Positive electrode material, positive electrode including the same, and lithium secondary battery

By mixing olivine-structured lithium iron phosphate manganese-based compounds and layered lithium composite transition metal oxides, a cathode material was prepared, solving the problems of low conductivity of lithium iron phosphate-based compounds and lifespan characteristics of lithium composite transition metal oxides in high-voltage ranges in lithium secondary batteries, and achieving improvements in thermal stability and capacity characteristics.

CN123165698APending Publication Date: 2026-11-24LG CHEM LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202580030674.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2024-04-30
Filing Date
2025-04-18
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

In existing lithium secondary batteries, the low conductivity of lithium iron phosphate-based compounds leads to increased internal resistance and reduced battery capacity. Furthermore, due to their low density, they cannot sufficiently increase energy density, resulting in poor output characteristics. Additionally, lithium composite transition metal oxides have issues with lifetime characteristics when operating in high voltage ranges.

Method used

A cathode material was prepared by mixing lithium iron phosphate manganese-based compounds with olivine structures and layered lithium composite transition metal oxides to meet specific discharge capacity and thermal stability requirements, control particle size and crystallite size, and form a carbon coating on the lithium iron phosphate manganese-based compound to improve electronic conductivity.

Benefits of technology

This approach achieves improved capacity and lifespan characteristics while maintaining thermal stability, enhances resistance characteristics, and improves the overall performance of lithium secondary batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123165698A_ABST
    Figure CN123165698A_ABST
Patent Text Reader

Abstract

The present invention relates to a positive electrode material capable of improving the performance of a lithium secondary battery, and a positive electrode and a lithium secondary battery including the same, and the positive electrode material includes a first positive electrode active material having an olivine structure and a second positive electrode active material having a layered structure, wherein the first positive electrode active material comprises a lithium iron phosphate manganese-based compound having manganese (Mn) in an amount of 20 mol% to 60 mol% of all metals except lithium, and satisfies Equation 1 and Equation 2 described in the specification.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] Cross-references to related applications

[0002] This application claims priority to Korean Patent Application No. 10-2024-0057865, filed on April 30, 2024, the disclosure of which is incorporated herein by reference. Technical Field

[0003] This invention relates to cathode materials, cathodes including the cathode materials, and lithium secondary batteries. Background Technology

[0004] With recent technological advancements and increased demand for mobile devices and electric vehicles, the need for secondary batteries as an energy source has increased significantly. Among these secondary batteries, lithium-ion batteries, characterized by high energy density, high voltage, long cycle life, and low self-discharge rate, have been commercialized and are widely used.

[0005] Lithium-ion batteries consist of four main components: the positive electrode, the negative electrode, the separator, and the electrolyte. Among these, the positive electrode active material plays a crucial role in determining the battery's capacity, output, and lifespan. To achieve high energy density, output, and lifespan in lithium-ion batteries, improvements in the performance of the positive electrode active material are necessary; therefore, extensive research has recently been conducted to develop high-performance positive electrode active materials.

[0006] Lithium transition metal oxides, such as lithium cobalt-based oxides like LiCoO2, lithium nickel-based oxides like LiNiO2, lithium manganese-based oxides like LiMnO2 or LiMn2O4, and lithium iron phosphate-based compounds like LiFePO4, have been developed as positive electrode active materials for lithium secondary batteries. More recently, lithium composite transition metal oxides including two or more transition metals, such as Li[Ni], have also been developed. a Co b Mn c O2, Li[Ni a Co b Al c ]O2 and Li[Ni a Co b Mn c Al d O2 has been developed and is widely used.

[0007] Because lithium iron phosphate-based compounds with an olivine structure have the best structural stability, they exhibit excellent lifetime characteristics and are promising active materials with superior advantages in all aspects of safety, including overcharge and over-discharge.

[0008] In particular, LiFePO4 exhibits excellent high-temperature stability due to the strong binding force of PO4, is cheaper than LiCoO2, LiNiO2, or LiMn2O4 due to its abundant and inexpensive iron content, and has a smaller environmental impact due to its low toxicity. However, due to the low conductivity of LiFePO4, there is a problem of increased internal resistance of the battery when LiFePO4 is used as the positive electrode active material. As a result, the battery capacity decreases because the polarization potential increases when the battery circuit is closed. Furthermore, LiFePO4 has limitations in that its lower density compared to conventional positive electrode active materials may not be sufficient to increase the battery's energy density, and because it typically has the form of secondary particles assembled from primary particles, the output characteristics are poor due to the large interfacial resistance between the primary particles.

[0009] To improve the capacity characteristics of lithium iron phosphate-based compounds, an attempt was made to use a mixture of lithium complex transition metal oxides and lithium iron phosphate-based compounds. However, since the operating voltage of lithium iron phosphate-based compounds is lower than that of lithium complex transition metal oxides, only the lithium complex transition metal oxides operate in the high voltage range, thus causing problems with lifetime characteristics. Summary of the Invention

[0010] Technical issues

[0011] One aspect of the present invention provides a cathode material that has improved capacity characteristics while maintaining thermal stability.

[0012] Another aspect of the present invention provides a positive electrode and a lithium secondary battery that have excellent thermal stability and capacity characteristics by including the above-described positive electrode material.

[0013] Technical solution

[0014] (1) This invention provides a cathode material comprising: a first cathode active material having an olivine structure; and a second cathode active material having a layered structure, wherein the first cathode active material comprises a lithium iron phosphate manganese-based compound, the lithium iron phosphate manganese-based compound having manganese (Mn) in an amount of 20 mol% to 60 mol% of all metals other than lithium, and satisfying Equations 1 and 2: [Equation 1] 1.45 ≤ T / D [°C·g / mAh] ≤ 1.70 [Equation 2] H / D [J / mAh] ≤ 5.10 Among them, in equations 1 and 2, For a lithium secondary battery comprising a positive electrode including a positive electrode active material layer, and based on the total weight of the positive electrode active material layer, the positive electrode active material layer containing 80% to 98% by weight of the positive electrode material, D is the discharge capacity (mAh / g) of the battery when it is charged to 4.25 V at 25°C in constant current (CC) (0.1 C) - constant voltage (CV) (cutoff current: 0.05 C) mode and discharged to 2.5 V in CC (0.1 C) mode.

[0015] T is the temperature (°C) of the maximum peak observed between 200°C and 350°C when the battery is charged to 4.25 V at 25°C in CC (0.2 C)-CV (cutoff current: 0.05 C) mode and discharged to 2.5 V in CC (0.2 C) mode to perform the activation process, and then charged to 4.25 V in CC (0.2 C)-CV (cutoff current: 0.05 C) mode again.

[0016] H is the calorific value (J / g) measured using a differential scanning calorimeter (DSC) in the range of 200°C to 350°C when the battery is charged to 4.25 V at 25°C in CC (0.2 C)-CV (cutoff current: 0.05 C) mode and discharged to 2.5 V in CC (0.2 C) mode to perform the activation process, and then charged to 4.25 V in CC (0.2 C)-CV (cutoff current: 0.05 C) mode.

[0017] (2) The present invention provides the positive electrode material of (1) above, wherein the average particle size (D) of the first positive electrode active material is... 50 The range is from 0.50 μm to 1.00 μm.

[0018] (3) The present invention provides the positive electrode material of (1) or (2) above, wherein the average crystallite size of the first positive electrode active material is 50 nm to 200 nm.

[0019] (4) The present invention provides a positive electrode material as described in any one of (1) to (3) above, wherein the first positive electrode active material further comprises a carbon (C) coating portion formed on the lithium iron phosphate manganese-based compound.

[0020] (5) The present invention provides the positive electrode material of (4) above, wherein the amount of carbon contained in the coating portion is from 1.50% by weight to 3.00% by weight based on the total weight of the first positive electrode active material.

[0021] (6) The present invention provides a cathode material of any one of (1) and (2) above, wherein the lithium iron phosphate manganese-based compound has a composition represented by chemical formula 1.

[0022] [Chemical Formula 1]

[0023] Li 1+y1 Fe 1-p1-q1 Mn p1 M' q1 (PO4)

[0024] M' is selected from at least one of the following groups: nickel (Ni), cobalt (Co), aluminum (Al), zirconium (Zr), strontium (Sr), tungsten (W), molybdenum (Mo), chromium (Cr), niobium (Nb), magnesium (Mg), hafnium (Hf), tantalum (Ta), lanthanum (La), titanium (Ti), boron (B), barium (Ba), cerium (Ce), tin (Sn), yttrium (Y), and zinc (Zn).

[0025] 0≤y1<1, 0.2≤p1≤0.6, 0≤q1≤0.2.

[0026] (7) The present invention provides a positive electrode material of any one of (1) to (6) above, wherein the second positive electrode active material comprises a lithium composite transition metal oxide containing nickel.

[0027] (8) The present invention provides a positive electrode material of any one of (1) to (7) above, wherein the amount of nickel in all transition metals of the second positive electrode active material is 50 mol% or more.

[0028] (9) The present invention provides a positive electrode material of any one of (1) to (8) above, wherein the second positive electrode active material has a composition represented by chemical formula 2.

[0029] [Chemical Formula 2]

[0030] Li 1+x1 Ni a1 Co b1 M 1 c1 M 2 d1 O2

[0031] In chemical formula 2, M 1 It is selected from at least one of the groups consisting of Mn and Al. M 2 It is selected from at least one of the group consisting of Zr, Sr, W, Mo, Cr, Nb, Mg, Hf, Ta, La, Ti, B, Ba, Ce, Sn, Y, and Zn, and -0.1≤x1≤0.3, 0.50≤a1<1.00, 0.00<b1<0.50, 0.00<c1<0.50 and 0.00≤d1≤0.10.

[0032] (10) The present invention provides the positive electrode material according to any one of (1) to (9) above, wherein the average particle diameter (D 50 ) of the second positive electrode active material is 3.00 μm to 15.00 μm.

[0033] (11) The present invention provides the positive electrode material according to any one of (1) to (10) above, wherein D is 160.0 mAh / g to 200.0 mAh / g.

[0034] (12) The present invention provides the positive electrode material according to any one of (1) to (11) above, wherein T is 260.0 °C to 280.0 °C.

[0035] (13) The present invention provides the positive electrode material according to any one of (1) to (12) above, wherein H is 400.0 J / g to 900.0 J / g.

[0036] (14) The present invention provides the positive electrode material according to any one of (1) to (13) above, wherein the powder resistance is 10.0 Ω·cm to 100.0 Ω·cm.

[0037] (15) The present invention provides the positive electrode material according to any one of (1) to (14) above, wherein the content of the first positive electrode active material is 60 wt% to 80 wt% based on the total weight of the first positive electrode active material and the second positive electrode active material.

[0038] (16) The present invention provides a positive electrode comprising the positive electrode material according to any one of (1) to (15) above.

[0039] (17) The present invention provides a lithium secondary battery comprising the positive electrode according to

[16] above.

[0040] Advantageous Effects

[0041] The positive electrode material according to the present invention is controlled so that data analyzed by DSC and discharge capacity satisfy a specific relationship. Specifically, by mixing the first positive electrode active material and the second positive electrode active material such that the relationship between the maximum peak temperature according to Equation 1 described in the present specification and the discharge capacity satisfies a specific range, and the relationship between the calorific value according to Equation 2 described in the present specification and the discharge capacity satisfies a specific range, effects of improving capacity characteristics while maintaining thermal stability and improving resistance characteristics while maintaining life characteristics are realized.

[0042] Therefore, it has the effect of improving the thermal stability, capacity characteristics, lifetime characteristics and resistance characteristics of cathodes and secondary batteries including the above-mentioned cathode materials. Attached Figure Description

[0043] Figure 1 This is a graph showing the heat flow (W / g) of the battery containing the positive electrode materials according to Example 1, Comparative Examples 1 to 3 and Comparative Example 6, with temperature (°C).

[0044] Figure 2 This is a graph showing the heat flow (W / g) of the battery containing the positive electrode materials according to Examples 2 to 4 and Comparative Examples 4 and 5 at the temperature (°C).

[0045] Figure 3 It is a graph of the heat flow (W / g) of the battery containing the positive electrode material according to Comparative Example 7 at temperature (°C). Detailed Implementation

[0046] The invention will be described in more detail below to allow for a clearer understanding of it.

[0047] It should be understood that the words or terms used in the specification and claims should not be interpreted as having the meaning defined in a common dictionary, and it should also be understood that, based on the inventor's ability to appropriately define the meaning of words or terms to best explain the principles of the invention, the words or terms should be interpreted as having a meaning consistent with their meaning in the relevant field and in the context of the technical idea of ​​the invention.

[0048] It should also be understood that the terms "comprising," "including," or "having" in this specification specify the presence of the stated features, numbers, steps, elements, or combinations thereof, but do not exclude the presence or addition of one or more other features, numbers, steps, elements, or combinations thereof.

[0049] The average particle size (D) in this specification 50 The particle size distribution (D) can be defined as the particle size at 50% of the volumetric cumulative distribution on the particle size distribution curve (a graph of particle size distribution). After dispersing the target powder in a dispersion medium, the dispersion medium is introduced into a commercial laser diffraction particle size analyzer (e.g., Mastersizer 3000, Malvern Panalytical Ltd.). The particle size distribution is calculated by measuring the difference in the diffraction pattern caused by particle size as the particles pass through the laser beam. D can be measured by calculating the particle size at 50% of the volumetric cumulative distribution using the analyzer. 50 .

[0050] In this specification, "microcrystal" refers to a particle unit having substantially the same crystal orientation.

[0051] The average crystallite size in this specification can be quantitatively analyzed using X-ray diffraction (XRD) with copper (Cu) Kα X-rays. Specifically, XRD data of the synthesized cathode active material were obtained using a Bruker's D8 XRD apparatus (Cu target, voltage: 45 kV, current: 40 mA, 2θ: 10° to 80°). Structural analysis was performed on the obtained data using the Rietveld refinement method, general structural analysis methods, and Highscore software from Malvern Panalytical Ltd.

[0052] The Rietveld refinement method is a technique in which a diffraction pattern is calculated from an initial structural model that the crystal structure of the material may have, and compared with a diffraction pattern measured from an actual synthetic material. Various structural factors are introduced and gradually and repeatedly adjusted by changing their values ​​until the two patterns match well.

[0053] The method iterates until the difference between the calculated and measured patterns is minimized, while its effectiveness is evaluated based on the difference between the two patterns. Among the structural factors that may be introduced in this process, the crystal size can be obtained by using the full width at half maximum (FWHM) of the peaks appearing on each crystal plane in the measured diffraction pattern.

[0054] cathode materials

[0055] The cathode material according to the present invention will be described below.

[0056] The cathode material according to the present invention comprises a first cathode active material having an olivine structure; and a second cathode active material having a layered structure, wherein the first cathode active material comprises a lithium iron phosphate manganese-based compound having manganese (Mn) in an amount of 20 mol% to 60 mol% of all metals other than lithium, and satisfies the following equations 1 and 2.

[0057] [Equation 1]

[0058] 1.45 ≤ T / D [°C·g / mAh] ≤ 1.70

[0059] [Equation 2]

[0060] H / D [J / mAh] ≤ 5.10

[0061] In equations 1 and 2, The positive electrode includes a positive electrode active material layer, and based on the total weight of the positive electrode active material layer, the positive electrode active material layer contains 80% to 98% by weight of the positive electrode material in the lithium secondary battery comprising the positive electrode. D is the discharge capacity (mAh / g) of the battery when it is charged to 4.25 V at 25°C in constant current (CC) (0.1 C) - constant voltage (CV) (cutoff current: 0.05 C) mode and discharged to 2.5 V in CC (0.1 C) mode.

[0062] T is the temperature (°C) of the maximum peak value in the range of 200°C to 350°C when the battery is charged to 4.25 V at 25°C in CC (0.2 C)-CV (cutoff current: 0.05 C) mode and discharged to 2.5 V in CC (0.2 C) mode to perform the activation process, and then charged to 4.25 V in CC (0.2 C)-CV (cutoff current: 0.05 C) mode.

[0063] H is the calorific value (J / g) measured using a differential scanning calorimeter (DSC) in the range of 200°C to 350°C when the battery is charged to 4.25 V at 25°C in CC(0.2 C)-CV (cutoff current: 0.05 C) mode and discharged to 2.5 V in CC(0.2 C) mode to perform the activation process, and then charged to 4.25 V in CC(0.2 C)-CV (cutoff current: 0.05 C) mode.

[0064] To improve the capacity and output characteristics of olivine-structured cathode active materials and enhance the thermal stability of layered cathode active materials, cathode materials can be prepared by mixing olivine-structured and layered cathode active materials. However, depending on the type and mixing ratio of the olivine-structured and layered cathode active materials, problems arise such as poor thermal stability or discharge capacity, significant output reduction due to differences in operating voltage, and accelerated degradation of the cathode materials.

[0065] As a result of repeated research to solve these problems, the inventors have discovered that, in preparing a first positive electrode active material having an olivine structure and a second positive electrode active material having a layered structure, wherein the first positive electrode active material comprises a lithium iron phosphate manganese-based compound having manganese (Mn) in an amount of 20 mol% to 60 mol% of all metals other than lithium, and satisfying Equations 1 and 2, the capacity, lifetime, and resistance characteristics are superior compared to using the first positive electrode active material alone; the thermal stability and lifetime characteristics are superior compared to using the second positive electrode active material alone; the resistance characteristics are superior compared to the first positive electrode active material comprising a lithium iron phosphate manganese-based compound and wherein the amount of manganese (Mn) in all metals other than lithium is outside the range of 20 mol% to 60 mol%; the thermal stability or discharge capacity and lifetime characteristics are superior compared to not satisfying Equation 1; and the thermal stability and lifetime characteristics are very superior compared to not satisfying Equation 2, thereby leading to the completion of the present invention.

[0066] Equations 1 and 2 described in this specification are determined by the complex interaction of various factors, such as the composition and particle size of the cathode material, the amount of carbon (C) in the first cathode active material, the average crystallite size, the powder resistance, and the mixing ratio of the first cathode active material and the second cathode active material.

[0067] Equations 1 and 2 described in this specification represent the relationship between the discharge capacity and thermal stability of the cathode material. Since discharge capacity and thermal stability are in a trade-off relationship, cathode materials that improve discharge capacity while maintaining thermal stability must satisfy Equations 1 and 2 above.

[0068] Regarding Equations 1 and 2 described herein, for a lithium secondary battery comprising a positive electrode including a positive electrode active material layer, and based on the total weight of the positive electrode active material layer, the positive electrode active material layer containing 80% to 98% by weight of the positive electrode material, D is the discharge capacity (mAh / g) when the battery is charged to 4.25 V and discharged to 2.5 V at 25°C under CC(0.1 C)-CV (cutoff current: 0.05 C) mode equation, and T is the temperature (°C) of the maximum peak in the range of 200°C to 350°C after the battery is charged to 4.25 V and discharged to 2.5 V at 25°C under CC(0.2 C)-CV (cutoff current: 0.05 C) mode equation to perform an activation process, as measured using a differential scanning calorimeter (DSC). C) Charged to 4.25 V under the equalization mode, H is the calorific value (J / g) in the range of 200°C to 350°C when the battery is charged to 4.25 V at 25°C in CC(0.2 C)-CV (cutoff current: 0.05 C) mode and discharged to 2.5 V in CC(0.2 C) mode to perform the activation process, and then charged to 4.25 V in CC(0.2 C)-CV (cutoff current: 0.05 C) mode and then charged to 4.25 V in CC(0.2 C)-CV (cutoff current: 0.05 C) mode.

[0069] The temperature (T) and calorific value (H) of the maximum peak value in this specification are indicators of thermal stability. The temperature (T) and calorific value (H) of the maximum peak value are measured using a differential scanning calorimeter (DSC). Specifically, a graph of heat flux (W / g) versus temperature (°C) is obtained by measuring the heat flux using a differential scanning calorimeter (DSC), and the temperature (T) and calorific value (H) of the maximum peak value are derived by analyzing the graph.

[0070] Regarding the maximum peak temperature (T), when analyzing the heat flux (W / g) graph based on temperature (°C), the point with the maximum heat flux observed between 200°C and 250°C is the first peak, where the temperature of the first peak is the temperature at which the decomposition reaction of lithium complex transition metal oxide and electrolyte solution occurs intensely. Furthermore, the point with the maximum heat flux observed between 250°C and 350°C is the second peak, where the temperature of the second peak is the temperature at which the decomposition reaction of lithium iron phosphate manganese-based compound and electrolyte solution occurs intensely.

[0071] In this specification, the point with greater heat flux between the first and second peaks is defined as the maximum peak (the point with the maximum heat flux between 200°C and 350°C), and the temperature at the maximum peak is defined as the temperature (T) of the maximum peak (°C). Since the decomposition reaction of the cathode material occurs intensely at the temperature of the maximum peak, the lower the temperature of the maximum peak, the worse the thermal stability.

[0072] Regarding calorific value, when analyzing a heat flow (W / g) curve based on temperature (°C), the calorific value (H) (J / g) is defined as the value obtained by integrating the area under the heat flow curve between 200°C and 350°C and then dividing the integral by the weight of the cathode material. Since the decomposition reaction of the cathode material accelerates during heating, a higher calorific value indicates poorer thermal stability.

[0073] In the cathode material according to the present invention, Equation 1 can be calculated using the temperature relative to the maximum peak value of the discharge capacity. A smaller value in Equation 1 indicates a higher discharge capacity or a lower temperature at the maximum peak value. Since a lower temperature at the maximum peak value implies poorer thermal stability, the relationship between the discharge capacity and the temperature at the maximum peak value can be defined by considering the trade-off between discharge capacity and thermal stability.

[0074] The cathode material according to the present invention has the value of Equation 1, that is, the temperature (T) of the maximum peak value relative to the discharge capacity (D) is 1.45 to 1.70. Specifically, the temperature (T) of the maximum peak value relative to the discharge capacity (D) of the cathode material can be 1.45 or higher, 1.46 or higher, 1.47 or higher, 1.48 or higher, 1.49 or higher, 1.50 or higher, 1.51 or higher, 1.52 or higher, or 1.53 or higher, and can be 1.68 or lower, 1.69 or lower, or 1.70 or lower. Since the temperature (T) of the maximum peak value relative to the discharge capacity (D) satisfies the above range, a secondary battery with excellent capacity characteristics while maintaining thermal stability can be prepared. When the temperature (T) of the maximum peak value relative to the discharge capacity (D) is less than 1.45, there is a problem of poor thermal stability due to the low maximum peak value temperature, and when the temperature (T) of the maximum peak value relative to the discharge capacity (D) is greater than 1.70, there is a problem of poor capacity characteristics due to the low discharge capacity.

[0075] In the cathode material according to the present invention, Equation 2 can be calculated using the calorific value relative to the discharge capacity. A smaller value in Equation 2 indicates a higher discharge capacity or a lower calorific value. Since a lower calorific value implies excellent thermal stability, the relationship between discharge capacity and calorific value can be defined by considering the trade-off between discharge capacity and thermal stability.

[0076] According to Equation 2 of the present invention, the calorific value (H) relative to the discharge capacity (D) is 5.10 or less. Specifically, the calorific value (H) relative to the discharge capacity (D) of the cathode material can be 5.10 or less, 5.09 or less, 5.08 or less, 5.07 or less, 5.06 or less, or 5.05 or less. Since the calorific value (H) relative to the discharge capacity (D) satisfies the above range, a secondary battery with excellent capacity characteristics while maintaining thermal stability can be prepared. When the calorific value (H) relative to the discharge capacity (D) is greater than 5.10, the thermal stability is poor due to the very high calorific value.

[0077] The first positive electrode active material according to the present invention will be described below.

[0078] The first positive electrode active material according to the present invention comprises a lithium iron phosphate manganese-based compound having a manganese (Mn) content of 20 mol% to 60 mol% in all metals other than lithium. Specifically, the manganese (Mn) content in the first positive electrode active material in all metals other than lithium can be 20 mol% or more, 25 mol% or more, or 30 mol% or more, and can be less than 60 mol%. When the manganese (Mn) content in the first positive electrode active material is within the above range, it exhibits high energy density, enabling high capacity characteristics. When the manganese (Mn) content in all metals other than lithium is less than 20 mol%, there is a problem of poor resistivity characteristics, and when the manganese (Mn) content in all metals other than lithium is greater than 60 mol%, there is a problem of poor lifetime characteristics.

[0079] According to an embodiment of the present invention, the first positive electrode active material may have an average particle size (D) of 0.50 μm to 1.00 μm. 50 Specifically, the average particle size (D) of the first positive electrode active material 50 The average particle size can be greater than or equal to 0.50 μm, and can be less than or equal to 0.85 μm, 0.86 μm, 0.87 μm, 0.88 μm, 0.89 μm, 0.90 μm, 0.95 μm, or 1.00 μm. When the average particle size of the first positive electrode active material is within the above range, a positive electrode material with excellent energy density and improved electrode density can be prepared. Since the coating formed on the lithium iron phosphate manganese-based compound according to the present invention has a nanoscale thickness, the average particle size difference between the lithium iron phosphate manganese-based compound and the first positive electrode active material can be small.

[0080] According to embodiments of the present invention, the first positive electrode active material may have an average crystallite size of 50 nm to 200 nm. Specifically, the average crystallite size of the first positive electrode active material may be 50 nm or more, 60 nm or more, 70 nm or more, 80 nm or more, 90 nm or more, 100 nm or more, or 110 nm or more, and may be less than 120 nm, 130 nm or less, 140 nm or less, 150 nm or less, 160 nm or less, 170 nm or less, 180 nm or less, 190 nm or less, or 200 nm or less. When the average crystallite size of the first positive electrode active material is within the above range, the structural stability of the first positive electrode active material increases, and the insertion and extraction of lithium ions are more active.

[0081] According to an embodiment of the present invention, the first positive electrode active material may further include a carbon (C)-containing coating portion formed on the lithium iron phosphate manganese-based compound. The electronic conductivity of the first positive electrode active material can be improved by further including a carbon (C)-containing coating portion.

[0082] Based on the total weight of the first positive electrode active material, the amount of carbon (C) contained in the coating portion can be in the range of 1.50 wt% to 3.00 wt%. Specifically, based on the total weight of the first positive electrode active material, the amount of carbon (C) contained in the coating portion of the first positive electrode active material can be 1.50 wt% or more, 1.60 wt% or more, 1.70 wt% or more, 1.80 wt% or more, 1.90 wt% or more, 2.00 wt% or more, 2.10 wt% or more, 2.20 wt% or more, 2.30 wt% or more, 2.40 wt% or more, 2.50 wt% or more, or 2.60 wt% or more, and can be 2.90 wt% or less, or 3.00 wt% or less. When the amount of carbon (C) contained in the coating portion of the first positive electrode active material is within the above range, the coating portion may improve the electronic conductivity of the positive electrode active material without acting as a resistor.

[0083] According to an embodiment of the present invention, the coating section can be of a continuous type. In this case, lifespan characteristics and output characteristics can be improved.

[0084] According to one embodiment of the present invention, the lithium iron phosphate manganese-based compound may have a composition represented by the following chemical formula 1.

[0085] [Chemical Formula 1]

[0086] Li 1+y1 Fe 1-p1-q1 Mn p1 M′ q1 (PO4)

[0087] M' is selected from at least one of the following groups: nickel (Ni), cobalt (Co), aluminum (Al), zirconium (Zr), strontium (Sr), tungsten (W), molybdenum (Mo), chromium (Cr), niobium (Nb), magnesium (Mg), hafnium (Hf), tantalum (Ta), lanthanum (La), titanium (Ti), boron (B), barium (Ba), cerium (Ce), tin (Sn), yttrium (Y), and zinc (Zn).

[0088] 0≤y1<1, 0.2≤p1≤0.6, 0≤q1≤0.2.

[0089] M' is generally not included, but when M' is included in an appropriate amount, it can improve the particle shape of the positive electrode active material and improve the stability of the crystal structure.

[0090] y1 can be greater than or equal to 0, and can also be less than or equal to 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, or less than 1. When y1 meets the above ranges, structural stability can be improved.

[0091] P1 is the mole fraction of manganese (Mn) in all metals other than lithium in a lithium iron phosphate manganese-based compound, where p1 can be greater than 0.2, greater than 0.3, or less than 0.60. When p1 meets the above range, it exhibits high energy density, enabling high capacity characteristics.

[0092] q1 is the mole fraction of M' in all metals other than lithium in the lithium iron phosphate manganese-based compound, where q1 can be 0 or more, 0.01 or more, 0.02 or more, 0.03 or more, 0.04 or more, 0.05 or more, 0.06 or more, 0.07 or more, 0.08 or more, 0.09 or more, or 0.1 or more, and can be less than 0.11, less than 0.12, less than 0.13, less than 0.14, less than 0.15, less than 0.16, less than 0.17, less than 0.18, less than 0.19, or less than 0.2. When q1 meets the above ranges, the structural stability of the lithium iron phosphate manganese-based compound can be improved.

[0093] Next, the second positive electrode active material according to the present invention will be described.

[0094] According to embodiments of the present invention, the second positive electrode active material may comprise a lithium composite transition metal oxide containing nickel. Specifically, the second positive electrode active material may comprise a lithium composite transition metal oxide that substantially comprises nickel and contains cobalt and manganese and / or aluminum. When the second positive electrode active material comprises nickel, high capacity characteristics can be achieved.

[0095] According to an embodiment of the present invention, the amount of nickel in all transition metals of the second positive electrode active material may be 50 mol% or more. Specifically, the amount of nickel in all transition metals of the second positive electrode active material may be 50 mol% or more, 55 mol% or more, 60 mol% or more, 65 mol% or more, 70 mol% or more, 75 mol% or more, or 80 mol% or more, and may be 99 mol% or less. When the amount of nickel in all transition metals of the second positive electrode active material is within the above range, high capacity characteristics can be realized.

[0096] According to an embodiment of the present invention, the second positive electrode active material may have a composition represented by the following Chemical Formula 2.

[0097] [Chemical Formula 2]

[0098] Li 1+x1 Ni a1 Co b1 M 1 c1 M 2 d1 O2

[0099] In Chemical Formula 2, M 1 is at least one selected from the group consisting of Mn and Al, M 2 is at least one selected from the group consisting of Zr, Sr, W, Mo, Cr, Nb, Mg, Hf, Ta, La, Ti, B, Ba, Ce, Sn, Y, and Zn, and -0.1≤x1≤0.3, 0.50≤a1<1.00, 0.00<b1<0.50, 0.00<c1<0.500, and 0.00≤d1≤0.10.

[0100] M 1 may be at least one selected from Mn and Al, and M 2 may be at least one selected from Zr, Sr, W, Mo, Cr, Nb, Mg, Hf, Ta, La, Ti, B, Ba, Ce, Sn, Y, and Zn. Basically, M 2 is not included, but when M 2 is included in an appropriate amount, the particle shape of the positive electrode active material may be improved, and the stability of the crystal structure may be improved.

[0101] x1 may be -0.1 or more or 0 or more, and may be 0.1 or less, 0.2 or less, or 0.3 or less. When x1 satisfies the above range, high capacity characteristics and high energy density per unit volume can be realized.

[0102] a1 is the mole fraction of nickel (Ni) in all metals other than lithium in a lithium-ion complex transition metal oxide. It can be greater than or equal to 0.50, 0.60, 0.70, or 0.80, and less than or equal to 0.81, 0.82, 0.83, 0.84, 0.85, 0.86, 0.87, 0.88, 0.89, 0.9, 0.91, 0.92, 0.93, 0.94, 0.95, 0.96, 0.97, 0.98, 0.99, or less than 1.00. When a1 meets the above ranges, it exhibits high energy density, enabling high capacity characteristics.

[0103] b1 is the molar fraction of cobalt (Co) in all metals other than lithium in a lithium-based complex transition metal oxide. It can be greater than 0.00, 0.01, 0.02, 0.03, 0.04, or 0.05, and less than 0.06, 0.07, 0.08, 0.09, 0.10, 0.20, 0.30, 0.40, or less than 0.50. When b1 meets the above ranges, high capacity characteristics can be achieved. Furthermore, structural stability can be improved.

[0104] c1 is the mole fraction of at least one metal selected from Mn and Al in the lithium complex transition metal oxide, excluding lithium. It can be greater than 0.00, 0.01 or more, 0.02 or more, 0.03 or more, 0.04 or more, 0.05 or more, 0.06 or more, 0.07 or more, 0.08 or more, 0.09 or more, or 0.10 or more, and can be less than 0.20, 0.30 or less, 0.40 or less, or less than 0.50. When c1 meets the above ranges, high capacity characteristics can be achieved. Furthermore, high-temperature stability can be improved, and the decomposition reaction of the electrolyte solution can be relatively reduced.

[0105] d1 is the M of all metals other than lithium in lithium complex transition metal oxides. 2 The mole fraction of d1 can be greater than 0, greater than 0.01, greater than 0.02, greater than 0.03, greater than 0.04, or greater than 0.05, and can be less than 0.06, less than 0.07, less than 0.08, less than 0.09, or less than 0.10. When d1 meets the above ranges, the particle shape of the positive electrode active material can be improved, and the stability of the crystal structure can be improved.

[0106] a1, b1, c1, and d1 can satisfy a1 + b1 + c1 + d1 = 1.00.

[0107] According to embodiments of the present invention, the second positive electrode active material may have an average particle size (D) of 3.00 μm to 15.00 μm. 50 Specifically, the average particle size (D) of the second positive electrode active material 50 The particle size can be 3.00 μm or larger, 4.00 μm or larger, 5.00 μm or larger, 6.00 μm or larger, 7.00 μm or larger, 8.00 μm or larger, 9.00 μm or larger, or 10.00 μm or larger, and can be less than 11.00 μm, less than 12.00 μm, less than 13.00 μm, less than 14.00 μm, or less than 15.00 μm. The average particle size (D) of the second positive electrode active material... 50 Within the above range, the average particle size (D) of the first positive electrode active material can be adjusted. 50 The average particle size (D) of the second positive electrode active material 50 This is used to increase electrode density.

[0108] According to embodiments of the present invention, D can be in the range of 160.0 mAh / g to 200.0 mAh / g. Specifically, D can be 160.0 mAh / g or more, 161.0 mAh / g or more, or 162.0 mAh / g or more, and can be 175.0 mAh / g or less, 180.0 mAh / g or less, 185.0 mAh / g or less, 190.0 mAh / g or less, 195.0 mAh / g or less, or 200.0 mAh / g or less. When D is within the above range, there is an effect of improving capacity characteristics while maintaining the thermal stability of the cathode material by satisfying Equations 1 and 2 described in this specification.

[0109] According to embodiments of the present invention, T can be in the range of 260.0°C to 280.0°C. Specifically, T can be above 260.0°C, above 261.0°C, or above 262.0°C, and can be below 276.0°C, below 277.0°C, below 278.0°C, below 279.0°C, or below 280.0°C. When T is within the above range, there is an effect of improving capacity characteristics while maintaining the thermal stability of the cathode material by satisfying Equations 1 and 2 described in this specification.

[0110] According to embodiments of the present invention, H can be in the range of 400.0 J / g to 900.0 J / g. Specifically, H can be 400.0 J / g or more, 410.0 J / g or more, 420.0 J / g or more, 430.0 J / g or more, 440.0 J / g or more, 450.0 J / g or more, 460.0 J / g or more, 470.0 J / g or more, 480.0 J / g or more, 490.0 J / g or more, 500.0 J / g or more, 510.0 J / g or more, 520.0 J / g or more, 530.0 J / g or more, 540.0 J / g or more, or 550.0 J / g or more, and can be 860.0 J / g or less, 870.0 J / g or less, 880.0 J / g or less, 8900.0 J / g or less, or 900.0 J / g or less. When H is within the above range, there is an effect of improving capacity characteristics while maintaining the thermal stability of the cathode material by satisfying Equations 1 and 2 described in this specification.

[0111] According to embodiments of the present invention, the cathode material according to the present invention can have a powder resistivity of 10.0 Ωxcm to 100.0 Ωxcm. Specifically, the cathode material can have a powder resistivity of 10.0 Ωxcm or more, and can have a powder resistivity of 90.0 Ωxcm or less, 95.0 Ωxcm or less, or 100.0 Ωxcm or less. Powder resistivity is an indicator for evaluating the electrical performance of a material. When the powder resistivity is within the above range, there is an effect of improving the resistance characteristics and output characteristics by improving the conductivity of the cathode material, and an effect of improving the lifetime characteristics by reducing side reactions with the electrolyte solution. Powder resistivity is closely related to the carbon coating of the cathode material, and is a technical feature exhibited by comprehensively adjusting the degree of graphitization, the amount of coating portion, the amount of carbon contained in the coating portion, the shape of the coating portion, and the surface area of ​​the coating portion.

[0112] According to an embodiment of the present invention, the content of the first positive electrode active material can be from 60% to 80% by weight, based on the total weight of the first positive electrode active material and the second positive electrode active material. Specifically, based on the total weight of the first positive electrode active material and the second positive electrode active material, the content of the first positive electrode active material can be 60% or more by weight, or 70% or more by weight, and 75% or less by weight, or 80% or less by weight. In this case, there is an effect of improving capacity characteristics while maintaining the thermal stability of the positive electrode material by satisfying Equations 1 and 2 described in this specification.

[0113] The first positive electrode active material of the present invention can be prepared according to conventional methods in the art. For example, it can be prepared by using a sintering precursor and a lithium-containing raw material.

[0114] Specifically, the first positive electrode active material of the present invention can be prepared by a method for preparing a first positive electrode active material, the method comprising the following steps: (a) preparing a mixture by mixing lithium-containing raw materials, iron phosphate (FePO4), manganese-containing raw materials and phosphoric acid-containing raw materials; and (b) preparing a lithium iron phosphate manganese-based compound by sintering the mixture.

[0115] As lithium-containing raw materials, lithium-containing sulfates, nitrates, acetates, carbonates, oxalates, citrates, halides, hydroxides, or hydroxyoxides can be used, and there are no particular restrictions on the lithium-containing raw materials, as long as they can dissolve in water. Specifically, lithium-containing raw materials can be Li₂CO₃, LiNO₃, LiNO₂, LiOH, LiOH·H₂O, LiH, LiF, LiCl, LiBr, LiI, CH₃COOLi, Li₂O, Li₂SO₄, CH₃COOLi, or Li₃C₆H₅O₇, and any one or a mixture of two or more of them can be used.

[0116] The manganese (Mn)-containing raw material can be selected from at least one of MnSO4, MnCO3, Mn2O3, MnO2, Mn3O4, Mn(NO3)2, manganese acetate, manganese dicarboxylate, manganese citrate, manganese salts of fatty acids, manganese hydroxyoxide, and manganese halides such as manganese chloride, and any one of them or a mixture of two or more of them can be used.

[0117] During the preparation of the mixture in step (a), the raw materials containing doped elements, such as zirconium-containing raw materials or yttrium-containing raw materials, may be further mixed.

[0118] According to the present invention, in step (a), the lithium-containing raw material, iron phosphate (FePO4), manganese-containing raw material and phosphoric acid-containing raw material can be mixed in amounts having the composition expressed by Formula 1 as described in this specification.

[0119] After step (a), an additional step of mixing the carbon-containing raw materials may be included.

[0120] The carbon-containing raw material can be at least one selected from sucrose, glucose, polyethylene glycol, polyvinyl alcohol, and polyvinyl acetate.

[0121] Based on the total weight of the first positive electrode active material, carbon-containing raw materials can be mixed in amounts ranging from 1% to 10% by weight.

[0122] Step (b) can be used to prepare lithium iron phosphate manganese-based compounds by sintering the mixture at a temperature of 600°C to 1,000°C.

[0123] The first positive electrode active material prepared according to the method for preparing the first positive electrode active material may have the composition represented by Formula 1 as described in this specification.

[0124] The second positive electrode active material of the present invention can be prepared according to conventional methods in the art. For example, it can be prepared by sintering a positive electrode active material precursor and a lithium-containing raw material.

[0125] Specifically, the second positive electrode active material of the present invention can be prepared by a method for preparing a second positive electrode active material, the method comprising the following steps: (A) preparing a mixture by mixing a positive electrode active material precursor, which is a composite transition metal hydroxide, a composite transition metal hydroxyl oxide or a combination thereof, with a lithium-containing raw material; and (B) preparing a lithium composite transition metal oxide by sintering the mixture.

[0126] As lithium-containing raw materials, lithium-containing sulfates, nitrates, acetates, carbonates, oxalates, citrates, halides, hydroxides, or hydroxyoxides can be used, and there are no particular restrictions on the lithium-containing raw materials, as long as they can dissolve in water. Specifically, lithium-containing raw materials can be Li₂CO₃, LiNO₃, LiNO₂, LiOH, LiOH·H₂O, LiH, LiF, LiCl, LiBr, LiI, CH₃COOLi, Li₂O, Li₂SO₄, CH₃COOLi, or Li₃C₆H₅O₇, and any one or a mixture of two or more of them can be used.

[0127] The composite transition metal hydroxide, composite transition metal hydroxyl oxide, or combination thereof can be mixed with a lithium-containing raw material such that the ratio (Li / M”) of the number of moles of lithium (Li) contained in the lithium-containing raw material to the total number of moles of transition metal (M”) contained in the composite transition metal hydroxide, composite transition metal hydroxyl oxide, or combination thereof is 1.00 or more, 1.01 or more, 1.02 or more, or 1.03 or more, and 1.05 or less, 1.06 or less, 1.07 or less, 1.08 or less, 1.09 or less, or 1.10 or less.

[0128] During the preparation of the mixture in step (A), the raw material containing doped elements, such as zirconium-containing raw material or yttrium-containing raw material, may be further mixed.

[0129] According to the present invention, in step (A), the composite transition metal hydroxide containing nickel and containing cobalt, aluminum and manganese and the raw material containing lithium (Li) can be mixed in amounts having the composition represented by Formula 2 as described in this specification.

[0130] Step (B) can be a single sintering, wherein the mixture is sintered at a temperature of 700°C to 1,000°C to prepare a lithium composite transition metal oxide, or it can be a multi-stage sintering, wherein the mixture is sintered at a temperature of 700°C to 1,000°C to prepare a sintered product, and then a lithium-containing raw material is added and sintered at a temperature of 700°C to 900°C to prepare a lithium composite transition metal oxide.

[0131] Sintering can be carried out in an oxygen atmosphere.

[0132] The second positive electrode active material prepared according to the method for preparing the second positive electrode active material may have the composition represented by Formula 2 as described in this specification, and may be in the form of secondary particles.

[0133] positive electrode

[0134] Next, the positive electrode according to the present invention will be described.

[0135] The positive electrode according to the present invention comprises a positive electrode active material layer containing the positive electrode material according to the present invention. Specifically, the positive electrode comprises a positive electrode current collector and a positive electrode active material layer formed on the positive electrode current collector and comprising the positive electrode material. Since the positive electrode material has been described above, its detailed description will be omitted, and only the remaining configurations will be described in detail below.

[0136] The positive electrode current collector is not particularly limited, as long as it is conductive and does not cause chemical changes in the battery. Materials used include, for example, stainless steel, aluminum, nickel, titanium, sintered carbon or aluminum, or stainless steel surface-treated with carbon, nickel, titanium, silver, etc. Furthermore, the positive electrode current collector typically has a thickness from 3 μm to 500 μm, and microscopic irregularities can be formed on its surface to improve the adhesion of the positive electrode active material. The positive electrode current collector can be used in various shapes, such as membranes, sheets, foils, meshes, porous bodies, foams, nonwoven fabrics, etc.

[0137] In addition to the positive electrode material, the positive electrode active material layer may also contain a conductive agent and a binder. In this case, based on the total weight of the positive electrode active material layer, the content of the positive electrode material can be from 80% to 99% by weight, more specifically from 85% to 98% by weight, and excellent capacity characteristics can be obtained within this range.

[0138] Conductive agents are used to provide conductivity to the electrodes. Any conductive agent can be used without particular limitation, as long as it has suitable electronic conductivity without causing chemical changes in the battery. Specific examples of conductive agents can be graphite, such as natural or artificial graphite; carbon-based materials, such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, thermal black, and carbon fibers; powders or fibers of metals (such as copper, nickel, aluminum, and silver); conductive whiskers, such as zinc oxide whiskers and potassium titanate whiskers; conductive metal oxides, such as titanium oxide; or conductive polymers, such as polyphenylene derivatives, and any one or a mixture of two or more of them. Based on the total weight of the positive electrode active material layer, the binder content can be from 0.1% by weight to 15% by weight.

[0139] The adhesive improves the adhesion between cathode material particles and the adhesion between the cathode material and the current collector. Specific examples of the adhesive can be polyvinylidene fluoride (PVDF), polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene polymer (EPDM), sulfonated EPDM, styrene-butadiene rubber (SBR), fluororubber, or various copolymers thereof, and any one of them or a mixture of two or more of them can be used. Based on the total weight of the cathode active material layer, the adhesive content can be from 0.1% by weight to 15% by weight.

[0140] The positive electrode can be prepared according to typical methods for preparing a positive electrode, the difference being the use of the aforementioned positive electrode material. Specifically, a positive electrode active material layer forming composition, prepared by dissolving or dispersing the aforementioned positive electrode material, along with optional binders and conductive agents, in a solvent, is applied to a positive electrode current collector. The positive electrode is then obtained by drying and rolling the coated positive electrode current collector. In this case, the type and amount of the positive electrode material, binder, and conductive agent are the same as those previously described. Alternatively, as another method, the positive electrode can be prepared by casting the positive electrode active material layer forming composition onto a separate carrier, and then pressing the film layer, separated from the carrier, onto the positive electrode current collector.

[0141] The solvent can be one commonly used in the art and can include dimethyl sulfoxide (DMSO), isopropanol, N-methylpyrrolidone (NMP), acetone, or water, and any one of them or a mixture of two or more of them can be used. Considering the coating thickness and manufacturing yield of the slurry, the amount of solvent used can be sufficient if it can dissolve or disperse the positive electrode active material, conductive agent, and binder, and can allow for a viscosity that provides excellent thickness uniformity during subsequent coatings used to prepare the positive electrode.

[0142] Lithium secondary batteries

[0143] Next, the lithium secondary battery according to the present invention will be described.

[0144] This invention can prepare an electrochemical device including a positive electrode. The electrochemical device can specifically be a battery or a capacitor, and more specifically a lithium secondary battery.

[0145] A lithium secondary battery specifically includes a positive electrode, a negative electrode facing the positive electrode, a separator disposed between the positive and negative electrodes, and an electrolyte. Since the positive electrode is the same as described above, its detailed description will be omitted, and only the remaining configurations will be described in detail below.

[0146] In addition, the lithium secondary battery may optionally include a battery container that houses an electrode assembly containing a positive electrode, a negative electrode and a separator, as well as a sealing member that seals the battery container.

[0147] In a lithium secondary battery, the negative electrode includes a negative electrode current collector and a layer of negative electrode active material disposed on the negative electrode current collector.

[0148] There are no particular restrictions on the negative electrode current collector, as long as it has high conductivity without causing chemical changes in the battery. Materials such as copper, stainless steel, aluminum, nickel, titanium, sintered carbon, copper, or stainless steel surface-treated with carbon, nickel, titanium, silver, etc., as well as aluminum-cadmium alloys, can be used. Furthermore, the negative electrode current collector typically has a thickness from 3 μm to 500 μm and, similar to the positive electrode current collector, can form microscopic irregularities on its surface to improve the adhesion of the negative electrode active material. For example, the negative electrode current collector can be used in various shapes, such as films, sheets, foils, meshes, porous bodies, foams, and nonwoven fabrics.

[0149] In addition to the negative electrode active material, the negative electrode active material layer may optionally include a binder and a conductive agent.

[0150] Compounds capable of reversibly inserting and deintercalating lithium can be used as anode active materials. Specific examples of anode active materials can be carbonaceous materials, such as artificial graphite, natural graphite, graphitized carbon fibers, and amorphous carbon; metallic compounds that can form alloys with lithium, such as silicon (Si), aluminum (Al), tin (Sn), lead (Pb), zinc (Zn), bismuth (Bi), indium (In), magnesium (Mg), gallium (Ga), cadmium (Cd), Si alloys, Sn alloys, or Al alloys; metal oxides that can be doped or undoped with lithium, such as SiOβ (0<β<2), SnO2, vanadium oxide, and lithium vanadium oxide; or composite materials comprising metallic compounds and carbonaceous materials, such as Si-C composites or Sn-C composites, and any one or a mixture of two or more of these can be used. Additionally, thin films of metallic lithium can be used as anode active materials. Furthermore, both low-crystallinity and high-crystallinity carbon can be used as carbon materials. Typical examples of low-crystallinity carbon can be soft carbon and hard carbon, while typical examples of high-crystallinity carbon can be irregular, planar, sheet-like, spherical or fibrous natural or artificial graphite, Kish graphite, pyrolytic carbon, mesophase pitch-based carbon fibers, mesophase carbon microspheres, mesophase pitch and high-temperature sintered carbon, such as coke derived from petroleum or coal tar pitch.

[0151] Based on the total weight of the negative electrode active material layer, the content of the negative electrode active material can be from 80% to 99% by weight.

[0152] Adhesives are components that facilitate adhesion between conductive materials, active materials, and current collectors. Based on the total weight of the negative electrode active material layer, adhesives are typically added in amounts ranging from 0.1% to 10% by weight. Examples of adhesives include polyvinylidene fluoride (PVDF), polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene polymer (EPDM), sulfonated EPDM, styrene-butadiene rubber, nitrile rubber, fluororubber, and various copolymers thereof.

[0153] A conductive agent is a component used to further improve the conductivity of the negative electrode active material. Based on the total weight of the negative electrode active material layer, the content of the conductive agent can be less than 10% by weight, specifically less than 5% by weight. There are no particular limitations on the conductive agent, as long as it is conductive without causing chemical changes in the battery. For example, conductive materials such as: graphite, such as natural or artificial graphite; carbon black, such as acetylene black, Ketjen black, channel black, furnace black, lamp black, and thermal black; conductive fibers, such as carbon fibers or metal fibers; fluorocarbons; metal powders, such as aluminum powder and nickel powder; conductive whiskers, such as zinc oxide whiskers and potassium titanate whiskers; conductive metal oxides, such as titanium oxide; or polyphenylene derivatives.

[0154] A composition for forming a negative electrode active material layer is prepared by dissolving or dispersing an optional binder and conductive agent, along with a negative electrode active material, in a solvent and drying the coated negative electrode current collector. The negative electrode active material layer can be prepared by coating the negative electrode active material layer forming composition onto the negative electrode current collector, or by casting the negative electrode active material layer forming composition onto a separate carrier and then pressing the film layer, separated from the carrier, onto the negative electrode current collector.

[0155] In lithium-ion secondary batteries, the separator separates the negative and positive electrodes and provides a path for lithium ions to move. Any separator can be used without particular limitation, as long as it is commonly used in lithium-ion secondary batteries. Separators with high moisture retention capacity for the electrolyte and low resistance to electrolyte ion transfer are particularly preferred. Specifically, porous polymer membranes can be used, such as porous polymer membranes prepared from polyolefin-based polymers (e.g., ethylene homopolymers, propylene homopolymers, ethylene / butene copolymers, ethylene / hexene copolymers, and ethylene / methacrylate copolymers), or laminated structures having two or more layers. Furthermore, typical porous nonwoven fabrics can be used, such as nonwoven fabrics formed from high-melting-point glass fibers or polyethylene terephthalate fibers. In addition, coated separators including ceramic components or polymer materials can be used to ensure heat resistance or mechanical strength, and separators with single-layer or multi-layer structures can optionally be used.

[0156] Furthermore, the electrolyte used in this invention may include organic liquid electrolytes, inorganic liquid electrolytes, solid polymer electrolytes, gel polymer electrolytes, solid inorganic electrolytes, or molten inorganic electrolytes that can be used to prepare lithium secondary batteries, but this invention is not limited thereto.

[0157] Specifically, the electrolyte may contain organic solvents and lithium salts.

[0158] Any organic solvent can be used without particular limitation, as long as it serves as a medium through which ions involved in the electrochemical reactions of the battery can move. Specifically, ester-based solvents, such as methyl acetate, ethyl acetate, γ-butyrolactone, and ε-caprolactone; ether-based solvents, such as dibutyl ether or tetrahydrofuran; ketone-based solvents, such as cyclohexanone; aromatic solvents, such as benzene and fluorobenzene; or carbonate-based solvents, such as dimethyl carbonate (DMC), diethyl carbonate (DEC), methyl ethyl carbonate (EMC), ethylene carbonate (EC), and propylene carbonate (PC); alcohol-based solvents, such as ethanol and isopropanol; nitriles, such as R-CN (where R is a straight-chain, branched, or cyclic C2-C20 hydrocarbon group, and may include double-bonded aromatic rings or ether bonds); amides, such as dimethylformamide; dioxolane, such as 1,3-dioxolane; or sulfolane can be used as organic solvents. Among these solvents, carbonate solvents are preferred, and mixtures of cyclic carbonates (e.g., ethylene carbonate or propylene carbonate) with high ionic conductivity and high dielectric constant and low viscosity linear carbonate compounds (e.g., ethyl methyl carbonate, dimethyl carbonate, or diethyl carbonate) are even more preferred, as this can improve the charge / discharge performance of the battery. In this case, the performance of the electrolyte solution can be excellent when cyclic carbonates and linear carbonates are mixed in a volume ratio of about 1:1 to about 1:9.

[0159] Lithium salts can be used without any specific limitations, as long as they are compounds capable of providing lithium ions for lithium secondary batteries. Specifically, LiPF6, LiClO4, LiAsF6, LiBF4, LiSbF6, LiAlO4, LiAlCl4, LiCF3SO3, LiC4F9SO3, LiN(C2F5SO3)2, LiN(C2F5SO2)2, LiN(CF3SO2)2, LiCl, LiI, or LiB(C2O4)2 can be used as lithium salts. Lithium salts can be used in concentration ranges from 0.1 M to 5.0 M, particularly from 0.1 M to 3.0 M. If the concentration of the lithium salt is within the above range, excellent electrolyte performance can be obtained due to the electrolyte having suitable conductivity and viscosity, and lithium ions can move efficiently.

[0160] To improve battery life characteristics, suppress battery capacity reduction, and improve battery discharge capacity, in addition to the electrolyte components mentioned above, the electrolyte may also include at least one additive, such as compounds based on haloalkyl carbonates like difluoroethylene carbonate, pyridine, triethyl phosphite, triethanolamine, cyclic ethers, ethylenediamine, n-glycol dimethyl ether, triammonium hexaphosphate, nitrobenzene derivatives, sulfur, quinone imine dyes, N-substituted oxazolidinones, N,N-substituted imidazolides, ethylene glycol dialkyl ethers, ammonium salts, pyrrole, 2-methoxyethanol, or aluminum trichloride. In this case, based on the total weight of the electrolyte, the content of the additive can be from 0.1% by weight to 10% by weight, specifically from 0.1% by weight to 5% by weight.

[0161] Because lithium secondary batteries containing the positive electrode active material according to the invention exhibit excellent capacity and efficiency characteristics as described above, they are suitable for portable devices such as mobile phones, laptops and digital cameras, as well as electric vehicles such as hybrid electric vehicles (HEVs).

[0162] Therefore, according to another embodiment of the present invention, a battery module including a lithium secondary battery as a unit battery and a battery pack including the battery module are provided.

[0163] Battery modules or battery packs can be used as a power source for at least one medium-sized and large unit of power tools; electric vehicles, including electric vehicles (EVs), hybrid electric vehicles and plug-in hybrid electric vehicles (PHEVs); or power storage systems.

[0164] The shape of the lithium secondary battery of the present invention is not particularly limited, but it can be cylindrical, prismatic, pouch-shaped or coin-shaped.

[0165] The lithium secondary battery described in this invention can be used not only as a power source for small devices in single-cell batteries, but also as a unit battery in medium and large battery modules containing multiple single-cell batteries.

[0166] In the following, examples of the invention will be described in detail in a manner readily practiced by those skilled in the art. However, the invention can be embodied in many different forms and should not be construed as limited to the examples set forth herein.

[0167] Example

[0168] Preparation Example

[0169] Preparation Example 1

[0170] Li₂CO₃, MnCO₃, FePO₄, and NH₄H₂PO₄ were mixed to achieve a Li:Mn:Fe:PO₄ molar ratio of 1.02:0.6:0.4:1. This mixture was then combined with water to achieve a solids concentration of 30% by weight. Finally, the mixture was wet-milled using a bead mill to prepare a slurry (D). 50 (200 nm). The slurry was then mixed with sucrose to prepare a mixture. In this case, sucrose was mixed in an amount of 8 parts by weight based on the total weight of 100 parts by weight of Li₂CO₃, MnCO₃, FePO₄, and NH₄H₂PO₄.

[0171] The mixture was spray-dried (inlet temperature 230°C, outlet temperature 95°C) and then sintered at 730°C for 10 hours in a nitrogen atmosphere to prepare the first positive electrode active material, which has an olivine structure and is composed of LiMn. 0.6 Fe 0.4 PO4 represents a carbon (C)-containing coating formed on a lithium iron phosphate manganese-based compound. The carbon-containing coating is a film type, and the amount of carbon contained in the coating is 2.62% by weight based on the total weight of the first positive electrode active material.

[0172] Preparation Example 2

[0173] Li₂CO₃, MnCO₃, FePO₄, and NH₄H₂PO₄ were mixed to achieve a Li:Mn:Fe:PO₄ molar ratio of 1.02:0.3:0.7:1. This mixture was then combined with water to achieve a solids concentration of 30% by weight. Finally, the mixture was wet-milled using a bead mill to prepare a slurry (D). 50 (200 nm). The slurry is then mixed with sucrose to prepare a mixture. In this case, sucrose is mixed in amounts of 10 parts by weight based on the total weight of 100 parts by weight of Li₂CO₃, MnCO₃, FePO₄, and NH₄H₂PO₄.

[0174] The mixture was spray-dried (inlet temperature 230°C, outlet temperature 95°C) and then sintered at 760°C for 10 hours in a nitrogen atmosphere to prepare the first positive electrode active material, which has an olivine structure and is composed of LiMn. 0.3 Fe 0.7 PO4 represents a carbon (C)-containing coating formed on a lithium iron phosphate manganese-based compound. The carbon-containing coating is a film type, and the amount of carbon contained in the coating is 2.81% by weight based on the total weight of the first positive electrode active material.

[0175] Preparation Example 3

[0176] Li₂CO₃, MnCO₃, FePO₄, and LiH₂PO₄ were mixed to achieve a Li:Mn:Fe:PO₄ molar ratio of 1.02:0.3:0.7:1. This mixture was then combined with water to achieve a solids content concentration of 35% by weight. Finally, the mixture was wet-milled using a bead mill to prepare a slurry (D). 50 (400 nm). Subsequently, the slurry is mixed with sucrose to prepare a mixture. In this case, sucrose is mixed in amounts of 10 parts by weight based on the total weight of 100 parts by weight of Li₂CO₃, MnCO₃, FePO₄, and LiH₂PO₄.

[0177] The mixture was spray-dried (inlet temperature 230°C, outlet temperature 95°C) and then sintered at 740°C for 10 hours in a nitrogen atmosphere to prepare the first positive electrode active material, which has an olivine structure and is composed of LiMn. 0.3 Fe 0.7 PO4 represents a carbon (C)-containing coating formed on a lithium iron phosphate manganese-based compound. The carbon-containing coating is a film type, and the amount of carbon contained in the coating is 2.98% by weight based on the total weight of the first positive electrode active material.

[0178] Preparation Example 4

[0179] Li₂CO₃, MnCO₃, FePO₄, and LiH₂PO₄ were mixed to achieve a Li:Mn:Fe:PO₄ molar ratio of 1.02:0.3:0.7:1. This mixture was then combined with water to achieve a solids content concentration of 35% by weight. Finally, the mixture was wet-milled using a bead mill to prepare a slurry (D). 50 (400 nm). Subsequently, the slurry is mixed with sucrose to prepare a mixture. In this case, sucrose is mixed in an amount of 6 parts by weight based on the total weight of 100 parts by weight of Li₂CO₃, MnCO₃, FePO₄, and LiH₂PO₄.

[0180] The mixture was spray-dried (inlet temperature 230°C, outlet temperature 95°C) and then sintered at 740°C for 10 hours in a nitrogen atmosphere to prepare the first positive electrode active material, which has an olivine structure and is composed of LiMn. 0.3 Fe 0.7 PO4 represents a carbon (C)-containing coating formed on a lithium iron phosphate manganese-based compound. The carbon-containing coating is a film type, and the amount of carbon contained in the coating is 1.73% by weight based on the total weight of the first positive electrode active material.

[0181] Comparative Preparation Example 1

[0182] Li₂CO₃, MnCO₃, FePO₄, and NH₄H₂PO₄ were mixed to achieve a Li:Mn:Fe:PO₄ molar ratio of 1.02:0.3:0.7:1. This mixture was then combined with water to achieve a solids concentration of 30% by weight. Finally, the mixture was wet-milled using a bead mill to prepare a slurry (D). 50 (200 nm). The slurry is then mixed with sucrose to prepare a mixture. In this case, sucrose is mixed in amounts of 5 parts by weight, based on the total weight of 100 parts by weight of Li₂CO₃, MnCO₃, FePO₄, and NH₄H₂PO₄.

[0183] The mixture was spray-dried (inlet temperature 230°C, outlet temperature 95°C) and then sintered at 760°C for 10 hours in a nitrogen atmosphere to prepare the first positive electrode active material, which has an olivine structure and is composed of LiMn. 0.3 Fe 0.7 PO4 represents a carbon (C)-containing coating formed on a lithium iron phosphate manganese-based compound. The carbon-containing coating is a film type, and the amount of carbon contained in the coating is 2.07% by weight based on the total weight of the first positive electrode active material.

[0184] Comparative Preparation Example 2

[0185] Li₂CO₃ and FePO₄ were mixed to a Li:Fe:PO₄ molar ratio of 1.05:1:1, and then mixed with water to achieve a solid content concentration of 40% by weight. The mixture was then wet-milled using a bead mill to prepare a slurry (D). 50 (200 nm). The slurry was then mixed with sucrose to prepare a mixture. In this case, sucrose was mixed in an amount of 12 parts by weight, based on 100 parts by weight of the total weight of Li₂CO₃ and FePO₄.

[0186] The mixture was spray-dried (inlet temperature 230°C, outlet temperature 95°C) and then sintered at 700°C for 10 hours in a nitrogen atmosphere to prepare a first positive electrode active material having an olivine structure and a carbon-containing (C) coating formed on a lithium iron phosphate manganese-based compound having a composition represented by LiFePO4. Based on the total weight of the first positive electrode active material, the amount of carbon contained in the coating is 2.60% by weight.

[0187] Examples and Comparative Examples

[0188] Example 1

[0189] NiSO4, CoSO4, MnSO4, and Al(OH)3 were dissolved in deionized water to prepare a 2M composite transition metal aqueous solution with a nickel:cobalt:manganese:aluminum molar ratio of 81:5:12:2. Inlet pipes for the composite transition metal aqueous solution, a 25 wt% NaOH aqueous solution, and a 15 wt% NH4OH aqueous solution were connected to a 200 L batch reactor. While the reactor was maintained at 56°C, dissolved oxygen was removed by purging with N2 gas to create a non-oxidizing atmosphere. Subsequently, the composite transition metal aqueous solution was continuously added to the reactor at a flow rate of 0.25 L / hr while stirring at 250 rpm. Then, the co-precipitation process and concentration were repeated 4 to 5 times over 6 hours to grow composite transition metal hydroxide particles, and the target particle size (D) was reached. 50 When the particle size reaches 10 μm, the addition of the aqueous solution of the complex transition metal hydroxide is terminated. After terminating the addition of the aqueous solution, the particles are separated from the reaction solution and then dried at 130 °C for 24 hours to prepare a product with Ni 0.81 Co 0.05 Mn 0.12 Al 0.02 (OH)2 represents the composition of the second positive electrode active material precursor (composite transition metal hydroxide).

[0190] LiOHH2O and composite transition metal hydroxide (Ni) 0.81 Co 0.05 Mn 0.12 Al 0.02 (OH)2) was mixed to achieve a Li:(Ni+Co+Mn) molar ratio of 1.03:1, and then sintered at 840°C in an oxygen atmosphere to prepare a product with LiNi 0.81 Co 0.05 Mn 0.12 Al 0.02 O2 represents the composition of the second positive electrode active material (lithium composite transition metal oxide).

[0191] The cathode material was prepared by mixing the first cathode active material prepared in Preparation Example 1 with the second cathode active material described above at a weight ratio of 70:30. That is, based on the total weight of the first cathode active material and the second cathode active material, the content of the first cathode active material was 70% by weight.

[0192] Example 2

[0193] The positive electrode material was prepared by mixing the first positive electrode active material prepared in Example 2 and the second positive electrode active material prepared in Example 1 at a weight ratio of 70:30. That is, based on the total weight of the first positive electrode active material and the second positive electrode active material, the content of the first positive electrode active material was 70% by weight.

[0194] Example 3

[0195] The positive electrode material was prepared by mixing the first positive electrode active material prepared in Example 3 and the second positive electrode active material prepared in Example 1 at a weight ratio of 70:30. That is, based on the total weight of the first positive electrode active material and the second positive electrode active material, the content of the first positive electrode active material was 70% by weight.

[0196] Example 4

[0197] The positive electrode material was prepared by mixing the first positive electrode active material prepared in Example 4 and the second positive electrode active material prepared in Example 1 at a weight ratio of 70:30. That is, based on the total weight of the first positive electrode active material and the second positive electrode active material, the content of the first positive electrode active material was 70% by weight.

[0198] Comparative Example 1

[0199] The first positive electrode active material prepared in Preparation Example 1 was used as the positive electrode material in Comparative Example 1.

[0200] Comparative Example 2

[0201] The positive electrode material was prepared by mixing the first positive electrode active material prepared in Example 1 and the second positive electrode active material prepared in Example 1 at a weight ratio of 80:20. That is, based on the total weight of the first positive electrode active material and the second positive electrode active material, the content of the first positive electrode active material was 80% by weight.

[0202] Comparative Example 3

[0203] The positive electrode material was prepared by mixing the first positive electrode active material prepared in Example 1 and the second positive electrode active material prepared in Example 1 at a weight ratio of 60:40. That is, based on the total weight of the first positive electrode active material and the second positive electrode active material, the content of the first positive electrode active material was 60% by weight.

[0204] Comparative Example 4

[0205] The first positive electrode active material prepared in Preparation Example 2 was used as the positive electrode material in Comparative Example 4.

[0206] Comparative Example 5

[0207] A positive electrode material was prepared by mixing the first positive electrode active material prepared in Comparative Preparation Example 1 and the second positive electrode active material prepared in Example 1 at a weight ratio of 70:30. That is, based on the total weight of the first positive electrode active material and the second positive electrode active material, the content of the first positive electrode active material was 70% by weight.

[0208] Comparative Example 6

[0209] The second positive electrode active material prepared in Example 1 was used as the positive electrode material in Comparative Example 6.

[0210] Comparative Example 7

[0211] A positive electrode material was prepared by mixing the first positive electrode active material prepared in Example 2 and the second positive electrode active material prepared in Example 1 at a weight ratio of 70:30. That is, based on the total weight of the first positive electrode active material and the second positive electrode active material, the content of the first positive electrode active material was 70% by weight.

[0212] Experimental Example

[0213] Experimental Example 1: Battery Characteristic Evaluation 1

[0214] - Preparation of coin-type half-cell

[0215] A positive electrode slurry was prepared by mixing 90 wt% of each of the positive electrode materials prepared in the examples and comparative examples, 5.0 wt% of carbon black as a conductive agent, and 5.0 wt% of polyvinylidene fluoride (PVDF) as a binder in an N-methylpyrrolidone (NMP) solvent. One surface of an aluminum current collector was coated with the above-prepared positive electrode slurry, dried at 130°C, and then rolled to have a porosity of 30% to prepare each positive electrode.

[0216] A lithium metal electrode is used as the negative electrode, and the electrode assembly is prepared by placing a porous polyethylene membrane between the positive and negative electrodes. A coin-shaped half-cell is prepared by placing the electrode assembly in a battery casing and injecting an electrolyte solution in which 1.0 M LiPF6 is dissolved in an organic solvent containing a mixture of ethylene carbonate (EC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC) in a volume ratio of 3:4:3.

[0217] After fabricating the coin-shaped half-cell, the capacity characteristics and thermal stability of the cell were evaluated using the following methods.

[0218] -Evaluation of capacity characteristics

[0219] Each coin-type half-cell was charged (0.1 C, cutoff current: 0.05 C) to 4.25 V in constant current-constant voltage (CC-CV) mode at 25°C, and then discharged (0.1 C) to 2.5 V in CC mode, and the discharge capacity (mAh / g) under these conditions was measured. The measured discharge capacity (D) (mAh / g) is presented in Table 1 below.

[0220] - Evaluation of thermal stability

[0221] Each coin-type half-cell is charged to 4.25V in CC-CV mode at 25°C (0.2C, cutoff current: 0.05C) and then discharged to 2.5V in CC mode (0.2C) to perform the formation process.

[0222] After the formation process, thermal stability was assessed using differential scanning calorimetry (DSC).

[0223] Specifically, after the battery undergoing formation was charged to 4.25 V at 25°C in CC-CV mode (0.2 C, cutoff current: 0.05 C), the battery was disassembled in a charged state to wash the positive electrode with DMC. The positive electrode was then positioned within the battery casing for DSC, and an electrolyte solution was injected to prepare the battery for DSC. In this electrolyte solution, 1.0 M LiPF6 was dissolved in an organic solvent in which ethylene carbonate (EC): ethyl methyl carbonate (EMC): diethyl carbonate (DEC) were mixed in a volume ratio of 1:2:1. Heat flow was measured while the battery for DSC was heated at 10°C / min using a DSC (DSC3, Mettler Toredo, LLC). The resulting graph of heat flow (W / g) based on temperature (°C) is shown in [the figure]. Figures 1 to 3 The results are shown in Table 1 below, and the calorific value (H) (J / g) and temperature (T) (°C) of the maximum peak are presented. Furthermore, the temperature (T / D) (°C·g / mAh) of the maximum peak relative to the discharge capacity and the calorific value (H / D) (J / mAh) relative to the discharge capacity are calculated and presented in Table 1 below.

[0224] In this case, the calorific value (H) (J / g) is obtained by integrating the area under the heat flow curve between 200°C and 350°C according to the heat flow (W / g) curve based on temperature (°C), and then dividing the integral value by the weight of the cathode material. The temperature of the maximum peak (T) (°C) is the temperature at the point (maximum peak) of the maximum heat flow between 200°C and 350°C according to the heat flow (W / g) curve based on temperature (°C).

[0225] Figure 1It is a graph showing the heat flow (W / g) of the battery with positive electrode materials including Example 1, Comparative Examples 1 to 3 and Comparative Example 6, based on temperature (°C).

[0226] Figure 2 This is a graph showing the heat flow (W / g) of batteries containing the cathode materials of Examples 2 to 4 and Comparative Examples 4 and 5 at temperature (°C).

[0227] Figure 3 This is a graph showing the heat flow (W / g) of a battery containing the cathode material of Comparative Example 7 at temperature (°C).

[0228] according to Figures 1 to 3 It can be confirmed that the batteries containing the cathode materials of Examples 1 to 4 have a maximum peak temperature (T) of 260.0°C to 280.0°C and a maximum peak heat flux of less than 3 W / g.

[0229] [Table 1]

[0230] Referring to Table 1, it was confirmed that the batteries comprising the cathode materials of Examples 1 to 4 have a D of 160.0 mAh / g to 200.0 mAh / g, a T of 260.0 °C to 280.0 °C, and an H of 400.0 J / g to 900.0 J / g. Furthermore, it was confirmed that the T / D ratio according to Equation 1 described in this specification is in the range of 1.45 to 1.70, and the H / D ratio according to Equation 2 described in this specification is 5.10 or less. In contrast, it was confirmed that the batteries comprising the cathode materials of Comparative Examples 1, 2, 4, and 5 have a D of less than 160.0 mAh / g or greater than 200.0 mAh / g, the batteries comprising the cathode materials of Comparative Examples 3 to 6 have an H of less than 400.0 J / g or greater than 900.0 J / g, and the batteries comprising the cathode materials of Comparative Examples 1, 3, 6, and 7 have a T of less than 260.0 °C or greater than 280.0 °C. Furthermore, it was confirmed that the batteries containing the positive electrode materials of Comparative Examples 1, 2, 4 and 7 have a T / D of less than 1.45 or greater than 1.70 according to Equation 1 described herein, and the batteries containing the positive electrode materials of Comparative Examples 3 and 5 have an H / D of greater than 5.10 according to Equation 2 described herein. It was also confirmed that the positive electrode material of Comparative Example 6 has a T / D of less than 1.45 according to Equation 1 described herein and an H / D of greater than 5.10 according to Equation 2.

[0231] Therefore, for cathode materials that satisfy Equations 1 and 2 according to this specification within a specific range, it has been confirmed that capacity characteristics are improved while maintaining thermal stability.

[0232] Experimental Example 2: PSA Analysis

[0233] The average particle size (D) of each of the first positive electrode active materials in the preparation examples and comparative preparation examples was measured using a particle size analyzer (PSA) (Mastersizer 3000, Malvern Panalytical Ltd.). 50 ), and is presented in Table 2 below.

[0234] [Table 2]

[0235] According to Table 2, the first positive electrode active materials prepared in Examples 1 to 4 were confirmed to have an average particle size (D) of 0.50 μm to 1.00 μm. 50 In contrast, the first positive electrode active materials of Comparative Examples 1 and 2 were confirmed to have an average particle size (D) of less than 0.50 μm or greater than 1.00 μm. 50 ).

[0236] Experiment Example 3: XRD Analysis

[0237] After X-ray diffraction (XRD) measurements were performed on each of the first positive electrode active materials prepared in the preparation examples and comparative preparation examples, XRD data analysis was performed, and the average crystallite size (nm) is presented in Table 3 below.

[0238] Specifically, XRD measurements were performed using a Bruker D8 XRD instrument, and 2 g to 3 g of particles were collected from the first positive electrode active material powder and measured with Cu-Kα radiation (wavelength 1.54 Å) at a scan rate of 0.2° / sec and a 2θ range of 10° to 80° under conditions of an accelerating voltage of 45 kV and a current of 40 mA.

[0239] [Table 3]

[0240] According to Table 3, the first positive electrode active materials prepared in Examples 1 to 4 and Comparative Examples 1 and 2 were confirmed to have an average crystallite size of 50 nm to 200 nm.

[0241] Experiment Example 4: Measurement of Carbon (C) Content

[0242] The amount of carbon (C) in each of the first positive electrode active materials of the preparation examples and comparative preparation examples was measured, and the amount of carbon (C) relative to the total weight of the first positive electrode active materials (carbon (C) content (weight %) of the first positive electrode active materials) is presented in Table 4 below.

[0243] The amount of carbon was measured using a carbon and sulfur analyzer (CS844, LECO Corporation). Specifically, analysis was performed automatically when a 1g sample of the first positive electrode active material powder was collected, placed in a crucible, and installed in a high-frequency induction furnace. The carbon gas from the sample generated in the high-frequency induction furnace combined with O2 as a combustion gas to produce CO and CO2. Since C was measured by a CO2 infrared detector, the CO gas was completely converted to CO2 via CuO. The amount of carbon in the CO2 gas was then measured by the detector based on the infrared absorption of CO2.

[0244] [Table 4]

[0245] According to Table 4, it was confirmed that the first positive electrode active material prepared in Examples 1 to 4 had an amount of carbon (C) contained in the coating portion of 1.50% to 3.00% by weight based on the total weight of the first positive electrode active material.

[0246] Experimental Example 5: Evaluation of Powder Resistance

[0247] Five g of each cathode material from the examples and comparative examples were placed into a circular 4-Point Probe (GoldPin) mold with a diameter of 22 mm, and resistivity measurement was performed using a Hantech Co., Ltd. resistivity measurement system under an applied pressure of 2000 kgf / cm². 2 The volume resistivity was measured under the condition of powder resistance and expressed as powder resistance (Ω x cm), as shown in Table 5 below.

[0248] [Table 5]

[0249] According to Table 5, the cathode materials of Examples 1 to 4 were confirmed to have a powder resistance of 10.0 Ωxcm to 100.0 Ωxcm. In contrast, the cathode materials of Comparative Examples 1 and 2 were confirmed to have a powder resistance of less than 10.0 Ωxcm, and the cathode materials of Comparative Examples 5 and 6 were confirmed to have a powder resistance of greater than 100.0 Ωxcm. In particular, with the cathode material of Comparative Example 5, which has the same composition as Example 2 but has a high powder resistance, it was confirmed that the powder resistance is closely related to the carbon coating of the cathode material, and is a technical feature that appears by comprehensively controlling the degree of graphitization, the amount of coating portion, the amount of carbon contained in the coating portion, the shape of the coating portion, and the surface area of ​​the coating portion.

[0250] Experimental Example 6: Battery Characteristic Evaluation 2

[0251] For the coin-shaped half-cell prepared in Experimental Example 1, the following methods were used to evaluate the battery's lifespan and resistance characteristics.

[0252] - Evaluation of lifetime and resistance characteristics

[0253] For each coin cell, a cycle is defined as charging the coin cell to 4.25 V in CC-CV mode (0.1 C, cutoff current: 0.05 C) and discharging it to 2.5 V in CC mode at 25°C (0.1 C) to form a cycle. This cycle is repeated for a total of 30 charge and discharge cycles. After measuring the discharge capacity in the 1st and 30th cycles, the percentage of the discharge capacity in the 30th cycle to the discharge capacity in the 1st cycle (capacity retention) is calculated. 100 (%), and the results are presented in Table 6 below.

[0254] Furthermore, the resistance immediately following the 30th cycle (resistance (Ω) in the 30th cycle) was calculated, and the results are presented in Table 6 below. The resistance immediately following the 30th cycle was calculated by dividing the difference between the voltage before discharge in the 30th cycle and the voltage 60 seconds after discharge by the applied current.

[0255] [Table 6]

[0256] According to Table 6, it was confirmed that the batteries containing the cathode materials of Examples 1 to 4 had a resistance of less than 45.0 Ω and a capacity retention rate of more than 97.0% (%) during the 30th cycle. In contrast, it was confirmed that the batteries containing the cathode materials of Comparative Examples 2 and 5 had a resistance greater than 45.0 Ω and a capacity retention rate of less than 97.0% (%) during the 30th cycle; the batteries containing the cathode materials of Comparative Examples 1, 4, and 7 had a capacity retention rate of more than 97.0% (%) but a resistance greater than 45.0 Ω during the 30th cycle; and the batteries containing the cathode materials of Comparative Examples 3 and 6 had a resistance of less than 45.0 Ω and a capacity retention rate of less than 97.0% (%) during the 30th cycle. As a result, it was confirmed that the resistance characteristics can be improved while maintaining the lifetime characteristics, regarding cathode materials that satisfy Equations 1 and 2 described in this specification within a specific range.

Claims

1. A cathode material comprising: A first positive electrode active material having an olivine structure; and a second positive electrode active material having a layered structure. The first positive electrode active material comprises a lithium iron phosphate manganese-based compound, wherein the lithium iron phosphate manganese-based compound has manganese (Mn) comprising 20 mol% to 60 mol% of all metals other than lithium, and Satisfying Equations 1 and 2: [Equation 1] 1.45 ≤ T / D [°C·g / mAh] ≤ 1.70 [Equation 2] H / D [J / mAh] ≤ 5.10 in, In equations 1 and 2, For a lithium secondary battery comprising a positive electrode as described below, the positive electrode includes a positive electrode active material layer, and based on the total weight of the positive electrode active material layer, the positive electrode active material layer contains 80% to 98% by weight of the positive electrode material. D is the discharge capacity, expressed in mAh / g, when the battery is charged to 4.25 V at 25°C in a constant current (CC)-constant voltage (CV) mode with a cutoff current of 0.05 C and discharged to 2.5 V in a 0.1 C CC mode. T is the maximum peak temperature, expressed in °C, observed between 200 °C and 350 °C when the battery is charged to 4.25 V at 25 °C with a 0.2 C CC-CV and a cutoff current of 0.05 C, discharged to 2.5 V at 0.2 C CC mode to perform the activation process, and then charged to 4.25 V again with a 0.2 C CC-CV and a cutoff current of 0.05 C mode, using a differential scanning calorimeter (DSC). H is the calorific value in J / g measured using a differential scanning calorimeter (DSC) in the range of 200°C to 350°C after the battery is charged to 4.25 V at 25°C with a 0.2 C CC-CV and a cutoff current of 0.05 C, discharged to 2.5 V in a 0.2 C CC mode to perform an activation process, and then charged to 4.25 V again with a 0.2 C CC-CV and a cutoff current of 0.05 C.

2. The cathode material as described in claim 1, wherein, The average particle size D of the first positive electrode active material 50 The range is from 0.50 μm to 1.00 μm.

3. The cathode material as described in claim 1, wherein, The average crystallite size of the first positive electrode active material is 50 nm to 200 nm.

4. The cathode material as described in claim 1, wherein, The first positive electrode active material further includes a carbon (C) coating formed on the lithium iron phosphate manganese-based compound.

5. The cathode material as described in claim 4, wherein, Based on the total weight of the first positive electrode active material, the amount of carbon contained in the coating portion is from 1.50% to 3.00% by weight.

6. The cathode material as described in claim 1, wherein, The lithium iron phosphate manganese-based compound has a composition represented by chemical formula 1: [Chemical Formula 1] Li 1+y1 Fe 1-p1-q1 Mn p1 M’ q1 (PO4) In chemical formula 1, M' is selected from at least one of the following groups: nickel (Ni), cobalt (Co), aluminum (Al), zirconium (Zr), strontium (Sr), tungsten (W), molybdenum (Mo), chromium (Cr), niobium (Nb), magnesium (Mg), hafnium (Hf), tantalum (Ta), lanthanum (La), titanium (Ti), boron (B), barium (Ba), cerium (Ce), tin (Sn), yttrium (Y), and zinc (Zn). 0≤y1<1, 0.2≤p1≤0.6, 0≤q1≤0.

2.

7. The cathode material as described in claim 1, wherein, The second cathode active material includes a lithium composite transition metal oxide including Ni.

8. The cathode material as described in claim 1, wherein, An amount of the Ni among all transition metals of the second cathode active material is 50 mol% or greater.

9. The cathode material as described in claim 1, wherein, The second cathode active material has a composition represented by Chemical Formula 2. [Chemical Formula 2] Li 1+x1 Ni a1 Co b1 M 1 c1 M 2 d1 O2 In Chemical Formula 2, M 1 It is selected from at least one of the groups consisting of Mn and Al. M 2 It is selected from at least one of the group consisting of Zr, Sr, W, Mo, Cr, Nb, Mg, Hf, Ta, La, Ti, B, Ba, Ce, Sn, Y, and Zn, and -0.1≤x1≤0.3, 0.50≤a1<1.00, 0.00<b1<0.50, 0.00<c1<0.50, and 0.00≤d1≤0.

10.

10. The cathode material as described in claim 1, wherein, The average particle size D of the second positive electrode active material 50 The range is from 3.00 μm to 15.00 μm.

11. The cathode material as described in claim 1, wherein, D is 160.0 mAh / g to 200.0 mAh / g.

12. The cathode material as described in claim 1, wherein, T is 260.0° C. to 280.0° C.

13. The cathode material as described in claim 1, wherein, H is 400.0 J / g to 900.0 J / g.

14. The cathode material as described in claim 1, wherein, a powder resistance is 10.0 Ω×cm to 100.0 Ω×cm.

15. The cathode material as described in claim 1, wherein, Based on a total weight of the first cathode active material and the second cathode active material, an amount of the first cathode active material is 60 wt% to 80 wt%.

16. A cathode including the cathode material of any of claims 1 to 15.

17. A lithium secondary battery including the cathode of claim 16.

Citation Information

Patent Citations

  • Database tuning method using knob vector

    KR1020240057865A