Negative electrode for nonaqueous electrolyte secondary battery and nonaqueous electrolyte secondary battery
By using a non-fibrous binder in the negative electrode composite material of a non-aqueous electrolyte secondary battery and controlling its dispersion and uniformity in the thickness direction, the problems of insufficient strength and battery capacity in the dry method are solved, and higher battery performance is achieved.
Patent Information
- Application Number
- CN202580029589.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-04-30
- Filing Date
- 2025-04-09
- Publication Date
- 2026-11-24
AI Technical Summary
The strength and battery capacity of the negative electrode composite materials for non-aqueous electrolyte secondary batteries produced by existing dry methods are sometimes reduced, especially when using fibrous binders.
By using a non-fibrous binder in the negative electrode composite material and controlling the binder dispersion to be above 0.01 and below 1.2, while controlling the uniformity of binder content in the thickness direction, local concentration can be avoided.
This improved the strength of the negative electrode composite material and the battery capacity, ensuring the battery's performance stability and efficiency.
Smart Images

Figure CN123165696A_ABST
Abstract
Description
Technical Field
[0001] This disclosure relates to a negative electrode for a non-aqueous electrolyte secondary battery and a non-aqueous electrolyte secondary battery, and particularly to a negative electrode for a non-aqueous electrolyte secondary battery comprising a negative electrode composite material formed by a dry process, and a non-aqueous electrolyte secondary battery having the negative electrode for a non-aqueous electrolyte secondary battery. Background Technology
[0002] Previously, electrodes for non-aqueous electrolyte secondary batteries such as lithium-ion batteries were manufactured using a wet method, which involved coating a slurry containing active materials and binders onto the surface of a core material that served as a metal foil, and then drying and compressing the coating.
[0003] In recent years, dry methods without using electrode composite slurry have been researched. The dry method refers to the process of manufacturing electrode composite materials by stretching electrode composite material particles into sheets, and then bonding these sheets to a core material to create an electrode. Typically, in the dry method, fibrous binders such as polytetrafluoroethylene (PTFE) are used to bond the active materials together. Patent Document 1 discloses an electrode composite material manufactured using a dry method with PTFE as an essential component. Furthermore, Patent Document 1 also discloses an electrode composite material containing polyvinylidene fluoride (PVDF) as a non-fibrous binder along with PTFE, stating that the PVDF content in the electrode composite material is half the mass ratio of PTFE.
[0004] Existing technical documents
[0005] Patent documents
[0006] Patent Document 1: Japanese Patent Publication No. 2021-504877 Summary of the Invention
[0007] The results of the inventors' research indicate that the strength and battery capacity of negative electrode composite materials manufactured using a dry method with fibrous binders such as PTFE sometimes decrease. The inventors further conducted in-depth research and discovered that regardless of the presence or absence of a fibrous binder, by setting the dispersion of the binder in the negative electrode composite material within a specified range, both the strength and battery capacity of the negative electrode composite material are improved. The technology disclosed in Patent Document 1 has not yet addressed the dispersion of the binder, leaving room for improvement.
[0008] The purpose of this disclosure is to provide a negative electrode that improves the strength and battery capacity of the negative electrode composite material.
[0009] One aspect of this disclosure relates to a negative electrode for a non-aqueous electrolyte secondary battery, characterized in that it comprises a negative electrode core material and a negative electrode composite material laminated on the surface of the negative electrode core material. The negative electrode composite material contains a negative electrode active material and a binder for bonding the negative electrode active material together. The binder comprises a non-fibrous binder and has a dispersion of 0.01 or more and 1.2 or less in the negative electrode composite material. When the negative electrode composite material is divided into three equal parts in the thickness direction and designated as a first region, a second region, and a third region from the negative electrode core material side, and the binder content in the first region, the binder content in the second region, and the binder content in the third region are designated as a, b, and c, respectively, the value obtained by subtracting the minimum value of a to c from the maximum value of a to c is 5% or less relative to the total value of a to c.
[0010] One aspect of the non-aqueous electrolyte secondary battery disclosed herein is characterized by comprising the aforementioned negative electrode, positive electrode, and non-aqueous electrolyte for a non-aqueous electrolyte secondary battery.
[0011] According to one embodiment of the present disclosure, a negative electrode for a non-aqueous electrolyte secondary battery can improve the strength of the negative electrode composite material and the battery capacity. Attached Figure Description
[0012] Figure 1 This is a cross-sectional view of the negative electrode as an example of an implementation method.
[0013] Figure 2 This is a schematic diagram showing the state of the negative electrode active material and non-fibrous binder in a negative electrode composite material as an example of an embodiment.
[0014] Figure 3 In the manufacturing process of the negative electrode, as an example of an implementation method, Figure 3 (a) is a diagram representing the mixing steps. Figure 3 (b) is a diagram showing the stretching steps.
[0015] Figure 4 This diagram illustrates the bonding step in the manufacturing process of the negative electrode, as an example of an implementation method.
[0016] Conventionally, when fabricating electrodes using the dry process, fibrous binders such as polytetrafluoroethylene (PTFE) are used to bond the active materials together. However, the results of the inventors' research show that the strength and battery capacity of the negative electrode composite material fabricated using fibrous binders sometimes decrease. The inventors further conducted in-depth research and discovered that by including a non-fibrous binder in the negative electrode composite material and setting the binder dispersion in the negative electrode composite material to 0.01 or higher and 1.2 or lower, the strength and battery capacity of the negative electrode composite material are improved. By using a non-fibrous binder, the binder dispersion in the negative electrode composite material can be achieved within the aforementioned range.
[0017] The following provides a detailed description of embodiments of the negative electrode (hereinafter, sometimes referred to as the negative electrode) and the non-aqueous electrolyte secondary battery disclosed herein. The embodiments described below are merely examples, and this disclosure is not limited to these embodiments. Furthermore, the accompanying drawings referenced in the description of the embodiments are schematic representations, and the dimensional ratios of the constituent elements depicted in the drawings should be determined with reference to the following description.
[0018] <Negative electrode>
[0019] First, refer to Figure 1 and Figure 2 The negative electrode 10 involved in this disclosure will be described in detail. Figure 1 This is a cross-sectional view of the negative electrode 10 as an example of an implementation method. Figure 2 This is a schematic diagram showing the state of the negative electrode active material and non-fibrous binder in the negative electrode composite material 12, which is an example of an embodiment.
[0020] like Figure 1 As shown, the negative electrode 10 includes a negative electrode core material 11 and a negative electrode composite material 12 laminated on the surface of the negative electrode core material 11. The negative electrode 10 may have the negative electrode composite material 12 on both sides of the negative electrode core material 11. The negative electrode 10 may be a strip-shaped electrode constituting a wound electrode body, or it may be a rectangular electrode constituting a laminated electrode body.
[0021] The negative electrode core material 11 can be a metal foil, a film with a metal layer formed on its surface, or the like. The thickness of the negative electrode core material 11 is, for example, 5 μm to 20 μm. As the negative electrode core material 11, a metal foil with copper as its main component can be used. In this specification, the main component refers to the component with the highest mass ratio. The negative electrode core material 11 can be a copper foil that is substantially 100% copper.
[0022] The negative electrode composite material 12 contains a negative electrode active material and a binder that binds the negative electrode active material together. The thickness of the negative electrode composite material 12 is, for example, 30 μm to 120 μm, preferably 50 μm to 100 μm. The negative electrode active material is the main component of the negative electrode composite material 12. The content of the negative electrode active material in the negative electrode composite material 12 relative to the total mass of the negative electrode composite material 12 is, for example, 90% by mass or more, and may also be 95% by mass or more.
[0023] The negative electrode active material contained in the negative electrode composite material 12 is not particularly limited as long as it can reversibly absorb, store and release lithium ions, and carbon materials such as graphite are generally used. The graphite may be any of natural graphite such as flake graphite, massive graphite and earthy graphite, as well as artificial graphite such as massive artificial graphite and graphitized mesocarbon microbeads. The volume-based median diameter (D50) of the graphite is, for example, 1 μm or more and 30 μm or less. The D50 of graphite refers to the particle size at which the cumulative frequency from the smaller particle size side accounts for 50% in the volume-based particle size distribution. The particle size distribution of graphite can be measured using a laser diffraction type particle size distribution measuring device (e.g., MT3000II manufactured by Microtrac BEL Co., Ltd.) with water or the like as a dispersion medium. It should be noted that the D50 of materials other than graphite can also be measured in the same manner.
[0024] As the negative electrode active material, in addition to graphite, metals that alloy with Li such as Si and Sn; metal compounds containing Si, Sn and the like; lithium-titanium composite oxides, etc., can be used. The negative electrode active material may include a Si-containing material. Examples of the Si-containing material include SiO x A Si-containing compound represented by (0.5≤x≤1.6), a Si-containing compound in which Si fine particles are dispersed in a lithium silicate phase represented by Li 2y SiO (2+y) (0<y<2), or a Si-containing compound in which Si is dispersed in a carbon material, etc. The Si-containing materials may be used alone or in combination of two or more. When the negative electrode composite material 12 contains a Si-containing compound, the battery capacity can be increased, but the expansion and contraction ratio of the negative electrode 10 during charging becomes larger. Therefore, when the negative electrode composite material 12 contains a Si-containing compound, the strength of the negative electrode composite material 12 and the battery capacity tend to decrease, so the effect of the non-fibrillated binder of the present disclosure described later is more significant. The content of the Si-containing material in the negative electrode composite material 12 is, for example, 6 mass% or more and 30 mass% or less with respect to the total mass of the negative electrode active material. The volume-based median diameter (D50) of the Si-containing material is, for example, 1 μm or more and 15 μm or less.
[0025] The binder contained in the negative electrode composite material 12 includes a non-fibrillated binder. As Figure 2 shown, the presence of the non-fibrillated binder 22 between the negative electrode active materials 20 strengthens the bonding between the negative electrode active materials, thereby improving the strength of the negative electrode composite material 12. In addition, the strengthened bonding between the negative electrode active materials maintains the conductive paths in the negative electrode composite material 12, thus improving the battery capacity.
[0026] The strength of the negative electrode composite material 12 is 200 gf or more. The strength of the negative electrode composite material 12 can be measured by the following procedure.
[0027] [Methods for determining the strength of composite materials]
[0028] First, a test piece measuring 2 cm in length and 3 cm in width is cut from the negative electrode 10, on which negative electrode composite material 12 is laminated on both sides of the negative electrode core material 11. The test piece is then attached to the adhesive side of double-sided adhesive tape (manufactured by Nitto Denko Corporation, No. 515) pasted on a glass plate to prepare a test sample with the negative electrode composite material 12 attached.
[0029] The adhesive surface of the test specimen after peeling from the glass plate is mounted on the front end of the probe (0.2 cm in diameter) of the adhesive testing machine (RESCA, TAC-II). Under the following conditions, the probe is pressed against the negative electrode composite material 12 of the test specimen and then pulled away to perform a peel test. The maximum load at which peeling occurs between the active material particles is measured 5 times, and the average value is taken as the composite material strength.
[0030] Probe indentation speed: 30mm / minute
[0031] Probe insertion time: 10 seconds
[0032] Indentation load of the probe: 400gf
[0033] Probe pull-out speed: 600mm / minute
[0034] The non-fibrous adhesive 22 is an adhesive that does not undergo fibrosis. Examples of non-fibrous adhesives 22 include vinylidene fluoride (PVDF), polyacrylonitrile (PAN), carboxymethyl cellulose (CMC) or its salts, polyacrylic acid (PAA) or its salts, styrene-butadiene rubber (SBR), nitrile-butadiene rubber (NBR), polyimide resins, acrylic resins, and polyolefin resins. These can be used alone or in combination of two or more. The non-fibrous adhesive 22 preferably contains PVDF.
[0035] The binder contained in the negative electrode composite material 12 may also include a fibrous binder (fibrous binder). Examples of fibrous binders include polytetrafluoroethylene (PTFE). One type may be used alone, or two or more may be used in combination. PTFE is preferably included as the fibrous binder.
[0036] The content of the non-fibrous binder 22 in the negative electrode composite material 12 is, for example, 0.1% by mass or more and 5% by mass or less relative to the total mass of the negative electrode active material 20. Conversely, the content of the fibrous binder in the negative electrode composite material 12 is, for example, 0.1% by mass or more and 5% by mass or less relative to the total mass of the negative electrode active material 20.
[0037] The non-fibrous binder 22 forms secondary particles from the aggregation of primary particles. The primary particles have a particle size of, for example, 50 nm or more and 300 nm or less, while the secondary particles have a particle size of, for example, 1 μm or more and 20 μm or less. It should be noted that... Figure 2 The non-fibrous binder 22 in the middle is a primary particle. The particle size of the secondary particles is the median particle size (D50) on a volume basis. The particle size of the primary particles is calculated by averaging the diameter of the circumcircle of the primary particles extracted from the analysis of scanning electron microscopy (SEM) images of the secondary particle cross-sections.
[0038] The dispersion of the binder in the negative electrode composite material 12 is, for example, greater than 0.01 and less than 1.2. The smaller the dispersion, the more uniformly the binder is dispersed. When the dispersion exceeds 1.2, the binder concentrates in one part, and the strength and battery capacity of the negative electrode composite material 12 are prone to decrease.
[0039] The dispersion of the binder was calculated by measuring the cross-section of the negative electrode composite material 12 using surface analysis (wavelength dispersion method) based on electron probe microanalysis (EPMA). That is, the dispersion of the binder is an indicator of the uniformity of the binder in the cross-section of the negative electrode composite material 12. For example, when the binder contains fluorine (F) such as PVDF or PTFE, the dispersion of the binder is measured as follows. It should be noted that by changing the element being measured according to the composition of the binder, the dispersion of the binder can be calculated in the same way as described below. For example, when calculating the dispersion of SBR, the SBR is stained with Br, and the Br is measured using EPMA. Similarly, when calculating the dispersion of CMC or PAA, the CMC or PAA is stained with Ag, and the Ag is measured using EPMA.
[0040] [Methods for calculating the dispersibility of adhesives]
[0041] (1) Using EPMA, the mapping of the region where F exists (F region) is determined. The size of the mapping image is, for example, 300 μm in length × 400 μm in width.
[0042] (2) Divide the mapped image vertically into 4 and horizontally into 5, for a total of 20 partitions, and calculate the sum of F detection intensities (F value) for each partition.
[0043] (4) Calculate the average value and standard deviation from the F values of the 20 partitions, and calculate the dispersion of the adhesive based on the following formula.
[0044] Adhesive dispersion = standard deviation / average
[0045] The negative electrode composite material 12 may contain a conductive material. Examples of conductive materials contained in the negative electrode composite material 12 include carbon materials such as acetylene black (AB), carbon black (CB) such as Ketjen black, and carbon nanotubes (CNT). The content of the conductive material in the negative electrode composite material 12 may be set to, for example, 0.01% by mass to 5.0% by mass.
[0046] When the negative electrode composite material 12 is divided into three equal parts along its thickness direction, designated as a first region, a second region, and a third region from the negative electrode core material 11 side, and the binder content in the first region, the second region, and the third region is designated as a, b, and c, respectively, the value obtained by subtracting the minimum value from the maximum value of a to c is less than 5% relative to the total value of a to c. Therefore, the binder will not be locally enriched in a portion of the negative electrode composite material 12 along its thickness direction, but will be present in a substantially uniform manner throughout the negative electrode composite material 12. By using the dry process described later, the binder can be made to be present in a substantially uniform manner throughout the negative electrode composite material 12. It should be noted that the lower limit of ((maximum value of a to c) - (minimum value of a to c)) / (a+b+c) is not particularly limited, for example, it is 0.1%. The binder content in each region is obtained by measuring the cross-section of the negative electrode composite material 12 using EPMA.
[0047] <Method for manufacturing the negative electrode>
[0048] Figure 3 and Figure 4 This diagram schematically illustrates the manufacturing process of the negative electrode 10 as an example of an implementation. The manufacturing method of the negative electrode 10 includes... Figure 3 The mixing steps shown in (a) Figure 3 The stretching steps shown in (b) and Figure 4 The bonding steps are shown below. In the mixing step, the negative electrode active material is mixed with a binder to produce negative electrode composite material particles 12a with a solid content of substantially 100%. In the stretching step, the negative electrode composite material particles 12a are mixed and stretched to form a sheet, thereby producing a negative electrode composite material 12b. In the bonding step, the negative electrode composite material 12b is bonded to the negative electrode core material 11 to produce an electrode.
[0049] The method for manufacturing the negative electrode 10 is a dry process using a negative electrode composite material 12 with a substantially 100% solids content. A dry process refers to a process in which the active material particles and binder particles are mixed without the use of solvents; that is, the mixing is carried out when the solids content in the active material and binder is substantially 100%. The method for manufacturing the negative electrode 10 disclosed herein does not require the use of solvents as in conventional methods for manufacturing negative electrodes 10. The absence of solvents not only means that no solvent is needed as a raw material, but also that no solvent drying process is required, nor are exhaust equipment or similar equipment required for the drying process.
[0050] exist Figure 3 In the mixing step shown in (a), raw materials such as the negative electrode active material and binder are mixed in the mixer 30 to produce negative electrode composite material particles 12a. The mixer 30 can be, for example, a conventionally known mechanical mixing mixer. Preferred examples of the mixer 30 include a shredder, pin mill, bead mill, microparticle compounding device (a device that generates shear force between a specially shaped rotor rotating at high speed inside a tank and an impact plate), granulator, twin-screw extrusion mixer, planetary mixer, etc., preferably a shredder, microparticle compounding device, granulator, or twin-screw extrusion mixer. In the mixing step, the non-fibrous binder is dispersed on the surface of the negative electrode active material. Furthermore, if the binder contains a fibrous binder, the fibrous binder is fibrousized in the mixing step. The processing time for the mixing step is preferably within 60 minutes, for example, it can be set to 1 minute to 20 minutes.
[0051] Next, in the stretching step, as... Figure 3As shown in (b), the negative electrode composite material particles 12a are mixed and stretched using a pair of rollers 32 to form a sheet. The pair of rollers 32 are arranged with a predetermined gap and rotate in the same direction. The negative electrode composite material particles 12a are fed into the gap between the pair of rollers 32, thereby being compressed and stretched into a sheet by the pair of rollers 32. The linear pressure of the pair of rollers 32 is, for example, 0.1 t / cm to 3 t / cm. The pair of rollers 32 have, for example, the same roller diameter. The temperature of the pair of rollers 32 is not particularly limited, for example, it can be at room temperature or heated to above room temperature. It should be noted that the resulting negative electrode composite material 12b can also be passed between the pair of rollers 32 again. This improves the in-plane dispersion of the binder, but even if the number of passes is too many, it will damage the active material, so it should not be too many. The number of times the negative electrode composite material particles 12a and the negative electrode composite material 12b formed from the negative electrode composite material particles 12a are passed between the pair of rollers 32 is preferably 1 to 50 times, more preferably 1 to 40 times, and particularly preferably 1 to 10 times. The stretching step is not limited to using only one pair of rollers; it can also include stretching using another pair of rollers with different roller diameters, circumferential speeds, gaps, etc.
[0052] The thickness of the negative electrode composite material 12b obtained after the stretching step can be controlled, for example, by the gap between the pair of rollers 32, the circumferential speed, and the number of stretching processes. In the stretching step, it is preferable to use a pair of rollers 32 with a circumferential speed ratio differing by more than 1.1 times to form the negative electrode composite material particles 12a into sheets. By using a different circumferential speed ratio between the pair of rollers 32, for example, thin-film formation of the negative electrode composite material 12b becomes easier, improving productivity. The density of the negative electrode composite material 12b is, for example, 0.8 g / cm³. 3 ~2g / cm 3 .
[0053] Next, in the bonding step, such as Figure 4 As shown, by bonding the negative electrode composite material 12b to the negative electrode core material 11, a negative electrode 10 is obtained in which a composite material layer composed of the negative electrode composite material 12 is disposed on the surface of the negative electrode core material 11. Figure 4 The diagram shows a state where the negative electrode composite material 12 is bonded to only one side of the negative electrode core material 11, but it is preferable that the negative electrode composite material 12 is bonded to both sides of the negative electrode core material 11. Two negative electrode composite materials 12 can be bonded to both sides of the negative electrode core material 11 simultaneously, or one piece can be bonded to one side of the negative electrode core material 11 and the other piece can be bonded to the other side.
[0054] In the bonding step, a pair of rollers 34 are used to bond the negative electrode composite material 12b to the surface of the negative electrode core material 11. The pair of rollers 34, for example, have the same roller diameter, are arranged with a predetermined gap, and rotate in the same direction at the same circumferential speed. The temperature of the pair of rollers 34 is, for example, 25°C to 300°C. The linear pressure applied by the pair of rollers 34 is preferably 0.01 t / cm to 3 t / cm, more preferably 0.02 t / cm to 1 t / cm. It should be noted that an intermediate layer may be provided between the negative electrode core material 11 and the negative electrode composite material 12 in the negative electrode 10. The intermediate layer, for example, contains a conductive material and an adhesive, which improves the bonding strength of the negative electrode composite material 12 to the negative electrode core material 11 and reduces the interfacial resistance.
[0055] Non-aqueous electrolyte secondary batteries
[0056] The non-aqueous electrolyte secondary battery disclosed herein includes the aforementioned negative electrode 10, positive electrode, and non-aqueous electrolyte. By using the aforementioned negative electrode 10, the battery capacity of the non-aqueous electrolyte secondary battery is improved.
[0057] There are no particular limitations on the manufacturing method of the positive electrode in a non-aqueous electrolyte secondary battery; it can be either a dry method or a wet method. When using the dry method, the positive electrode can be manufactured using a non-fibrous binder, similar to the negative electrode 10, or it can be manufactured using a fibrous binder such as PTFE. The positive electrode core, positive electrode active material, and other components included in the positive electrode can be made from known materials.
[0058] Non-aqueous electrolyte secondary batteries possess non-aqueous electrolytes, such as those with lithium-ion conductivity. The non-aqueous electrolyte can be a liquid electrolyte (electrolyte) or a solid electrolyte.
[0059] Liquid electrolytes (electrolytes) may include, for example, a non-aqueous solvent and an electrolyte salt dissolved in the non-aqueous solvent. Non-aqueous solvents may include, for example, esters, ethers, nitriles such as acetonitrile, amides such as dimethylformamide, and mixtures of two or more of these. The non-aqueous solvent may contain halogen-substituted derivatives formed by substituting at least a portion of the hydrogen atoms of these solvents with halogen atoms such as fluorine. Examples of halogen-substituted derivatives include fluorocyclic carbonates such as fluoroethylene carbonate (FEC), fluorochain carbonates, and fluorochain carboxylic acid esters such as methyl fluoropropionate (FMP).
[0060] Examples of the aforementioned esters include cyclic carbonates such as ethylene carbonate (EC), propylene carbonate (PC), and butyl carbonate; chain carbonates such as dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), methyl propyl carbonate, ethyl propyl carbonate, and methyl isopropyl carbonate; cyclic carboxylic acid esters such as γ-butyrolactone (GBL) and γ-valerolactone (GVL); and chain carboxylic acid esters such as methyl acetate, ethyl acetate, propyl acetate, methyl propionate (MP), and ethyl propionate (EP).
[0061] Examples of the aforementioned ethers include 1,3-dioxolane, 4-methyl-1,3-dioxolane, tetrahydrofuran, 2-methyltetrahydrofuran, propylene oxide, 1,2-epoxybutane, 1,3-dioxane, 1,4-dioxane, 1,3,5-trioxane, furan, 2-methylfuran, 1,8-eucalyptol, crown ethers, cyclic ethers, 1,2-dimethoxyethane, diethyl ether, dipropyl ether, diisopropyl ether, dibutyl ether, and dihexyl ether. Ethyl vinyl ether, butyl vinyl ether, methyl phenyl ether, ethyl phenyl ether, butyl phenyl ether, pentyl phenyl ether, methoxytoluene, benzyl ethyl ether, diphenyl ether, dibenzyl ether, o-dimethoxybenzene, 1,2-diethoxyethane, 1,2-dibutoxyethane, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol dibutyl ether, 1,1-dimethoxymethane, 1,1-diethoxyethane, triethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether, and other chain ethers.
[0062] The preferred electrolyte salt is a lithium salt. Examples of lithium salts include LiClO4, LiBF4, LiPF6, LiAlCl4, LiSbF6, LiSCN, LiCF3SO3, LiCF3CO2, LiAsF6, and LiB. 10 Cl 10Examples of lithium salts include lower aliphatic carboxylic acids such as lithium Cl, LiBr, LiI, phosphates, borates, and imide salts. Examples of phosphates include lithium difluorophosphate (LiPO₂F₂), lithium difluorobis(oxalate)phosphate (LiDFBOP), and lithium tetrafluoro(oxalate)phosphate. Examples of borates include lithium bis(oxalate)borate (LiBOB) and lithium difluoro(oxalate)borate (LiDFOB). Examples of imide salts include lithium difluorosulfonylimide (LiN(FSO₂)₂), lithium bis(trifluoromethanesulfonylimide) (LiN(CF₃SO₂)₂), lithium trifluoromethanesulfonate nonafluorobutanesulfonate imide (LiN(CF₃SO₂)(C₄F₉SO₂)), and lithium bis(pentafluoroethanesulfonylimide) (LiN(C₂F₅SO₂)₂). Among these, LiPF₆ is preferred from the perspective of ionic conductivity and electrochemical stability. The concentration of lithium salt can be, for example, less than 4 moles per 1 L of non-aqueous solvent, less than 3 moles, preferably less than 1.8 moles, more preferably more than 0.8 moles and less than 1.8 moles.
[0063] Non-aqueous electrolytes may contain additives. Examples of additives include unsaturated carbonates, acid anhydrides, phenolic compounds, benzene compounds, nitrile compounds, isocyanate compounds, sulpholactone compounds, sulfuric acid compounds, borate ester compounds, phosphate ester compounds, and phosphite ester compounds.
[0064] Examples of unsaturated cyclic carbonates include vinylene carbonate, 4-methylvinylene carbonate, 4,5-dimethylvinylene carbonate, 4-ethylvinylene carbonate, 4,5-diethylvinylene carbonate, 4-propylvinylene carbonate, 4,5-dipropylvinylene carbonate, 4-phenylvinylene carbonate, 4,5-diphenylvinylene carbonate, vinylene carbonate, and divinylene carbonate. Unsaturated cyclic carbonates can be used alone or in combination of two or more. Some hydrogen atoms in the unsaturated cyclic carbonate can be replaced by fluorine atoms. The anhydride can be an anhydride formed by the intermolecular condensation of multiple carboxylic acid molecules, preferably an anhydride of a polycarboxylic acid. Examples of anhydrides of polycarboxylic acids include succinic anhydride, maleic anhydride, and phthalic anhydride.
[0065] Examples of phenolic compounds include phenol and hydroxytoluene. Examples of benzene compounds include fluorobenzene, hexafluorobenzene, and cyclohexylbenzene (CHB).
[0066] Examples of nitrile compounds include adiponitrile, heptanonitrile, propionitrile, and succinic anionyl. Examples of isocyanate compounds include methyl isocyanate (MIC), diphenylmethane diisocyanate (MDI), hexamethylene diisocyanate (HDI), toluene diisocyanate (TDI), isophorone diisocyanate (IPDI), and 1,3-bis(isocyanate methyl)cyclohexane (BIMCH). Examples of sulcolone compounds include propane sulcolone and propene sulcolone. Examples of sulfuric acid compounds include vinyl sulfate, vinyl sulfite, dimethyl sulfate, and lithium fluorosulfate. Examples of borate ester compounds include trimethyl borate and tri(trimethylsilyl) borate. Examples of phosphate ester compounds include trimethyl phosphate and tri(trimethylsilyl) phosphate. Examples of phosphite ester compounds include trimethyl phosphite and tri(trimethylsilyl) phosphite.
[0067] As a solid electrolyte, examples include solid or gel-like polymer electrolytes and inorganic solid electrolytes. As an inorganic solid electrolyte, materials known in all-solid-state lithium-ion secondary batteries (e.g., oxide-based solid electrolytes, sulfide-based solid electrolytes, halogen-based solid electrolytes, etc.) can be used. Polymer electrolytes may contain, for example, lithium salts and a matrix polymer, or non-aqueous solvents, lithium salts, and a matrix polymer. As a matrix polymer, for example, a polymer material that gels by absorbing non-aqueous solvents can be used. Examples of polymer materials include fluoropolymers, acrylic resins, and polyether resins. Example
[0068] The present disclosure is further illustrated below by way of examples, but the present disclosure is not limited to these examples.
[0069] <Example 1>
[0070] [Preparation of negative electrode composite material particles (mixing steps)]
[0071] As the negative electrode active material, a mixture of graphite and SiC at a mass ratio of 94:6 was used. This negative electrode active material and PVDF (model: 301F, primary particle size: 165 nm, secondary particle size: 5 μm) manufactured by Arkema were added to a mixer (Osaka Chemical, Wonder Crusher) at a mass ratio of 97:3 and mixed at room temperature for 5 minutes at a speed of 5 (scale 5). It should be noted that the speed of the Wonder Crusher is a maximum of 28,000 rpm at scale 10. This mixing process yielded a positive electrode composite material with uniformly dispersed negative electrode active material and PVDF. The solid content concentration of the obtained positive electrode composite material was 100%.
[0072] [Fabrication of Negative Electrode Composite Material (Stretching Step)]
[0073] The obtained negative electrode composite material particles were stretched twice between a pair of rollers heated to 160°C to produce sheet-like negative electrode composite materials. The circumferential speed ratio of the pair of rollers was set to 1:1.5, and the thickness of the negative electrode composite material was adjusted to approximately 140 μm.
[0074] [Making the negative electrode]
[0075] Using a negative electrode core with an intermediate layer composed of conductive material and adhesive formed on both sides, the resulting negative electrode composite material is placed on the surface of the negative electrode core. Two rollers are used to press the laminate of the negative electrode composite material and the negative electrode core (linear pressing: 0.1 t / cm, 140℃) to obtain the negative electrode (lamination step). It should be noted that copper foil is used as the negative electrode core.
[0076] For the obtained negative electrode, the composite material density, binder dispersion, and composite material strength were measured. The composite material density was 1.6 g / cm³. 3 The binder dispersion is 0.12, and the composite material strength is 340.9 gf.
[0077] [Preparation of non-aqueous electrolytes]
[0078] Ethyl carbonate (EC), ethyl methyl carbonate (EMC), and dimethyl carbonate (DMC) were mixed in a volume ratio of 3:3:4. Lithium hexafluorophosphate (LiPF6) was dissolved in this mixed solvent to a concentration of 1.2 mol / L to prepare a non-aqueous electrolyte.
[0079] [Fabrication of the Experimental Battery Cell]
[0080] A button cell is fabricated by using lithium metal foil as the positive electrode, overlapping the positive and negative electrodes with a non-woven fabric separator, and injecting the aforementioned non-aqueous electrolyte.
[0081] [Battery Capacity Evaluation]
[0082] For the obtained test battery cells, at a temperature of 25°C, they were charged with a constant current at 0.1C until the battery voltage reached 5mV (vs. Li), and then charged with a constant voltage at 5mV until the current value reached 0.01C. Then, they were discharged with a constant current of 0.1C until reaching 1000mV. This charge-discharge cycle was counted as one cycle, and three cycles were performed. The discharge capacity of the third cycle was taken as the battery capacity.
[0083] <Example 2>
[0084] In the preparation (mixing step) of the negative electrode composite material particles, the PVDF used was changed to PVDF manufactured by Arkema (model: 1810, primary particle size: 140 nm, secondary particle size: 15 μm). Otherwise, the negative electrode and test battery cell were prepared in the same manner as in Example 1 and evaluated.
[0085] <Example 3>
[0086] In the preparation (mixing step) of the negative electrode composite material particles, PTFE (particle size: 300 μm) was used as a binder in conjunction with PVDF. The negative electrode active material, PVDF and PTFE were mixed at a mass ratio of 97:1.5:1.5. Otherwise, the negative electrode and test battery cell were prepared in the same manner as in Example 1 and evaluated.
[0087] <Comparative Example 1>
[0088] The negative electrode was fabricated using a wet process. Except for this, the negative electrode and test battery cells were fabricated and evaluated in the same manner as in Example 1. Specifically, a negative electrode active material, polyacrylic acid (PAA), carboxymethyl cellulose (CMC), and styrene-butadiene rubber (SBR) were mixed in a solid content mass ratio of 97:1:1:1, and an appropriate amount of water was added to prepare a negative electrode composite slurry. This negative electrode composite slurry was coated onto both sides of a negative electrode core made of copper foil. After the coating dried, the coating was calendered using rollers to obtain a negative electrode with the negative electrode composite material formed on both sides of the negative electrode core.
[0089] <Comparative Example 2>
[0090] In the preparation (mixing step) of the negative electrode composite material particles, PTFE (particle size: 300 μm) was used instead of PVDF. Otherwise, the negative electrode and test cell were prepared in the same manner as in Example 1 and evaluated.
[0091] <Comparative Example 3>
[0092] In the preparation (mixing step) of the negative electrode composite material particles, the PVDF used was changed to Solvay PVDF (model: 5130, primary particle size: 150 μm). Otherwise, the negative electrode and test battery cell were prepared in the same manner as in Example 1 and evaluated.
[0093] The results of the composite material strength and battery capacity measured for the Examples and Comparative Examples are shown in Table 1. The battery capacities of Examples 1-3 and Comparative Examples 2-3 are relative values when the battery capacity of Comparative Example 1 is set to 100. In addition, Table 2 shows the content of binder in the first region (a), the content of binder in the second region (b), the content of binder in the third region (c), and the value of ((maximum value of a-c) - (minimum value of a-c)) / (a+b+c) for the Examples and Comparative Examples.
[0094] [Table 1]
[0095]
[0096] [Table 2]
[0097]
[0098] As shown in Table 1, the negative electrodes of Examples 1-3 have composite material strength and battery capacity equivalent to those of the negative electrode of Comparative Example 1, which was manufactured using a wet process. Furthermore, as shown in Table 2, in the negative electrodes of Examples 1-3, compared to the negative electrode of Comparative Example 1, the binder is also present in the electrode composite material in a substantially uniform manner throughout the thickness direction. On the other hand, the negative electrodes of Comparative Examples 2-3, where the binder dispersion in the negative electrode composite material is 1.2 or higher, show significantly worse composite material strength and battery capacity compared to the negative electrode of Comparative Example 1. Therefore, it can be seen that by including a non-fibrous binder in the negative electrode composite material and setting the binder dispersion in the negative electrode composite material to 0.01 or higher and 1.2 or lower, the strength and battery capacity of the negative electrode composite material are improved.
[0099] This disclosure is further illustrated by the following embodiments.
[0100] Option 1:
[0101] A negative electrode for a non-aqueous electrolyte secondary battery comprises a negative electrode core material and a negative electrode composite material laminated on the surface of the negative electrode core material.
[0102] The negative electrode composite material contains a negative electrode active material and a binder that binds the negative electrode active material together.
[0103] The binder comprises a non-fibrous binder, and its dispersion in the negative electrode composite material is greater than 0.01 and less than 1.2.
[0104] When the negative electrode composite material is divided into three equal parts along its thickness direction, designated as a first region, a second region, and a third region from the core material side, and the binder content in the first region, the second region, and the third region is designated as a, b, and c, respectively,
[0105] The value obtained by subtracting the minimum value of a to c from the maximum value of a to c is less than 5% of the total value of a to c.
[0106] Option 2:
[0107] According to Scheme 1, the negative electrode for a non-aqueous electrolyte secondary battery, wherein the non-fibrous binder comprises PVDF.
[0108] Option 3:
[0109] The negative electrode for a non-aqueous electrolyte secondary battery according to Scheme 1 or 2, wherein the binder further comprises PTFE.
[0110] Option 4:
[0111] The negative electrode for a non-aqueous electrolyte secondary battery according to any one of Schemes 1 to 3, wherein the negative electrode active material comprises a Si-containing material.
[0112] Option 5:
[0113] According to any one of Schemes 1 to 4, the content of the non-fibrous binder in the negative electrode composite material is 0.1% by mass or more and 5% by mass or less relative to the total mass of the negative electrode active material.
[0114] Option 6:
[0115] The negative electrode for a non-aqueous electrolyte secondary battery according to any one of Schemes 1 to 5, wherein the strength of the negative electrode composite material is 200 gf or higher.
[0116] Option 7:
[0117] A non-aqueous electrolyte secondary battery, comprising:
[0118] The negative electrode for a non-aqueous electrolyte secondary battery as described in any one of Schemes 1 to 6;
[0119] Positive electrode; and
[0120] Non-aqueous electrolyte.
[0121] Explanation of reference numerals in the attached figures
[0122] 10 Negative electrode, 11 Negative electrode core material, 12 Negative electrode composite material, 12a Electrode composite material particles, 12b Electrode composite material sheet, 20 Negative electrode active material, 22 Non-fibrous binder, 30 Mixer, 32, 34 Rollers.
Claims
1. A negative electrode for a non-aqueous electrolyte secondary battery, comprising a negative electrode core material and a negative electrode composite material laminated on the surface of the negative electrode core material. The negative electrode composite material contains a negative electrode active material and a binder that binds the negative electrode active material together. The binder comprises a non-fibrous binder, and its dispersion in the negative electrode composite material is greater than 0.01 and less than 1.
2. When the negative electrode composite material is divided into three equal parts in the thickness direction, and designated as a first region, a second region, and a third region from the side of the negative electrode core material, and the content of the binder in the first region, the second region, and the third region is designated as a, b, and c, respectively, The value obtained by subtracting the minimum value of a to c from the maximum value of a to c is less than 5% of the total value of a to c.
2. The negative electrode for a non-aqueous electrolyte secondary battery according to claim 1, wherein, The non-fibrous adhesive contains PVDF.
3. The negative electrode for a non-aqueous electrolyte secondary battery according to claim 1, wherein, The adhesive also contains PTFE.
4. The negative electrode for a non-aqueous electrolyte secondary battery according to claim 1, wherein, The negative electrode active material contains Si.
5. The negative electrode for a non-aqueous electrolyte secondary battery according to claim 1, wherein, The content of the non-fibrous binder in the negative electrode composite material is more than 0.1% by mass and less than 5% by mass relative to the total mass of the negative electrode active material.
6. The negative electrode for a non-aqueous electrolyte secondary battery according to claim 1, wherein, The strength of the negative electrode composite material is above 200 gf.
7. A non-aqueous electrolyte secondary battery, comprising: The negative electrode for a non-aqueous electrolyte secondary battery according to any one of claims 1 to 6; Positive electrode; and Non-aqueous electrolyte.
Citation Information
Patent Citations
Compositions and methods for energy storage devices with improved performance