Pressure-sensitive adhesives comprising acrylic copolymers and polyalkylene oxide polymers and related articles

By using a combination of acrylic copolymers and polyoxyethylene polymers, the balance between water vapor permeability and adhesive properties of pressure-sensitive adhesives is solved, providing a water vapor permeable pressure-sensitive adhesive with excellent viscoelasticity to meet a variety of application requirements.

CN123165433APending Publication Date: 2026-11-243M INNOVATIVE PROPERTIES CO
View PDF 46 Cites 0 Cited by

Patent Information

Application Number
CN202580027440.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2024-04-18
Filing Date
2025-04-18
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing pressure-sensitive adhesives struggle to strike a balance between maintaining water vapor permeability and adhesive properties, resulting in inadequate performance in some applications.

Method used

A pressure-sensitive adhesive formulation containing acrylic copolymers and polyoxyethylene polymers without fluorinated carbon atoms is formed by copolymerizing linear or branched alkyl acrylates and acrylic monomer units in a specific ratio, combined with the use of a crosslinking agent, to create a pressure-sensitive adhesive with excellent viscoelasticity.

Benefits of technology

It achieves a water vapor permeable pressure-sensitive adhesive with good adhesion, holding power and cohesive strength, meeting a variety of application requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123165433A_ABST
    Figure CN123165433A_ABST
Patent Text Reader

Abstract

A pressure-sensitive adhesive comprises an acrylic copolymer and a polyoxyethylene polymer without fluorinated carbon atoms. The acrylic copolymer comprises at least 60% by weight of linear or branched alkyl (meth)acrylate monomer units based on the weight of the acrylic copolymer, and 12.5% ​​to 40% by weight of (meth)acrylate monomer units based on the weight of the acrylic copolymer. An article comprises the pressure-sensitive adhesive disposed on a backing. The article may be water vapor permeable. A method for preparing the pressure-sensitive adhesive is also disclosed.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] Cross-references to related applications

[0002] This application claims priority to U.S. Provisional Applications No. 63 / 635,815 and No. 63 / 635,837, filed April 18, 2024, the disclosure of which is incorporated herein by reference in its entirety. Background Technology

[0003] Water vapor permeable air and water barrier articles are disclosed in U.S. Patent Nos. 10,704,254 (Seabaugh et al.), 11,105,089 (Widenbrant et al.), 11,365,328 (Seabaugh et al.), 11,512,463 (Widenbrant et al.), and 11,731,394 (Seabaugh et al.), as well as U.S. Patent Application Publications Nos. 2017 / 0173916 (Widenbrant et al.), 2021 / 0207005 (Seabaugh et al.), and 2022 / 0282476 (Widenbrant et al.). Self-adhesive permeable diaphragms for use in buildings are disclosed in U.S. Patent Nos. 10,899,107 (Bess) and 9,562,174 (Russell). Summary of the Invention

[0004] In one aspect, this disclosure provides a pressure-sensitive adhesive comprising an acrylic copolymer and a polyoxyethylene polymer without fluorinated carbon atoms. The acrylic copolymer comprises at least 60% by weight of linear or branched alkyl (meth)acrylate monomer units based on the weight of the acrylic copolymer, and from 12.5% ​​to 40% by weight of (meth)acrylate monomer units based on the weight of the acrylic copolymer. Typically, and advantageously, the pressure-sensitive adhesive is water vapor permeable.

[0005] In another aspect, this disclosure provides an article comprising a pressure-sensitive adhesive disposed on a backing. Typically, and advantageously, the article is water vapor permeable.

[0006] In another aspect, this disclosure provides a method for preparing a pressure-sensitive adhesive. The method includes partially polymerizing a first polymerizable composition comprising a linear or branched alkyl (meth)acrylate and (meth)acrylic acid to form a slurry composition. The method further includes combining the slurry composition with a polyoxyethylene polymer and optionally a crosslinking agent to provide a second polymerizable composition, and polymerizing the second polymerizable composition to form a pressure-sensitive adhesive.

[0007] In this application, terms such as “a,” “an,” and “the / described” are not intended to refer to a single entity, but rather to include a general category encompassing specific examples that can be used for illustration. The terms “a,” “an,” and “the / described” are used interchangeably with the term “at least one (a kind).” Phrases such as “at least one of…” and “containing at least one of…” followed by the conjunction “or” in a list refer to any item in the list and any combination of two or more items in the list. Unless otherwise indicated, all numerical ranges include the endpoints and are non-integer values ​​between the endpoints (e.g., 1 to 5, including 1, 1.5, 2, 2.75, 3, 3.8, 4, and 5, etc.).

[0008] As used herein, the term “vapor-permeable” means an article that, according to ASTM E 96 Procedure A (desiccant method), has a permeability greater than 1 perm (inch-pound) (57.2135 nanograms / second / square meter / pascal (ng·s·m²·Pa)).

[0009] As used herein, the term "continuous" refers to a coating that extends uninterruptedly along a two-dimensional surface. For example, in some embodiments, in articles having a continuous pressure-sensitive adhesive layer, the pressure-sensitive adhesive covers the main surface of the backing.

[0010] As used herein, the term "discontinuous" means a coating that extends intermittently along a two-dimensional surface. For example, in some embodiments, in an article having a discontinuous coating of pressure-sensitive adhesive, the pressure-sensitive adhesive does not cover the main surface of the backing.

[0011] The term "polymer" refers to a molecule having a structure comprising multiple repeating units, actually or conceptually derived from one or more monomers. The term "monomer" refers to a molecule with a relatively low molecular weight that can combine with other molecules to form a polymer. The term "polymer" includes homopolymers and copolymers, as well as homopolymers or copolymers that can be formed in miscible blends (e.g., by co-extrusion or by reaction). The term "polymer" includes random polymers, block polymers, graft polymers, and star polymers. The term "polymer" includes oligomers.

[0012] A "monomer unit" of a polymer or oligomer is a segment of the polymer or oligomer derived from a single monomer. For example, the monomer unit of acrylic acid (H₂C=CH-(C=O)-OH) is...

[0013] Among them, the asterisk ( ) indicates the connection site with another group (such as another monomer unit in the polymer).

[0014] The term "acrylic" refers to acrylic and methacrylic polymers, oligomers and monomers.

[0015] The term “(meth)acryl” refers to acryl (also known in the art as acryloyl / acrylyl) and / or methacryl (also known in the art as methacryloyl / methacrylyl)).

[0016] Unless otherwise specified, "alkyl group" and the prefix "alkane-" include both straight-chain and branched groups having up to 30 carbon atoms (in some embodiments, up to 20, 15, 12, 10, 8, 7, 6, or 5 carbon atoms) as well as cyclic groups. Cyclic groups can be monocyclic or polycyclic, and in some embodiments, have 3 to 10 cyclic carbon atoms.

[0017] "alkylene" refers to the polyvalent (e.g., divalent or trivalent) form of the "alkyl" group as defined above.

[0018] Those skilled in the art are well aware that pressure-sensitive adhesives (PSAs) possess properties including (1) strong and durable adhesion, (2) adhesion with no more than finger pressure, (3) sufficient ability to hold to the adherend, and (4) sufficient cohesive strength to allow for clean removal from the adherend. Materials found well for use as PSAs are polymers designed and formulated to exhibit the desired viscoelasticity, thus achieving a desired balance of tack, peel strength, and shear retention. One available method for identifying pressure-sensitive adhesives is the Dahlquist criterion. As described in *Handbook of Pressure Sensitive Adhesive Technology*, edited by Donatas Satas, 2nd ed., p. 172, Van Nostrand Reinhold, New York, NY, 1989, this criterion defines a pressure-sensitive adhesive as having a strength greater than 3 × 10⁻⁶. -6 cm 2 / Dyne's creep compliance adhesive. Alternatively, since the modulus is approximately the reciprocal of the creep compliance, pressure-sensitive adhesives can be defined as having a storage modulus of less than approximately 3 × 10⁻⁶. 5 N / m 2 Adhesive. Attached Figure Description

[0019] Figure 1This is a side view of an embodiment of the article of the present disclosure, including a pressure-sensitive adhesive disposed on a backing.

[0020] Figure 2 This is a side view of another embodiment of the article of this disclosure, including a pressure-sensitive adhesive disposed on a backing and a release liner on the pressure-sensitive adhesive.

[0021] Figure 3 This is a side view of yet another embodiment of the article of this disclosure, including a pressure-sensitive adhesive disposed on a multilayer backing and a release liner on the pressure-sensitive adhesive.

[0022] Figure 4 This is a perspective view of another embodiment of the article of this disclosure applied to a window frame. Detailed Implementation

[0023] The pressure-sensitive adhesive (PSA) disclosed herein and / or the pressure-sensitive adhesive (PSA) that can be used in articles of this disclosure comprises an acrylic copolymer and a polyoxyethylene polymer. The acrylic copolymer comprises at least 60 wt%, 65 wt%, or 70 wt% of linear or branched alkyl (meth)acrylate monomer units based on the weight of the acrylic copolymer. In some embodiments, the acrylic copolymer comprises less than 85 wt% or up to 84 wt%, 83 wt%, 82 wt%, 81 wt%, or 80 wt% of linear or branched alkyl (meth)acrylate monomer units based on the weight of the acrylic copolymer. The acrylic copolymer comprises from 12.5 wt% to 40 wt% of (meth)acrylate monomer units based on the weight of the acrylic copolymer. In some embodiments, the acrylic copolymer comprises at least 12.5 wt%, greater than 12.5 wt%, at least 15 wt%, greater than 15 wt%, at least 16 wt%, or at least 17 wt% of (meth)acrylate monomer units based on the weight of the acrylic copolymer. In some embodiments, the acrylic copolymer comprises 15.5% to 40% by weight, 16% to 40% by weight, 16% to 35% by weight, 16% to 30% by weight, 16% to 25% by weight, 17% to 25% by weight, 17% to 23% by weight, 17% to 20% by weight, or 17% to 19.5% by weight of (meth)acrylic acid monomer units based on the weight of the acrylic copolymer.

[0024] In some embodiments, the linear or branched alkyl (meth)acrylate monomer unit is C1-C. 32 (meth)acrylate monomer unit, C1-C 24 (meth)acrylate monomer units or C1-C 18(Meth)acrylate monomer units. Examples of suitable (meth)acrylate alkyl esters that can be used to provide these monomer units include those represented by the formula CH2=C(R)COOR', where R is a hydrogen or methyl group, and R' is an alkyl group having 1 to 30, 4 to 30, 6 to 30, 8 to 30, 6 to 24, 6 to 20, 6 to 18, 8 to 24, 8 to 20, or 8 to 20 carbon atoms, and can be straight-chain or branched. Suitable examples of monomers represented by this formula include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl acrylate, isobutyl acrylate, tert-butyl (meth)acrylate, n-pentyl (meth)acrylate, isoamyl (meth)acrylate, n-hexyl (meth)acrylate, isohexyl (meth)acrylate, octyl (meth)acrylate, isooctyl (meth)acrylate, 2-octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, decyl (meth)acrylate, and isodecyl acrylate. Undecyl acrylate, n-Dodecyl acrylate, lauryl acrylate, tridecyl acrylate, tetradecyl acrylate, pentadecyl acrylate, hexadecyl acrylate, heptadecanyl acrylate, 2-propylheptyl acrylate, stearyl acrylate, n-nonyl acrylate, isononyl acrylate, isomyristyl acrylate, isostearyl acrylate, octadecyl acrylate, and docosyl acrylate.

[0025] Suitable linear or branched alkyl (meth)acrylate monomer units also include a mixture of at least two or at least three structural isomers of the secondary alkyl (meth)acrylate of formula (I):

[0026] Where R 1 and R 2 Each independently is C1 to C 30 Saturated straight-chain alkyl groups, wherein R 1 and R 2 The total number of carbon atoms in them ranges from 7 to 31, and R 3 It is H or CH3. In some implementations, R 1 and R 2 The total number of carbons in the monomers can be 7 to 27, 7 to 25, 7 to 21, 7 to 17, 7 to 11, or 7. Methods for preparing and using such monomers and monomer mixtures are described in U.S. Patent No. 9,102,774 (Clapper et al.).

[0027] In some embodiments, the linear or branched alkyl (meth)acrylate monomer unit is low-T g Single unit cell. Low T g Monomers provide homopolymers with a glass transition temperature (Tg) not exceeding 20°C. g The thermal transition of monomers, such as homopolymers, is reported in sigmaaldrich.com: Glass Transition Temperature and Melting Point. Glass transition temperature tables for homopolymers are also available from various monomer suppliers, such as Polyscience and BASF. Low T g Examples of monomers include n-butyl acrylate, isobutyl acrylate, sec-butyl acrylate, isoamyl acrylate, n-hexyl acrylate, 2-methylbutyl acrylate, 4-methyl-2-pentyl acrylate, 2-methylhexyl acrylate, n-octyl acrylate, 2-octyl acrylate, isooctyl acrylate, 2-ethylhexyl acrylate, nonyl acrylate, isononyl acrylate, n-decyl acrylate, isodecyl acrylate, undecyl acrylate, dodecyl acrylate, lauryl acrylate, isotridecyl acrylate, isostearyl acrylate, and octadecyl acrylate. In some embodiments, the linear or branched (meth)acrylate alkyl ester monomer unit is a unit of n-butyl acrylate, n-octyl acrylate, 2-octyl acrylate, isooctyl acrylate, 2-ethylhexyl acrylate, 2-propylheptyl acrylate, or isononyl acrylate.

[0028] Examples of (meth)acrylic acid monomer units include acrylic acid, methacrylic acid, itaconic acid, maleic acid, fumaric acid, ethylacrylic acid, crotonic acid, citracic acid, cinnamic acid, ethyl β-carboxyacrylate, and 2-methacryloyloxyethyl succinate. In some embodiments, the (meth)acrylic acid monomer unit is an acrylic acid monomer unit or a methacrylic acid monomer unit. The (meth)acrylic acid monomer unit includes salts of these acids, such as alkali metal salts and ammonium salts.

[0029] In some embodiments, the acrylic copolymers used in the PSA of this disclosure further comprise monomer units of a "high Tg" monomer that, upon polymerization, provides a homopolymer having a glass transition temperature (Tg) of at least 50°C, 60°C, or 70°C (i.e., the homopolymer formed from the monomer has a Tg of at least 50°C, 60°C, or 70°C). In some embodiments, the acrylic copolymers further comprise at least 5% by weight (in some embodiments, at least 7.5% by weight, 10% by weight, 12.5% ​​by weight, or 15% by weight) monomer units of a "high Tg" monomer. Some suitable high-Tg monomers include methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, sec-butyl methacrylate, tert-butyl methacrylate, cyclohexyl methacrylate, isobornyl methacrylate, stearyl methacrylate, phenyl acrylate, benzyl methacrylate, 3,3,5-trimethylcyclohexyl methacrylate, tert-butylcyclohexyl methacrylate, 2-phenoxyethyl methacrylate, N-octyl(meth)acrylamide, tetrahydrofurfuryl methacrylate, and mixtures thereof. Other suitable high-Tg monomers have a single vinyl group that is not a (meth)acryloyl group, such as various vinyl ethers (e.g., vinyl methyl ether), vinyl esters (e.g., vinyl acetate and vinyl propionate), styrene, substituted styrene (e.g., α-methylstyrene), vinyl halides, and mixtures thereof. The Tg of many homopolymers is reported in the section on thermal transition, glass transition, and melting point of homopolymers (sigmaaldrich.com). Glass transition temperature gauges for homopolymers are also available from various monomer suppliers, such as Polyscience and BASF.

[0030] Other optional monomers that may be used in some embodiments of the acrylic copolymers of the PSA disclosed herein include (meth)acrylamide (e.g., acrylamide, methacrylamide, N-ethylacrylamide, N-hydroxyethylacrylamide, N-octylacrylamide, N-tert-butylacrylamide, N,N-dimethylacrylamide, N,N-diethylacrylamide, N-ethyl-N-dihydroxyethylacrylamide, and the methacrylamide of the aforementioned acrylamides), hydroxy-functional (meth)acrylates (e.g., 2-hydroxyethylacrylate or methacrylate), N-vinylpyrrolidone, N-vinylcaprolactam, α-olefins, vinyl ethers, allyl ethers, or maleates.

[0031] In some embodiments, the acrylic copolymers that can be used in the PSA of this disclosure are crosslinked. The acrylic copolymers can be crosslinked by including a crosslinking agent in the formulation. Examples of crosslinking agents include copolymerizable polyfunctional olefinically unsaturated monomers, such as those described below; olefinically unsaturated compounds that are capable of hydrogen abstraction in an excited state (such as acrylated benzophenone, for example, as described in U.S. Patent No. 4,737,559 (Kellen et al.); p-acryloyloxybenzophenone, available from Sartoma Company, Ekdon, Pennsylvania; and monomers described in U.S. Patent No. 5,073,611 (Rehmer et al.), including p-N-(methacryloyl-4- Oxapentamethylene)-carbamoyloxybenzophenone, N-(benzoyl-p-phenylene)-N'-(methacryloyloxymethylene)-carbodiimide, and p-acryloyloxybenzophenone; nonionic crosslinkers that are substantially free of olefinic unsaturated groups and capable of reacting with, for example, the carboxylic acid groups in the second monomer described above (such as 1,4-bis(ethyleneiminocarbonylamino)benzene; 4,4-bis(ethyleneiminocarbonylamino)diphenylmethane; 1,8-bis(ethyleneiminocarbonylamino)octane; 1,4-toluene diisocyanate; 1, 6-Hexamethylene diisocyanate, N,N'-bis-1,2-propylidene isophthalamide, diepoxide, dianhydride, bis(amide) and bis(imide); and nonionic crosslinking agents that are substantially free of olefinic unsaturated groups, cannot copolymerize with the first and second monomers, and are capable of hydrogen abstraction in the excited state (such as 2,4-bis(trichloromethyl)-6-(4-methoxy)phenyl)triazine; 2,4-bis(trichloromethyl)-6-(3,4-dimethoxy)phenyl)triazine; 2,4-bis(trichloromethyl)-6-(3, 4,5-Trimethoxy)phenyl)triazine; 2,4-bis(trichloromethyl)-6-(2,4-dimethoxy)phenyl)triazine; 2,4-bis(trichloromethyl)-6-(3-methoxy)phenyl)triazine, as described in U.S. Patent No. 4,330,590 (Vesley); 2,4-bis(trichloromethyl)-6-naphthyl-s-triazine and 2,4-bis(trichloromethyl)-6-(4-methoxy)naphthyl-s-triazine, as described in U.S. Patent No. 4,329,384 (Vesley). In some embodiments, the acrylic copolymer is crosslinked with a triazine; in some embodiments, it is crosslinked with any of the aforementioned triazines. If a photocrosslinking agent is used, the coated adhesive can be exposed to ultraviolet (UV) radiation with wavelengths from about 250 nm to about 400 nm. The radiation energy required in this wavelength range for crosslinking the adhesive is about 100 mJ / cm². 2 Approximately 1,500 mJ / cm 2 Or, in some implementations, approximately 200 millijoules / cm 2 Approximately 800 millijoules / cm 2.

[0032] Suitable copolymerizable polyfunctional olefinically unsaturated monomers include diacrylates of diols, such as ethylene glycol diacrylate, diethylene glycol diacrylate, propylene glycol diacrylate, butanediol diacrylate, butane-1,3-dimethyl diacrylate, pentanediol diacrylate, hexanediol diacrylate (including 1,6-hexanediol diacrylate), heptadecyl glycol diacrylate, octyl glycol diacrylate, nonanediol diacrylate, decanedyl glycol diacrylate, and dimethacrylates of any of the aforementioned diacrylates. Other suitable polyfunctional monomers include polyacrylates of polyols, such as glycerol triacrylate, dipropylene glycol diacrylate, tripropylene glycol diacrylate, trimethylolpropane triacrylate, pentaerythritol tetraacrylate, neopentyl glycol diacrylate, dipentaerythritol pentaacrylate, methacrylates of the aforementioned acrylates, and combinations thereof. Other suitable multifunctional crosslinking monomers include divinylbenzene, allyl methacrylate, diallyl maleate, diallyl phthalate, and combinations thereof. Further suitable multifunctional crosslinking monomers include multifunctional acrylate oligomers containing two or more acrylate groups. Multifunctional acrylate oligomers can be urethane acrylate oligomers, epoxy acrylate oligomers, polyester acrylates, polyether acrylates, polyacrylate acrylates, methacrylates of any of the aforementioned acrylates, or combinations thereof. Any combination of these crosslinking agents is available.

[0033] Based on the combined weight of monomers, the crosslinking agent (including any of the crosslinking agents described above) may be used in amounts from 0.005 wt% to 4 wt%, for example from about 0.01 wt% to about 2 wt%, or from about 0.05 wt% to 1 wt%. In some embodiments, based on the total weight of monomer units in the acrylic copolymer, the crosslinking agent is used in amounts of up to 4.0 wt%, 3.0 wt%, 2.0 wt%, or 1.0 wt%. In some embodiments, based on the total weight of monomer units in the acrylic copolymer, the crosslinking agent is used in amounts of at least 0.10 wt%, 0.15 wt%, 0.20 wt%, 0.25 wt%, 0.30 wt%, 0.40 wt%, 0.50 wt%, 0.60 wt%, or 0.70 wt%.

[0034] In some embodiments of the PSA disclosed herein, the acrylic copolymer has a T value in the range of 2°C to 100°C, between 2°C and 80°C, between 2°C and 60°C, between 2°C and 50°C, between 2°C and 45°C, between 5°C and 45°C, between 5°C and 40°C, between 5°C and 35°C, or between 10°C and 30°C. g .

[0035] Mixtures of acrylic copolymers can be used in the PSA of this disclosure. However, in some embodiments, the PSA of this disclosure comprises no more than 5 wt%, 4 wt%, 3 wt%, 2 wt%, 1 wt%, or 0 wt% of an additional acrylic copolymer having 0.1 wt% to 15 wt% (in some embodiments, 0.1 wt% to 14.5 wt%, 0.1 wt% to 12 wt%, 0.1 wt% to 11 wt%, 0.1 wt% to 10 wt%, 0.2 wt% to 10 wt%, 0.2 wt% to 9 wt%, 0.2 wt% to 8 wt%, 0.3 wt% to 8 wt%, 0.5 wt% to 8 wt%, 0.5 wt% to 6 wt%, 1 wt% to 6 wt%, or 1 wt% to 5 wt%) of (meth)acrylic acid monomer units based on the weight of the additional (meth)acrylate copolymer. Such additional (meth)acrylate copolymer in the PSA of this disclosure tends to reduce the T of the PSA. g Cohesive strength and / or energy storage modulus.

[0036] Acrylic polymers can be analyzed by nuclear magnetic resonance spectroscopy (NMR spectroscopy). 1 H or 13 Analysis using C10 NMR is performed to identify monomer units in the polymer. Depending on the level of crosslinking in the polymer, solid-state or solution NMR may be useful. For solid-state NMR, acrylic polymers can be swollen in a suitable solvent for analysis.

[0037] Acrylic polymers suitable for use in the articles of this disclosure can be prepared by any conventional free radical polymerization method, including solution polymerization, radiation polymerization, bulk polymerization, dispersion polymerization, emulsification polymerization, solvent-free polymerization, and suspension polymerization. In some embodiments, the acrylic copolymers are prepared in a solvent or by solvent-free batch free radical polymerization methods (e.g., using heat, electron beam radiation, or UV radiation). Such polymerization is typically promoted by a polymerization initiator (e.g., a photoinitiator or a thermal initiator). The polymerization initiator is used in an amount that effectively promotes monomer polymerization (e.g., from 0.1 parts by weight to about 5.0 parts by weight or from 0.2 parts by weight to about 1.0 parts by weight based on 100 parts of total monomer content). The resulting copolymers can be random copolymers or block copolymers.

[0038] A typical solution polymerization process is carried out as follows: monomers, a suitable solvent, and optionally a chain transfer agent are added to a reaction vessel, a free radical initiator is added, the reactor is purged with nitrogen, and the reactor is maintained at a high temperature (typically in the range of about 40°C to 100°C) until the reaction is complete, usually for about 1 to 24 hours depending on the batch size and temperature. Examples of solvents include methanol, tetrahydrofuran, ethanol, isopropanol, tert-butanol, acetone, methyl ethyl ketone, methyl acetate, ethyl acetate, toluene, xylene, and ethylene glycol alkyl ethers. These solvents can be used alone or as mixtures thereof. In a typical thermal polymerization process, the monomer mixture is subjected to thermal energy in the presence of a thermal polymerization initiator (i.e., a thermal initiator). Examples of suitable thermal initiators are those available from DuPont under the trade name "VAZO".

[0039] Slurry polymer technology involves partially polymerizing monomers to produce a slurry polymer comprising an acrylic copolymer and unpolymerized monomers. The slurry polymer composition is polymerized to a usable coating viscosity, allowing it to be coated onto a substrate (such as a backing) and further polymerized. In some embodiments, polymerization is carried out in the absence of a solvent (such as ethyl acetate, toluene, or tetrahydrofuran) that does not react with the functional groups of the slurry polymer components. Polymerization can be carried out to achieve a coating viscosity such that the monomer-to-polymer conversion is at most about 20%, 15%, or 10%. Polymerization can be achieved by exposing the slurry polymer composition to light energy in the presence of a photoinitiator. When the desired conversion and viscosity have been achieved, polymerization can be terminated by removing the light source and by quenching propagating free radicals by bubbling air (oxygen) into the solution. In cases where polymerization is initiated, for example using ionizing radiation, an energy-activated initiator may not be required.

[0040] In some embodiments, a free radical photoinitiator can be used for polymerization to prepare acrylic copolymers. In some embodiments, the free radical photoinitiator is a type I (cleavage-type) photoinitiator. Cleavage-type photoinitiators include acetophenone, α-aminoalkylphenyl ketone, benzoin ethers, benzoyl oximes, acyl (e.g., benzoyl)phosphine oxides, acyl (e.g., benzoyl) phosphonates, and mixtures thereof. Examples of available benzoin ethers include benzoin methyl ether and benzoin butyl ether. Examples of suitable acetophenone compounds include 4-diethylaminoacetophenone, 1-hydroxycyclohexylphenyl ketone, 2-benzyl-2-dimethylamino-4'-morpholinobutyroylbenzene, 2-hydroxy-2-methyl-1-phenylprop-1-one, 2,2-dimethoxyacetophenone, and 2,2-dimethoxy-1,2-diphenylethyl-1-one. Examples of suitable acylphosphine oxides, acylphosphonates, and acylphosphonate compounds include bis(2,6-dimethoxybenzoyl)-2,4,4-trimethylpentylphosphine oxide, phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide, ethylphenyl(2,4,6-trimethylbenzoyl)phosphonate, (2,4,6-trimethylbenzoyl)diphenylphosphine oxide, dimethylneoptiylphosphonate, and poly(oxy-1,2-ethylenedimethyl), α,α',α''-1,2,3-propanetriyltri[ω-[[phenyl(2,4,6-trimethylbenzoyl)phosphoryl]oxy]. Other suitable photoinitiators include substituted α-keto alcohols, such as 2-methyl-2-hydroxyphenylacetone; aromatic sulfonyl chlorides, such as 2-naphthalene-sulfonyl chloride; and photoactive oximes, such as 1-phenyl-1,2-propanedione-2-(O-ethoxy-carbonyl)oxime. Many photoinitiators are available, for example, under the trade names “OMNIRAD” and “ESACURE” from IGM Resins, Waalwijk, Netherlands. Two or more of these photoinitiators can also be used in any combination. Additional photoinitiators can be added to the mixture to be coated after the copolymer has been formed (i.e., photoinitiators can be added to the slurry polymer mixture).

[0041] The degree of conversion (from monomer to copolymer) can be monitored by measuring the refractive index of the polymer mixture during irradiation.

[0042] If desired, a chain transfer agent may be added to the monomer mixture to prepare an acrylic copolymer suitable for use in the PSA disclosed herein. Examples of usable chain transfer agents include carbon tetrabromide, alcohols, thiols, and mixtures thereof. In some embodiments, the chain transfer agent comprises at least one of isooctyl mercaptoacetate or carbon tetrabromide.

[0043] Available solvent-free polymerization methods are disclosed in U.S. Patent No. 4,379,201 (Heilmann et al.). Initially, a mixture of a first and second monomer can be polymerized by exposing a portion of the photoinitiator to UV radiation in an inert environment for a duration sufficient to form a coatable base slurry. Subsequently, a crosslinking agent and the remaining photoinitiator can be added to polymerize the mixture. The final slurry containing the crosslinking agent (e.g., the slurry having a Brookfield viscosity of about 100 to about 6000 centipoise at 23°C, as measured with a No. 4 LTV mandrel at 60 rpm) can then be coated onto a substrate, such as a polymer film substrate. After coating the slurry onto the substrate (e.g., the polymer film substrate), further polymerization and crosslinking can be carried out in an inert environment (e.g., nitrogen, carbon dioxide, helium, and argon, excluding oxygen). A sufficiently inert atmosphere can be achieved by coating a polymer film (such as a silicone-treated PET film that is permeable to UV radiation or electron beams) with a photosensitive slurry and then irradiating the film with air.

[0044] The PSA disclosed herein, and which can be used in articles thereof, comprises a polyoxyethylene polymer. It should be understood that the polyoxyethylene polymer is a separate polymer from the acrylic copolymer in the PSA. In other words, the acrylic copolymer and the polyoxyethylene polymer are not covalently attached. In some embodiments, suitable polyoxyethylene polymers include ethoxy groups (e.g., -CH2CH2O-), propylene oxy groups (e.g., –CH(CH3)CH2O-, –CH2CH2CH2O-, –CH2CH(CH3)O-), or butenoxy groups (e.g., –CH2CH2CH2CH2O-, –CH(CH2CH3)CH2O-, –CH2CH(CH2CH3)O-, and –CH2C(CH3)2O-) or combinations thereof. The polyoxyethylene polymer may have a variety of terminal groups, including alkyl (e.g., having up to 30 carbon atoms), hydroxyl (i.e., -OH), amino (i.e., -N(R)-), and hydroxyl (i.e., -N(R)-). 4 )2) and silane (i.e., -Si(Y)) 3-x (R 5 ) x Terminal groups. Each R 4 Independently hydrogen, an alkyl group having up to 8 carbon atoms (e.g., methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, tert-butyl, n-pentyl, isopentyl, neopentyl, n-hexyl, n-heptyl, or n-octyl), a phenyl group, or a polyoxyethylene group, such as any of the above. In some embodiments, each R 4 It is hydrogen. R 5It is an alkyl group (e.g., methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, tert-butyl, n-pentyl, isopentyl, neopentyl, n-hexyl, n-heptyl, or n-octyl) or a phenyl group having up to 8 carbon atoms. In some embodiments, R 5 It is an alkyl group having at most four carbon atoms. In some embodiments, R 5 The group is methyl or ethyl. Each Y is independently a hydrolyzable group, such as a halogen (i.e., fluorine, chlorine, bromine, or iodine), an alkoxy (i.e., -O-alkyl), an acyloxy (i.e., -OC(O)alkyl), or an aryloxy (i.e., -O-aryl), and x is 0, 1, or 2. The Y group is generally capable of hydrolyzing, for example, in the presence of water under acidic conditions, to produce a group capable of undergoing a condensation reaction, such as a silanol group. In these embodiments, the alkyl group (e.g., in the alkoxy and acyloxy groups) is optionally substituted with one or more halogen atoms. In some embodiments, the alkoxy and acyloxy groups have up to 8, 6, 4, 3, or 2 carbon atoms. In some embodiments, the aryloxy group has 6 to 12 (or 6 to 10) carbon atoms, which may be unsubstituted or substituted with halogens, alkyl groups (e.g., having up to 4 carbon atoms), and haloalkyl groups. Polyoxyolefin polymers may also contain functional groups other than ethers in the main chain, such as secondary and tertiary amines, esters, amides, ureas and carbamates.

[0045] In some embodiments, the polyoxyenol polymer comprises at least one of alkoxylated alcohols, diols or polyols, alkoxylated amines, diamines or polyamines, alkoxylated esters, alkoxylated amides, or alkoxylated carbamates. Monofunctional or polyfunctional alcohols and amines can be alkoxylated using methods known in the art. Carboxylic acids and amides can be alkoxylated using methods known in the art to provide alkoxylated esters and amides. Polyoxyenols can be reacted with isocyanates using known methods to provide carbamates.

[0046] In some embodiments, the polyoxyethylene polymer is a polyether represented by the following formula: R 7 O-(EO) p -(R 6 O) q -(EO) p -R 7 or R 7 O-(R 6 O) q -(EO) p -(R 6 O) q -R 7 In these formulas, each R 7Independently hydrogen or an alkyl group having at most 4 carbon atoms (e.g., methyl, ethyl, n-propyl, isopropyl, butyl, isobutyl, or tert-butyl), wherein the alkyl group is unsubstituted or converted to hydrogen by a hydroxyl group (i.e., -OH), an amino group (i.e., -N(R)), or an amino group (i.e., -N(R)). 4 )2) or silane (i.e., -Si(Y) 3-x (R 5 ) x ) replace, where R 4 R 5 And x as described above in any of its implementation embodiments. In some embodiments, each R 7 It is hydrogen. In some implementations, each R... 7 It is a methyl group. EO represents -CH2CH2O-. Each R 6 O is independently –CH(CH3)CH2O–, –CH2CH2CH2O–, –CH2CH(CH3)O–, –CH2CH2CH2CH2O–, –CH(CH2CH3)CH2O–, –CH2CH(CH2CH3)O–, or –CH2C(CH3)2O–. In some embodiments, each R 6 O independently represents –CH(CH3)CH2O–, –CH2CH(CH3)O–, –CH2CH2CH2CH2O–. Each p is independently a value from 0 to 150 (in some embodiments, 7 to about 130, or 14 to about 130); and each q is independently a value from 0 to 150 (in some embodiments, about 20 to about 100, 1 to 55, or about 9 to about 25). The sum of p+q is at least 3 (in some embodiments, at least 5, 10, 15, 20, or at least 25). In some embodiments, the p / q ratio is from at least 0.5, 0.75, 1, or 1.5 to 2.5, 2.7, 3, 4, 5, or more. For example, based on EO and R in polyoxyethylene polymers. 6The total number of O groups and the percentage of repeating EO groups in the polyoxyethylene polymer can range from 10 to 90, 10 to 75, or 20 to 50. Available polyoxyethylene polymers include those available under the trade names “CARBOWAX” and “UCON” from Dow Chemical Company, Midland, MI, Michigan, and block copolymers of ethylene oxide and propylene oxide with molecular weights from about 500 g / mol to 15,000 g / mol (e.g., those block copolymers available under the trade name “PLURONIC” from BASF Corporation, Ludwigshafen, Germany). In some embodiments, the polyoxyethylene polymer has a number-average molecular weight in the range of 200 g / mol to 15,000 g / mol, 1,000 g / mol to 15,000 g / mol, 1,000 g / mol to 10,000 g / mol, or 1,000 g / mol to 5,000 g / mol.

[0047] In some embodiments, the polyoxyethylene polymer contains ethylene glycol repeating units and hydroxyl-terminal groups. Examples of polyols having ethylene glycol repeating units include polyethylene glycol, poly(ethylene glycol-block-propylene glycol), poly(ethylene glycol-random-propylene glycol), poly(diethylene glycol) adipate, bisphenol A ethoxylate, and combinations of these polyols. In some embodiments, the polyoxyethylene polymer is polyethylene glycol diol. In some embodiments, the number average molecular weight of the polyethylene glycol diol is at least 500 g / mol, 800 g / mol, or 1000 g / mol. In some embodiments, the molecular weight of the polyethylene glycol diol does not exceed 4000 g / mol, 3000 g / mol, 2500 g / mol, or 1000 g / mol.

[0048] In some embodiments, the polyoxyethylene polymer is a monoamine, diamine, or triamine, each having one, two, or three primary amino groups. The polyetheramine typically has a number-average molecular weight of at least 200 g / mol and may have molecular weights of up to 2500 g / mol, 2000 g / mol, 1500 g / mol, 1000 g / mol, or 500 g / mol. Available polyetheramines are, for example, commercially available under the trade name “JEFFAMINE” from Huntsman Chemical, The Woodlands, Texas, and BASF, Florham Park, New Jersey.

[0049] In some embodiments, the polyoxyethylene polymer is a fatty acid ester or an ethoxylated fatty amine. In some embodiments, the polyoxyethylene polymer is a tallow alkylamine ethoxylated. In some embodiments, the polyoxyethylene polymer is trimeroxyethylene (15)-N-tallow alkyl-1,3-diaminopropane. Some fatty amines are commercially available, for example, under the trade names “ETHOMEENT / 25” and “ETHODUOMEEN T / 25” from Nouryon, Amsterdam, The Netherlands. Fatty acid esters can be prepared, for example, by ethoxylation of fatty acids.

[0050] Commercially available polyoxyethylene polymers with silane-terminated groups are available, for example, in various grades (e.g., “MS S203”, “MS S303”, “SILYL SAT10”, and “SILYL SAT30”) under the trade names “MS” and “SILYL”, from Kaneka Corporation. In some embodiments, the main chain of the polyoxyethylene polymer may contain other functional groups, such as those derived from the formula -NR. 8 The group represented by -C(O)-W-, where W is -O-, -S-, or -NR. 8 - and where R 8 This refers to a hydrogen atom or a monovalent organic group, such as a substituted or unsubstituted monovalent carbon atom. 1-20 Hydrocarbon groups, either substituted or unsubstituted monovalent carbons 1-8 Hydrocarbon group. Contains -NR 8 Polyoxyolefin polymers with -C(O)-W- groups can be produced, for example, through the reaction of isocyanate groups with hydroxyl groups; through the reaction of isocyanate groups with amino groups; or through the reaction of isocyanate groups with thiol groups. This is used to produce polyoxyolefin polymers with the formula -NR 8 The group represented by -C(O)-W- and the group represented by the formula -Si(Y) 3-x (R 5 ) xExamples of methods for producing polyoxyethylene polymers with indicated groups include U.S. Patents 3,632,557 (Brode), 3,711,445 (Chu), 4,067,844 (Barron), 4,345,053 (Rizk), 4,374,237 (Berger), 4,645,816 (Pohl), 5,068,304 (Higuchi), and 5,364. The patents described in No. 955 (Zwiener), No. 5,756,751 (Schmalstieg), No. 5,990,257 (Johnston), No. 6,001,946 (Waldman), No. 6,046,270 (Roesler), No. 6,197,912 (Huang), and No. 7,060,750 (Jansen), as well as those described in European Patent Publication EP 0676403 published on October 11, 1995. Examples of suitable commercially available polymers with silane-terminated groups include the GENIOSIL STP-E series from Wacker Chemicals, such as GENIOSIL STP-E10 and GENIOSIL STP-E35, which are trimethoxysilylpropyl-urethane-terminated polyethers, and GENIOSIL STP-E30, which is a silane-terminated polyether with dimethoxy(methyl)silylmethylurethane-terminated groups.

[0051] In some embodiments of the PSA disclosed herein, the PSA comprises 55 wt% to 80 wt%, 55 wt% to 75 wt%, 55 wt% to 70 wt%, 60 wt% to 75 wt%, or 60 wt% to 70 wt% of an acrylic copolymer, wherein the weight percentages are based on the total weight of the PSA. In some embodiments, the PSA comprises 20 wt% to 45 wt%, 21 wt% to 45 wt%, 22 wt% to 45 wt%, 25 wt% to 45 wt%, 30 wt% to 45 wt%, 25 wt% to 40 wt%, or 30 wt% to 40 wt% of a polyoxyethylene polymer, wherein the weight percentages are based on the total weight of the PSA. The amount of polyoxyethylene polymer in these ranges is generally sufficient to make the PSA tacky.

[0052] In some embodiments, for example, when the PSA is present in a layer with a thickness ranging from 25 micrometers to 1000 micrometers, 500 micrometers, 250 micrometers, or 100 micrometers, the PSA of this disclosure has a moisture transmittance of at least 3 perm, at least 4 perm, at least 5 perm, at least 10 perm, or at least 15 perm. Despite the presence of a significant amount of (meth)acrylic acid monomer units in the PSA, the PSA is tacky at room temperature. For example, U.S. Patent No. 4,415,615 (Esmay et al.) has taught that a PSA having more than 15% by weight of (meth)acrylic acid monomer units is not tacky at room temperature. Polyoxyethylene polymers are typically present in the PSA in an amount sufficient to make it tacky.

[0053] In some embodiments, the PSA disclosed herein comprises a tackifying resin. A tackifying resin generally refers to a material that increases the viscosity of the PSA and has a number average molecular weight of up to 10,000 g / mol. Available tackifying resins may have a number average molecular weight of at least 70, as determined using a globe and ballpoint oscillator. The softening point and, as measured by differential scanning calorimetry, at least -30°C. The glass transition temperature. In some embodiments, the tackifying resin comprises at least one of the following: rosin, polyterpenes (e.g., those based on α-pinene, β-pinene, or limonene), aliphatic hydrocarbon resins (e.g., those based on cis- or trans-pentadiene, isoprene, 2-methyl-but-2-ene, cyclopentadiene, dicyclopentadiene, or combinations thereof), aromatic resins (e.g., based on styrene, α-methylstyrene, methylindene, indene, coumarone, or combinations thereof), or mixtures of aliphatic-aromatic hydrocarbon resins. Any of these tackifying resins may be hydrogenated (e.g., partially or completely). In some embodiments, the PSA comprises at least about 1% by weight and at most about 50% by weight of the tackifying resin based on the total weight of the PSA. In some embodiments, the tackifying resin is present in the range of 1% to 25% by weight, 2% to 20% by weight, 2% to 15% by weight, 1% to 10% by weight, or 3% to 10% by weight, based on the total weight of the PSA. In some embodiments, the PSA does not contain tackifier or contains less than 1% by weight, 0.5% by weight, 0.1% by weight, or 0.05% by weight, based on the total weight of the PSA.

[0054] If desired, other additives may be added to the PSA in any of the above embodiments of the present disclosure. For example, these may include homogenizers, UV absorbers, hindered amine light stabilizers (HALS), oxygen inhibitors, wetting agents, rheology modifiers, defoamers, biocides, flame retardants, dyes, and particulate fillers. Natural and petroleum waxes, oils, and bitumen can be used as additives to the PSA.

[0055] In some embodiments, the PSA of this disclosure is in the form of a foam. The foam includes voids, which may be open-cell or closed-cell. In some embodiments, the voids are present in the foam in an amount of at least 5% by volume, from 10% by volume to 55% by volume, from 10% by volume to 45% by volume, from 15% by volume to 45% by volume, or from 20% by volume to 45% by volume. The voids or pores in the foam can be generated by any known method described in the art, and include the use of a gas or foaming agent and / or the inclusion of hollow particles in the composition for use with the foam. For example, according to a method of generating foam described in U.S. Patent No. 4,415,615 (Esmay et al.), an acrylic foam can be obtained by foaming a composition containing acrylate monomers and optionally comonomers, coating the foamed foam onto a backing, and polymerizing the foamed composition. It is also possible to coat an unfoamed composition of acrylate monomers and optionally comonomers onto a backing and then simultaneously foam and polymerize the composition. Foaming of the composition can be achieved by optionally incorporating a gas into the polymerizable composition in the presence of a surfactant (e.g., a hydrocarbon or fluorinated surfactant) or surface-modified nanoparticles to stabilize the foam. Inert gases (such as nitrogen, argon, and carbon dioxide) can be useful, especially when the polymerization is photoinitiated. In some embodiments, the PSA used in the articles of manufacture of this disclosure may be non-foaming or non-foaming. In some embodiments, the PSA is free of fluorinated surfactants.

[0056] In some embodiments, the PSA disclosed herein incorporates hollow fillers, such as hollow polymer particles, hollow glass microspheres, and hollow ceramic microspheres. Hollow polymer microspheres include elastomer particles that can be obtained, for example, from Akzo Nobel, Amsterdam, The Netherlands, under the trade name “EXPANCEL.” Examples of hollow ceramic microspheres include alumina / silica microspheres (“FILLITE”, Pluress-Stauffer International) with a particle size ranging from 5 micrometers to 300 micrometers and a specific gravity of 0.7; alumina silicate microspheres (“Z-LIGHT”) with a specific gravity of about 0.45 to about 0.7; calcium carbonate-coated polyvinylidene copolymer microspheres (“DUALITE 6001AE”, Pierce & Stevens Corp.) with a specific gravity of 0.13; and those from 3M Company, Saint Paul, Minnesota. Minnesota sells glass bubbles in grades K1, K15, K20, K25, K37, K46, S15, S22, S32, S35, S38, S38HS, S38XHS, S42HS, S42XHS, S60, S60HS, iM30K, iM16K, XLD3000, XLD6000, and G-65 of "3M GLASS BUBBLES," as well as any HGS series of "3M GLASS BUBBLES." Foams containing hollow microspheres are referred to as composite foams. In some embodiments, the PSA contains no hollow microspheres or includes no more than 1% by weight, 0.5% by weight, 0.1% by weight, 0.05% by weight, or 0.01% by weight of hollow microspheres.

[0057] In some embodiments, the PSA disclosed herein is free of transition metal complexes, or contains less than 0.01 wt%, 0.010 wt%, 0.005 wt%, or 0.001 wt% of transition metal complexes based on the total weight of the PSA. Such transition metal complexes include copper complexes, such as copper(II) 2-ethylhexanoate, copper(II) acetate, copper(II) acetylacetonate, copper(II) trifluoroacetate, and combinations thereof.

[0058] The PSA that can be used in the articles of this disclosure can be prepared by simply blending an acrylic copolymer, in some embodiments a polyoxyethylene polymer, and in some embodiments optional components such as filler materials and tackifying resins. Several conventional methods, such as melt blending, solvent blending, or any suitable physical blending apparatus, can be used to blend the components.

[0059] This disclosure provides a method for preparing the PSA of this disclosure. The method includes forming a slurry composition by partially polymerizing a first polymerizable composition comprising a linear or branched alkyl (meth)acrylate and (meth)acrylic acid. The slurry composition comprises 1% to 20% by weight of an acrylic copolymer and 80% to 99% by weight of monomers based on the total weight of the slurry composition, wherein the monomers comprise linear or branched alkyl (meth)acrylates and (meth)acrylic acid. The composition is a solution of the acrylic copolymer in the monomers and may be, for example, about 3% to 15% by weight or 5% to 10% by weight of the acrylic copolymer and 85% to 97% by weight or 90% to 95% by weight of monomers. The method further includes combining the slurry composition with a polyoxyethylene polymer and optionally a crosslinking agent to provide a second polymerizable composition, and polymerizing the second polymerizable composition to form a PSA.

[0060] This disclosure provides an article of manufacture comprising a PSA disposed on a backing as described above in any of its embodiments. Figure 1 As shown, the article 10 includes a backing 20 having a first surface 24 and a second surface 22. In the illustrated embodiment, the PSA 50 of this disclosure is disposed on the first surface 24 of the backing 20.

[0061] In some embodiments, the article is water vapor permeable. By selecting the composition of the PSA and backing, the thickness of the PSA and backing, and the coverage of the pressure-sensitive adhesive (e.g., continuous or discontinuous), the article of this disclosure can advantageously have a moisture permeability of at least 3 perm, at least 4 perm, at least 5 perm, at least 10 perm, or at least 15 perm.

[0062] In embodiments where the article is water vapor permeable, the backing is also water vapor permeable. In some embodiments, the backing may be a continuous membrane. The water vapor permeability of the backing may be affected by the hydrophilicity of at least a portion of the polymer constituting the continuous membrane. A higher degree of swelling in water can be used to enhance the water vapor permeability of the continuous polymer membrane. In some embodiments, at least a portion of the polymer in the polymer membrane backing comprises polyether segments (e.g., polytetrahydrofuran, polypropylene oxide, polyethylene oxide, or combinations thereof).

[0063] In some embodiments, the polymer film backing comprises at least one of polyurethane, polyamide, polylactic acid, acrylic block copolymer, or amorphous polyester. In some embodiments, the polymer film backing is not covalently crosslinked, but in some embodiments, the second polymer film is a physically crosslinked thermoplastic elastomer.

[0064] In some embodiments, the polymer film backing (which may be a continuous polymer film backing) in the articles of manufacture disclosed herein is polyurethane. Polyurethane can be formed using any suitable reactants and any suitable method. Polyurethane is typically formed from starting materials comprising one or more isocyanates, one or more polyols, and optionally one or more additional reactants (e.g., having one or more active hydrogen groups). In some cases, a stoichiometric excess of isocyanate reacts with the polyol. For example, the ratio of isocyanate groups to hydroxyl groups can range from about 1.1:1 to 3:1 (NCO:OH), about 1.2:1 to 2.5:1, or about 1.3:1 to 2:1. Polyurethane can have any suitable molecular weight, for example, a number average molecular weight of about 1,000 g / mol to about 10,000 g / mol, or about 2,500 g / mol to about 7,500 g / mol.

[0065] Suitable isocyanates include those having one, two, three, or four isocyanate groups, as well as mixtures thereof. Suitable diisocyanates include isophorone diisocyanates (i.e., 5-isocyano-1-isocyano-methyl-1,3,3-trimethylcyclohexane); 5-isocyano-1-(2-isocyano-ethyl-1-yl)-1,3,3-trimethylcyclohexane; 5-isocyano-1-(3-isocyano-propyl-1-yl)-1,3,3-trimethylcyclohexane; 5-isocyano-(4 -Isocyanate butyl-1-yl)-1,3,3-trimethylcyclohexane; 1-Isocyanate 2-(3-isocyanate prop-1-yl)cyclohexane; 1-Isocyanate 2-(3-isocyanate ethyl-1-yl)cyclohexane; 1-Isocyanate 2-(4-isocyanate butyl-1-yl)cyclohexane; 1,2-Diisocyanate cyclohexane; 1,3-Diisocyanate cyclohexane; 1, 4-Diisocyanate cyclohexane; dicyclohexylmethane 2,4'-diisocyanate; trimethylene diisocyanate; tetramethylene diisocyanate; pentamethylene diisocyanate; hexamethylene diisocyanate; ethylethylene diisocyanate; trimethylhexane diisocyanate; heptamethyl diisocyanate; 2-heptyl-3,4-bis(9-isocyanate nonyl)-1-pentyl-cyclohexane; 1,2-, 1,4 - and 1,3-bis(isocyanate-methyl)cyclohexane; 1,2-, 1,4- and 1,3-bis(2-isocyanate-ethyl-1-yl)cyclohexane; 1,3-bis(3-isocyanate-propyl-1-yl)cyclohexane; 1,2-, 1,4- or 1,3-bis(4-isocyanate-butyl-1-yl)cyclohexane; liquid bis(4-isocyanate-cyclohexyl)-methane; and derivatives or mixtures thereof. In some embodiments, the isocyanate or mixture of isocyanates is non-aromatic (e.g., aliphatic). In some embodiments, the isocyanate includes at least one of isophorone diisocyanate (IPDI) or hexamethylene diisocyanate (HMDI). In some embodiments, HMDI is the primary isocyanate used to prepare polyurethanes; in other words, there are more HMDI units present than any other isocyanate unit.

[0066] In some embodiments, the polyurethane backing of the polymer film is formed using an aliphatic isocyanate, which provides improved stability against UV exposure compared to aromatic isocyanates. In some embodiments, the isocyanate is dicyclohexylmethane-2,4'-diisocyanate, dicyclohexylmethane-4,4'-diisocyanate, or liquid bis(4-isocyanate-cyclohexyl)-methane.

[0067] Suitable polyols for the preparation of polyurethanes include monomers, oligomers, polymers, and mixtures thereof, and include diols, triols, polyols having four or more hydroxyl groups, and mixtures thereof. Examples of polyols used as reactants or starting materials for oligomer or polymer polyols include ethylene glycol, propylene glycol, 1,3-propanediol, glycerol, diethylene glycol, dipropylene glycol, triethylene glycol, trimethylolpropane, trimethylolethane, tripropylene glycol, neopentyl glycol, pentaerythritol, 1,4-butanediol, hexanediol, 1,6-hexanediol, cyclohexanediol, polyethylene glycol or polypropylene glycol, isopropylidene bis(p-phenyleneoxypropanol-2), and mixtures thereof. Examples of suitable oligomer and / or polymer polyols include polyether polyols, polyester polyols, polyether ester polyols, polyurea polyols, polyamide polyols, polycarbonate polyols, saturated or unsaturated polyolefin polyols, and combinations thereof. In some embodiments, the soft segments in the polyurethane of the polymer film backing comprise polyethers (e.g., polytetrahydrofuran, polypropylene oxide, polyethylene oxide, or combinations thereof). The polyether segments can be incorporated into the polyurethane via a reaction of a polyoxyethylene polymer having hydroxyl-terminated groups, as described above in any of the embodiments of the polyoxyethylene polymer. In some embodiments, the number-average molecular weight of the polyether is, for example, in the range of 600 g / mol to 6000 g / mol.

[0068] In some embodiments, the polyurethane of the polymer membrane backing is formed using a polyol that provides high water vapor permeability. In some embodiments, the polyol contains repeating ethylene glycol units. Examples of polyols having repeating ethylene glycol units include polyethylene glycol, poly(ethylene glycol-block-propylene glycol), poly(ethylene glycol-random-propylene glycol), poly(diethylene glycol) adipate, bisphenol A ethoxylate, and combinations of these polyols. In some embodiments, the polyol is polyethylene glycol diol. In some embodiments, the number average molecular weight of the polyethylene glycol diol is at least 500 g / mol, 800 g / mol, or 1000 g / mol. In some embodiments, the molecular weight of the polyethylene glycol diol does not exceed 4000 g / mol, 3000 g / mol, 2500 g / mol, or 1000 g / mol.

[0069] In some embodiments, the polyurethane is a reaction product comprising polyethylene glycol, a chain extender, and an aliphatic isocyanate. The polyethylene glycol and aliphatic isocyanate can be any of the polyethylene glycols and aliphatic isocyanates described above in any of its embodiments. The chain extender is a diol with a molecular weight not exceeding 250 g / mol, and can be any of the chain extenders described above.

[0070] In some embodiments, the polyurethane of the polymer film backing is formed using at least one polyol with a functionality greater than two, and in some embodiments, a functionality of about three. Examples of polyols with a functionality of three include glycerol, polycaprolactone triol, polypropylene triol, poly(ethylene-co-propylene oxide) triol, and trimethylolpropane. In some embodiments, the hydroxyl groups from the triol account for at least or more than 1 mole percentage (mol%), 2 mole%, or 3 mole% of the total number of hydroxyl groups in the formulation used to prepare the polyurethane. In some embodiments, the hydroxyl groups from the triol account for no more than or less than 10 mole%, 6 mole%, or 4 mole% of the total number of hydroxyl groups in the formulation used to prepare the polyurethane. Including at least one polyol with a functionality greater than two in the preparation of the polyurethane can, for example, increase the melt viscosity of the polyurethane of the polymer film backing.

[0071] In some embodiments, the polyurethane is a TPU, which consists of substantially linear molecules and typically has some physical crosslinking through interactions between urethane groups in the molecule. Commercially available polyurethanes that can be used as polymeric film backings in articles of this disclosure include those produced under the trade name “ELASTOLLAN” from BASF Company, Ludwigshafen, Germany; under the trade name “ELASTOLLAN” from Covestro Company; and under the trade name “ESTANE” from Lubrizol, Wickliffe, OH.

[0072] In some embodiments, the polymer film backing comprises an acrylic block copolymer having hard and soft segments. In some embodiments, the acrylic block copolymer comprises poly(methyl methacrylate) (PMMA) hard segments, and the soft segments of the acrylic block copolymer may be formed from monomers of acrylates or methacrylates, such as those having C4-C9 alkyl side chains, or mixtures thereof. Examples of monomers that can be used to form the second block include n-butyl acrylate, n-pentyl acrylate, n-hexyl acrylate, n-heptyl acrylate, 2-ethylhexyl acrylate, isooctyl acrylate, n-octyl acrylate, n-nonyl acrylate, methacrylates of the aforementioned acrylates, and mixtures thereof. In some embodiments, monomers that can be used to form the soft segments include C-acrylate. 2-4 Hydroxyalkyl esters or C methacrylate 2-4Hydroxyalkyl esters, such as 2-hydroxyethyl acrylate, 3-hydroxypropyl acrylate, 2-hydroxyethyl methacrylate, and 3-hydroxypropyl methacrylate. In some embodiments, the acrylic block copolymer is a poly(methyl methacrylate)-poly(n-butyl acrylate)-poly(methyl methacrylate) triblock copolymer. In some embodiments, the block copolymer contains about 70% PMMA and 30% poly(n-butyl acrylate). The block copolymer may have a number average molecular weight of up to about 120,000 g / mol. Suitable commercially available materials for use in block copolymers include those from Kuraray, Chiyoda City, Japan, under the trade name "KURARITY" (e.g., LA2330 and LA3320 grades), and those from Arkema, King of Prussia, PA, under the trade name "NANOSTRENGTH".

[0073] In some embodiments, the polymer film backing comprises a polyamide. In some embodiments, the polyamide is a thermoplastic polyamide elastomer, and the soft segment is a polyether polyol segment, such as any of the above. Certain available thermoplastic polyamides are commercially available, for example, under the trade name "PEBAX" from Arkema. In some embodiments, the polymer film backing comprises an amorphous polyester. In some embodiments, the amorphous polyester has polyether polyol segments, such as any of the above. Available amorphous polyesters include those available under the trade name "ARNITEL" from BASF, Florham Park, NJ. In some embodiments, the polymer film backing comprises polylactic acid (PLA). PLA is typically prepared from renewable resources such as corn starch, cassava, or sugarcane, and is commercially available, for example, from NatureWorks, LLC, Plymouth, MN.

[0074] Continuous polymer film backings can be provided by techniques known in the art, such as hot melt extrusion of extrudable compositions comprising components of a continuous polymer film. Examples of methods for preparing extrudable continuous layers are described, for example, in Progelhof, RC and Throne, JL, “Polymer Engineering Principles,” Hanser / Gardner Publications, Inc., Cincinnati, OH, 1993.

[0075] In some embodiments, the backing for the article of this disclosure includes a fiber layer. The fiber layer may comprise a variety of suitable materials, including woven fabrics, nonwoven webs, knitted fabrics (e.g., formed by warp knitting, weft knitting, and circular knitting), nets, loose fabrics, and combinations thereof. In some embodiments, the fiber layer comprises woven, nonwoven, or knitted materials. Available fiber layers may be made from natural fibers (e.g., natural cellulosic fibers such as wood, cotton, flax, hemp, jute, and ramie), synthetic fibers (e.g., thermoplastic fibers), or combinations of natural and synthetic fibers. Examples of suitable materials for forming thermoplastic fibers include polyolefins (e.g., polyethylene, polypropylene, polybutene, ethylene copolymers, propylene copolymers, butene copolymers, and copolymers and blends of these polymers), polyesters, rayon, polyamides, and polylactic acid. The fiber may also be a multi-component fiber, for example, having a core of one thermoplastic material and an outer sheath of another thermoplastic material.

[0076] A fiber can be defined as an elongated material having a substantially uniform cross-sectional diameter or thickness and an aspect ratio greater than about 100, whereby the aspect ratio is defined as the ratio of the fiber length to the fiber's cross-sectional diameter or thickness. "Substantially uniform" means that the cross-sectional dimensions vary by no more than 10%. Typically, the diameter or thickness of a fiber is less than 250 μm.

[0077] The term "nonwoven" refers to a material having a structure of individual fibers or spindles that are sandwiched, but not in an identifiable manner such as being sandwiched in a knitted fabric. Examples of nonwoven webs include spunbond webs, hydroentangled webs, air-jet webs, wet-laid webs, meltblown webs, and bonded carded webs. In some embodiments, the fiber layer comprises multiple layers of nonwoven material, having, for example, at least one layer of meltblown nonwoven material and at least one layer of spunbond nonwoven material, or any other suitable combination of nonwoven materials. For example, the fiber layer may be a spunbond-meltblown-spunbond, spunbond-spunbond, or spunbond-spunbond-spunbond multilayer material. In some embodiments, the fiber layer is a nonwoven fabric comprising fibers selected from polyesters, polylactic acid, polyolefins, polyamides, rayon, and combinations thereof.

[0078] In some embodiments, the backing for the article of manufacture of the present disclosure comprises a polymer film layer comprising a porous random network of strands and connecting regions. In some embodiments, the strands are elongated strands. In some embodiments, the random network has a first optical density and the connecting regions have a second optical density, wherein the first optical density is greater than the second optical density. Optical density can be determined visually. If the random network of strands appears to have higher opacity than the connecting regions, a person skilled in the art can determine whether the first optical density is greater than the second optical density. At least some of the connecting regions have openings (i.e., through-holes). In some embodiments, at least some of the connecting regions do not have openings (i.e., no through-holes). In some embodiments, at least two, three, four, five, six, or seven polymer layers exhibiting the random network of strands and connecting regions are present. In some embodiments, some of the layers are adjacent to another layer exhibiting the random network of strands and connecting regions. In some embodiments, at least one of a first main surface or a second main surface of the polymer multilayer film (in some embodiments, each of the first and second main surfaces) exhibits the random network of strands and connecting regions. The polymer film layer containing a porous random network of strands and connecting regions differs from a fiber layer in that it does not contain fibers as defined above. Therefore, a layer containing a porous random network of strands and connecting regions is not a nonwoven, woven, or knitted fabric layer.

[0079] In some embodiments, the backing of the polymer layer comprising a porous random network of strands and connecting regions comprises at least one of the following: a polyolefin material (e.g., polypropylene and / or polyethylene), a modified polyolefin material, polyvinyl chloride, polycarbonate, polystyrene, polyester (including copolyester), polylactide, polyvinylidene fluoride, (meth)acrylates (e.g., polymethyl methacrylate), thermoplastic polyurethane (TPU), urethane acrylate, ethylene vinyl acetate copolymer, acrylate-modified ethylene vinyl acetate polymer, ethylene acrylic copolymer, nylon, engineered polymers (e.g., polyketone and / or polymethylpentane), or elastomers (e.g., natural rubber; synthetic rubber; styrene block copolymers containing isoprene, butadiene, or ethylene (butene) blocks; metallocene-catalyzed polyolefins, polyurethanes; or polydiorganosiloxanes). TPU is a thermoplastic block copolymer composed of alternating soft and hard segments, wherein the hard segments are isocyanate segments (e.g., including aliphatic isocyanate segments, aromatic isocyanate segments, or combinations thereof), and the soft segments are polyether polyol segments or polyester polyol segments, as described in detail above. The soft segments and the amorphous hard segments form an amorphous phase, and a portion of the hard segments crystallizes to form crystalline microdomains that can serve as physical crosslinking domains. Available TPUs for polymer layers comprising a porous random network of strands and connecting regions may have a high percentage of hard segments. In some embodiments, each polymer layer comprising the porous random network of strands and connecting regions comprises a vapor-impermeable resin. In some embodiments, each polymer layer comprising the porous random network of strands and connecting regions comprises a polyolefin. In some embodiments, each polymer layer comprising the porous random network of strands and connecting regions comprises at least one of polyethylene or polypropylene. In some embodiments, the polymer layer comprising a porous random network of strands and connecting regions comprises low-density polyethylene, high-density polyethylene, ethylene-containing copolymers, or combinations thereof. In some embodiments, the polymer layer comprising a porous random network of strands and connecting regions comprises a thermoplastic polyolefin resin that may be available under the trade name “ADFLEX KS 021 P” from LyondellBasell, Houston, TX.

[0080] In some embodiments, the polymer layer comprising a porous random network of strands and connecting regions contains an ethylene copolymer. The copolymer may include a polar comonomer. Examples of ethylene copolymers containing polar comonomers include ethylene-vinyl acetate copolymers, ethylene-acrylic acid copolymers, and ethylene-methacrylic acid copolymers. In some embodiments, the ethylene copolymer of the polymer layer comprising a porous random network of strands and connecting regions contains at least 70 wt%, at least 75 wt%, or at least 80 wt% ethylene. In some embodiments, the ethylene copolymer of the polymer layer contains at most 99 wt%, at most 95 wt%, at most 90 wt%, or at most 85 wt% ethylene. In some embodiments, the ethylene copolymer contains at least 1 wt%, at least 5 wt%, at least 10 wt%, or at least 15 wt% of one or more polar comonomers. In some embodiments, the ethylene copolymer contains at most 30 wt%, at most 25 wt%, or at most 20 wt% of one or more polar comonomers. Ethylene-vinyl acetate copolymers are available under the trade name "ELVAX" (e.g., grades 750, 550, and 350) from various suppliers, including DuPont Packaging and Industrial Polymers. Ethylene-acrylic acid copolymers are available under the trade name "PRIMACOR" (e.g., grades 1410 or 3460) from various suppliers, such as Dow Chemical Company. Ethylene-methacrylic acid copolymers are available under the trade name "NUCREL" (e.g., grades 0403 and 0903) from various suppliers, including DuPont Packaging and Industrial Polymers. Available ethylene-containing copolymers may also contain two or more polar comonomers. Examples of such ethylene-containing copolymers include carbon monoxide-modified ethylene-vinyl acetate or anhydride-modified ethylene-vinyl acetate. Such ethylene-containing copolymers are available under the trade names "BYNEL E418" and "ELVALOY 741" from various suppliers, including DuPont Packaging and Industrial Polymers. A mixture of at least two different ethylene-containing copolymers (e.g., each with different polar comonomers or each with the same polar comonomers but in different amounts) can also be useful.

[0081] Polymer layers containing a porous, random network of strands and connecting regions can be foamed or over-foamed, for example, by introducing gas into the molten polymer within an extruder. Under the heat and pressure of the extrusion process, gas is readily absorbed into the polymer. As the molten polymer exits the extrusion die, the absorbed pressurized gas rapidly expands and forms voids. Appropriate process conditions can be adjusted so that the void structure is "locked in" when the polymer solidifies, thereby creating a foam structure within the polymer film.

[0082] Foaming of the polymer layer can be promoted, for example, by including or injecting a foaming agent into the resin of the layer. Blowing agents are known in the art and include injected gases (e.g., nitrogen or carbon dioxide); blends of alkaline earth metal carbonates and alkali metal salts, as described in U.S. Patent No. 8,563,621 (Lapierre), the disclosure of which is incorporated herein by reference; hydrazine; acyl hydrazine; and azodicarbonamide materials (e.g., 4,4'-oxobis(benzenesulfonylhydrazine) (OBSH)) (e.g., available as a masterbatch under the trade name "CELOGEN OT" from ChemPoint, Bellevue, WA). Further examples of commercially available blowing agents include those available under the trade name "ECOCELL H" from Polyfil Corp., Rockaway, NJ, an endothermic blowing agent available as a masterbatch under the trade name "FCX111263" from RTP Company, Winona, Minnesota. MN), and purchased under the trade name "HYDROCEROL CF 40 E" from Avient, Avon Lake, OH.

[0083] In some embodiments, a foaming agent is added to a resin that is fed into an extruder. The foaming agent and other processing conditions are selected or adjusted to provide a desired or acceptable polymer layer exhibiting a random network of strands and connecting regions.

[0084] See now Figure 2 Article 10 includes a backing 20, the backing having, for example... Figure 1 The first surface 24 and the second surface 22 are described. In an illustrated embodiment, the PSA 50 of this disclosure is disposed on the first surface 24 of the backing 20. The article 10 includes a release liner 25 disposed on the PSA 50 opposite to the backing 20. For example, the release liner can be useful when the article is wound into a roll. In some embodiments, the release liner 25 is coated on at least one main surface of a main surface having a release coating. In some embodiments, both main surfaces of the release liner 25 are coated with a release coating. In this case, the release coating on each of the main surfaces of the release liner 50 can be the same or different. Examples of materials that can be used as the release coating for the liner disclosed herein include acrylic resins, silicones, siloxanes, fluoropolymers, and urethanes. In some embodiments, a silicone coating can be used to facilitate the release of the PSA.

[0085] Various release liner options are available. In some embodiments, the release liner comprises at least one of polyester film, polyethylene film, polypropylene film, polymer film coated with polyolefin, paper coated with polyolefin, polymer film coated with acrylic resin, and kraft paper coated with polymer. The polyolefin-coated film or paper may be a polyethylene-coated film or paper. Examples of suitable commercially available pads include those available under the trade names “2.0 CL PET U4162 / U4162”, “48#CL PET H / H UE1095 / 000”, and “4 BU DHP UE1094B / 000” from Loparex, Hammond, Wisconsin, USA; red-colored multilayer thermoplastic olefin films with a thickness of approximately 63 micrometers (0.0025 inches) containing a proprietary blend of high-density polyethylene and low-density polyethylene, available from Iso Poly Films, Incorporated, Gray Court, South Carolina, USA; and transparent polyester release pads available under the name “2PAKN” from Mitsubishi Polyester Films, Greer, South Carolina.

[0086] Release liner can be prepared using a variety of processing techniques. For example, liner processing techniques such as those disclosed in U.S. Patent Application 2013 / 0059105 (Wright et al.) can be used to prepare liner suitable for implementing this disclosure. A suitable liner processing technique may include the steps of: applying a layer comprising a (meth)acrylate-functionalized siloxane to the main surface of a substrate; and irradiating the layer with a short-wavelength multicolor ultraviolet light source having at least one peak intensity at a wavelength of about 160 nm to about 240 nm in a substantially inert atmosphere containing no more than 500 ppm oxygen. Irradiation may at least partially cure the layer. In some embodiments, the layer is cured at a curing temperature greater than 25°C. The layer can be at a temperature of at least 50°C, 60°C, 70°C, 80°C, 90°C, 100°C, 125°C or at least 150°C, and in some embodiments, not exceeding 250°C, 225°C, 200°C, 190°C, 180°C, 170°C, 160°C or 155°C.

[0087] See again at another location. Figure 1 The second surface 22 of the backing 20 may include a low surface energy release layer or low adhesion adhesive (LAB) that can be used to cover or coat an unpadded article.

[0088] Figure 3Another embodiment of the article 100 according to this disclosure is illustrated, wherein the backing comprises multiple layers. Some of the aforementioned porous layers are not considered barrier materials in themselves because they do not provide a barrier against air or liquid water. The article 100 includes a water vapor-permeable polymeric material 130 disposed on a first main surface 122 of the porous layer 120. The polymeric material 130 and the porous layer 120 together form the backing of the article 100, which provides air and water barriers. The polymeric material 130 may be present in at least one of the following ways: completely covering or impregnating the porous layer 120. A PSA 150 of this disclosure is disposed on a second main surface 124 of the porous layer 120 opposite the first main surface 122. In the illustrated embodiment, surface 152 of the PSA 150 is attached to a release liner 125, which may be any of the release liners described above in any of its embodiments.

[0089] In some embodiments, the peel adhesion between one primary surface of the liner 125 and the adhesive surface 152 is less than or equal to the peel adhesion between another primary surface of the liner 125 and the surface 132 of the polymer material 130. In some embodiments, the liner may be surface-treated (e.g., on at least one primary surface) to increase the adhesion or bonding force between the liner and the polymer material 130. Examples of materials or surface treatments that can be used to increase the adhesion or bonding force between the polymer coating and the liner surface include any chemical or physical surface modification of the polymer material 130, the liner surface, or either of them. For example, chemical surface modifiers or chemical coatings may be used. In some embodiments, adhesion modification may be accomplished by selecting a specific liner surface morphology to increase the surface area and physical interlocking of the polymer coating. In these embodiments, the release liner 125 may adhere to the surface 132 when the article is unwound from the roller, for example, by providing a reverse winding roller with a PSA 150 on the outside of the roller.

[0090] A multi-layered backing can be prepared, for example, by extruding a continuous polymer film as described in any of the embodiments above onto a porous layer as described in any of the embodiments above, such as a polymer layer comprising a porous random network of strands and connecting regions. Alternatively, the continuous polymer film can be extruded as a separate sheet and laminated with another layer, such as a polymer layer comprising a porous random network of strands and connecting regions or a fibrous layer as described in any of the embodiments above.

[0091] In some embodiments, the water vapor permeable polymer material 130 is a crosslinked polymer layer. In some embodiments, the polymer layer comprises a polyoxyethylene polymer having at least one crosslinking site derived from a silane having a hydrolyzable group. Crosslinking can occur when the hydrolyzable group of the silane hydrolyzes to a silanol group, which then condenses to form a siloxane bond. The polyoxyethylene having silicon atoms with hydrolyzable groups can be any of those described above in conjunction with PSA in any of its embodiments. Crosslinkable compositions comprising polyoxyethylene having silicon atoms with hydrolyzable groups typically contain one or more catalysts. The catalyst may be present in the polymer material in an amount from about 0.05 wt% to about 5 wt%, in some embodiments from about 0.1 wt% to about 2 wt%, and in some embodiments from about 0.1 wt% to about 1 wt%. Available catalysts include organometallic compounds and amines known as silanol condensation catalysts. Examples of suitable silanol condensation catalysts include titanates such as tetrabutyl titanate and tetrapropyl titanate; organotin compounds such as dibutyltin dilaurate, dibutyltin maleate, dibutyltin diacetate, stannous octoate, stannous naphthenate, reaction products from dibutyltin oxide and phthalates, and dibutyltin diacetylacetonate; organoaluminum compounds such as aluminum triacetylacetonate, aluminum tri(ethylacetoacetate), and diisopropylaluminum ethylacetoacetate; reaction products from bismuth salts and organic carboxylic acids such as bismuth tris(2-ethylhexanoate) and bismuth tris(neodecanoate); chelates Compounds such as zirconium tetraacetylacetonate and titanium tetraacetylacetonate; organolead compounds such as lead octanoate; organovanadium compounds; amines such as butylamine, octylamine, dibutylamine, monoethanolamine, oleylamine, cyclohexylamine, benzylamine, diethylaminopropylamine, xylenediamine, triethylenediamine, guanidine, diphenylguanidine, 2,4,6-tris(dimethylaminomethyl)phenol, morpholine, N-methylmorpholine, 2-ethyl-4-methylimidazolium and carboxylic acids and other acids; low molecular weight polyamide resins derived from excess polyamines and polybasic acids; and reaction products derived from excess polyamines and epoxy compounds. Any of these compounds may be used alone or in combination.

[0092] Compositions comprising polyoxyethylene having silicon atoms with hydrolyzable groups may optionally include a variety of additives, such as dehydrating agents, fillers, rheology modifiers, compatibilizers, tackifiers, storage stability improvers, adhesion promoters, ultraviolet absorbers, metal passivators, anti-ozone agents, antioxidants, light stabilizers, lubricants, amine radical chain inhibitors, phosphorus peroxide decomposers, pigments, foaming agents, solvents, flame retardants, antifungal agents, foaming agents, and antistatic agents, each included in any suitable amount and in any combination. Specific examples of these additives are disclosed in U.S. Patent Nos. 10,704,254 (Seabaugh et al.), 11,105,089 (Widenbrant et al.), 11,365,328 (Seabaugh et al.), 11,512,463 (Widenbrant et al.), and 11,731,394 (Seabaugh et al.), as well as U.S. Patent Application Publications Nos. 2017 / 0173916 (Widenbrant et al.), 2021 / 0207005 (Seabaugh et al.), and 2022 / 0282476 (Widenbrant et al.).

[0093] Any suitable method may be used to apply a crosslinkable polymer composition to a porous layer. Examples of such methods include doctor blade coating, slot coating, die coating, overflow coating, bar coating, curtain coating, cast coating, spray coating, brush coating, dip coating, kiss coating, gravure coating, and printing coating operations (such as flexographic, inkjet, or screen printing coating). The composition may then be heated at elevated temperatures (e.g., at least 50°C, 60°C, 70°C, 80°C, or 90°C, and in some embodiments, not exceeding 250°C, 225°C, 200°C, 190°C, 180°C, 170°C, 160°C, or 150°C) to crosslink the composition, thereby forming a polymer layer on the porous layer comprising a polyoxyethylene polymer having at least one crosslinking site derived from a silane having a hydrolyzable group.

[0094] In some embodiments of the backing material that can be used in the articles of this disclosure, comprising multiple layers, a polymer layer comprising a porous random network of strands and connecting regions is co-extruded with a continuous polymer film layer as described above in any of its embodiments. For the purposes of this disclosure, co-extrusion means the simultaneous melting and processing of multiple melt flows, and the combination of such melt flows, for example, from a single extrusion die into a single integral structure or co-extruded film. In some embodiments of the articles of this disclosure, the backing material can be co-extruded using any suitable type of co-extrusion die and any suitable film-forming method, such as blown film extrusion or cast film extrusion. In some embodiments, the multilayer melt flow can be formed by a multilayer feed head, such as the multilayer feed head shown in U.S. Patent No. 4,839,131 (Cloeren) or other specialized feed heads or dies, such as those manufactured by Cloeren Co., Orange, TX. The feed heads and dies used are typically heated to promote polymer flow and layer adhesion, wherein the temperature of the die depends on the polymer used. Co-extrusion technology can be found in many polymer processing references, including Progelhof, RC and Throne, JL, "Polymer Engineering Principles", Hanser / Gardner Publications, Inc., Cincinnati, Ohio, 1993.

[0095] In some embodiments of the backing for articles of this disclosure, a polymer layer comprising a porous random network of strands and connecting regions is co-extruded with a continuous polymer film layer as described above in any of the embodiments thereof by foaming the layers in a blown film process. This blown film process uses an annular die to form radially oriented molten film tubes by air pressure in the “bubble” and also longitudinally pulls the molten area to thin the film to the final desired thickness. Suitable annular dies and apparatus are illustrated and described, for example, in U.S. Patent Nos. 10,953,573 (Emslander et al.), 10,953,574 (Young et al.), 10,953,623 (Young et al.), and 10,987,894 (Emslander et al.). The number of layers in the co-extruded film can be adjusted by the number of stacked templates in the annular die. For example, a polymer layer comprising a porous random network of strands and connecting regions can be co-extruded with a continuous polymer film layer in a blown film apparatus by omitting or injecting a foaming agent into the resin of a continuous layer in an annular stacking die. To facilitate co-extrusion, in some embodiments, the melt viscosity of the polymer in the continuous polymer film layer is similar to the melt viscosity of the polymer in the porous random network comprising strands and connecting regions.

[0096] In some embodiments, the backing material that can be used in the articles of this disclosure is a polymer multilayer film comprising a polymer layer with a porous random network of strands and connecting regions, and a continuous polymer film layer as described above in any of the embodiments thereof. In some embodiments of the backing material that can be used in the articles of this disclosure, there are at least two, three, four, five, six, or seven polymer film layers with a porous random network of strands and connecting regions, and at least two, three, four, five, six, or seven continuous polymer film layers as described above in any of the embodiments thereof. In some embodiments having more than one polymer film layer with a porous random network of strands and connecting regions, at least two such layers exhibit different random networks of strands and connecting regions. In some embodiments having more than one continuous polymer film layer, at least two such layers have different polymer compositions. In some embodiments, the polymer film layer with a porous random network of strands and connecting regions alternates at least partially with the continuous polymer film layer. In some embodiments, only one polymer film layer with a porous random network of strands and connecting regions is in direct contact with the continuous polymer film layer. In some embodiments, at least one polymer film layer comprising a porous random network of strands and connecting regions is disposed between two consecutive polymer film layers. In some embodiments, a consecutive polymer film layer is disposed between two polymer film layers comprising a porous random network of strands and connecting regions. In some embodiments, a first main surface of the backing comprises a polymer film layer comprising a porous random network of strands and connecting regions. In some embodiments, a second main surface of the backing comprises a consecutive polymer film layer. Further information regarding multilayer films comprising a porous random network of strands and connecting regions and consecutive polymer film layers that can be used in articles of manufacture of this disclosure is available in co-pending U.S. Patent Application Serial No. 63 / 635,837, filed on the same day as this application, the entire contents of which are incorporated herein by reference.

[0097] In some embodiments, at least one layer of the polymer multilayer film described above comprises a release agent. Examples of suitable release agents include at least one of alkyl polydimethylsiloxane, polyethylene octadecyl carbamate, or ethylene bis-stearamide. Alkyl polydimethylsiloxane is described, for example, in U.S. Patent 9,187,678 (Boardman et al.). Polyethylene octadecyl carbamate is commercially available, for example, under the trade name “ESCOAT P-77” (polyethylene octadecyl carbamate in linear low-density carrier resin) from Mayzo, Inc., Suwanee, GA. Ethylene bis-stearamide is commercially available, for example, under the trade name “AMPACET 100666” from Ampacet Corporation, Tarrytown, NY. The layer containing the release agent may exhibit a random network of strands and connecting regions, or it may be a continuous film.

[0098] In some embodiments, at least one layer of the polymer multilayer film described above comprises at least one dye or pigment (e.g., imparting a color such as white, yellow, green, blue, red, orange, brown, black, etc.). Examples of suitable dyes include those commercially available, for example, under the trade name "CLARIANT REMAFIN PE63421213-ZN" (green dye masterbatch) from Clariant International AG, Muttenz, Switzerland. Examples of suitable pigments include titanium dioxide, zinc oxide, and zirconium dioxide. In some embodiments, the polymer multilayer film described above includes a layer separable from the first polymer layer and the second polymer layer.

[0099] In some embodiments of the polymer multilayer film that can be used as a backing in articles of this disclosure, a bonding layer exists between a polymer film layer comprising a porous random network of strands and connecting regions and a continuous polymer film layer. In some embodiments, the bonding layer comprises an ethylene-containing copolymer, for example, comprising a polar comonomer, as described above in any of its embodiments. Examples of ethylene-containing copolymers comprising polar comonomers include ethylene-vinyl acetate copolymers, ethylene-acrylic acid copolymers, and ethylene-methacrylic acid copolymers. In some embodiments, the ethylene-containing copolymer of the bonding layer comprises at least 70% by weight, at least 75% by weight, or at least 80% by weight of ethylene. In some embodiments, the ethylene-containing copolymer of the first polymer layer comprises at most 99% by weight, at most 95% by weight, at most 90% by weight, or at most 85% by weight of ethylene. The bonding layer may comprise a porous random network of strands and connecting regions as described above in any of its embodiments. In some embodiments, the bonding layer is a continuous layer.

[0100] In some embodiments, the polymer multilayer membrane that can be used as a backing in the articles of manufacture disclosed herein is water vapor permeable. In some embodiments, the polymer multilayer membrane has a moisture permeability of at least 5 μm, at least 10 μm, at least 15 μm, or at least 20 μm. In some embodiments, the polymer multilayer membrane described herein has a thickness in the range of 1 micrometer to 1000 micrometers (in some embodiments, in the range of 25 micrometers to 500 micrometers, 50 micrometers to 250 micrometers, or even 2 micrometers to 10 micrometers). The number, thickness, and material (e.g., in the first and second polymer membrane layers) of open pores affect the permeability. Those skilled in the art can select the material (e.g., in the first and second polymer membrane layers) and porosity (e.g., in the first polymer membrane layer) according to the desired permeability.

[0101] In some embodiments, to maintain the desired level of water vapor permeability in the article, the pressure-sensitive adhesive layer is discontinuous, leaving portions of the main surface of the backing exposed. For discontinuous layers, typically about 10% to 90%, more typically about 30% to 80%, and most commonly 40% to 70% of the area of ​​the main surface of the backing is covered by the adhesive. In other words, at least 10% to 90%, and in some embodiments 20% to 70% or 30% to 60% of the area of ​​the main surface of the backing may be adhesive-free.

[0102] Discontinuous layers of pressure-sensitive adhesives can be applied in a random manner or in a specific pattern. Some examples of discontinuous coatings of adhesives are described, for example, in U.S. Patent Nos. 3,039,893 (Banigan, Jr.), 3,426,754 (Bierenbaum), 5,374,477 (Lawless), 5,593,771 (Lawless), 5,895,301 (Porter), 6,495,229 (Carte), 6,901,712 (Lionel), and 10,704,254 (Seabaugh et al.), and U.S. Patent Application Publication No. US 2017 / 0072430 (Maier et al.).

[0103] To prevent lateral movement of air between the article of this disclosure and the substrate to which it is bonded, and through the overlap of the article, the adhesive-coated areas of the article can be made intersecting to isolate the uncoated areas, thereby eliminating channels through which air can move laterally. This can be achieved through any number of patterns, such as intersecting circles with the center of the uncoated area, with squares or rectangles of the adhesive, and with stripes of a checkered pattern. In some embodiments of the article of this disclosure, the PSA is present in a continuous layer.

[0104] The PSA used in the articles of manufacture disclosed herein can have a variety of thicknesses, depending on the desired application. In some embodiments, the PSA has a thickness in the range of 50 micrometers to 6000 micrometers, 100 micrometers to 4000 micrometers, 100 micrometers to 2000 micrometers, or 100 micrometers to 1500 micrometers. In some embodiments, the PSA has a thickness of at least 100 micrometers.

[0105] In some embodiments, the article of this disclosure and / or prepared by the methods disclosed herein is applied to a substrate. The substrate can be made of a variety of materials such as wood, vinyl resin, metal, or concrete. In some embodiments, the article of this disclosure can be adhered to two different substrates simultaneously (e.g., side-by-side substrates). Useful substrates may include at least one of air and water barrier membranes, subfloors, window frames, door frames, and wall cladding materials (e.g., oriented strand board (OSB), foam insulation cladding, exterior-grade gypsum board, concrete, concrete blocks (CMU)). In some cases, the substrate may be compacted soil or gravel. The substrate may be horizontal or vertical. In some embodiments, the article of this disclosure and / or prepared by the methods disclosed herein is at least a portion of an interior wall, exterior wall, floor, ceiling, or roof.

[0106] The method disclosed herein includes applying the article disclosed herein to a substrate using a pressure-sensitive adhesive layer. The substrate can be any of the substrates described above. The article disclosed herein can be in the form of a strip, for example, it can be used as a seam tape or a waterproof tape.

[0107] This disclosure also provides a method for installing a window or door. Figure 4 This is an exploded perspective view of an embodiment of the article of the present disclosure, which is applied to a window frame in the form of strip material. Figure 4 A window 434 is shown in a wall cladding 432 optionally covered with building cladding 436. Suitable materials for wall cladding include plywood, oriented strand board (OSB), foam insulation cladding, exterior-grade gypsum board, concrete, concrete blocks (CMU), and other conventional cladding materials commonly used in the construction industry. Figure 4 As shown, strip 405, as an article of manufacture as described in any of the above embodiments, is applied to the building cladding 436 or wall panel 432 flush with the bottom edge of the rough-opening window frame 434 to form a window sill waterproofing plate. A window sill plate may be installed in the opening, and the first layer 405 may overlap the window sill plate. A window 446 is inserted into the opening 434. Typically, a window frame is fitted within the opening, and a flange extends from the window frame and onto the wall panel. The window flange is secured to the wall. Strips 415 and 425 of this disclosure may also be applied to the window frame extending from the window flange onto the building cladding 436 or wall panel 432. Strip 435 of this disclosure may also be applied to the top flange of the window and cladding. Cutting the flaps of the building cladding 436 to expose the wall panel 432 may allow for a gap at the top of the window for strip 435.

[0108] In some embodiments, the articles of this disclosure and / or prepared according to the methods of this disclosure are air and water barrier membranes. Air and water barrier membranes can be, for example, building cladding as described above or membranes used under concrete floors or on interior walls. Air and water barrier membranes can be used, for example, to prevent external liquid water from penetrating through sheets, but allow water to escape in the form of vapor. In some embodiments where the articles of this disclosure are strips, the strips of this disclosure can be used, for example, as seam strips or waterproof strips, for example, in combination with air and water barrier membranes. Air and water barrier membranes can be articles of this disclosure as described above in any of its embodiments. Another example of a suitable air and water barrier membrane is available under the trade name “TYVEK” from DuPont, Wilmington, Delaware USA, obtained by hot-pressing three-dimensional mesh fibers of high-density polyethylene.

[0109] The articles disclosed herein can have a variety of widths. Available widths of waterproof or sealing tapes can range from 2 inches (5.1 cm) to 18 inches (45.7 cm). In some embodiments, the tape width is at least 1 inch (2.5 cm). In some embodiments, the tape width is at least 5 cm. In some embodiments, the article (in some embodiments, the tape) has a width of up to 75 cm (29.5 inches), 45 cm (17.7 inches), 30.5 cm (12 inches), or 10 cm (3.9 inches). In some embodiments, the article width is up to 75 cm (29.5 inches), up to 150 cm (59.1 inches), or up to 160 cm (63.0 inches).

[0110] In a first embodiment, this disclosure provides a pressure-sensitive adhesive comprising an acrylic copolymer and a polyoxyethylene polymer without fluorinated carbon atoms, the acrylic copolymer comprising: at least 60 wt% of linear or branched alkyl (meth)acrylate monomer units based on the weight of the acrylic copolymer; and 12.5 wt% to 40 wt% of (meth)acrylate monomer units based on the weight of the acrylic copolymer. In a second embodiment, this disclosure provides a pressure-sensitive adhesive according to the first embodiment, wherein the polyoxyethylene polymer is present in an amount of 20 wt% to 45 wt% based on the total weight of the pressure-sensitive adhesive. In a third embodiment, this disclosure provides a pressure-sensitive adhesive according to the first or second embodiment, wherein the acrylic copolymer is crosslinked. In a fourth embodiment, this disclosure provides a pressure-sensitive adhesive according to any one of the first to third embodiments, wherein the acrylic copolymer is crosslinked with triazine. In a fifth embodiment, this disclosure provides a pressure-sensitive adhesive according to any one of the first to fourth embodiments, wherein the pressure-sensitive adhesive is free of fluorinated surfactants and / or free of transition metal complexes or contains less than 0.01 wt%, 0.010 wt%, 0.005 wt%, or 0.001 wt% of transition metal complexes based on the total weight of the pressure-sensitive adhesive. In a sixth embodiment, this disclosure provides a pressure-sensitive adhesive according to any one of the first to fifth embodiments, wherein the pressure-sensitive adhesive is non-foaming. In a seventh embodiment, this disclosure provides a pressure-sensitive adhesive according to any one of the first to sixth embodiments, wherein the polyoxyethylene polymer comprises at least one of alkoxylated alcohols, diols, or polyols, alkoxylated amines, diamines, or polyamines, alkoxylated esters, alkoxylated amides, or alkoxylated carbamates. In an eighth embodiment, this disclosure provides a pressure-sensitive adhesive according to any one of the first to seventh embodiments, wherein the polyoxyethylene polymer is divalent or polyvalent and comprises at least one of a plurality of ethoxy groups, propoxy groups, or butoxy groups and terminal groups comprising at least one of alkyl, hydroxyl, amino, or silyl groups. In the ninth embodiment, this disclosure provides a pressure-sensitive adhesive according to any one of the first to eighth embodiments, wherein the polyoxyethylene polymer is represented by the following formula R 7 O-(EO) p -(R 6 O) q -(EO) p -R 7 or R 7 O-(R 6 O) q -(EO) p -(R 6O) q -R 7 , where each R 7 Independently hydrogen or an alkyl group having at most 4 carbon atoms (e.g., methyl, ethyl, n-propyl, isopropyl, butyl, isobutyl, or tert-butyl), wherein the alkyl group is unsubstituted or converted by a hydroxyl group, -N(R) 4 )2 or -Si(Y) 3-x (R 5 ) x Replacement; each R 4 Independently hydrogen, an alkyl group having up to 8 carbon atoms, a phenyl group, or a polyoxyethylene group; each R 5 Each Y is independently an alkyl or phenyl group having up to 8 carbon atoms; each Y is independently a hydrolyzable group; x is 0, 1, or 2; EO represents -CH2CH2O-; each R 6 The group consisting of –CH(CH3)CH2O–, –CH2CH2CH2O–, –CH2CH(CH3)O–, –CH2CH2CH2CH2O–, –CH(CH2CH3)CH2O–, –CH2CH(CH2CH3)O–, and –CH2C(CH3)2O– is independently selected; each p is independently from 1 to 150; and each q is independently from 0 to 150, wherein p+q is at least 3. In a tenth embodiment, this disclosure provides a pressure-sensitive adhesive according to any one of the first to ninth embodiments, wherein the linear or branched (meth)acrylate alkyl monomer unit comprises a unit of at least one of n-butyl acrylate, n-octyl acrylate, 2-octyl acrylate, isooctyl acrylate, 2-ethylhexyl acrylate, 2-propylheptyl acrylate, or isononyl acrylate; and the (meth)acrylate monomer unit is an acrylic monomer unit.

[0111] In an eleventh embodiment, this disclosure provides a method for preparing a pressure-sensitive adhesive according to any one of the first to tenth embodiments, the method comprising partially polymerizing a first polymerizable composition comprising linear or branched alkyl (meth)acrylates and (meth)acrylic acid to form a slurry composition; combining the slurry composition with the polyoxyethylene polymer and optionally a crosslinking agent to provide a second polymerizable composition; and polymerizing the second polymerizable composition to form a pressure-sensitive adhesive. In a twelfth embodiment, this disclosure provides a method according to the eleventh embodiment, wherein the slurry composition comprises 1% to 20% by weight of an acrylic copolymer and 80% to 99% by weight of monomers based on the total weight of the slurry composition, wherein the monomers comprise linear or branched alkyl (meth)acrylates and (meth)acrylic acid.

[0112] In a thirteenth embodiment, this disclosure provides an article comprising a pressure-sensitive adhesive disposed on a backing according to any one of the first to tenth embodiments, or a pressure-sensitive adhesive prepared by the method described in the eleventh or twelfth embodiment. In a fourteenth embodiment, this disclosure provides an article according to a thirteenth embodiment, wherein the pressure-sensitive adhesive is present in a discontinuous pattern. In a fifteenth embodiment, this disclosure provides an article according to a thirteenth embodiment, wherein the pressure-sensitive adhesive is present in a continuous layer. In a sixteenth embodiment, this disclosure provides an article according to any one of the thirteenth to fifteenth embodiments, wherein the article is water vapor permeable. In a seventeenth embodiment, this disclosure provides an article according to any one of the thirteenth to sixteenth embodiments, wherein the article has a water vapor permeability of at least 5 US Perm. In an eighteenth embodiment, this disclosure provides an article according to any one of the thirteenth to sixteenth embodiments, wherein a release liner is disposed on the pressure-sensitive adhesive opposite to the backing.

[0113] In a nineteenth embodiment, this disclosure provides an article according to any one of embodiments thirteen through eighteen, wherein the backing comprises at least one of polyurethane, polyamide, polylactic acid, acrylic block copolymer, or amorphous polyester. In a twentyth embodiment, this disclosure provides an article according to any one of embodiments thirteen through nineteen, wherein the backing comprises a porous layer having a first main surface and a second main surface, and a polymer layer disposed on at least the first main surface of the porous layer. In a twenty-first embodiment, this disclosure provides an article according to an embodiment twenty, wherein the polymer layer comprises a crosslinked polyoxyethylene polymer having at least one crosslinking site comprising at least one siloxane bond. In a twenty-second embodiment, this disclosure provides an article according to an embodiment twenty or twenty-first, wherein the porous layer is fibrous. In a twenty-third embodiment, this disclosure provides an article according to any one of embodiments twenty through twenty-two, wherein the porous layer comprises a nonwoven fabric.

[0114] In a twenty-fourth embodiment, this disclosure provides an article according to any one of embodiments twenty to twenty-three, wherein the backing comprises a porous random network of strands and connecting regions. In a twenty-fifth embodiment, this disclosure provides an article according to an embodiment twenty-four, wherein the random network of strands has a first optical density and the connecting regions have a second optical density, wherein the first optical density is greater than the second optical density. In a twenty-sixth embodiment, this disclosure provides an article according to an embodiment twenty-four or twenty-five, wherein a portion of the connecting regions includes through-holes, and a portion of the connecting regions does not include through-holes. In a twenty-seventh embodiment, this disclosure provides an article according to any one of embodiments twenty-four to twenty-six, wherein the porous random network of strands and connecting regions comprises a polyolefin. In a twenty-eighth embodiment, this disclosure provides an article according to any one of embodiments twenty-four to twenty-seven, wherein the backing comprises a polymer multilayer film, the polymer multilayer film comprising a first polymer layer and a second polymer layer, wherein the first polymer layer comprises a porous random network of strands and connecting regions, and wherein the second polymer layer is a continuous polymer film layer. In a twenty-ninth embodiment, this disclosure provides an article of the twenty-eighth embodiment, wherein the second polymer layer comprises at least one of polyurethane, polyamide, polylactic acid, acrylic block copolymer, or amorphous polyester. In a thirtieth embodiment, this disclosure provides an article of the nineteenth or twenty-ninth embodiment, wherein the polyurethane is a reaction product comprising a component comprising polyethylene glycol, a chain extender, and an aliphatic isocyanate. In a thirty-first embodiment, this disclosure provides an article of the thirty-fifth embodiment, wherein the polyethylene glycol has a number-average molecular weight in the range of 500 g / mol to 2500 g / mol, and wherein the aliphatic isocyanate comprises dicyclohexylmethane-4,4'-diisocyanate. In a thirty-second embodiment, this disclosure provides an article of the thirty-first or thirty-first embodiment, wherein the component further comprises a triol, and wherein the triol contributes 2 mol% to 10 mol% of hydroxyl groups based on the total molar number of hydroxyl groups in the polyethylene glycol, the chain extender, and the triol. In a thirty-third embodiment, this disclosure provides an article of any one of embodiments twenty-eight to thirty-two, the article further comprising a bonding layer located between the first polymer layer and the second polymer layer. In a thirty-fourth embodiment, this disclosure provides an article of the thirty-third embodiment, wherein the bonding layer comprises an ethylene-containing copolymer.In the thirty-fifth embodiment, this disclosure provides an article of manufacture according to any one of the twenty-eighth to thirty-fourth embodiments, wherein the first polymer layer is one of a plurality of layers comprising a porous random network of strands and connecting regions, and wherein the second polymer layer is one of a plurality of continuous polymer film layers.

[0115] The following examples further illustrate the advantages and embodiments of the present invention; however, the specific materials and quantities mentioned in these examples, as well as other conditions and details, should not be construed as undue limitation of the invention. Unless otherwise specified, all parts and percentages are by weight.

[0116] Example

[0117] Example 1: Pressure-sensitive adhesive

[0118] The pressure-sensitive adhesive precursor composition was prepared by mixing 84 parts by weight (pbw) of isooctyl acrylate (IOA), 16 pbw of acrylic acid (AA), and 0.04 pbw of 2,2-dimethoxy-1,2-diphenylethyl-1-one. The mixture was partially polymerized under a nitrogen atmosphere by exposure to low-intensity ultraviolet radiation to obtain a coatable slurry. A monobutyl ether of a linear polymer of 2,2-dimethoxy-1,2-diphenylethyl-1-one, 0.467 pbw of 2,4-bis-trichloromethyl-6-(4-methoxyphenyl)-s-triazine, and 56 pbw of ethylene oxide:propylene oxide (1:1) polyol was added to the slurry and mixed until all components were completely dissolved to obtain the pressure-sensitive adhesive precursor composition.

[0119] The adhesive precursor composition was then applied to a silicone-coated polyethylene-based kraft paper liner using a notched scraper, with a gap set to 0.130 mm (0.005 inch), greater than the liner thickness. The adhesive precursor was then exposed to a total energy of 850 millijoules / cm² from an ultraviolet radiation source, which has a maximum at 351 nm, in a nitrogen-rich environment. The result was a release liner coated with a pressure-sensitive adhesive.

[0120] Example 2: Product

[0121] A seven-layer film was fabricated using a seven-layer annular stacked die (trade name "COEX 7-LAYER" (LF-400 model) from Labtech Engineering, Samut Prakan, Thailand), but with only seven stacked die plates. Airflow to the die was manually controlled to achieve a blow-up ratio of approximately 2:1. The bubbles then collapsed and rolled up approximately 3 meters (10 feet) above the die. Feed material was supplied by seven independent 20mm diameter extruders with an aspect ratio of approximately 30:1.

[0122] A blend containing 91.0 wt% polyurethane 1 and 9 wt% antiblocking agent was melted and fed into the internal channel of an annular stack die using a first extruder at a rate of 15 rpm. The extrusion temperature was maintained at 180°C. Polyurethane 1 was melted and fed onto the subsequent outer layer of the first resin using a second, third, fourth, and fifth extruder at a rate of 15 rpm. A blend containing 46.5 wt% thermoplastic polyolefin, 46.5 wt% EMA, 5 wt% CBA, and 2 wt% carbon black was fed using a sixth extruder at a rate of 60 rpm. The extrusion temperature was maintained at 215°C in layer 6. A blend containing 93.0 wt% thermoplastic polyolefin, 5 wt% CBA, and 2 wt% carbon black was fed using a seventh extruder at a rate of 60 rpm. The 7-layer co-extruded blown film bubbles were collected at a linear velocity of 3.7 ft / min (fpm) and cut to produce individual films. The vapor-permeable pressure-sensitive adhesive of Example 1 on the release liner is manually laminated to the first extruder feed side of the film to obtain an overall vapor-permeable structure with a removable release liner.

[0123] Example 3: Product

[0124] Example 3 was prepared using the method of Example 2 with the following modifications. Both the sixth and seventh extruders were fed at a rate of 90 rpm, and the blown film bubbles were collected at a linear velocity of 4.1 fpm.

[0125] Example 4: Product

[0126] Example 4 was prepared using the method of Example 2 with the following modifications. The blown film bubbles were collected at a linear velocity of 4.1 fpm.

[0127] Example 5: Product

[0128] Example 4 was prepared using the method of Example 2 with the following modifications. Blown film bubbles were collected at a linear velocity of 4.1 fpm. Both the fourth and fifth extruders were fed at a rate of 20 rpm.

[0129] Example 6: Product

[0130] The seven-layer annular stack die described in Example 2 was used. LDPE was melted and fed into the internal channels of the annular stack die at a rate of 60 rpm using the first and second extruders. Polyurethane 1 was melted and extruded onto the subsequent outer layer of the first resin using the third, fourth, and fifth extruders at a rate of 15 rpm using the sixth extruder. A blend containing 46.5 wt% thermoplastic polyolefin, 46.5 wt% EMA, 5 wt% CBA, and 2 wt% carbon black was fed using the sixth extruder at a rate of 60 rpm. The extrusion temperature was maintained at 215°C in layer 6. A blend containing 93.0 wt% thermoplastic polyolefin, 5 wt% CBA, and 2 wt% carbon black was fed using the seventh extruder at a rate of 60 rpm. The 7-layer co-extruded blown film bubbles were collected at a linear velocity of 4.1 fpm and cut to produce individual films. The two inner LDPE layers were peeled off from the film to produce a monolithic 5-layer co-extruded blown film. The vapor-permeable pressure-sensitive adhesive of Example 1 on the release liner is manually laminated to the polyurethane side of the membrane to create an overall vapor-permeable structure with a removable release liner.

[0131] Example 7: Product

[0132] Example 7 was prepared using the method of Example 6 with the following modifications. Both the sixth and seventh extruders were fed at a rate of 90 rpm.

[0133] Water vapor transmission rate evaluation

[0134] The water vapor transmission rates of Examples 1 through 6 were generally evaluated using paragraph 11 of ASTM E96 / E96M, “Standard Test Methods for Water Vapor Transmission of Materials,” at 23°C (73℉) and 50% relative humidity, with the following modifications. Six data points were obtained and used to calculate the transmission rate values. The average transmission rate was determined using the six individual values ​​and reported in Perm. The transmission rates of both samples under each condition were evaluated and reported. The results are shown in Table 2 below.

[0135] Tensile strength

[0136] According to ASTM D412, Method A, Die C, the tensile strength of the specimens was evaluated using an elongation of 508 mm / min (20 inches / min). Tensile strength was measured in both the longitudinal (MD) and transverse (CD) directions. Three measurements were performed for each condition, and the average tensile strength is expressed in pounds per square inch (lb / in). 2 Report as a unit.

[0137] Peel adhesion

[0138] According to ASTM D3330, Method F, peel adhesion was evaluated at a 90-degree angle on stainless steel after a 24-hour dwell time. Measurements were performed twice for each condition, and the average peel adhesion was reported in pounds per inch (lb / in).

[0139]

[0140] Example 8: Product

[0141] The pressure-sensitive adhesive-coated liner was prepared as described in Example 1 above. Polyurethane 2 was hot-melt extruded through a casting die using a twin-screw extruder onto a polyethylene-coated kraft paper liner with a thickness of 0.102 mm (0.004 inches). The pressure-sensitive adhesive was manually laminated onto the polyurethane 2 film. Water vapor transmission rate was evaluated as described above, with results of 13.71 US Perm and 14.57 US Perm.

[0142] Example 9: Product

[0143] As described in Example 8, Example 9 was prepared except that polyurethane 1 was used instead of polyurethane 2. Water vapor transmission rate was evaluated as described above, with results of 18.52 US Perm and 16.65 US Perm.

[0144] Example 10: Product

[0145] As described in Example 8, Example 10 was prepared, except that polyurethane 3 was used instead of polyurethane 2. Water vapor transmission rate was evaluated as described above, with results of 14.31 US Perm and 13.91 US Perm.

[0146] Preparation of aliphatic thermoplastic polyurethane

[0147] Aliphatic thermoplastic polyurethane granules were prepared by reactive extrusion using a ZSK25 twin-screw extruder, available from Coperion Corp., Stuttgart, Germany. This twin-screw extruder has 12 barrel sections, each 100 mm in length. The first barrel is closest to the extruder drive mechanism, and the twelfth barrel is closest to the extruder outlet. Polyethylene glycol diol (added at a rate of 75 g / min) was added to the first barrel section via a heated ZENITH B-9000 gear pump (circor International, Inc., Burlington, MA). 1,4-Butanediol (addition rate 15.4 g / min) was added to the second barrel section via a flowmeter-controlled pump, a Mini-Cori series pump sold by Bronkhorst, Ruurlo, The Netherlands. Dibutyltin dilaurate (addition rate 0.15 g / min) was added to the second barrel section via a syringe pump, purchased from Harvard Apparatus, Holliston, MA. Polycaprolactone triol (addition rate 1.2 g / min) was added to the second barrel section via a syringe pump. A blend of 3 parts by weight of UV absorber and 2 parts by weight of HALS was added to the fourth barrel section via a syringe pump (addition rate 2.25 g / min). H12MDI (addition rate 59.6 g / min) was added to the third barrel section via a second ZENITH B-9000 gear pump. Molten polyurethane was discharged from the extruder into a ZENITH PEP II gear pump, purchased from Circor International, Inc. The polyurethane was then pumped into an underwater pelletizer, model EUP10, purchased from ECON Inc. Monroe, MI.

[0148] Example 11: Product

[0149] The seven-layer annular stacking die described in Example 2 was used. LDPE was melted and fed into the internal channels of the annular stacking die at a rate of 40 rpm using the first, second, and third extruders. The aliphatic thermoplastic polyurethane described above was melted and extruded onto the subsequent outer layer of the first resin using the fourth extruder at a rate of 20 rpm. A blend containing 70.0 wt% EVA 1, 23.0 wt% EVA 2, 5.0 wt% CBA, and 2 wt% TiO2 was melted and fed using the fifth extruder at a rate of 20 rpm. A blend containing 70.0 wt% thermoplastic polyolefin, 23.0 wt% EMA, 5 wt% CBA, and 2 wt% TiO2 was melted and fed using the sixth and seventh extruders at rates of 20 rpm and 60 rpm, respectively. The seven-layer co-extruded blown film bubbles were collected at a linear velocity of 4.1 fpm and cut to produce individual films. The three inner LDPE layers were peeled off from the membrane to produce an integral 4-layer co-extruded blown film. A vapor-permeable pressure-sensitive adhesive on the release liner prepared as described in Example 1 was manually laminated to the polyurethane side of layer 4 of the membrane, resulting in an integrally vapor-permeable structure with a removable release liner. Water vapor transmission rate was evaluated as described above, yielding results of 5.50 US Perm and 5.58 US Perm.

[0150] Examples 12 and 13 and Comparative Example A: Pressure-sensitive adhesive

[0151] A pressure-sensitive adhesive precursor composition was prepared by mixing 90 pbw of IOA, 10 pbw of AA, 0.19 pbw of 2,2-dimethoxy-1,2-diphenylethyl-1-one, and 0.1 pbw of 2,4-bis(trichloromethyl)-6-(4-methoxyphenyl)-triazine. The mixture was partially polymerized under a nitrogen atmosphere by exposure to low-intensity ultraviolet radiation to obtain a coatable slurry. An additional 6.8 pbw of AA, 0.13 pbw of 2,2-dimethoxy-1,2-diphenylethyl-1-one, and amounts of 2,4-bis(trichloromethyl)-6-(4-methoxyphenyl)-triazine, isooctyl mercaptoacetate (IOTG), tallow amine ethoxylate, and tris(15-hydroxyethyl)-N-tallow alkyl-1,3-diaminopropane were added to the slurry and mixed until all components were completely dissolved to obtain the pressure-sensitive adhesive precursor composition. The adhesive precursor composition was then applied to the release liner and cured as described in Example 1.

[0152] Pressure-sensitive adhesive was transferred onto a paper towel for measuring water vapor transmission rate as described above. Additionally, peel adhesion was measured using a 50.8-micron (2 mil) aluminum foil backing according to the test method described above. The results are shown in Table 3 below.

[0153]

[0154] Foreseeable variations and modifications of this disclosure will be apparent to those skilled in the art without departing from the scope and spirit of the invention. The invention should not be limited to the embodiments shown in this application for illustrative purposes.

Claims

1. A pressure-sensitive adhesive comprising an acrylic copolymer and a polyoxyethylene polymer without fluorinated carbon atoms, wherein the acrylic copolymer comprises: Based on the acrylic copolymer, at least 60% by weight of linear or branched (meth)acrylate monomer units; and Based on the acrylic copolymer, there are 12.5% ​​to 40% by weight of (meth)acrylic acid monomer units.

2. The pressure-sensitive adhesive according to claim 1, wherein the acrylic copolymer is crosslinked.

3. The pressure-sensitive adhesive according to claim 1 or 2, wherein the acrylic copolymer is crosslinked with triazine.

4. The pressure-sensitive adhesive according to any one of claims 1 to 3, wherein the pressure-sensitive adhesive is non-foaming.

5. The pressure-sensitive adhesive according to any one of claims 1 to 4, wherein the polyoxyethylene polymer is present in an amount of 20% to 45% by weight based on the total weight of the pressure-sensitive adhesive.

6. The pressure-sensitive adhesive according to any one of claims 1 to 5, wherein the polyoxyethylene polymer is divalent or polyvalent and comprises: At least one of a plurality of ethoxy groups, propoxy groups, or butoxy groups; and It contains a terminal group consisting of at least one of alkyl, hydroxyl, amino, or silyl groups.

7. The pressure-sensitive adhesive according to any one of claims 1 to 6, wherein the polyoxyethylene polymer comprises at least one of alkoxylated alcohols, diols or polyols, alkoxylated amines, diamines or polyamines, alkoxylated esters, alkoxylated amides or alkoxylated carbamates.

8. An article comprising a pressure-sensitive adhesive disposed on a backing according to any one of claims 1 to 7.

9. The article of claim 8, wherein the backing comprises at least one of polyurethane, polyamide, polylactic acid, acrylic block copolymer or amorphous polyester.

10. The article of claim 8 or 9, wherein the backing comprises a porous layer having a first main surface and a second main surface, and a polymer layer disposed on at least the first main surface of the porous layer.

11. The article of claim 10, wherein the polymer layer comprises a crosslinked polyoxyethylene polymer having at least one crosslinking site comprising at least one siloxane bond.

12. The article of any one of claims 8 to 10, wherein the backing comprises a polymer layer containing polyurethane, and wherein the polyurethane is a reaction product of polyethylene glycol, a chain extender, and an aliphatic isocyanate.

13. The article of any one of claims 8 to 12, wherein the pressure-sensitive adhesive is a continuous layer on the backing.

14. The article of any one of claims 8 to 13, wherein the article has a water vapor permeability greater than 1 US Perm or at least 5 US Perm.

15. The article of any one of claims 8 to 14, wherein the release liner is disposed on the pressure-sensitive adhesive opposite to the backing.

Citation Information

Patent Citations

  • Arylaminosilane end-capped urethane sealants

    EP0676403A1

  • Easy to apply air and water barrier articles

    US10704254B2

  • Building membrane with porous pressure sensitive adhesive

    US10899107B2

  • Polymeric multilayer film

    US10953573B2

  • Polymeric multilayer film

    US10953574B2