Glass yarn, glass cloth, prepreg and printed circuit board

By controlling the silicon content and kink index of the glass cloth, combined with optimized silane coupling agent treatment, the flatness and fuzziness problems of the glass cloth are solved, and the dielectric properties of the glass cloth are improved, making it suitable for high-performance printed circuit boards and electronic devices.

CN123165481APending Publication Date: 2026-11-24ASAHI KASEI KOGYO KABUSHIKI KAISHA
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202480091359.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2024-05-09
Filing Date
2024-12-24
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

In the prior art, the flatness and fuzziness problems of glass cloth have not been effectively solved, and the residue of silane coupling agent causes the dielectric loss tangent to increase, affecting the dielectric properties of glass cloth.

Method used

By controlling the silicon content and kink index of the glass yarn, and by selectively using silane coupling agents, the manufacturing process of glass cloth can be optimized to reduce the kink index and improve the flatness and hairiness frequency of the glass cloth.

Benefits of technology

It achieves excellent flatness and reduced fuzz frequency of glass cloth, while improving dielectric properties, making it suitable for high-performance printed circuit boards and electronic devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123165481A_ABST
    Figure CN123165481A_ABST
Patent Text Reader

Abstract

The problem to be solved by this invention is to provide a glass cloth with excellent flatness and reduced fuzzing frequency. The glass cloth of this invention is a glass cloth composed of glass yarn, wherein the silicon (Si) content in the glass yarn is 95.0 to 100% by mass (converted to silicon dioxide (SiO2), and the twist index of the glass yarn is 400 mm or less. Alternatively, the glass cloth of this invention is a glass cloth composed of glass yarn, wherein the bulk dielectric loss tangent of the glass constituting the glass yarn is 0.001 or less at 10 GHz, and the twist index of the glass yarn is 400 mm or less.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This disclosure relates to glass yarn, glass cloth, prepreg, and printed circuit boards, etc. Background Technology

[0002] Currently, the high performance of information terminals such as smartphones and the high speed of communication, represented by 5G, are constantly developing. Against this backdrop, especially for printed circuit boards (PCBs) used in high-speed communication, there is a demand not only for improvements in heat resistance, which has always been required, but also for further improvements in the dielectric properties of their insulating materials (e.g., lower dielectric loss tangent). Similarly, improvements in the dielectric properties of the prepregs used in the insulating materials of PCBs, as well as the glass yarn and glass cloth contained within those prepregs, are also desired.

[0003] To achieve low dielectric properties in insulating materials, methods for constructing insulating materials using prepregs made by impregnating glass cloth with a low dielectric resin (hereinafter referred to as "matrix resin") are known (e.g., Patent Documents 1 and 2). Patent Documents 1 and 2 describe that polyphenylene ethers end-modified with vinyl or methacryloyloxy groups are advantageous in terms of low dielectric properties and heat resistance; and that such modified polyphenylene ethers are used as matrix resins.

[0004] Furthermore, for the purpose of improving the flatness of glass cloth and stabilizing signal transmission speed, a glass fiber yarn with a yarn bending density of 0.10 bends / cm or less, using yarn bending points with a radius of curvature of 5 mm or less and a bend angle of 120 degrees or less, has been reported (see, for example, Patent Document 3). Patent Document 3 describes obtaining a quartz glass ingot with a desired roundness by externally grinding a quartz glass ingot using an external cylindrical grinding machine, and then obtaining glass filaments as raw materials for glass fiber yarn by using such a quartz glass ingot with the desired roundness.

[0005] In addition, inventions that include surface treatment of glass cloth with a silane coupling agent and adjustment of the loss on ignition value of the glass cloth to 0.13 to 0.40% by mass have been reported (see, for example, Patent Document 4). Patent Document 4 describes that by adjusting the loss on ignition value of glass cloth woven from glass yarn formed of glass filaments with a silica (SiO2) composition of 98 to 100% by mass to the above range, insulation reliability can be improved, and the generation of fuzz in the glass cloth can be suppressed.

[0006] In addition, the invention described in Patent Document 5 is reported as an invention in this technical field.

[0007] Existing technical documents

[0008] Patent documents

[0009] Patent Document 1: International Publication No. 2019 / 065940

[0010] Patent Document 2: International Publication No. 2019 / 065941

[0011] Patent Document 3: Japanese Patent Application Publication No. 2020-90432

[0012] Patent Document 4: Japanese Patent Application Publication No. 2018-127747

[0013] Patent Document 5: International Publication No. 2022 / 215288 Summary of the Invention

[0014] The problem the invention aims to solve

[0015] However, in the invention described in Patent Document 3, the yield rate is reduced because the quartz glass ingot needs to be ground on its outer diameter. Therefore, there is a strong demand for a technology that can improve the flatness of glass cloth without requiring special processing such as outer diameter grinding.

[0016] Furthermore, as described in Patent Document 4, in inventions that include surface treatment of glass cloth using a silane coupling agent as a requirement, there is a problem of an increase in the dielectric loss tangent of the glass cloth if the silane coupling agent is accidentally left on the glass surface (see, for example, Patent Document 5 above). Therefore, there is also a strong demand for a technique to suppress the fuzzing of glass cloth by means other than adjusting the loss on ignition value.

[0017] The purpose of this disclosure is to provide a glass cloth with excellent flatness and reduced fuzz generation frequency. Another purpose of this disclosure is to provide a method for manufacturing the glass cloth, a glass yarn roll, and the glass yarn itself. Furthermore, another purpose of this disclosure is to provide prepregs, printed circuit boards, integrated circuits, and electronic devices using the glass cloth.

[0018] Solution for solving the problem

[0019] Examples of embodiments of this disclosure are described below. [1]

[0021] A type of glass cloth, which is a glass cloth made of glass yarn.

[0022] The silicon (Si) content in the glass yarn, converted from silicon dioxide (SiO2), is 95.0~100% by mass, and the snarl index of the glass yarn is below 400 mm. [2]

[0024] A type of glass cloth, which is a glass cloth made of glass yarn.

[0025] The bulk dielectric loss tangent of the glass constituting the glass yarn is 0.001 or less at 10 GHz, and the kink index of the glass yarn is 400 mm or less. [3]

[0027] According to the glass cloth described in Project 1 or 2, the twist index of the glass yarn is 70 mm or more. [4]

[0029] According to the glass cloth of Project 1 or 2, wherein the glass yarn comprises glass yarn satisfying the ranges described in the following formulas (A), (B) and (C):

[0030] (A)x+y+z=100% mass

[0031] (B)x≥99.5% of mass

[0032] (C) 0.0003ppm ≤ y ≤ 0.50ppm

[0033] x: Silicon content when converted to silicon dioxide (SiO2)

[0034] y: Total content of uranium and thorium

[0035] z: Total content of elements other than silicon, uranium, and thorium. [5]

[0037] According to the glass cloth described in Project 4, the range of x is 99.6% by mass or more. [6]

[0039] According to the glass cloth described in Project 4, the range of x is 99.9% or more by mass. [7]

[0041] The glass cloth according to any one of items 1 to 6, wherein the glass yarn is treated with a surface treatment agent containing a silane coupling agent. [8]

[0043] The glass cloth according to Project 7, wherein the surface treatment agent comprises the silane coupling agent shown in Formula (1).

[0044] X(R) 3-n SiY n ···(1)

[0045] (In formula (1), X is an organic functional group having at least one of an amino group and an unsaturated double bond group, wherein the unsaturated double bond group is free radical reactive, Y is each independently an alkoxy group, n is an integer of 1 or more and 3 or less, and R is each independently a group selected from the group consisting of methyl, ethyl and phenyl groups) [9]

[0047] According to the glass cloth described in Project 8, X in the formula (1) is an organic functional group that does not form salts with ionic compounds.

[10]

[0049] The glass cloth according to item 8 or 9, wherein X in formula (1) is free of amines and / or ammonium cations.

[11]

[0051] The glass cloth according to any one of items 8 to 10, wherein X in formula (1) is an organic functional group having methacryloyloxy and / or acryloyloxy.

[12]

[0053] The glass cloth according to any one of items 1 to 11, wherein the absolute value of the twist count of the glass yarn is in the range of 0.5 to 1.5 times / 25 mm.

[13]

[0055] The glass cloth according to any one of items 1 to 12, wherein the glass cloth has the glass yarn as warp and weft yarn,

[0056] The absolute value of the difference in twist count between the warp and weft yarns is in the range of 0.01 to 0.70 twists / 25mm.

[14]

[0058] The glass cloth according to any one of items 1 to 13, wherein the thickness of the glass cloth is less than 60 μm.

[15]

[0060] The glass cloth according to any one of items 1 to 14 is used for printed circuit boards.

[16]

[0062] A prepreg comprising glass cloth and thermosetting resin as described in any one of items 1 to 15.

[17]

[0064] A printed circuit board comprising the prepreg described in item 16.

[18]

[0066] An integrated circuit comprising the printed circuit board described in item 17.

[19]

[0068] An electronic device comprising the printed circuit board described in item 17.

[20]

[0070] A method for manufacturing glass cloth includes a step of obtaining glass cloth using glass yarn.

[0071] The silicon (Si) content in the glass yarn, calculated as silicon dioxide (SiO2), is in the range of 95.0~100% by mass.

[0072] The twist index of the glass yarn is below 400 mm. [twenty one]

[0074] A method for manufacturing glass cloth includes a step of obtaining glass cloth using glass yarn.

[0075] The bulk dielectric loss tangent of the glass constituting the glass yarn is below 0.001 at 10 GHz.

[0076] The twist index of the glass yarn is below 400 mm. [twenty two]

[0078] According to the manufacturing method of glass cloth described in Project 20 or 21, the twist index of the glass yarn is 70 mm or more. [twenty three]

[0080] The method for manufacturing glass cloth according to item 20 or 21 includes the step of obtaining glass cloth using glass yarn.

[0081] The glass yarn satisfies the ranges described in equations (A), (B), and (C) below:

[0082] (A)x+y+z=100% mass

[0083] (B)x≥99.5% of mass

[0084] (C) 0.0003ppm ≤ y ≤ 0.50ppm

[0085] x: Silicon content when converted to silicon dioxide (SiO2)

[0086] y: Total content of uranium and thorium

[0087] z: Total content of elements other than silicon, uranium, and thorium. [twenty four]

[0089] The method for manufacturing glass cloth according to any one of items 20 to 23 includes:

[0090] The process of warping the glass yarn used as warp yarn (warp warping process), and

[0091] The process of weaving using the aforementioned glass yarn (weaving process),

[0092] In the warp winding process and / or the weaving process, the absolute value of the twist count of the glass yarn is adjusted to a range of 0.5 to 1.5 times / 25 mm.

[25]

[0094] According to the method for manufacturing glass cloth described in Project 24, the glass cloth has glass yarn as warp and weft yarn.

[0095] The manufacturing method includes a step of adjusting the twist of the weft yarn such that the absolute value of the difference between the twist count of the warp yarn and the weft yarn is in the range of 0.01 to 0.70 times / 25mm.

[26]

[0097] According to the glass cloth manufacturing method described in item 24 or 25, the warp warping process and / or the weaving process are performed using glass yarn with a value in the range of 10 to 30 obtained by dividing the width of the glass yarn by TEX.

[27]

[0099] A glass yarn roll having a core material and glass yarn wound around the core material.

[0100] The silicon (Si) content in the glass yarn, converted from silicon dioxide (SiO2), is 95.0~100% by mass, and the twist index of the glass yarn is below 400mm.

[28]

[0102] According to the glass yarn roll as described in Project 27, the twist index of the glass yarn is 70 mm or more.

[29]

[0104] According to item 27 or 28, the glass yarn rolls, wherein the glass yarn satisfies the ranges described in formulas (A), (B) and (C) below:

[0105] (A)x+y+z=100% mass

[0106] (B)x≥99.5% of mass

[0107] (C) 0.0003ppm ≤ y ≤ 0.50ppm

[0108] x: Silicon content when converted to silicon dioxide (SiO2)

[0109] y: Total content of uranium and thorium

[0110] z: Total content of elements other than silicon, uranium, and thorium.

[30]

[0112] According to any one of items 27 to 29, the glass yarn roll has an absolute value of 0.5 to 1.5 twists / 25mm.

[31]

[0114] According to item 27 or 28, the glass yarn roll is such that the width of the glass yarn divided by TEX is in the range of 10 to 30.

[32]

[0116] A type of glass yarn used in the weaving of glass cloth.

[0117] The silicon (Si) content in the glass yarn, converted from silicon dioxide (SiO2), is 95.0~100% by mass, and the twist index of the glass yarn is below 400mm.

[33]

[0119] According to the glass yarn described in Project 32, the twist index of the glass yarn is 70 mm or more.

[34]

[0121] According to item 32 or 33, the glass yarn satisfies the ranges described in formulas (A), (B) and (C) below:

[0122] (A)x+y+z=100% mass

[0123] (B)x≥99.5% of mass

[0124] (C) 0.0003ppm ≤ y ≤ 0.50ppm

[0125] x: Silicon content when converted to silicon dioxide (SiO2)

[0126] y: Total content of uranium and thorium

[0127] z: Total content of elements other than silicon, uranium, and thorium.

[35]

[0129] According to the glass yarn of Project 34, y, representing the total content of uranium and thorium, is in the range of 0.0003 to 0.0010 ppm.

[36]

[0131] According to the glass yarn of Project 34, y, which represents the total content of uranium and thorium, is in the range of more than 0.0010 and less than 0.0015 ppm.

[37]

[0133] According to the glass yarn of Project 34, y, which represents the total content of uranium and thorium, is in the range of more than 0.0015 and less than 0.0018 ppm.

[38]

[0135] According to the glass yarn of Project 34, y, which represents the total content of uranium and thorium, is in the range of more than 0.0018 and less than 0.0035 ppm.

[39]

[0137] According to the glass yarn of Project 34, y, which represents the total content of uranium and thorium, is in the range of more than 0.0035 and less than 0.0040 ppm.

[40]

[0139] According to the glass yarn of Project 34, y, which represents the total content of uranium and thorium, is in the range of more than 0.0040 and less than 0.09 ppm.

[41]

[0141] According to the glass yarn of Project 34, y, which represents the total content of uranium and thorium, is in the range of more than 0.09 and less than 0.12 ppm.

[42]

[0143] According to the glass yarn of Project 34, y, which represents the total content of uranium and thorium, is in the range of more than 0.12 and less than 0.50 ppm.

[43]

[0145] The glass yarn according to any one of items 32 to 42, wherein the twist index of the glass yarn is in the range of 330 to 400 mm.

[44]

[0147] The glass yarn according to any one of items 32 to 42, wherein the twist index of the glass yarn is in the range of 300 to 329 mm.

[45]

[0149] The glass yarn according to any one of items 32 to 42, wherein the twist index of the glass yarn is in the range of 220 to 299 mm.

[46]

[0151] The glass yarn according to any one of items 32 to 42, wherein the twist index of the glass yarn is in the range of 200 to 219 mm.

[47]

[0153] The glass yarn according to any one of items 32 to 42, wherein the twist index of the glass yarn is in the range of 125 to 199 mm.

[48]

[0155] The glass yarn according to any one of items 32 to 42, wherein the twist index of the glass yarn is in the range of 110 to 124 mm.

[49]

[0157] According to any one of items 32 to 42, the glass yarn has a twist index of 110 mm or less.

[0158] The effects of the invention

[0159] According to this disclosure, a glass cloth with excellent flatness and reduced fuzz generation frequency can be provided. Furthermore, according to this disclosure, a method for manufacturing the glass cloth, a glass yarn roll, and the glass yarn itself can be provided. Additionally, according to this disclosure, prepregs, printed circuit boards, integrated circuits, and electronic devices using the glass cloth can be provided. Attached Figure Description

[0160] Figure 1 This is a schematic diagram illustrating the method for determining warpage in this disclosure.

[0161] Figure 2 This is a schematic diagram illustrating the method for determining warpage in this disclosure. Detailed Implementation

[0162] Hereinafter, examples of embodiments of the present disclosure will be described. However, the present disclosure is not limited to the following embodiments, and various modifications can be made without departing from its spirit.

[0163] In this specification, when multiple structures represented by the same symbol exist in the same formula, each structure can be selected independently unless otherwise specified, and they can be the same or different. Similarly, when multiple structures represented by the same symbol exist in different formulas, each structure can be selected independently unless otherwise specified, and they can be the same or different. Furthermore, in this specification, the upper or lower limit of a numerical range described in a stage can be replaced with the upper or lower limit of a corresponding numerical range described in another stage, and further, with the corresponding value described in the embodiment. Additionally, in this specification, the term "process" is used not only when it is an independent process, but also when it cannot be clearly distinguished from other processes, as long as the function of the process can be achieved. In the accompanying drawings, for further clarity, the scale, shape, and length are sometimes exaggerated.

[0164] Glass cloth

[0165] <Overall Composition>

[0166] The glass cloth disclosed herein is a glass cloth composed of glass yarn, wherein the silicon (Si) content in the glass yarn is 95.0 to 100% by mass (converted to silicon dioxide (SiO2), and the twist index of the glass yarn is in the range of 400 mm or less.

[0167] In addition, the glass cloth disclosed herein is a glass cloth made of glass yarn, wherein the bulk dielectric loss tangent of the glass constituting the glass yarn is in the range of 0.001 or less at 10 GHz, and the kink index of the glass yarn is in the range of 400 mm or less.

[0168] The inventors have discovered two points in glass yarns that are advantageous for improving the dielectric properties of glass cloth, such as (1) and / or (2) below: residual stress is easily generated in the glass cloth obtained by using them, and such glass yarns tend to have a high kink index.

[0169] (1) The silicon (Si) content in the glass yarn, calculated as silicon dioxide (SiO2), is 95.0~100% by mass.

[0170] (2) The glass yarn in which the bulk dielectric loss tangent at 10 GHz is 0.001 or less. The inventors further clarified that the higher the kink index of the glass cloth, the more adverse the effect on the flatness (warping) of the glass cloth.

[0171] Here, snarl refers to the twisting that occurs in twisted yarn during untwisting. In this specification, a higher snarl index indicates a greater likelihood of snarl formation. It should be noted that in JIS-L-0210:1981, section 3.1, item 1113, snarl is defined as "the entanglement (knotting) of yarn formed due to twisting when the twisted yarn is relaxed." Regarding this point, there has been no previous research on the impact of the snarl index on the quality of glass cloth.

[0172] Furthermore, the inventors have clarified that for glass yarn wound around a core material (in one embodiment, a bobbin) (referred to herein as "glass yarn package"), the higher the twist index of the glass yarn, the easier it is for the glass yarn to rub against the surface of the bobbin while unwinding from the bobbin. As a result, the surface of the glass cloth obtained using this glass yarn is more prone to fuzzing. In particular, the inventors have also found that in the process of warping the glass yarn used as the warp yarn of the glass cloth (warp warping process), compared with the process of weaving using the glass yarn (weaving process), the unwinding speed of the glass yarn is slower, and therefore there is a tendency for the glass yarn to easily rub against the surface of the bobbin.

[0173] Therefore, the inventors conducted research from the viewpoint of reducing the twist index, and found that the twist index can be adjusted according to the spinning conditions of the glass yarn. In one preferred embodiment, the glass yarn can be made from a glass rod with a silicon content of 99.5% by mass or more. After heating and stretching the glass rod, annealing can be performed to reduce residual stress generated in the glass yarn (in one embodiment, eliminating residual stress). According to this disclosure, a glass cloth can be provided that uses glass yarn with a controlled twist index, thereby achieving improved flatness and a reduction in the frequency of hair generation.

[0174] The preferred unit area weight (mass of the glass cloth) is 8~250 g / m². 2 More preferably 8~100g / m 2 A further preferred value is 8~80g / m 2 The preferred concentration is 8~50g / m³. 2 When the weight per unit area of ​​the glass cloth is within the above-mentioned range, the effects of this disclosure are easily obtained.

[0175] The thickness of the glass cloth is preferably 60 μm or less, more preferably 55 μm or less, and even more preferably 50 μm or less. When the thickness of the glass cloth is within the above-mentioned range, the effects of this disclosure are easily obtained. The thickness of the glass cloth can be greater than 0, 5 μm or more, or 5 μm or more.

[0176] <Glassy yarn>

[0177] The twist index of glass yarn is in the range of 400 mm or less. When the yarn is twisted, an untwisting torque is generated that needs to be detwisted, at which point the yarn twists. Such twisting is referred to as "knot" in this specification. In addition, the twist index described in JIS L1095 can be used as an indicator of the ease with which this knot is generated.

[0178] It is known that glass fiber yarn, which is suitable for use in printed circuit boards, is obtained by extruding a substance made by melting glass in a melting furnace through a nozzle to obtain glass filaments with a diameter of several μm, and then processing the filaments.

[0179] On the other hand, quartz glass with a silicon (Si) content of 95.0 to 100% by mass (converted to silicon dioxide (SiO2)) has a very high melting point compared to other glasses. Therefore, the method of obtaining glass filaments as raw materials by heating and stretching a quartz glass rod (quartz glass ingot) differs from the aforementioned E-glass fiber yarn. When a quartz glass rod is heated and stretched, the siloxane bonds constituting the glass align along the stretching direction, and in this case, the resulting glass filaments are prone to residual stress.

[0180] The inventors have discovered that, due to residual stress, "twist," which was not previously considered a problem in glass fiber yarns, adversely affects the fuzz quality and flatness of glass cloth. Specifically, glass fiber yarns with a higher twist index are more likely to come into contact with the bobbin surface during warping of the glass cloth, resulting in more fuzz formation on the glass cloth surface. Furthermore, even when in the glass cloth state, glass fiber yarns with a high twist index exhibit stronger yarn undulation, thus easily negatively impacting the flatness (warping) of the glass cloth.

[0181] For "twist," which was not previously considered a problem in glass fiber yarns, from the viewpoint of further reducing the twist index of quartz glass fiber yarns, it is preferable to anneal the glass filament or glass yarn immediately after heating and stretching it. This method is relatively simple and also advantageous in providing glass cloth with excellent hairiness and flatness.

[0182] The inventors conducted research and found that by setting the twist index of the glass yarn to 400 mm or less, it is possible to reduce the frequency of fuzz generation on the glass cloth surface while performing warping. From the viewpoint of easily obtaining the effects of this disclosure, the twist index of the glass yarn is preferably 70 to 400 mm. From the viewpoint of suppressing fuzz on the glass surface, the upper limit of the twist index is preferably 380 mm or less, more preferably 370 mm or less, further preferably 350 mm or less, even more preferably 330 mm or less, particularly preferably 310 mm or less, and for example, it can be 300 mm or less, 250 mm or less, 200 mm or less, 150 mm or less, or 100 mm or less. The lower limit of the twist index, which can be arbitrarily combined with these upper limits, can be 70 mm or more, 100 mm or more, 150 mm or more, 200 mm or more, 250 mm or more, 300 mm or more, or 330 mm or more. For example, from the viewpoint of easily obtaining the effects of this disclosure, the twist index of the glass yarn is preferably in the range of 330-400 mm, 300-329 mm, or 220-299 mm. From the viewpoint of slightly valuing the surface hairiness of the glass cloth in addition to the productivity of the glass yarn, the range of 200-219 mm is preferred. From the viewpoint of valuing the surface hairiness of the glass cloth even more in addition to the productivity of the glass yarn, the range of 125-199 mm is preferred. From the viewpoint of further valuing the surface hairiness of the glass cloth in addition to the productivity of the glass yarn, the range of 110-124 mm is even more preferred. From the viewpoint of particularly valuing the surface hairiness of the glass cloth in addition to the productivity of the glass yarn, the range of 110 mm or less, for example, 70-110 mm or less, is particularly preferred.

[0183] From the viewpoint that it is easy to obtain the effect of reducing the kink index based on annealing treatment, the silicon (Si) content in the glass yarn, converted to silicon dioxide (SiO2), is preferably 99.5% by mass or more, more preferably 99.6% by mass or more, even more preferably 99.7% by mass or more, even more preferably 99.8% by mass or more, particularly preferably 99.9% by mass or more, and 99.95% by mass or more.

[0184] Glass cloth is obtained by weaving glass yarn (e.g., glass yarn formed from multiple glass filaments) as both warp and weft yarns. Examples of weaving structures for glass cloth include plain weave, square weave, satin weave, and twill weave, with plain weave being the preferred structure.

[0185] The warp and weft yarn weave density is preferably 10 to 120 yarns / inch (= 10 to 120 yarns / 25 mm), more preferably 40 to 100 yarns / inch. If the weave density is within the above range, the effects of this disclosure are easily obtained. The warp and weft yarn weave densities can be different from each other.

[0186] The glass yarn that makes up the glass cloth can be obtained by including so-called "low dielectric glass" in the raw materials.

[0187] The glass yarn preferably includes glass yarn that satisfies the ranges described in (A), (B) and (C), and more preferably glass yarn that satisfies the ranges described in (A), (B) and (C);

[0188] (A)x+y+z=100% mass

[0189] (B)x≥99.5% of mass

[0190] (C) 0.0003ppm ≤ y ≤ 0.50ppm

[0191] x: Silicon content when converted to silicon dioxide (SiO2)

[0192] y: Total content of uranium and thorium

[0193] z: Total content of elements other than silicon, uranium, and thorium.

[0194] By using glass yarn that satisfies the ranges described in (A), (B) and (C), for example, it is easy to achieve an improvement in the dielectric properties of the resulting glass cloth.

[0195] From the viewpoint of improving the dielectric properties of the obtained glass cloth, the range of x is preferably 99.6% by mass or more, more preferably 99.7% by mass or more, even more preferably 99.8% by mass or more, even more preferably 99.9% by mass or more, and particularly preferably 99.95% by mass or more.

[0196] The range of y is preferably the range described in (C) above, i.e., 0.0003ppm ≤ y ≤ 0.50ppm. Uranium (U) and thorium (Th) in glass yarn can cause memory malfunctions in electronic devices, therefore, a lower total content is preferred. The inventors conducted research and found that, although the mechanism of action is not necessarily clear, the total content of uranium and thorium has an effect on controlling the residual stress in the glass yarn and adjusting the kink index. Specifically, the inventors found that, as a phenomenon unique to glass yarn made from glass rods with a silicon content of 99.5% by mass or more, if the total content of uranium and thorium is 0.0003ppm or more, the residual stress in the glass yarn is easily reduced. Regarding this, the inventors also clarified that glass yarn with high residual stress has strong untwisting force, thus tending to have a high kink index; glass cloth made from such glass yarn is prone to warping and its flatness deteriorates.

[0197] From the above perspective, conventionally, the prevailing technical understanding is to keep the total content of uranium (U) and thorium (Th) as low as possible. In contrast, until now, there has been no practice of intentionally adjusting the total content of uranium and thorium within an appropriate range from the perspective of improving the flatness of the glass cloth. The inventors have conducted in-depth research and found that the higher the total content of uranium and thorium in the glass yarn, the easier it is to achieve the effect of annealing treatment for reducing the kink index in the glass yarn. From the viewpoint of easily obtaining the effects of the present disclosure, the range of y can be 0.0003ppm ≤ y ≤ 0.50ppm, the lower limit is preferably 0.001ppm or more, more preferably 0.003ppm or more, further preferably 0.005ppm or more, even more preferably 0.007ppm or more, and particularly preferably 0.01ppm or more. The upper limit of y, which can be arbitrarily combined with these lower limits, is preferably 0.45 ppm or less, more preferably 0.40 ppm or less, further preferably 0.35 ppm or less, even more preferably 0.30 ppm or less, and particularly preferably 0.25 ppm or less. If y is 0.0003 ppm or more, it is easy to avoid the situation where the residual stress generated during heating and stretching is high due to the excessive purity of silicon content in the glass. As a result, it is easy to control the kink index of the glass yarn to be below 400 mm. On the other hand, if y is 0.50 ppm or less, it is easy to avoid the situation where the malfunction of the memory in electronic devices containing glass yarn as a component is caused by the influence of uranium and thorium, for example, becoming a problem in use. In addition, from the viewpoint of easily improving the malfunction performance of the memory, y is preferably in the range of 0.0003 to 0.0010 ppm. From the viewpoint that, in addition to reducing the malfunction performance of the memory, it is also easy to reduce the kinking of the glass fiber, y is more preferably in the range of more than 0.0010 and less than 0.0015 ppm. From the viewpoint that, in addition to reducing the malfunction performance of the memory, it is also easy to further reduce the kinking of the glass fiber, y is more preferably in the range of more than 0.0015 and less than 0.0018 ppm. From the viewpoint that, in addition to reducing the malfunction performance of the memory, it is also easy to further reduce the kinking of the glass fiber, y is more preferably in the range of more than 0.0018 and less than 0.0035 ppm. From the viewpoint that, in addition to reducing the malfunction performance of the memory, it is also easy to reduce the kinking of the glass fiber and to facilitate the purification process of the quartz rod, y is more preferably in the range of more than 0.0035 and less than 0.0040 ppm. From the viewpoint that, in addition to reducing the malfunction performance of the memory, it is also easy to further reduce the kinking of the glass fiber and to facilitate the purification process of the quartz rod, y is particularly preferably in the range of more than 0.0040 and less than 0.09 ppm.

[0198] <Bulk dielectric loss tangent>

[0199] In this specification, the bulk dielectric loss tangent refers to the dielectric loss tangent measured at 10 GHz using a split cylindrical resonator for the raw material of the glass cloth. The raw material of the glass cloth can be, for example, glass type, glass filament, glass yarn, etc. The bulk dielectric loss tangent of the glass raw material constituting the glass cloth can be measured using the same method as that used to measure the dielectric loss tangent of the glass cloth for a glass plate with the same type and composition as the glass raw material and a thickness of 300 μm or less.

[0200] From the viewpoint of easily obtaining the effects of this disclosure, the bulk dielectric loss tangent at 10 GHz is preferably 0.0009 or less, more preferably 0.0008 or less, even more preferably 0.0007 or less, even more preferably 0.0005 or less, even more preferably 0.0004 or less, particularly preferably 0.0003 or less, and most preferably 0.0002 or less. The bulk dielectric loss tangent can exceed 0.

[0201] <Average fiber openness of glass cloth>

[0202] The average open fiber content of the glass cloth is preferably 38% or more, or more than 40%, more preferably more than 43%, even more preferably more than 46%, more than 50%, more than 53%, more than 56%, or more than 60%, and particularly preferably more than 65%. If the average open fiber content of the glass cloth is 38% or more, it is easier to suppress air bubbles, known as voids, remaining in the glass yarn bundles during the fabrication of prepregs or printed circuit boards containing them. This reduces the likelihood of adverse effects on solder heat resistance and insulation reliability. Furthermore, if the average open fiber content of the glass cloth is 38% or more, it is less susceptible to the effects of glass yarn twisting, thus ensuring the flatness of the glass cloth even when using glass yarn with a high twist index.

[0203] <Silane Coupling Agent>

[0204] The glass yarn (containing glass filaments) constituting the glass cloth is preferably surface-treated with a silane coupling agent. That is, in one embodiment, the surface treatment agent for the glass yarn contains a silane coupling agent.

[0205] As a silane coupling agent, it is preferred to include, for example, the silane coupling agent shown in the following formula (1).

[0206] X(R) 3-n SiY n …(1)

[0207] {In formula (1), X is an organic functional group having at least one of an amino group and an unsaturated double bond group, wherein the unsaturated double bond group is free radical reactive, Y is independently an alkoxy group, n is an integer greater than or less than 1 and less than 3, and R is a group selected from the group consisting of methyl, ethyl and phenyl}

[0208] Previously, it was believed that the increase in the dielectric loss tangent of glass cloth was due to: (i) trace amounts of thermally oxidized deteriorated binder residues remaining in a state of physical adhesion to the surface of the glass fiber yarn; and (ii) residues or modifications of surface treatment agents that were physically adhered to the glass surface without forming chemical bonds and could not be reduced by water washing. From the viewpoint of suppressing the generation of the aforementioned (i) thermally oxidized deteriorated binder and / or (ii) residues or modifications, X in formula (1) is preferably an organic functional group that does not form a salt with ionic compounds. Furthermore, from the viewpoint of reactivity with the matrix resin, X in formula (1) is more preferably an organic functional group having a methacryloyloxy group and / or an acryloxy group. From the viewpoint of easily obtaining the effects of this disclosure, X in formula (1) preferably does not contain amines such as primary amines, secondary amines, and tertiary amines, and preferably does not contain ammonium cations such as quaternary ammonium cations.

[0209] Regarding Y in the above formula (1), from the viewpoint of stabilizing the glass cloth, an alkoxy group with 1 to 5 carbon atoms (1, 2, 3, 4 or 5 carbon atoms) is preferred.

[0210] As a surface treatment agent, the silane coupling agent shown in formula (1) can be used alone or in combination with two or more silane coupling agents different from X in formula (1). Furthermore, the silane coupling agent shown in formula (1) can be used, for example, in the form of vinyltrimethoxysilane, 3-methacryloyloxypropyltrimethoxysilane, acryloyloxypropyltrimethoxysilane, 3-acryloyloxypropyltrimethoxysilane, 5-hexenyltrimethoxysilane, or mixtures thereof.

[0211] The molecular weight of the silane coupling agent is preferably 100-600, more preferably 150-500, and even more preferably 200-450. Particularly preferred are the use of two or more silane coupling agents with different molecular weights. By treating glass yarn with two or more silane coupling agents with different molecular weights, the density of the treatment agent on the glass surface increases, thereby tending to further improve the reactivity with the matrix resin.

[0212] From the viewpoint of minimizing interference with resin reactivity, silane coupling agents are preferably nonionic. Among nonionic silane coupling agents, those having at least one group selected from the group consisting of vinyl, methacryloxy, and acryloyloxy groups are preferred, with those having methacryloxy and / or acryloyloxy groups being particularly preferred. By ensuring reactivity with the resin, the heat resistance and reliability of the printed circuit board are easily improved.

[0213] In one embodiment, in formula (1), X is an organic functional group having at least one of the aforementioned unsaturated double bond group and amino group. Therefore, not only is the embodiment where X has both the aforementioned unsaturated double bond group and amino group included, but also the embodiment where X has the aforementioned unsaturated double bond group but not the aforementioned amino group, and the embodiment where X does not have the aforementioned unsaturated double bond group but has the aforementioned amino group, included within the scope of formula (1). Wherein, X in formula (1) is preferably the aforementioned unsaturated double bond group, and preferably does not contain an amino group.

[0214] <Loss on Ignition Value of Glass Cloth>

[0215] From the viewpoint of reducing the dielectric loss tangent of the glass cloth, the loss on ignition value of the glass cloth is preferably 0.010% by mass or more and less than 0.180% by mass, more preferably 0.010% by mass or more and less than 0.174% by mass, more preferably 0.010% by mass or more and less than 0.150% by mass, and even more preferably 0.010% by mass or more and less than 0.130% by mass. If the loss on ignition value is less than 0.180% by mass, it does not form chemical bonds with the glass surface but physically adheres, thus easily avoiding the situation where a large amount of surface treatment agent residue and / or its modifiers are present on the surface of the glass cloth that cannot be reduced by water washing. As a result, it is easy to reduce the dielectric loss tangent of the glass cloth. If the loss on ignition value is 0.010% by mass or more, it is easy to achieve sufficient adhesion between the matrix resin and the glass cloth, thus easily ensuring its heat resistance and insulation reliability when manufacturing printed circuit boards.

[0216] <Yarn width / TEX value>

[0217] The "yarn width / TEX" value, obtained by dividing the width of the glass yarn by its TEX (tex per inch), is preferably in the range of 10 to 30. This value is more preferably in the range of 11 to 29, more preferably in the range of 12 to 28, even more preferably in the range of 13 to 27, and particularly preferably in the range of 14 to 26. Here, the "yarn width / TEX" value corresponds to a parameter representing the bundled nature of the glass yarn. In the warp warping process of glass cloth, if the bundled nature of the warp yarn is insufficient, the warp yarn is prone to pilling, thus easily leading to yarn breakage. Therefore, if the "yarn width / TEX" value is 30 or less, it is easy to ensure the bundled nature of the glass yarn, thus easily preventing the glass yarn from being cut during the warp warping process. When the "yarn width / TEX" value is 10 or more, the opening of the glass yarn in the next process is easy, thus easily preventing poor impregnation of the matrix resin during prepreg preparation.

[0218] <Average filament diameter>

[0219] The average filament diameter of the glass filaments constituting the glass yarn is preferably in the range of 2.5 to 10.0 μm, more preferably in the range of 2.5 to 9.0 μm, even more preferably in the range of 3.5 to 8.5 μm, even more preferably in the range of 3.5 to 8.0 μm, and particularly preferably in the range of 3.5 to 7.5 μm. If the filament diameter is 2.5 μm or more, it is easy to ensure the breaking strength of the filaments, thus easily preventing the formation of fuzz in the resulting glass cloth. When the filament diameter is 10.0 μm or less, it is easy to avoid an increase in the mass of the glass cloth, thus facilitating conveying or processing.

[0220] <Number of Twists>

[0221] The absolute value of the twist count of the glass yarn is preferably in the range of 0.5 to 1.5 twists / 25 mm. More preferably, it is in the range of 0.55 to 1.45 twists / 25 mm, even more preferably, it is in the range of 0.57 to 1.4 twists / 25 mm, and even more preferably, it is in the range of 0.59 to 1.3 twists / 25 mm. Particularly preferably, it is in the range of 0.60 to 1.2 twists / 25 mm. By adjusting the twist count of the glass yarn, the twist index of the glass yarn can be controlled. The larger the absolute value of the twist count, the easier it is to untwist the glass yarn, and therefore, it tends to exhibit a large twist index. If the absolute value of the twist count of the glass yarn is 0.5 twists / 25 mm or more, it is easy to ensure the bundled nature of the glass yarn, thus it is easy to prevent the cutting of the glass yarn during the warping process and to prevent the generation of fuzz on the surface of the glass cloth. If the absolute value of the twist count of the glass yarn is less than 1.5 times / 25mm, it is easy to prevent the twist index of the glass yarn from becoming too large. In this case, it is easy to avoid the glass yarn rubbing against the surface of the bobbin during unwinding, which can easily cause fuzz on the surface of the glass cloth.

[0222] The absolute value of the difference between the twist count of the warp and weft yarns is preferably in the range of 0.01 to 0.70 twists / 25 mm. When this absolute value difference is 0.01 twists / 25 mm or more, it is easy to improve the flatness of the glass cloth, and it is also easier to open the glass yarn during the manufacturing of the glass cloth. When this absolute value difference exceeds 0.7 twists / 25 mm, the directions of the untwisting forces of the warp and weft yarns are different (e.g., the warp is in the z-direction and the weft is in the s-direction), thus showing a tendency for the glass cloth to warp significantly. In addition, even if the untwisting force direction is the same, when the absolute value difference is large, the difference in untwisting force is also likely to increase, thus easily causing the glass cloth to warp. Therefore, when the absolute value difference is 0.7 twists / 25 mm or less, it is easier to suppress the generation of fuzz in the resulting glass cloth. The absolute value of the difference between the twist count of the warp and weft yarns of the glass cloth is more preferably in the range of 0.05 to 0.65 twists / 25 mm, and even more preferably in the range of 0.07 to 0.55 twists / 25 mm. Furthermore, the absolute value of the difference between the twist count of the warp and weft yarns of the glass cloth is more preferably in the range of 0.10 to 0.50 times / 25 mm, and even more preferably in the range of 0.15 to 0.45 times / 25 mm.

[0223] The twist direction of glass yarn is classified as z-direction or s-direction depending on the direction in which the twisting is performed. In this disclosure, twist in the z-direction is defined as "positive" and twist in the s-direction is defined as "negative". For example, in this specification, "twist count of 1.00z" is expressed as a twist count of 1.00, and "twist count of 1.00s" is expressed as a twist count of -1.00.

[0224] The twist count of the glass yarn can be adjusted, for example, during the twisting process (twisting process). In one method, the twist count of the glass yarn can be easily increased by bundling the glass filaments. Increasing the twist count of the glass yarn makes it easier to suppress the formation of fuzz caused by the breakage of the glass filaments, and also makes it easier to suppress yarn breakage caused by the warping process of the glass cloth. On the other hand, due to the twisting of the glass yarn, it is easy to hinder the expansion of the glass yarn, and also easy to produce uneven thickness of the glass cloth at the twisted part. Therefore, it is advantageous to find an appropriate twist count and use glass yarn adjusted to that twist count in the manufacture of high-quality glass cloth.

[0225] Glass gauze roll

[0226] In a preferred embodiment, this disclosure provides a glass yarn roll, which is formed by winding glass yarn around a core material. The silicon (Si) content in the glass yarn of the glass yarn roll is 95.0 to 100% by mass (equivalent to silicon dioxide (SiO2), and the twist index of the glass yarn is less than 400 mm. By using this glass yarn roll, it is possible to provide a glass cloth that achieves improved flatness and a reduced frequency of fuzz generation.

[0227] As preferred elements for glass yarn constituting glass yarn rolls, reference can be made to preferred elements for glass yarn constituting glass cloth.

[0228] For example, the glass yarn constituting the glass yarn roll preferably satisfies the ranges described in the following formulas (A), (B), and (C):

[0229] (A)x+y+z=100% mass

[0230] (B)x≥99.5% of mass

[0231] (C) 0.0003ppm ≤ y ≤ 0.50ppm

[0232] x: Silicon content when converted to silicon dioxide (SiO2)

[0233] y: Total content of uranium and thorium

[0234] z: The total content of elements other than silicon, uranium, and thorium. Furthermore, for glass yarn constituting a glass yarn roll, the absolute value of its twist count is preferably in the range of 0.5 to 1.5 twists / 25 mm, and the value of "yarn width / TEX" is preferably in the range of 10 to 30. It should be noted that the preferred numerical ranges for glass yarn constituting a glass yarn roll can also be referred to the preferred numerical ranges for glass yarn constituting a glass cloth.

[0235] The core material used for winding glass yarn only needs to allow for proper unwinding of the glass yarn from the core material; in one embodiment, it is a bobbin. However, the core material is not limited to a bobbin, as long as it has a function or structure equivalent to a bobbin.

[0236] Manufacturing methods for glass yarn, glass yarn rolls, and glass cloth

[0237] This disclosure provides, in preferred embodiments, various methods for manufacturing glass yarn, glass yarn rolls, and glass cloth. One aspect of this manufacturing method is a method for manufacturing the glass yarn, wherein the silicon (Si) content in the glass yarn, converted to silicon dioxide (SiO2), is 95.0 to 100% by mass, and the twist index of the glass yarn is 400 mm or less.

[0238] Another aspect of this manufacturing method is a method for manufacturing a glass yarn roll, which includes a step of winding the glass yarn around a core material and then forming a roll.

[0239] Another aspect of this manufacturing method is a method for manufacturing glass cloth, which includes a step of obtaining glass cloth using glass yarn, wherein the silicon (Si) content in the glass yarn, converted to silicon dioxide (SiO2), is in the range of 95.0 to 100% by mass, and the twist index of the glass yarn is in the range of 400 mm or less.

[0240] Another aspect of this manufacturing method is a method for manufacturing glass cloth, which includes a step of obtaining glass cloth using glass yarn, wherein the bulk dielectric loss tangent of the glass constituting the glass yarn is in the range of 0.001 or less at 10 GHz, and the kink index of the glass yarn is in the range of 400 mm or less.

[0241] The manufacturing methods described above in this disclosure may include: a process of manufacturing glass filaments by heating and stretching a glass rod (glass filament manufacturing process); and a process of bundling multiple glass filaments (glass filament bundling process).

[0242] <Making process of glass rod>

[0243] As a method for manufacturing the glass rod used to manufacture the glass cloth of this disclosure, known techniques can be utilized. The glass rod can be fused silica glass produced by methods such as electrofusion and flame melting, or synthetic quartz rod produced by methods such as sol-gel. In any manufacturing method, to adjust the silicon content in the glass yarn, it is preferable to purify the glass rod used as a raw material. Furthermore, to easily control the kink index of the glass yarn, it is preferable to purify the glass rod so that the total uranium and thorium content in the glass yarn is in the range of 0.0003 to 0.50 ppm. For example, in fused silica glass, it is advantageous to use raw material powder with low uranium and thorium content. By using a glass rod with a total uranium and thorium content within the above range, it is easier to reduce the tensile stress during processing of the glass filament, which in turn makes it easier to reduce the residual stress in the glass yarn, and consequently, to reduce the kink index of the glass yarn.

[0244] <Making Process of Glass Filaments>

[0245] In this process, glass filaments are manufactured by heating and stretching a glass rod. Known techniques can be used as methods for manufacturing and further processing the glass filaments. For example, a method of heating and stretching a glass rod can be employed. In one approach, a glass rod with a diameter of 1 to 50 mm can be heated and stretched in an electric furnace under an inactive atmosphere at a temperature of 2000°C to manufacture glass filaments with a diameter of 3 to 10 μm. The diameter of the glass filament can be controlled by adjusting the ratio of the speed at which the glass rod is fed into the furnace to the speed at which the glass filament is stretched. From the viewpoint of reducing stress during the stretching of the glass rod, the temperature during heating and stretching is preferably in the range of 1700 to 2500°C, more preferably in the range of 1800 to 2400°C, and even more preferably in the range of 1900 to 2300°C.

[0246] The inventors have discovered that stress generated during the heating and stretching of a glass rod can sometimes remain in the resulting glass yarn, and the higher the residual stress, the greater the kink index tends to be in the glass yarn. Furthermore, the inventors have clarified that reducing the residual stress in the glass yarn after stretching, for example by annealing, is effective in adjusting the kink index. Annealing transforms the microcrystalline structure oriented by stretching into a non-oriented state, thereby easily reducing the kink index of the glass yarn.

[0247] The annealing treatment is preferably performed between the steps of heating and stretching the glass rod and coating the glass yarn with a bundling agent. Furthermore, from the viewpoint of easily reducing residual stress in the glass yarn, the annealing temperature is preferably in the range of 1000~1900℃, more preferably in the range of 1100~1800℃, even more preferably in the range of 1200~1700℃, even more preferably in the range of 1300~1650℃, and particularly preferably in the range of 1400~1600℃. When the annealing temperature is below 1900℃, there is a tendency to easily prevent the glass filaments from cutting after heating and stretching. Additionally, when the annealing temperature is above 1100℃, it is easier to reduce residual stress in the glass yarn. Furthermore, the annealing time is preferably in the range of 0.1~30 seconds, more preferably in the range of 0.2~20 seconds, even more preferably in the range of 0.3~5 seconds, and particularly preferably in the range of 0.4~3 seconds.

[0248] <Glass filament bundling process>

[0249] In this process, multiple glass filaments are bundled together. The bundled glass filaments are typically referred to as "raw filaments," therefore this process can also be understood as a "method for producing glass raw filaments." Known techniques can be used to produce glass raw filaments.

[0250] In the production of glass filaments, a filament-coating agent is preferably applied to improve the bundled properties of the filaments and to protect their surface. Methods for applying the filament-coating agent include, for example, using a roller applicator.

[0251] As a slugging agent, resin-based slugging agents such as PVA, polyurethane, and epoxy resins, as well as starch-based slugging agents, are known. From the viewpoint of the scattering of glass yarn during the weaving process and the ease of removing the slugging agent from the glass yarn, starch-based slugging agents are preferred. To improve the functionality of the glass yarn, additives such as lubricants and antistatic agents can be added to the slugging agent. From the viewpoint of easily suppressing the twisting of the glass yarn, when bundling the glass filaments, it is preferable to adjust the yarn path and the shape of the heating and stretching furnace in a way that applies as uniform a tension as possible to each glass filament.

[0252] To adjust the "yarn width / TEX" value (obtained by dividing the glass yarn width by the glass yarn's TEX) to a range of 10 to 30, the amount of bundling agent can be adjusted during the glass filament bundling process. Here, from the viewpoint of easily achieving the effects of this disclosure, the loss on ignition (LOI) of the glass yarn is preferably in the range of 1.0 to 2.5% by mass, more preferably in the range of 1.1 to 2.4% by mass, even more preferably in the range of 1.2 to 2.3% by mass, and particularly preferably in the range of 1.3 to 2.2% by mass. When the loss on ignition of the glass yarn is 1.0% by mass or higher, it is easy to ensure the bundling properties of the glass filaments; in this case, it is easy to adjust the "yarn width / TEX" value to a range of 10 to 30. When the loss on ignition of the glass yarn is 2.5% by mass or lower, it is easy to prevent poor degreasing and insufficient fiber opening during the degreasing and fiber opening processes of the glass yarn.

[0253] <Twisting Process>

[0254] The method may include a process of twisting glass filaments in a prescribed manner (twisting process). For example, a twisting machine can be used to perform the prescribed twisting of the glass filaments. Known devices or methods can be utilized as the twisting machine or twisting method. For example, a method can be described where a roll of glass filaments coated with a binding agent (e.g., called a "collet") is pulled out and twisted to wind around a core material (in one case, a bobbin). In this case, a fixing clamp called a spindle is used to mount the bobbin to the twisting machine. The twisting machine typically has components called wire travelers around the spindle, and the number of twists applied to the glass filaments can be adjusted by the speed ratio of the movement of these various components.

[0255] The twisting process can also be used to wind the twisted glass filaments onto the core material. This allows for the production of glass yarn rolls.

[0256] <Method for manufacturing glass cloth>

[0257] The manufacturing method of glass cloth includes a process of weaving the above-mentioned glass yarn as warp and weft yarn to obtain glass cloth (weaving process).

[0258] Furthermore, the manufacturing method of glass cloth can include the following steps before the aforementioned weaving process: a warping process in which the warp yarns of the glass cloth are combined using glass yarn with a value in the range of 10 to 30 obtained by dividing the yarn width by the TEX of the glass yarn, and then coated with a bubbling agent; a heating and degreasing process (heating and degreasing process) of the glass yarn to remove the bubbling agent adhering to the glass yarn after the aforementioned warping process and before, during, or after the aforementioned weaving process; a process of coating the glass yarn with a surface treatment agent (surface treatment process); and a process of opening the glass yarn (opening process). By including these steps, glass cloth with excellent flatness and hairiness quality can be easily provided.

[0259] The aforementioned glass processing method (heating degreasing process, surface treatment process, and fiber opening process) can be applied to glass yarn before weaving, and also to woven glass cloth. In other words, the process of weaving glass yarn to obtain glass cloth can be set before, during, or after the glass processing method. It should be noted that in the glass processing method, "reduction" means, for example, removing at least a portion of the bundling agent or silane coupling agent, and there may be residues that are not completely removed. Hereinafter, an example is given that the process sequentially includes a warping process, a weaving process, a heating degreasing process, a surface treatment process, and a fiber opening process. However, this disclosure is not limited to the following example.

[0260] <Warping Process>

[0261] In the warping process, glass yarn with a Si content (converted to SiO2) ranging from 95.0% to 100% by mass can be used. After the warp yarns are combined, a sizing agent is applied to the glass yarn. By providing a sizing agent to the glass yarn, the formation of fuzz in the glass cloth is easily suppressed. As a sizing agent, starch and PVA, which have high sizing properties, are preferred. To ensure uniform application of the sizing agent to the glass yarn, it is preferable to impregnate the glass yarn with the sizing agent, remove excess sizing agent using a squeeze roller, and then dry the sizing agent.

[0262] <Weaving process>

[0263] In the weaving process, a loom can be used to weave the weft yarn into the warp yarn prepared in the warping process. Known looms include air-jet, rapier, and shuttle looms, but from the viewpoint of suppressing fuzz in the glass cloth, an air-jet loom is preferred.

[0264] The absolute value of the twist count of the glass yarn in the warp setting and weaving process is preferably in the range of 0.5 to 1.5 times / 25 mm. Furthermore, in this process, it is preferable to adjust the weft twist count so that the absolute value of the difference between the warp and weft twist counts is in the range of 0.01 to 0.70 times / 25 mm.

[0265] <Heating and oil removal process>

[0266] In the heat degreasing process of glass cloth, heating the glass yarn reduces the amount of any adhering sizing agent (coating agent) and its residues, as well as their modifiers, on the glass yarn, and preferably removes them. By performing the heat degreasing process, a surface treatment layer can be formed on the surface of the glass yarn (glass filament) while reducing organic matter that can increase the dielectric loss tangent, thus making it easier to produce glass cloth with excellent dielectric properties.

[0267] As a means of removing oil by heating, known means (heating means, heating medium, heating mechanism, heating device and heating component, etc.) can be used.

[0268] As a method of heating and degreasing, for example, there is a known method of heating glass cloth at a temperature of 600~1600℃.

[0269] In the heat treatment process, by heating the glass cloth blank, whose softening point is above 900°C, within a temperature range of 600~1600°C, damage to the glass cloth is easily suppressed, and the dielectric loss tangent of the glass cloth is easily reduced. From the viewpoint of appropriately obtaining the effects of this disclosure, the heat degreasing temperature is preferably 700~1500°C, more preferably 800~1400°C, even more preferably 900~1300°C, and particularly preferably 1000~1200°C. When the heat degreasing temperature is above 600°C, the slugging agent and the like adhering to the cloth can be removed effectively, thus making it easier to produce glass cloth with excellent dielectric properties. When the heat degreasing temperature is below 1600°C, devitrification of the glass is easily suppressed, and as a result, the strength of the glass cloth is easily prevented.

[0270] The heating time is preferably 30 minutes or less, more preferably 15 minutes or less, even more preferably 5 minutes or less, and particularly preferably 90 seconds or less. Since the heating treatment is performed at a high temperature, damage to the glass cloth is minimized when the heating time is 30 minutes or less. In this case, for example, problems such as localized openings in the glass cloth or cutting of the glass cloth during processing are easily avoided. From the viewpoint of effectively removing the slub, etc., the heating time can be, for example, 1 second or more, 5 seconds or more, 10 seconds or more, or 15 seconds or more.

[0271] In the case of heating and degreasing glass cloth using a closed system, from the viewpoint of achieving suitable heating using heating methods, it is preferable to place the glass cloth inside a heating furnace. Furthermore, from the viewpoint of maximizing storage space and heating range efficiency, it is preferable to heat the glass cloth while storing it in a rolled-up state. Moreover, from the viewpoint of improving the removal efficiency of organic matter and shortening the removal time of organic matter, it is preferable to heat the glass cloth while it is being conveyed within the heating furnace. The conveying of the glass cloth can, for example, be achieved through a combination of an unwinding mechanism and a winding mechanism.

[0272] In the case of heating and degreasing glass cloth in an open system, from the viewpoint of ensuring the heated area, it is preferable to heat the glass cloth while it is being fed. The glass cloth can be fed, for example, by a combination of an unwinding mechanism and a winding mechanism.

[0273] The heating degreasing process is not limited to the above-mentioned methods. As another method of heating degreasing, it is known to heat in a vacuum or a gas with a dew point below 15°C, where the heating amount expressed as a heating temperature (°C) of 100°C or higher × heating time (h) is 450 (°C·h) or higher (where the highest heating temperature is 100~600°C).

[0274] <Heating methods>

[0275] As heating methods, options include furnaces, electric heaters, and burners, with gas-fired single-radiant-tube burners or electric heaters being preferred. Multiple different heating methods can be combined.

[0276] From the viewpoint of efficiently removing organic matter adhering to the surface of the glass cloth, a continuous heating method is preferred over an intermittent method of heating the glass cloth wound around the core at a specified atmosphere temperature, in which the glass cloth is continuously passed through the heating furnace while being heated. Even more preferred is a method that uses cleaning water with low metal ion content, such as reverse osmosis (RO) water or ion-exchange water, to continuously clean the glass cloth.

[0277] In addition, from the perspective of low operating costs, as a heating method, the glass cloth can be heated by bringing a component heated to a specified temperature (contact component) into contact with the glass cloth.

[0278] The contact member is preferably capable of heating the glass cloth at high temperatures. The shape of the contact member is preferably a roller shape, considering the ease of conveying the glass cloth. Specifically, as a contact member, a roller that heats the glass cloth by induction heating and is suitable for use in high-temperature regions with minimal temperature deviation in the width direction is preferred. It is assumed that when the glass cloth is heated using the contact member, the temperature of the contact member is approximately equal to the surface temperature of the glass cloth.

[0279] When the glass cloth is continuously heated, in order to remove the carbides adhering to the roller, the roller is preferably equipped with a mechanism for removing the adhering foreign matter, such as a blade.

[0280] <Steam Application Methods>

[0281] The methods used to apply the above-mentioned vapor application methods to glass cloth can include spraying, spray diffusion, jet nozzles, etc. Alternatively, the gas discharged from the heating furnace can be reused as high-temperature steam.

[0282] The vapor used in glass cloth may include, for example, volatile solvents, water vapor, or gases other than water vapor. From the viewpoint of suppressing toxicity to humans and from the viewpoint of easily promoting the decomposition of the bridging agent used in glass fibers, water vapor is preferred. The temperature of the high-temperature vapor can be a temperature higher than 650°C for the surface temperature of the glass cloth. In this case, a method that can supply high-temperature vapor and heated air in any proportion can be used as needed. The temperature of the high-temperature vapor can be above 400°C, above 450°C, above 550°C, above 600°C, or above 650°C.

[0283] Surface treatment process

[0284] The surface treatment process can be applied to glass yarn, and also to glass cloth. In other words, the process of weaving glass yarn to obtain glass cloth can be set before, during, or after the glass treatment method disclosed herein.

[0285] The process of attaching the surface treatment agent can include, for example, at least one of the following steps: a covering step in which a treatment solution with a concentration of 0.1 to 0.5% by mass is used to attach the silane coupling agent to the surface of the glass, and a fixing step in which the silane coupling agent is fixed to the surface of the glass by heating and drying. Thus, the glass can be readily and appropriately surface-treated.

[0286] As a method for applying the treatment solution to glass in the coating process, it can be (a) immersing the glass in or passing it through a treatment solution stored in a tank (hereinafter referred to as "immersion method"), or (b) applying the treatment solution to the glass using a roller coater, die coater, or gravure coater. When using the immersion method, it is preferable to select an immersion time of 0.5 seconds or more and 1 minute or less in the treatment solution. Furthermore, when using the immersion method, the glass can be conveyed through the treatment solution at a speed of 10 to 50 m / min while being subjected to a specified tension (e.g., 100 to 250 N). After the treatment solution is applied to the glass, the solvent contained in the treatment solution can be heated and dried using methods such as hot air or electromagnetic waves.

[0287] The concentration of the treatment solution is preferably 0.1 to 0.5% by mass, more preferably 0.1 to 0.45% by mass, and even more preferably 0.1 to 0.4% by mass. This allows for easier and more appropriate surface treatment of the glass.

[0288] In the fixed process, to ensure sufficient reaction between the silane coupling agent and the glass, the heating and drying temperature is preferably 80°C or higher, more preferably 90°C or higher. Furthermore, to prevent the deterioration of the organic functional groups in the silane coupling agent, the heating and drying temperature is preferably 300°C or lower, more preferably 180°C or lower.

[0289] The process for reducing silane coupling agents can, for example, include at least one of the following steps: a cleaning step to remove silane coupling agents that have not formed chemical bonds with the glass surface; a drying step to heat and dry the cleaned glass; and a fine cleaning step to reduce unwanted components that have not formed chemical bonds with the glass surface and were not completely removed. This makes it easier to control the loss on ignition value. It should be noted that the process for reducing silane coupling agents can include, for example, a fine drying step after the fine cleaning step.

[0290] In the fine cleaning process, unwanted components that were not completely removed by water during the cleaning process and did not form chemical bonds with the glass surface can be reduced. In this fine cleaning process, for example, an organic solvent can be used as the cleaning fluid. By having a fine cleaning process, even when using low-dielectric glass as disclosed herein, it is easy to adjust the difference between the dielectric loss tangent of the obtained glass cloth and the dielectric loss tangent of the bulk phase to the numerical range described above. As the organic solvent used here, a highly hydrophobic organic solvent is preferred; furthermore, an organic solvent with high affinity for residues and modifiers of silane coupling agents with hydroxyl groups is also preferred. The cleaning method can be immersion, spraying, etc., and heating or cooling can be performed as needed. In order to suppress the re-adhesion of glass dissolved in the cleaning fluid, it is preferable to use a pressure roller or the like to reduce excess solvent from the cleaned glass.

[0291] Organic solvents that can be used as cleaning fluids in the fine cleaning process include, for example, the following solvents, used alone or in combination. Examples of highly hydrophobic organic solvents include saturated chain aliphatic hydrocarbons such as n-pentane, isopentane, n-hexane, isohexane, n-heptane, isoheptane, n-octane, isooctane, 2,2,4-trimethylpentane (isooctane), n-nonane, isononane, n-decane, isodecanane, and 2,2,4,6,6-pentamethylheptane (isododecane); saturated cyclic aliphatic hydrocarbons such as cyclopentane, cyclohexane, methylcyclohexane, dimethylcyclohexane, and ethylcyclohexane; aromatic hydrocarbons such as benzene, toluene, xylene, ethylbenzene, diethylbenzene, trimethylbenzene, and triethylbenzene; and halogenated solvents such as chloroform, dichloromethane, and dichloroethane. Examples of organic solvents with high affinity for residues or modifiers of silane coupling agents include alcohols such as methanol, ethanol, and butanol; ketones such as acetone and methyl ethyl ketone; ethers such as methyl ethyl ether and diethyl ether; amides such as N,N-dimethylformamide and N,N-dimethylacetamide; and dimethyl sulfoxide. From the viewpoint of easily and efficiently reducing the physical adhesion of silane coupling agents to glass, aromatic hydrocarbons, alcohols, or ketones are preferred, and methanol is more preferred. Therefore, as the cleaning fluid in the fine cleaning process, a cleaning fluid with methanol as the main component (50% or more, or 60% or more, relative to 100% by mass of the cleaning fluid) is preferred.

[0292] In the fine drying process, the amount of cleaning fluid used in the aforementioned fine cleaning process can be reduced. From the perspective of ease of reducing the amount of cleaning fluid through drying, the boiling point of the cleaning fluid used in the aforementioned fine cleaning process is preferably below 120°C. Drying can be performed by heating or by blowing air. It should be noted that, when using an organic solvent as the cleaning fluid, from a safety point of view, heating drying using hot air with low-pressure steam or thermal oil as the heat source is preferred. The drying temperature is preferably above the boiling point of the cleaning fluid, and from the viewpoint of suppressing the deterioration of the silane coupling agent, it is preferably below 180°C.

[0293] <Fiber Opening Process>

[0294] As a fiber-opening process, methods such as using water spray (high-pressure water fiber opening), vibrating washing machines, ultrasonic water, or cloth rolling machines can be employed to open the fiber of the glass cloth. During this fiber-opening process, by reducing the tension applied to the glass cloth, there is a tendency to further reduce air permeability. It should be noted that, in order to suppress the decrease in tensile strength of the glass cloth caused by the fiber-opening process, it is preferable to implement countermeasures such as reducing friction between the glass yarn and the contact components, optimizing the sizing agent, and increasing adhesion. As a fiber-opening method for glass cloth composed of glass yarn with high glass hardness, dry ice blasting is preferred.

[0295] The above-mentioned processes do not necessarily need to be performed in other processes; multiple processes can be combined into one. For example, if a cleaning process is performed after the weaving process, the cleaning process can also serve as a fiber-opening process by using high-pressure water spray. The composition of the glass cloth usually remains unchanged before and after fiber opening. Furthermore, the manufacturing method of glass cloth can include any processes other than those described above. For example, a slitting process can be performed after the fiber opening process. Additionally, the order of the above-mentioned processes can be changed if possible.

[0296] <Prepreg>

[0297] The prepreg disclosed herein contains the aforementioned glass cloth and a matrix resin impregnated in the aforementioned glass cloth. Therefore, a prepreg with fewer voids can be provided.

[0298] Thermosetting or thermoplastic resins can be used as the base resin. If possible, a combination of both can be used, and other resins may also be included.

[0299] Examples of thermosetting resins include:

[0300] (a) An epoxy resin formed by reacting and curing a compound having an epoxy group with a compound having at least one group selected from the group consisting of amino, phenol, acid anhydride, hydrazide, isocyanate, cyanate and hydroxyl groups that react with the epoxy group.

[0301] (b) A free radical polymeric cured resin formed by curing a compound having at least one group selected from the group consisting of allyl, methacryl, and acryloyl;

[0302] (c) Maleimide triazine resin formed by reacting a compound having a cyanate ester group with a compound having a maleimide group and then curing it;

[0303] (d) A thermosetting polyimide resin formed by reacting maleimide compounds with amine compounds and then curing them;

[0304] (e) Benzoxazine resin formed by crosslinking and curing a compound having a benzoxazine ring through heating polymerization;

[0305] It should be noted that, in obtaining (a) epoxy resin, the compound can be reacted without a catalyst. Alternatively, catalysts with reaction catalytic ability, such as imidazole compounds, tertiary amine compounds, urea compounds, and phosphorus compounds, can be added to induce the reaction. Furthermore, in obtaining (b) free radical polymerization type cured resin, thermally decomposable catalysts or photodecomposable catalysts can be used as reaction initiators.

[0306] Examples of thermoplastic resins include polyphenylene ether, modified polyphenylene ether, polyphenylene sulfide, polysulfone, polyethersulfone, polyarylate, aromatic polyamide, polyetheretherketone, thermoplastic polyimide, insoluble polyimide, polyamide-imide, and fluoropolymers. For use as an insulating material in printed circuit boards for high-speed communication, polyphenylene ether or modified polyphenylene ether with high free radical reactivity is preferred.

[0307] When the matrix resin used in printed circuit boards for high-speed communication has vinyl or methacryloyl groups, silane coupling agents with high hydrophobicity and functional groups such as methacryloyl groups that participate in free radical reactions have good compatibility with the matrix resin.

[0308] As mentioned above, thermosetting resins and thermoplastic resins can be used in combination. Furthermore, the prepreg may contain inorganic fillers. Inorganic fillers are preferably used in combination with thermosetting resins, and examples include aluminum hydroxide, zirconium oxide, calcium carbonate, alumina, mica, aluminum carbonate, magnesium silicate, aluminum silicate, silica, talc, short glass fibers, aluminum borate, and silicon carbide. Inorganic fillers can be used alone or in combination of two or more.

[0309] Printed Circuit Boards

[0310] The printed circuit board disclosed herein contains the aforementioned prepreg. Therefore, a printed circuit board with excellent insulation reliability can be provided.

[0311] Integrated Circuits and Electronic Devices

[0312] Furthermore, integrated circuits and electronic devices incorporating the aforementioned printed circuit boards are also embodiments of this disclosure. Integrated circuits and electronic devices obtained using the printed circuit boards of this disclosure exhibit excellent characteristics.

[0313] Example

[0314] Hereinafter, examples and comparative examples are given to illustrate embodiments of the present disclosure. However, the present disclosure is not limited to the following examples. Regarding the examples and comparative examples, various manufacturing, measurement, and evaluation processes are performed using the following methods. It should be noted that, unless otherwise specified, all manufacturing, measurement, and evaluation processes are performed at room temperature (25°C) and atmospheric pressure.

[0315] Measurement

[0316] <Thickness of the glass cloth (μm)>

[0317] According to JIS R 3420, section 7.10, determine the thickness of the glass cloth. Specifically, using a micrometer, gently rotate the spindle until it is parallel to the measurement surface of the sample and lightly contacts it. Then, read the scale after the ratchet clicks three times.

[0318] It should be noted that section 7.10 of JIS R 3420 specifies the general test methods for fabric products such as glass cloth.

[0319] <Twist index of glass yarn (mm)>

[0320] According to JIS L 1095, 9.17, the kink index of the glass yarn was determined. Specifically, firstly, with the initial load described in Method A of JIS L 1095, 9.17.1, applied to the glass yarn (sample), the glass yarn was stretched in a straight manner relative to the clamps, and then a 1.1 × 10⁻⁶ ohmmeter was placed at its center. -6 A load of N / tex is applied. One clamp B is brought close to another clamp A at a speed of 0.5 m / min to relax the sample. The scale reading of the position of clamp B at the load point where kinking occurs is recorded. The test is repeated 30 times, and the average value is calculated to determine the kink index.

[0321] <TEX (g / 1000m) of glass yarn>

[0322] According to JIS R3420 2012, the TEX of the glass yarn was determined. Specifically, glass yarn samples taken in 1000m lengths were subjected to a heat degreasing treatment in a muffle furnace set at 625±20℃ for 30 minutes to remove the binding agent adhering to the glass yarn. The removal of the binding agent was determined by whether the weight reduction of the glass yarn before and after the heat degreasing was less than 0.1% by mass. That is, if the weight reduction of the glass yarn before and after the heat degreasing was less than 0.1% by mass, the binding agent was considered to have been removed. The TEX of the glass yarn was determined by measuring the weight of the 1000m length of glass yarn after the heat degreasing treatment.

[0323] <Content of various elements contained in glass yarn>

[0324] The contents of silicon, uranium, and thorium in the glass fiber were determined using the absolute standard curve method with an ICP mass spectrometer.

[0325] <Silicon content (mass %)>

[0326] To reduce impurities (such as sizing agents) adhering to glass yarn or its raw materials, a volume-fixing solution is prepared using the following method: The glass yarn (sample) is weighed, then hydrolyzed with sodium hydroxide, and finally dissolved in dilute nitric acid to prepare the volume-fixing solution.

[0327] The silicon content of the obtained diluted solution was determined using an ICP emission spectrometer (Hitachi High-Tech Science PS3520VDDII), and then converted to an oxide value to calculate the silicon content in the sample.

[0328] <Uranium and thorium content (ppm)>

[0329] The weighed glass gauze (sample) was washed with aqua regia under heating, and then rinsed with ultrapure water. The sample was then decomposed with nitric acid, hydrofluoric acid, and sulfuric acid, and then heated and concentrated until sulfuric acid fumes were produced. Finally, a solution was prepared to volume using dilute nitric acid.

[0330] The obtained diluted solution was analyzed using an ICP mass spectrometer (SPQ9400, manufactured by SII NanoTechnology) to determine the uranium and thorium content in the sample.

[0331] <Content of other ingredients (mass %)>

[0332] Subtract the values ​​of silicon, uranium, and thorium from 100% by mass to determine the content of other components (elements other than silicon, uranium, and thorium) in the glass fiber (sample). Other components are referred to as "impurities" in the table below.

[0333] Here, the unit "ppm" used to express the content of uranium and thorium is converted according to the formula 1ppm = 0.0001% by mass.

[0334] <Twist count of glass yarn and its absolute difference (twists / 25mm)>

[0335] The twist count (twists / 25mm) of the glass yarn was determined according to JIS R3420. To accurately measure the twist count of the glass yarn in the glass cloth, a piece of glass yarn (warp or weft) was extracted from the glass cloth, and then the twist count was measured. For the obtained value, the twist in the z-direction was considered positive, and the twist in the s-direction was considered negative. For example, a twist of 1.00z (1.00 twists / 25mm in the z-direction) was treated as +1.00, and a twist of 1.00s (1.00 twists / 25mm in the s-direction) was treated as -1.00.

[0336] Then, calculate the absolute difference in twist count between the warp and weft yarns (times / 25mm) using the following formula.

[0337] The absolute difference in twist count = |warp twist count - weft twist count|

[0338] <Width of glass yarn (μm)>

[0339] While feeding glass yarn at a speed of 1 m / min, the yarn bundle width was measured over a 50 m length using a transmission-type dimension measuring instrument with LED projection (HIGH ACCURACY CMOS MICROMETER LS-9006MR / KEYENCE). Based on the yarn bundle width data obtained over the 50 m length, the proportion of yarn bundles with widths below a specific length and the average yarn bundle width were calculated. The yarn bundle width measurement using the transmission-type dimension measuring instrument with LED projection was performed with 1934 measurement points per m. In cases where errors occurred due to LED focusing issues (displaying a value of -9999), the measurement value was deleted, and the average glass yarn width was calculated. Furthermore, measurement values ​​that caused errors were appropriately omitted during the calculation. It should be noted that the tension acting on the glass yarn during feeding, measured using a tension meter (SCHMIDT Conrol instruments ETPB-100-C0585), was 0.12~0.18 N.

[0340] <Yarn width / TEX(μm / (g / 1000m))>

[0341] Divide the yarn width obtained above by the TEX obtained above to obtain the yarn width / TEX value.

[0342] <Bulk dielectric loss tangent at 10GHz>

[0343] According to IEC 62562, the bulk dielectric loss tangent at 10 GHz was determined for each glass rod (bulk phase) used as the raw material for each glass yarn. Specifically, glass plate samples smaller than 300 μm, taken at the size required for the measurement of the split cylindrical resonator, were stored for 8 hours in a constant temperature and humidity oven at 23°C and 50% RH. Then, the dielectric properties of the stored samples were measured using a split cylindrical resonator (EM Labo) and an impedance analyzer (Agilent Technologies). Five measurements were performed on each sample, and the average value was calculated. It should be noted that IEC 62562 primarily specifies the method for determining the dielectric properties of fine ceramic materials used in microwave circuits in the microwave frequency band.

[0344] <Number of warp and weft filaments and filament diameter (μm)>

[0345] When calculating the average fiber opening, the number of filaments and the diameter of each filament in the warp and weft yarns are determined by observing cross-sectional images of the glass yarn. Specifically, a cross-sectional image of the glass yarn used as the warp (or weft) is obtained, and the number of filaments and the diameter of the filaments in that warp (or weft) are measured in the cross-sectional image. Similarly, the acquisition of the glass yarn image and the measurement of the number of filaments are repeated, and the average of the five measurements is used as the number of filaments and the diameter of the warp (or weft).

[0346] <Warp yarn width and weft yarn width>

[0347] When calculating the average fiber opening, the warp and weft yarn widths are determined using the following method. First, five samples of glass cloth, each 70 mm in the warp direction and 70 mm in the weft direction, are cut from the glass cloth. The cut samples are then observed vertically at 100x magnification using a microscope. For each sample, the width of 250 warp (or weft) yarns is randomly measured, and the average width of these 250 yarns is calculated. This average value is then used as the warp (or weft) yarn width.

[0348] <Fiber opening degree (%) of warp and weft yarns and average fiber opening degree (%) of glass cloth>

[0349] The open fiber density of the warp yarns of glass cloth is calculated using the following formula.

[0350] Warp yarn openness (%) = [warp yarn width (μm) / {number of warp filaments × warp filament diameter (μm)}] × 100

[0351] In addition, the open fiber density of the weft yarn of the glass cloth is calculated using the following formula.

[0352] Weft yarn openness (%) = [Weft yarn width (μm) / {number of weft filaments × weft filament diameter (μm)}] × 100

[0353] The average openness is calculated using the calculated warp openness (%) and weft openness (%).

[0354] Average fiber opening degree (%) = {fiber opening degree of warp yarn (%) + fiber opening degree of weft yarn (%)} / 2

[0355] <Feather quality>

[0356] For the glass cloth obtained in the examples and comparative examples, a roll-to-roll inspection table was used, a tension of 100 N / 1000 mm was applied, and halogen lamps were used for illumination. Simultaneously, the number of hairs, especially protrusions larger than 1 mm, was visually determined. Each 1 m... 2 The number of feathers was used as the frequency of feathers, and then the quality of feathers was evaluated according to the following criteria.

[0357] (Measurement Standard)

[0358] Feather quality A: Feather frequency is 10 feathers / m 2 the following.

[0359] Feather quality B: Feather frequency is 11~20 feathers / m 2 .

[0360] Feather quality C: Feather frequency is 21 feathers / m 2 above.

[0361] <Warp of glass cloth>

[0362] The glass cloth obtained in the examples and comparative examples was cut into 200mm × 200mm pieces to obtain samples. The samples were placed on a flat measuring stage, and the warpage of the glass cloth was then measured.

[0363] Figure 1 Figures (a) to (b) are schematic diagrams illustrating the method for determining the warpage of glass cloth. Among them, Figure 1 (a) schematically shows a top view of the glass cloth and the mounting platform as seen from above. Figure 1 (b) schematically shows the view with the left end becoming the front-interior. Figure 1 A cross-sectional view of the left end portion of the glass cloth in (a) (the portion enclosed by dashed line A). Figure 1 In (a)~(b), the x-direction, y-direction and z-direction correspond respectively.

[0364] As shown in the figure, sample 2 of glass cloth is placed on a flat measuring stage 1. Sample 2 is bent at its left end so as to stand upright from the measuring stage 1, thereby only floating a height T1. At this time, the height T1 is treated as the amount of warping at the left end of the glass cloth.

[0365] Then, with Figure 1 Similarly, the examples shown in (a) to (b) will...

[0366] The height T2 at the upper part of the glass cloth

[0367] The height T3 at the right end of the glass cloth, and

[0368] The height T4 at the lower end of the glass cloth

[0369] The warping is treated as the amount of warping at the top, right, and bottom of the glass cloth, respectively.

[0370] The warp value Tmax, which is the maximum value among the warp values ​​at the four ends of the glass cloth, is represented as "warp value" in the table below.

[0371] Figure 2 (a) to (b) are schematic diagrams used to further illustrate the method for measuring warp. Figure 2 (a)~(b) and Figure 1 The section enclosed by the dashed line A in (a) corresponds to the cross section.

[0372] in, Figure 2 In (a), the sample is curled at the left end. In this case, the height Ta of the curled vertex portion is treated as the amount of warpage at the left end of the glass cloth.

[0373] in addition, Figure 2 In (b), the sample is bent into a mountain shape at the left end. In this case, the height Tb of the apex of the mountain is also treated as the amount of warpage at the left end of the glass cloth.

[0374] <Preparation of Prepreg Samples>

[0375] 45 parts by weight of polyphenylene ether (manufactured by SABIC, Noryl SA9000), 10 parts by weight of triallyl isocyanurate, 45 parts by weight of toluene, and 0.6 parts by weight of 1,3-di(tert-butylisopropylbenzene) were added to a stainless steel container and stirred at room temperature for 1 hour to prepare a varnish.

[0376] After impregnating the prepared varnish into the glass cloth obtained in the examples and comparative examples, the varnish was dried at 115°C for 1 minute. This yielded samples of the prepreg.

[0377] <Misoperation Performance Test>

[0378] The two prepreg sheets obtained above are sandwiched between two copper foils with a thickness of 18 μm. Then, they are subjected to a temperature of 200°C and a pressure of 40 kg / cm². 2 The substrate was solidified by heating and pressurizing for 2 hours. A copper wiring pattern with an L / S (linewidth / spacing) of 10 μm was then fabricated on the substrate, and 30 DRAMs were mounted in connection with this wiring pattern. The substrate with the DRAMs was continuously driven at 150°C and 10 GHz for 1000 hours. Based on these results, the malfunction performance based on the uranium and thorium contained in the glass fiber was evaluated.

[0379] (Evaluation Criteria)

[0380] A: There were 0 DRAM malfunctions.

[0381] B: There are 1 to 2 DRAM malfunctions.

[0382] C: There are 3 to 4 malfunctions in DRAM.

[0383] D: The number of DRAM malfunctions is 5 to 6.

[0384] E: The number of DRAM malfunctions is 7 to 8.

[0385] F: There are 9 DRAM malfunctions.

[0386] G: The number of DRAM malfunctions is more than 10.

[0387] Examples and Comparative Examples

[0388] <Manufacturing of Glass Yarn 1 and its Rolls>

[0389] Glass yarn was manufactured using a quartz glass rod (1 mm in diameter) with a silicon content of 99.92% by mass and a total uranium and thorium content of 0.103 ppm. The quartz glass rod was fed into a furnace filled with sufficient argon gas at a set temperature of 1970°C and then heated and stretched to produce glass yarn with a diameter of 5.0 μm and 50 filaments. It should be noted that each glass filament after heating and stretching was passed through a furnace at a set temperature of 1500°C for 1 second to reduce residual stress (annealing). The annealed glass filaments were then bundled together, and a binding agent using starch as the main agent was applied to bind them together before winding them onto a spool to obtain a glass filament bundle (glass precursor). Using a twisting machine, the obtained filament bundle was twisted in the z-direction at intervals of 0.8 times / 25 mm, and then wound onto a bobbin to obtain glass yarn 1 and its package.

[0390] <Manufacturing of Glass Yarn 2 and its Rolls>

[0391] Using a quartz glass rod (diameter = 1 mm) with a silicon content of 99.98% by mass and a total uranium and thorium content of 0.0036 ppm, glass yarn 2 and its rolls were obtained by the same method as glass yarn 1.

[0392] <Manufacturing of Glass Yarn 3 and its Rolls>

[0393] Using a quartz glass rod (diameter = 1 mm) with a silicon content of 99.90% by mass and a total uranium and thorium content of 0.204 ppm, glass yarn 3 and its rolls were obtained by the same method as glass yarn 1.

[0394] <Manufacturing of Glass Yarn 4 and its Rolls>

[0395] Using a quartz glass rod (diameter = 1 mm) with a silicon content of 99.85% by mass and a total uranium and thorium content of 0.389 ppm, glass yarn 4 and its rolls were obtained by the same method as glass yarn 1.

[0396] <Manufacturing of Glass Yarn 5 and its Rolls>

[0397] The glass rod was heated and stretched to have 200 filaments. Otherwise, glass yarn 5 and its roll were obtained by the same method as in Example 1.

[0398] <Manufacturing of Glass Yarn 6 and its Rolls>

[0399] The glass rod was heated and stretched to have 200 filaments. Otherwise, glass yarn 6 and its rolls were obtained by the same method as in Example 2.

[0400] <Manufacturing of Glass Yarn 7 and its Rolls>

[0401] Twisting was performed in the z-direction at intervals of 0.4 times / 25 mm. Otherwise, glass yarn 7 and its rolls were obtained by the same method as in Example 1.

[0402] <Manufacturing of Glass Yarn 8 and its Rolls>

[0403] The annealing temperature for the glass filaments was set to 1200°C. Otherwise, glass yarn 8 and its rolls were obtained by the same method as in Example 1.

[0404] <Manufacturing of Glass Yarn 9 and its Rolls>

[0405] The annealing temperature for the glass filaments was set to 1200°C. Otherwise, glass yarn 9 and its rolls were obtained by the same method as in Example 2.

[0406] <Manufacturing of Glass Yarn 10 and its Rolls>

[0407] The glass filaments were not annealed. Otherwise, the glass yarn 10 and its rolls were obtained by the same method as in Example 1.

[0408] <Manufacturing of Glass Yarn 11 and its Rolls>

[0409] Using a quartz glass rod (diameter = 1 mm) with a silicon content of 99.70% by mass and a total uranium and thorium content of 0.561 ppm, glass yarn 11 and its rolls were obtained by the same method as glass yarn 1.

[0410] <Manufacturing of Glass Wool 12>

[0411] The glass filaments were annealed at 2000°C, and otherwise processed using the same method as in Example 1. However, several glass filaments were cut during the annealing process, so glass yarn and its rolls could not be obtained.

[0412] <Manufacturing of Glass Yarn 13 and its Rolls>

[0413] Using a quartz glass rod (diameter = 1 mm) with a silicon content of 99.99% by mass and a total uranium and thorium content of 0.0017 ppm, glass yarn 13 and its rolls were obtained by the same method as glass yarn 1.

[0414] <Manufacturing of Glass Yarn 14 and its Rolls>

[0415] Using a quartz glass rod (diameter = 1 mm) with a silicon content of 99.91% by mass and a total uranium and thorium content of 0.09 ppm, glass yarn 14 and its rolls were obtained by the same method as glass yarn 1.

[0416] <Manufacturing of Glass Yarn 15 and its Rolls>

[0417] Using a quartz glass rod (diameter = 1 mm) with a silicon content of 99.99% by mass and a total uranium and thorium content of 0.0006 ppm, glass yarn 15 and its rolls were obtained by the same method as glass yarn 1.

[0418] <Manufacturing of Glass Yarn 16 and its Rolls>

[0419] Using a quartz glass rod (diameter = 1 mm) with a silicon content of 99.99% by mass and a total uranium and thorium content of 0.0010 ppm, glass yarn 16 and its rolls were obtained by the same method as glass yarn 1.

[0420] <Manufacturing of Glass Yarn 17 and its Rolls>

[0421] Using a quartz glass rod (diameter = 1 mm) with a silicon content of 99.98% by mass and a total uranium and thorium content of 0.0022 ppm, glass yarn 17 and its rolls were obtained by the same method as glass yarn 1.

[0422] <Manufacturing of Glass Yarn 18 and its Rolls>

[0423] Using a quartz glass rod (diameter = 1 mm) with a silicon content of 99.93% by mass and a total uranium and thorium content of 0.03 ppm, glass yarn 18 and its rolls were obtained by the same method as glass yarn 1.

[0424] <Example 1>

[0425] Glass yarn 1 was used as both warp and weft. In the warp winding process, the warp yarns were bundled at a linear speed of 60 m / min, and then a loom warp beam was prepared using a PVA-based sizing agent for two sizing treatments. Then, using an air-jet loom, a plain weave glass cloth fabric with a fabric density of 66 warp ends / 25 mm and 68 weft ends / 25 mm, and a width of 1300 mm, was woven. It should be noted that during the weaving process, the weft twist could be adjusted according to the loom conditions; therefore, the main nozzle pressure and secondary nozzle angle of the loom were adjusted to make the weft twist in the z-direction 0.6 times / 25 mm.

[0426] The obtained glass cloth blank is washed with deionized water and then dried. This removes alkali metal ions and other contaminants adhering to the cloth surface. Then, it is heated at 1000°C for 15 seconds for degreasing (heating degreasing process).

[0427] Next, a treatment solution was prepared by dispersing 0.3% by mass of 3-methacryloyloxypropyltrimethoxysilane (silane coupling agent A) and Z6030 (manufactured by Dow Toray) in pure water adjusted to pH=3 with acetic acid. The fabric was immersed in the treatment solution at a linear tension of 100 N and a linear speed of 15 m / min (surface treatment step). After squeezing the treatment solution out of the fabric, it was heated and dried at 130°C for 60 seconds to fix the silane coupling agent (fixation step).

[0428] The dried fabric was irradiated in water at a frequency of 25 kHz with an output power of 0.50 W / cm². 2 The fabric is then subjected to ultrasonic treatment. Next, a jet of water sprayed from a 1.4 MPa high-pressure water sprayer is used to reduce excess silane coupling agent physically adhering to the fabric, while simultaneously performing a fiber-opening process (fiber-opening step). Finally, the fabric is dried at 130°C for 1 minute (drying step).

[0429] Through the above operations, the glass cloth of Example 1 is obtained.

[0430] <Examples 2-16 and Comparative Example 1>

[0431] The items listed in the table below are changed as shown below. Otherwise, the glass cloth is obtained by the same method as in Example 1.

[0432] For the embodiments and comparative examples, the manufacturing conditions and evaluation results are shown in the table below. It should be noted that the glass cloth used in the embodiments can be used to manufacture prepregs, printed circuit boards, integrated circuits, and electronic devices using conventional methods.

[0433] [Table 1]

[0434]

[0435] [Table 2]

[0436]

[0437] [Table 3]

[0438]

[0439] [Table 4]

[0440]

[0441] [Table 5]

[0442]

[0443] [Table 6]

[0444]

[0445] The table above confirms that, according to the embodiments, a glass cloth capable of achieving improved flatness and a reduced frequency of fuzz generation can be provided. Furthermore, the table also confirms that appropriately controlling the total content of uranium and thorium in the glass cloth is beneficial for evaluating the malfunction performance test.

[0446] Industrial availability

[0447] This disclosure is applicable to fields related to glass yarn, glass cloth, prepreg, printed circuit boards, and methods of manufacturing glass cloth.

[0448] Explanation of reference numerals in the attached figures

[0449] 1: Measuring platform

[0450] 2: Sample of glass cloth

Claims

1. A type of glass cloth, which is a glass cloth composed of glass yarn. The silicon (Si) content in the glass yarn, converted from silicon dioxide (SiO2), is 95.0~100% by mass, and the twist index of the glass yarn is below 400mm.

2. A type of glass cloth, which is a glass cloth composed of glass yarn. The bulk dielectric loss tangent of the glass constituting the glass yarn is 0.001 or less at 10 GHz, and the kink index of the glass yarn is 400 mm or less.

3. The glass cloth according to claim 1 or 2, wherein, The twist index of the glass yarn is above 70mm.

4. The glass cloth according to claim 1 or 2, wherein, The glass yarn comprises glass yarn that satisfies the ranges described in the following formulas (A), (B) and (C): (A)x+y+z=100% mass (B)x≥99.5% of mass (C) 0.0003ppm ≤ y ≤ 0.50ppm x: Silicon content when converted to silicon dioxide (SiO2) y: Total content of uranium and thorium z: Total content of elements other than silicon, uranium, and thorium.

5. The glass cloth according to claim 4, wherein, The range of x is 99.6% or more by mass.

6. The glass cloth according to claim 4, wherein, The range of x is 99.9% or higher in mass.

7. The glass cloth according to claim 1 or 2, wherein, The glass yarn was treated with a surface treatment agent containing a silane coupling agent.

8. The glass cloth according to claim 7, wherein, The surface treatment agent comprises the silane coupling agent shown in formula (1) below: X(R) 3-n Yes n ···(1) In formula (1), X is an organic functional group having at least one of an amino group and an unsaturated double bond group, the unsaturated double bond group having free radical reactivity, Y is each independently an alkoxy group, n is an integer of 1 or more and 3 or less, and R is each independently a group selected from the group consisting of methyl, ethyl and phenyl.

9. The glass cloth according to claim 8, wherein, In the formula (1), X is an organic functional group that does not form salts with ionic compounds.

10. The glass cloth according to claim 8, wherein, X in formula (1) does not contain amines and / or ammonium cations.

11. The glass cloth according to claim 8, wherein, In the formula (1), X is an organic functional group having methacryloyloxy and / or acryloyloxy.

12. The glass cloth according to claim 1 or 2, wherein, The absolute value of the twist count of the glass yarn is in the range of 0.5 to 1.5 times / 25 mm.

13. The glass cloth according to claim 1 or 2, wherein, The glass cloth has the glass yarn as both warp and weft yarns. The absolute value of the difference in twist count between the warp and weft yarns is in the range of 0.01 to 0.70 twists / 25mm.

14. The glass cloth according to claim 1 or 2, wherein, The thickness of the glass cloth is less than 60 μm.

15. The glass cloth according to claim 1 or 2, used for printed circuit boards.

16. A prepreg comprising the glass cloth as described in claim 1 or 2 and a thermosetting resin.

17. A printed circuit board comprising the prepreg of claim 16.

18. An integrated circuit comprising the printed circuit board of claim 17.

19. An electronic device comprising the printed circuit board of claim 17.

20. A method for manufacturing glass cloth, comprising the step of obtaining glass cloth using glass yarn, The silicon (Si) content in the glass yarn, calculated as silicon dioxide (SiO2), is in the range of 95.0~100% by mass. The twist index of the glass yarn is below 400 mm.

21. A method for manufacturing glass cloth, comprising the step of obtaining glass cloth using glass yarn, The bulk dielectric loss tangent of the glass constituting the glass yarn is below 0.001 at 10 GHz. The twist index of the glass yarn is below 400 mm.

22. The method for manufacturing glass cloth according to claim 20 or 21, wherein, The twist index of the glass yarn is above 70mm.

23. The method for manufacturing glass cloth according to claim 20 or 21, comprising the step of obtaining glass cloth using glass yarn. The glass yarn satisfies the ranges described in equations (A), (B), and (C) below: (A)x+y+z=100% mass (B)x≥99.5% of mass (C) 0.0003ppm ≤ y ≤ 0.50ppm x: Silicon content when converted to silicon dioxide (SiO2) y: Total content of uranium and thorium z: Total content of elements other than silicon, uranium, and thorium.

24. The method for manufacturing glass cloth according to claim 20 or 21, comprising: The process of warping the glass yarn used as warp yarn is called the warp warping process, and The process of weaving using the glass yarn is called the weaving process. In the warp winding process and / or the weaving process, the absolute value of the twist count of the glass yarn is adjusted to a range of 0.5 to 1.5 times / 25 mm.

25. The method for manufacturing glass cloth according to claim 24, wherein, The glass cloth has the glass yarn as both warp and weft yarns. The manufacturing method includes a step of adjusting the twist of the weft yarn such that the absolute value of the difference between the twist count of the warp yarn and the weft yarn is in the range of 0.01 to 0.70 times / 25mm.

26. The method for manufacturing glass cloth according to claim 24 or 25, wherein, The glass yarn, whose width is divided by TEX to obtain a value in the range of 10 to 30, is used for the warping process and / or the weaving process.

27. A glass yarn roll having a core material and glass yarn wound around said core material, The silicon (Si) content in the glass yarn, converted from silicon dioxide (SiO2), is 95.0~100% by mass, and the twist index of the glass yarn is below 400mm.

28. The glass yarn roll according to claim 27, wherein, The twist index of the glass yarn is above 70mm.

29. The glass yarn roll according to claim 27 or 28, wherein, The glass yarn satisfies the ranges described in equations (A), (B), and (C) below: (A)x+y+z=100% mass (B)x≥99.5% of mass (C) 0.0003ppm ≤ y ≤ 0.50ppm x: Silicon content when converted to silicon dioxide (SiO2) y: Total content of uranium and thorium z: Total content of elements other than silicon, uranium, and thorium.

30. The glass yarn roll according to claim 27 or 28, wherein, The absolute value of the twist count of the glass yarn is in the range of 0.5 to 1.5 times / 25 mm.

31. The glass yarn roll according to claim 27 or 28, wherein, The width of the glass yarn divided by TEX is in the range of 10 to 30.

32. A type of glass yarn used in the weaving of glass cloth. The silicon (Si) content in the glass yarn, converted from silicon dioxide (SiO2), is 95.0~100% by mass, and the twist index of the glass yarn is below 400mm.

33. The glass yarn according to claim 32, wherein, The twist index of the glass yarn is above 70mm.

34. The glass yarn according to claim 32 or 33, wherein, The glass yarn satisfies the ranges described in equations (A), (B), and (C) below: (A)x+y+z=100% mass (B)x≥99.5% of mass (C) 0.0003ppm ≤ y ≤ 0.50ppm x: Silicon content when converted to silicon dioxide (SiO2) y: Total content of uranium and thorium z: Total content of elements other than silicon, uranium, and thorium.

35. The glass yarn according to claim 34, wherein, The total amount of uranium and thorium, represented by y, is in the range of 0.0003 to 0.0010 ppm.

36. The glass yarn according to claim 34, wherein, The total amount of uranium and thorium, represented by y, is in the range of more than 0.0010 and less than 0.0015 ppm.

37. The glass yarn according to claim 34, wherein, The value of y, representing the total content of uranium and thorium, is in the range of more than 0.0015 and less than 0.0018 ppm.

38. The glass yarn according to claim 34, wherein, The value of y, representing the total content of uranium and thorium, is in the range of more than 0.0018 and less than 0.0035 ppm.

39. The glass yarn according to claim 34, wherein, The value of y, representing the total content of uranium and thorium, is in the range of more than 0.0035 and less than 0.0040 ppm.

40. The glass yarn according to claim 34, wherein, The value of y, representing the total content of uranium and thorium, is in the range of more than 0.0040 and less than 0.09 ppm.

41. The glass yarn according to claim 34, wherein, The value of y, representing the total content of uranium and thorium, is in the range of more than 0.09 and less than 0.12 ppm.

42. The glass yarn according to claim 34, wherein, The value of y, representing the total content of uranium and thorium, is in the range of more than 0.12 and less than 0.50 ppm.

43. The glass yarn according to claim 32 or 33, wherein, The twist index of the glass yarn is in the range of 330~400mm.

44. The glass yarn according to claim 32 or 33, wherein, The twist index of the glass yarn is in the range of 300~329mm.

45. The glass yarn according to claim 32 or 33, wherein, The twist index of the glass yarn is in the range of 220~299mm.

46. ​​The glass yarn according to claim 32 or 33, wherein, The twist index of the glass yarn is in the range of 200~219mm.

47. The glass yarn according to claim 32 or 33, wherein, The twist index of the glass yarn is in the range of 125~199mm.

48. The glass yarn according to claim 32 or 33, wherein, The twist index of the glass yarn is in the range of 110~124mm.

49. The glass yarn according to claim 32 or 33, wherein, The twist index of the glass yarn is below 110 mm.

Citation Information

Patent Citations

  • Glass cloth, prepreg and printed wiring board

    JP2018127747A

  • Silica glass yarn, and silica glass cloth

    JP2020090432A

  • Prepreg, metal-clad laminate, and wiring board

    WO2019065940A1

  • Prepreg, metal-clad laminate, and wiring board

    WO2019065941A1

  • Glass cloth, prepreg, and printed wiring board

    WO2022215288A1