Polymer, protective film agent for laser cutting
By using polymers prepared from monomers such as N,N-dimethylacrylamide as protective film agents, the problem of insufficient heat resistance in existing technologies is solved, and the effective cleaning of the protective film and the improvement of product quality are achieved during high-temperature laser cutting.
Patent Information
- Application Number
- CN202580030034.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-10-15
- Filing Date
- 2025-10-09
- Publication Date
- 2026-11-24
AI Technical Summary
Existing protective film agents have insufficient heat resistance during the laser cutting of semiconductor wafers, leading to the deterioration of the protective film agent, which is difficult to remove by water washing, thus affecting the quality and performance of the products.
Homopolymers or copolymers containing monomers such as N,N-dimethylacrylamide as structural units are used, with a polymer weight-average molecular weight in the range of 30,000 to 100,000 and a viscosity of 10% by mass aqueous solution of 100 mPas to 15,000 mPas. A light absorber is added to form a protective film.
The polymer does not deteriorate under high-temperature laser irradiation, is easy to remove after washing, and leaves no protective film residue, thus improving the cleaning efficiency and quality of the products.
Smart Images

Figure CN123165408A_ABST
Abstract
Description
Technical Field
[0001] This involves polymers with excellent acid resistance and protective film agents for laser cutting that use these polymers and have excellent heat resistance. Background Technology
[0002] A method is known for processing a substrate (e.g., glass, semiconductor wafer, resin molded article, etc.) in which a protective film is formed on the surface of the substrate to protect the non-processed areas, and then removing the protective film after processing.
[0003] Such methods are used, for example, in the processing of semiconductor wafers. A semiconductor wafer is a laminate of insulating and functional films stacked on the surface of a semiconductor substrate such as silicon. A semiconductor chip is manufactured by creating grooves by irradiating the semiconductor wafer with a laser, and then cutting along those grooves. However, since the laser is absorbed by the semiconductor substrate when it is irradiated onto the semiconductor wafer, there is a problem that molten material and thermal decomposition products from the semiconductor substrate are generated. These molten material and thermal decomposition products adhere to the surface of the semiconductor wafer and semiconductor chip as processing debris.
[0004] Therefore, a method (laser cutting) is known for forming a protective film that can be removed by water onto the surface of a semiconductor wafer and then processing it by irradiating it with a laser. By irradiating the protective film with a laser, debris can be made to adhere to the surface of the protective film, and the debris can be removed together with the protective film by water washing.
[0005] Generally, such protective film agents use substances that contain water-soluble polymers and water-soluble laser absorbers with a specific range of absorbance.
[0006] Because traditional blade cutting is unsuitable for brittle low-k materials, laser processing is used for these materials. Laser processing is broadly divided into two types: continuous wave operation (CWOperation) and pulsed operation. In the monolithic processing of semiconductor substrates, pulsed operation, which can suppress the thermal impact, is mainly used. Although the thermal impact is suppressed, the local areas are still subjected to considerable heat.
[0007] Generally, in order to facilitate the cleaning of machining debris (fragments) generated during this process, a water-soluble polymer protective film is used on the machining area before the cutting process, as described above. However, since the flying debris is at high temperature, the water-soluble polymer in the protective film sometimes undergoes cross-linking and thermal degradation, making it difficult to clean with water and potentially causing a significant impact on the quality and performance of the product.
[0008] For example, in Patent Document 1 (Japanese Patent Application Publication No. 2023-41313), polyvinyl alcohol, polyvinylpyrrolidone, hydroxypropyl cellulose, or polyvinyl alcohol are used. Water-soluble polymers such as azoline, and light absorbers with flavonoid, flavonol, or isoflavone structures.
[0009] Furthermore, a protective film agent comprising a polyvinylpyrrolidone resin, a solvent, and a laser absorber is proposed in Patent Document 2 (Japanese Patent Application Publication No. 2020-066667).
[0010] Furthermore, a protective film composition containing a water-soluble polymer composed of polyvinyl alcohol or polyvinylpyrrolidone, a resin capsule encapsulating a laser absorber, and an aqueous solvent was also proposed in Patent Document 3 (Japanese Patent Application Publication No. 2016-066768).
[0011] Furthermore, Patent Document 4 (Japanese Patent Application Publication No. 2015-134373) discloses a protective film agent for laser processing containing poly-N-vinylacetamide. Further, Patent Document 5 (Japanese Patent Application Publication No. 2019-12807) discloses a protective film agent for laser processing as a mixture of polyvinyl alcohol and poly-N-vinylacetamide.
[0012] Existing technical documents
[0013] Patent documents
[0014] Patent Document 1: Japanese Patent Application Publication No. 2023-41313
[0015] Patent Document 2: Japanese Patent Application Publication No. 2020-066667
[0016] Patent Document 3: Japanese Patent Application Publication No. 2016-066768
[0017] Patent Document 4: Japanese Patent Application Publication No. 2015-134373
[0018] Patent Document 5: Japanese Patent Application Publication No. 2019-12807 Summary of the Invention
[0019] The problem that the invention aims to solve
[0020] However, in Patent Document 1, the resin used has relatively low heat resistance, leading to thermal cross-linking and thermal degradation, thus making it difficult to clean with water. Furthermore, Patent Documents 2 and 3 lack descriptions of the heat resistance of polyvinylpyrrolidone (PVP). Although PPVP has a high thermal decomposition point as determined by TG / DTA, it exhibits problems with degradation and insolubility under strong heating in aqueous solutions. Additionally, no research has been conducted on the degradation of the resin under laser irradiation.
[0021] Although the heat resistance of the poly-N-vinylacetamide used in Patent Documents 4 and 5 is improved by the aforementioned polymers, it cannot be said to be sufficient.
[0022] Protective film agents have long been known to have the following problems: when laser cutting semiconductor wafers, the water-soluble polymers used in the protective film agent have insufficient heat resistance, resulting in the deterioration of the protective film agent, and making it difficult to remove the protective film agent that should be rinsed with water.
[0023] Methods for solving problems
[0024] In this context, it was discovered that homopolymers (hereinafter sometimes referred to as PDMA) or copolymers with monomers such as N,N-dimethylacrylamide as structural units, which can withstand even high-temperature laser irradiation, do not deteriorate even during high-temperature thermal processes and exhibit good resolubility in water after the thermal process, thus completing the present invention. The structure of the present invention is as follows.
[0025] [1] A polymer comprising the structural unit shown in formula (1) below,
[0026] (In equation (1), R) 1 ~R 5 (Representing any one of hydrogen atoms, alkyl groups having 1 to 8 carbon atoms, and hydroxyalkyl groups)
[0027] The polymer is either (i) a homopolymer of the above-mentioned structural unit or (ii) a copolymer of the above-mentioned structural unit with a structural unit derived from at least one monomer selected from N-vinylcarboxylic amide, unsaturated carboxylic acid monomer, salt of unsaturated carboxylic acid monomer, unsaturated carboxylic acid ester monomer, vinyl ester monomer, and unsaturated nitrile monomer (referred to as other monomers). The weight-average molecular weight of the above polymers is less than 1 million.
[0028] [2] According to the polymer in [1], the viscosity of a 10% by mass aqueous solution is 100 mPa. s or higher and 15000mPa Below s.
[0029] [3] According to the polymer of [1] or [2], the content of the other monomer structural units mentioned above is less than 90 mol% of the total 100 mol% of the polymer.
[0030] [4] The polymers according to [1] to [3] have a weight average molecular weight in the range of more than 30,000 and less than 1,000,000.
[0031] [5] A protective film agent comprising the polymers of [1] to [4] above.
[0032] [6] The protective film agent according to [5] also contains a light absorber.
[0033] [7] A protective film that uses the protective film agent of [5] or [6].
[0034] The effects of the invention
[0035] The polymer of the present invention is a material with high heat resistance, capable of withstanding high-temperature laser irradiation used in laser cutting, etc. Therefore, when used as a protective film agent, it will not deteriorate, leaves no residue after washing with water, and can be easily removed. Attached Figure Description
[0036] Figure 1 The transmission spectra of the polymer of Example 2, obtained by FT-IR, are shown before and after heating to 250°C.
[0037] Figure 2 The transmission spectra of the polymer of Comparative Example 2, obtained by FT-IR, are shown before and after heating to 250°C.
[0038] Figure 3 The photographs show the changes in appearance of the samples from the examples and comparative examples before and after heating at 250°C for 1 hour. Detailed Implementation
[0039] The following describes embodiments of the present invention, but these embodiments are not limited to the following description.
[0040] (1) Polymer
[0041] This embodiment is a polymer containing the structural unit shown in formula (1) below.
[0042]
[0043] (In equation (1), R) 1 ~R 5 (representing alkyl or hydroxyalkyl groups with 1 to 8 hydrogen atoms)
[0044] Such polymers are water-soluble macromolecules and exhibit amphiphilicity.
[0045] The polymer in this embodiment is either (i) a homopolymer of the above-described structural unit or (ii) a copolymer of the above-described structural unit with a structural unit derived from at least one monomer (referred to as other monomers) selected from N-vinylcarboxylic acid amide, unsaturated carboxylic acid monomer, salt of unsaturated carboxylic acid monomer, unsaturated carboxylic acid ester monomer, vinyl ester monomer, or unsaturated nitrile monomer.
[0046] Other monomers are further preferably (meth)acrylic acid and its salts, and even more preferably sodium acrylate. It should be noted that, in this specification, "(meth)acrylic acid" refers to acrylic acid and methacrylic acid.
[0047] In this embodiment, the polymer preferably has 90 mol% or less of the structural units other than those shown in formula (1), and more preferably 80 mol% or less, out of 100 mol% of all structural units. This ratio provides good solubility in water, which is preferred. It is even more preferred that the ratio of other structural units is 0. Therefore, the polymer in this embodiment is preferably a homopolymer composed of structural units of formula (1).
[0048] Preferably, R is selected from general formula (1). 1 ~R 3 For hydrogen atoms, R 4 and R 5 Both are alkyl structural units II and R with 1 to 6 carbon atoms. 4 It is a hydrogen atom and R 5 Structural units I-II and R of alkyl groups having 1 to 8 carbon atoms 4 It is a hydrogen atom and R 5 It is at least one of structural units I-III of a hydroxyalkyl group having 1 to 2 carbon atoms. R is preferred. 4 and R 5 All are methyl or ethyl, more preferably methyl.
[0049] The polymer of this embodiment has a weight-average molecular weight of less than 1.3 million, more preferably less than 1 million, and more preferably more than 30,000 and less than 1,000,000. Such a polymer has high solubility in water and high heat resistance, and can even withstand high-temperature laser irradiation used in laser cutting and other applications.
[0050] As one embodiment, the viscosity of a 10% by mass aqueous solution of the polymer at 20°C is 100 mPa. The viscosity of a 10% by mass aqueous solution of the polymer in this embodiment at 20°C is 15000 mPa. Below s. Polymers of this type can be obtained through the following manufacturing methods.
[0051] (2) Polymer manufacturing methods
[0052] The method for manufacturing the polymer in this embodiment is to perform free radical polymerization of the monomer shown in the following formula (2) in an aqueous solution using an aqueous medium.
[0053]
[0054] (In equation (2), R) 1 ~R 5 (This refers to alkyl or hydroxyalkyl groups with 1 to 8 hydrogen atoms and carbon atoms.)
[0055] As the monomer shown in general formula (2), similarly to formula (1) above, it is preferably selected from R. 4 and R 5 All are monomers of alkyl groups having 1 to 6 carbon atoms (but they can be the same or different), R 4 It is a hydrogen atom and R 5 Monomers of alkyl groups having 1 to 8 carbon atoms, R 4 It is a hydrogen atom and R 5 It is at least one of the monomers that are hydroxyalkyl groups having 1 to 2 carbon atoms.
[0056] R is preferred. 4 It is a hydrogen atom and R 5 The monomer is methyl or ethyl, more preferably methyl. If R 4 It is a hydrogen atom and R 5 If the methyl or ethyl form is used, the hydrogen bonding and coagulation strength are moderate, making it a preferred coating agent.
[0057] R 4 With R 5 Compounds that are bound by covalent bonds are not included in the monomers of formula (2).
[0058] Examples of monomers represented by general formula (2) include N-methylacrylamide (MAA), N-ethylacrylamide, N-propylacrylamide, N-isopropylacrylamide (NIPAM), N-butylacrylamide, N-isobutylacrylamide, N-tert-butylacrylamide, N-heptylacrylamide, N-octylacrylamide, N-hydroxymethylacrylamide, N-hydroxyethylacrylamide (HEAA), N,N-dimethylacrylamide (DMAA), N,N-diethylacrylamide (DEAA), N,N-dipropylacrylamide, N,N-diisopropylacrylamide, N,N-dibutylacrylamide, N,N-diisobutylacrylamide, N,N-diheptylacrylamide, N,N-dioctylacrylamide, N,N-dihydroxymethylacrylamide, and N,N-dihydroxyethylacrylamide. They can be used alone or in combination of two or more. Among these monomers, N-isopropylacrylamide, N-hydroxyethylacrylamide, N,N-dimethylacrylamide, and N,N-diethylacrylamide are preferred, with N-hydroxyethylacrylamide and N,N-diethylacrylamide being more preferred.
[0059] In addition to the monomers mentioned above, the product may also contain copolymerizable monomers (hereinafter sometimes referred to as "other monomers"). Other monomers are at least one monomer selected from unsaturated carboxylic acid monomers, salts of unsaturated carboxylic acid monomers, unsaturated carboxylic acid ester monomers, vinyl ester monomers, and unsaturated nitrile monomers. More preferably, (meth)acrylic acid and its salts, and even more preferably, sodium acrylate. It should be noted that, in this specification, "(meth)acrylic acid" refers to acrylic acid and methacrylic acid.
[0060] As a polymerization method, conventional free radical polymerization methods can be applied. As a polymerization form, solution polymerization and dropwise polymerization can be applied. Free radical polymerization using water-soluble free radical polymerization initiators and in aqueous solutions with low chain transfer effects is suitable. In the case of obtaining high viscosity products, copolymerization is preferred, in which the monomers are mixed in the aqueous solution. In the case of obtaining medium to low viscosity products, dropwise polymerization, in which individual or one monomer is added, is preferred.
[0061] A solvent is preferably included during polymerization. A more preferred solvent is water, preferably pure water treated with an ion exchange resin. Ultrapure water is even more preferred.
[0062] It is preferable to polymerize while stirring.
[0063] More preferably, the reaction system is mixed using a device that combines a motor, shaft, and stirring blades. It is particularly preferable to adjust the stirring speed according to the progress of the polymerization reaction. Regarding the shape of the stirring blades, turbine blades, paddle blades, propeller blades, anchor blades, and three-bladed swept-back blades are all acceptable. In each case, only the appropriate material needs to be used; however, in the case of medium to low viscosity as described in this embodiment, three-bladed swept-back blades are suitable.
[0064] It is preferred to obtain a polymer with a uniform and appropriate molecular weight distribution by means of stirring during the manufacture of the polymer of the present invention.
[0065] As polymerization initiators, substances commonly used in the free radical polymerization of vinyl compounds can be used without limitation. Examples include redox polymerization initiators, azo compound polymerization initiators, and peroxide polymerization initiators. They can be used individually or in combination of two or more. Depending on the circumstances, chain transfer agents can be used to adjust the molecular weight.
[0066] Examples of redox polymerization initiators include combinations of ammonium persulfate with sodium thiosulfate, sodium thiosulfate, trimethylamine or tetramethylethylenediamine, and combinations of tert-butyl hydroperoxide with sodium thiosulfate or sodium thiosulfate.
[0067] Examples of peroxide-based polymerization initiators include persulfates of sodium, potassium, and ammonium, benzoyl peroxide, lauroyl peroxide, hexanoyl peroxide, tert-butyl peroxyisooctanoate, and diacetyl peroxide.
[0068] Examples of polymerization initiators for azo compounds include 2,2'-azobis(2-methylbutyronitrile), 2,2'-azobis(2,4-dimethylpentanonitrile), dimethyl-2,2'-azobis(isobutyrate), dimethyl-2,2'-azobis(2-methylbutyrate), dimethyl-2,2'-azobis(2,4-dimethylpentanonitrile), 2,2'-azobis(2-amidinylpropane) dihydrochloride, and 2,2'-azobis[2-(2-imidazolin-2-yl)propane]. Dihydrochloride, 2,2'-azobis[N-(2-carboxyethyl)-2-methylpropanediamine]n hydrate, 2,2'-azobis{2-[N-(2-carboxyethyl)amidine]propane}n hydrate, 2,2'-azobis(2-methylpropionic acid)dimethyl ester, 2,2-azobis(2-methylpropionic acid)dimethyl ester, etc.
[0069] Among the above-mentioned polymerization initiators, for polymerization methods using water as the solvent, considering the impact of halogen-containing residues in the polymer on the coating agent, electronic devices, heat resistance, and especially heat discoloration properties, a halogen-free azo compound polymerization initiator is preferred. 2,2'-azobis[N-(carboxyethyl)-2-methylpropanediamine] tetrahydrate (trade name: Fujifilm Wako Pure Medicine Co., Ltd., azo compound polymerization initiator VA-057) is even more preferred.
[0070] The amount of free radical polymerization initiator used relative to 100 parts by mass of all monomers is preferably 0.05 parts by mass or more and 2.0 parts by mass or less, more preferably 0.1 parts by mass or more and 0.8 parts by mass or less, and even more preferably 0.4 parts by mass or more and 0.7 parts by mass or less, relative to 100 parts by mass of all monomers. In the case of redox polymerization initiators, the amount is preferably 0.001 parts by mass or more and 0.03 parts by mass or less, more preferably 0.003 parts by mass or more and 0.01 parts by mass or less, and even more preferably 0.004 parts by mass or more and 0.009 parts by mass or less, relative to 100 parts by mass of all monomers. When the amount of free radical polymerization initiator used is within the above range, the polymerization rate and the molecular weight of the copolymer are easily made suitable.
[0071] For such a manufacturing method, it is preferable to add a liquid containing at least a polymerization initiator dropwise to an aqueous medium solution of the monomer for polymerization. Furthermore, when a copolymer component is included, it is also preferable to add the aqueous medium solution constituting the copolymer dropwise to the aqueous medium solution of the monomer.
[0072] Chain transfer agents can be used during copolymerization for the purpose of adjusting the degree of polymerization of the polymer and introducing modifying groups at the ends of the copolymer, provided that the scope of the invention is not impaired. Examples of chain transfer agents include aldehydes such as acetaldehyde and propionaldehyde, ketones such as acetone and methyl ethyl ketone, thiols such as 2-hydroxyethanethiol, 3-mercaptopropionic acid, dodecyl mercaptan, and thioacetic acid, halogenated hydrocarbons such as carbon tetrachloride, trichloroethylene, and perchloroethylene, and phosphines such as sodium hypophosphite monohydrate. Thiols, aldehydes, and ketones are particularly suitable among these. The amount of chain transfer agent added is preferably 0.1 parts by mass or more and 2.0 parts by mass or less relative to 100 parts by mass of all monomers. Within this range, the purposes of adjusting the degree of polymerization and introducing modifying groups at the ends of the polymer can be fully realized.
[0073] In addition, regarding the mixing method, it can be carried out by stirring in a tank, or it can be added during the mixing process and mixed as a mixture.
[0074] The polymerization temperature is preferably 30–100°C. More preferably 60–98°C, and most preferably 70–95°C.
[0075] The obtained polymer can also be dried and made into powder.
[0076] Specifically, powdering can be achieved through cryogenic pulverization, dry curing pulverization, spray drying, etc., but spray drying is the preferred method.
[0077] (3) Protective film agent
[0078] The protective film agent of this embodiment comprises the polymer described above. Further, it may include additives such as solvents and light absorbers, as needed.
[0079] Specifically, there are no particular limitations on the solvent; examples include water, alcohols and their derivatives, and esters. Examples of alcohols include monohydric alcohols such as methanol, ethanol, propanol, and butanol, and polyhydric alcohols such as ethylene glycol, diethylene glycol, and propylene glycol. Furthermore, examples of alcohol derivatives include... Ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monopropyl ether, ethylene glycol monobutyl ether, etc.; ethylene glycol monoalkyl ethers, ethylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether acetate, etc.; propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monopropyl ether, propylene glycol monobutyl ether, etc.; propylene glycol monoalkyl ethers, propylene glycol monomethyl ether acetate, propylene glycol monoethyl ether acetate, propylene glycol monopropyl ether acetate, propylene glycol monobutyl ether acetate, etc.
[0080] Examples of esters include methyl 3-methoxypropionate and ethyl 3-ethoxypropionate.
[0081] Among these, water with high rinsing properties is the preferred choice. It should be noted that one or more solvents can be used in combination.
[0082] Such a protective film agent can be used as a variety of protective film agents, such as a protective film agent for laser processing.
[0083] Protective film agents can be applied to the surface of substrates such as wafers using spin coaters, sprayers, etc. However, to prevent repulsion from the substrate surface, improve wetting and coating properties, and further enhance the storage stability of the solution, protective film agents may also contain surfactants. Any surfactant, whether nonionic or cationic, can be used.
[0084] Examples of nonionic surfactants include, for example, nonylphenol, higher alcohols, polyols, polyoxyethylene glycols, polyoxyethylene alkyl esters, polyoxyethylene alkyl ethers, polyoxyethylene alkylphenol ethers, and polyoxyethylene sorbitol alkyl esters.
[0085] In addition, examples of cationic surfactants include quaternary ammonium salts and amine salts; examples of anionic surfactants include alkylbenzene sulfonic acids and their salts, alkyl sulfate ester salts, methyl taurate, ether sulfonates, etc.; and examples of amphoteric surfactants include imidazolines. Betaine-based, amyl betaine-based, and aminodipropionate-based surfactants, etc. One or more of these surfactants can be selected and used appropriately. It is generally preferable to use surfactants at 0.05% to 5% by mass relative to the total amount of the protective film agent as the active ingredient.
[0086] There are no particular limitations on the absorbent, and examples include ultraviolet absorbers and pigments, among which water-soluble substances are preferred.
[0087] Examples of UV absorbers include, for example, benzophenone-based UV absorbers {e.g., polyhydroxybenzophenone (e.g., 2,2',4,4'-tetrahydroxybenzophenone, 2,2'-dihydroxy-4,4'-dimethoxybenzophenone, 2,4-dihydroxybenzophenone, 2,2'-dihydroxy-4-methoxybenzophenone)}, benzotriazole-based UV absorbers (e.g., 2,2'-methylenebis[6-(benzotriazole-2-yl)-4-tert-octylphenol]), ferulic acid, etc.
[0088] Examples of pigments include food additive pigments {e.g., edible red pigments (e.g., edible red No. 2, edible red No. 40, edible red No. 102, edible red No. 104, edible red No. 105, edible red No. 106), edible yellow pigments (e.g., edible yellow NY, edible yellow No. 4 tartrazine, edible yellow No. 5), edible blue pigments (e.g., edible blue No. 1, edible blue No. 2), edible green pigments (e.g., edible green No. 3)}, etc.
[0089] In addition, water-soluble compounds with flavonoid, flavonol, or isoflavone structures can also be used as absorbents. Representative examples of such compounds include isorhamnetin, flavonols, 4'-hydroxyflavones, 5-hydroxyflavones, farnesin, baicalin, 3-hydroxy-4'-methoxyflavones, 7,8-dihydroxyflavones, ascorbic acid C, quercetin, begaline, norihesperidin, rutin, icariin, icariin, 7-hydroxyflavones, morin, kaempferol, hesperidin, 6-hydroxyflavones, kaempferol, baicalin, isohypericin, 5-methoxyflavones, luteolin, myricetin, 3-methylflavonoid-8-carboxylic acid, 6-methylflavones, apigenin, 3-methoxyflavones, baicalin, 3,4'-dihydroxyflavones, isohypericin, 3' 4'-Dihydroxyflavone, methyl hesperidin, coin, 6-methoxyflavone, hesperidin, geraniol, galangin, flavonoids, zeolite, diosmin, neodiosmin, troxerutin, 2-(2-amino-3-methoxyphenyl)chromone, flavonol-2'-sulfonic acid, flavonol ester, genistein, irisin, styracin, 4',6,7-trihydroxyisoflavone, epaflavone, psoralen isoflavone, sophoroside, irisin, puerarin, chickpea extract A, styracin, irisin, 7-methoxy-5-methylisoflavone, 4',6,7-trimethoxyisoflavone, daidzein, dihydrodaidzein, daidzein.
[0090] In addition, preservatives such as phenyl glycol may be added as needed to adjust the shelf life of the protective film. Furthermore, plasticizers, organic acids, etc., may also be used as needed.
[0091] The proportion of polymer in the protective film agent is not particularly limited, for example, it is 1 to 30% by mass, preferably 1 to 25% by mass, more preferably 1 to 20% by mass, and can be 1 to 15% by mass.
[0092] The proportion of solvent in the protective film agent is not particularly limited, but is preferably 50-99% by mass, more preferably 50-95% by mass, 60-99% by mass, 60-95% by mass, 70-99% by mass, and 70-95% by mass.
[0093] The proportion of light absorber in the protective film agent is not particularly limited, but is preferably 0.01 to 5% by mass, more preferably 0.01 to 3% by mass, 0.01 to 1% by mass, 0.01 to 0.5% by mass, and 0.05 to 0.5% by mass.
[0094] In addition, surfactants are generally only required to be in the range of 0.05% to 5% by mass as an active ingredient relative to the total amount of protective film agent.
[0095] The method for manufacturing the protective film agent of the present invention is not particularly limited. For example, the polymer, solvent, and light absorber, and further, other components as needed, can be mixed. Mixing can be carried out at room temperature or while heating. Furthermore, mixing can also be carried out while stirring. It should be noted that the order in which the components are added is not particularly limited.
[0096] The protective film of the present invention is formed using the above-described protective film agent. Specifically, a protective film can be formed by applying the above-described protective film agent to the surface of a substrate.
[0097] There are no particular limitations on the substrate, and examples include glass, synthetic quartz, resin molded articles, semiconductors (e.g., semiconductor wafers), etc.
[0098] There are no particular limitations on the coating method. It can be appropriately selected according to the type of substrate, etc. For example, a rotary coating machine or a jet coating machine can be used for coating. This process alone can achieve uniform coating.
[0099] The thickness of the protective film is not particularly limited and can be appropriately selected according to the application of the composition, for example, 0.01 to 50 μm, for example, 0.01 to 30 μm, preferably 0.01 to 20 μm (for example, 0.01 to 15 μm), and more preferably 0.01 to 10 μm.
[0100] By processing the substrate through a protective film formed on the surface of the substrate as described above, the substrate can be processed while protecting the non-processed areas.
[0101] There are no particular limitations on the processing method. It can be appropriately selected according to the type of substrate, etc. Examples include machining (e.g., cutting, grinding) and laser processing (e.g., laser cutting).
[0102] The protective film can be removed by washing it after the above processing. The washing method is not particularly limited; the protective film formed by the composition of the present invention can be efficiently removed by washing with water {for example, water, warm water (e.g., warm water at 40–90°C)}.
[0103] Furthermore, by cleaning such a protective film, deposits generated during processing (e.g., melts, thermal decomposition products, etc.) can also be removed efficiently.
[0104] Example
[0105] The following embodiments further illustrate this implementation in detail, but they are illustrative and not limited to these embodiments.
[0106] The following evaluations were conducted in the embodiments and comparative examples.
[0107] Viscosity Measurement
[0108] The plastic bottle containing the sample was immersed in a circulating constant temperature water bath at 20℃, and the temperature was adjusted so that the internal polymer aqueous solution was 20℃±0.5℃.
[0109] After reaching this temperature, the viscosity was measured using a Type B viscometer as shown in JIS K-7117-1-1999. The value after 5 minutes at 50 rpm was recorded as the measured value.
[0110] Molecular weight determination
[0111] Each material was dissolved in the eluent and allowed to stand for 20 hours. The concentration of solids in the solution was 0.1% by mass.
[0112] The solution was filtered using a 0.45 μm membrane filter, and the weight-average molecular weight (Mw) of the filtrate was determined using GPC-MALS (multi-angle light scattering detector).
[0113] MALS Detector: Made by Towtech Instruments Co., Ltd. DAWN HELEOS 8+ pillars: Resonak Shodex Co., Ltd. (registered trademark) SB-G 8B, SB-807HQ×2, SB-806M-HQ pillars Temperature: 40℃ Eluent: Adjusted to pH 9.0 using a 0.025 mol sodium bicarbonate and 0.025 mol sodium carbonate aqueous solution. Flow rate: 0.7 mL / min Sample injection volume: 300 μL Laser wavelength: 633nm Multi-angle fitting method: Zimm method
[0114] Residual rate test
[0115] Using a 60ml aluminum dish manufactured by Kenis Corporation, the weight of the dish was measured beforehand. Then, 30g of a water-soluble polymer aqueous solution was added, and the mass was measured. This mass was set as the initial mass.
[0116] The aluminum dish was placed in an oven set to 250°C and left to stand. After one hour, the dish was removed and allowed to cool. The oven used was a DRA330DC Adband Toyo Co., Ltd.
[0117] Then, the aluminum dish was placed in a covered resin container with 1000g of water and left to stand at room temperature for 15 hours. After 15 hours, the aluminum dish was removed and placed in an oven at 150°C. The weight of the aluminum dish was measured after 1 hour.
[0118]
[0119] In the residual rate calculated using the number 1, materials with a residual rate of 10% or higher are judged as unqualified.
[0120] Appearance changes
[0121] The initial state and the state after a period of time at 250°C were compared and determined using the following criteria.
[0122] 〇: Less coloring, no degradation observed
[0123] ×: Significant color degradation.
[0124] Membrane evaluation
[0125] The uniformity of spreading onto silicon wafers was evaluated using a spin coater (Blue Oscintillation Co., Ltd. AJC-300-BOT). The silicon wafer used was AKD Co., Ltd. 4-520P1FME.
[0126] Conditions: 5000 rpm, 10 ssec, sample 0.5 g, 46
[0127] 〇: Uniform, thin film state
[0128] ×: Uneven, thick film state
[0129] <Comprehensive Judgment>
[0130] A comprehensive judgment was made using the following criteria.
[0131] ○: Dissolution residue rate less than 10%, film-forming property evaluation ○, appearance change ○
[0132] ×: In addition to this
[0133] FT-IR
[0134] The evaluation was conducted using Thermo Scientific Nicolet iS20.
[0135] [Example 1]
[0136] PDMA medium to high molecular weight
[0137] Polymer production
[0138] A nitrogen inserter, stirrer, solvent dropper, thermometer, and nitrogen exhaust pipe were installed in a 2L detachable flask with four necks. An aqueous solution was prepared in the detachable flask by dissolving 70g of N,N-dimethylacrylamide in 700g of ion-exchanged water.
[0139] Then, while introducing nitrogen gas into the system at a rate of 200 ml / min, the internal temperature was raised to 58°C. Two hours after the start of heating, 20 g of an aqueous solution containing 0.48 g (0.6% by mass) of 2,2'-azobis[N-(carboxyethyl)-2-methylpropanediamine] tetrahydrate (trade name: Fuji Film Wako Pure Medicine Co., Ltd., azo compound polymerization initiator VA-057, hereinafter also referred to as "initiator VA-057") was added using a syringe. The polymerization was carried out by stirring for 4 hours at an internal temperature of 58.0–68.0°C. Then, the temperature bath was raised to 80°C, and the internal temperature was maintained at 75°C for 1 hour. The outside of the container was then cooled with tap water at 23°C, and the container was left to cool until the next day.
[0140] The obtained polymer (PDMA-103) was evaluated for its heat resolubility, appearance, and film-forming properties. The results are shown in Table 1.
[0141] [Example 2]
[0142] Medium molecular weight PDMA
[0143] A 1L detachable flask with four necks was fitted with a nitrogen insert, stirrer, solvent dropper, thermometer, and nitrogen vent. 350g of ion-exchanged water was added to the flask, and the internal temperature was raised to 68.0℃. Simultaneously, 65g of N,N-dimethylacrylamide was added to a 500ml flask, followed by 204.3g of ion-exchanged water, and the mixture was stirred. Two hours after the start of heating, at an internal temperature of 68.0℃, 20g of an aqueous solution containing 0.293g of initiator VA-057 (monomer ratio 0.45 by mass) was added to the 1L flask using a syringe. This solution was then added dropwise to the N,N-dimethylacrylamide solution mixed in the 500ml flask using a pump.
[0144] The polymerization was carried out dropwise over 2.5 hours with stirring at an internal temperature of 68.0–72.0°C. Then, the temperature bath was set to 80°C, and the internal temperature was maintained at 75°C for 1 hour. After stirring for dilution for about 1 hour, the external temperature of the container was cooled with tap water and then allowed to cool.
[0145] The obtained polymer (PDMA-104) was evaluated in the same way as in Example 1.
[0146] Regarding Example 2, the polymer heated to 250°C was confirmed by FT-IR.
[0147] [Example 3]
[0148] PDMA low molecular weight
[0149] Install a nitrogen insert tube, stirrer, solvent dropper, thermometer, and nitrogen exhaust tube on a 1L detachable flask with four necks. Add 600g of ion-exchanged water to the detachable flask. While introducing nitrogen into the system at a rate of 200ml / min, start heating to adjust the internal temperature to 90.0℃.
[0150] Simultaneously, 107g of N,N-dimethylacrylamide was added to a 500ml flask, followed by 200g of deionized water, and the mixture was dissolved and mixed. Next, 3.2g of initiator VA-057 (monomer ratio 2.99% by mass) was measured into a 200ml beaker, and 100g of deionized water was added, and the mixture was dissolved and mixed.
[0151] Two hours after the start of heating, the dissolved initiator VA-057 was added dropwise to a 1L flask using a pump at an internal temperature of 90.0°C. Then, N-vinylacetamide dissolved in water was added dropwise to a 500ml flask using a pump. Polymerization was carried out by adding the solution dropwise while stirring at an internal temperature of 90.0–95.0°C for 2.5 hours. After stirring and maintaining the solution at 90.0–95.0°C for 30 minutes, a liquid obtained by dissolving 0.5g of initiator VA-057 in 55g of deionized water was added using a pump. The mixture was then stirred and maintained at 90.0–95.0°C for 30 minutes. The container was then cooled to a comfortable temperature using tap water.
[0152] The obtained polymer (PDMA-107) was evaluated in the same way as in Example 1.
[0153] [Comparative Example 1]
[0154] PDMA high molecular weight type
[0155] (Weight-average molecular weight: 1.5 million to 4 million)
[0156] A nitrogen insert tube, stirrer, solvent dropper, thermometer, and nitrogen exhaust pipe were installed in a 2L detachable flask with four necks. An aqueous solution was prepared in the detachable flask by dissolving 66.1g of N,N-dimethylacrylamide in 708.0g of ion-exchanged water.
[0157] Then, the internal temperature was adjusted to 53.5℃ by raising the temperature. 10g of an aqueous solution containing 0.053g of polymerization initiator (VA-057) (monomer ratio 0.08% by mass) was added using a syringe, and polymerization was carried out while stirring for 4 hours at an internal temperature of 50.0–62.0℃. Then, the temperature bath was raised to 80℃, and the internal temperature was maintained at 75℃ for 1 hour. 865.4g of dilution deionized water was then added, and stirring continued for approximately 1 hour. Finally, the container was cooled to 23℃ using tap water.
[0158] The obtained polymer (PDMA-043) was evaluated in the same manner as in Example 1.
[0159] [Comparative Examples 2-5]
[0160] The following polymers were used, adjusted to the concentrations shown in Table 1, and evaluated in the same manner as in Example 1.
[0161] Regarding Comparative Example 2, the polymer heated to 250°C was confirmed by FT-IR.
[0162] Comparative Example 2: Polyvinyl alcohol (PVA) PVA124 5% aqueous solution (by Clare Co., Ltd.)
[0163] Comparative Example 3: Polyvinylpyrrolidone (PVP) K-90 10% by mass aqueous solution (Nippon Shokubai Co., Ltd.)
[0164] Comparative Example 4: Sodium Carboxymethyl Cellulose (CMC) Sunroes (CMC) 350HC 2% by mass aqueous solution Nippon Paper Co., Ltd.
[0165] Comparative Example 5: Polyethylene Glycol (PEG) PEG500000 Reagent 10% (w / w) Aqueous Solution Fuji Film & Wako Pure Medicine Co., Ltd.
[0166] [Table 1]
[0167] Regarding Examples 1-3, the residual rate was less than 10%, and the change in the appearance of the material after the test was minimal. Regarding Comparative Example 1, judging from the changes in resolubility and appearance, it can be considered that there was no deterioration, but due to its high viscosity, its film-forming properties were low.
[0168] On the other hand, Comparative Examples 2, 3, and 4 showed high residue rates and significant changes in appearance. In Comparative Example 5, even after the moisture disappeared during the heating test at 250°C, evaporation continued, indicating that decomposition had occurred.
[0169] Furthermore, the state of the polymers in Example 2 and Comparative Example 2 after heating to 250°C was confirmed by FT-IR. Regarding Example 2, no changes were observed in appearance, similar to the previous observations. However, regarding Comparative Example 2, the state of the polymers after heating to 250°C was confirmed by FT-IR. -1 The number of C=O bond sites around the periphery increased significantly, confirming a substantial promotion of oxidative degradation.
Claims
1. A polymer comprising the structural unit shown in formula (1) below, In formula (1), R 1 ~R 5 represents any of a hydrogen atom, an alkyl group having 1 to 8 carbon atoms, and a hydroxyalkyl group, The polymer is either (i) a homopolymer of the structural unit or (ii) a copolymer of the structural unit with a structural unit derived from other monomers, wherein the other monomers are at least one monomer selected from N-vinylcarboxylic acid amides, unsaturated carboxylic acid monomers, salts of unsaturated carboxylic acid monomers, unsaturated carboxylic acid ester monomers, vinyl ester monomers, and unsaturated nitrile monomers. The polymer has a weight-average molecular weight of less than 1 million.
2. The polymer according to claim 1, which has a viscosity of 100 mPa s or more and 15000 mPa s or less for a 10 mass% aqueous solution thereof.
3. The polymer according to claim 1, wherein the content of the other monomer structural units is less than 90 mol% of all structural units in the polymer (100 mol%).
4. The polymer according to claim 1, wherein the weight-average molecular weight is in the range of more than 30,000 and less than 1,000,000.
5. A protective film agent comprising the polymer according to any one of claims 1 to 4.
6. The protective film agent according to claim 5, further comprising a light absorber.
7. A protective film using the protective film agent of claim 6.
Citation Information
Patent Citations
Protective film agent for laser processing
JP2015134373A
Protection film composition, method for manufacturing semiconductor device, and laser dicing method
JP2016066768A
Protective film agent for laser processing
JP2019012807A
Protective film-forming composition