Power module integrated structure and assembling process under high temperature environment
By using high-temperature solder sintering and laser sealing processes on SiC power chips and double-layer DPC substrates, the problems of high current carrying capacity and miniaturization of existing power modules in a high-temperature environment of 200℃ have been solved, achieving efficient heat dissipation and reliability.
Patent Information
- Application Number
- CN202611663790.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-27
- Publication Date
- 2026-11-24
AI Technical Summary
Existing power modules cannot simultaneously meet the requirements of high current carrying capacity and miniaturized packaging in a high-temperature environment of 200℃. They have problems such as low junction temperature limit of silicon-based chips, mismatch of thermal expansion coefficient of PCB substrate, solder creep fatigue and expansion cracking of silicon gel.
By employing SiC power chips, double-layer DPC substrates, tungsten copper base plates, and high-temperature solder sintering technology, combined with nano-silver sintering paste and laser sealing process, a high-temperature oxidation-resistant interconnect structure is constructed to achieve vertical wiring and hermetically sealed packaging.
It achieves long-term stable operation in a high-temperature environment of 200℃, reduces thermal resistance, improves heat dissipation capacity, reduces thermomechanical stress, and ensures the reliability and lifespan of the module.
Smart Images

Figure CN123165115A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of semiconductor device packaging technology, specifically to a power module integrated structure and assembly process for high-temperature environments. Background Technology
[0002] As deep earth exploration projects continue to advance to depths of 10,000 meters, the operating environment temperature of downhole measurement-while-drilling (MWD) systems is constantly rising. In China, the downhole ambient temperature in 10,000-meter scientific exploration wells can reach over 200°C. As the power core of the MWD system, the power module's ability to withstand high temperatures and high currents directly determines the reliability and service life of the entire system.
[0003] Most existing power modules use silicon-based chips, ordinary PCB substrates, and conventional solder and silicone gel encapsulation processes, which are only suitable for operating conditions at 150°C and below. When faced with the extreme downhole environment of 200°C, they expose many defects: 1. The junction temperature limit of silicon-based power chips is generally below 175℃, and they cannot operate stably in an environment of 200℃ for a long time; 2. The thermal expansion coefficient of the PCB substrate is severely mismatched with that of the silicon carbide chip, resulting in significant thermomechanical stress under high-temperature cycling, which leads to solder joint cracking and package failure. 3. To meet the requirement of carrying a 20A high current on a single-layer copper-clad ceramic substrate, a large wiring area is required. Due to the limitation of the inner diameter of the downhole instrument tube, it is difficult to achieve both high current and miniaturization at the same time. 4. Conventional tin-based solders have melting points close to their operating temperature of 200°C, making them highly susceptible to creep and fatigue failure under high-temperature conditions; 5. In conventional reflow soldering processes, the weld interface is prone to oxidation, resulting in a high porosity in the weld layer, increased thermal resistance, and poor heat dissipation performance. 6. Silicone gel potting materials undergo severe thermal expansion at 200°C, compressing bonding wires and bonding tapes and causing interconnect structure cracking and failure.
[0004] Therefore, developing a power module integration structure and assembly process that is compatible with high temperatures of 200℃ and takes into account both high current carrying capacity and miniaturization is an urgent need for the development of deep well drilling equipment. Summary of the Invention
[0005] The purpose of this invention is to provide an integrated structure and assembly process for a power module in a high-temperature environment, so as to solve the technical problem mentioned in the background art that existing power modules are difficult to simultaneously meet the requirements of 200°C high-temperature resistance, high current, and miniaturized packaging.
[0006] To achieve the above objectives, the present invention provides the following technical solution: A power module integrated structure for high-temperature environments includes a tungsten copper base plate, a frame, a high-current connector, a cover plate, a double-layer DPC substrate, and multiple SiC power chips. The dual-layer DPC substrate includes an upper DPC substrate and a lower DPC substrate. The back side of the upper DPC substrate and the front side of the lower DPC substrate are connected by high-temperature solder stacking and sintering to form a dual-layer DPC substrate. The frame is fixed to the tungsten copper base plate by high-temperature soldering, the high-current connector is fixed to the frame by high-temperature soldering, and the back of the lower DPC substrate is fixed to the tungsten copper base plate by high-temperature soldering. The SiC power chip is sintered and fixed to the front pads of the upper DPC substrate using nano-silver sintering paste; the SiC power chip and the upper DPC substrate are bonded and interconnected using thick aluminum wire; the high-current connector and the lower DPC substrate are bonded and interconnected using wide gold strips via electronic spot welding; the cover plate and the frame are sealed and connected by laser sealing.
[0007] More preferably, the high-current connector has a glass sintered hermetic structure and a rated current ≥20A.
[0008] More preferably, the copper trace current carrying capacity of the double-layer DPC substrate is ≥20A.
[0009] More preferably, the upper DPC substrate is provided with an array of copper vias, and the front traces of the upper DPC substrate are electrically connected by the array of copper vias and the back traces.
[0010] More preferably, a waffle-structured copper layer is provided on the back side of the lower DPC substrate, with a grid trench width of 0.2mm-0.5mm and a grid unit size of 3mm×5mm to 5mm×5mm.
[0011] More preferably, each SiC power chip is equipped with six thick aluminum wires with a diameter of 100μm, which are bonded to the upper DPC substrate by ultrasonic wedge welding.
[0012] More preferably, the wide gold strip has a width of 1000 μm and a thickness of 25 μm.
[0013] More preferably, the high-temperature solder is selected from Au80Sn20 or Pb92.5Sn5Ag2.5 alloy solder; the copper layer thickness on both sides of the upper and lower DPC substrates is 100μm; the ceramic substrate of the upper and lower DPC substrates is selected from aluminum nitride or alumina ceramic with a thickness of 0.38mm.
[0014] The present invention also provides an assembly process for a power module integrated structure under high temperature conditions, comprising the following steps: Step 1: Select Au80Sn20 and Pb92.5Sn5Ag2.5 high-temperature solders, and in a vacuum formic acid atmosphere, perform integrated sintering on the frame and tungsten copper base plate, the high-current connector and frame, the upper DPC substrate and the lower DPC substrate, and the lower DPC substrate and the tungsten copper base plate. Step 2: Using nano-silver sintering paste, sinter and fix the SiC power chip to the front pads of the upper DPC substrate. Step 3: Using thick aluminum wire, ultrasonic wedge welding is used to complete the bonding and interconnection between the SiC power chip and the upper DPC substrate; Step 4: Select wide gold strips and complete the bonding and interconnection between the high-current connector and the lower DPC substrate through electronic spot welding process; Step 5: Using laser sealing welding technology, the cover plate and the frame are sealed and welded. The module cavity is filled with nitrogen or argon for protection, and the oxygen content in the cavity is controlled below 100ppm. Step 6, Post-weld inspection: After the sealing is completed, the module is subjected to airtightness testing, X-ray inspection and electrical performance testing.
[0015] More preferably, in step one, the vacuum formic acid atmosphere process conditions are as follows: the furnace cavity is first evacuated to 10... -2 Below Pa, formic acid gas is introduced, and the formic acid gas pressure inside the cavity is maintained at 100 Pa–500 Pa; after assembly, a pressure of 3 kPa is applied through one of a graphite jig, a copper jig, or a ceramic jig. 20 kPa pressure; sintering temperature 310℃-320℃, holding time 3 min-5 min, cooling rate ≤3℃ / min; In step two, the SiC power chip is sintered and fixed to the front pad of the upper DPC substrate using nano silver sintering paste. The temperature is raised to 125°C and held for 30 minutes to remove the organic carrier. The temperature is then raised to 200°C and held for 90 minutes to complete the chip sintering. The cooling rate is ≤3°C / min. Before welding, all parts are ultrasonically cleaned with organic solvents, dried, and baked to remove moisture. Air tightness testing: Leak detection was performed using a helium mass spectrometer, with a leak rate ≤ 8 × 10⁻⁶. -2 Pa·cm³ / s is acceptable; X-ray inspection: Checks the internal void rate of the weld layer, requiring a void rate of ≤1%; Electrical performance testing: The module's on-resistance, insulation withstand voltage, and leakage current parameters were tested at room temperature and 200℃, respectively.
[0016] Compared with the prior art, the beneficial effects of the present invention are: This invention uses SiC power chips, which allow for high junction temperatures. Combined with Au80Sn20, Pb92.5Sn5Ag2.5 high-temperature solder and a nano-silver sintering layer, the solder melting point is far higher than the 200℃ operating temperature. The interconnects employ ultrasonic wedge welding with thick aluminum wire and electronic spot welding with wide gold strips; the gold strips exhibit superior high-temperature oxidation resistance compared to traditional copper strips. Silicon gel potting is abandoned in favor of laser-sealed hermetic cavity encapsulation, eliminating the risk of interconnect failure caused by the expansion of potting materials at high temperatures. The entire module can operate stably at 200℃ for extended periods.
[0017] A double-layer DPC substrate is constructed by stacking an upper DPC substrate and a lower DPC substrate. Electrical connections between the layers are achieved by arrayed copper vias. The power circuits that originally required a planar arrangement are now arranged vertically, which greatly reduces the substrate area and enables module miniaturization. The copper layer of the substrate is 100μm thick, and the two layers work together to carry current, with a trace current carrying capacity of ≥20A. The chip heat can be conducted vertically downward to the tungsten copper base plate through the arrayed copper vias, creating an efficient vertical heat dissipation path and effectively reducing the chip's operating junction temperature.
[0018] The vacuum environment, combined with the reducing atmosphere of formic acid, reduces metal oxides at the welding interface and rapidly removes air bubbles from the molten solder, keeping the weld void rate below 1%, far lower than the 5% of conventional reflow soldering. A 10% void level reduces interfacial thermal resistance and improves heat dissipation; the frame, connector, double-layer substrate, and base plate are sintered in one step, reducing multiple high-temperature thermal shocks and simplifying the production process.
[0019] The SiC power chip nano-silver sintering is performed after high-temperature solder sintering at 310-320℃. The chip only undergoes one thermal cycle at 200℃, avoiding performance degradation of the nano-silver layer due to high temperature exposure. The volatilization of organic matter in the nano-silver paste will not contaminate the already completed solder interface. The chip mounting quality is not affected by the sintering process of other components, resulting in high process consistency.
[0020] The thermal expansion coefficient of the tungsten copper substrate can be adjusted to be close to that of the double-layer DPC substrate and SiC power chip, reducing thermal stress caused by temperature cycling; the waffle structure copper layer on the back of the lower DPC substrate ensures large-area thermally conductive contact and releases residual stress of the electroplated copper layer; laser sealing forms a sealed airtight cavity, isolating external high temperature, water vapor and corrosive media, protecting the internal chip and bonding structure.
[0021] The wide gold strip, combined with electronic spot welding process, enables the interconnection of high-current connectors with the underlying DPC substrate. It has strong oxidation resistance in high-temperature environments, good solder joint consistency, and avoids the increase in contact thermal resistance caused by high-temperature oxidation. Attached Figure Description
[0022] Figure 1 This is a schematic diagram of the overall integrated structure of the present invention; Figure 2 This is a top view of the integrated structure of the present invention; Figure 3 This is a cross-sectional view of the integrated structure of the present invention; Figure 4 This is a schematic diagram of the front wiring structure of the upper DPC substrate of the present invention; Figure 5 This is a schematic diagram of the back trace structure of the upper DPC substrate of the present invention; Figure 6 This is a schematic diagram of the array of through-hole structures on the surface of the upper DPC substrate of the present invention; Figure 7 This is a schematic diagram of the front wiring structure of the lower DPC substrate of the present invention; Figure 8 This is a schematic diagram of the waffle structure copper layer on the back side of the lower DPC substrate of the present invention. In the diagram: 1. Tungsten copper base plate; 2. Frame; 3. High current connector; 4. Cover plate; 5. Double-layer DPC substrate; 6. Upper DPC substrate; 7. Lower DPC substrate; 8. SiC power chip; 9. Coarse aluminum wire; 10. Wide gold strip; 11. High-temperature solder; 12. Arrayed copper vias; 13. Waffle structure copper layer. Detailed Implementation
[0023] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0024] Please see Figure 1 - Figure 8 The present invention provides a technical solution: A power module integrated structure for high-temperature environments includes a tungsten copper base plate 1, a frame 2, a high-current connector 3, a cover plate 4, a double-layer DPC substrate 5, and multiple SiC power chips 8. The double-layer DPC substrate 5 includes an upper DPC substrate 6 and a lower DPC substrate 7. The back side of the upper DPC substrate 6 and the front side of the lower DPC substrate 7 are connected by high-temperature solder 11 through stacking and sintering to form the double-layer DPC substrate 5. The frame 2 is sintered and fixed to the tungsten copper base plate 1 by high-temperature solder 11, the high-current connector 3 is sintered and fixed to the frame 2 by high-temperature solder 11, and the back of the lower DPC substrate 7 is sintered and fixed to the tungsten copper base plate 1 by high-temperature solder 11. The SiC power chip 8 is sintered and fixed to the front pads of the upper DPC substrate 6 using nano-silver sintering paste; the SiC power chip 8 and the upper DPC substrate 6 are bonded and interconnected using thick aluminum wire 9; the high-current connector 3 and the lower DPC substrate 7 are bonded and interconnected using wide gold strip 10 via electronic spot welding process; the cover plate 4 and the frame 2 are sealed and connected by laser sealing.
[0025] In this invention, the high-current connector 3 has a glass sintered hermetic structure and a rated current ≥20A.
[0026] In this invention, the copper layer trace current carrying capacity of the double-layer DPC substrate 5 is ≥20A.
[0027] In this invention, the upper DPC substrate 6 is provided with arrayed copper vias 12, and the front traces of the upper DPC substrate 6 are electrically connected by the arrayed copper vias 12 and the back traces.
[0028] In this invention, a waffle-structured copper layer 13 is provided on the back side of the lower DPC substrate 7, with a grid trench width of 0.2mm-0.5mm and a grid unit size of 3mm×5mm to 5mm×5mm.
[0029] In this invention, each SiC power chip 8 is equipped with 6 thick aluminum wires 9 with a diameter of 100μm, which are bonded to the upper DPC substrate 6 by ultrasonic wedge welding.
[0030] In this invention, the wide gold strip 10 has a width of 1000μm and a thickness of 25μm.
[0031] In this invention, the high-temperature solder 11 is selected from Au80Sn20 or Pb92.5Sn5Ag2.5 alloy solder; the copper layer thickness on the front and back sides of the upper DPC substrate 6 and the lower DPC substrate 7 is 100μm; the ceramic substrate of the upper DPC substrate 6 and the lower DPC substrate 7 is selected from aluminum nitride or alumina ceramic with a thickness of 0.38mm.
[0032] The present invention also provides an assembly process for a power module integrated structure under high temperature conditions, comprising the following steps: Step 1: Select Au80Sn20 and Pb92.5Sn5Ag2.5 high-temperature solder 11, and in a vacuum formic acid atmosphere, perform integrated sintering on the frame 2 and tungsten copper base plate 1, the high current connector 3 and frame 2, the upper DPC substrate 6 and lower DPC substrate 7, and the lower DPC substrate 7 and tungsten copper base plate 1. Step 2: Using nano-silver sintering paste, sinter and fix the SiC power chip 8 to the front pads of the upper DPC substrate 6. Step 3: Using coarse aluminum wire 9, ultrasonic wedge welding is used to complete the bonding and interconnection between the SiC power chip 8 and the upper DPC substrate 6; Step 4: Select wide gold strip 10 and complete the bonding and interconnection between high current connector 3 and lower DPC substrate 7 through electronic spot welding process; Step 5: Using laser sealing welding technology, seal and weld the cover plate 4 to the frame 2. Fill the module cavity with nitrogen or argon for protection, and control the oxygen content in the cavity to below 100ppm. Step 6, Post-weld inspection: After the sealing is completed, the module is subjected to airtightness testing, X-ray inspection and electrical performance testing.
[0033] In this invention, in step one, the vacuum formic acid atmosphere process conditions are as follows: the furnace cavity is first evacuated to 10... -2 Below Pa, formic acid gas is introduced, and the formic acid gas pressure in the cavity is maintained at 100Pa-500Pa; after assembly, a pressure of 3kPa-20kPa is applied through one of graphite jig, copper jig or ceramic jig; sintering temperature is 310℃-320℃, holding temperature is 3min-5min, and cooling rate is ≤3℃ / min. In step two, the SiC power chip 8 is sintered and fixed to the front pad of the upper DPC substrate 6 using nano silver sintering paste. The temperature is raised to 125℃ and held for 30 minutes to remove the organic carrier. The temperature is then raised to 200℃ and held for 90 minutes to complete the chip sintering. The cooling rate is ≤3℃ / min. Before welding, all parts are ultrasonically cleaned with organic solvents, dried, and baked to remove moisture. Air tightness testing: Leak detection was performed using a helium mass spectrometer, with a leak rate ≤ 8 × 10⁻⁶. -2 Pa·cm³ / s is acceptable; X-ray inspection: Checks the internal void rate of the weld layer, requiring a void rate of ≤1%; Electrical performance testing: The module's on-resistance, insulation withstand voltage, and leakage current parameters were tested at room temperature and 200℃, respectively.
[0034] Example 1: Taking a drilling three-phase full-bridge rectifier circuit module as an example, the SiC power chip 8 consists of ten SiC Schottky diodes: 6 form a three-phase full-bridge rectifier circuit, 2 are for redundancy, and 2 are for clamping protection circuits.
[0035] The double-layer DPC substrate 5 serves as the wiring layer for the power circuit. The upper DPC substrate 6 is used to arrange the cathode interconnects of the diodes, and the lower DPC substrate 7 is used to arrange the anode interconnects of the diodes. The electrical connection between the upper DPC substrate 6 and the lower DPC substrate 7 is achieved through the array of copper vias 12, thereby realizing the complete power circuit layout of the three-phase rectifier bridge within a limited substrate area.
[0036] In this embodiment, the SiC power chip 8 consists of ten SiC Schottky diodes. The cathodes of the SiC Schottky diodes are directly soldered to the upper DPC substrate 6, interconnected with the lower DPC substrate 7 through arrayed copper vias 12, and then connected to the terminals of the high-current connector 3 through wide gold strips 10. The anodes of the SiC Schottky diodes are bonded to the copper layer traces of the upper DPC substrate 6 through thick aluminum wires 9, interconnected with the lower DPC substrate 7 through arrayed copper vias 12, and then connected to the terminals of the high-current connector 3 through wide gold strips 10.
[0037] The frame 2 is sintered and fixed to the upper surface of the tungsten copper base plate 1 using Pb92.5Sn5Ag2.5 high-temperature solder 11. The high-current connector 3 is a glass-sintered hermetic structure with a rated current of 20A, and two high-current connectors 3 are provided. The high-current connector 3 is sintered and fixed to the side wall opening of the frame 2 using Au80Sn20 high-temperature solder 11.
[0038] Ten SiC power chips 8 are sintered and fixed to the front pads of the upper DPC substrate 6 using nano-silver sintering paste. The front traces of the upper DPC substrate 6 are connected to the back traces through arrayed copper vias 12. The back of the upper DPC substrate 6 is stacked and sintered with the front traces of the lower DPC substrate 7 using Pb92.5Sn5Ag2.5 high-temperature solder 11. A waffle-structured copper layer 13 is deposited on the back of the lower DPC substrate 7 and sintered and fixed to the tungsten copper base plate 1 using Pb92.5Sn5Ag2.5 high-temperature solder 11.
[0039] The three-phase AC input is introduced through two high-current connectors 3, and electrically connected to the anode or cathode of the corresponding SiC Schottky diode via traces and arrayed copper vias 12 on the upper DPC substrate 6. The rectified DC output is led out to the subsequent circuitry through two other high-current connectors 3.
[0040] The double-layer DPC substrate 5 serves as the main wiring layer for the power circuit: the upper DPC substrate 6 arranges the cathode interconnects of the SiC Schottky diodes, and the lower DPC substrate 7 arranges the anode interconnects of the SiC Schottky diodes. The electrical connection between the upper and lower layers is achieved through the array of copper vias 12, thereby realizing the complete power circuit layout of the three-phase rectifier bridge within a limited substrate area.
[0041] Each SiC power chip 8 is interconnected with the upper DPC substrate 6 by ultrasonic wedge bonding using six thick aluminum wires 9, each with a diameter of 100μm. The high-current connector 3 uses a wide gold strip 10 with a width of 1000μm and a thickness of 25μm, and is connected to the corresponding pads of the lower DPC substrate 7 by electronic spot welding.
[0042] The cover plate 4 is sealed to the upper edge of the frame 2 using laser sealing welding technology to form an airtight seal. The internal protective gas is nitrogen or argon, and the oxygen content is controlled below 100 ppm.
[0043] In this embodiment, the upper DPC substrate 6 and the lower DPC substrate 7 are fabricated using a direct copper plating ceramic substrate process, and the fabrication process is as follows: First, aluminum nitride (AlN) or alumina (Al2O3) ceramic blanks are selected as the insulating substrate, with a thickness of 0.38 mm. Through-hole arrays are formed on the substrate using laser drilling or mechanical drilling processes, with through-hole diameters of 0.1 mm.
[0044] Secondly, a titanium / copper seed layer (Ti / Cu) with a thickness of 0.1μm-0.3μm is deposited on the surface of the ceramic substrate and the inner wall of the through hole using a magnetron sputtering process, which serves as a conductive seed layer for subsequent electroplating.
[0045] Then, the circuit pattern is formed through photolithography processes such as development and exposure, and the copper layer is thickened to the required thickness using electroplating. In this embodiment, the copper layer thickness on both sides of the upper DPC substrate 6 and the lower DPC substrate 7 is 100μm to ensure that the current carrying capacity of the traces is ≥20A. During the electroplating process, copper layers are deposited simultaneously on the inner walls of the vias to form an array of copper vias 12, realizing the electrical connection between the traces on the front and back sides of the substrate.
[0046] Finally, the electroplated copper circuit undergoes surface treatment using a thin palladium plating process to form a palladium layer (thickness: palladium layer ≥ 0.05 μm, gold layer ≥ 0.05 μm) on the copper surface to improve its solderability, oxidation resistance, and corrosion resistance.
[0047] The back side of the lower DPC substrate 7 employs a waffle-structured copper layer 13 with a thickness of 100 μm. The waffle-structured copper layer 13 is divided into a regular array of crisscrossing trenches, with trench widths ranging from 0.2 mm to 0.5 mm, lengths from 3 mm to 5 mm, and a width of 5 mm. This structure ensures large-area thermally conductive contact with the tungsten-copper base plate 1, while also releasing residual stress from high-temperature welding through the design of the waffle-structured copper layer 13, thus enhancing the weld bond strength.
[0048] The tungsten copper base plate 1 is made of WuCu material, and its CTE matches that of the ceramic substrate. Its surface is subjected to chemical nickel plating and gold plating in sequence. The nickel layer thickness is 3μm-5μm and the gold layer thickness is 0.05μm-0.1μm to improve its wettability and bonding strength with the high-temperature solder 11.
[0049] The frame 2 is made of Kovar alloy (Fe-29Ni-17Co), and its CTE matches that of the tungsten copper base plate 1. The surface of the frame 2 is also plated with nickel / gold, with a nickel layer thickness of 3μm-5μm and a gold layer thickness of 0.05μm-0.1μm.
[0050] The high-current connector 3 features a glass-sintered hermetic structure, with a hermetic seal formed between its metal outer conductor and the glass insulator. Both the inner and outer leads of the high-current connector 3 are made with 2.1mm thick terminals, with nickel / gold plating, and a rated current ≥20A.
[0051] Example 2: An assembly process for a power module integrated structure under high temperature conditions, comprising the following steps: Step 1: Select Au80Sn20 and Pb92.5Sn5Ag2.5 high-temperature solder 11, and in a vacuum formic acid atmosphere, perform integrated sintering on the frame 2 and tungsten copper base plate 1, the high current connector 3 and frame 2, the upper DPC substrate 6 and lower DPC substrate 7, and the lower DPC substrate 7 and tungsten copper base plate 1. Before welding, the tungsten copper base plate 1, frame 2, upper DPC substrate 6, and lower DPC substrate 7 are sequentially ultrasonically cleaned in anhydrous ethanol or isopropanol for 5-10 minutes to remove surface oil and particulate contaminants. After cleaning, they are dried in a nitrogen stream and then baked in an oven at 120℃-150℃ for 2-4 hours to completely remove moisture.
[0052] Specifically, Pb92.5Sn5Ag2.5 and Au80Sn20 alloy solder preforms (30μm-50μm thick) are pre-placed on the welding surfaces of each component to be welded. After assembly in the order of assembly, a pressure of 3kPa-20kPa is applied using graphite, copper blocks, or ceramic sheet jigs. The assembly is then placed in a vacuum welding furnace, and the furnace chamber is first evacuated to 10 kPa. - Below 2 Pa, formic acid gas (HCOOH) is then introduced into the furnace cavity to maintain the formic acid atmosphere pressure within the cavity at 100 Pa–500 Pa. The temperature is then increased to 310–320 °C at a heating rate of 5–10 °C / min and held for 3–5 minutes. During this process, the formic acid gas decomposes under heating conditions, and its reduction products reduce the metal oxides at the welding interface to pure metal, achieving low-void welding. The vacuum environment inhibits secondary oxidation of the metal surface and rapidly removes bubbles escaping from the molten solder, effectively reducing the void ratio of the weld layer. After holding at this temperature, the furnace is slowly cooled to below 150 °C at a rate not exceeding 3 °C / min, and then allowed to cool naturally to room temperature.
[0053] The integrated sintering process completes all the high-temperature welding of the frame 2, high-current connector 3, double-layer DPC substrate 5 and tungsten copper base plate 1 in the same vacuum formic acid atmosphere in one go, which reduces the thermal shock to the materials caused by multiple heatings, and avoids the problem of secondary melting and interface aging of the welded interfaces in subsequent high-temperature processes when each component is sintered separately.
[0054] Step 2: Using nano-silver sintering paste, sinter and fix the SiC power chip 8 to the front pads of the upper DPC substrate 6. Nano-silver sintering paste with a thickness of 30μm-50μm is applied to the front pads of the upper DPC substrate 6. After the SiC power chip 8 is mounted on the pads, it is placed in a vacuum soldering furnace, and the furnace chamber is evacuated to 10°C. -2 Below Pa, the temperature is increased to 125℃ at a rate of 5℃ / min-10℃ / min, and held for 30 minutes to pre-burn off the organic carrier, allowing it to fully volatilize. The temperature is then increased to 200℃ and held for 90 minutes to complete sintering. After holding, the temperature is slowly cooled to below 150℃ at a rate not exceeding 3℃ / min, and then allowed to cool naturally to room temperature in the furnace. The sintered silver layer has a melting point of approximately 960℃ and exhibits excellent thermal conductivity, electrical conductivity, and high-temperature reliability.
[0055] The advantage of placing the SiC power chip sintering step as the final process step is: (1) The SiC power chip 8 only needs to undergo a sintering 200℃ thermal cycle once, avoiding the silver layer densification or interface thermal stress damage that may occur when sintering first and then undergoing high temperature solder 11 at 310℃-320℃. (2) The volatile products of the organic carrier in the nano silver paste during the sintering process will not cause contamination to the completed welding interface; (3) The SiC power chip mounting quality is not affected by the sintering process of other components, resulting in better process consistency.
[0056] Step 3: Using coarse aluminum wire 9, ultrasonic wedge welding is used to complete the bonding and interconnection between the SiC power chip 8 and the upper DPC substrate 6; A coarse aluminum wire wedge bonding device is used to bond the pads of the SiC power chip 8 to the corresponding pads of the upper DPC substrate 6 using a coarse aluminum wire 9 with a diameter of 100μm.
[0057] Step 4: Select wide gold strip 10 and complete the bonding and interconnection between high current connector 3 and lower DPC substrate 7 through electronic spot welding process; Using electronic spot welding equipment, a wide gold strip 10 with a width of 1000μm and a thickness of 25μm is used to spot weld the inner leads of the high-current connector 3 to the corresponding pads of the lower DPC substrate 7.
[0058] Step 5: Using laser sealing welding technology, seal and weld the cover plate 4 to the frame 2. Fill the module cavity with nitrogen or argon for protection, and control the oxygen content in the cavity to below 100ppm. Cover plate 4 is placed over the cover plate protrusion of frame 2, and continuous laser welding is performed along the upper edge of frame 2 using laser sealing equipment. The internal shielding gas is nitrogen, and the oxygen content in the welding chamber is controlled below 100ppm. After laser sealing, an airtight sealed cavity is formed inside the module, effectively protecting the internal chips and interconnect structures from external high temperature, high humidity, and corrosive gases.
[0059] Step 6, Post-weld inspection: After the sealing is completed, the module is subjected to airtightness testing, X-ray inspection and electrical performance testing.
[0060] After the sealing process is completed, the module undergoes the following inspections: (1) Air tightness test: Leak detection was performed using a helium mass spectrometer, with a leak rate ≤8×10 -2 Pa·cm³ / s is acceptable; (2) X-ray inspection: Check the void rate inside the weld layer, requiring a void rate ≤1%; (3) Electrical performance test: The on-resistance, insulation withstand voltage and leakage current of the module were tested at room temperature and 200℃ respectively to ensure that the design specifications are met.
[0061] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above, and that the invention can be implemented in other specific forms without departing from its spirit or essential characteristics. Therefore, the embodiments should be considered illustrative and non-limiting in all respects, and the scope of the invention is defined by the appended claims rather than the foregoing description. Thus, all variations falling within the meaning and scope of equivalents of the claims are intended to be included within the present invention, and no reference numerals in the claims should be construed as limiting the scope of the claims.
[0062] The above description is only a preferred embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any equivalent substitutions or modifications made by those skilled in the art within the scope of the technology disclosed in the present invention, based on the technical solution and inventive concept of the present invention, should be covered within the scope of protection of the present invention.
Claims
1. A power module integrated structure for high-temperature environments, characterized in that, It includes a tungsten copper base plate (1), a frame (2), a high-current connector (3), a cover plate (4), a double-layer DPC substrate (5), and multiple SiC power chips (8). The double-layer DPC substrate (5) includes an upper DPC substrate (6) and a lower DPC substrate (7). The back side of the upper DPC substrate (6) and the front side of the lower DPC substrate (7) are connected by high-temperature solder (11) to form a double-layer DPC substrate (5). The frame (2) is sintered and fixed on the tungsten copper base plate (1) by high-temperature solder (11), the high-current connector (3) is sintered and fixed on the frame (2) by high-temperature solder (11), and the back of the lower DPC substrate (7) is sintered and fixed on the tungsten copper base plate (1) by high-temperature solder (11). The SiC power chip (8) is sintered and fixed to the front pad of the upper DPC substrate (6) by nano-silver sintering paste; the SiC power chip (8) and the upper DPC substrate (6) are bonded and interconnected by thick aluminum wire (9); the high current connector (3) and the lower DPC substrate (7) are bonded and interconnected by wide gold strip (10) through electronic spot welding process; the cover plate (4) and the frame (2) are sealed and connected by laser sealing.
2. The power module integration structure under high temperature environment according to claim 1, characterized in that, The high-current connector (3) has a glass sintered hermetically sealed structure and a rated current ≥20A.
3. The power module integration structure under high temperature environment according to claim 1, characterized in that, The copper layer trace current carrying capacity of the double-layer DPC substrate (5) is ≥20A.
4. The power module integration structure under high temperature environment according to claim 1, characterized in that, The upper DPC substrate (6) is provided with an array of copper vias (12), and the front traces of the upper DPC substrate (6) are electrically connected by the array of copper vias (12) and the back traces.
5. The power module integration structure under high temperature environment according to claim 1, characterized in that, The lower DPC substrate (7) has a waffle-structured copper layer (13) on its back side, with a grid trench width of 0.2mm-0.5mm and a grid unit size of 3mm×5mm to 5mm×5mm.
6. The power module integration structure under high temperature environment according to claim 1, characterized in that, Each SiC power chip (8) is equipped with 6 thick aluminum wires (9) with a diameter of 100μm, which are bonded to the upper DPC substrate (6) by ultrasonic wedge welding.
7. The power module integration structure under high temperature environment according to claim 1, characterized in that, The wide gold strip (10) has a width of 1000 μm and a thickness of 25 μm.
8. The power module integration structure under high temperature environment according to claim 1, characterized in that, The high-temperature solder (11) is selected from Au80Sn20 or Pb92.5Sn5Ag2.5 alloy solder; the copper layer thickness on the front and back of the upper DPC substrate (6) and the lower DPC substrate (7) is 100μm; the ceramic substrate of the upper DPC substrate (6) and the lower DPC substrate (7) is selected from aluminum nitride or alumina ceramic with a thickness of 0.38mm.
9. An assembly process for a power module integrated structure under high temperature conditions, characterized in that, It includes the following steps: Step 1: Select Au80Sn20 and Pb92.5Sn5Ag2.5 high-temperature solder (11), and in a vacuum formic acid atmosphere, perform integrated sintering on the frame (2) and tungsten copper base plate (1), high current connector (3) and frame (2), upper DPC substrate (6) and lower DPC substrate (7) and lower DPC substrate (7) and tungsten copper base plate (1); Step 2: Using nano-silver sintering paste, sinter and fix the SiC power chip (8) to the front pad of the upper DPC substrate (6); Step 3: Using coarse aluminum wire (9), ultrasonic wedge welding is used to complete the bonding interconnection between the SiC power chip (8) and the upper DPC substrate (6); Step 4: Select a wide gold strip (10) and complete the bonding and interconnection between the high current connector (3) and the lower DPC substrate (7) through electronic spot welding process; Step 5: Using laser sealing welding process, seal the cover plate (4) and the frame (2) together. Fill the module cavity with nitrogen or argon for protection and control the oxygen content in the cavity to below 100ppm. Step 6, Post-weld inspection: After the sealing is completed, the module is subjected to airtightness testing, X-ray inspection and electrical performance testing.
10. The assembly process of a power module integrated structure under high temperature environment according to claim 9, characterized in that, In step one, the vacuum formic acid atmosphere process conditions are as follows: the furnace cavity is first evacuated to 10... -2 Below Pa, formic acid gas is introduced, and the formic acid gas pressure in the cavity is maintained at 100Pa-500Pa; after assembly, a pressure of 3kPa-20kPa is applied through one of graphite jig, copper jig or ceramic jig; sintering temperature is 310℃-320℃, holding temperature is 3min-5min, and cooling rate is ≤3℃ / min. In step two, the SiC power chip (8) is sintered and fixed to the front pad of the upper DPC substrate (6) using nano silver sintering paste. The temperature is raised to 125°C and held for 30 minutes to remove the organic carrier. The temperature is then raised to 200°C and held for 90 minutes to complete the chip sintering. The cooling rate is ≤3°C / min. Before welding, all parts are ultrasonically cleaned with organic solvents, dried, and baked to remove moisture. Air tightness testing: Leak detection was performed using a helium mass spectrometer, with a leak rate ≤ 8 × 10⁻⁶. -2 Pa·cm³ / s is acceptable; X-ray inspection: Checks the internal void rate of the weld layer, requiring a void rate of ≤1%; Electrical performance testing: The module's on-resistance, insulation withstand voltage, and leakage current parameters were tested at room temperature and 200℃, respectively.