Method for activating calcium silicate minerals in a cement plant to produce reactive materials
By thermally activating calcium silicate mineral materials in the clinker cooler of a cement kiln, the problems of low utilization efficiency and dust pollution of calcium silicate materials in cement production have been solved, achieving efficient and environmentally friendly cement production.
Patent Information
- Application Number
- CN202580030684.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-04-29
- Filing Date
- 2025-04-29
- Publication Date
- 2026-11-24
AI Technical Summary
Existing technologies make it difficult to effectively utilize widely available calcium silicate minerals in cement production, and the thermal activation process presents problems of dust pollution and heat energy waste.
In the clinker cooler of a cement kiln, calcium silicate mineral materials are thermally activated at a temperature of 600-900℃. The activation is carried out using the sensible heat of the clinker cooler, and the materials are introduced into the cooling zone to reduce dust circulation. An airtight metering system is used to control the amount of materials added.
It achieves efficient and environmentally friendly activation of calcium silicate mineral materials, reduces dust pollution, optimizes heat energy utilization, and improves the reactivity and production efficiency of cement.
Smart Images

Figure CN123165366A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to a method for activating calcium silicate minerals in a cement manufacturing plant to produce reactive materials.
[0002] Furthermore, the present invention relates to a method for producing composite cement containing cement clinker and reactive materials in a cement manufacturing plant. Background Technology
[0003] Various types of mineral components can be added to Portland cement to obtain composite cement. In particular, the use of pozzolanic and / or potentially hydraulic materials as auxiliary binders in Portland cement blends has become common practice.
[0004] By replacing Portland cement with auxiliary cementitious materials, CO2 emissions from cement production will be reduced. During the production of Portland cement clinker, a significant amount of CO2 per ton of Portland cement clinker is emitted due to the decarbonization of raw materials and the fuel oxidation that occurs during the calcination of raw materials in the rotary kiln.
[0005] Auxiliary cementitious materials include a wide range of siliceous, or siliceous and aluminous, materials that are finely dispersed and react chemically with calcium hydroxide at room temperature in the presence of water to form compounds with cementing properties. Examples of auxiliary cementitious materials include granulated blast furnace slag, fly ash, natural volcanic ash and calcined volcanic ash, combusted oil shale, or concrete demolition waste, recycled concrete fine powder (as defined in standard NF EN 197-5:2021).
[0006] Cement is a product that is used in most cases relatively close to its manufacturing location. Therefore, in the case of compound cement, its production requires the availability of sources of auxiliary cementitious materials, whether natural or synthetic. However, local availability of such sources is not guaranteed in all cement-producing regions, primarily due to the declining availability of synthetic sources of some auxiliary cementitious materials. Synthetic auxiliary cementitious materials are, in most cases, byproducts of various industrial processes, such as fly ash from coal-fired power plants or blast furnace slag from steel mills. The decreasing supply of fly ash from the power industry is encouraging the search for new sources of auxiliary cementitious materials for cement and concrete production.
[0007] Therefore, increasing efforts are being made to use widely available sources to produce auxiliary cementitious materials, such as concrete demolition waste.
[0008] Calcium silicate is known to be thermally activated. As known from “Recycled cement”; Junjie Wang, Mulan Mu, Yongliang Liu, Construction and Building Materials, Vol. 190, November 30, 2018, pp. 1124-1132, the recycling of cement (a calcium silicate mineral) can reduce the environmental impact caused by landfilling of concrete demolition materials and the demand for raw materials used in cement production, because waste cement paste from demolished concrete can be used to produce recycled cement. Recycled cement was produced by burning 2-year-old waste cement paste at four different temperatures (120°C, 450°C, 750°C, and 1150°C) and then grinding it into powder. The selected temperatures were those where significant weight loss was observed in the thermogravimetric analysis (TGA) results of the old cement paste. The results showed that the highest compressive strength occurred at 450°C, and the recycled cement paste had similar strength to OPC paste, but with poor workability, even exceeding the measurement range of the rheometer. It was found that increasing the particle size of recycled cement powder and partially replacing the cement powder with ground granulated blast furnace slag (GGBS) can effectively improve the workability of recycled cement paste without reducing the resulting compressive strength.
[0009] There is a need to provide a method for activating calcium silicate materials that is feasible on an industrial scale. This means that such industrial methods need to be efficient in terms of thermal energy consumption, enabling the continuous and controlled production of activated calcium silicate in large quantities.
[0010] Therefore, the object of the present invention is to provide a method for thermally activating calcium silicate minerals.
[0011] WO 2022 / 106966 A1 discloses a method comprising adding raw clay and aluminosilicate minerals into a clinker cooler to obtain calcined clay cement. This method has several advantages because it enables the production of calcined clay without the need to construct and operate dedicated equipment for calcining clay. Furthermore, the method utilizes heat derived from the clinker in a rotary kiln used for clinker production, thereby subsequently calcining the clay, meaning the clay is calcined without the need for an additional heat source.
[0012] However, introducing raw clay into the clinker cooler tends to generate a large amount of dust. This dust can be recycled back into the cement kiln, leading to the following problems: it can contaminate the clinker, thereby affecting its quality and performance; it can reduce the proportion of calcined clay present in the final cement product; it can lower the flame temperature in the kiln due to additional dust in the secondary air; and it can increase the specific heat loss caused by the heat absorbed by the mineral materials into the rotary kiln. Furthermore, the calcination process, as described, lacks precise control. This lack of control can lead to over-burning or under-calcination of the minerals, ultimately impairing the reactivity of the resulting cementitious material. Summary of the Invention
[0013] To address this objective, the present invention provides a method for producing reactive materials in a cement manufacturing plant including a cement kiln and a clinker cooler, wherein the head region of the clinker cooler is connected to the outlet end of the cement kiln to cool cement clinker from the cement kiln, the method comprising: - A calcium silicate mineral material that readily becomes reactive upon heat treatment is provided. - The calcium silicate mineral material is introduced into a clinker cooler and thermally activated in the clinker cooler at a temperature of 600-900°C to obtain the reactive material.
[0014] Therefore, the present invention is based on the concept of using the sensible heat from the hot clinker from the cement kiln to thermally activate calcium silicate mineral materials.
[0015] Preferably, the clinker cooler includes a recovery zone adjacent to the outlet end, in which incoming cooling air is heated by the cement clinker, and the heated cooling air is fed into the cement kiln as secondary air via the head region and / or used as tertiary air, and a cooling zone away from the outlet end, in which incoming cooling air is used to cool the cement clinker and exhaust gas is released from the clinker cooler through an exhaust pipe, and calcium silicate mineral material is introduced into the cooling zone of the clinker cooler and thermally activated in the cooling zone.
[0016] In this preferred embodiment, the invention is based on the concept of introducing calcium silicate mineral material into the cooling zone rather than the recycling zone of the clinker cooler, which significantly reduces dust recycling back to the cement kiln due to the airflow difference between the two zones.
[0017] In the recovery zone, located closer to the outlet end of the cement kiln, the primary objective is to heat the incoming cooling air through direct contact with the hot cement clinker. This heated air is then directed back into the cement kiln as secondary air or used as tertiary air. Due to the direction and purpose of the airflow in this zone—capturing heat and carrying it back to the kiln—the likelihood of entraining fine particles and dust from additives is significantly higher. If calcium silicate mineral materials are added in this zone, the strong airflow designed to maximize heat recovery can easily stir up dust particles and transport them back to the kiln, leading to contamination problems and a reduction in the quality of the activated materials in the cement.
[0018] On the other hand, the cooling zone, located further from the kiln's outlet, uses incoming cooling air primarily to lower the temperature of the cement clinker. The airflow in this zone is designed to cool the clinker and then exit through exhaust ducts, rather than being recirculated back into the kiln. By introducing the calcium silicate mineral material into this zone, the likelihood of dust being agitated by the airflow and transported back to the kiln is minimized. Here, the airflow is directed towards the exhaust system rather than the kiln, meaning that any dust generated during the heat treatment of the calcium silicate material is more likely to be contained within the cooler and then safely discharged through the exhaust system, where filters can be installed to capture suspended particles in the airflow.
[0019] The cooling zone of a clinker cooler is typically characterized by what is known as the cooler's zero point. The cooler's zero point is defined as the point in the cooler above which no gas flows back to the kiln. It is easily determined by technicians through airflow measurements and represents the optimal clinker temperature for the heat treatment of calcium silicate mineral materials.
[0020] Another effect of this invention is that, by introducing the calcium silicate mineral material into the cooling zone, particularly at the upstream region of the cooling zone, i.e., at the zero point, the calcium silicate mineral material can be heat-treated at a temperature of 600-900°C to obtain a reactive material. At the zero point of the clinker cooler, the clinker is typically at a temperature between 600°C and 900°C. Thermal activation of the calcium silicate mineral material at a temperature of 600-900°C means that the material is heated to a temperature of 600-900°C, i.e., at least 600°C and not exceeding 900°C.
[0021] By reaching a specific temperature range of 600°C to 900°C, the desired mineralogical changes in calcium silicate mineral materials can be obtained, changes that are unique to the mineral composition of the material. These changes can produce reactive materials in cement or concrete compositions. If the specific activation temperature range of the calcium silicate mineral material is exceeded, overheating occurs and the silica phase crystallizes, leading to a decrease in the material's reactivity. Detailed Implementation
[0022] As used herein, the reactivity of a reactive material refers to the ability of the material to react with the hydration products of cement to form additional binding compounds and contribute to the development of the compressive strength of the cement, and preferably refers to the pozzolanic and / or hydraulic reactivity of the material.
[0023] In the recycling zone of the clinker cooler, finer particles of the material are transported back to the cement kiln via the airflow necessary for recovering heat energy from the clinker, in order to achieve lower specific heat consumption. The particles recycled back to the cement kiln reach temperatures as high as 1450°C, which leads to the undesirable effects of overburned calcium silicate mineral materials as described above.
[0024] To safely achieve the desired thermal activation of the calcium silicate mineral material, the method of the present invention preferably includes an initial step: selecting a calcium silicate mineral material whose pozzolanic activity can be activated within a temperature range of 600-900°C, preferably 600-700°C. The selection process preferably includes the following steps: a) Chemical XRF analysis of available calcium silicate mineral materials. b) Activate the material at different temperatures ranging from 500°C to 900°C with a gradual gradient of, for example, 100°C. c) Perform activity analysis on the material at each temperature, preferably pozzolanic reactivity analysis. d) Select materials whose reactivity is preferably matched or exceeds that of cement clinker.
[0025] The step of thermally activating the calcium silicate mineral material in the clinker cooler preferably includes contacting the calcium silicate mineral material with cement clinker being transported through the cooling zone of the clinker cooler.
[0026] Therefore, the present invention uses waste energy from clinker cooling to thermally activate the mineralogical phases of calcium silicate mineral materials, which would otherwise have to be produced in a separate process with additional thermal power input to achieve the same temperature conditions as described herein.
[0027] According to a preferred embodiment of the method of the present invention, the calcium silicate mineral material is introduced into the clinker cooler, preferably into the cooling zone, at a vertical distance of 10-20 cm above the bed of cement clinker being conveyed through the clinker cooler. This prevents the calcium silicate mineral material from being suspended in the airflow.
[0028] According to a preferred embodiment of the invention, the clinker cooler is designed as a grate cooler. The grate cooler is essentially constructed of horizontal, movable grates through which cement clinker travels from the kiln outlet to the cooler's discharge end. Cooling air is blown from below over the grates, passing through the hot clinker and promoting heat exchange. This process not only cools the clinker but also heats the cooling air. The cooling air is typically introduced into the clinker cooler from below by means of multiple cooling fans distributed along the length of the cooler, i.e., along the conveying direction of one or more grates. This allows for the existence of separate fans for the clinker cooler's recovery zone and cooling zone.
[0029] Preferably, the clinker cooler is designed as a single-chamber cooler, and the calcium silicate mineral material is introduced into the clinker cooler at the zero point of the clinker cooler.
[0030] Alternatively, the clinker cooler may comprise two or more consecutive cooling chambers, and calcium silicate mineral material is introduced into a second cooling chamber located downstream of the first cooling chamber, wherein the calcium silicate mineral material is preferably introduced at the upstream end of the second cooling chamber. At least two cooling chambers allow for a two-stage cooling process, wherein the two stages are typically physically separated, each designed for a specific cooling and heat recovery task within the overall clinker cooling process. Specifically, the first cooling chamber contains the recovery zone of the clinker cooler, and the second cooling chamber contains the cooling zone of the clinker cooler. Physical separation of the two stages can be achieved, for example, by a separation wall that helps control the flow of clinker and cooling air between the stages, ensuring that the cooling air in each stage can be managed independently. In particular, the physical separation is designed to allow clinker to transition from the first stage to the second stage while maintaining separate flow of cooling air.
[0031] According to a preferred embodiment of the invention, calcium silicate mineral material is introduced into a clinker cooler, preferably in the cooling zone, by means of an airtight metering system. The airtight metering system ensures that the precise required amount of calcium silicate mineral material is introduced into the clinker cooler, thereby eliminating the risk of air pollution and preventing fine particulate matter from escaping into the surrounding environment.
[0032] Preferably, the calcium silicate mineral material is introduced into the clinker cooler, preferably in the cooling zone, at a dosage rate of 0.05-20% by weight, more preferably 1-10% by weight, of the cement clinker. This ensures the optimal ratio of cement clinker to reactive material in the final product and achieves a balance between maximizing the reactivity of the reactive material without compromising the performance of the final product.
[0033] In a preferred embodiment, the calcium silicate mineral material is continuously fed into the clinker bed in the clinker cooler, preferably by means of a rotary valve or a feed screw. Rotary valves or feed screws have the advantage of providing a more continuous material supply to the hot clinker bed. Conversely, feeding devices using dual inlet valves are not preferred because they deliver material discontinuously, resulting in thickness variations of the calcium silicate mineral material on the hot clinker, which in turn does not allow for uniform calcination of the material. In an even more preferred embodiment, the material is discharged into the hot clinker bed in the clinker cooler by means of a method that does not include dual inlet valves.
[0034] Preferably, a first temperature of the cement clinker is measured upstream of the cooling zone, and a second temperature of the cement clinker is measured at the discharge end of the clinker cooler. The feed rate of the calcium silicate mineral material introduced into the clinker cooler is controlled according to the first and second temperatures, such that the calcium silicate mineral material is heated to a temperature of at least 600°C and not exceeding 900°C. Preferably, the first temperature is measured at the inlet of the clinker cooler. By correlating the feed rate with the real-time temperature reading of the clinker, this method improves the efficiency of the heat exchange process and optimizes the use of residual heat energy from the clinker for the thermal activation of the mineral material.
[0035] The appropriate particle size of the calcium silicate material during this process can be selected based on the specific circumstances of each process. A finer particle size is generally preferred because it provides a larger surface area for heat and chemical reactions, promoting more uniform and complete activation. However, the particle size should not be too fine, as this can lead to operational challenges, such as dust generation or handling difficulties. The optimal particle size is typically determined by balancing maximizing reactivity with practical considerations related to processing and handling in the specific calcination system used. Preferably, the particle size of the calcium silicate mineral material undergoing the activation step is in the range of 50 micrometers to 8 millimeters, preferably 1 to 4 millimeters. This particle size selection allows for a reduction in the amount of dust generated during the introduction of the calcium silicate mineral material into the clinker cooler.
[0036] Calcium silicate mineral materials can be selected from concrete demolition materials, recycled cement paste, concrete sludge from ready-mix concrete production plants, concrete waste from precast plants, or mixtures thereof.
[0037] Preferably, concrete demolition material or recycled concrete slurry is used as the calcium silicate mineral material. The concrete demolition material may preferably contain at least 10% by weight of cement slurry, more preferably 20% by weight, and even more preferably 30% by weight. This substantial proportion of cement slurry constituting the final activated material maintains a high calcium silicate content, which is necessary for the pozzolanic reaction in cementitious applications.
[0038] Demolition materials, or concrete demolition waste, are mixtures of different materials from old building demolition sites. They typically include concrete demolition waste, drywall, brick, steel, timber, ceramic tiles, or glass. A common practice is to sort these materials at recycling centers to separate the materials listed above so they can be reused for applications where their chemical composition is best suited.
[0039] These demolition wastes are classified according to their composition and potential pollution using different waste codes in the European Waste Catalog (EWC). The EWC is a tiered list of waste descriptions established by the European Commission in decision 2000 / 532 / EC2. Construction and demolition wastes fall under Chapter 17 of the EWC. Concrete demolition wastes fall under Sub-Chapter 17.01 and include the following waste codes: • 17 01 01: Concrete • 17 01 02: Brick • 17 01 03: Tiles and Ceramics • 17 01 06: Mixtures or individual grades of concrete, bricks, tiles, and ceramics containing hazardous substances. • 17 01 07: Mixtures of concrete, brick, tile, and ceramics other than those mentioned in 17 01 06. Other sub-chapters include timber, glass and plastics (17 02), bitumen mixtures, coal tar and tar-coated products (17 03), metals (17 04), soils (17 05) and other fractions (17 06–17 09).
[0040] For the purposes of this invention, concrete demolition waste according to EWC waste codes 17 01, particularly 17 01 01 and / or 17 01 07, can be used as calcium silicate mineral material.
[0041] Preferably, the calcium silicate mineral material contains 2-25% by weight of water. If the calcium silicate mineral material has a moisture content exceeding 25% by weight, waste heat from the cement process can be used to reduce the amount of water in the material before it is introduced into the clinker cooler. Furthermore, the water content should preferably be higher than 5% by weight of the calcium silicate mineral material to ensure minimal dust generation during the process of adding the material to the hot clinker bed.
[0042] Thermal activation of calcium silicate mineral materials in clinker coolers at cement plants, particularly through contact with the clinker bed, advantageously results in the combination of reactive materials with cement clinker. Therefore, a preferred embodiment of the invention provides a combined material comprising cement clinker and reactive materials discharged from the discharge end of the clinker cooler. This combined material offers environmental benefits due to the ability of the reactive materials to replace a portion of the cement clinker, effectively reducing the carbon footprint of cement.
[0043] This composite material can then be ground together with a calcium sulfate source and other optional mineral components to form composite Portland cement. Calcium sulfate is used as a setting time regulator for hydrated cement at a concentration of 1-10% by weight. Due to the rapid hardening of clinker, the addition of calcium sulfate prolongs the cement's hardening time proportionally to its increase in the composite cement.
[0044] In a preferred embodiment, calcium carbonate may be added as an additional component to the composite cement in an amount of 1-35% by weight of the total weight of the composite cement.
[0045] According to a second aspect, the present invention provides a method for producing composite cement containing cement clinker and reactive materials in a cement manufacturing plant including a cement kiln and a clinker cooler, wherein the head region of the clinker cooler is connected to the outlet end of the cement kiln to cool the cement clinker from the cement kiln, the method comprising: - Calcining cement clinker in a cement kiln - Cement clinker is discharged from the cement kiln into a clinker cooler and cooled there. - A reactive material is produced by a method according to a first aspect of the invention, wherein the material is brought into contact with cement clinker present in a clinker cooler. - A composite material containing cement clinker and reactive materials is discharged from the clinker cooler. - The mixture is ground together with a calcium sulfate source in a cement mill to obtain the composite cement.
[0046] Preferably, the composite cement further comprises calcium carbonate, preferably in an amount of 1-35% by weight of the total weight of the composite cement.
[0047] Preferably, the composite cement further comprises auxiliary cementitious materials, such as natural volcanic ash, fly ash, granulated blast furnace slag and / or siliceous-alumina natural or artificial minerals with volcanic ash activity.
[0048] Now refer to Figure 1 The invention is described in more detail with an exemplary embodiment shown.
[0049] Figure 1The image shows a cement kiln 1 used for calcining cement clinker, such as the outlet end of a rotary kiln. Cement clinker is discharged from the cement kiln 1 into a clinker cooler 2 (as indicated by arrow 3) and forms a clinker bed 4, which is conveyed through the clinker cooler 2 to the discharge end 5 by means of a moving grate 6, from where the clinker falls onto a conveyor 7 for further transport to a storage facility.
[0050] The burner used to provide heat energy to the cement kiln 1 is indicated by reference numeral 8 in the attached figure. Fuel 9 and primary air 10 are fed into the burner.
[0051] To cool the cement clinker, ambient air is blown into the clinker cooler 2 by multiple fans 11 distributed along its length. The cooling air is blown from below over the grate 6 and through the clinker bed 4, thereby cooling the cement clinker and increasing the temperature of the cooling air. The clinker cooler includes a recovery zone 12 adjacent to the outlet end of the cement kiln 1, where the incoming cooling air is heated by the cement clinker, and the heated cooling air is fed into the cement kiln 1 as secondary air 14 and / or used as tertiary air 15 via the head region 20, and a cooling zone 13 away from the outlet end, where the incoming cooling air is used to cool the cement clinker, and exhaust gas 17 is released from the clinker cooler 2 through an exhaust pipe 16. The zero point 18 of the clinker cooler 2 is located at the beginning of the cooling zone 13. As indicated by the upward-pointing arrow, the cooling airflow in the recovery zone 12 is directed to the head region 20 of the cooler, and the cooling airflow in the cooling zone 13 is directed to the exhaust pipe 16.
[0052] Calcium silicate mineral materials, such as concrete demolition waste, which readily become reactive through heat treatment, are introduced into the cooling zone 13 of the clinker cooler 2, as indicated by arrow 18, to thermally activate the calcium silicate mineral materials at a temperature of 600-900°C. The introduction point of the calcium silicate mineral material 19 is located approximately 10-20 cm above the clinker bed 4. In this way, the calcium silicate mineral material 19 is brought into contact with the clinker bed 4 and heated to a temperature of 600-900°C to thermally activate it. The activated material is carried by the moving clinker bed 4 and conveyed to the discharge end 5. Thus, as a result of the method, a combined product containing cement clinker and reactive materials is obtained.
Claims
1. A method for producing reactive materials in a cement manufacturing plant including a cement kiln (1) and a clinker cooler (2), wherein the head region (20) of the clinker cooler (2) is connected to the outlet end of the cement kiln (1) to cool cement clinker from the cement kiln (1), the method comprising: - Provides calcium silicate mineral materials that readily become reactive through heat treatment. - The calcium silicate mineral material is introduced into the clinker cooler (2) and thermally activated in the clinker cooler (2) at a temperature of 600-900°C to obtain the reactive material.
2. The method according to claim 1, wherein the clinker cooler (2) comprises a recovery zone (12) adjacent to the outlet end, wherein incoming cooling air is heated by the cement clinker (4) and the heated cooling air is fed into the cement kiln (1) as secondary air (14) via the head region (20) and / or used as tertiary air (15), and a cooling zone (13) away from the outlet end, wherein incoming cooling air is used to cool the cement clinker (4) and exhaust gas is released from the clinker cooler (2) through an exhaust pipe (16), and wherein the calcium silicate mineral material is introduced into the cooling zone (13) of the clinker cooler (2) and is thermally activated in the cooling zone (13).
3. The method according to claim 2, wherein the calcium silicate mineral material is introduced into the clinker cooler (2) at the upstream region of the cooling zone (13).
4. The method according to claim 1, 2 or 3, wherein the calcium silicate mineral material is introduced into the clinker cooler (2) at a vertical distance of 10-20 cm above the bed (4) of cement clinker (4) conveyed through the clinker cooler (2), preferably in the cooling zone (13).
5. The method according to any one of claims 1 to 4, wherein the clinker cooler (2) is designed as a grate cooler.
6. The method according to any one of claims 1 to 5, wherein the clinker cooler (2) is designed as a single-chamber cooler, and the calcium silicate mineral material is introduced into the clinker cooler (2) at zero point (18).
7. The method according to any one of claims 1 to 5, wherein the clinker cooler (2) comprises two or more consecutive cooling chambers, and the calcium silicate mineral material is introduced into a second cooling chamber disposed downstream of the first cooling chamber, wherein the calcium silicate mineral material is preferably introduced at the upstream end of the second cooling chamber.
8. The method according to any one of claims 1 to 7, wherein the calcium silicate mineral material is introduced into the clinker cooler (2), preferably the cooling zone (13), by means of an airtight metering system.
9. The method according to any one of claims 1 to 8, wherein the calcium silicate mineral material is introduced into the clinker cooler (2), preferably the cooling zone (13), by means of a rotary valve or a feed screw.
10. The method according to any one of claims 1 to 9, wherein the calcium silicate mineral material is introduced into the clinker cooler (2), preferably the cooling zone (13), at a quantitative feed rate of 0.5-20% by weight, preferably 1-10% by weight, of the cement clinker (4).
11. The method according to any one of claims 2 to 10, wherein a first temperature of the cement clinker (4) is measured upstream of the cooling zone (13), and a second temperature of the cement clinker (4) is measured at the discharge end (5) of the clinker cooler (2), and the feed rate of the calcium silicate mineral material introduced into the clinker cooler (2) is controlled according to the first and second temperatures, such that the calcium silicate mineral material is heated to a temperature of at least 600°C and not higher than 900°C.
12. The method according to any one of claims 1 to 11, wherein concrete demolition waste or hardened cement paste is used as the calcium silicate mineral material.
13. The method according to any one of claims 1 to 12, wherein the calcium silicate mineral material comprises 2-25% by weight of water content of the total weight of the calcium silicate mineral material.
14. The method according to any one of claims 1 to 13, wherein the mixture of the cement clinker (4) and the reactive material is discharged from the discharge end (5) of the clinker cooler (2).
15. A method for producing composite cement containing cement clinker and reactive materials in a cement manufacturing plant including a cement kiln (1) and a clinker cooler (2), wherein the head region (20) of the clinker cooler (2) is connected to the outlet end of the cement kiln (1) to cool cement clinker (4) from the cement kiln, the method comprising: - Cement clinker is calcined in the cement kiln (1). - The cement clinker is discharged from the cement kiln (1) into the clinker cooler (2) and the cement clinker (4) is cooled in the clinker cooler (2). - The reactive material is produced by the method according to any one of claims 1 to 14, wherein the material is brought into contact with the cement clinker (4) present in the clinker cooler (2). - A combined material comprising the cement clinker (4) and the reactive material is discharged from the clinker cooler (2). - The mixture is ground together with a calcium sulfate source in a cement mill to obtain the composite cement.
16. The method of claim 15, wherein the composite cement further comprises calcium carbonate, preferably in an amount of 1-35% by weight of the total weight of the composite cement.
17. The method according to claim 15 or 16, wherein the composite cement further comprises auxiliary cementitious materials, such as natural volcanic ash, fly ash, granulated blast furnace slag, calcined clay and / or siliceous-aluminous natural or artificial minerals with volcanic ash activity.
Citation Information
Patent Citations
A low-carbon cement and its method of production
WO2022106966A1