SiC epitaxial wafer, method for inspecting siC epitaxial wafer, and method for manufacturing siC epitaxial wafer
By bonding a SiC single-crystal substrate layer to a SiC epitaxial wafer and combining it with FT-IR measurement, the problem of accurately measuring the thickness of the SiC epitaxial layer was solved, achieving high-precision thickness determination and ensuring the quality and manufacturing stability of the SiC epitaxial wafer.
Patent Information
- Application Number
- CN202480091399.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-12-09
- Publication Date
- 2026-11-24
AI Technical Summary
In the measurement of SiC epitaxial layer thickness, existing techniques struggle to accurately separate multiple interference waveforms, leading to inaccurate thickness measurement and impacting the stability of the device manufacturing process.
By attaching a SiC single-crystal substrate layer to a substrate, the thickness of the SiC epitaxial layer is calculated using Fourier transform infrared spectroscopy (FT-IR) combined with the film thickness information of the SiC single-crystal substrate layer. The film thickness at multiple measurement points is determined using a non-destructive measurement method.
This technology enables accurate determination of SiC epitaxial layer thickness, improves the quality assurance accuracy of SiC epitaxial wafers, and reduces the risk of failures during the process.
Smart Images

Figure CN123165477A_ABST
Abstract
Description
Technical Field
[0001] This disclosure relates to SiC epitaxial wafers, methods for inspecting SiC epitaxial wafers, and methods for manufacturing SiC epitaxial wafers. Background Technology
[0002] Compared to silicon (Si), silicon carbide (SiC) has an insulating breakdown electric field that is an order of magnitude larger and a band gap that is three times larger. Furthermore, SiC exhibits approximately three times the thermal conductivity of silicon (Si). Therefore, SiC is expected to be used in power devices, high-frequency devices, and similar applications. Moreover, devices using SiC can operate at temperatures above 150°C. Consequently, in recent years, SiC epitaxial wafers have been used as substrates for semiconductor devices as described above.
[0003] SiC epitaxial wafers are obtained by stacking SiC epitaxial layers on the surface of a SiC substrate. High-quality SiC substrates are expensive. On the other hand, the active layer that embodies the actual function of the device is a thin region of about a few μm to several hundred μm on the surface of the SiC epitaxial wafer, while the rest serves as a support to facilitate handling.
[0004] In recent years, in order to prevent the high cost of SiC epitaxial wafers, research has been conducted on bonding high-quality SiC substrates to low-cost substrates (e.g., Patent Document 1).
[0005] Existing technical documents
[0006] Patent documents
[0007] Patent Document 1: Japanese Patent Application Publication No. 2023-118516 Summary of the Invention
[0008] The problem the invention aims to solve
[0009] When fabricating SiC devices using SiC epitaxial wafers, the thickness of the SiC epitaxial layer is crucial information. If the measured thickness differs from the actual thickness, it can sometimes cause malfunctions during the fabrication process. The thickness of the SiC epitaxial layer is sometimes determined, for example, using Fourier transform infrared spectroscopy (FT-IR). FT-IR determines the thickness based on the interference waveforms of surface and interface reflections through Fourier transform. In cases with multiple interfaces, multiple interference waveforms are typically generated. However, if these interference waveforms overlap, it becomes impossible to separate the expected interference waveforms, sometimes resulting in inaccurate measurement of the thickness of the layer being measured.
[0010] This disclosure was made in view of the above-mentioned problems, and provides a SiC epitaxial wafer in which the thickness of the SiC epitaxial layer can be determined even when a composite substrate with a SiC single crystal layer attached to a substrate is used, as well as a method for inspecting and manufacturing the SiC epitaxial wafer.
[0011] Technical solutions for solving the problem
[0012] Based on in-depth research, the inventors discovered that when a SiC epitaxial layer is crystallized and grown on a composite substrate with a SiC single crystal layer attached to the substrate, the film thickness of the SiC epitaxial layer cannot be directly measured from the interference waveform of FT-IR.
[0013] To address the aforementioned problems, this disclosure provides the following technical solutions.
[0014] (1) The SiC epitaxial wafer of the first embodiment includes a substrate, a SiC single crystal substrate layer, and a SiC epitaxial layer. The SiC single crystal substrate layer is attached to the substrate. The SiC epitaxial layer is stacked on the side of the SiC single crystal substrate layer facing the side that contacts the substrate and the SiC single crystal substrate layer. The film thickness of the SiC epitaxial layer of the SiC epitaxial wafer of the first embodiment has been determined.
[0015] (2) In the SiC epitaxial wafer involved in the above scheme, the film thickness of the SiC epitaxial layer can also be determined by directly measuring the substrate to which the film thickness is to be determined.
[0016] (3) In the SiC epitaxial wafer involved in the above scheme, the film thickness of the SiC epitaxial layer at multiple different measurement points in the plane may also be determined.
[0017] (4) In the SiC epitaxial wafer involved in the above scheme, the film thickness of the SiC epitaxial layer can also be a value obtained from the first film thickness determined by Fourier transform infrared spectroscopy and the film thickness of the SiC single crystal substrate layer.
[0018] (5) The inspection method for SiC epitaxial wafers involved in the second scheme includes a Fourier transform infrared spectroscopy measurement step and a film thickness determination step. In the Fourier transform infrared spectroscopy measurement step, incident light is irradiated from the SiC epitaxial layer side of the SiC epitaxial wafer, which is formed by bonding a SiC single crystal substrate layer to a substrate and depositing a SiC epitaxial layer on the SiC single crystal substrate layer, and the first film thickness is measured. In the film thickness determination step, the film thickness of the SiC epitaxial layer is determined based on the first film thickness and the film thickness of the SiC single crystal substrate layer.
[0019] (6) The manufacturing method of SiC epitaxial wafer involved in the third scheme includes the inspection method of SiC epitaxial wafer involved in the above scheme.
[0020] Invention Effects
[0021] The thickness of the SiC epitaxial layer in the SiC epitaxial wafer disclosed herein has been determined, ensuring high precision in quality assurance. Furthermore, the inspection and manufacturing methods for the SiC epitaxial wafer disclosed herein enable the determination of the SiC epitaxial layer thickness. Attached Figure Description
[0022] Figure 1 This is a plan view of the SiC epitaxial wafer according to the first embodiment.
[0023] Figure 2 This is a cross-sectional view of the SiC epitaxial wafer according to the first embodiment.
[0024] Figure 3 This is a schematic diagram illustrating the Fourier transform infrared spectroscopy measurement step in the inspection method for SiC epitaxial wafers according to the first embodiment.
[0025] Figure 4 The results are FT-IR measurements of the SiC epitaxial wafer according to the first embodiment. Detailed Implementation
[0026] Hereinafter, this embodiment will be described in detail with appropriate reference to the accompanying drawings. To facilitate understanding of the features of this embodiment, the drawings used in the following description may sometimes show enlarged portions of the features for convenience, and the dimensions and proportions of the constituent elements may sometimes differ from the actual dimensions. The materials, dimensions, etc., illustrated in the following description are examples, and this disclosure is not limited thereto; appropriate modifications can be made to implement the embodiment without altering its spirit.
[0027] In this specification, [] represents a single orientation, <> represents a group orientation, () represents a single facet, and {} represents a group facet. Regarding negative exponents, in crystallography, a "-" (hyphen) is marked above the number, but in this specification, a minus sign is marked before the number.
[0028] First, the direction is defined. The thickness direction of the SiC epitaxial wafer 10 is set as the Z direction. The Z direction can be the thickness direction of the SiC epitaxial layer 3. <0001> Direction can also be relative to <0001> Directional tilt deviation angle. One direction of the plane orthogonal to the Z direction is designated as the X direction. Additionally, within the plane orthogonal to the Z direction, a direction orthogonal to the X direction is designated as the Y direction. The X direction is, for example, <11-20> of SiC epitaxial layer 3. The Y direction is, for example, <1-100> of SiC epitaxial layer 3.
[0029] Figure 1This is a plan view of the SiC epitaxial wafer 10 according to this embodiment. The SiC epitaxial wafer 10 is a generally circular wafer when viewed from above. The SiC epitaxial wafer 10 may also have positioning grooves or positioning edges for guiding the orientation of the crystal axis.
[0030] The diameter of the SiC epitaxial wafer 10 is not particularly limited. The diameter of the SiC epitaxial wafer 10 is, for example, 145 mm or more, preferably 149 mm or more. The diameter of the SiC epitaxial wafer 10 is, for example, 155 mm or less, preferably 151 mm or less. The diameter of the SiC epitaxial wafer 10 is, for example, 195 mm or more, preferably 199 mm or more. The diameter of the SiC epitaxial wafer 10 is, for example, 205 mm or less, preferably 201 mm or less. The diameter of the SiC epitaxial wafer 10 is, for example, 245 mm or more, preferably 249 mm or more. The diameter of the SiC epitaxial wafer 10 is, for example, 255 mm or less, preferably 251 mm or less. The diameter of the SiC epitaxial wafer 10 is, for example, 295 mm or more, preferably 299 mm or more. The diameter of the SiC epitaxial wafer 10 is, for example, 305 mm or less, preferably 301 mm or less.
[0031] Figure 2 This is a cross-sectional view of the SiC epitaxial wafer 10 according to this embodiment. The SiC epitaxial wafer 10 has a substrate 1, a SiC single crystal substrate layer 2, and a SiC epitaxial layer 3.
[0032] The substrate 1 is a support substrate that improves the transportability of the SiC epitaxial wafer 10. The substrate 1 can be, for example, polycrystalline SiC, single-crystal SiC, SiC sintered material, ceramic, single-crystal Si, or Si with a SiO2 film. When the substrate 1 is single-crystal SiC, the quality of the single-crystal SiC in the substrate 1 can be lower than that in the SiC single-crystal substrate layer 2. For example, the defect density in the single-crystal SiC of the substrate 1 can be higher than the defect density in the SiC single-crystal substrate layer 2. The substrate 1 is not limited to a single layer and can also be composed of multiple layers.
[0033] The thickness of the substrate 1 is, for example, 100 μm or more and 1000 μm or less. The thickness of the substrate 1 is preferably 150 μm or more and 500 μm or less, more preferably 200 μm or more and 400 μm or less, and even more preferably 325 μm or more and 375 μm or less.
[0034] If the substrate is in a state before the SiC single crystal substrate layer 2 is attached, the thickness of the substrate 1 can be measured using a thickness gauge or spectral interferometry. When measuring the thickness of the substrate 1 in the state of the SiC epitaxial wafer 10, a cross-section is cut, and the thickness of the substrate 1 is measured from the cross-sectional image using a scanning electron microscope (SEM) or a transmission electron microscope (TEM).
[0035] The thickness of the substrate 1 is measured, for example, at its center when viewed from above. Alternatively, the thickness of the substrate 1 can be measured at multiple equally spaced measurement points along a straight line passing through the center of the substrate 1 when viewed from above. For example, the thickness of the substrate 1 can be measured at each of the following points: the center, points equally spaced in the X direction with reference to the center, and points equally spaced in the Y direction with reference to the center. When the thickness of the substrate 1 is measured at multiple measurement points, the average value of the measurements at each measurement point can be considered as the thickness of the substrate 1.
[0036] The SiC single crystal substrate layer 2 is bonded to the substrate 1. The SiC single crystal substrate layer 2 is in contact with the substrate 1 and is bonded to the substrate 1.
[0037] The SiC single crystal substrate layer 2 is formed, for example, from a single crystal of SiC. There are no particular limitations on the polymorphism of the SiC single crystal substrate layer 2; it can be any of 2H, 3C, 4H, or 6H. For example, the SiC single crystal substrate layer 2 is 4H-SiC.
[0038] The SiC single-crystal substrate layer 2 can also be doped with a dopant element, for example, nitrogen. The concentration of the dopant element in the SiC single-crystal substrate layer 2 is, for example, 5 × 10⁻⁶. 18 atoms / cm 3 Above and 2×10 19 atoms / cm 3 the following.
[0039] The film thickness of the SiC single crystal substrate layer 2 is, for example, 3 μm or less. The film thickness of the SiC single crystal substrate layer 2 is preferably 0.3 μm or more and 2 μm or less, more preferably 0.5 μm or more and 1.5 μm or less, and even more preferably 0.8 μm or more and 1.2 μm or less.
[0040] For example, if it is possible to obtain substrates before and after the SiC single crystal substrate layer 2 is bonded to the substrate 1, the film thickness of the SiC single crystal substrate layer 2 can be determined by subtracting the thickness of the substrate before bonding the SiC single crystal substrate layer 2 from the thickness of the substrate after bonding the SiC single crystal substrate layer 2. Alternatively, if a finished SiC epitaxial wafer 10 is obtained, a cross-section is cut, and the film thickness of the SiC single crystal substrate layer 2 is measured from the cross-sectional image using a scanning electron microscope (SEM) or a transmission electron microscope (TEM). However, measuring the film thickness of the SiC single crystal substrate layer 2 requires destructive testing of the SiC epitaxial wafer 10, making it difficult to determine the film thickness of the SiC single crystal substrate layer 2 non-destructively. The measurement location of the film thickness of the SiC single crystal substrate layer 2 is the same as the measurement location of the thickness of the substrate 1. Preferably, the film thickness of the SiC single crystal substrate layer 2 is measured at the same location as the location where the thickness of the substrate 1 was measured. In addition, when the film thickness of SiC single crystal substrate layer 2 is measured at multiple measurement points, the average value of the measured values at each measurement point can be regarded as the film thickness of SiC single crystal substrate layer 2.
[0041] The first surface of the SiC single-crystal substrate layer 2 may or may not have an offset angle relative to the (0001) surface in the <11-20> direction. The first surface of the SiC single-crystal substrate layer 2 preferably has an offset angle in the <11-20> direction. The offset angle is, for example, greater than 0° and less than 10°, preferably more than 0.1° and less than 8°, more preferably more than 3.5° and less than 4.5°, and even more preferably 4°. The first surface of the SiC single-crystal substrate layer 2 may also not have an offset angle relative to the (0001) surface in the <1-100> direction. The first surface of the SiC single-crystal substrate layer 2 is, for example, the surface that contacts the SiC epitaxial layer 3 of the SiC single-crystal substrate layer 2.
[0042] The SiC epitaxial layer 3 is stacked on the SiC single crystal substrate layer 2. The SiC epitaxial layer 3 is stacked on the SiC single crystal substrate layer 2, with the surfaces that are in contact with the substrate 1 and the SiC single crystal substrate layer 2 facing each other.
[0043] The SiC epitaxial layer 3 is formed from a single crystal of SiC. The SiC epitaxial layer 3 is a layer obtained by epitaxial growth of SiC on a SiC single-crystal substrate layer 2. The SiC epitaxial layer 3 may also contain dopant elements, for example, nitrogen. The concentration of the dopant element in the SiC epitaxial layer 3 is, for example, 5 × 10⁻⁶. 13 atoms / cm 3 Above and 2×10 18 atoms / cm 3 the following.
[0044] The thickness of the SiC epitaxial layer 3 has been determined. The thickness of the SiC epitaxial layer 3 is determined non-destructively, allowing the SiC epitaxial wafer 10 to be marketed as a product. The thickness of the SiC epitaxial layer 3 is determined as information to ensure the quality of the SiC epitaxial wafer 10. The thickness of the SiC epitaxial layer 3 is processed along with the SiC epitaxial wafer 10, for example, as an inspection report. The inspection report can be an actual written document or data. The SiC epitaxial wafer 10 and the inspection report are processed as a dataset of the SiC epitaxial wafer. Those responsible for subsequent processes in the fabrication of SiC devices can verify quality using the dataset of the SiC epitaxial wafer.
[0045] The thickness of the SiC epitaxial layer 3 can be determined at a predetermined location within the plane, or at multiple locations within the plane. For example, the thickness of the SiC epitaxial layer 3 can be determined at the center of the SiC epitaxial wafer 10. Alternatively, the thickness of the SiC epitaxial layer 3 can be determined at multiple measurement points within the plane of the SiC epitaxial wafer 10. These multiple measurement points are, for example, the same locations where the thickness was measured on the substrate 1. By determining the thickness of the SiC epitaxial layer 3 at these multiple measurement points, the in-plane distribution of the thickness can be confirmed. Alternatively, the thickness of the SiC epitaxial layer 3 can be determined at multiple measurement points, and the average thickness of each measurement point can be considered as the thickness of the SiC epitaxial layer 3.
[0046] The thickness of the SiC epitaxial layer 3 can be determined, for example, by directly measuring the target substrate. By determining the thickness of the target substrate itself, rather than preparing a measurement substrate or the like under the same conditions, the accuracy of quality assurance for the SiC epitaxial wafer 10 is improved. The thickness of the SiC epitaxial layer 3 can be determined, for example, based on the state of the SiC epitaxial wafer 10 having the SiC epitaxial layer 3.
[0047] The thickness of the SiC epitaxial layer 3 in the target substrate can be determined, for example, from the first film thickness measured by Fourier transform infrared spectroscopy (FT-IR) and the film thickness of the SiC single crystal substrate layer 2. If this method is used, the film thickness of the SiC epitaxial layer 3 can be measured non-destructively without damaging the target substrate.
[0048] The thickness of the SiC epitaxial layer 3 can be determined, for example, according to the following inspection method for the SiC epitaxial wafer 10.
[0049] The inspection methods for SiC epitaxial wafer 10 include a Fourier transform infrared spectroscopy measurement process and a film thickness determination process.
[0050] Figure 3This is a schematic diagram illustrating the Fourier transform infrared spectroscopy measurement process in the inspection method for SiC epitaxial wafer 10. In the Fourier transform infrared spectroscopy measurement process, incident light L1 is irradiated from the SiC epitaxial layer 3 side of the SiC epitaxial wafer 10. A portion of the incident light L1 is reflected at the surface of the SiC epitaxial layer 3, becoming reflected light L2. A portion of the incident light L1 is reflected at the interface between the SiC single crystal substrate layer 2 and the SiC epitaxial layer 3, becoming reflected light L3. A portion of the incident light L1 is reflected at the interface between the substrate 1 and the SiC single crystal substrate layer 2, becoming reflected light L4.
[0051] Figure 4 This example illustrates the results of a Fourier transform infrared spectroscopy (FT-IR) measurement process on the SiC epitaxial wafer 10 according to this embodiment. FT-IR determines the film thickness using Fourier transform based on the interference waveforms of surface and interface reflections. In cases with multiple interfaces, multiple interference waveforms are generally generated, but... Figure 4 In the example shown, the interference waveforms are superimposed to each other, resulting in a single interference waveform. This is attributed to the superposition of the interference waveforms of reflected light L2 and L3 with those of reflected light L2 and L4. In the Fourier transform infrared spectroscopy measurement process, only one film thickness is determined as the first film thickness.
[0052] Since the first film thickness is calculated based on the information obtained by superimposing the interference waveforms of reflected light L2 and L3 with the interference waveforms of reflected light L2 and L4, it does not accurately represent the film thickness of SiC epitaxial layer 3.
[0053] In the film thickness determination process, the film thickness of the SiC epitaxial layer 3 is determined based on the first film thickness and the film thickness of the SiC single crystal substrate layer 2. The film thickness of the SiC epitaxial layer 3 is determined, for example, based on the following formula (1).
[0054] t3 = t1 - t2 + a (1)
[0055] In equation (1), t3 is the thickness of the SiC epitaxial layer 3, t1 is the first film thickness, t2 is the thickness of the SiC single crystal substrate layer 2, and a is a correction value.
[0056] The first film thickness t1 is determined based on the FT-IR measurement results described above. The film thickness t2 of the SiC single crystal substrate layer 2 can be confirmed based on the manufacturing history information during the fabrication of the SiC single crystal substrate layer 2. If manufacturing history information is unavailable, measurements can be performed, for example, using spectral interferometry, before the SiC epitaxial layer 3 is formed. Before the SiC epitaxial layer 3 is formed, there is no problem of interference waveform superposition, thus the film thickness of the SiC single crystal substrate layer 2 can be measured. The correction value a is determined by the film thickness t2 of the SiC single crystal substrate layer 2 and the concentration of the dopant element in the SiC single crystal substrate layer 2. The specific value of the correction value for a SiC single crystal substrate layer 2 with a predetermined thickness and a predetermined dopant element concentration is determined through prior research. For example, a table outlining the relationship between film thickness, dopant element concentration, and correction value can be prepared in advance, and an appropriate correction value can be selected based on the structure of the SiC single crystal substrate layer 2.
[0057] If the inspection method of the SiC epitaxial wafer 10 according to this embodiment is used, the film thickness of the SiC epitaxial layer 3 of the substrate to be evaluated can be determined in a non-destructive manner.
[0058] The inspection method for the SiC epitaxial wafer 10 described in this embodiment can be incorporated into the manufacturing method of the SiC epitaxial wafer 10. The manufacturing method of the SiC epitaxial wafer 10 includes, for example, a substrate preparation process, a SiC single crystal substrate preparation process, a bonding process, a SiC single crystal substrate separation process, a SiC epitaxial layer deposition process, and an inspection process.
[0059] In the substrate preparation process, the substrate 1 described above is prepared. In the SiC single crystal substrate preparation process, a SiC single crystal substrate is prepared. By performing the single crystal substrate separation process described later, a portion of the SiC single crystal substrate becomes the SiC single crystal substrate layer 2. Therefore, the SiC single crystal substrate is the same as the SiC single crystal substrate layer 2 described above. The SiC single crystal substrate can be fabricated, for example, by sublimation, by gas chromatography, or by solution chromatography.
[0060] Ions can be implanted into SiC single-crystal substrates. The implanted ions can be, for example, hydrogen ions. By keeping the ion implantation energy constant, ion-implanted regions can be formed at the same height. By changing the ion implantation energy, the location of the ion-implanted region can be freely controlled. When cutting a portion of the SiC single-crystal substrate using a wire saw, laser, or similar method, it is not necessary to implant ions into the SiC single-crystal substrate.
[0061] In the bonding process, the substrate 1 and the SiC single crystal substrate are bonded together. The substrate 1 and the SiC single crystal substrate can be bonded by overlapping and applying pressure after the bonding surfaces have been activated. Activation of the bonding surfaces can be performed, for example, by irradiating the bonding surfaces with ions. By performing the bonding process, a composite substrate formed by bonding the substrate 1 and the SiC single crystal substrate can be obtained.
[0062] In the SiC single crystal substrate separation process, a portion of the SiC single crystal substrate is separated from the composite substrate. The SiC single crystal substrate is separated in the thickness direction. For example, by heating the SiC single crystal substrate, the SiC single crystal substrate is separated along the ion-implanted portion. Alternatively, the SiC single crystal substrate can also be cut and separated using a wire saw, laser, or the like. By separating a portion of the SiC single crystal substrate, SiC single crystal substrate layer 2 is obtained.
[0063] In the SiC epitaxial layer deposition process, a SiC epitaxial layer 3 is deposited on one side of the aforementioned SiC single-crystal substrate layer 2. The SiC epitaxial layer 3 can be fabricated using known methods.
[0064] The inspection process can be performed using the method described above. By performing the inspection process, a SiC epitaxial wafer 10 in which the thickness of the SiC epitaxial layer 3 is appropriately determined can be fabricated.
[0065] Furthermore, a device structure is formed on the SiC epitaxial layer 3 of the SiC epitaxial wafer 10, and the wafer is chip-sized to obtain a SiC device. In the manufacturing process of the SiC device, if the film thickness of the SiC epitaxial layer 3 is appropriately determined, process defects are less likely to occur.
[0066] For the SiC epitaxial wafer 10 according to this embodiment, since the film thickness of the SiC epitaxial layer 3 has been appropriately determined, the quality of the SiC epitaxial wafer 10 can be guaranteed with high precision. A SiC epitaxial wafer assembly containing an inspection result sheet of the SiC epitaxial wafer 10 and the film thickness of the SiC epitaxial layer 3 can suppress process defects caused by differences between the measured film thickness and the actual film thickness of the SiC epitaxial layer.
[0067] The preferred embodiments of this disclosure have been described in detail above, but this disclosure is not limited to specific embodiments. Various modifications and alterations can be made within the scope of the spirit of this disclosure as set forth in the claims.
[0068] The SiC epitaxial wafer 10 may also have a bonding layer between the substrate 1 and the SiC single-crystal substrate layer 2. The bonding layer, located between the substrate 1 and the SiC single-crystal substrate layer 2, is a layer containing carbon, silicon, and nitrogen. The bonding layer is formed by bonding the substrate 1 and the SiC single-crystal substrate layer 2 together. The bonding layer contains, for example, elements constituting the substrate 1 or the SiC single-crystal substrate layer 2. The bonding layer can sometimes be identified by observing a cross-section of the composite substrate 10 using a transmission electron microscope (TEM). The thickness of the bonding layer can be, for example, 0.25 nm or more and 10 nm or less. The thickness of the bonding layer can sometimes be determined based on a cross-sectional image taken with a transmission electron microscope (TEM). However, the resolution of the transmission electron microscope needs to be considered.
[0069] Explanation of reference numerals in the attached figures
[0070] 1. Substrate
[0071] 2 SiC single crystal substrate layer
[0072] 3 SiC epitaxial layer
[0073] 10 SiC epitaxial wafers
[0074] L1 Incident light
[0075] L2, L3, L4 reflected light
Claims
1. A SiC epitaxial wafer, It comprises a substrate, a SiC single-crystal substrate layer, and a SiC epitaxial layer. The SiC single crystal substrate layer is bonded to the substrate. The SiC epitaxial layer is stacked on the SiC single crystal substrate layer, with the surfaces facing each other and in contact with the substrate and the SiC single crystal substrate layer. The thickness of the SiC epitaxial layer has been determined.
2. The SiC epitaxial wafer according to claim 1, The thickness of the SiC epitaxial layer is determined by directly measuring the substrate on which the thickness is to be determined.
3. The SiC epitaxial wafer according to claim 1, The film thickness of the SiC epitaxial layer at multiple different measurement points within the plane has been determined.
4. The SiC epitaxial wafer according to claim 1, The thickness of the SiC epitaxial layer is a value obtained by combining the first film thickness determined by Fourier transform infrared spectroscopy with the film thickness of the SiC single crystal substrate layer.
5. A method for inspecting SiC epitaxial wafers, It has a Fourier transform infrared spectroscopy measurement process and a film thickness determination process. In the Fourier transform infrared spectroscopy measurement process, incident light is irradiated from the SiC epitaxial layer side of the SiC epitaxial wafer, which is formed by bonding a SiC single crystal substrate layer to a substrate and depositing a SiC epitaxial layer on the SiC single crystal substrate layer, and the thickness of the first film is measured. In the film thickness determination process, the film thickness of the SiC epitaxial layer is determined based on the first film thickness and the film thickness of the SiC single crystal substrate layer.
6. A method for manufacturing SiC epitaxial wafers, The method for inspecting SiC epitaxial wafers as described in claim 5.
Citation Information
Patent Citations
Polycrystalline sic substrate and semiconductor substrate
JP2023118516A