Solder paste and method for producing a bonded body
By using a solder paste with a first solder alloy powder of Sn, Ag and In and a second solder alloy powder of Sn, Ag and Cu, the failure mode and high-speed shear strength of the solder joint were optimized, the problems of unmelted solder alloy powder and difficult-to-control properties were solved, and the stability and strength of the solder were improved.
Patent Information
- Application Number
- CN202580031278.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-05-24
- Filing Date
- 2025-04-25
- Publication Date
- 2026-11-24
AI Technical Summary
In existing solder pastes, the unmelted phenomenon of solder alloy powder and the characteristics of solder joints are difficult to control during multiple heating processes, resulting in easy breakage of solder joints, difficulty in predicting characteristic differences, and difficulty in optimizing the failure mode and high-speed shear strength of solder joints.
Solder paste containing a first solder alloy powder of Sn, Ag and In and a second solder alloy powder of Sn, Ag and Cu is used. By controlling the mixing ratio of the two and the composition of the flux, the failure mode and high-speed shear strength of the solder joint are optimized.
It improves the meltability of solder paste, optimizes the failure mode and high-speed shear strength of solder joints, and enhances the reliability and stability of welding.
Smart Images

Figure FT_1 
Figure FT_2 
Figure SMS_1
Abstract
Description
Technical Field
[0001] This invention relates to solder paste and a method for preparing a bonding agent.
[0002] This application claims priority based on Japanese Patent Application No. 2024-085077, filed in Japan on May 24, 2024, the contents of which are incorporated herein by reference. Background Technology
[0003] In the electronics industry, the miniaturization of components continues to advance with the increasing use of System-in-Package (SiP) designs for electronic devices. SiP is a type of integrated circuit that uses a high-density mounting technology to achieve large-capacity memory and multifunctionality by stacking multiple ICs or packages.
[0004] This SiP is applied in various fields such as smartphones, tablet PCs, digital cameras, automotive electronic devices, medical devices, and IoT (Internet of Things) devices.
[0005] In SiP design, multiple components need to be interconnected into a single assembly, sometimes requiring soldering with multiple heating steps. When performing multi-stage soldering interconnects with multiple heating steps, solders with different liquidus temperatures are needed to prevent the solder that molten in previous heating steps from remelting in subsequent heating steps.
[0006] Generally, SnAgCu solder is used for the initial soldering connections. SnAgCu solder, widely used as a lead-free solder, has a liquidus temperature that is further towards a higher temperature than that of SnPb eutectic solder. Therefore, in subsequent soldering stages, the liquidus temperature of the solder needs to be set lower than that of the SnAgCu solder.
[0007] Low-temperature solders, also known as Sn-Bi-based lead-free solders, are characterized by their low liquidus temperature. However, Sn-Bi-based lead-free solders are brittle due to their high Bi content, which is a typical alloy composition. Furthermore, their low melting temperature results in poor reliability against thermal fatigue.
[0008] In contrast, conventionally, solder pastes with two or more different compositions of solder alloy powders, in which one solder alloy powder has a lower liquidus temperature than the other solder alloy powder, are used, as are methods for forming components using the solder paste and methods for forming solder joints using the solder paste (for example, see Patent Document 1).
[0009] Existing technical documents Patent documents Patent Document 1: International Publication No. 2020 / 227638 Summary of the Invention The problem to be solved by the present invention As electronic components continue to become smaller and more functional, there is a need to further improve the performance of traditional solder pastes.
[0010] However, as mentioned above, solder pastes using solder alloy powders with different liquidus temperatures may experience incomplete melting of the solder alloy powders depending on the heating conditions. Furthermore, in such solder pastes, due to the different characteristics of each solder alloy powder, it is difficult to control the characteristics of the resulting solder joint (failure mode, high-speed shear strength, etc.), and it is also difficult to predict the differences in characteristics resulting from the combination of solder alloy powders.
[0011] In particular, simply increasing the mechanical strength of the solder alloy causes stress concentration at the joint interface, which can easily lead to fracture at the joint interface. This can sometimes be the most undesirable failure mode for solder joints.
[0012] Therefore, the inventors aimed to evaluate solder alloys under more stringent conditions than those typically used in mechanical strength testing, conducting shear strength tests (high-speed shear tests) at a much higher speed than before. This evaluation differs significantly from previous shear strength test conditions, enabling the identification of the failure mode that causes the solder joint to fracture instantaneously.
[0013] The present invention was made in view of the above circumstances, and provides a solder paste and a method for preparing a joint using the solder paste, wherein the solder paste can improve the meltability of the solder paste and optimize the failure mode and high-speed shear strength.
[0014] Problem-solving methods To address the aforementioned issues, the present invention employs the following configuration.
[0015] [1] A solder paste comprising a first solder alloy powder, a second solder alloy powder and a flux, wherein the first solder alloy powder is a powder of an alloy containing Sn, Ag and In and having an Ag content of 3.9% by mass or more, and the second solder alloy powder is a powder of an alloy containing Sn, Ag and Cu.
[0016] [2] According to the solder paste of [1], wherein the mixing ratio of the first solder alloy powder and the second solder alloy powder is: the first solder alloy powder is 45 parts by mass or more and 65 parts by mass or less, and the second solder alloy powder is 35 parts by mass or more and 55 parts by mass or less.
[0017] [3] According to the solder paste of [2], wherein the mixing ratio of the first solder alloy powder and the second solder alloy powder is: the first solder alloy powder is more than 50 parts by mass and less than 65 parts by mass, and the second solder alloy powder is more than 35 parts by mass and less than 50 parts by mass.
[0018] [4] The solder paste according to any one of [1] to [3], wherein the content of Ag in the first solder alloy powder is 3.9% by mass or more and 4.5% by mass or less, the content of In is 18% by mass or more and 22% by mass or less, and the balance is Sn.
[0019] [5] The solder paste according to any one of [1] to [4], wherein the content of Ag in the second solder alloy powder is 2.9% by mass or more and 4% by mass or less, the content of Cu is 0.3% by mass or more and 1% by mass or less, and the balance is Sn.
[0020] [6] The solder paste according to any one of [1] to [5], wherein the mass ratio of In / Ag in the first solder alloy powder is 4 or more and 5.5 or less.
[0021] [7] A method for preparing a joint, comprising a step of obtaining the joint by welding, wherein, during the welding, the solder paste described in any one of [1] to [6] is used for heating.
[0022] In addition, unless otherwise specified, the percentage of alloy composition expressed in this specification is "mass %". The solidus temperature and liquidus temperature of the alloy are temperatures measured by differential thermal analysis. The average particle size of the first solder alloy powder and the average particle size of the second solder alloy powder are average particle sizes relative to the volume basis of each solder alloy particle group.
[0023] The failure modes of solder joints include failure of the solder itself (solder block) at the joint, peeling failure at the interface between the solder block and the intermetallic compound (IMC), and peeling failure at the IMC interface.
[0024] The IMC interface (bonding interface) is bonded to the electrode, making it difficult to mitigate stress at the bonding interface. However, physical and electrical loads are primarily applied to the bonding interface of the solder joint. Therefore, it is believed that stress mitigation using a more easily deformable bulk material can suppress failure.
[0025] The failure modes of the aforementioned solder joints were evaluated through high-speed shear tests.
[0026] Effects of the present invention According to the present invention, a solder paste and a method for preparing a joint using the solder paste are provided, wherein the solder paste can improve the meltability of the solder paste and optimize the failure mode and high-speed shear strength. Attached Figure Description
[0027] Figure 1 It is a graph representing the reflow soldering curve in the evaluation of solder paste melt properties.
[0028] Figure 2 This is a diagram representing the evaluation criteria in the evaluation of solder paste fusibility. Detailed Implementation
[0029] (Solder paste) One embodiment of the solder paste is a solder paste containing a first solder alloy powder, a second solder alloy powder, and a flux.
[0030] In the solder paste of this embodiment, the first solder alloy powder is a powder containing Sn, Ag, and In, with the Ag content being 3.9% by mass or more. The second solder alloy powder is a powder containing an alloy containing Sn, Ag, and Cu.
[0031] The solder paste of this embodiment is suitable for soldering applications from low to medium temperatures (150~210°C), for example, for soldering at temperatures where the peak soldering temperature is lower than the peak temperature when Sn-Ag-Cu solder is heated.
[0032] In the solder paste of this embodiment, a first solder alloy powder and a second solder alloy powder with different liquidus temperatures are used. The first solder alloy powder containing In has a relatively lower liquidus temperature compared to the second solder alloy powder containing Sn, Ag, and Cu.
[0033] When using solder paste with such an embodiment, it can be designed to be heated at a peak temperature that is lower than the solidus temperature of the second solder alloy powder and higher than the liquidus temperature of the first solder alloy powder.
[0034] <First Solder Alloy Powder> In the solder paste of this embodiment, the first solder alloy powder is an alloy powder containing Sn, Ag and In.
[0035] The Ag content relative to the total mass of the first solder alloy powder is 3.9% by mass or more, which can be 3.9% by mass or more and less than 5% by mass, or 3.9% by mass or more and less than 4.5% by mass. For example, the Ag content can be 3.9% by mass, 4% by mass, or 4.5% by mass.
[0036] The In content relative to the total mass of the first solder alloy powder can be, for example, 18% by mass or more, 18% by mass or more and 25% by mass or less, or 18% by mass or more and 22% by mass or less. For example, the In content can be 19% by mass, 20% by mass, or 21% by mass.
[0037] The Sn content is the balance relative to the total mass of the first solder alloy powder, and can also be 90% or more by mass.
[0038] The alloy constituting the first solder alloy powder may also contain metallic elements other than Sn, Ag, and In. Examples of metallic elements other than Sn, Ag, and In include Cu, Ni, Bi, Ge, P, Co, Ga, Zn, Sb, Pb, Au, Al, Pt, Pd, Fe, Mn, Zr, and As. Furthermore, the first solder alloy powder may also contain unavoidable impurities.
[0039] The solder paste of this embodiment may also contain two or more first solder alloy powders with different alloy compositions and particle sizes.
[0040] The preferred first solder alloy powder is an alloy powder containing Sn, Ag, and In, wherein the content of Ag is 3.9% by mass or more and 4.5% by mass or less, and the content of In is 18% by mass or more and 22% by mass or less; a more preferred first solder alloy powder is a Sn-Ag-In alloy powder containing 3.9% by mass or more and 4.5% by mass or less, the content of In is 18% by mass or more and 22% by mass or less, and the balance is Sn.
[0041] In the first solder alloy powder, the mass ratio of In / Ag is preferably 4 or more and 5.5 or less, and can be 4.2 or more and 5.4 or less, or 4.4 or more and 5.2 or less.
[0042] When the mass ratio of In / Ag is above the lower limit of the above-mentioned preferred range, it can prevent the solder itself (solder block) at the joint from having excessively high bulk strength, and it is easier to control the failure mode in a more suitable state.
[0043] Furthermore, when the mass ratio of In / Ag is above the lower limit of the aforementioned preferred range, it is possible to prevent the solder itself (solder block) at the joint from generating excessively high shear strength, making it easier to obtain a suitable shear strength. On the other hand, when it is below the upper limit of the aforementioned preferred range, it is possible to prevent a significant decrease in joint strength, making it easier to obtain the target high-speed shear strength.
[0044] The solidus temperature of the first solder alloy powder is, for example, above 135°C and below 150°C, or above 140°C and below 145°C.
[0045] The liquidus temperature of the first solder alloy powder may be, for example, above 180°C and below 200°C, or above 190°C and below 200°C.
[0046] There are no particular restrictions on the particle size of the first solder alloy powder, as long as it is the same particle size as that used in conventional solder paste. When it has a particle size distribution that conforms to symbols 1 to 8 in the powder size classification (Table 2) of JIS Z3284-1:2014, it can be used to solder fine components. For example, the average particle size of the first solder alloy powder is 1 μm or more and 1000 μm or less.
[0047] The average particle size of the first solder alloy powder here refers to the particle size at which the cumulative value in the particle size distribution measured by a laser diffraction scattering particle size distribution measuring device is 50%.
[0048] <Second Solder Alloy Powder> In the solder paste of this embodiment, the second solder alloy powder is a powder containing an alloy of Sn, Ag and Cu.
[0049] The Ag content relative to the total mass of the second solder alloy powder can be, for example, 2.9% by mass or more and 4% by mass or less, or 3% by mass or more and 4% by mass or less. For example, the Ag content can be 2.9% by mass, 3% by mass, 3.2% by mass, 3.5% by mass, or 4% by mass.
[0050] The Cu content relative to the total mass of the second solder alloy powder can be, for example, 0.3% by mass or more and 1.5% by mass, 0.3% by mass or more and 1% by mass, or 0.3% by mass or more and 0.7% by mass. For example, the Cu content can be 0.3% by mass, 0.5% by mass, 0.7% by mass, 0.75% by mass, 0.8% by mass, or 0.9% by mass.
[0051] The Sn content is the balance relative to the total mass of the second solder alloy powder, and can be above 90% by mass.
[0052] The alloy constituting the second solder alloy powder may also contain metallic elements other than Sn, Ag, and Cu. Examples of metallic elements other than Sn, Ag, and Cu include Ni, Bi, In, Ge, P, Co, Ga, Zn, Sb, Pb, Au, Al, Pt, Pd, Fe, Mn, Zr, and As. Additionally, the second solder alloy powder may contain unavoidable impurities.
[0053] The solder paste of this embodiment may also contain two or more second solder alloy powders with different alloy compositions and particle sizes.
[0054] The preferred second solder alloy powder is an alloy powder containing Sn, Ag, and Cu, wherein the content of Ag is 2.9% by mass or more and 4% by mass or less, and the content of Cu is 0.3% by mass or more and 1% by mass or less; the more preferred second solder alloy powder is a Sn-Ag-Cu alloy powder containing 3% by mass or more and 4% by mass or less, the content of Cu is 0.3% by mass or more and 0.7% by mass or less, and the balance being Sn.
[0055] In the second solder alloy powder, the mass ratio of Ag / Cu is preferably 10 or less, but can be 3 or more and 9 or less, 5 or more and 8.5 or less, or 6 or more and 8 or less.
[0056] When the mass ratio of Ag / Cu is within the above range, it is easy to improve the meltability of the solder paste. In addition, it is easy to simultaneously optimize the failure mode and high-speed shear strength.
[0057] The solidus temperature of the second solder alloy powder is, for example, above 205°C and below 225°C, or above 210°C and below 220°C.
[0058] The liquidus temperature of the second solder alloy powder is, for example, above 215°C and below 235°C, or above 215°C and below 230°C.
[0059] There are no particular restrictions on the particle size of the second solder alloy powder, as long as it is of the same particle size as that used in conventional solder paste. When it has a particle size distribution that conforms to symbols 1 to 8 in the powder size classification (Table 2) of JIS Z3284-1:2014, it can be used to solder fine components. For example, the average particle size of the second solder alloy powder is 1 μm or more and 1000 μm or less.
[0060] The average particle size of the second solder alloy powder here refers to the particle size at which the cumulative value in the particle size distribution measured by a laser diffraction scattering particle size distribution measuring device is 50%.
[0061] Mixing ratio of the first solder alloy powder and the second solder alloy powder In the solder paste of this embodiment, the mixing ratio of the first solder alloy powder and the second solder alloy powder is: the first solder alloy powder is 45 parts by mass or more and 65 parts by mass or less, and the second solder alloy powder is 35 parts by mass or more and 55 parts by mass or less.
[0062] From the perspective of optimizing the failure mode and high-speed shear strength, the mixing ratio of the two is preferably 50 parts by mass and 65 parts by mass of the first solder alloy powder and 35 parts by mass and 50 parts by mass of the second solder alloy powder. More preferably, the first solder alloy powder is more than 50 parts by mass and 65 parts by mass of the first solder alloy powder and 35 parts by mass and less than 50 parts by mass of the second solder alloy powder. Further preferably, the first solder alloy powder is 55 parts by mass and 65 parts by mass of the first solder alloy powder and 35 parts by mass and 45 parts by mass of the second solder alloy powder. Even more preferably, the first solder alloy powder is 60 parts by mass and 65 parts by mass of the first solder alloy powder and 35 parts by mass and 40 parts by mass of the second solder alloy powder.
[0063] Flux In the solder paste of this embodiment, there are no particular limitations on the flux. For example, it may contain rosin, solvent, activator, thixotropic agent, etc. as resin components.
[0064] Examples of active agents include organic acids, halogen compounds, and amine compounds.
[0065] Examples of thixotropic agents include ester-based thixotropic agents, amide-based thixotropic agents, sorbitol-based thixotropic agents, and cellulose nanofibers.
[0066] In the solder paste of this embodiment, the flux content is preferably 5% or more and 30% or less by mass relative to the total mass of the solder paste, more preferably 5% or more and 15% or less by mass; the total content of the first solder alloy powder and the second solder alloy powder is preferably 70% or more and 95% or less by mass relative to the total mass of the solder paste, more preferably 85% or more and 95% or less by mass.
[0067] In the solder paste of this embodiment, there may be any metal powder that is different from the first solder alloy powder and the second solder alloy powder. There are no restrictions on the composition of this metal powder; examples of metals that may be included include Sn, Ag, Cu, In, Bi, Ni, Ge, P, Co, Ga, Zn, Sb, Pb, Au, Al, Pt, Pd, Fe, Mn, Zr, and As. One or more of these metals may be included.
[0068] Metal powder can also be two or more powders with different compositions and particle sizes.
[0069] Furthermore, the surface of the metal powder can be plated with a metal different from the metal constituting the metal powder, and it can also contain resin powder or carbon fiber. For example, plastic powder can be used as resin powder, and carbon fiber can be used as carbon fiber. The resin powder or carbon fiber can also be two or more powders with different compositions or particle sizes. In addition, the resin powder or carbon fiber can also be plated with metal on its surface.
[0070] As explained above, the solder paste of this embodiment contains a first solder alloy powder and a second solder alloy powder having a specific alloy composition, and a flux.
[0071] The first solder alloy powder is a powder containing Sn, Ag, and In, with the Ag content being 3.9% by mass or more. By containing In, the peak soldering temperature can be reduced. Furthermore, unlike brittle Bi, the use of In improves melt permeability while preventing the solder block strength from becoming excessive. Since the Ag content is 3.9% by mass or more, the strength of the solder block at the joint is increased.
[0072] Furthermore, by using a second solder alloy powder containing Sn, Ag, and Cu with different liquidus temperatures and the aforementioned first solder alloy powder, the solder alloys exhibit good melting properties when heated.
[0073] Therefore, the solder paste according to this embodiment can improve the meltability of the solder paste and optimize the failure mode and high-speed shear strength.
[0074] The preferred mixing ratio of the first solder alloy powder and the second solder alloy powder is: 45 parts by mass or more and 65 parts by mass or less of the first solder alloy powder, and 35 parts by mass or more and 55 parts by mass or less of the second solder alloy powder. By controlling the mixing ratio of the two within the above-mentioned preferred range, the characteristics of both the first solder alloy powder and the second solder alloy powder can be fully utilized.
[0075] A more preferred mixing ratio of the first solder alloy powder and the second solder alloy powder is: more than 50 parts by mass and less than 65 parts by mass of the first solder alloy powder, and more than 35 parts by mass and less than 50 parts by mass of the second solder alloy powder. By controlling the mixing ratio of the two within the above-mentioned more preferred range, the meltability of the solder paste is improved, and the optimization of the failure mode and high-speed shear strength of the solder joint is easily achieved.
[0076] When soldering using the solder paste of this embodiment, for example, during heating, the first solder alloy powder with a lower solidus temperature melts first. Simultaneously, the second solder alloy powder with a relatively higher solidus temperature can partially or completely melt within the alloy (first solder alloy powder) that has been molten by heating. The solder joint produced in this way achieves optimized failure modes and high-speed shear strength.
[0077] The solder paste is preferably composed of a first solder alloy powder, a second solder alloy powder, and a flux. The first solder alloy powder is an alloy powder containing Sn, Ag, and In, with the Ag content being 3.9% by mass or more. The second solder alloy powder is an alloy powder containing Sn, Ag, and Cu. The mixing ratio of the first solder alloy powder and the second solder alloy powder is: the first solder alloy powder is 45 parts by mass or more and 65 parts by mass or less, and the second solder alloy powder is 35 parts by mass or more and 55 parts by mass or less.
[0078] Another preferred embodiment of the solder paste is a solder paste composed of a first solder alloy powder, a second solder alloy powder, and a flux. The first solder alloy powder is an alloy powder containing Sn, Ag, and In, with Ag content of 3.9% by mass or more and 4.5% by mass or less, In content of 18% by mass or more and 22% by mass or less, and the balance being Sn. The second solder alloy powder is an alloy powder containing Sn, Ag, and Cu, with Ag content of 2.9% by mass or more and 4% by mass or less, Cu content of 0.3% by mass or more and 1% by mass or less, and the balance being Sn. The mixing ratio of the first solder alloy powder and the second solder alloy powder is: the first solder alloy powder is 45% by mass or more and 65% by mass or less, and the second solder alloy powder is 35% by mass or more and 55% by mass or less.
[0079] Another preferred embodiment of the solder paste is a solder paste composed of a first solder alloy powder, a second solder alloy powder, and a flux. The first solder alloy powder is an alloy powder containing Sn, Ag, and In, with Ag content of 3.9% by mass or more and 4.5% by mass or less, In content of 18% by mass or more and 22% by mass or less, the balance being Sn, and the mass ratio of In / Ag in the first solder alloy powder being 4% by mass or more and 5.5% by mass or less. The second solder alloy powder is an alloy powder containing Sn, Ag, and Cu, with Ag content of 2.9% by mass or more and 4% by mass or less, Cu content of 0.3% by mass or more and 1% by mass or less, the balance being Sn. The mixing ratio of the first solder alloy powder and the second solder alloy powder is: the first solder alloy powder is 45 parts by mass or more and 65 parts by mass or less, and the second solder alloy powder is 35 parts by mass or more and 55 parts by mass or less.
[0080] Another preferred embodiment of the solder paste is a solder paste composed of a first solder alloy powder, a second solder alloy powder, and a flux, wherein the first solder alloy powder is a Sn-Ag-In alloy powder with an Ag content of 3.9% to 4.5% by mass, an In content of 18% to 22% by mass, and the balance being Sn; the second solder alloy powder is a Sn-Ag-Cu alloy powder with an Ag content of 3% to 4% by mass, a Cu content of 0.3% to 0.7% by mass, and the balance being Sn; and the mixing ratio of the first solder alloy powder and the second solder alloy powder is: the first solder alloy powder is 45 parts by mass to 65 parts by mass, and the second solder alloy powder is 35 parts by mass to 55 parts by mass.
[0081] Another preferred embodiment of the solder paste is a solder paste composed of a first solder alloy powder, a second solder alloy powder, and a flux. The first solder alloy powder is a Sn-Ag-In alloy powder with an Ag content of 3.9% to 4.5% by mass, an In content of 18% to 22% by mass, and the balance being Sn, and the In / Ag mass ratio of the first solder alloy powder is 4 to 5.5. The second solder alloy powder is a Sn-Ag-Cu alloy powder with an Ag content of 3% to 4% by mass, a Cu content of 0.3% to 0.7% by mass, and the balance being Sn. The mixing ratio of the first solder alloy powder and the second solder alloy powder is: the first solder alloy powder is 45% to 65% by mass, and the second solder alloy powder is 35% to 55% by mass.
[0082] (Preparation method of the conjugate) One embodiment of the method for preparing the joint is a method that includes a step of obtaining the joint by welding. In the method for preparing the joint of this embodiment, the above-described solder paste is used for heating during the welding process.
[0083] Hereinafter, as a method for preparing the bonding body according to this embodiment, the following describes the sequential process of solder paste application, component assembly, and reflow soldering as an example of a heating method.
[0084] Solder paste application operation In the solder paste application process, the above-mentioned solder paste is applied to the surface of the substrate.
[0085] Examples of substrates include printed circuit boards and wafers.
[0086] Methods for applying solder paste include, for example, printing solder paste using a mask with an opening, dispensing solder paste using a dispenser, or transferring solder paste using a probe.
[0087] Component installation operation In the component mounting operation, the component is mounted at the specified position on the substrate printed with solder paste.
[0088] Examples of components include, for example, chips, integrated circuits, transistors, diodes, resistors, capacitors, semiconductor packages, substrates, etc.
[0089] Reflow soldering operation The atmosphere used in the reflow soldering operation is not particularly limited as long as it can achieve the effect of the present invention. For example, it can be a nitrogen atmosphere or a reducing gas atmosphere.
[0090] The reducing gas atmosphere can be formed, for example, by volatilizing the reducing compound in a reflux furnace, or by supplying the reflux furnace with a reducing gas obtained by introducing nitrogen into a liquid reducing compound. Formic acid is preferred as the reducing compound.
[0091] When the reflow soldering operation is performed in a reducing gas atmosphere, the amount of activator used can be reduced, or even eliminated entirely. This further reduces flux residue.
[0092] In a reflow soldering operation, the substrate after the components are mounted is heated in a reflow oven at a temperature (i.e., peak temperature) that is lower than the solidus temperature of the second solder alloy powder contained in the solder paste and higher than the liquidus temperature of the first solder alloy powder. This is referred to as formal heating.
[0093] The heating temperature can be, for example, 10 to 20°C higher than the liquidus temperature of the first solder alloy powder. The heating time can be, for example, 10 seconds to 3 minutes.
[0094] Reflow soldering can also be performed by preheating the substrate after component mounting at a temperature lower than the actual heating temperature before the actual heating.
[0095] During reflow soldering, when the heating temperature rises above the solidus temperature of the first solder alloy powder, the first solder alloy powder begins to melt, becoming molten solder. This molten solder spreads and begins to wet the interface between the component and the substrate. Simultaneously, the second solder alloy powder begins to melt within the molten solder. As formal heating continues, the molten solder completely melts, and the second solder alloy powder continues to melt within the molten solder, forming a solder joint. The continuous melting of the second solder alloy powder within the molten solder allows for the formation of a homogeneous liquid state. As a result, the mechanical properties of the solder joint are improved.
[0096] According to the above-described method for preparing the joint, since the specific solder paste described above is used, the failure mode and high-speed shear strength can be optimized in the prepared joint, thereby improving the joint strength.
[0097] The aforementioned specific solder paste and the method for preparing the joint using the solder paste are useful technologies for soldering applications in fields such as smartphones, tablet PCs, digital cameras, automotive electronic devices, medical devices, and IoT devices.
[0098] Example The present invention will be described below through embodiments, but the present invention is not limited to the following embodiments.
[0099] <Preparation of solder paste> (Examples 1-5, Comparative Examples 1-35) The solder alloys with the alloy compositions shown in Tables 1-3 were atomized to produce first solder alloy powder and second solder alloy powder with an average particle size of 32 μm when measured by volume reference.
[0100] The solidus temperature and liquidus temperature of a portion of the solder alloy powder produced are shown below.
[0101] Sn-4 Ag-20In has a solidus temperature of 143°C and a liquidus temperature of 198°C. Sn-3.2 Ag-20In has a solidus temperature of 141°C and a liquidus temperature of 195°C. Sn-3 Ag-0.5Cu has a solidus temperature of 217°C and a liquidus temperature of 220°C. Sn-2.9 Ag-0.5Cu has a solidus temperature of 217°C and a liquidus temperature of 220°C. Sn-4 Ag-0.5Cu has a solidus temperature of 217°C and a liquidus temperature of 229°C. Sn-3.8 Ag-0.5Cu has a solidus temperature of 217°C and a liquidus temperature of 217°C. Sn-3 Ag-0.3Cu has a solidus temperature of 218 °C and a liquidus temperature of 221 °C. Sn-3 Ag-1Cu has a solidus temperature of 216 °C and a liquidus temperature of 224 °C. Sn-3 Ag-2Cu has a solidus temperature of 216 °C and a liquidus temperature of 277 °C. Sn-3 Ag has a solidus temperature of 221°C and a liquidus temperature of 222°C. Sn-3.5 Ag has a solidus temperature of 220°C and a liquidus temperature of 221°C. Sn-5 Ag has a solidus temperature of 220°C and a liquidus temperature of 245°C. Sn-5 Sb solidus temperature 240 (°C), liquidus temperature 243 (°C) Next, the first solder alloy powder and the second solder alloy powder are mixed according to the mixing ratios shown in Tables 1-3. Then, they are mixed with the flux with the following composition to prepare solder pastes for each example. At this time, the mixing ratio of solder alloy powder to flux is set to 88.5 parts by mass of the mixture of the first solder alloy powder and the second solder alloy powder, and 11.5 parts by mass of flux.
[0102] Flux composition: 40% by mass of hydrogenated acid modified rosin, 40% by mass of solvent, 10% by mass of organic acid, and 10% by mass of thixotropic agent. <Evaluation> For each solder paste example, the evaluation of its meltability, failure mode, and high-speed shear strength was performed as described below. These evaluation results are recorded in Tables 1-3.
[0103] [The fusibility of solder paste] The following shows the substrate, components, reflow soldering equipment, and observation equipment used.
[0104] Substrate: FR-4, substrate size 105mm × 105mm × 0.8mm Component: QFP Reflow soldering equipment: SNR-615 manufactured by Senju Metal Industries, Ltd. Observation apparatus: Optical microscope, KEYENCE VHX-6000, Inc. Solder paste application and component assembly operations: Solder paste is applied to the surface of the substrate, and the component is installed at a specified position on the substrate coated with solder paste.
[0105] • Reflow soldering operation: Next, the substrate after the components are mounted is heated using the reflow soldering apparatus described above.
[0106] As heating conditions, under a nitrogen atmosphere, the temperature was increased to 190°C at a rate of 1°C / s, and maintained within the range of 190°C to 210°C (peak temperature) for 150 seconds. The reflow soldering profile at this time is as follows. Figure 1 As shown.
[0107] The fusibility of the solder paste is evaluated by observing a specified location (the part where the component is mounted) of the substrate coated with solder paste on the substrate using the above-mentioned observation device after the reflow soldering operation and determining the melting state (molten, unmolded) of the solder alloy powder based on the following evaluation criteria. Figure 2 The evaluation benchmark is shown.
[0108] Evaluation Criteria A: The solder alloy powder has melted, but no surface irregularities were detected (no surface irregularities).
[0109] B: The solder alloy powder has melted, but surface irregularities have been confirmed (there are surface irregularities).
[0110] C: Insufficient melting of solder alloy powder (insufficient melting).
[0111] D: The solder alloy powder is not melted (not melted).
[0112] [Failure Mode and High-Voltage Shear Strength] High-speed shear (HSS) tests were conducted to evaluate failure modes and high-speed shear strength as characteristics of solder joints.
[0113] Fabrication of substrates used for HSS testing Solder paste was printed onto a substrate using a mask with an opening (dia) of 0.91 mm and a mask thickness of 0.24 mm, and then reflow soldered to obtain an HSS test substrate with solder joints.
[0114] Reflow soldering details Reflow soldering equipment: SNR-615 manufactured by Senju Metal Industries, Ltd. Reflow soldering conditions: peak temperature 220℃, peak time 35 seconds, nitrogen atmosphere: peak temperature is set to 220℃ to avoid affecting this evaluation due to differences in melt properties.
[0115] HSS research The obtained substrate for HSS testing was mounted on the fixture in the HSS testing machine (DAGE-4000HS manufactured by Nordson Dage). Five solder joints made according to the above manufacturing steps were sheared, and the strength required for shearing at this time (high-speed shear strength) was measured.
[0116] The conditions for the HSS test are as follows.
[0117] Shearing speed 4000 mm / sec, shearing height 10 μm • Evaluation of the destruction mode The substrates subjected to the HSS test after the above-mentioned HSS test were observed using an optical microscope (VHX-6000 manufactured by KEYENCE Co., Ltd.) to evaluate the damage modes.
[0118] The evaluation of failure modes is carried out by determining the failure pattern caused by shear according to the following evaluation criteria.
[0119] Evaluation Criteria For the 5 solder joints A: All five cases showed no peeling failure at the intermetallic compound (IMC) interface spanning the entire bump surface, and at least one failure occurred within the solder itself (solder block) covering more than 90% of the bump surface area. B: All 5 bumps simultaneously experience peeling failure at the IMC interface and failure within the solder block, with the failure area within the solder itself on the bump surface being less than 90%. C: Cases involving more than one peeling failure at the IMC interface spanning the entire face of the bump. Evaluation of high-speed shear strength The evaluation of high-speed shear strength is based on the strength (high-speed shear strength) measured in the above-mentioned HSS test, and is carried out according to the following evaluation criteria.
[0120] The high-speed shear strength mentioned here must show a value above a certain level. However, from the perspective that not only should the value be high, but the probability of inappropriate failure modes increases when the shear strength is too high, it must be a value within a certain range of the following evaluation criteria.
[0121] Evaluation Criteria In the five solder joints, A: Cases where the average high-speed shear strength exceeds 10.5 N but is less than 13 N. C: Cases where the average high-speed shear strength is above 13N or below 10.5N. [Table 1]
[0122] [Table 2]
[0123] [Table 3]
[0124] The results shown in Tables 1-3 confirm that the solder pastes of Examples 1-5 can improve the meltability of the solder paste and optimize the failure mode and high-speed shear strength.
[0125] On the other hand, among the solder pastes of Comparative Examples 1 to 35, there were solder pastes with insufficient high-speed shear strength. In the solder pastes of Comparative Examples 1 to 35, no improvement in meltability, failure mode, or optimization of high-speed shear strength was observed.
[0126] The preferred embodiments of the present invention have been described above, but the present invention is not limited to these embodiments. Additions, omissions, substitutions, and other modifications can be made to the configuration without departing from the spirit of the invention. The present invention is not limited by the above description, but only by the appended claims.
Claims
1. A solder paste comprising a first solder alloy powder, a second solder alloy powder, and a flux. in, The first solder alloy powder is an alloy powder containing Sn, Ag, and In, with the Ag content being 3.9% by mass or more. The second solder alloy powder is a powder containing an alloy of Sn, Ag and Cu.
2. The solder paste according to claim 1, wherein, The mixing ratio of the first solder alloy powder and the second solder alloy powder is: the first solder alloy powder is 45 parts by mass or more and 65 parts by mass or less, and the second solder alloy powder is 35 parts by mass or more and 55 parts by mass or less.
3. The solder paste according to claim 2, wherein, The mixing ratio of the first solder alloy powder and the second solder alloy powder is: the first solder alloy powder is more than 50 parts by mass and less than 65 parts by mass, and the second solder alloy powder is more than 35 parts by mass and less than 50 parts by mass.
4. The solder paste according to claim 1, wherein, In the first solder alloy powder, the content of Ag is 3.9% by mass or more and 4.5% by mass or less, the content of In is 18% by mass or more and 22% by mass or less, and the balance is Sn.
5. The solder paste according to claim 1, wherein, In the second solder alloy powder, the content of Ag is 2.9% by mass or more and 4% by mass or less, the content of Cu is 0.3% by mass or more and 1% by mass or less, and the balance is Sn.
6. The solder paste according to claim 1, wherein, In the first solder alloy powder, the mass ratio of In / Ag is 4 or more and 5.5 or less.
7. A method for preparing a joint, comprising a step of obtaining the joint by welding, wherein, During the welding process, the solder paste described in any one of claims 1 to 6 is used for heating.
Citation Information
Patent Citations
Aqueous coating composition
JP2024085077A
Low temperature melting and mid temperature melting lead-free solder paste with mixed solder alloy powders
WO2020227638A1