Positive electrode and secondary battery comprising the same

By using overlithiation compounds and metal oxide additives with specific chemical formulas in the positive electrode of lithium secondary batteries, the problems of lithium consumption and oxygen generation have been solved, thereby improving the safety and cycle characteristics of high-capacity batteries.

CN123165697APending Publication Date: 2026-11-24LG ENERGY SOLUTION LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202680003551.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2025-02-07
Filing Date
2026-01-26
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing high-capacity lithium secondary batteries consume a large amount of lithium during the initial charge and discharge process, resulting in severe irreversible capacity loss. Furthermore, when Li₅FeO₄ is used as a positive electrode additive, it generates oxygen, affecting battery safety and cycle characteristics.

Method used

The cathode structure comprises first and second cathode additives, the first cathode additive comprising a perlithiated compound represented by chemical formula 2, and the second cathode additive comprising a metal oxide represented by chemical formula 1. Lithium loss is compensated and oxygen is removed by adjusting the particle size and content. The first layer also comprises conductive material and binder to enhance bonding strength and conductivity.

Benefits of technology

It effectively compensates for the initial irreversible capacity loss, improves the battery's charge and discharge capacity and safety, and enhances the battery's cycle characteristics and lifespan.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

This invention relates to a positive electrode and a secondary battery comprising the positive electrode. The positive electrode comprises a perlithiated compound represented by chemical formula 2, which compensates for the irreversible capacity loss generated at the negative electrode during the initial charge and discharge process and improves the conductivity degradation caused by the compound, thereby exhibiting excellent charge and discharge capacity characteristics. Furthermore, since the positive electrode suppresses oxygen generation during charge and discharge, the secondary battery comprising this positive electrode not only has high safety but also excellent cycle characteristics and lifespan.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a positive electrode and a secondary battery containing the positive electrode.

[0002] This application claims priority to Korean Patent Application No. 10-2025-0016196, filed on February 7, 2025, the entire contents of which are incorporated herein by reference. Background Technology

[0003] In recent years, lithium-ion batteries have been widely used not only in small devices such as portable electronic devices, but also in medium and large-sized devices such as battery packs or energy storage systems for hybrid and electric vehicles. In particular, with increasing attention to environmental issues, the demand for high-capacity batteries is expanding, consistent with the market growth for devices using high-capacity batteries (such as electric vehicles and hybrid electric vehicles, which can replace fossil fuel-powered vehicles such as gasoline and diesel vehicles, which are major contributors to air pollution). As a power source for these devices, high-capacity electrode designs are required to manufacture lithium-ion batteries with high energy density, high output, and high discharge voltage.

[0004] Research directions for increasing the capacity of such lithium secondary batteries include various methods such as using non-carbon anode materials such as silicon, which have a higher energy density than graphite, developing and using novel cathode materials, or developing lithium metal batteries that use lithium metal as the anode.

[0005] However, these high-capacity lithium-ion batteries suffer from significant lithium consumption and irreversible capacity loss during the initial charge and discharge processes. More specifically, during the initial charge and discharge of a lithium-ion battery, lithium ions migrate to the negative electrode and trigger side reactions, forming an SEI layer. High-capacity lithium-ion batteries consume a particularly large amount of lithium to form this SEI layer, thus leading to increased irreversible capacity loss.

[0006] In existing technologies, methods such as pre-lithiation or the application of lithium alloys have been considered to compensate for lithium-ion consumption and irreversible capacity loss; however, these methods have been found to be difficult to apply to the manufacture of commercial batteries. Therefore, in recent years, the most widely used method has been to add overlithiated metal oxides as additives to conventional positive electrode active materials to compensate for the irreversible capacity loss of the negative electrode.

[0007] Various materials are known as positive electrode additives, such as Li2NiO2, Li6CoO4 and Li5FeO4. Among them, the application of Li5FeO4 is being widely studied due to its relatively low cost.

[0008] However, Li5FeO4 has low conductivity, which may prevent it from adequately compensating for irreversible capacity. Consequently, the need for large amounts of Li5FeO4 to compensate for the significant irreversible capacity in high-capacity next-generation lithium-ion batteries presents a limitation. Furthermore, even after the initial charge-discharge cycle, Li5FeO4 remains in the positive electrode active layer, generating substantial amounts of oxygen (O2). This oxygen increases the internal pressure of the battery cell, potentially causing deformation and / or damage to the battery casing during use, thus degrading battery safety. Additionally, oxygen can form gas traps at the interface between the positive and / or negative electrodes, interfering with electrochemical reactions or damaging the active layers of each electrode, thereby contributing to reduced cycle and lifespan characteristics of the secondary battery. Therefore, the commercialization of Li5FeO4 has been delayed.

[0009] [Existing technical documents]

[0010] [Patent Literature]

[0011] Korean Patent Application Publication No. 10-2023-0057858 Summary of the Invention

[0012] Technical issues

[0013] The purpose of this invention is to provide a positive electrode that can compensate for the initial irreversible capacity loss of the negative electrode while having improved lifetime and cycle characteristics, as well as a secondary battery containing the positive electrode.

[0014] Technical solution

[0015] To solve the above problems, This invention provides a positive electrode comprising: Positive current collector; A first layer, wherein the first layer is disposed on at least one surface of the positive electrode current collector, and comprises a first positive electrode additive and a second positive electrode additive; and The second layer is disposed on the first layer and contains a positive electrode active material. The first positive electrode additive includes a compound whose activation voltage range overlaps with the working voltage range of the positive electrode active material by more than 50%, based on the working voltage of the positive electrode active material. The second positive electrode additive comprises one or more compounds represented by the following chemical formula 1, and Wherein, the average particle size of the second positive electrode additive is smaller than the average particle size of the first positive electrode additive: [Chemical Formula 1] M 1 x M 2y O z (In chemical formula 1, M 1 and M 2 Each of the following is a given element: Li, W, Mo, Ni, Co, Nb, Ge, Ti, Ta, or Ce, provided that M is present. 1 and M 2 Including different metals, and x, y, and z are 1≤x≤3, 0≤y≤1, and 1≤z≤6, respectively.

[0016] At this time, the average particle size (D) of the first positive electrode additive 50 The diameter can range from 0.5 μm to 20 μm.

[0017] The ratio of the average particle size of the second positive electrode additive to the average particle size of the first positive electrode additive can be greater than 0.5 and less than 1.0.

[0018] The first positive electrode additive may include one or more compounds represented by the following chemical formula 2: [Chemical Formula 2] Li a M 3 (1-b) M 4 b O c In chemical formula 2, M 3 It is Fe, Co, Mn, Zn, Al or Ga, M 4 M is at least one metal selected from W, Cu, Fe, V, Cr, Ti, Zr, Zn, Co, Al, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B, and Mo, provided that M is a metal selected from W, Cu, Fe, V, Cr, Ti, Zr, Zn, Co, Al, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B, and Mo. 3 and M 4 Including different metals, and a, b, and c are 1≤a≤7, 0≤b≤0.5, and 1.8≤c≤4.5, respectively.

[0019] Based on the total weight of the first layer and the second layer, the content of the first cathode additive can be from 0.5% by weight to 5% by weight.

[0020] Based on the total weight of the first cathode additive, the content of the second cathode additive can be from 5% by weight to 25% by weight.

[0021] The first layer may further comprise a third positive electrode additive, which includes at least one of the following: metal carbonates; metal halides; photosensitive dyes; unsaturated hydrocarbons; polymers having repeating units containing amide groups; catechols; sulfites; ascorbic acid derivatives; and enzymes.

[0022] At this time, the metal carbonate or the metal halide may contain at least one metal selected from iron (Fe), cobalt (Co), nickel (Ni) and copper (Cu).

[0023] Based on 100 parts by weight of the first cathode additive, the content of the third cathode additive can be from 1 part by weight to 25 parts by weight.

[0024] The average thickness of the first layer can be from 1 μm to 30 μm.

[0025] The ratio of the average thickness of the first layer to the average thickness of the second layer can be from 0.05 to 1.

[0026] The first layer may also contain a positive electrode active material.

[0027] The positive electrode active material contained in the first layer and the second layer respectively may include lithium iron phosphate compounds represented by the following chemical formula 3: [Chemical Formula 3] LiFe r M 5 (1-r) XO4 (in chemical formula 3, M 5 It is at least one element selected from W, Cu, Fe, V, Cr, Co, Ni, Mn, Ti, Zr, Zn, Al, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B, and Mo. X is at least one element selected from P, Si, S, As, and Sb, and (r is 0 ≤ r ≤ 0.9).

[0028] This invention provides a secondary battery comprising: An electrode assembly comprising a positive electrode, a negative electrode, and a separator sandwiched between the positive and negative electrodes, as described above; and An electrolyte composition, wherein the electrolyte composition impregnates the electrode assembly.

[0029] At this time, the negative electrode may include: a negative electrode active layer containing a carbon-based negative electrode active material on at least one surface of the negative electrode current collector.

[0030] The negative electrode active layer may further contain materials selected from Si, SiC, and SiO. q One or more silicon-based anode active materials (where 0.5≤q≤2.5).

[0031] Beneficial effects

[0032] The positive electrode of the present invention contains a perlithiated compound represented by Chemical Formula 2, thus compensating for the irreversible capacity loss generated at the negative electrode during the initial charge and discharge process, and improving the conductivity degradation caused by the compound, thereby exhibiting excellent charge and discharge capacity characteristics. Furthermore, since this positive electrode suppresses the generation of oxygen and other substances during charge and discharge after the initial charge and discharge, the secondary battery containing this positive electrode not only has high safety but also excellent cycle characteristics and lifespan. Detailed Implementation

[0033] This invention can have various modifications and implementations, the specific implementations of which will be described in detail below.

[0034] The terms “comprising,” “including,” or “having” as used herein specify the presence of a feature, number, step, action, component, or part or combination thereof described in the specification, and it should be understood that the possibility of the presence or addition of more than one other feature, number, step, action, component, part or combination thereof is not excluded in advance.

[0035] In this specification, "comprising as a major component" can mean that, based on the total weight (or total volume), the defined component contains 50% by weight or more (or 50% by volume), 60% by weight or more (or 60% by volume), 70% by weight or more (or 70% by volume), 80% by weight or more (or 80% by volume), 90% by weight or more (or 90% by volume), or 95% by weight or more (or 95% by volume). For example, "containing carbon atoms as a major component" can mean that, based on the total weight of the carbonaceous compound, its content is 50% by weight or more, 60% by weight or more, 70% by weight or more, 80% by weight or more, 90% by weight or more, or 95% by weight or more. In some cases, it can also mean that the entire carbonaceous compound is composed of carbon atoms, i.e., containing 100% by weight.

[0036] Furthermore, in this specification, "average particle size (D)" 50 "Median diameter" refers to the particle size that accounts for 50% of the total particle size distribution, also known as the median particle size. Average particle size (D) 50 The average particle size (D) can be measured using methods such as laser diffraction. 50The average particle size (D) can be calculated as follows: Particles are dispersed in a dispersion medium, introduced into a commercially available laser diffraction particle size analyzer (e.g., Microtrac MT 3000), irradiated with ultrasound at approximately 28 kHz and 60 W output, and the average particle size corresponding to 50% of the cumulative volume is calculated from the results measured by the measuring device. 50 Laser diffraction can typically measure particle sizes from the submicron region to several millimeters, and can obtain highly reproducible and high-resolution results.

[0037] The present invention will now be described in more detail.

[0038] positive electrode

[0039] This invention provides a positive electrode comprising: Positive current collector; The first layer is disposed on at least one surface of the positive electrode current collector and comprises a first positive electrode additive and a second positive electrode additive; and The second layer is disposed on the first layer and contains the positive electrode active material.

[0040] The positive electrode of this invention can be applied to lithium secondary batteries. The positive electrode can have a structure in which a first layer and a second layer are sequentially arranged on the positive electrode current collector.

[0041] At this point, the first layer can function as a functional layer that improves or enhances the physical properties of the positive electrode. For example, the first layer can be located between the second layer and the positive electrode current collector, acting as a primer layer to enhance the bonding strength between them. In addition, the first layer can compensate for lithium loss caused by the negative electrode during the initial charging of the secondary battery, or it can remove oxygen (O2) generated during the charging and discharging of the secondary battery after the initial charging and discharging.

[0042] The first layer can have a patterned structure to enhance the bonding strength between the positive electrode current collector and the second layer. At this time, there are no particular restrictions on the patterned structure, as long as it can increase the surface area of ​​the first layer; however, considering the productivity and processability in the positive electrode manufacturing process, the patterned structure can have a striped patterned structure or a dotted patterned structure.

[0043] In addition, to compensate for the lithium lost during the initial charge and discharge process, the first layer, as the first positive electrode additive, may include a compound whose activation voltage range overlaps with the working voltage range of the positive electrode active material by more than 50%.

[0044] Specifically, the first positive electrode additive may include one or more compounds represented by the following chemical formula 2: [Chemical Formula 2] Li a M 3 (1-b) M 4 b O c In chemical formula 2, M 3 It is Fe, Co, Mn, Zn, Al or Ga, M 4 M is at least one metal selected from W, Cu, Fe, V, Cr, Ti, Zr, Zn, Co, Al, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B, and Mo, provided that M is a metal selected from W, Cu, Fe, V, Cr, Ti, Zr, Zn, Co, Al, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B, and Mo. 3 and M 4 Including different metals, and a, b, and c are 1≤a≤7, 0≤b≤0.5, and 1.8≤c≤4.5, respectively.

[0045] The compound represented by chemical formula 2 is a perlithiated compound containing excess lithium and can compensate for irreversible lithium loss by releasing additional lithium during the initial charging process.

[0046] The compound represented by chemical formula 2 can be alone or in combination of two or more, including Li6CoO4, Li6Co 0.5 Zn 0.5 O4, Li6Co 0.7 Zn 0.3 O4, Li6Co 0.7 Zn 0.2 Al 0.1 Examples of compounds represented by formula 2 include O4, Li5FeO4, Li6MnO4, Li6ZnO4, Li5AlO4, and Li5GaO4. For instance, compounds represented by formula 2 may include Li6CoO4 and Li6Co. 0.5 Zn 0.5 O4, Li6Co 0.7 Zn 0.3 O4, Li6Co 0.7 Zn 0.2 Al 0.1 O4, Li5FeO4, Li5Fe 0.7 Mn 0.3 O4, Li5Fe 0.5 Mn 0.5 At least one of O4 and Li6MnO4, wherein M 3 It can be Fe, Co, or Mn.

[0047] These compounds release a significantly larger amount of lithium ions during secondary battery charging, thus compensating for lithium ion losses even with small amounts. Furthermore, these compounds are readily applicable to lithium-ion secondary batteries because the minimum potential required for lithium release, i.e., the activation voltage (or decomposition voltage), exists within the charging potential range of lithium-ion secondary batteries. Specifically, the first positive electrode additive decomposes during the initial charge-discharge process due to structural instability, releasing lithium ions, which compensate for the lithium lost by the secondary battery during the initial charge-discharge process.

[0048] At this point, the degree of lithium-ion compensation can vary depending on the overlap between the activation voltage (the minimum potential at which the first cathode additive is decomposed) and the operating voltage of the cathode active material receiving lithium compensation. Therefore, the first cathode additive of the present invention may include a compound represented by Chemical Formula 2, such that its activation voltage range overlaps with the operating voltage range of the cathode active material by more than 50%. Specifically, based on the operating voltage range of the cathode active material, the overlap ratio between the activation voltage range of the first cathode additive and the operating voltage range of the cathode active material can be 60% or more, 70% or more, 80% or more, 50% to 95%, 50% to 90%, 60% to 85%, or 65% to 85%. If the overlap ratio between the activation voltage range of the first cathode additive and the operating voltage range of the cathode active material is lower than the aforementioned lower limit, the first cathode additive cannot be sufficiently decomposed during the initial charge and discharge process, resulting in the problem that the charge and discharge capacity of the secondary battery cannot be fully realized. Furthermore, if the overlap ratio is higher than the aforementioned upper limit, the side reactions caused by the first cathode additive increase, which may reduce the electrochemical performance and / or safety of the secondary battery.

[0049] For example, when LiFePO4 with an operating voltage range of approximately 3.2 to 3.6 V is used as the positive electrode active material, Li6CoO4 with an activation voltage of approximately 3.7 to 4.2 V does not have an overlapping voltage range; however, based on the operating voltage of the positive electrode active material, Li5FeO4 with an activation voltage of approximately 3.3 to 3.8 V can overlap with the operating voltage by approximately 73 to 77%. Therefore, Li5FeO4 can be included as the first positive electrode additive.

[0050] In secondary batteries using LiFePO4 and other materials as positive electrode active materials, Li5FeO4 exhibits excellent compatibility with the positive electrode active material. Due to the high overlap ratio of the operating voltage ranges of Li5FeO4 and LiFePO4, it is characterized by high positive electrode charge-discharge performance after the initial charge-discharge cycle. Furthermore, Li5FeO4 has a relatively low cost compared to other over-lithiation compounds, thus offering excellent economic efficiency.

[0051] Meanwhile, the first positive electrode additive has low conductivity, thus preventing the full realization of the positive electrode's charge-discharge capacity when applied. However, the present invention is characterized by the fact that, since the first positive electrode additive is contained in the first layer adjacent to the positive electrode current collector, the charge transfer distance achieved from the first positive electrode additive is shortened, thereby improving the problem of charge-discharge capacity degradation of the positive electrode. Furthermore, over-lithiation compounds generally have low structural stability and may be damaged under high temperature and / or high pressure conditions, causing them to lose function. In this case, a rolling process is performed during the positive electrode manufacturing process to increase energy density. In this situation, since the first layer may be subjected to relatively less compressive stress during the rolling process compared to the second layer, it has the advantage of significantly reducing damage to the first positive electrode additive.

[0052] Based on the total weight of the first and second layers, the content of the first cathode additive can be from 0.5 wt% to 5 wt%. For example, based on the total weight of the first and second layers, the content of the first cathode additive can be from 0.5 wt% to 4 wt%; 0.5 wt% to 3 wt%; 0.5 wt% to 2 wt%; 0.5 wt% to 1 wt%; 1 wt% to 5 wt%; 2.5 wt% to 5 wt%; 1 wt% to 4 wt%; 1 wt% to 3 wt%; 2 wt% to 4 wt%; 0.5 wt% to 1.3 wt%; or 0.5 wt% to 0.9 wt%. This invention controls the content of the first cathode additive within the above range, thereby preventing capacity degradation due to insufficient replenishment of lithium ions lost through irreversible reactions when the content of the first cathode additive is low. Furthermore, it prevents the generation of large amounts of oxygen during battery charging and discharging due to excessive first cathode additive.

[0053] Furthermore, the compounds represented by chemical formula 2 may include LiFeO2 and Li3FeO. 3.5 At least one of Li5FeO4 and Li3FeO4. When the compound represented by Formula 2 is Li5FeO4, after the initial charging of the secondary battery, Li5FeO4 may remain in the first layer in the form of decomposition products remaining after the release of additional lithium ions and oxygen (O2). In this case, when the secondary battery is charged at a charging voltage in the range of 3.5 V to 4.0 V, the decomposition products of Li5FeO4 may include LiFeO2, Li3FeO4, and Li3FeO4. 3.5 Furthermore, when the secondary battery is charged at a charging voltage above 4.0 V, the decomposition products of Li5FeO4 may include Li3FeO4, etc. Since LiFeO2 has a structure capable of intercalating and deintercalating lithium ions, it can participate in the electrochemical reactions in the first layer during the charging and discharging process of the secondary battery. Furthermore, since Li3FeO... 3.5 Li3FeO4 and other compounds retain spare lithium ions, which can contribute to the charge-discharge capacity of the cathode after the initial charge-discharge / activation.

[0054] When the first cathode additive comprises Li5FeO4 and LiFeO2, they can have a predetermined content ratio. Specifically, when the first cathode additive comprises Li5FeO4 and LiFeO2, the content of LiFeO2 relative to 1 part by weight of Li5FeO4 can be from 10 parts by weight to 500 parts by weight. For example, the content of LiFeO2 relative to 1 part by weight of Li5FeO4 can be from 10 parts by weight to 250 parts by weight; from 10 parts by weight to 100 parts by weight; from 10 parts by weight to 50 parts by weight; from 50 parts by weight to 200 parts by weight; from 100 parts by weight to 300 parts by weight; from 250 parts by weight to 500 parts by weight; from 50 parts by weight to 100 parts by weight; from 10 parts by weight to 30 parts by weight; from 20 parts by weight to 30 parts by weight; from 10 parts by weight to 19 parts by weight; or from 11 parts by weight to 29 parts by weight. This invention controls the content ratio of Li5FeO4 and LiFeO2 contained in the first positive electrode additive within the aforementioned range, thereby preventing a sharp increase in the resistance of the positive electrode due to a high LiFeO2 content ratio. Furthermore, a high Li5FeO4 content ratio can prevent insufficient compensation for irreversible lithium loss caused by the negative electrode, thus preventing degradation of the positive electrode's charge / discharge capacity.

[0055] Considering the reactivity of the compound represented by chemical formula 2 during the initial charging process, the first positive electrode additive can have a predetermined average particle size (D). 50 1st Specifically, the average particle size (D) of the first cathode additive 50 1st The average particle size (D) of the first cathode additive can range from 0.5 μm to 20 μm. For example, the average particle size of the first cathode additive (D...) 50 1st The micrometers can be 0.5 μm to 18 μm; 0.5 μm to 15 μm; 0.5 μm to 12 μm; 0.5 μm to 10 μm; 0.5 μm to 5 μm; 0.5 μm to 3 μm; 1 μm to 9 μm; 5 μm to 20 μm; 5 μm to 15 μm; 5 μm to 13 μm; 8 μm to 19 μm; 9 μm to 15 μm; 10 μm to 20 μm; 10 μm to 15 μm; 7 μm to 14 μm; or 8 μm to 12 μm.

[0056] This invention increases the average particle size (D) of the first positive electrode additive 50 1stThe average particle size is controlled within the aforementioned range to prevent a large amount of unreacted compounds represented by Formula 2 from remaining after the initial charge / discharge / activation due to the average particle size exceeding the aforementioned upper limit. Compounds represented by Formula 2 remaining after the initial charge / discharge / activation may act as a factor in the generation of gas during the release of lithium ions during charge / discharge. The generated gas may increase the internal pressure of the secondary battery, thereby compromising its safety. Therefore, it is preferable to control the average particle size (D) within the aforementioned range to prevent the residue of unreacted compounds represented by Formula 2 after the initial charge / discharge / activation. 50 1st The particle size is controlled to be equal to or below the aforementioned upper limit, so that all or most of the compounds represented by Formula 2 can participate in the irreversible reaction during the initial charge / discharge / activation process. Furthermore, this invention minimizes the impact of average particle size (D) on the overall particle size distribution. 50 1st The amount of loss caused by the uneven dispersion or distribution of the first cathode additive in the first layer during the cathode manufacturing process, which is less than the aforementioned lower limit.

[0057] In addition to the first positive electrode additive, the first layer also includes a second positive electrode additive, which comprises at least one compound represented by the following chemical formula 1: [Chemical Formula 1] M 1 x M 2 y O z In chemical formula 1, M 1 and M 2 Each of the following is a given element: Li, W, Mo, Ni, Co, Nb, Ge, Ti, Ta, or Ce, provided that M is present. 1 and M 2 Including different metals, and x, y, and z are 1≤x≤3, 0≤y≤1, and 1≤z≤6, respectively.

[0058] The first positive electrode additive releases additional lithium during the charging process of the secondary battery, and in doing so, generates a considerable amount of oxygen (O2). Furthermore, the first positive electrode additive remaining in the positive electrode active layer after the initial charge-discharge and / or its decomposed oxides may continue to decompose during subsequent charge-discharge cycles, generating additional oxygen (O2). This generated oxygen (O2) increases the internal pressure of the battery cell, which may cause deformation and / or damage to the battery casing during secondary battery use, thereby degrading battery safety. In addition, oxygen may form gas traps at the interface between the positive and / or negative electrodes, interfering with the electrochemical reactions of the electrodes or damaging the active layers of each electrode, thus acting as a factor that reduces the cycle characteristics and lifespan of the secondary battery. However, the present invention overcomes this problem by including a second positive electrode additive in the first layer of the positive electrode.

[0059] The second cathode additive comprises one or more compounds represented by Formula 1. The compounds represented by Formula 1 include oxides of a single metal and / or dissimilar metals with oxidation states of +2 to +6. Under voltage conditions in the range of 2.0 to 4.0 V, these compounds can undergo metal element transformation due to activation by redox reactions during the charging and discharging of the secondary battery. In this process, the metal element in the metal oxide can react with oxygen ions. That is, the metal element can be oxidized by reacting with oxygen ions, thereby capturing and / or removing oxygen (O2) generated inside the cathode and / or the battery. Examples of such second cathode additives include WO, WO2, WO3, MoO, MoO2, MoO3, NiO, NiO2, CoO, CoO2, NbO, NbO2, Nb2O5, GeO, GeO2, TiO, TiO2, TaO, Ta2O5, CeO2, NbTiO2, NbTiO5, NbTaO2, NbTaO5, Li2NiO2, or combinations thereof.

[0060] There is no limitation on the size of the second positive electrode additive; however, its average particle size is preferably smaller than that of the first positive electrode additive. In this case, the second positive electrode additive has a larger specific surface area than the first positive electrode additive that generates oxygen, and therefore can effectively remove oxygen (O2) generated in the first layer during the charging and discharging process of the secondary battery (especially during the initial charging and discharging process).

[0061] The average particle size (D) of the second cathode additive 50 2nd ) relative to the average particle size (D) of the first cathode additive 50 1st The size ratio can be greater than 0.5 and less than 1.0. For example, based on the average particle size (D) of the first cathode additive... 50 1st The average particle size (D) of the second cathode additive 50 2nd The size ratio can be 0.6 or more and less than 1.0; 0.7 or more and less than 1.0; 0.8 or more and less than 1.0; 0.9 or more and less than 1.0; 0.5 to 0.95; 0.5 to 0.9; 0.5 to 0.75; 0.5 to 0.6; 0.7 to 0.95; 0.8 to 0.95; 0.6 to 0.8; 0.75 to 0.9; or 0.8 to 0.9. The present invention uses the average particle size (D) of the second positive electrode additive. 50 2nd ) and the average particle size (D) of the first positive electrode additive 50 1stThe ratio of the first positive electrode additive to the second positive electrode additive is controlled within the aforementioned range, thereby more effectively adsorbing and removing oxygen generated in the first layer due to the first positive electrode additive. Specifically, when the average particle size ratio of the second positive electrode additive exceeds the aforementioned upper limit, it may gain electrons during charging and discharging, which may instead promote the generation of oxygen (O2). Furthermore, when the average particle size ratio of the second positive electrode additive is below the aforementioned lower limit, the specific surface area of ​​the second positive electrode additive increases, but the second positive electrode additive is not uniformly dispersed in the first layer during the positive electrode manufacturing process. In this case, there is a problem of reduced removal efficiency of oxygen generated not only in the first layer but also inside the battery.

[0062] Based on the total weight of the first cathode additive, the content of the second cathode additive can be from 5% to 25% by weight. For example, based on the total weight of the first cathode additive, the content of the second cathode additive can be from 5% to 20% by weight; 5% to 15% by weight; 5% to 10% by weight; 10% to 25% by weight; 15% to 25% by weight; 20% to 25% by weight; 10% to 20% by weight; 11% to 25% by weight; 13% to 24% by weight; 11% to 19% by weight; or 8% to 17% by weight. This invention controls the content of the second cathode additive within the above range, thereby more effectively removing oxygen generated during the charging and discharging of the secondary battery without degrading the energy density and cycle characteristics of the cathode.

[0063] The second positive electrode additive is uniformly dispersed together with the first positive electrode additive in the first layer, thereby effectively removing oxygen (O2) generated inside the positive electrode without degrading the charge-discharge characteristics and / or lifetime characteristics of the positive electrode. This contrasts with the case where the first positive electrode additive is coated with the second positive electrode additive. The first positive electrode additive generally has very low conductivity. When the second positive electrode additive is coated on the surface of the first positive electrode additive, the conductivity of the first positive electrode additive is further reduced, thus presenting a limitation of degrading the charge-discharge characteristics and / or lifetime characteristics of the positive electrode containing the aforementioned additive.

[0064] In addition to the second cathode additive, the first layer may also contain additional additives with a high affinity for oxygen (O2), such as metal compounds, organic compounds, and polymer compounds. Specifically, the first layer may also contain a third cathode additive, which includes at least one of the following: metal carbonates; metal halides; photosensitive dyes; unsaturated hydrocarbons; polymers having repeating units containing amide groups; catechols; sulfites; ascorbic acid derivatives; and enzymes. The third cathode additive is a compound with a high affinity for oxygen (O2), and when used together with the second cathode additive, it can further maximize the efficiency of removing oxygen (O2) generated inside the cathode.

[0065] The third cathode additive may include the following compounds: - Metal carbonates, such as iron carbonate (FeCO3); - Metal halides, such as cobalt chloride (CoCl2), cobalt bromide (CoBr2), cobalt iodide (CoI2), ferric chloride (FeCl2), ferric bromide (FeBr2), ferric iodide (FeI2), nickel chloride (NiCl2), nickel bromide (NiBr2), nickel iodide (NiI2), copper chloride (CuCl2), copper bromide (CuBr2), and copper iodide (CuI2); - Photosensitive dyes, such as quercetin, luteolin, beta-carotene, lycopene, astaxanthin, HEME derivatives, chlorophyll derivatives, phthalocyanine derivatives, coumarin derivatives, indigo and indirubin; - Unsaturated hydrocarbons, such as carotenoids, resveratrol, curcumin, tocopherol, squalene, and fullerenes (C60, C70, etc.); - Polymers having repeating units containing amide groups, such as nylon-6 and nylon-66; - Catechins, such as epicatechin, epigallocatechin gallate (EGCG), dopamine, pyrogallol and hydroquinone; - Sulfites, such as sodium sulfite (Na2SO3), sodium metabisulfite (Na2S2O5), and potassium metabisulfite (K2S2O5); - Ascorbic acid derivatives, such as ascorbic acid, and ascorbates containing sodium bicarbonate (ascorbates containing NaHCO3); - Enzymes, such as glucose oxidase, superoxide dismutase (SOD), catalase (CAT), glutathione peroxidase (GPx), hemoglobin (Hb), myoglobin (Mb), tyrosinase, and lipoxygenase (LOX).

[0066] Based on 100 parts by weight of the first cathode additive, the content of the third cathode additive can be from 1 part by weight to 25 parts by weight. For example, based on 100 parts by weight of the first cathode additive, the content of the third cathode additive can be from 1 part by weight to 20 parts by weight; 1 part by weight to 15 parts by weight; 1 part by weight to 10 parts by weight; 10 parts by weight to 25 parts by weight; 15 parts by weight to 25 parts by weight; 20 parts by weight to 25 parts by weight; 10 parts by weight to 20 parts by weight; 11 parts by weight to 22 parts by weight; 13 parts by weight to 24 parts by weight; 11 parts by weight to 19 parts by weight; 8 parts by weight to 17 parts by weight; 1 part by weight to 9 parts by weight; 1 part by weight to 5 parts by weight; or 1 part by weight to 3 parts by weight. This invention controls the content of the third cathode additive within the above ranges, thereby more effectively removing oxygen generated during the charging and discharging process of the secondary battery without degrading the energy density and cycle characteristics of the cathode.

[0067] In addition to the first positive electrode additive and the second positive electrode additive, the first layer may also include a first conductive material and a first adhesive.

[0068] The first conductive material can be used to compensate for conductivity degradation caused by the first positive electrode additive. Examples of such first conductive materials include graphite; carbon black, such as acetylene black, channel black, furnace black, lamp black, and thermally cracked carbon black; carbon nanostructures, such as carbon nanotubes and graphene; conductive fibers, such as carbon fibers and metal fibers; metal powders, such as fluorocarbons, aluminum powder, and nickel powder; conductive whiskers, such as zinc oxide and potassium titanate; conductive metal oxides, such as titanium oxide; and conductive materials, such as polyphenylene derivatives. These can be used alone or in combination.

[0069] Based on the total weight of the first and second layers, the content of the first conductive material can be from 0.1 wt% to 5 wt%. For example, based on the total weight of the first and second layers, the content of the first conductive material can be from 0.1 wt% to 4 wt%; 2 wt% to 4 wt%; 1.5 wt% to 5 wt%; 1 wt% to 3 wt%; 0.1 wt% to 2 wt%; or 0.1 wt% to 1 wt%.

[0070] The first adhesive can be used to fix the components contained in the first layer. The first adhesive can be an adhesive that is both adhesive and electrochemically stable. Specifically, examples of the first adhesive include styrene-butadiene rubber (SBR), butadiene rubber (BR), nitrile rubber (NBR), styrene-butadiene-styrene block polymer (SBS), styrene-vinyl butadiene block polymer (SEB), styrene-(styrene-butadiene)-styrene block polymer, natural rubber (NR), isoprene rubber (IR), ethylene-propylene-diene terpolymer (EPDM), poly(ethylene-co-propylene-co-5-methylene-2-norbornene), polytetrafluoroethylene (PTFE), polyvinylidene fluoride, polyvinyl chloride, polyvinylidene fluoride-co-hexafluoropropylene, polyvinylidene fluoride-co-trichloroethylene, poly(meth)acrylate, ethylhexyl polyacrylate, polybutyl acrylate, polyacrylonitrile, polyvinylpyrrolidone, polyvinyl acetate, polyethylene, polypropylene, polyethylene-co-vinyl acetate, polyethylene oxide, polypropylene oxide, polyarylate, cyanoethyl amylopectin, cyanoethyl polyvinyl alcohol, or combinations thereof.

[0071] The content of the first adhesive can be from 0.1% to 5% by weight, based on the total weight of the first and second layers. For example, the content of the first adhesive can be from 0.1% to 4% by weight; 2% to 4% by weight; 1.5% to 5% by weight; 1% to 3% by weight; 0.1% to 2% by weight; or 0.1% to 1% by weight, based on the total weight of the first and second layers.

[0072] Furthermore, the first layer may also contain positive electrode active material, just like the second layer. In this case, the first layer, together with the second layer, can function as a positive electrode active layer that contains the positive electrode active material and carries out electrochemical reactions, thus having the advantage of helping to increase the charge-discharge capacity and energy density of the positive electrode.

[0073] The positive electrode active material contained in the first layer may be the same as or different from the positive electrode active material contained in the second layer.

[0074] Specifically, the positive electrode active materials contained in the first and second layers are substances capable of inducing electrochemical reactions, and may each include lithium iron phosphate compounds represented by the following chemical formula 3 that are capable of reversibly inserting and deintercalating lithium ions: [Chemical Formula 3] LiFe r M 5 (1-r) XO4 In chemical formula 3, M 5 It is at least one element selected from W, Cu, Fe, V, Cr, Co, Ni, Mn, Ti, Zr, Zn, Al, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B, and Mo. X is at least one element selected from P, Si, S, As, and Sb, and r is 0 ≤ r ≤ 0.9.

[0075] The lithium iron phosphate compound represented by chemical formula 3 has an olivine structure, thus exhibiting superior structural stability, making it a promising active material with excellent lifetime characteristics and superior safety in all aspects, including overcharge and over-discharge. In particular, lithium iron phosphate compounds, due to PO4... - It exhibits excellent high-temperature stability due to strong bonding forces and contains abundant and inexpensive iron, making it more economical than LiCoO2, LiNiO2, or LiMn2O4. Furthermore, it has low toxicity, resulting in a smaller environmental impact.

[0076] Lithium iron phosphate compounds are phosphates containing iron (Fe) from transition metals, and in some cases may be doped with other transition metals (M). 5In the form of ), for example, lithium iron phosphate compounds can include LiFePO4, LiFe 0.9 Mn 0.1 PO4, LiFe 0.8 Mn 0.2 PO4, LiFe 0.7 Mn 0.3 PO4, LiFe 0.5 Mn 0.5 PO4, LiFe 0.3 Mn 0.7 PO4, LiFe 0.2 Mn 0.8 PO4, LiFe 0.1 Mn 0.9 PO4, etc.

[0077] In addition to the positive electrode active material, the second layer may also include a second conductive material, a second binder, and other additives.

[0078] At this point, since the second conductive material and the second adhesive have the same composition as the first conductive material and the first adhesive described above, a detailed description thereof will be omitted. However, based on the total weight of the first layer and the second layer, the total weight of the first conductive material and the second conductive material may be less than 10% by weight, less than 7.5% by weight, less than 5% by weight, or from 0.1% by weight to 5% by weight. More specifically, based on the total weight of the first layer and the second layer, the total weight of the first conductive material and the second conductive material may be from 0.1% by weight to 4% by weight; 2% by weight to 4% by weight; 1.5% by weight to 5% by weight; 1% by weight to 3% by weight; 0.1% by weight to 2% by weight; or 0.1% by weight to 1% by weight.

[0079] Furthermore, based on the total weight of the first and second layers, the total weight of the first adhesive and the second adhesive can be less than 10% by weight, less than 7.5% by weight, less than 5% by weight, or from 0.1% by weight to 5% by weight. More specifically, based on the total weight of the first and second layers, the total weight of the first adhesive and the second adhesive can be from 0.1% by weight to 4% by weight; 2% by weight to 4% by weight; 1.5% by weight to 5% by weight; 1% by weight to 3% by weight; 0.1% by weight to 2% by weight; or 0.1% by weight to 1% by weight.

[0080] Considering the electrical performance and lifespan of the positive electrode, the first and second layers can have specific thicknesses.

[0081] Specifically, there is no particular limitation on the total thickness of the first and second layers, but it can be specific to 50 μm to 500 μm. For example, the total thickness of the first and second layers can be 100 μm to 500 μm; 200 μm to 500 μm; 300 μm to 500 μm; 400 μm to 500 μm; 100 μm to 400 μm; 100 μm to 300 μm; 100 μm to 350 μm; 200 μm to 400 μm; 150 μm to 430 μm; 100 μm to 200 μm; 80 μm to 150 μm; 120 μm to 170 μm; 150 μm to 300 μm; 200 μm to 300 μm; or 150 μm to 190 μm.

[0082] The average thickness of the first layer can be from 1 μm to 30 μm. For example, the average thickness of the first layer can be from 1 μm to 20 μm; 1 μm to 10 μm; 5 μm to 30 μm; 10 μm to 30 μm; 15 μm to 30 μm; 20 μm to 30 μm; 5 μm to 15 μm; 15 μm to 25 μm; 8 μm to 14 μm; 1 μm to 5 μm; or 11 μm to 19 μm.

[0083] The ratio of the average thickness of the first layer to the average thickness of the second layer can be from 0.05 to 1.0. For example, the thickness ratio of the average thickness of the first layer to the average thickness of the second layer can be 0.05 to 0.8; 0.05 to 0.6; 0.05 to 0.5; 0.05 to 0.3; 0.05 to 0.2; 0.05 to 0.15; 0.1 to 0.2; 0.1 to 0.3; 0.2 to 0.4; 0.08 to 0.14; or 0.05 to 0.11.

[0084] The average thickness of the first layer and the average thickness of the second layer can be confirmed by scanning electron microscopy (SEM) analysis of a cross-section in the thickness direction of the positive electrode, and can refer to the average value of the thickness analyzed at three or more arbitrary points confirmed by the analysis.

[0085] As described above, this invention controls the average thickness of the first and second layers, thereby preventing the degradation of the positive electrode's energy density and output performance due to an excessively thick first layer. Furthermore, it prevents problems such as reduced bonding strength between the positive electrode current collector and the second layer due to an excessively thin first layer, or the inability to effectively remove oxygen generated during charging and discharging.

[0086] The positive electrode can be a material with high conductivity that will not cause chemical changes in the battery. For example, thin plates or films containing stainless steel, aluminum, nickel, titanium, calcined carbon, etc., can be used as the positive electrode current collector. In the case of aluminum or stainless steel, materials that have undergone surface treatment with carbon, nickel, titanium, silver, etc., can also be used. Furthermore, considering conductivity and the total thickness of the positive electrode to be manufactured, the average thickness of the current collector can be appropriately from 3 μm to 500 μm.

[0087] The positive electrode of the present invention has the above-described structure, and therefore has the effect of improving the safety issues caused by oxygen generated during charging and discharging. Furthermore, the positive electrode has the advantages of excellent cycle characteristics and lifespan characteristics.

[0088] Method for manufacturing positive electrode

[0089] This invention provides a method for manufacturing a positive electrode, comprising: Step (S1): Coat a first slurry containing a first positive electrode additive and a second positive electrode additive onto at least one surface of the positive electrode current collector; Step (S2): Coating a second slurry containing the positive electrode active material onto the already coated first slurry; and Step (S3): Dry the coated first and second slurries.

[0090] The method for manufacturing the positive electrode of the present invention refers to the method used to manufacture the positive electrode of the present invention described above.

[0091] The method for manufacturing the positive electrode of the present invention includes: step (S1), coating a first slurry containing a first positive electrode additive and a second positive electrode additive onto at least one surface of a positive electrode current collector; step (S2), coating a second slurry containing a positive electrode active material onto the coated first slurry; and step (S3), drying the coated first slurry and the second slurry.

[0092] At this point, steps (S1) and (S2) refer to the process of simultaneously or continuously discharging and coating a first slurry containing a first positive electrode additive and a second positive electrode additive, and a second slurry containing a positive electrode active material, onto the surface of a moving positive electrode current collector. Thus, the first slurry is coated onto at least one surface of the positive electrode current collector, and the second slurry is coated onto the coated first slurry.

[0093] Steps (S1) and (S2) can be applied without particular limitations, as long as they are methods commonly used in the art; however, die coating is preferred. Die coating can be performed using a slit die equipped with a shim for controlling slurry discharge conditions. In this case, the loading amount and coating thickness of the slurry coated onto the positive current collector can be easily controlled by controlling the shape, position, etc., of the shim.

[0094] As an example, the present invention can use a dual-die head to simultaneously coat the first and second slurries onto the positive current collector. In this case, compared with coating each slurry sequentially, it has the advantage of significantly improving process efficiency.

[0095] Step (S1) can be performed under specific conditions. The first positive electrode additive contained in the first slurry has low structural stability and may easily decompose under high temperature conditions or in the presence of water (H2O) and / or oxygen. When the first positive electrode additive decomposes in this way and is contained in the first layer of the positive electrode, the effect of compensating for irreversible lithium loss during the initial charge-discharge / activation process of the secondary battery may be significantly reduced. Therefore, the present invention allows for the coating of a first slurry containing the first positive electrode additive under specific conditions.

[0096] Specifically, step (S1) can be performed under any one or more of the following atmospheres: temperature conditions, humidity conditions, and gas conditions.

[0097] Step (S1) can be performed at a temperature below 30°C. For example, step (S1) can be performed at a temperature of 10°C to 30°C; 15°C to 30°C; 20°C to 30°C; 10°C to 25°C; 10°C to 20°C; 15°C to 25°C; 15°C to 22°C; 15°C to 20°C; or 11°C to 21°C.

[0098] Step (S1) can be performed under relative humidity (RH) conditions below 10%. For example, step (S1) can be performed under relative humidity (RH) conditions of 0% to 10%; 0% to 8%; 0% to 6%; 0% to 5%; 0% to 4%; 0% to 3%; 0% to 1%; 0.001% to 0.9%; 1% to 9%; 2% to 8%; 4% to 5%; 0.001% to 0.1%; or 0.001% to 0.01%. Here, relative humidity refers to (current water vapor quantity / saturated water vapor quantity) × 100, and can be calculated based on the internal temperature of the reactor coated with the first slurry, from the measured ratio of internal humidity to saturated water vapor quantity.

[0099] Step (S1) can be performed under oxygen partial pressure conditions of less than 5%. For example, step (S1) can be performed under oxygen partial pressure conditions of 0% to 5%; 0% to 4%; 0% to 3%; 0% to 2%; 0% to 1%; 0.1% to 5%; 0.5% to 5%; 1% to 5%; 2.5% to 5%; 0.1% to 2%; 0.1% to 1%; 0.5% to 1%; or 0.01% to 0.9%.

[0100] This invention controls the temperature, relative humidity, and / or oxygen partial pressure conditions within the aforementioned ranges, thereby minimizing structural damage to the first cathode additive contained in the first slurry caused by conditions exceeding the upper limit of the aforementioned ranges during the coating process. Furthermore, it prevents increased costs associated with step (S1) due to conditions below the lower limit of the aforementioned ranges.

[0101] Meanwhile, since the first slurry and the second slurry have the same structure as the first layer and the second layer of the above-mentioned positive electrode, a detailed description of them will be omitted.

[0102] The solids content of the first slurry can be controlled depending on whether a positive electrode active material is added. Specifically, when the first slurry contains a first positive electrode additive, a second positive electrode additive, a conductive material, and a binder, its solids content can be from 1% to 20%. For example, when the first slurry contains a first positive electrode additive, a second positive electrode additive, a conductive material, and a binder, its solids content can be from 1% to 15%, 1% to 10%, 1% to 9%, 5% to 15%, 5% to 10%, or 3% to 9%.

[0103] Furthermore, when the first slurry comprises a positive electrode active material, a first positive electrode additive, a second positive electrode additive, a conductive material, and a binder, its solid content can be from 20% to 70%. For example, when the first slurry comprises a positive electrode active material, a first positive electrode additive, a second positive electrode additive, a conductive material, and a binder, its solid content can be 25% to 70%, 30% to 70%, 40% to 70%, 45% to 70%, 50% to 70%, 25% to 60%, 25% to 50%, 25% to 40%, 30% to 60%, or 45% to 60%.

[0104] The present invention controls the solid content of the first slurry within the above-mentioned range based on whether it contains a positive electrode active material, thereby enabling not only uniform coating of the first slurry, but also easy control of the loading and / or thickness of the coated first slurry.

[0105] The method for manufacturing the positive electrode of the present invention includes step (S3) after step (S2): drying the coated first slurry and second slurry to form a first layer and a second layer on the positive electrode current collector.

[0106] At this point, drying can be applied without particular restrictions, as long as it is a method commonly applicable in the art. For example, drying can be achieved by applying heat to the coated slurry using a hot air dryer, vacuum oven, or similar equipment to dry the slurry.

[0107] Furthermore, after step (S3), a step (S4) may be included: rolling the first and second layers formed by drying. Rolling refers to the process of applying pressure to the surfaces of the first and second layers formed using a roller press or similar equipment to increase the density of the entire layer.

[0108] At this point, rolling can be performed using rolling equipment such as a rolling mill under linear pressure conditions until the target thickness and target porosity are achieved, followed by vacuum drying to manufacture a positive electrode containing a first layer and a second layer formed on the positive electrode current collector.

[0109] For example, roll forming can be performed with a target thickness (i.e., the average thickness of the first and second layers) of 100 μm to 400 μm and a target porosity (i.e., the porosity after roll forming) of 21% to 30%.

[0110] Specifically, the rolling can be carried out at temperatures ranging from 20°C to 100°C, more specifically 20°C to 80°C; 20°C to 60°C; 20°C to 40°C; 20°C to 30°C; 30°C to 100°C; 40°C to 100°C; 60°C to 100°C; 75°C to 100°C; 85°C to 100°C; 50°C to 90°C; 60°C to 80°C; or 65°C to 90°C.

[0111] Furthermore, the rolling can be carried out at rolling speeds of 2 m / s to 7 m / s, more specifically at 2 m / s to 6.5 m / s; 2 m / s to 6 m / s; 2 m / s to 5.5 m / s; 2 m / s to 5 m / s; 2 m / s to 4.5 m / s; 2 m / s to 4 m / s; 2.5 m / s to 4 m / s; 2.5 m / s to 3.5 m / s; 3.5 m / s to 5 m / s; 5 m / s to 7 m / s; 5.5 m / s to 6.5 m / s; or 6 m / s to 7 m / s.

[0112] In addition, the rolling can be carried out under pressure conditions of 50 MPa to 200 MPa, specifically 50 MPa to 150 MPa; 50 MPa to 100 MPa; 100 MPa to 200 MPa; 150 MPa to 200 MPa; or 80 MPa to 140 MPa.

[0113] In addition, the vacuum drying conditions can be carried out for 1 to 15 hours at, for example, 100°C to 250°C, specifically 160°C to 200°C.

[0114] The present invention performs rolling under the above-mentioned temperature, speed and / or pressure conditions, thereby maximizing the energy density of the first and second layers while minimizing structural damage to the first positive electrode additive contained in the first layer.

[0115] Lithium secondary batteries

[0116] Furthermore, the present invention provides a secondary battery comprising: An electrode assembly comprising a positive electrode, a negative electrode, and a separator disposed between the positive and negative electrodes as described above; and An electrolyte composition, wherein an electrode assembly is impregnated.

[0117] The secondary battery of the present invention can be a lithium secondary battery. The lithium secondary battery incorporates the positive electrode of the present invention in its electrode assembly, thus exhibiting excellent stability, as well as outstanding cycle characteristics and lifespan.

[0118] At this point, the electrode assembly can have a structure in which a positive electrode, a negative electrode, and a separator sandwiched between the positive and negative electrodes to insulate them from each other are positioned, and can be wound in a stacked, stacked-folded, or jelly-roll shape. This type of electrode assembly has high energy density within a limited space, thus offering the advantage of high practicality in terms of energy density and output of secondary batteries.

[0119] The electrode assembly can have a structure in which it is embedded in the pouch-like shell in a state where it is connected to corresponding leads for a positive and a negative electrode formed on the outside of the pouch-like shell. Specifically, the positive and negative leads can be formed to extend from the inside of the pouch-like shell to the outside. In this case, the positive and negative leads can be led out to the outside of the pouch-like shell and can have a structure that extends in the same direction or in opposite directions.

[0120] Meanwhile, since the positive electrode included in the electrode assembly has the same structure as described above, a detailed description of it will be omitted.

[0121] In addition, similar to the positive electrode, the negative electrode comprises: a negative electrode active layer containing a negative electrode active material on at least one surface of the negative electrode current collector.

[0122] At this point, materials capable of reversibly inserting / deintercalating lithium ions can be used as anode active materials.

[0123] Examples of materials capable of reversibly inserting / deintercalating lithium ions include carbon materials, namely carbon-based anode active materials commonly used in lithium-ion secondary batteries. Carbon-based anode active materials refer to materials containing carbon atoms as the main component, and such carbon-based anode active materials can include graphite compounds. For example, carbon-based anode active materials can include natural graphite, artificial graphite, Kish graphite, pyrolytic carbon, carbon microspheres, and mesophase calcined carbon (bulk mesophase, liquid crystal pitch-based carbon fibers, etc.) and graphitized coke (raw coke, raw petroleum coke, needle coke, petroleum coke, coal coke, etc.) using tar / pitch as raw materials.

[0124] Carbon-based anode active materials can be in the form of assemblies composed of multiple particles. In this case, a graphite assembly can be composed of 2 to 100, preferably 3 to 20, graphite particles.

[0125] The negative electrode active material can also include silicon-based negative electrode active materials. Silicon-based negative electrode active materials are materials that contain silicon (Si) as a main component and can increase the charge-discharge capacity and energy density per unit volume of the negative electrode. Examples of such silicon-based negative electrode active materials include silicon (Si), silicon carbide (SiC), silicon monoxide (SiO), and silicon dioxide (SiO2), which can be contained individually or in combination in the negative electrode active layer. When silicon monoxide (SiO) and silicon dioxide (SiO2) as silicon-based negative electrode active materials are uniformly mixed or composited and contained in the negative electrode active layer, they can be represented as silicon oxide (SiO2). q (where 0.5≤q≤2.5).

[0126] Furthermore, silicon-based anode active materials can be doped with C, Li, Mg, Al, Ca, and / or Ti, or alloyed with them. Additionally, when silicon-based anode active materials contain oxygen (O), their surface can be treated with a carbon coating or similar method to suppress volume expansion during charging and improve the conductivity of the anode active material.

[0127] Furthermore, based on the total weight of the second negative electrode active layer, the content of silicon-based negative electrode active material can be from 0.1 wt% to 30 wt%. Specifically, based on the total weight of the second negative electrode active layer, the content of silicon-based negative electrode active material can be from 0.1 wt% to 25 wt%, 20 wt% to 30 wt%, 10 wt% to 30 wt%, 0.5 wt% to 20 wt%, 1 wt% to 9 wt%, 5 wt% to 15 wt%, 3 wt% to 7 wt%, 11 wt% to 19 wt%, 13 wt% to 17 wt%, 15 wt% to 20 wt%, 3 wt% to 13 wt%, or 1 wt% to 15 wt%. This invention controls the content ratio of silicon-based negative electrode active material within the above range, thereby improving the charging capacity per unit mass while reducing lithium consumption and irreversible capacity loss during the initial charge and discharge process of the secondary battery. Furthermore, since the structural stability of the negative electrode active layer can be improved by minimizing the volume change of the negative electrode active layer during battery charge and discharge, the lifespan of the secondary battery can be extended.

[0128] In addition to the negative electrode active material as the main component, the negative electrode active layer may selectively contain conductive materials, binders, other additives, etc., if necessary.

[0129] Conductive materials may include one or more of the following, but are not limited to: carbon black, acetylene black, Ketjen black, carbon nanotubes, carbon fibers, etc.

[0130] For example, the negative electrode active layer can be made of carbon black, carbon nanotubes, carbon fibers, etc., either alone or in combination, as a conductive material.

[0131] At this point, based on a total of 100 parts by weight of the negative electrode active layer, the content of conductive material can be from 0.1 parts by weight to 10 parts by weight. Specifically, the conductive material can be from 0.1 parts by weight to 8 parts by weight, 0.1 parts by weight to 5 parts by weight, 0.1 parts by weight to 3 parts by weight, 2 parts by weight to 6 parts by weight, or 0.5 parts by weight to 2 parts by weight. This invention controls the content of conductive material within the above range, thereby preventing an increase in the resistance of the negative electrode and a deterioration in the charging capacity due to a low content of conductive material. Furthermore, this invention can prevent the problem of charging capacity deterioration caused by a decrease in the content of the negative electrode active material due to excessive conductive material exceeding the above range, or the problem of increased resistance due to an increase in the loading of the negative electrode active layer.

[0132] Furthermore, the adhesive is a component that assists in the bonding between the negative electrode active material and the conductive material, as well as the bonding with the current collector, and can be appropriately applied within a range that does not degrade the electrical properties of the negative electrode. For example, the adhesive may include one or more of the following: vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinylidene fluoride (PVdF), polyacrylonitrile, polymethyl methacrylate, polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, polyacrylic acid, ethylene-propylene-diene monomer, sulfonated ethylene-propylene-diene monomer, styrene-butadiene rubber (SBR), and fluororubber.

[0133] Based on a total of 100 parts by weight of the negative electrode active layer, the content of the adhesive can be from 0.1 parts by weight to 10 parts by weight. Specifically, the adhesive can be from 0.1 parts by weight to 8 parts by weight, 0.1 parts by weight to 5 parts by weight, 0.1 parts by weight to 3 parts by weight, or 2 parts by weight to 6 parts by weight. This invention controls the content of the adhesive contained in the negative electrode active layer within the above range, thereby preventing degradation of the adhesion strength of the active layer due to low adhesive content, or degradation of the electrical properties of the negative electrode due to excessive adhesive.

[0134] Furthermore, the negative electrode can be a material with high conductivity that will not cause chemical changes in the battery as the negative electrode current collector. For example, thin plates or films containing stainless steel, aluminum, nickel, titanium, calcined carbon, etc., can be used as the negative electrode current collector, and in the case of aluminum or stainless steel, materials that have undergone surface treatment with carbon, nickel, titanium, silver, etc., can also be used. In addition, considering conductivity and the total thickness of the positive electrode to be manufactured, the average thickness of the current collector can be appropriately from 3 μm to 500 μm.

[0135] The separator sandwiched between the positive and negative electrodes of a lithium secondary battery is an insulating film with high ion permeability and mechanical strength, and is not particularly limited, as long as it is a separator commonly used in the art. Specifically, the separator may include one or more polymers selected from chemically resistant and hydrophobic polypropylene, polyethylene, and polyethylene-propylene copolymers. The separator may be in the form of a porous polymer substrate such as a sheet or nonwoven fabric containing the above polymers, and in some cases, it may be in the form of a composite separator in which organic or inorganic particles are coated onto a porous polymer substrate by an organic adhesive. Furthermore, the average pore size of the separator may be from 0.01 μm to 10 μm, and the average thickness may be from 5 μm to 300 μm.

[0136] In addition, the electrolyte composition may contain non-aqueous organic solvents, lithium salts, electrolyte additives, etc.

[0137] Non-aqueous organic solvents may be used without particular restrictions, provided they are non-aqueous organic solvents used in non-aqueous electrolytes in the art. For example, non-protic organic solvents such as N-methyl-2-pyrrolidone, ethylene carbonate (EC), propylene carbonate (PC), butyl carbonate, dimethyl carbonate (DMC), diethyl carbonate (DEC), γ-butyrolactone, 1,2-dimethoxyethane (DME), tetrahydrofuran, 2-methyltetrahydrofuran, dimethyl sulfoxide, 1,3-dioxolane, formamide, dimethylformamide, dioxolane, acetonitrile, nitromethane, methyl formate, methyl acetate, triethyl phosphate, trimethoxymethane, dioxolane derivatives, sulfolane, methyl sulfolane, 1,3-dimethyl-2-imidazolium ketone, ether, methyl propionate (MP), ethyl propionate (EP), and propyl propionate (PP) may be used as non-aqueous organic solvents.

[0138] Furthermore, the non-aqueous organic solvents used in this invention can be used alone or in mixtures of two or more in any combination or ratio, depending on the desired application. From the perspective of electrochemical stability against redox reactions and chemical stability against thermal or solute reactions, mixtures of propylene carbonate, ethylene carbonate, fluoroethylene carbonate, diethyl carbonate, dimethyl carbonate, and ethyl methyl carbonate are particularly preferred.

[0139] Lithium salts can be used without particular restrictions, as long as they are lithium salts used in non-aqueous electrolytes in the art. Specifically, lithium salts may include LiCl, LiBr, LiI, LiClO4, LiBF4, and LiB. 10 Cl 10 One or more of the following: LiPF6, LiCF3SO3, LiCF3CO2, LiAsF6, LiSbF6, LiAlCl4, CH3SO3Li, (CF3SO2)2NLi and (FSO2)2NLi.

[0140] The appropriate concentration range for lithium salts is defined as follows: lower limit ≥ 0.5 mol / L, specifically ≥ 0.7 mol / L, more specifically ≥ 0.9 mol / L, and upper limit ≤ 2.5 mol / L, specifically ≤ 2.0 mol / L, more specifically ≤ 1.5 mol / L. If the lithium salt concentration is below 0.5 mol / L, the ionic conductivity decreases, potentially degrading the cycle and output characteristics of the non-aqueous electrolyte battery. Furthermore, if the lithium salt concentration exceeds 2.5 mol / L, the viscosity of the electrolyte used in the non-aqueous electrolyte battery increases, which may also reduce ionic conductivity and potentially degrade the cycle and output characteristics of the non-aqueous electrolyte battery.

[0141] Furthermore, when a large quantity of lithium salt is dissolved in a non-aqueous organic solvent at once, the temperature of the electrolyte composition may rise due to the heat of dissolution of the lithium salt. When the temperature of the non-aqueous organic solvent is significantly increased by the heat of dissolution of the lithium salt in this manner, decomposition may be accelerated in the case of fluorine-containing lithium salts, potentially producing hydrogen fluoride (HF). Since hydrogen fluoride (HF) degrades battery performance, it is undesirable. Therefore, there are no particular limitations on the temperature at which lithium salt is dissolved in a non-aqueous organic solvent, but it can be controlled within the range of -20°C to 80°C, specifically within the range of 0°C to 60°C.

[0142] Furthermore, electrolyte additives may be included as additional auxiliary components to improve the physical properties of the electrolyte composition. The electrolyte additives commonly used in the non-aqueous electrolytes of this invention can be added in any ratio. Specifically, compounds having overcharge prevention effects, negative electrode film-forming effects, and positive electrode protection effects may be mentioned, such as cyclohexylbenzene, biphenyl, tert-butylbenzene, carbonates, vinyl ethylene carbonate, difluoroanisole, fluoroethylene carbonate, propane sulpholactone, succinate, and dimethyl vinyl carbonate. Furthermore, as in the case of non-aqueous electrolyte batteries known as lithium polymer batteries, the electrolyte for non-aqueous electrolyte batteries may be used in a quasi-solid-state form using gelling agents or crosslinking polymers.

[0143] For example, in order to suppress the generation of oxygen inside the secondary battery or remove oxygen generated during charging and discharging, electrolyte additives may include compounds represented by the following chemical formula 4: [Chemical Formula 4]

[0144] In chemical formula 4, R1 to R6 are each hydrogen, an alkyl group having 1 to 10 carbon atoms, or an alkoxy group having 1 to 10 carbon atoms, provided that at least one of R1 to R6 is -L1-(CH). n -R7, L1 can be direct bonding, -O-, or -COO-. R7 is an aliphatic unsaturated hydrocarbon group with 2 to 6 carbon atoms, and n is an integer from 1 to 6.

[0145] Specifically, in chemical formula 4, R1 through R6 are each hydrogen, methyl, ethyl, propyl, butyl, methoxy, ethoxy, or propoxy, provided that at least one of R1 through R6 is -L1-(CH). n -R7, L1 can be direct bonding, -O-, or -COO-. R7 is an alkenyl group having 2 to 4 carbon atoms or an alkynyl group having 2 to 4 carbon atoms, and n is an integer from 1 to 3.

[0146] More specifically, in chemical formula 4, R1 through R6 are each hydrogen, methyl, ethyl, methoxy, or ethoxy, provided that at least one of R1 through R6 is -L1-(CH). n -R7, L1 can be direct bonding, -O-, or -COO-. R7 is vinyl or acetylene, and n is 1 or 2.

[0147] The compound represented by Formula 4 has a structure incorporating an aliphatic unsaturated hydrocarbon group surrounding a coumarin group serving as the parent nucleus. The bicyclic hydrocarbon group contained within the coumarin group includes an ester group within the introduced ring, thus exhibiting a higher affinity for oxygen than the non-aqueous organic solvents in the electrolyte composition. Therefore, the compound represented by Formula 4 can rapidly react with and remove oxygen present inside the secondary battery. Furthermore, the aliphatic unsaturated hydrocarbon group incorporating the coumarin group can participate in the formation of organic and inorganic films on the surfaces of the positive and / or negative electrodes, thereby suppressing oxygen generation inside the battery during charging and discharging.

[0148] Examples of compounds represented by chemical formula 4 include compounds represented by the following structural formulas 1 through 11: <Structure 1>

[0149] <Structure 2>

[0150] <Structure 3>

[0151] <Structure 4>

[0152] <Structure 5>

[0153] <Structure 6>

[0154] <Structure 7>

[0155] <Structure 8>

[0156] <Structure 9>

[0157] <Structure 10>

[0158] <Structure 11>

[0159] The compounds represented by <Structural Formulas 1> to <Structural Formulas 11> above exhibit excellent reactivity with oxygen, thus enabling them to efficiently remove oxygen present inside secondary batteries. Furthermore, these compounds participate in the formation of organic and inorganic films on the surfaces of the positive and / or negative electrodes and effectively suppress side reactions between the electrode and electrolyte composition, thus demonstrating superior performance in suppressing oxygen generation during charging and discharging.

[0160] When the electrolyte additive is a compound represented by Formula 4, the content of the electrolyte additive can be from 0.01 wt% to 5 wt% based on the total weight of the electrolyte composition. For example, when the electrolyte additive is a compound represented by Formula 4, the content of the electrolyte additive can be in the range of 0.01 wt% to 4 wt%, 0.02 wt% to 4.5 wt%, 0.05 wt% to 4 wt%, 0.07 wt% to 3.7 wt%, 0.1 wt% to 3.5 wt%, 0.15 wt% to 3.3 wt%, 0.2 wt% to 3 wt%, 0.3 wt% to 2.7 wt%, 0.4 wt% to 2.5 wt%, 0.5 wt% to 2.2 wt%, 0.6 wt% to 2 wt%, 0.7 wt% to 1.8 wt%, 0.8 wt% to 1.5 wt%, or any two of these values.

[0161] When the content of the electrolyte additive is below the lower limit of the above range, the oxygen removal effect may be insignificant. Furthermore, when the content of the electrolyte additive exceeds the upper limit of the above range, the resistance of the electrolyte composition increases significantly, leading to deterioration in the cycle characteristics and lifespan of the secondary battery.

[0162] The present invention will now be described in more detail through examples and comparative examples.

[0163] However, the following embodiments and comparative examples are only used to illustrate the present invention, and the content of the present invention is not limited to the following embodiments and comparative examples.

[0164] Examples 1 to 10 and Comparative Examples 1 to 2. Manufacturing of the positive electrode

[0165] Prepare LiFePO4 (D 50 Li5FeO4 (D) was prepared as the positive electrode active material (approximately 1 μm). 501st Approximately 1 μm) was used as the first positive electrode additive. In addition, WO3, Li2NiO2, and TiO2 were prepared as the second positive electrode additives, respectively, and carbon black (D...) was prepared. 50 A conductive material of approximately 3 to 5 μm was prepared, and polyvinylidene fluoride (PVdF) was prepared as an adhesive.

[0166] After preparation, the first positive electrode additive, the second positive electrode additive, the positive electrode active material, the conductive material, and the binder are mixed in N-methylpyrrolidone (NMP) such that the content based on the total weight of the first and second layers contained in the positive electrode is as shown in Table 1 below, to prepare a first slurry (solid content: 45%) for forming the first layer. At this time, ① the average particle size (D) of the second positive electrode additive is... 50 The types of the second positive electrode additives (②) are controlled as shown in Table 1 below.

[0167] Individually, the positive electrode active material, conductive material, and binder are each mixed in N-methylpyrrolidone (NMP) such that the content of the first and second layers contained in the positive electrode is as shown in Table 2 below, to prepare a second slurry (solid content: 50%) for forming the second layer.

[0168] The prepared first and second slurries were sequentially coated onto an aluminum sheet (average thickness: 10 μm), followed by drying and rolling to manufacture the positive electrode. The first slurry was coated at 20 ± 2 °C, relative humidity (RH) below 5%, and oxygen partial pressure between 0.1% and 1.0%. Furthermore, the average thickness (T) of the first layer of the manufactured positive electrode was... 1st ) and the average thickness ratio of the first layer to the second layer (T) 1st / T 2nd The control is performed as shown in Table 2 below.

[0169] [Table 1]

[0170] [Table 2]

[0171] Examples 11 to 20 and Comparative Examples 3 to 4. Manufacturing of secondary batteries

[0172] The negative electrode slurry contains 97% by weight of artificial graphite as a carbon-based negative electrode active material, and 3% by weight of a 1:1 mixture of carboxymethyl cellulose (CMC) and styrene-butadiene rubber (SBR) as a binder. The negative electrode slurry is coated onto a copper sheet (average thickness: 12 μm), and then dried and rolled to manufacture a negative electrode containing a negative electrode active layer.

[0173] Nine positive electrodes and ten negative electrodes prepared in the above embodiments or comparative examples are arranged alternately, with an 18 μm porous polyethylene membrane sandwiched between them to prepare an electrode assembly. The prepared electrode assembly is inserted into a battery case and an electrolyte composition is injected to manufacture a small pouch-type lithium secondary battery.

[0174] Here, as the electrolyte composition, a solution prepared by dissolving 1 M LiPF6 in an organic solvent obtained by mixing ethylene carbonate (EC), dimethyl carbonate (DMC), and ethyl methyl carbonate (EMC) in a volume ratio of 3:4:3 is used.

[0175] [Table 3]

[0176] Examples 21 and 22. Manufacturing of secondary batteries

[0177] A small pouch-type lithium secondary battery was manufactured in the same manner as in Example 14 above, except that 0.1% by weight of the electrolyte additive represented by <Structural Formula 1> or <Structural Formula 10> was added based on the total weight of the electrolyte composition.

[0178] <Structure 1>

[0179] <Structure 10>

[0180] Experimental example.

[0181] The following experiments were conducted to evaluate the performance of the positive electrode of the present invention and the secondary battery containing the positive electrode.

[0182] oxygen removal capacity

[0183] The thickness of each lithium secondary battery manufactured in the examples and comparative examples was measured for the first time. Subsequently, each lithium secondary battery was pre-aged at room temperature (22±2°C) for 2 days, and then charged at 0.1C to 30% state of charge (SOC) for activation. Then, each activated lithium secondary battery was aged at room temperature (22±2°C) and 60°C for one day each, and the thickness of each lithium secondary battery was measured a second time. Based on the thickness of the secondary batteries measured in the first measurement, the rate of change of thickness in the second measurement was calculated. It was determined that the smaller the calculated rate of change of thickness, the higher the removal rate of gases generated during the activation process.

[0184] In addition, each activated lithium secondary battery underwent a total of 300 charge-discharge cycles, and the thickness of each lithium secondary battery was measured for the third time. During this process, the batteries were charged at 45±2°C under constant current / constant voltage conditions of 2.0C and 3.65V, with a cutoff current of 0.05C, and discharged under constant current conditions of 0.5C, with a cutoff voltage of 2.5V. This charge-discharge cycle constituted one cycle.

[0185] Based on the thickness of the secondary battery measured in the first measurement, the rate of change of the secondary battery thickness in the third measurement was calculated. It was determined that the smaller the calculated rate of change of thickness, the higher the removal rate of gases generated during the charge-discharge process after activation. The calculation results are shown in Table 4 below.

[0186] Cyclic characteristics

[0187] Each lithium secondary battery manufactured in the examples and comparative examples was charged to 4.2V at 0.3C under CC-CV conditions at 25°C and discharged to 2.5V at 0.3C under CC conditions for activation.

[0188] Each activated lithium secondary battery was charged to 4.2V at a rate of 1.0C under CC-CV conditions at 25°C, and then discharged to 2.5V at a rate of 1.0C under CC conditions. This constitutes one cycle, and each lithium secondary battery manufactured in the examples and comparative examples was subjected to one charge-discharge cycle. At this time, the capacity during the charge-discharge process was measured to determine the charge-discharge capacity of the first cycle. Subsequently, each lithium secondary battery was subjected to 499 more charge-discharge cycles, for a total of 500 charge-discharge cycles. At this time, the charge-discharge capacity of the 500th cycle was confirmed at the last cycle. Based on the measured charge-discharge capacity of the first cycle, the charge-discharge capacity retention rate of the 500th cycle was calculated. The results are shown in Table 4 below.

[0189] [Table 4]

[0190] As shown in Table 4 above, it can be seen that the positive electrode manufactured in the examples has an excellent effect in removing oxygen generated during the activation process of the secondary battery and during subsequent charging and discharging processes.

[0191] Furthermore, it was found that the positive electrode exhibits excellent charge-discharge capacity retention after 500 cycles because it contains a first positive electrode additive and a second positive electrode additive in the first layer adjacent to the positive electrode current collector.

[0192] These results demonstrate that the positive electrode of the present invention contains a lithium-ionized compound as a first positive electrode additive, thereby compensating for the lithium lost at the negative electrode during activation and effectively removing the oxygen generated at this time. Furthermore, the positive electrode exhibits good conductivity, thus demonstrating excellent cycle characteristics and lifetime performance.

[0193] Although the invention has been described with reference to preferred embodiments, those skilled in the art will understand that various modifications and variations can be made therein without departing from the invention as defined in the appended claims. Therefore, the scope of the invention should not be limited by the detailed description in the specification, but rather by the appended claims.

[0194] Therefore, the scope of the present invention should not be limited to the contents described in the detailed description of the specification, but should be determined by the claims.

Claims

1. A positive electrode comprising: Positive current collector; A first layer, wherein the first layer is disposed on at least one surface of the positive electrode current collector, and comprises a first positive electrode additive and a second positive electrode additive; and The second layer is disposed on the first layer and contains a positive electrode active material. in, The first positive electrode additive includes: a compound whose activation voltage range overlaps with the working voltage range of the positive electrode active material by more than 50%, based on the working voltage of the positive electrode active material. The second positive electrode additive comprises one or more compounds represented by the following chemical formula 1, and Wherein, the average particle size of the second positive electrode additive is smaller than the average particle size of the first positive electrode additive: [Chemical Formula 1] M 1 x M 2 y O z In chemical formula 1, M 1 and M 2 Each of the following is a given element: Li, W, Mo, Ni, Co, Nb, Ge, Ti, Ta, or Ce, provided that M is present. 1 and M 2 Including different metals, and x, y, and z are 1≤x≤3, 0≤y≤1, and 1≤z≤6, respectively.

2. The positive electrode as described in claim 1, wherein, The average particle size D of the first positive electrode additive 50 The range is from 0.5 μm to 20 μm.

3. The positive electrode as described in claim 1, wherein, The ratio of the average particle size of the second positive electrode additive to the average particle size of the first positive electrode additive is 0.5 or more and less than 1.

0.

4. The positive electrode as described in claim 1, wherein, The first positive electrode additive comprises one or more compounds represented by the following chemical formula 2: [Chemical Formula 2] Li a M 3 (1-b) M 4 b O c In chemical formula 2, M 3 It is Fe, Co, Mn, Zn, Al or Ga, M 4 M is at least one metal selected from W, Cu, Fe, V, Cr, Ti, Zr, Zn, Co, Al, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B, and Mo, provided that M is a metal selected from W, Cu, Fe, V, Cr, Ti, Zr, Zn, Co, Al, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B, and Mo. 3 and M 4 Including different metals, and a, b, and c are 1≤a≤7, 0≤b≤0.5, and 1.8≤c≤4.5, respectively.

5. The positive electrode as described in claim 1, wherein, Based on the total weight of the first layer and the second layer, the content of the first cathode additive is 0.5% to 5% by weight.

6. The positive electrode as described in claim 1, wherein, Based on the total weight of the first cathode additive, the content of the second cathode additive is 5% to 25% by weight.

7. The positive electrode as described in claim 1, wherein, The first layer further comprises a third positive electrode additive, which includes at least one of the following: metal carbonates; metal halides; photosensitive dyes; unsaturated hydrocarbons; polymers having repeating units containing amide groups; catechols; sulfites; ascorbic acid derivatives; And enzymes, The metal carbonate or the metal halide contains at least one metal selected from iron (Fe), cobalt (Co), nickel (Ni) and copper (Cu).

8. The positive electrode as described in claim 7, wherein, The content of the third cathode additive is from 1 part to 25 parts by weight, based on 100 parts by weight of the first cathode additive.

9. The positive electrode as claimed in claim 1, wherein, The average thickness of the first layer is 1 μm to 30 μm.

10. The positive electrode as claimed in claim 1, wherein, The ratio of the average thickness of the first layer to the average thickness of the second layer is 0.05 to 1.

11. The positive electrode as claimed in claim 1, wherein, The first layer also contains a positive electrode active material.

12. The positive electrode as claimed in claim 11, wherein, The positive electrode active material contained in each of the first and second layers comprises a lithium iron phosphate compound represented by the following chemical formula 3: [Chemical Formula 3] LiFe r M 5 (1-r) XO4 In chemical formula 3, M 5 It is at least one element selected from W, Cu, Fe, V, Cr, Co, Ni, Mn, Ti, Zr, Zn, Al, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B, and Mo. X is at least one element selected from P, Si, S, As, and Sb, and r is 0 ≤ r ≤ 0.

9.

13. A secondary battery comprising: An electrode assembly comprising a positive electrode, a negative electrode, and a separator sandwiched between the positive and negative electrodes as described in claim 1; and An electrolyte composition, wherein the electrolyte composition impregnates the electrode assembly.

14. The secondary battery as claimed in claim 13, wherein, The negative electrode comprises: a negative electrode active layer containing a carbon-based negative electrode active material on at least one surface of the negative electrode current collector.

15. The secondary battery as described in claim 13, wherein, The negative electrode active layer further comprises materials selected from Si, SiC, and SiO. q At least one silicon-based anode active material, wherein 0.5 ≤ q ≤ 2.5.

Citation Information

Patent Citations

  • Lithium transition metal oxide, positive electrode additive for lithium secondary battery, lithium secondary battery comprising the same

    KR1020230057858A

  • Afrocitentan for the treatment of hypertension

    KR1020250016196A