molded article

By preparing molded products with appropriate load and thermal conductivity, the problem of uneven heat transfer of positive electrode active materials in the crucible was solved, realizing the production of positive electrode active materials with uniform physical properties, and improving battery performance and safety.

CN123165702APending Publication Date: 2026-11-24LG CHEM LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202680003582.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2025-01-03
Filing Date
2026-01-02
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

In the prior art, the heat transfer is uneven when the positive electrode active material is prepared in the crucible, resulting in uneven physical properties and making it difficult to prepare positive electrode active materials with uniform physical properties.

Method used

A molded article is provided, comprising a positive electrode active material precursor and a lithium-containing raw material, which is prepared by compression molding under free load conditions with a load of 4 N to 1050 N, a thermal conductivity of 0.25 W/(m·K) to 2.0 W/(m·K), and without binder, with an average porosity of 0.30 to 0.60, and in the form of a briquette, cylinder, granule, plate, truncated pyramid, elongated ellipse or truncated cone, by methods such as pressing, briquetting, and extrusion.

Benefits of technology

This technology enables the large-scale production of positive electrode active materials with uniform physical properties, improves the uniformity of the calcination reaction and gas exchange efficiency, reduces residual lithium content, improves the initial charge/discharge capacity and initial resistance of the battery, and ensures the safety and high quality of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123165702A_ABST
    Figure CN123165702A_ABST
Patent Text Reader

Abstract

The present invention relates to a molded article having suitable strength and comprising a positive electrode active material precursor having excellent thermal conductivity, and more specifically to a molded article comprising a positive electrode active material precursor and a lithium-containing raw material, wherein the failure load and thermal conductivity respectively meet specific ranges.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] Cross-references to related applications

[0002] This application claims priority to Korean Patent Application No. 10-2025-0001055, filed on January 3, 2025, the disclosure of which is incorporated herein by reference in its entirety. Technical Field

[0003] This invention relates to molded articles containing a positive electrode active material precursor, and more particularly to molded articles having suitable strength and excellent thermal conductivity. Background Technology

[0004] In recent years, with technological advancements and increasing demand for mobile devices and electric vehicles, the demand for secondary batteries as an energy source has also grown rapidly. Among these secondary batteries, lithium-ion batteries, characterized by high energy density and voltage, long cycle life, and low self-discharge rate, have been commercialized and are widely used.

[0005] Lithium transition metal oxides such as lithium cobalt oxides like LiCoO2, lithium nickel oxides like LiNiO2, lithium manganese oxides like LiMnO2 or LiMn2O4, and lithium iron phosphate oxides like LiFePO4 have been developed as positive electrode active materials for lithium secondary batteries. More recently, lithium composite transition metal oxides containing two or more transition metals, such as Li[Ni], have also been developed. a Co b Mn c O2, Li[Ni a Co b Al c O2, Li[Ni a Co b Mn c Al d O2 has been developed and is widely used.

[0006] On the other hand, positive electrode active materials are typically prepared as follows: A precursor powder for the positive electrode active material, such as a composite transition metal hydroxide, a composite transition metal oxide, the transition metal itself, a transition metal oxide, a transition metal hydrate, a transition metal hydroxide, a transition metal carbonate, or a transition metal chloride, is mixed with a lithium raw material. This mixture is then placed in a crucible and calcined. However, in this case, the degree of heat transfer between the mixture in the lower part and the mixture in the upper part of the crucible may differ, thus the physical properties of the positive electrode active material prepared in the same crucible may be non-uniform. Therefore, the problem is that calcination is not performed by filling the crucible with the mixture.

[0007] Therefore, it is necessary to develop a method for preparing positive electrode active materials with uniform physical properties, which allows for efficient heat transfer even when the crucible is completely filled with the mixture. Summary of the Invention

[0008] Technical issues

[0009] The present invention aims to solve the above-mentioned problems, and the object of the present invention is to provide a molded article comprising a positive electrode active material precursor having appropriate strength and excellent thermal conductivity.

[0010] Technical solution

[0011] To address the above problems, the present invention provides a molded article.

[0012] (1) The present invention provides a molded article comprising: a positive electrode active material precursor and a lithium-containing raw material, wherein when a sample of the molded article is compressed under free load conditions using a universal testing machine equipped with a 10 kN load cell, the load measured when the sample is destroyed by the compressive load is greater than 4 N and less than 1050 N, and the thermal conductivity is greater than 0.25 W / (m·K) and less than 2.0 W / (m·K).

[0013] (2) The present invention provides a molded article according to (1) above, wherein when a sample of the molded article is compressed under free load conditions using a universal testing machine equipped with a 10 kN force sensor, the load measured when the sample is destroyed by the compressive load is 5 N to 1050 N.

[0014] (3) The present invention provides a molded article according to any one of (1) or (2), wherein the thermal conductivity is 0.30 W / (m·K) or more and 2.0 W / (m·K) or less.

[0015] (4) The present invention provides a molded article according to any one of (1) to (3) above, wherein the positive electrode active material precursor comprises one or more selected from composite transition metal hydroxides, composite transition metal oxides, transition metals, transition metal oxides, transition metal hydrates, transition metal hydroxides, transition metal carbonates and transition metal chlorides.

[0016] (5) The present invention provides a molded article according to any one of (1) to (4) above, wherein the molar ratio (M:Li) of the total number of moles (M) of the transition metal contained in the positive electrode active material precursor to the number of moles (Li) of lithium contained in the lithium-containing raw material is 1:1 to 1.05.

[0017] (6) The present invention provides a molded article according to any one of (1) to (5) above, wherein the molded article does not include an adhesive.

[0018] (7) The present invention provides a molded article according to any one of (1) to (6), wherein the average porosity is 0.30 or more and 0.60 or less.

[0019] (8) The present invention provides a molded article according to any one of (1) to (7), wherein the average porosity is 0.45 or more and 0.60 or less.

[0020] (9) The present invention provides a molded article according to any one of (1) to (8) above, wherein the molded article is in the form of a block, cylinder, granule, plate, truncated pyramid, elongated ellipse, cuboid or truncated cone.

[0021] Beneficial effects

[0022] When positive electrode active materials are prepared using the molded articles according to the present invention, positive electrode active materials with uniform physical properties can be easily mass-produced.

[0023] That is, when using the molded article according to the present invention to prepare positive electrode active materials, positive electrode active materials with uniform physical properties can be easily mass-produced. Attached Figure Description

[0024] Figure 1 It is a graph showing the relationship between the mass of the briquette (m) and the failure load (F). Detailed Implementation

[0025] The present invention will be described in more detail below to facilitate understanding of the invention.

[0026] It should be understood that the terms or words used in this invention and the claims should not be construed as having the meanings defined in commonly used dictionaries, but should be interpreted as having meanings and concepts consistent with the technical ideas of this invention, based on the principle that the inventors can appropriately define the concepts of the terms to best interpret the invention.

[0027] It should also be understood that the terms “comprising,” “including,” or “having” in this invention specify the presence of the stated features, numbers, steps, elements, or combinations thereof, but do not exclude the presence or addition of one or more other features, numbers, steps, elements, or combinations thereof.

[0028] In this specification, the term "on" is intended to include not only cases where one element is directly formed on another element, but also cases where a third element is inserted between these components.

[0029] Molded products

[0030] This invention provides a molded article comprising: a positive electrode active material precursor; and a lithium-containing raw material. For the molded article according to the invention, when a sample of the molded article is compressed under free load conditions using a universal testing machine equipped with a 10 kN force sensor, the load measured when the sample fails under the compressive load (hereinafter referred to as the failure load) is greater than 4 N and less than 1050 N, and the thermal conductivity is greater than 0.25 W / (m·K) and less than 2.0 W / (m·K).

[0031] The inventors discovered that, regardless of the shape of the molded article, when the load at which the molded article breaks is greater than 4N and less than 1050N, the molded article is not damaged during the transfer process. Furthermore, when the thermal conductivity of the molded article is greater than 0.25W / (m·K) and less than 2.0W / (m·K), positive electrode active materials with uniform physical properties can be mass-produced, thus completing the present invention.

[0032] On the other hand, when the load at which the molded part breaks is below 4N, the molded part is prone to breakage. Furthermore, when the load exceeds 1050N, the molded part has high strength but may not calcine well, and may not be well pulverized during post-processing. Additionally, when the thermal conductivity of the molded part is less than 0.25 W / (m·K), it is difficult to prepare positive electrode active materials with uniform physical properties. When the thermal conductivity is greater than 2.0 W / (m·K), excessive heat transfer can lead to insufficient calcine formation and large particles, or insufficient porosity can impair gas exchange during the calcine reaction. In other words, as the strength of the molded part increases, there are benefits such as less breakage and higher thermal conductivity. However, when the strength is too high, the disadvantages during calcine and pulverization are that a large amount of raw material may be discarded, reducing production volume and degrading quality, making it difficult to produce high-quality positive electrode materials.

[0033] According to the present invention, when a sample of a molded article is compressed under free load conditions using a universal testing machine equipped with a 10 kN force sensor, the load measured when the sample fails under the compressive load is preferably between 5 N and 1050 N. Specifically, the load at which the molded article fails can be 5 N or more or 6 N or more, and can be less than 1047 N, less than 1048 N, less than 1049 N, or less than 1050 N.

[0034] According to the present invention, the thermal conductivity of the molded article is preferably 0.30 W / (m·K) or higher and 2.0 W / (m·K) or lower. Specifically, the thermal conductivity of the molded article may be 0.30 W / (m·K) or higher, 0.35 W / (m·K) or higher, 0.45 W / (m·K) or lower, 0.50 W / (m·K) or lower, 0.60 W / (m·K) or lower, 0.70 W / (m·K) or lower, 0.80 W / (m·K) or lower, 0.90 W / (m·K) or lower, 1.0 W / (m·K) or lower, 1.5 W / (m·K) or lower, or 2.0 W / (m·K) or lower.

[0035] For reference, the inventors conducted experiments to demonstrate that there is a linear relationship, as shown in Equation 1, between the load (F, unit: N) at failure and the mass (m, unit: g) of the molded article (pressed block). Figure 1 It is a graph showing the relationship between the mass of the briquette (m) and the failure load (F), and the following equation 1 is derived from actual measurement data.

[0036] [Equation 1]

[0037] F = 123.9 × m - 733.31

[0038] In Equation 1, F represents the failure load (N) of the molded product, and m represents the mass (g) of the briquette.

[0039] Equation 1 above was determined based on 21 experimental data points, and the coefficient of determination (R²) is... 2 The reliability of ) is 0.77.

[0040] Equation 1 above is an expression derived from the briquetting (roller pressing) method, and can be summarized as Equation 2 below.

[0041] [Equation 2]

[0042] F = 123.9 × C × (k 成形品 ) n’ -733.31

[0043] In equation 2, k 成形品 It is the thermal conductivity of the molded product, n'=1 / n, C is a constant, k 成形品 m n And n is a coefficient that varies depending on the molding equipment and conditions.

[0044] Furthermore, a relationship was established between the failure load (F) and thermal conductivity (k_molded_article) of the molded article as shown in Equation 3 below (the control equation for failure load and thermal conductivity).

[0045] [Equation 3]

[0046] F=C×k 成形品 n +b

[0047] In Equation 3, c and b are constants, and n is a coefficient that varies depending on the molding equipment and conditions.

[0048] k 成形品 It is the thermal conductivity of the molded article, and is the thermal conductivity (k) of the solid portion (positive electrode material) in the molded article (a composite structure consisting of a solid (e.g., positive electrode material) and pores). s ), thermal conductivity of air (pores) (k) 空气 ) and average porosity ( The following equation 4 is a limitation.

[0049] [Equation 4]

[0050] k 成形品 =k s ×(1- )+k 空气 ×

[0051] On the other hand, in the case of vertical compression (pressing method), as shown in Equation 5 below, the failure load of the molded article can be simplified.

[0052] [Equation 5]

[0053] F=C×k 成形品 n

[0054] According to the present invention, the failure load of the molded article must be below 1050 N, and for this purpose, the strength of the molded article is optimized by appropriately adjusting the pressure and porosity, which makes it possible to prepare positive electrode active materials with excellent quality.

[0055] According to the present invention, the positive electrode active material precursor may include one or more selected from complex transition metal hydroxides, complex transition metal oxides, transition metals, transition metal oxides, transition metal hydrates, transition metal hydroxides, transition metal carbonates, and transition metal chlorides.

[0056] Complex transition metal hydroxides may include nickel and one or more selected from cobalt, manganese and aluminum.

[0057] Complex transition metal hydroxides can be represented by the following formula 1: [Formula 1] Ni a1 Co b1 M 1 c1 M 2 d1 (OH)2+x1 In Equation 1, M 1 It is Mn, Al or a combination thereof, and M 2 It is a dopant element other than Ni, Co, Mn and Al. Among them 0 <a1<1.0,0≤b1<1.0,0≤c1<1.0,0≤d1≤0.1,0≤x1≤0.03。

[0058] Complex transition metal oxides may include nickel and one or more selected from cobalt, manganese and aluminum.

[0059] Complex transition metal hydroxides can be represented by the following formula 2: [Equation 2] Ni a2 Co b2 M 1 c M 2 d O 1+x2 In Equation 1, M 1 It is Mn, Al or a combination thereof, and M 2 It is a dopant element other than Ni, Co, Mn and Al. Among them 0 <a2<1.0,0≤b2<1.0,0≤c2<1.0,0≤d2≤0.1,0≤x2≤0.03。

[0060] The transition metal can be one or more selected from nickel, cobalt, manganese and aluminum.

[0061] The transition metal oxide can be one or more selected from nickel oxide, cobalt oxide, manganese oxide, and aluminum oxide.

[0062] Transition metal hydrates are compounds that include transition metals and water molecules, and can be one or more selected from nickel-containing hydrates, cobalt-containing hydrates, manganese-containing hydrates, and aluminum-containing hydrates.

[0063] A transition metal hydroxide is a structure in which a transition metal is coordinated via a hydroxyl group, and may be one or more selected from nickel hydroxide, cobalt hydroxide, manganese hydroxide, and aluminum hydroxide.

[0064] Transition metal carbonates are compounds composed of transition metals and carbonates, and can be one or more selected from nickel carbonate, cobalt carbonate, manganese carbonate, and aluminum carbonate.

[0065] Transition metal chlorides are compounds composed of transition metals and chlorine (Cl), and can be one or more selected from nickel chloride, cobalt chloride, manganese chloride, and aluminum chloride.

[0066] According to the present invention, lithium-containing sulfates, nitrates, acetates, carbonates, oxalates, citrates, halides, hydroxides, or hydroxyoxides can be used as lithium-containing raw materials, and there are no particular limitations, as long as they are soluble in water. Specifically, the lithium-containing raw materials can be Li₂CO₃, LiNO₃, LiNO₂, LiOH, LiOH·H₂O, LiH, LiF, LiCl, LiBr, LiI, CH₃COOLi, Li₂O, Li₂SO₄, or Li₃C₆H₅O₇, and any one of these or a mixture of two or more of them can be used. For example, the lithium-containing raw material can be Li₂CO₃.

[0067] According to the present invention, the molar ratio (M:Li) of the total number of moles of transition metals (M) in the cathode active material precursor to the molar ratio (Li) of lithium in the lithium-containing raw material is 1:1 to 1.05. That is, the cathode active material precursor and the lithium-containing raw material can be included in the molded article such that the molar ratio (M:Li) of the total number of moles of transition metals (M) in the cathode active material precursor to the molar ratio (Li) of lithium in the lithium-containing raw material is 1:1 to 1.05. In this case, since lithium is not excessive, the content of residual lithium as a byproduct after calcination may be low.

[0068] The molded articles according to the present invention may not include adhesives.

[0069] According to the present invention, the molded article preferably has an average porosity of 0.30 or more and 0.60 or less. Specifically, the average porosity of the molded article may be 0.30 or more, 0.35 or more, 0.40 or more, or 0.45 or more, and may be 0.60 or less. Average porosity is used to indicate the degree to which pores (voids) exist in the molded article, and is the ratio of the volume occupied by pores (the total volume of pores in the molded article) to the total volume of the molded article, and is a dimensionless number without units. Average porosity is used as an index to average the pore distribution within the molded article. When the average porosity of the molded article meets the above-mentioned range, there is an advantage that gas appropriately permeates into the molded article during the calcination reaction, allowing calcination to occur uniformly throughout the molded article. Furthermore, the average porosity range allows for uniform heat and gas transfer during calcination and allows for uniform growth of the positive electrode active material crystal particles.

[0070] According to the present invention, the molded articles can have shapes such as briquettes, cylinders, granules, plates, truncated pyramids, elongated ellipses, cuboids, or truncated cones (cylindrical shapes with different diameters at the top and bottom). In this case, efficient material and heat transfer allows for a well-conducted calcination reaction for preparing the positive electrode active material, and the crystals of the positive electrode active material can be formed into uniform sizes. The shapes of the molded articles according to the present invention can include various shapes (cylinders, truncated cones, elongated ellipses, cuboids, etc.) according to embodiments.

[0071] The molded articles according to the invention can be prepared by appropriately adjusting conditions (such as applied pressure and shear force) using various methods capable of granulating or molding powder: for example, press, briquette, extruder, spray dryer, disk pelletizer, roll compactor, low-shear wet pelletizer, fluidized bed pelletizer, twin-screw wet pelletizer, extrusion spheronisation, rotary tablet press, etc., but not limited thereto.

[0072] For example, the molded article according to the present invention can be prepared by the following method.

[0073] The molded article according to the present invention can be prepared by a method for preparing the molded article, the method comprising the steps of mixing a positive electrode active material precursor and a lithium-containing raw material to prepare a mixture; and the steps of taking out a predetermined amount of the mixture, placing the mixture into a molding apparatus and performing compression molding.

[0074] The molding apparatus can be any of a rotary tablet press, a conventional press, or a briquetting device, and the molding process can be single or continuous. The force or pressure applied during molding can be set within a range that ensures the shape stability of the molded article and the uniformity of reaction during the subsequent calcination process. For example, the force or pressure applied during molding in compression molding can be from about 0.1 tonf to 6 tonf, and the average linear pressure in briquetting molding can be from about 8.5 tons / cm to 9.5 tons / cm. The pressure range is to prevent over-densification of the mixture or conversely, to prevent insufficient mechanical strength of the molded article. The shape of the molded article is not particularly limited and can be, for example, a truncated cone, cylinder, elongated ellipse, or cuboid. Furthermore, the dimensions of the molded article can be adjusted according to the molding apparatus and purpose, but are preferably set within a range that allows for uniform heat transfer during calcination. The molded article thus prepared can then be fed into the calcination process and used to prepare positive electrode active materials.

[0075] Methods of implementing the present invention

[0076] Embodiments of the present invention will be described in detail below to enable those skilled in the art to readily implement the invention. However, the invention can be implemented in many different forms and is not limited to the embodiments described herein.

[0077] Examples and Comparative Examples

[0078] Example 1

[0079] The composite transition metal hydroxide (composition: Ni) is formed by the aggregation of tens to hundreds of primary particles into secondary particles. 0.62 Co 0.05 Mn 0.33 (OH)2, D 50 A mixture was prepared by mixing (Ni+Co+Mn) and Li2CO3 such that the ratio of the total moles of transition metals (Ni+Co+Mn) included in the composite transition metal hydroxide to the moles of lithium (Li) included in Li2CO3 ((Ni+Co+Mn):Li) was 1:1.05.

[0080] After placing 200 g of the mixture into a rotary tablet press, it is pressed with a force of 0.1 tonf to 1 tonf to obtain a truncated conical molded product (one bottom surface has a diameter of 5 mm to 10 mm, the other bottom surface has a diameter of 8 mm, and the height is 7 mm to 10 mm).

[0081] The molded product is placed in an alumina circular crucible (Φ75 mm) and then calcined in air at 850°C to 960°C for 16 hours to prepare the positive electrode active material.

[0082] Example 2

[0083] The composite transition metal hydroxide (composition: Ni) is formed by the aggregation of tens to hundreds of primary particles into secondary particles. 0.62 Co 0.05 Mn 0.33 (OH)2, D 50 A mixture was prepared by mixing (Ni+Co+Mn) and Li2CO3 such that the ratio of the total moles of transition metals (Ni+Co+Mn) included in the composite transition metal hydroxide to the moles of lithium (Li) included in Li2CO3 ((Ni+Co+Mn):Li) was 1:1.05.

[0084] Using a press, 180 g of the mixture is compressed with a force of 1 to 1.5 tonf to prepare cylindrical articles (diameter: 15 mm, height: 5 to 10 mm).

[0085] The molded product is placed in an alumina circular crucible (Φ75 mm) and then calcined in air at 850°C to 960°C for 16 hours to prepare the positive electrode active material.

[0086] Example 3

[0087] A mixture was prepared by mixing Ni(OH)2, Co(OH)2 and Mn3O4 such that the molar ratio of Ni:Co:Mn was 62:6:32, and Li2CO3 was added such that the ratio of the total molar number of transition metals (Ni+Co+Mn) to the molar number of lithium (Li) ((Ni+Co+Mn):Li) was 1:1.05.

[0088] A 100g mixture was shaped using a briquetting device under an average linear pressure of 8.92 tons / cm to produce a molded article with an elongated elliptical shape (width: 20 cm to 25 cm, vertical: 20 cm to 25 cm, height: 8 mm to 15 mm).

[0089] The molded product is placed in an alumina circular crucible (Φ75 mm) and then calcined in air at 850°C to 960°C for 16 hours to prepare the positive electrode active material.

[0090] Example 4

[0091] A mixture was prepared by mixing Ni(OH)2, Co(OH)2 and Mn3O4 such that the molar ratio of Ni:Co:Mn was 62:6:32, and Li2CO3 was added such that the ratio of the total molar number of transition metals (Ni+Co+Mn) to the molar number of lithium (Li) ((Ni+Co+Mn):Li) was 1:1.05.

[0092] A 100g mixture was shaped using a briquetting device under an average linear pressure of 8.72 t / cm to produce a molded article with an elongated elliptical shape (width: 20 cm to 25 cm, vertical: 20 cm to 25 cm, height: 8 mm to 15 mm).

[0093] The molded product is placed in an alumina circular crucible (Φ75 mm) and then calcined in air at 850°C to 960°C for 16 hours to prepare the positive electrode active material.

[0094] Example 5

[0095] A mixture was prepared by mixing Ni(OH)2, Co(OH)2 and Mn3O4 such that the molar ratio of Ni:Co:Mn was 62:6:32, and Li2CO3 was added such that the ratio of the total molar number of transition metals (Ni+Co+Mn) to the molar number of lithium (Li) ((Ni+Co+Mn):Li) was 1:1.05.

[0096] A 270g mixture was shaped using a briquetting device under an average linear pressure of 8.8 t / cm to produce a molded article with an elongated elliptical shape (width: 20 cm to 25 cm, vertical: 20 cm to 25 cm, height: 8 mm to 15 mm).

[0097] The molded product is placed in an alumina circular crucible (Φ75 mm) and then calcined in air at 850°C to 960°C for 16 hours to prepare the positive electrode active material.

[0098] Example 6

[0099] A mixture was prepared by mixing Ni(OH)2, Co(OH)2 and Mn3O4 such that the molar ratio of Ni:Co:Mn was 62:6:32, and Li2CO3 was added such that the ratio of the total molar number of transition metals (Ni+Co+Mn) to the molar number of lithium (Li) ((Ni+Co+Mn):Li) was 1:1.05.

[0100] Using a press, 160 g of the mixture is compressed with a force of 6 tonf to prepare a cuboid (diameter: 50 mm, vertical: 50 mm, height: 2 mm to 3 mm).

[0101] The molded product is placed in an alumina circular crucible (Φ75 mm) and then calcined in air at 850°C to 960°C for 16 hours to prepare the positive electrode active material.

[0102] Comparative Example 1

[0103] After placing 200g of the mixture prepared in Example 1 into a hopper, a press was operated with a force of 2.5 tonf to produce multiple molded articles. For reference, when molding using a hopper, a large number of small molded articles were randomly formed.

[0104] The molded product is placed in an alumina circular crucible (Φ75mm) and then baked in air at 850°C to 960°C for 16 hours to prepare the positive electrode active material.

[0105] Comparative Example 2

[0106] The mixture (powder state) prepared in Example 1 was placed in an alumina circular crucible (Φ75mm) and then calcined in air at 850°C to 960°C for 16 hours to prepare the positive electrode active material. That is, the mixture was directly calcined in powder state to prepare the positive electrode active material without a separate molding process.

[0107] Comparative Example 3

[0108] A mixture was prepared by mixing Ni(OH)2, Co(OH)2 and Mn3O4 such that the molar ratio of Ni:Co:Mn was 62:6:32, and Li2CO3 was added such that the ratio of the total molar number of transition metals (Ni+Co+Mn) to the molar number of lithium (Li) ((Ni+Co+Mn):Li) was 1:1.05.

[0109] A 100g mixture was shaped using a briquetting device under an average linear pressure of 10.2 t / cm to produce a molded article with an elongated elliptical shape (width: 40 cm, vertical: 25 cm, height: 10 mm to 16 mm).

[0110] The molded product is placed in an alumina circular crucible (Φ75mm) and then calcined in air at 850°C to 960°C for 16 hours to prepare the positive electrode active material.

[0111] Comparative Example 4

[0112] A mixture was prepared by mixing Ni(OH)2, Co(OH)2 and Mn3O4 such that the molar ratio of Ni:Co:Mn was 62:6:32, and Li2CO3 was added such that the ratio of the total molar number of transition metals (Ni+Co+Mn) to the molar number of lithium (Li) ((Ni+Co+Mn):Li) was 1:1.05.

[0113] Using a press, 150g of the mixture is compressed with a force of 2 tonf or more to prepare cylindrical molded articles (diameter: 15mm, height: 5mm to 10mm).

[0114] The molded product is placed in an alumina circular crucible (Φ75 mm) and then calcined in air at 850°C to 960°C for 16 hours to prepare the positive electrode active material.

[0115] Experimental Example

[0116] Experimental Example 1. Analysis of Failure Load of Molded Articles

[0117] Using a universal testing machine equipped with a 10kN force sensor, the molded articles prepared in the examples and comparative examples were compressed under free load conditions. The load measured when the sample failed due to the compressive load (at the point of fracture) was determined as the failure load. The results are shown in Table 1 below.

[0118] Experimental Example 2. Thermal Conductivity Analysis of Molded Products

[0119] The thermal conductivity of the molded articles prepared in the examples and comparative examples was analyzed using an LFA 467 apparatus manufactured by Netzsch, and the results are shown in Table 1 below. To measure the thermal conductivity, the molded articles were processed to conform to the measurement sample, then coated with a thin layer of toner and heated to a preset temperature in the LFA 467 apparatus to measure the thermal conductivity.

[0120] Experimental Example 3. Porosity Analysis of Molded Articles

[0121] Using micro-CT technology based on three-dimensional X-ray microscopy (hereinafter referred to as XRM), hundreds of images were obtained through two-dimensional scanning at intervals of 50 nm to 100 nm using a nanoscale three-dimensional X-ray microscope device. Then, through data analysis, the pore region and the solid (positron material) region in the molded article (positive electrode material and pores) were separated to measure the average porosity. Specifically, pore information measured at 100 nm intervals per unit height in the obtained images was accumulated to calculate the pore volume per unit cell (1 μm to 5 μm), and these were summed to obtain the total pore volume. The average porosity was then obtained as the ratio of the pore volume to the total volume of the molded article.

[0122] For reference, in Comparative Example 2, since no molded product was prepared, the mixture in powder form was evaluated.

[0123] [Table 1]

[0124] Referring to Table 1 above, in Comparative Example 2, the powder was in a powder state, therefore it was not necessary to evaluate the physical properties of the powder as a molded product and the battery performance. Therefore, the evaluation of residual lithium in Experimental Example 4 and the evaluation of battery performance in Experimental Example 5 were not performed.

[0125] Example 4. Evaluation of Residual Lithium

[0126] The positive electrode active materials prepared in the examples and comparative examples were pulverized using a roller mill or jet mill to prepare powder with a particle size of less than 1 mm. Then, 5 g of powder was taken and added to 100 ml of distilled water, followed by stirring for 5 minutes to obtain a filtrate.

[0127] The residual lithium content was measured by titrating lithium ions with a standard 0.1N hydrochloric acid solution using a lithium ion titration apparatus manufactured by Metrohm.

[0128] [Table 2]

[0129] It can be determined that when the residual lithium content in the powder physical properties is less than 0.70% by weight, specifically less than 0.65% by weight, less than 0.60% by weight, or less than 0.58% by weight, the positive electrode active material exhibits excellent performance, while when the residual lithium content is greater than 0.70% by weight, the positive electrode active material exhibits poor performance. Therefore, the battery performance evaluation of Experiment 5 below was not performed on Examples 3 to 6 and Comparative Examples 3 and 4.

[0130] On the other hand, in Comparative Examples 3 and 4, the residual lithium content was as high as 0.70% by weight or more, and there was a high possibility of gas generation caused by the reaction between the electrolyte solution and the residual lithium, which led to concerns about battery swelling.

[0131] In Tables 1 and 2 above, Comparative Example 4 has a failure load of 4533 N and an average porosity of 0.40, which is lower than that of Examples 4 and 5. However, the higher residual lithium content of Comparative Example 4 compared to Examples 4 and 5 is due to the difference in molding methods. In the case of the pressing (vertical compression) molding method, the porosity difference between the surface and interior of the molded article is relatively large, ranging from 0.05 to 0.15. On the other hand, since the compact is formed by the linear compression method, the porosity difference between the surface and interior is relatively small. Therefore, although its average porosity is high, Comparative Example 4, prepared by the pressing method, exhibits poor gas exchange due to the inhomogeneity of the internal pores (relatively low porosity on the surface). This hinders the calcination reaction from proceeding well, resulting in a relatively high measured residual lithium.

[0132] Experimental Example 5. Battery Performance Evaluation

[0133] A positive electrode slurry was prepared by mixing the positive electrode active material, FX35 conductive material, and polyvinylidene fluoride (PVDF) binder prepared in the examples and comparative examples in an N-methylpyrrolidone (NMP) solvent at a ratio of 95:3:2. The prepared positive electrode slurry was then widely coated onto aluminum foil, dried at 130°C for 10 minutes, and then rolled to prepare the positive electrode.

[0134] After forming the electrode assembly and housing it in a battery case, a half-cell is prepared by injecting an electrolyte solution into the battery case. In the electrode assembly, a lithium metal electrode serves as the negative electrode, and a porous polyethylene separator is inserted between the positive and negative electrodes. Here, the electrolyte solution is obtained by dissolving 1M LiPF6 in an organic solvent, wherein ethylene carbonate (EC): ethyl methyl carbonate (EMC): diethyl carbonate (DEC) are mixed in a volume ratio of 3:4:3.

[0135] Each of the half-cells prepared as described above was charged to 4.4V at a rate of 0.1C in CC-CV mode at 25°C and discharged to 2.5V at a rate of 0.1C in CC mode. The initial charge capacity and initial discharge capacity were measured to calculate the initial efficiency. The results are listed in Table 3 below. For reference, the initial efficiency value is a percentage of the initial discharge capacity relative to the initial charge capacity.

[0136] Additionally, the initial resistance is R = (V 60 -V0) / I 60 The subscript 0 represents the value at 0 seconds and 60 represents the value at 60 seconds. V represents voltage and I represents current.

[0137] [Table 3]

[0138] Referring to Table 3, it can be confirmed that, compared with the battery containing the positive electrode active material prepared from the molded article of Comparative Example 1, the battery containing the positive electrode active material prepared from the molded article of Example 1 according to the present invention exhibits superior initial charge / discharge capacity and significantly lower initial resistance. Furthermore, it can be confirmed that, compared with the battery containing the positive electrode active material prepared from the molded article of Comparative Example 1, the battery containing the positive electrode active material prepared from the molded article of Example 2 according to the present invention exhibits superior initial efficiency and significantly lower initial resistance.

[0139] In other words, it can be confirmed that in the molded articles of Embodiments 1 and 2 according to the present invention, the reactive gas can relatively easily penetrate into the interior of the molded article, thereby enabling easy mass production of positive electrode active materials with uniform physical properties and improved performance.

[0140] According to the present invention, the positive electrode active material prepared by the molded article of the embodiment uniformly maintains the powder physical properties, such as failure load, thermal conductivity and porosity, so that when the battery is assembled, the contact resistance between the active materials is low and the electrolyte solution permeates uniformly, thereby improving the initial charge / discharge capacity, initial efficiency and initial resistance of the battery.

[0141] Furthermore, by keeping the residual lithium content in the powder less than 0.70% by weight, the possibility of gas generation due to reaction with the electrolyte is low, thereby minimizing battery swelling and safety issues.

[0142] Furthermore, by optimizing the pressing and calcination conditions to prepare molded products, powder handling becomes easier during the preparation of pulverized slurry and electrode coating, thereby ensuring the efficiency of the preparation process suitable for large-scale production.

[0143] Therefore, the molded articles according to the present invention provide positive electrode active materials with uniform structure and stable physical properties, which leads to the production of high-quality batteries with excellent initial performance and guaranteed safety.

Claims

1. A molded article comprising a positive electrode active material precursor and a lithium-containing raw material, wherein When a universal testing machine equipped with a 10 kN force sensor compresses a molded sample under free load conditions, the load measured when the sample fails under compressive load is greater than 4 N and less than 1050 N. Thermal conductivity is above 0.25 W / (m·K) and below 2.0 W / (m·K).

2. The molded article as described in claim 1, wherein, When a universal testing machine equipped with a 10 kN force sensor is used to compress a sample of a molded product under free load conditions, the load measured when the sample is destroyed by the compressive load ranges from 5 N to 1050 N.

3. The molded article as described in claim 1, wherein, The thermal conductivity is above 0.30 W / (m·K) and below 2.0 W / (m·K).

4. The molded article as described in claim 1, wherein, The positive electrode active material precursor comprises one or more selected from complex transition metal hydroxides, complex transition metal oxides, transition metals, transition metal oxides, transition metal hydrates, transition metal hydroxides, transition metal carbonates, and transition metal chlorides.

5. The molded article as described in claim 1, wherein, The molar ratio (M:Li) of the total number of moles of transition metals (M) contained in the positive electrode active material precursor to the number of moles of lithium (Li) contained in the lithium-containing raw material is from 1:1 to 1.

05.

6. The molded article as claimed in claim 1, wherein, The molded article does not include adhesives.

7. The molded article as claimed in claim 1, wherein, The average porosity of the molded article is above 0.30 and below 0.

60.

8. The molded article as claimed in claim 1, wherein, The average porosity of the molded article is above 0.45 and below 0.

60.

9. The molded article as claimed in claim 1, wherein, The molded product is in the form of a block, cylinder, granule, plate, truncated pyramid, elongated ellipse, cuboid, or truncated cone.

Citation Information

Patent Citations

  • Laser heat treatment method for wafer structure and manufacturing method of semiconductor device using the same

    KR1020250001055A