Method for manufacturing a masonry structure and masonry structure
By applying a fiber material coating with a length of 3mm or more and less than 20mm to the masonry wall surface to form a reinforcing coating, the problem of complex procedures is solved, and simple construction and efficient reinforcement effect are achieved, which is suitable for lightweight buildings.
Patent Information
- Application Number
- CN202580029957.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-04-23
- Filing Date
- 2025-04-18
- Publication Date
- 2026-11-24
AI Technical Summary
In existing technologies, the preparation of masonry wall reinforcement materials and the application of photosensitive resin need to be carried out in different processes, resulting in complex procedures.
A reinforcing coating is formed on the surface of the masonry wall by applying a coating containing fiber material with a length of 3mm or more and less than 20mm, which simplifies the process and improves the reinforcement effect.
It enables simplified masonry structure construction, achieves higher reinforcement effect than traditional walls, and can be used in lightweight building design to reduce materials and costs.
Smart Images

Figure CN123165490A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to a method for manufacturing masonry structures and to masonry structures in general. Background Technology
[0002] Previously, it was known that the following construction method was used: a fibrous reinforcing material was placed on the wall surface of a brick wall, and a photosensitive resin was applied to it and cured, thereby reinforcing the wall surface (for example, see Patent Document 1). Existing technical documents
[0003] Patent Document 1: Japanese Patent Application Publication No. 2003-293693 Summary of the Invention The problem the invention aims to solve
[0004] However, in the past, the preparation of reinforcing materials and the coating of photosensitive resins had to be carried out in separate processes, which resulted in complex procedures.
[0005] Therefore, the present invention was made in view of the above-mentioned problems, and its object is to provide a method for manufacturing a masonry structure and a masonry structure that can be constructed with a simple procedure and can achieve a reinforcement effect on the wall surface.
[0006] One aspect of the invention is a method for manufacturing a masonry structure, comprising the step of forming a reinforcing coating on the wall surface of a masonry wall in which a plurality of blocks are arranged in a vertical and horizontal direction. The step of forming the reinforcing coating comprises applying a coating of fibrous material comprising a length longer than the distance between any first block and a second block adjacent to the first block to the wall surface.
[0007] In the step of forming the reinforcing coating, the coating material containing the fiber material with a length of 3 mm or more and 20 mm or less may also be applied to the wall surface.
[0008] It also includes the step of preparing the masonry wall. In the step of preparing the masonry wall, the multiple blocks may be configured without setting a filling material between the first block and the second block.
[0009] One aspect of the masonry structure of the present invention includes: a masonry wall comprising a plurality of blocks arranged in a vertical and horizontal direction; and a reinforcing coating formed on the wall surface of the masonry wall, the reinforcing coating being a layer of coating of fibrous material having a length greater than the distance between any first block among the plurality of blocks and a second block adjacent to the first block.
[0010] The length of the fiber material can also be more than 3 mm and less than 20 mm.
[0011] The method for manufacturing a masonry structure according to the present invention includes: a step of forming a masonry wall by stacking layers formed by supplying material from a moving material supply unit or by irradiating a selected area with light; and a step of forming a reinforcing coating on the wall surface of the masonry wall, wherein the step of forming the reinforcing coating includes applying a coating containing a fiber material of 3 mm or more and 20 mm or less to the wall surface. Invention Effects
[0012] According to the present invention, a method for manufacturing a masonry structure and a masonry structure that can be constructed with a simple procedure and achieve a wall reinforcement effect are provided. It should be noted that the wall reinforcement effect can be used to obtain a wall with higher strength than a normal wall, or it can be used to reconsider the overall composition of the wall based on the existence of the reinforcement effect to obtain a wall with the same strength as a normal wall. Attached Figure Description
[0013] [ Figure 1 [Illustration 1] is a perspective view of a masonry structure representing one aspect of the present invention.
[0014] [ Figure 2 ] is the composition Figure 1 The front view of the masonry wall of the masonry structure.
[0015] [ Figure 3 [This is a diagram used to illustrate the cross-sectional shape of reinforced coatings and masonry walls.]
[0016] [ Figure 4 [ ] is a flowchart illustrating an example of the process of manufacturing a masonry structure.
[0017] [ Figure 5 [] is a graph representing the simulation results.
[0018] [ Figure 6 [] is a graph representing the simulation results.
[0019] [ Figure 7 [ is used for explanation] Figure 6 A schematic diagram of the simulation conditions.
[0020] [ Figure 8 [Illustration 1] is a cross-sectional view schematically showing a modified example of the masonry structure of the present invention. Detailed Implementation
[0021] Figure 1 This is a perspective view of a masonry structure representing one aspect of the present invention. Figure 2 It constitutes Figure 1 The front view of a masonry wall in a masonry structure. Figure 1The figures depict a portion of the reinforcing coating being removed. It should be noted that the vertical direction corresponds to the vertical direction, and the horizontal direction corresponds to the horizontal direction in each figure of this application.
[0022] like Figure 1 As shown, the masonry structure S100 of this embodiment includes a masonry wall 10 and a reinforcing coating 20. The masonry structure S100 is used as an example of an interior or exterior wall of a building.
[0023] The masonry wall 10 has blocks 11 and infill material 15. The blocks 11 are... Figure 1 The example has a cuboid shape. Block 11, as an example, is a block without through holes. Specifically, block 11 is, for example, a block made of lightweight aerated concrete (AAC). In the masonry structure S100, multiple blocks 11 are arranged in both the vertical and horizontal directions. Multiple blocks 11 are, as an example, stacked in a grid-like manner, a so-called through-joint masonry method. It should be noted that the present invention can also be applied to masonry such as sintered bricks or concrete blocks.
[0024] It should be noted that block 11 can also be a block with through holes. Multiple blocks 11 can also be stacked in a staggered masonry manner, in which the positions of blocks 11 of a predetermined skin are staggered in the horizontal direction from the positions of blocks 11 of the skin above or below it.
[0025] The density of block 11 is, for example, 0.3 g / cm³ or more and less than 1.5 g / cm³. Block 11 may not have such a low density; for example, the density of block 11 may be 1.5 g / cm³ or more.
[0026] Multiple blocks 11 are arranged with predetermined gaps between them. Figure 2 In the diagram, one of the multiple blocks 11 is shown as the first block 11-1, and the block 11 disposed thereon is shown as the second block 11-2.
[0027] A gap Sa1 is provided between the first block 11-1 and the second block 11-2. The distance d1 of this gap is, for example, more than a few millimeters (e.g., 2 mm) and less than a dozen millimeters (e.g., 15 mm). A gap Sa2 is provided between the first block 11-1 and the block 11 that is horizontally adjacent to the first block 11-1. The distance d2 of this gap is also, for example, more than a few millimeters and less than a dozen millimeters. The distances d1 and d2 can be the same length or different lengths, but in this embodiment, they are the same length as an example.
[0028] Distances d1 and d2 are, for example, the arithmetic mean of the lengths between the edges of one block 11 and the edges of another block 11, measured at any 10 points from an image obtained by photographing the masonry wall 10 from the front. When calculating distance d1, the vertical length between the edge of one block 11 and the edge of another block 11 adjacent in the vertical direction is measured at any 10 points. The distance d1 is measured at the following locations: in the case of so-called continuous-joint masonry, in the area of vertical overlap between adjacent blocks 11 (the area where the edges of one block 11 and the edges of another block 11 are opposite each other), in the horizontal direction centered on the central portion of this overlap. Figure 2 Measurements were taken over approximately four-fifths of the area on the left-right side of the paper. Additionally, in the case of a so-called staggered masonry layering method, measurements were taken in the area where two adjacent blocks 11 overlapped vertically, within the region centered on the center of that overlapping portion, in the horizontal direction (…). Figure 2 The measurement was performed over approximately four-fifths of the area on the paper (in the left-right direction) (excluding the horizontal end of block 11 from the measurement point).
[0029] Furthermore, when determining distance d2, the horizontal length between the edge of one block 11 and the edge of another block 11 adjacent in the horizontal direction is measured at any 10 points. The distance d2 is measured in the region where the horizontally adjacent blocks 11 overlap in the horizontal direction, within the vertical direction centered on the center of that overlapping portion. Figure 2 The measurement was performed over approximately four-fifths of the area on the paper (in the vertical direction) (excluding the vertical end of block 11 from the measurement point).
[0030] It should be noted that in this embodiment, since the filling material 15 is provided, the distance between the blocks (e.g., distance d1 and / or distance d2) is several millimeters or more. However, if the filling material 15 is not provided, the distance between the blocks may be less than several millimeters (e.g., 2 mm) (e.g., less than 1 mm). The blocks may also be made to fit together and the distance d1 and distance d2 may be set to 0 mm.
[0031] In addition, by appropriately adjusting the amount of filling material 15 used, the distance between the blocks (e.g., distance d1 and / or distance d2) can be set to less than a few millimeters (e.g., 2 mm) (e.g., less than 1 mm), or the blocks can be made to fit together and set to 0 mm.
[0032] For the masonry wall 10, it is preferable that, on average, the distance between blocks (e.g., distance d1 and / or distance d2) is the predetermined length as described above for at least one segment of the wall surface (e.g., a segment consisting of any block A and a plurality of blocks B arranged adjacent to block A in the horizontal or vertical direction, or a segment consisting of any block A, a plurality of blocks B arranged adjacent to block A in the horizontal or vertical direction, and a plurality of blocks C arranged adjacent to block B in the horizontal or vertical direction). It is also preferable that, on average, the distance between blocks (e.g., distance d1 and / or distance d2) is the predetermined length as described above. A reinforcement effect can be obtained as long as the predetermined length is achieved in at least one segment of the wall surface, and a higher degree of reinforcement effect can be obtained as long as the predetermined length is achieved on average as a whole.
[0033] The filler material 15 is the material disposed between adjacent blocks 11. The filler material 15 is, for example, mortar. As mortar, any mortar such as cement mortar, mud mortar, or lime mortar can be used, but as an example, cement mortar can also be used. Cement mortar is made by mixing cement and sand in a predetermined ratio and applying it to the space between the blocks in a paste-like state.
[0034] As filler material 15, a reinforcing coating material may also be used. Alternatively, in one example, filler material 15 may not be used.
[0035] Figure 3 This diagram illustrates the cross-sectional shape of the reinforcing coating and the masonry wall. The reinforcing coating 20 is a layer formed on the surface of the masonry wall 10. Specifically, the reinforcing coating 20 is formed in a state of being fixed to the surface of the masonry wall 10. The reinforcing coating 20 can be formed on both sides of the masonry wall 10 or on one side, but in this embodiment, it is formed on one side. The reinforcing coating 20 can be formed on only a portion of the surface of the masonry wall 10 or on the entire surface, but in this embodiment, it is formed on the entire surface.
[0036] Reinforced coating 20 Figure 3 The example shown is formed by a coating in which fiber material 22 is dispersed in resin material 21. Specifically, the reinforcing coating 20 is formed, for example, by curing a resin material 21 containing fiber material 22 and in a slurry form. In the following description, reference numerals for the various components will be largely omitted.
[0037] (Regarding specific fibers) The reinforcing coating preferably comprises fibers of a predetermined length (hereinafter referred to as "specific length"). Hereinafter, the fiber of this specific length will be referred to as specific fiber. It should be noted that, in this specification, the length of the fiber material refers to its actual length.
[0038] From the perspective of achieving a better reinforcement effect by means of a reinforcing coating, the specific length is preferably 1 mm or more, more preferably 3 mm or more, further preferably 6 mm or more, and particularly preferably 13 mm or more.
[0039] From the perspective of workability (hereinafter also simply referred to as "workability") when forming a reinforced coating by applying a coating containing specific fibers (hereinafter referred to as "this coating"), the specific length is preferably 50 mm or less, more preferably 20 mm or less, and even more preferably 16 mm or less.
[0040] The type of specific fiber can also be the same as the type of fiber that can be used as a fiber material. From the perspective of superior weather resistance and reinforcement effect, the specific fiber is preferably an inorganic fiber (such as glass fiber).
[0041] From the perspective of achieving a better reinforcement effect, the content of specific fibers relative to the total mass of the reinforcement coating is preferably 0.1% by mass or more, more preferably 0.3% by mass or more, even more preferably 0.5% by mass or more, even more preferably 1.0% by mass or more, and particularly preferably 2.0% by mass or more.
[0042] From the perspective of better workability, the content of specific fibers relative to the total mass of the reinforcing coating is preferably 75% by mass or less, more preferably 65% by mass or less, even more preferably 55% by mass or less, and particularly preferably 20% by mass or less.
[0043] From the perspective of achieving a better reinforcement effect, the content of the specific fiber relative to the total mass of the coating is preferably 0.1% by mass or more, more preferably 0.3% by mass or more, further preferably 0.5% by mass or more, and even more preferably 1.0% by mass or more.
[0044] From the perspective of superior workability, the content of the specific fiber relative to the total mass of the coating is preferably 60% by mass or less, more preferably 50% by mass or less, even more preferably 40% by mass or less, and particularly preferably 18% by mass or less.
[0045] From the perspective of achieving a good balance between reinforcement effect and workability, the content of the specific fiber relative to the total mass of fiber material contained in the reinforcing coating or this coating is preferably 50% by mass or more, more preferably 75% by mass or more, further preferably 92% by mass or more, and particularly preferably 99% by mass or more. There is no particular upper limit, and it is 100% by mass.
[0046] (Determination of the content of specific fibers) When determining the content of fiber materials and specific fibers contained in this coating, an appropriate method can be used, taking into account the composition and characteristics of the coating. In the case where the coating is composed of resin materials, solvents, and fiber materials (containing specific fibers) that are inorganic fibers (preferably glass fibers), the content of fiber materials and specific fibers contained in the coating can be determined, for example, by performing operations (A) and (B) as shown below.
[0047] (A) An organic solvent compatible with the resin material is added to the coating to reduce its viscosity, and the resulting mixture is filtered. The resulting filter residue is thoroughly washed with the organic solvent and then dried. The dried residue is taken as the fiber material contained in the coating. The mass of the dried residue (fiber material) is taken as the fiber material content contained in the coating.
[0048] (B) The dried material (fiber material) obtained in (A) above is sorted based on fiber length while being observed with a magnifying glass or microscope to obtain specific fibers (fiber material with a specific length). The mass of the obtained specific fibers is taken as the content of the specific fibers contained in this coating.
[0049] It should be noted that in cases where the coating contains solid materials (fillers, etc.) that are different from the fiber materials, a process may be added to separate the solid materials from the fiber materials by redispersing the dried material obtained in (A) above in a suitable liquid and then centrifuging it. The content of fiber materials and specific fibers contained in the coating can be determined by appropriate methods based on the composition of the coating.
[0050] The method for determining the content of fiber materials and specific fibers contained in the reinforcing coating can be any appropriate method that takes into account the composition and characteristics of the reinforcing coating. In the case where the reinforcing coating is composed of resin material and fiber material (containing specific fibers) as inorganic fibers (preferably glass fibers), the content of fiber materials and specific fibers contained in the reinforcing coating can be determined by performing operations (a) and (b) as shown below, for example.
[0051] (a) An organic solvent capable of dissolving the resin material is added to the reinforcing coating to dissolve it, and the resulting mixture is filtered. The resulting filter residue is thoroughly washed with the organic solvent and then dried. The dried residue is taken as the fibrous material contained in the reinforcing coating. The mass of the dried residue (fibrous material) is taken as the content of the fibrous material contained in the reinforcing coating.
[0052] (b) The dried material (fiber material) obtained in (a) above is sorted based on fiber length while being observed with a magnifying glass or microscope to obtain specific fibers (fiber material with a specific length). The mass of the obtained specific fibers is taken as the content of the specific fibers contained in the reinforcing coating.
[0053] It should be noted that, in the absence of organic solvents capable of dissolving the resin material contained in the reinforcing coating, the reinforcing coating can also be heat-treated in air to remove the resin material and extract the dried material (fiber material). The heat treatment conditions can be appropriately determined based on the properties of the resin composition and the fiber material, but for example, heating at 400°C for 10 hours in an atmospheric atmosphere can be considered.
[0054] When the reinforcing coating contains a solid material (filler, etc.) that is different from the fiber material, an additional step is added to separate the solid material from the fiber material by centrifugation after redispersing the dried material (the dried material obtained in (a) above or the dried material obtained in the heat treatment above) in a suitable liquid. The content of the fiber material and the specific fiber contained in the reinforcing coating can be determined by an appropriate method according to the composition of the reinforcing coating.
[0055] Refer again Figure 3 The resin material 21 can also be a so-called elastic coating with a single-layer rubber-like coating surface. For example, an acrylic coating with a cross-linked acrylic emulsion as the main component is preferred as the resin material 21. The content of the resin material 21 relative to the total mass of the reinforcing coating 20 is preferably 80 to 99.5% by mass, for example. The reinforcing coating 20 improves at least one of the stiffness, strength, and deformation capacity of the masonry structure S100 by forming it in a manner that ensures close adhesion to the wall surface.
[0056] It should be noted that polyurethane-based coatings can be used instead of acrylic coatings as resin material 21. In addition, a portion (preferably more than half the amount by weight) or all of the resin contained in the fiber-reinforced resin that can form the reinforcing coating 20 is preferably an elastic resin, preferably an acrylic resin, a silicone resin, an acrylic silicone resin, a polyurethane resin or a natural resin (latex coating).
[0057] The fiber material 22 can be either inorganic fiber (glass fiber, carbon fiber, boron fiber, etc.) or organic fiber (aramid fiber, plant fiber, etc.), preferably inorganic fiber. In this embodiment, glass fiber is exemplified. The average diameter of the fiber material 22 is, for example, 0.5 μm or more and 20 μm or less. By mixing the fiber material 22 into an acrylic coating, a slurry in which the fiber material 22 is suspended in the resin material can be obtained. The weight ratio of the fiber material 22 to the coating is, for example, 1% to 40%. As glass fiber, it can be, for example, glass fiber obtained by removing the binding agent (e.g., PVA, methylcellulose, etc., adhesive polymers) from chopped glass fiber filaments cut to a predetermined length using organic solvents such as toluene or styrene. The fiber material 22 may also be surface-treated to adjust its adhesion to the resin. The content of the fiber material 22 is preferably 0.75% to 4% by mass relative to the total mass of the reinforcing coating 20. The fiber material 22 is not limited to one type and may include multiple fiber materials.
[0058] (The relationship between the length of the fiber material and the distance between the blocks) The inventors discovered that, in Figure 3 When the length L of the fiber material 22 is longer than the distance d1 between the blocks, the reinforcement effect achieved by applying the reinforcing coating 20 to the masonry wall 10 can be effectively obtained. It should be noted that the following mainly describes the relationship between the distance d1 between the blocks in the vertical direction and the length L of the fiber material 22, but the length L of the fiber material 22 can also be longer than the distance d2 between the blocks in the horizontal direction.
[0059] The length L of the fiber material 22 is only required to be longer than the distance d1 and / or d2 between the blocks, and is not limited to a specific size. In the coating of this embodiment, the fiber material acts as a spring-like component in the resin. If the fiber material adheres well to the resin, an increase in the stiffness and / or strength of the resin surrounding the fiber material can be expected.
[0060] For example, when the distance d1 between the blocks is 5 mm, the length L of the fiber material 22 only needs to be longer than 5 mm. As an example, the length L of the fiber material 22 is preferably 10% or more longer than the lengths of distances d1 and d2 in one embodiment, and more preferably 20% or more longer in another embodiment. Furthermore, the specific length is preferably longer than distances d1 and / or d2, more preferably 10% or more longer than distances d1 and / or d2, and even more preferably 20% or more longer than distances d1 and / or d2.
[0061] The length L can refer to the length of the longest fiber in the fiber material 22, or it can be the weighted average of the fiber lengths of the fiber material 22 (length-average fiber length). In the case of obtaining the weighted average of the fiber lengths of the fiber material 22, it can be determined by analyzing a photomicrograph (or a photograph with sufficiently high magnification) using an image analysis device.
[0062] As an example, the weighted average of the fiber lengths of fiber material 22 can also be the weighted average of the fiber lengths of 50 randomly selected fiber materials. These "50 fiber materials" can be fiber materials contained in the coating used to form the reinforcing coating, or fiber materials contained in the reinforcing coating formed on the surface of a masonry wall. The fiber material contained in the coating can also be obtained, for example, through the aforementioned operation (A). It should be noted that, as needed, the aforementioned step of separating the solid material from the fiber material can be added to operation (A). The fiber material contained in the coating can also be obtained, for example, through the aforementioned operation (a). It should be noted that, as needed, the aforementioned method of heating the coating in air to remove the fiber material can be performed instead of operation (a), and the aforementioned step of separating the solid material from the fiber material can also be added.
[0063] Alternatively, the fiber material obtained from the coating or coating can be redispersed in a suitable solvent, and the resulting mixture can be spread on a clean glass plate. After obtaining a photomicrograph (or a sufficiently high magnification photomicrograph) of the group of fiber materials dispersed on the glass plate, the photomicrograph can be analyzed using an image analysis device (software) to obtain a weighted average of the fiber lengths (actual lengths) of 50 randomly selected fiber materials.
[0064] (Coating of the reinforcing coating) The coating forming the reinforcing coating 20 is applied to the masonry wall 10 by means of a roller, trowel, brush, or sprayer and adheres to the wall surface. Specifically, the reinforcing coating 20 is formed, for example, by applying a coating in which glass fibers are suspended and then curing it. In the case of a cross-linked acrylic emulsion, for example, the coating forms a single layer that is firmly adhered to the wall regardless of the surface morphology of the masonry wall 10.
[0065] It should be noted that the coating can also be applied after the primer material has been applied to and dried on the masonry wall 10. The reinforcing coating 20 does not need to be a single layer; it can also be formed by layering multiple layers with different properties. The reinforcing coating 20 may also not be formed directly on the surface of the masonry wall 10, but rather in the presence of a layer such as mortar. The curing of the reinforcing coating 20 can be achieved through drying, curing with a curing agent, or a combination of both.
[0066] (Manufacturing of masonry structures) Figure 4 This is a flowchart illustrating an example of the process of manufacturing a masonry structure. In step S1, the worker prepares the masonry wall 10. The worker forms the masonry wall 10, which consists of multiple stacked blocks 11, for example, by repeatedly arranging the blocks 11 and applying mortar as filler material 15. It should be noted that this example shows the same worker performing steps S1 to S3, but the invention is not limited to this; the worker may also perform steps S2 and S3 on a pre-formed masonry wall 10.
[0067] Next, in step S2, the worker applies the coating of the reinforcing coating 20 to the wall surface of the masonry wall 10. As described above, the worker applies the coating, which is made by dispersing the fiber material 22 in the resin material 21, to the wall surface using a roller, trowel, brush, or sprayer.
[0068] Next, in step S3, the operator cures the applied coating. In the case of forming multiple reinforcing coatings, coatings for forming other reinforcing coatings may also be applied before the reinforcing coatings are completely dry.
[0069] By forming the reinforcing coating 20 through steps S2 and S3, a masonry structure S100 reinforced by the reinforcing coating 20 is manufactured through the above series of manufacturing methods.
[0070] It should be noted that in step S1 of preparing the masonry wall, multiple blocks 11 can be configured without the infill material 15. For example, a masonry wall can be formed without the infill material 15 between adjacent blocks in the vertical direction, without the infill material 15 between adjacent blocks in the horizontal direction, or without the infill material 15 between adjacent blocks in both the vertical and horizontal directions.
[0071] (Effects of this implementation method) According to the masonry structure S100 of this embodiment described above, a reinforcing coating 20 is formed by applying a coating containing fiber material 22 longer than the distance d1 and d2 between the blocks to the wall surface of the masonry wall 10 and then curing it. Therefore, the reinforced masonry structure S100 can be manufactured in a simple process.
[0072] The reinforcing coating 20 of the masonry structure S100 has a higher reinforcement effect compared to coatings that do not contain fiber material 22. Therefore, even if the rigidity of the masonry wall 10 is insufficient, the final masonry structure S100 reinforced by the reinforcing coating 20 has sufficient rigidity. In addition, by forming the reinforcing coating 20, the strength of the masonry structure S100 can also be expected to be improved.
[0073] Furthermore, according to the configuration of this embodiment, compared with buildings using existing masonry walls, it is advantageous to make the building lighter overall, thus allowing for a reconsideration of the overall building design. Therefore, it is also possible to reduce the materials and costs used in building construction, as well as reduce carbon dioxide emissions.
[0074] It should be noted that, in Figure 2 In the previous description, the block 11 above the first block 11-1 was referred to as the second block 11-2. However, the relationship between the first block and the second block in this invention is not necessarily a vertically adjacent relationship; it can also be a horizontally adjacent relationship. That is to say, the statement that the fiber material is "longer than the distance between the first block and the second block adjacent to the first block" also includes the statement that the length of the fiber material is longer than the horizontal distance between the blocks.
[0075] The inventors conducted simulations to verify the relationship between fiber length relative to the distance between blocks and the effect of stiffness improvement. Figure 5 and Figure 6 It is a graph representing the results of the simulation. Figure 5 It is a semi-logarithmic graph, with the horizontal axis representing the fiber content (%) and the vertical axis representing the increase in stiffness. Figure 6 This is also a semi-logarithmic graph, with the horizontal axis representing the distance between blocks (mm) and the vertical axis representing the increase in stiffness. It should be noted that... Figure 5 and Figure 6 It is related to the initial stiffness.
[0076] The purpose of this simulation is to verify the effect of changing the length of the fiber material on the stiffness of the resin, as well as the effect of changing the length of the fiber material / the distance between the blocks. The simulation conditions are as follows.
[0077] - Analysis method: Finite element method (FEM) - The resin was modeled using a standard FEM model with elastic two-dimensional constant strain triangular elements.
[0078] - The fiber material was modeled using a standard FEM model with one-dimensional axial elements.
[0079] - Young's modulus of fiber material (glass fiber) = 100,000 MPa - The Poisson's ratio of the fiber material (glass fiber) is 0.2. - Young's modulus of the resin = 1 MPa One of the parameters affecting the results is the ratio of the Young's modulus of the resin to that of the glass fiber; in this analysis, this ratio is set to 1:100,000. The fiber material is assumed to exist at random locations within the resin. Furthermore, since it is difficult to conduct experiments to obtain the nonlinear load-slip behavior of the fibers within the resin, the boundaries between the fiber material and the resin, as well as the boundaries between the fiber material and the resin and the bulk, are set to be fixed.
[0080] The degree of increase is given by the following formula.
[0081] Increase rate = (Stiffness of the fiber-containing coating) / (Stiffness of the non-fiber-containing coating) = (Applied load / Displacement of the fiber-containing coating) / (Applied load / Displacement of the non-fiber-containing coating) exist Figure 5 The simulation verified the tensile strength of materials containing fiber materials dispersed in resin. Specifically, the tensile strength was verified by varying the percentage of fiber content in materials containing 3mm, 6mm, and 13mm fibers. Figure 5 As shown, it was confirmed that for 3mm fiber materials, tensile strength increases with increasing fiber content. For 6mm fiber materials, tensile strength effectively increases until the fiber content reaches approximately 4%, and for 13mm fiber materials, tensile strength increases significantly with increasing fiber content.
[0082] exist Figure 6 In the simulation, the tensile strength of coatings containing 3mm, 6mm, and 13mm fiber materials formed on the wall surface was verified. Specifically, as... Figure 7 As shown, the tensile strength (with tension applied in the vertical direction) of a structure in which a reinforcing coating containing fiber material is formed on the wall surface of two blocks arranged vertically at a predetermined interval was verified. The fiber material content was set to 4%, and the distance between the blocks varied from 1 mm to 30 mm.
[0083] like Figure 6 As shown, regardless of whether the fiber material is 3mm, 6mm, or 13mm, in the region where the fiber material is longer than the distance between the blocks, the "increase in stiffness" exceeds "5" (it can be confirmed that the effect exceeds the increase in stiffness brought by the reinforcing coating itself). Therefore, it is confirmed that by forming a reinforcing coating with a coating containing fiber material longer than the distance between the blocks, the effect of increasing the stiffness of the masonry structure can be obtained.
[0084] Specifically, for 3mm fiber materials, when the fiber length exceeds the distance between blocks (the area to the left of reference line a), although not as good as for 6mm and 13mm fiber materials, it was confirmed that the structure of the reinforcing coating formed by the coating containing fiber material longer than the distance between blocks has an effect on increasing stiffness. Furthermore, for 6mm fiber materials, when the fiber length exceeds the distance between blocks (the area to the left of reference line b), a better stiffness increase effect was obtained than for 3mm fiber materials. Similarly, for 13mm fiber materials, when the fiber length exceeds the distance between blocks (the area to the left of reference line c), a better stiffness increase effect was also obtained than for 3mm fiber materials.
[0085] The simulation results confirmed that in the formation of a reinforcing coating by a coating containing fiber material longer than the distance between the blocks, a minimum fiber material length of 3 mm or more, especially 6 mm or more, is more preferred in terms of effectively reinforcing the structure.
[0086] It should be noted that, Figure 5 and Figure 6 The results are relative rather than absolute values compared to resins without fibrous materials, so the same tendency can be expected even with different coating thicknesses.
[0087] (Variation example) Figure 8 This is a cross-sectional view schematically illustrating a modified example of the masonry structure of the present invention. Figure 8 The up-down direction is taken as an example corresponding to the vertical direction. In the foregoing embodiment, an example of forming a reinforcing coating 20 on a masonry wall 10 with multiple stacked blocks 11 has been described, but the present invention is not limited thereto.
[0088] Figure 8 The masonry structure includes a masonry wall 110 and a reinforcing coating 120. The masonry wall 110, as an example, is a wall manufactured using a 3D printer additive manufacturing process. The masonry wall 110 (especially in the case of forming the masonry wall 110 using a 3D printer) only requires the existence of a surface (wall surface) capable of forming the reinforcing coating 120. The masonry wall 110 can be part or all of a structure, such as a wall in a building or structure, or part or all of a component other than a wall, or part or all of a component of a bridge pier, monument, furniture, ornament, etc. The masonry wall 110 has multiple layers 111. Additive manufacturing using a 3D printer can be based on material extrusion, material jetting, stereolithography, or powder bed fusion; any of these methods are acceptable.
[0089] Layer 111 can be formed, for example, by ejecting material from the nozzle while moving the nozzle of the 3D printer. Alternatively, if the material is photocurable, layer 111 can be formed by irradiating a selected area of the uncured layer with light. The material of layer 111 can be any material that can be ejected by the 3D printer, but for example, mortar. The material of layer 111 can also be cement, concrete, or resin, etc.
[0090] exist Figure 8 In one example, no other material is interposed between a layer 111 and other layers 111 adjacent to it in the vertical direction. However, in one aspect of the invention, other materials may be interposed between layers 111. The thickness da of layer 111 is, for example, 1 mm or more and less than 200 mm, specifically, for example, 15 mm or more and less than 50 mm.
[0091] The reinforcing coating 120 is a reinforcing layer formed on the surface of the masonry wall 110. The material of the reinforcing coating 120 is the same as that of the aforementioned reinforcing coating 20. The reinforcing coating 120 can be either opaque or transparent.
[0092] like Figure 8 The masonry wall 110, formed by stacking multiple layers 111 as described above, may experience reduced bonding strength between layers 111 (or, in the case of interlayer material between adjacent layers 111) depending on the material and the 3D printer manufacturing process. Therefore, in Figure 8 In the example, the masonry structure can be reinforced by setting a reinforcing coating 120 containing fiber material.
[0093] exist Figure 8 In the composition, the length of the fiber material contained in the reinforcing coating 120 is, for example, 3 mm or more and 20 mm or less. From the perspective of obtaining a good reinforcement effect, the length of the fiber material is preferably 1.5% or more of the thickness da of the layer 111 (for example, 3 mm or more for a layer 111 with a thickness of 200 mm).
[0094] Figure 8 The method for manufacturing a masonry structure includes the steps of stacking layers 111 formed by supplying material from a moving material supply unit (e.g., the nozzle of a 3D printer) to form a masonry wall 110; and the step of forming a reinforcing coating 120 on the wall surface of the masonry wall 110.
[0095] Thus, based on the masonry structure comprising a masonry wall 110 formed by additive manufacturing and a reinforcing coating 120 formed on its surface, the strength and stiffness of the masonry wall can be improved because the masonry wall 110 is well reinforced by the reinforcing coating 120.
[0096] It should be noted that the "movement" in the aforementioned "moving material supply unit" refers to any change in position relative to the masonry wall to be formed. That is, the material supply unit is considered to be moving not only when the material supply unit itself moves, but also when the material supply unit itself is fixed while the base (platform) for forming the masonry wall moves. Furthermore, a step of smoothing the surface of the masonry wall 110 (making the surface smooth, etc.) can be performed between the step of forming the masonry wall 110 and the step of forming the reinforcing coating 120 on the surface of the masonry wall 110.
[0097] When using a 3D printer for layering, the length of the fiber material is not limited to the above; it can be more than 1 mm and less than 20 mm.
[0098] The present invention has been described above using embodiments, but the technical scope of the present invention is not limited to the scope described in the above embodiments, and various modifications and alterations can be made within its scope. For example, all or part of the device can be configured in any unit, functionally or physically distributed or integrated. In addition, new embodiments resulting from any combination of multiple embodiments are also included in the embodiments of the present invention. The effects of new embodiments resulting from combinations are the same as the effects of the original embodiments. Explanation of reference numerals in the attached figures
[0099] 10 and 110 masonry walls 11, 111 blocks 11-1 First Block 11-2 Second block 15. Filling material 20, 120 Reinforced Coating 21 Resin Materials 22 Fiber Materials S100 Masonry Structure
Claims
1. A method for manufacturing a masonry structure, comprising: The step of forming a reinforcing coating on the surface of a masonry wall in which multiple blocks are arranged vertically and horizontally. Steps to form a reinforcing coating The coating comprises a fibrous material having a length greater than the distance between any first block among the plurality of blocks and a second block adjacent to the first block, applied to the wall surface.
2. The method for manufacturing a masonry structure according to claim 1, wherein, In the step of forming the reinforcing coating The coating, in which the fiber material with a length of 3 mm or more and less than 20 mm is dispersed, is applied to the wall surface.
3. The method for manufacturing a masonry structure according to claim 1 or 2, wherein, It also includes the steps of preparing the masonry wall. In the step of preparing the masonry wall, the plurality of blocks are configured without placing a filling material between the first block and the second block.
4. A masonry structure, comprising: A masonry wall consisting of multiple blocks arranged vertically and horizontally; as well as A reinforcing coating formed on the surface of the masonry wall. The reinforcing coating It is a layer of coating made of fibrous material that is longer than the distance between any first block among the plurality of blocks and a second block adjacent to the first block.
5. The masonry structure according to claim 4, wherein, The length of the fiber material is more than 3 mm and less than 20 mm.
6. A method for manufacturing a masonry structure, comprising: The steps of forming a masonry wall include supplying materials from a moving material supply unit or irradiating a selected area with light to form layers of stacked materials; as well as The step of forming a reinforcing coating on the surface of the masonry wall. The steps to form a reinforcing coating, The method involves applying a coating containing fiber material of 3mm or more and 20mm or less to the wall surface.
Citation Information
Patent Citations
Peeling prevention method for brick-line wall surface
JP2003293693A