this embodiment, the target material is tan, the first reactant gas is nitrogen, the second reactant gas is oxygen, the DC power supply is 15000W, and the process time is 2s. Thus, an initial interface region i is formed through a first physical vapor deposition process. The material of this initial interface region i is tan nitride doped with oxygen atoms. The oxygen atoms form tantalum oxide within the initial interface region i, resulting in a low tantalum oxide (TAOx, x < 2.5) material. The tantalum oxide improves the metal diffusion barrier capability of the initial interface region i.
[0073] The process parameters of the second physical vapor deposition process include: the target material includes tan or titanium, the first reaction gas includes nitrogen, the nitrogen gas flow rate is 10 sccm to 30 sccm, the DC power supply power range is 5000W to 20000W, and the process time range is 1s to 6s.
[0074] In this embodiment, the target material is tan, the second reactant gas is nitrogen, the DC power supply is 15000W, and the process time is 2s. The initial host region ii is formed by a second physical vapor deposition process, and its material is tan nitride.
[0075] In this embodiment, the first physical vapor deposition process includes a self-ionizing physical vapor deposition process.
[0076] In other embodiments, the first physical vapor deposition process may also be a sputtering process, an evaporation process, etc.
[0077] It should be noted that ionized physical vapor deposition (IPVD) is more advantageous than ordinary physical vapor deposition processes in improving the step coverage of the material film.
[0078] In this embodiment, the second physical vapor deposition process includes a self-ionizing physical vapor deposition process.
[0079] In other embodiments, the second physical vapor deposition process may also be a sputtering process, an evaporation process, etc.
[0080] In this embodiment, before forming the seed crystal material layer, an adhesion material layer 206 is formed on the surface of the barrier material layer 205, and subsequently, a seed crystal material layer is formed on the surface of the adhesion material layer 206. The adhesion material layer 206 is used to form an adhesion layer to increase the adhesion between the first conductive layer and the dielectric layer 201 and reduce the occurrence of the first conductive layer falling off.
[0081] The formation process of the adhesive material layer 206 includes a third physical vapor deposition process or an atomic layer deposition process. In this embodiment, the formation process of the adhesive material layer 206 is a third physical vapor deposition process.
[0082] In this embodiment, the third physical vapor deposition process includes a self-ionization physical vapor deposition process.
[0083] In other embodiments, the third physical vapor deposition process may also be a sputtering process, an evaporation process, etc.
[0084] The material of the adhesive layer 206 includes one or more of tantalum, titanium, and cobalt. In this embodiment, the material of the adhesive layer 206 is tantalum.
[0085] The thickness of the adhesive material layer 206 ranges from 3 nm to 10 nm.
[0086] In this embodiment, the method for forming the adhesive material layer 206 includes: forming a first sub-adhesive material layer (not shown in the figure) on the surface of the barrier material layer using the third physical vapor deposition process; after forming the first sub-adhesive material layer, transferring or partially transferring the first sub-adhesive material layer deposited at the bottom of the opening 202 to the sidewall of the opening 202 using a first reverse sputtering process; after the first reverse sputtering process, continuing to use the third physical vapor deposition process to form a second sub-adhesive material layer (not shown in the figure) on the surface of the first sub-adhesive material layer, with the first sub-adhesive material layer and the second sub-adhesive material layer constituting the adhesive material layer 206.
[0087] The process parameters for the third physical vapor deposition process include: the target material is tan, the DC power supply power range is 5000W to 20000W, and the deposition time is 2s to 8s. In this embodiment, the target material is tan, the DC power supply power is 15000W, and the deposition time is 4s.
[0088] The process parameters for the first anti-sputtering process include: an RF power supply range of 400W to 1000W and a process time of 2s to 8s. In this embodiment, the RF power supply is 700W and the process time is 3s.
[0089] In another embodiment, the adhesive material layer may not be formed.
[0090] Please refer to Figure 6 and Figure 7 , Figure 7 for Figure 6 The enlarged view of the area indicated by the dashed box shows that a seed crystal material layer 207 is formed on the surface of the barrier material layer 205.
[0091] Specifically, the seed crystal material layer 207 is formed on the surface of the adhesive material layer 206.
[0092] In this embodiment, the seed crystal material layer 207 is doped with a second barrier atom a2.
[0093] In other embodiments, the seed crystal material layer may not be doped with the second blocking atom.
[0094] In this embodiment, the second blocking atom a2 is manganese.
[0095] In other embodiments, the second blocking atom a2 may be aluminum.
[0096] The seed crystal material layer 207 is used to provide a seed crystal for the subsequently formed metal material layer.
[0097] The thickness of the seed crystal material layer 207 ranges from 20 nm to 60 nm. In this embodiment, the thickness of the seed crystal material layer 207 is 45 nm.
[0098] The formation process of the seed crystal material layer 207 includes a fourth physical vapor deposition process.
[0099] In this embodiment, the fourth physical vapor deposition process includes a self-ionization physical vapor deposition process.
[0100] In another embodiment, the fourth physical vapor deposition process can also be a sputtering process, an evaporation process, etc.
[0101] The process parameters of the fourth physical vapor deposition process include: the seed target material includes a first metal, the first metal is doped with a second barrier atom, the proportion of the second barrier atom in the seed target material is in the range of 0.2at% to 1.0at, and the power of the DC power supply is in the range of 20000W to 50000W; the first metal includes copper, and the second barrier atom includes aluminum or manganese.
[0102] In this embodiment, the first metal is copper, the second blocking atom is manganese, the proportion of manganese atoms in the seed crystal target is 0.8 at%, and the power of the DC power supply is 38000W.
[0103] In another embodiment, the first metal is copper, the second blocking atom is aluminum, and the proportion of aluminum atoms in the seed crystal target is 0.25 at.
[0104] The seed crystal material layer 207 is used to provide a seed crystal for the subsequent formation of the metal material layer; that is, the seed crystal material layer 207 is made of the same material as the metal material layer. In other embodiments, the first metal may also be made of aluminum, tungsten, etc.
[0105] In this embodiment, the method for forming the seed crystal material layer further includes: after the fourth physical vapor deposition process, a second reverse sputtering process is used to deposit the seed crystal material layer at the bottom of the opening to the sidewall of the opening.
[0106] The process parameters for the second anti-sputtering process include: the power range of the RF power supply is 600W to 1500W. In this embodiment, the power of the RF power supply is 1000W.
[0107] Please refer to Figure 8 and Figure 9 , Figure 9 for Figure 8The enlarged view of the area indicated by the dashed box shows that a metal material layer 208 is formed on the surface of the seed crystal material layer 207. The region adjacent to the barrier material layer 205 and the dielectric layer 201 has an initial first blocking ability for the diffusion of metal ions in the metal material layer 208. The initial first blocking ability is greater than the blocking ability of other regions of the barrier material layer 205 for the diffusion of metal ions in the metal material layer 208.
[0108] Specifically, the initial interface region i has an initial first blocking capability for the diffusion of metal ions within the metal material layer 208, and the initial main body region ii has an initial second blocking capability for the diffusion of metal ions within the metal material layer 208, wherein the initial first blocking capability is greater than the initial second blocking capability.
[0109] That is, the initial interface region i is doped with a first barrier atom relative to the initial host region ii, so that the initial first barrier capability is greater than the initial second barrier capability.
[0110] The metal material layer 208 is used to form a first conductive layer, and after the metal material layer 208 is formed, the opening 202 is filled.
[0111] In this embodiment, the thickness of the metal material layer 208 is 750 nm.
[0112] The metal material layer 208 is made of copper, aluminum, or tungsten. In this embodiment, the metal material layer 208 is made of copper.
[0113] In this embodiment, the formation process of the metal material layer 208 includes an electrochemical plating process.
[0114] The electrochemical plating process parameters include: an accelerator concentration ranging from 6 mL / L to 10 mL / L, an inhibitor concentration ranging from 1 mL / L to 5 mL / L, and a leveling agent concentration ranging from 2 mL / L to 6 mL / L. The purpose of selecting these parameters is to achieve a Cu(111) texture, facilitate stress release, and improve grain size. In this embodiment, the accelerator concentration is 9 mL / L, the inhibitor concentration is 2 mL / L, and the leveling agent concentration is 3 mL / L.
[0115] In this embodiment, after the metal material layer 208 is formed and before the planarization process, please refer to... Figure 10 and Figure 11 .
[0116] Please refer to Figure 10 and Figure 11 , Figure 11 for Figure 10The enlarged view of the area indicated by the dashed box shows the annealing treatment of the barrier material layer 205 and the seed crystal material layer 207, so that the second barrier atom a2 (as shown in the dashed box) is annealed. Figure 9 (As shown) diffuses into the initial interface region i, and interacts with the first blocking atom a1 (as shown) Figure 9 (As shown) Combined to form a compound (not shown in the figure) to enhance the initial first blocking capability.
[0117] In another embodiment, the seed crystal material layer is not doped with the second barrier atom, therefore, the annealing process is not required.
[0118] The annealing process parameters include: an annealing temperature of 300°C to 350°C and an annealing time of 5 min to 10 min. In this embodiment, the annealing temperature is 350°C, the annealing time is 10 minutes, and saturated nitrogen is used as the protective gas.
[0119] Please refer to Figure 12 and Figure 13 , Figure 13 for Figure 12 The enlarged view of the area indicated by the dashed box shows the planarization of the metal material layer 208, the seed crystal material layer 207, and the barrier material layer 205 until the surface of the dielectric layer 201 is exposed. The metal material layer 208 forms a first conductive layer 209, the seed crystal material layer 207 forms a seed crystal layer 210, and the barrier material layer 205 forms a first barrier layer 211. The region of the first barrier layer 211 adjacent to the dielectric layer 201 has a first blocking ability against the diffusion of metal ions in the first conductive layer 209. The first blocking ability is greater than the blocking ability of other regions of the first barrier layer 211 against the diffusion of metal ions in the first conductive layer 209.
[0120] Thus, in the final metal interconnect structure, the region adjacent to the first barrier layer 211 and the dielectric layer 201 improves the barrier layer 211's ability to block metal ion diffusion, which is beneficial to improving the electromigration lifetime of the metal interconnect structure. At the same time, it is beneficial to control the thickness of the first barrier layer 211, reducing the increase in contact resistance caused by the increase in thickness, and overall improving the stability of device performance.
[0121] In this embodiment, the first barrier layer 211 includes an interface region I and a main body region II, with the initial interface region i forming the interface region I and the initial main body region ii forming the main body region II.
[0122] The interface region I is the region adjacent to the first barrier layer 211 and the dielectric layer 201, and the main body region II is the other regions below the barrier layer. The interface region I has a first blocking ability to prevent the diffusion of metal ions in the first conductive layer 209, and the main body region II has a second blocking ability to prevent the diffusion of metal ions in the first conductive layer 209. The first blocking ability is greater than the second blocking ability.
[0123] The initial interface region i is doped with a first barrier a1 to improve the diffusion ability of metal ions in the initial interface region i, thereby improving the barrier ability of the first barrier layer 211 to block the diffusion of metal ions in the interface region I.
[0124] More optimally, the seed crystal material layer 207 is doped with a second barrier atom a2. The barrier material layer 205 and the seed crystal material layer 207 are annealed to allow the second barrier atom a2 to diffuse into the initial interface region i and combine with the first barrier atom a1 to form a compound, thereby improving the initial first barrier capability. This further enhances the barrier capability of the first barrier layer 211 against the diffusion of metal ions, which is beneficial for improving the electromigration lifetime of the metal interconnect structure. At the same time, it is beneficial for controlling the thickness of the first barrier layer, reducing the increase in contact resistance caused by the increase in thickness, and overall improving the stability of device performance.
[0125] The first blocking atom includes oxygen atoms, and the proportion of the first blocking atom in the interface region I ranges from 10 at% to 20 at%. In this embodiment, the first blocking atom is an oxygen atom.
[0126] The second blocking atom includes manganese atoms or aluminum atoms, and the proportion of the second blocking atom in the interface region I ranges from 1 at% to 5 at%. In this embodiment, the second blocking atom is a manganese atom.
[0127] The thickness of the interface region I ranges from 1 nm to 2 nm.
[0128] The thickness of the first barrier layer 211 ranges from 3 nm to 10 nm. In this embodiment, the thickness of the first barrier layer 211 is 4 nm.
[0129] In this embodiment, the planarization process further forms an adhesion layer 212 using the adhesion material layer 206.
[0130] The material of the adhesive layer 212 includes one or more of tank, titanium, and cobalt. In this embodiment, the material of the adhesive layer is tank.
[0131] The thickness of the adhesion layer 212 ranges from 3 nm to 10 nm.
[0132] In this embodiment, after the first conductive layer 209 is formed, a second barrier layer 213 is formed on the surface of the first conductive layer 209 by chemical vapor deposition.
[0133] In this embodiment, the material of the second barrier layer 213 includes a cobalt metal compound, and the cobalt metal compound includes a copper-cobalt compound.
[0134] In this embodiment, the second barrier layer 213 is formed by a selective growth process, that is, it is formed only on the exposed surfaces of the first conductive layer 209 and the seed layer 210.
[0135] In another embodiment, the second barrier layer also covers the top surface of the medium layer and the first barrier layer.
[0136] In yet another embodiment, the second barrier layer may not be formed.
[0137] Accordingly, another embodiment of the present invention also provides a metal interconnect structure formed by the above method. Please refer to [link / reference needed]. Figure 12 and Figure 13 The substrate 20 includes a base 200 and a dielectric layer 201 located on the surface of the base 200, wherein the dielectric layer 201 has an opening 202 (e.g., ...). Figure 3 As shown), the opening 202 exposes the surface of the substrate 200; a first barrier layer 211 is located on the sidewall and bottom of the opening 202, a seed layer 210 is located on the surface of the first barrier layer 211, and a first conductive layer 209 is located on the surface of the seed layer 210. The region of the first barrier layer 211 adjacent to the dielectric layer 201 has a first blocking ability to prevent the diffusion of metal ions in the first conductive layer 209. The first blocking ability is greater than the blocking ability of other regions of the first barrier layer 211 to prevent the diffusion of metal ions in the first conductive layer 209.
[0138] Thus, the region adjacent to the first barrier layer 211 and the dielectric layer 201 improves the barrier layer 211's ability to block metal ion diffusion, which is beneficial to improving the electromigration lifetime of the metal interconnect structure. At the same time, it is beneficial to control the thickness of the first barrier layer 211, reducing the increase in contact resistance caused by the increase in thickness, and overall improving the stability of device performance.
[0139] In this embodiment, the first barrier layer 211 includes an interface region I and a main region II. The region adjacent to the dielectric layer 201 is the interface region I, and the other regions of the first barrier layer 211 are the main region II. The interface region I is doped with a first barrier atom a1 (e.g., ...). Figure 9As shown in the figure, the interface region I has a first blocking ability to prevent the diffusion of metal ions in the first conductive layer 209, and the main body region II has a second blocking ability to prevent the diffusion of metal ions in the first conductive layer 209. The first blocking ability is greater than the second blocking ability.
[0140] In this embodiment, the substrate 200 has a second conductive layer 203, and the bottom of the opening 202 exposes the surface of the second conductive layer 203.
[0141] The dielectric layer 201 is made of a low-k dielectric material, which includes one or more of silicon carbonitride, silicon carbide, and silicon hydroxide. In this embodiment, the dielectric layer 201 is made of silicon carbide (Si-CO).
[0142] The oxygen content in the dielectric layer 201 is less than or equal to 10 at%. Due to the low oxygen content, the dielectric constant of the dielectric layer 201 is low.
[0143] In this embodiment, an etch stop layer 204 is further provided between the dielectric layer 201 and the substrate 200, and the opening 202 is located within the etch stop layer 204.
[0144] The first barrier atom a1 includes oxygen atoms; the proportion of the first barrier atom a1 in the interface region ranges from 10 at% to 20 at%.
[0145] In this embodiment, the interface region I is also doped with a second barrier atom a2 (such as...). Figure 9 As shown in the figure), the first blocking atom a1 and the second blocking atom a2 combine to form a compound (not shown in the figure).
[0146] Here, the second barrier atom a2 further enhances the barrier capability of the first barrier layer 211 against the diffusion of metal ions, which is beneficial to improving the electromigration lifetime of the metal interconnect structure. At the same time, it is beneficial to control the thickness of the first barrier layer 211, reduce the increase in contact resistance caused by the increase in thickness, and improve the overall stability of device performance.
[0147] The second barrier atom a2 includes manganese atoms or aluminum atoms; the proportion of the second barrier atom a2 in the interface region ranges from 1 at% to 5 at%.
[0148] The material of the first barrier layer 211 includes tanium nitride or titanium nitride. In this embodiment, the material of the first barrier layer 211 is tanium nitride.
[0149] In this embodiment, the metal interconnect structure further includes an adhesion layer 212 located between the first barrier layer 211 and the seed layer 210.
[0150] The material of the adhesion layer 212 includes one or more of tantalum, titanium, and cobalt. In this embodiment, the material of the adhesion layer 212 is tantalum.
[0151] In this embodiment, the metal interconnect structure further includes a second barrier layer 213 located on top of the first conductive layer 209.
[0152] The second barrier layer 213 is made of a cobalt compound, including a copper-cobalt compound. The second barrier layer 213 serves to block the diffusion of dielectric material from the top of the first conductive layer 209 to the outside.
[0153] The top of the first conductive layer 219 is lower than or flush with the top surface of the dielectric layer 201. In this embodiment, the top of the first conductive layer 219 is flush with the top surface of the dielectric layer 201.
[0154] In this embodiment, the thickness of the interface region I ranges from 1 nm to 2 nm.
[0155] In this embodiment, the thickness of the first barrier layer 211 ranges from 3 nm to 10 nm.
[0156] While the present invention has been disclosed above, it is not limited thereto. Any person skilled in the art can make various modifications and alterations without departing from the spirit and scope of the invention; therefore, the scope of protection of the present invention should be determined by the scope defined in the claims.
Claims
1. A metal interconnect structure, characterized in that, include: A substrate, the substrate comprising a base and a dielectric layer located on the surface of the base, the dielectric layer having an opening that exposes the surface of the base; The first barrier layer located on the sidewall and bottom of the opening, the seed crystal layer located on the surface of the first barrier layer, and the first conductive layer located on the surface of the seed crystal layer, wherein the region of the first barrier layer adjacent to the dielectric layer has a first blocking ability to prevent the diffusion of metal ions in the first conductive layer, and the first blocking ability is greater than the blocking ability of other regions of the first barrier layer to prevent the diffusion of metal ions in the first conductive layer.
2. The metal interconnect structure as described in claim 1, characterized in that, The first barrier layer includes an interface region and a main body region, with the region adjacent to the dielectric layer being the interface region and the other regions of the first barrier layer being the main body region; the interface region is doped with first barrier atoms.
3. The metal interconnect structure as described in claim 2, characterized in that, The thickness of the interface region ranges from 1 nm to 2 nm; the thickness of the first barrier layer ranges from 3 nm to 10 nm.
4. The metal interconnect structure as described in claim 2, characterized in that, The first barrier atom includes oxygen atoms; the proportion of the first barrier atom in the interface region ranges from 10 at% to 20 at%; the material of the first barrier layer includes titanium nitride or titanium nitride.
5. The metal interconnect structure as described in claim 2, characterized in that, The interface region is also doped with a second barrier atom, and the first barrier atom and the second barrier atom are combined to form a compound; the second barrier atom includes manganese atoms or aluminum atoms; the proportion of the second barrier atom in the interface region ranges from 1 at% to 5 at%.
6. The metal interconnect structure as described in claim 1, characterized in that, Also includes: An adhesive layer is located between the first barrier layer and the seed crystal layer; the material of the adhesive layer includes one or more of tank, titanium and cobalt.
7. The metal interconnect structure as claimed in claim 1, characterized in that, Also includes: A second barrier layer is located on top of the first conductive layer; the material of the second barrier layer includes a cobalt metal compound, and the cobalt metal compound includes a copper-cobalt compound.
8. The metal interconnect structure as claimed in claim 1, characterized in that, The top of the first conductive layer is lower than or flush with the top surface of the dielectric layer.
9. The metal interconnect structure as claimed in claim 1, characterized in that, The dielectric layer is made of a low-K dielectric material, which includes one or more of silicon carbonitride, silicon carbon oxycarbonate, and silicon hydroxide; the oxygen content in the dielectric layer is less than or equal to 10 at.
10. A method for forming a metal interconnect structure, characterized in that, include: A substrate is provided, the substrate including a base and a dielectric layer located on the surface of the base, the dielectric layer having an opening, the bottom of the opening exposing the surface of the base; A barrier material layer is formed on the sidewalls and bottom of the opening, as well as on the surface of the medium layer; A seed crystal material layer is formed on the surface of the barrier material layer; A metal material layer is formed on the surface of the seed crystal material layer. The region adjacent to the barrier material layer and the dielectric layer has an initial first blocking ability for the diffusion of metal ions in the metal material layer. The initial first blocking ability is greater than the blocking ability of other regions of the barrier material layer for the diffusion of metal ions in the metal material layer. The metal material layer, the seed crystal material layer, and the barrier material layer are planarized until the surface of the dielectric layer is exposed. A first conductive layer is formed with the metal material layer, a seed crystal layer is formed with the seed crystal material layer, and a first barrier layer is formed with the barrier material layer. The region of the first barrier layer adjacent to the dielectric layer has a first blocking ability to prevent the diffusion of metal ions in the first conductive layer. The first blocking ability is greater than the blocking ability of other regions of the first barrier layer to prevent the diffusion of metal ions in the first conductive layer.
11. The method for forming a metal interconnect structure as described in claim 10, characterized in that, The barrier material layer includes an initial interface region and an initial host region, wherein the region adjacent to the dielectric layer is the initial interface region, and other regions of the barrier material layer are the initial host regions; the initial interface region is doped with a first barrier atom; the first barrier layer includes an interface region and a host region, wherein the interface region is formed by the initial interface, and the host region is formed by the initial host region.
12. The method for forming a metal interconnect structure as described in claim 11, characterized in that, The method for forming the barrier material layer includes: placing the substrate in a barrier layer deposition chamber; introducing a first reactive gas and a second reactive gas into the barrier layer deposition chamber, and forming the initial interface region using a first physical vapor deposition process, wherein the second reactive gas is used to provide the first barrier atoms, and the ratio of the flow rate of the first reactive gas to the flow rate of the second reactive gas is in the range of 1% to 5%; stopping the introduction of the second reactive gas while maintaining the introduction of the first reactive gas, and forming the initial host region on the initial interface region using a second physical vapor deposition process.
13. The method for forming a metal interconnect structure as described in claim 12, characterized in that, The process parameters of the first physical vapor deposition process include: the target material includes tan or titanium, the first reactant gas includes nitrogen, the second reactant gas includes oxygen, the flow rate of nitrogen ranges from 10 sccm to 30 sccm, the flow rate of oxygen ranges from 0.1 sccm to 1.4 sccm, the DC power supply ranges from 5000W to 20000W, and the process time ranges from 2s to 4s.
14. The method for forming a metal interconnect structure as described in claim 12, characterized in that, The process parameters of the second physical vapor deposition process include: the target material includes tan or titanium, the first reaction gas includes nitrogen, the nitrogen gas flow rate is 10 sccm to 30 sccm, the DC power supply power range is 5000W to 20000W, and the process time range is 1s to 6s.
15. The method for forming a metal interconnect structure as described in claim 12, characterized in that, The first physical vapor deposition process includes an ionization physical vapor deposition process; the second physical vapor deposition process includes an ionization physical vapor deposition process.
16. The method for forming a metal interconnect structure as described in claim 12, characterized in that, Also includes: An adhesive material layer is formed on the surface of the barrier material layer, and the seed crystal material layer is formed on the surface of the adhesive material layer; The planarization process further includes: forming an adhesion layer with the adhesion material layer; The material of the adhesive layer includes one or more of tank, titanium, and cobalt.
17. The method for forming a metal interconnect structure as described in claim 16, characterized in that, The process for forming the adhesive material layer includes a third physical vapor deposition process or an atomic layer deposition process; the third physical vapor deposition process includes a self-ionization physical vapor deposition process.
18. The method for forming a metal interconnect structure as described in claim 17, characterized in that, The method for forming the adhesive material layer includes: forming a first sub-adhesive material layer on the surface of the barrier material layer using the third physical vapor deposition process; after forming the first sub-adhesive material layer, transferring or partially transferring the first sub-adhesive material layer deposited at the bottom of the opening to the sidewall of the opening using a first backsputtering process; and after the first backsputtering process, continuing to use the third physical vapor deposition process to form a second sub-adhesive material layer on the surface of the first sub-adhesive material layer, with the first sub-adhesive material layer and the second sub-adhesive material layer constituting the adhesive material layer.
19. The method for forming a metal interconnect structure as described in claim 18, characterized in that, The process parameters of the third physical vapor deposition process include: the target material includes tan, the DC power supply power range is 5000W to 20000W, and the deposition time is 2s to 8s; the process parameters of the first anti-sputtering process include: the RF power supply power range is 400W to 1000W, and the process time is 2s to 8s.
20. The method for forming a metal interconnect structure as described in claim 11, characterized in that, The seed crystal material layer is doped with a second barrier atom; After the metal material layer is formed, and before the planarization process, the process further includes: annealing the barrier material layer and the seed crystal material layer to allow the second barrier atoms to diffuse into the initial interface region and combine with the first barrier atoms to form a compound, thereby improving the initial first barrier capability.
21. The method for forming a metal interconnect structure as described in claim 20, characterized in that, The annealing process parameters include: annealing temperature of 300℃ to 350℃ and annealing time of 5min to 10min.
22. The method for forming a metal interconnect structure as described in claim 20, characterized in that, The formation process of the seed crystal material layer includes a fourth physical vapor deposition process; the fourth physical vapor deposition process includes a self-ionization physical vapor deposition process.
23. The method for forming a metal interconnect structure as described in claim 22, characterized in that, The process parameters of the fourth physical vapor deposition process include: the seed target material includes a first metal, the first metal is doped with a second barrier atom, the proportion of the second barrier atom in the seed target material is in the range of 0.2at% to 1.0at, and the power of the DC power supply is in the range of 20000W to 50000W; the first metal includes copper, and the second barrier atom includes aluminum or manganese.
24. The method for forming a metal interconnect structure as described in claim 22, characterized in that, The method for forming the seed crystal material layer further includes: after the fourth physical vapor deposition process, a second reverse sputtering process is used to deposit the seed crystal material layer at the bottom of the opening to the sidewall of the opening.
25. The method for forming a metal interconnect structure as described in claim 24, characterized in that, The process parameters for the second anti-sputtering process include: the power range of the RF power supply is 600W to 1500W.
26. The method for forming a metal interconnect structure as described in claim 10, characterized in that, The material of the metal layer includes copper; the formation process of the metal layer includes an electrochemical plating process; the electrochemical plating process parameters include: an accelerator concentration range of 6 mL / L to 10 mL / L, an inhibitor concentration range of 1 mL / L to 5 mL / L, and a leveling agent concentration range of 2 mL / L to 6 mL / L.
27. The method for forming a metal interconnect structure as described in claim 10, characterized in that, After forming the first conductive layer, the process further includes: forming a second barrier layer on the surface of the first conductive layer using a chemical vapor deposition process; the material of the second barrier layer includes a cobalt compound, and the cobalt compound includes a copper-cobalt compound.