Anion exchange polymer membranes and methods of synthesizing the same by electron beam irradiation
An anion exchange membrane resistant to alkaline media was prepared by crosslinking block polymers with electron beam irradiation. This solved the problem of shortened lifespan of existing membranes in alkaline environments, improved the water absorption performance and service life of the membrane, and maintained the ionic conductivity.
Patent Information
- Application Number
- CN202580030667.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-05-02
- Filing Date
- 2025-04-17
- Publication Date
- 2026-11-24
AI Technical Summary
Existing anion exchange membranes suffer from shortened lifespans in fuel cells and electrolyzers due to exposure to highly alkaline environments, necessitating the development of newer anion exchange membranes that are more resistant to alkaline media.
A block polymer in thin film form was crosslinked by electron beam irradiation to prepare a crosslinked ion exchange polymer membrane. The block polymer was block polymer (AB)nA of formula (I), where A represents a polyvinyl aromatic block with a quaternary ammonium group and B represents a hydrogenated block of poly(1,3-diene) or a hydrogenated block of a copolymer containing monomer units of 1,3-diene and vinyl aromatic monomers.
It improves the membrane's performance in terms of water absorption and service life, while maintaining ionic conductivity and enhancing its resistance to alkaline media.
Smart Images

Figure SMS_1 
Figure SMS_3 
Figure SMS_4
Abstract
Description
Technical Field
[0001] The field of the present invention is a method for synthesizing anion exchange polymer membranes, the anion exchange polymer membranes comprising ionomers and intended for use in electrolyzers or fuel cells. Background Technology
[0002] The core of a fuel cell and electrolyzer consists of two electrodes (anode and cathode), an electrolyte layer separating the two electrodes, and a catalyst located at the interface between the electrolyte layer and each electrode. The fuel cell and electrolyzer include a membrane constituting the electrolyte layer. One of the components of this membrane is an ionomer, i.e., a polymer with ionic or ionizable groups. The presence of ionic or ionizable groups in the polymer is crucial for imparting ionic conductivity to the polymer, allowing anions to transfer from the cathode to the anode. The most well-known ionic or ionizable groups in polymers that can be used in anion exchange membrane fuel cells are quaternary ammonium groups, imidazolium groups, phosphonium groups, and sulfonium groups. Ionomers with quaternary ammonium or imidazolium ionic groups are typically derived from halogenated polymers modified by reaction with tertiary amines or imidazolium. For example, see reference WO2019010290, which describes the reaction between a tertiary amine and pre-brominated alkylated aromatic units constituting rigid blocks (wherein the rigid blocks are linked together by soft blocks) of a block polymer. It is also known from the literature “Energy Technol. 2017, 5, 929-936” that ionomers with imidazolium groups are synthesized by reacting 1-methylimidazolium with copolymers of styrene and chloromethylstyrene.
[0003] When used in fuel cells or electrolyzers, anion exchange membranes are typically exposed to highly alkaline environments, which have proven to be highly corrosive to ionomers, leading to a shortened membrane lifespan. Therefore, there is a need to find novel anion exchange membranes that can better withstand these alkaline media in order to extend their service life. Summary of the Invention
[0004] The applicant discovered a solution to the above problem.
[0005] Therefore, a first object of the present invention is a method for preparing anion exchange polymer membranes comprising cross-linked ionomers, the method comprising electron beam irradiation of the ionomers in the form of a thin film, the ionomers being block polymers of formula (I). (AB) n -A (I), Symbol A represents a polyvinyl aromatic block containing a quaternary ammonium group. The symbol B represents a hydrogenated block of poly(1,3-diene) or a hydrogenated block of a copolymer containing monomer units of 1,3-diene and vinyl aromatic monomers. n is an integer equal to or greater than 1.
[0006] Another subject of the present invention is an anion exchange polymer membrane comprising a crosslinked ionomer, said crosslinked ionomer being a block polymer of formula (I) crosslinked by electron beam irradiation. (AB) n -A (I), Symbol A represents a polyvinyl aromatic block containing a quaternary ammonium group. The symbol B represents a hydrogenated block of poly(1,3-diene) or a hydrogenated block of a copolymer containing monomer units of 1,3-diene and vinyl aromatic monomers. n is an integer equal to or greater than 1. The membrane can be obtained by the method according to the invention.
[0007] The present invention also relates to crosslinked ionomers, which are block polymers of formula (I) crosslinked by electron beam irradiation.
[0008] The present invention also relates to fuel cells or electrolyzers comprising the membrane according to the present invention.
[0009] Detailed Description of the Invention The polymers mentioned in the specification may be fossil-derived or bio-based. In the case of bio-based polymers, they may be partially or wholly derived from biomass or obtained from renewable raw materials derived from biomass. Similarly, they may originate from the recycling of used materials, meaning they may be partially or wholly derived from recycling processes or obtained from raw materials that themselves originated from recycling processes.
[0010] The terms "membrane" and "thin film" are well known to those skilled in the art. To recap, in a well-known manner, a membrane is a structure defined by IUPAC in "IUPAC recommendations 1996". Similarly, in the same known manner and according to the definition given by IUPAC, the term "thin film" is understood according to the definition given by IUPAC in "IUPAC recommendations 1996".
[0011] The ionomer used in the method according to the invention is a block polymer of formula (I) with quaternary ammonium groups. (AB) n -A (I), Symbol A represents a polyvinyl aromatic block containing a quaternary ammonium ion group. The symbol B represents a hydrogenated block of poly(1,3-diene) or a hydrogenated block of a copolymer containing monomer units of 1,3-diene and vinyl aromatic monomers. n is an integer equal to or greater than 1.
[0012] According to any embodiment of the present invention, the block polymer of formula (I) is preferably a linear polymer.
[0013] Preferably, n equals 1, in which case the block polymer of formula (I) is a triblock. The triblock has the formula ABA, wherein symbol A represents a polyvinyl aromatic block with a quaternary ammonium group, and symbol B represents a hydrogenated block of a homopolymer of 1,3-diene or a hydrogenated block of a copolymer containing monomer units of 1,3-diene and vinyl aromatic monomers.
[0014] The polyvinyl aromatic blocks of the ionomer can be blocks of homopolymers of vinyl aromatic monomers or blocks of copolymers of two or more vinyl aromatic monomers. The vinyl aromatic monomers of the polyvinyl aromatic blocks of the ionomer are also referred to as "first vinyl aromatics". In this invention, "vinyl aromatic monomer" should be understood to refer to monomers of the formula Ar-CH=CH2 or Ar-CR=CH2, where the symbol Ar represents a substituted or unsubstituted aryl group, and the symbol R represents an alkyl group, such as methyl. The aryl group represented by the symbol Ar is preferably a phenyl group or a phenyl group substituted with an alkyl group having 1 to 4 carbon atoms. As vinyl aromatic monomers suitable for use in this invention, styrene and styrene substituted with alkyl groups at the para, meta, or ortho, or α-positions may be mentioned, for example. The alkyl group is preferably an alkyl group having 1 to 4 carbon atoms. The polyvinyl aromatic blocks are preferably polystyrene blocks, poly(α-methylstyrene) blocks, or styrene / α-methylstyrene copolymer blocks. The styrene / α-methylstyrene copolymer blocks can be random, gradient, or block copolymers.
[0015] The polyvinyl aromatic block of the ionomer also possesses the essential characteristic of having a quaternary ammonium group. The polyvinyl aromatic block of the ionomer is a polyvinyl aromatic block that typically comprises a vinyl aromatic monomer unit with a quaternary ammonium group. The vinyl aromatic monomer unit with a quaternary ammonium group is typically a monomer unit in which the aryl group is linked to the quaternary ammonium group via a saturated hydrocarbon chain. In other words, the aromatic ring of the vinyl aromatic monomer unit with a quaternary ammonium group is replaced by a saturated hydrocarbon chain (particularly an alkyl chain substituted with a quaternary ammonium group) substituted with a quaternary ammonium group. The saturated hydrocarbon chain substituted with a quaternary ammonium group present in the block represented by the symbol A is preferably a linear chain containing 1 to 10 carbon atoms, more preferably a linear chain containing 2 to 8 carbon atoms. In this application, "linear chain" should be understood to mean an acyclic and unbranched chain. Preferably, the quaternary ammonium group is N-alkylpiperidinium. More preferably, the quaternary ammonium group is N-methylpiperidinium. The quaternary ammonium group is preferably N-alkylpiperidinium, more preferably N-methylpiperidinium.
[0016] In a known manner, polyvinyl aromatic blocks with quaternary ammonium groups are obtained by aryl modification in two steps: haloalkylation of the aromatic ring to form a halopolymer, followed by reaction with a tertiary amine to form an ionomer. See, for example, patent application WO 2010010290.
[0017] According to the present invention, the block represented by the symbol B is a hydrogenated block of poly(1,3-diene) or a hydrogenated block of a copolymer containing monomer units of 1,3-diene and vinyl aromatic monomers. The vinyl aromatic monomer of the copolymer containing monomer units of 1,3-diene and vinyl aromatic monomers is also referred to as "second vinyl aromatic".
[0018] "Hydrogenated blocks of poly(1,3-diene) or hydrogenated blocks of copolymers comprising monomer units of 1,3-diene and vinyl aromatic monomers" should be understood as referring to blocks in which the monomer units of 1,3-diene are reduced to a degree greater than 95 mol%, preferably greater than 98 mol%; more preferably, greater than 99 mol% of the monomer units of 1,3-diene are reduced. Hydrogenation of poly(1,3-diene) or hydrogenation of copolymers comprising monomer units of 1,3-diene and vinyl aromatic monomers are well-known reactions. References, for example, can be made to EP 1840993 B1, US 5239010, US 5468574, and US20070021569, which describe the selective hydrogenation of poly(1,3-diene) or selective hydrogenation of copolymers comprising monomer units of 1,3-diene and vinyl aromatic monomers of block polymers of formula (I).
[0019] "1,3-diene" should be understood as referring to one or more 1,3-dienes. "Multiple" should be understood as referring to at least two. 1,3-diene preferably contains 4 to 8 carbon atoms. 1,3-diene is preferably 1,3-butadiene, isoprene, or a mixture of 1,3-butadiene and isoprene, more preferably 1,3-butadiene.
[0020] According to the first variant, the block represented by the symbol B is a hydrogenated block of poly(1,3-diene). In this invention, "poly(1,3-diene)" should be understood to refer to a polymer whose constituent units are 1,3-diene monomer units. Poly(1,3-diene) is preferably a homopolymer of 1,3-diene, in which case the constituent unit of poly(1,3-diene) is a single 1,3-diene monomer unit. Poly(1,3-diene) is more preferably a homopolymer of 1,3-butadiene.
[0021] According to the second variant, the block represented by the symbol B is a hydrogenated block of a copolymer containing monomer units of 1,3-diene and vinyl aromatic monomers. The copolymer containing monomer units of 1,3-diene and vinyl aromatic monomers can be random or gradient.
[0022] The vinyl aromatic monomers constituting the copolymers comprising monomer units of 1,3-diene and vinyl aromatic monomers may be the same as or different from the vinyl aromatic monomers of polyvinyl aromatic blocks. The vinyl aromatic monomers constituting the copolymers comprising monomer units of 1,3-diene and vinyl aromatic monomers are preferably styrene. The 1,3-diene constituting the copolymers comprising monomer units of 1,3-diene and vinyl aromatic monomers is preferably 1,3-butadiene.
[0023] Copolymers comprising monomer units of 1,3-diene and vinyl aromatic monomers preferably comprise monomer units of vinyl aromatic monomers in which the aryl (preferably phenyl) group is substituted by an alkyl chain substituted with a quaternary ammonium group. Preferably, the 1,3-diene and vinyl aromatic monomers of the copolymer comprising monomer units of 1,3-diene and vinyl aromatic monomers are 1,3-butadiene and styrene, respectively. Copolymers comprising monomer units of 1,3-diene and vinyl aromatic monomers are advantageously copolymers of 1,3-diene and vinyl aromatic monomers in which some or all of the vinyl aromatic monomer units have aryl groups substituted by alkyl chains substituted with quaternary ammonium groups, preferably phenyl. The quaternary ammonium-substituted alkyl chains present in the blocks represented by the symbol B are preferably linear chains comprising 1 to 10 carbon atoms, more preferably linear chains comprising 2 to 8 carbon atoms. Advantageously, they are the same as the quaternary ammonium-substituted saturated hydrocarbon chains present in the blocks represented by the symbol A.
[0024] The molar content of vinyl aromatic monomer units and vinyl aromatic monomer units with quaternary ammonium groups in the hydrogenated block of the copolymer containing monomer units of 1,3-diene and vinyl aromatic monomers is preferably in the range of 1% to 25%, more preferably 5% to 20%, of the repeating units constituting the hydrogenated block.
[0025] According to any embodiment of the invention, the block represented by the symbol B is preferably a hydrogenated block of a homopolymer of 1,3-butadiene or a hydrogenated block of a copolymer of 1,3-butadiene and styrene, wherein all or part of the styrene monomer units have phenyl groups substituted with alkyl chains replaced by quaternary ammonium groups, and the quaternary ammonium-substituted alkyl chains present in the block represented by the symbol B are preferably linear chains containing 1 to 10 carbon atoms, more preferably linear chains containing 2 to 8 carbon atoms.
[0026] In the ionomer, i.e. the block polymer of formula (I), the block represented by the symbol B preferably accounts for 50% to 90% by mass of the total mass of the ionomer (i.e. the block polymer of formula (I), more preferably 60% to 80% by mass of the total mass of the ionomer (i.e. the block polymer of formula (I)).
[0027] According to any embodiment of the invention, the quaternary ammonium group preferably has formula (II) or formula (III). N + (R1)3 (II) R1 can be the same or different and is an alkyl group, while R2 represents an unbranched, saturated or unsaturated divalent hydrocarbon chain containing 3 to 5 carbon atoms and may be interrupted by one or more heteroatoms selected from oxygen, nitrogen, and sulfur. In formulas (II) and (III), bonds that connect the nitrogen atom to the monomer unit of the ionomer, particularly via the alkyl chain substituted with a quaternary ammonium group, are not shown. More preferably, the quaternary ammonium group has the formula (III), preferably N-alkylpiperidinium, more preferably N-methylpiperidinium.
[0028] The content of quaternary ammonium groups in the block polymer of formula (I) can vary considerably and can be adjusted by those skilled in the art according to the desired performance qualities of the anion exchange membrane, particularly according to the desired trade-off between water absorption and ionic conductivity. It is known that increasing the content of groups in the ionomer is beneficial to the ionic conductivity of the membrane containing the ionomer, but often reduces the stability of the membrane in highly alkaline media. Preferably, the content of quaternary ammonium groups in the ionomer is greater than or equal to 0.1 meq / g ionomer (meq / g, milliequivalents per gram) and less than or equal to 1 meq / g ionomer, said ionomer being a block polymer of formula (I).
[0029] The quaternary ammonium group's counterion is preferably a halide anion, and more preferably a bromide anion.
[0030] The average molar mass of the ionomer (i.e., the block polymer of formula (I)) can vary considerably and is selected by those skilled in the art based on the desired performance qualities of the anion exchange membrane, particularly based on the required trade-off between its mechanical properties and its ability to form a thin film. Preferably, the number-average molar mass of the ionomer (i.e., the block polymer of formula (I)) is greater than 20,000 g / mol and less than 500,000 g / mol based on polystyrene standards (a value determined by size exclusion chromatography (SEC) coupled with a refractometer).
[0031] The average molar mass of the block represented by the symbol A can vary considerably and is selected by those skilled in the art based on the desired performance qualities of the proton exchange membrane, particularly the desired trade-off between the membrane's mechanical and electrical properties. It is well known that an increase in average molecular mass is beneficial to the membrane's mechanical properties, while a decrease in average molecular mass tends to reduce the membrane's electrical resistance. Preferably, the number-average molar mass of the block represented by the symbol A, based on polystyrene standards, is greater than 1000 g / mol and less than 100000 g / mol (a value determined by size exclusion chromatography (SEC) coupled with a refractometer).
[0032] The number-average molar mass of the ionomer (i.e., the block polymer of formula (I)) is the number-average molar mass of the block polymer before the quaternary ammonium group is introduced into the block polymer. Similarly, the number-average molar mass of the block represented by the symbol A is the number-average molar mass of the block represented by the symbol A before the quaternary ammonium group is introduced into the block polymer.
[0033] The ionomer, i.e., the block polymer of formula (I), can be prepared from a starting block polymer. The number-average molar mass of the ionomer can be determined as described above from the number-average molar mass of the starting block polymer. The starting block polymer differs from the block polymer of formula (I) in that the aromatic ring is not substituted with a group containing a quaternary ammonium group and the 1,3-diene monomer unit is not reduced. To prepare the ionomer, the 1,3-diene monomer unit of the starting block polymer is selectively hydrogenated, and then the vinyl aromatic monomer unit of the starting block polymer is modified first by a halogenation reaction of the aromatic ring, followed by a reaction with a tertiary amine, referred to below as a quaternization reaction. The reactants used in the halogenation reaction are typically haloalkenes. In the haloalkene, the halogen atom and the double bond are preferably located at different ends of the carbon chain of the haloalkene. The haloalkene preferably contains 2 to 10 carbon atoms, more preferably 4 to 8 carbon atoms. The carbon chain constituting the haloalkene is preferably linear.
[0034] Tertiary amines used in quaternization reactions preferably have formula (IV) or formula (V). N(R1)3 (IV) (V) R1 can be the same or different and is an alkyl group, while R2 represents an unbranched, saturated or unsaturated divalent hydrocarbon chain containing 3 to 5 carbon atoms and may be interrupted by one or more heteroatoms selected from oxygen, nitrogen and sulfur. The tertiary amine preferably has the formula (V), more preferably N-alkylpiperidine, and even more preferably N-methylpiperidine.
[0035] Typically, the block polymer is a thermoplastic elastomer, preferably triblock. According to any embodiment of the invention, the starting block polymer is preferably a linear polymer.
[0036] The starting block polymer can be a commercial product, for example, obtained from Kraton or Kuraray, or can be prepared according to any of the known synthetic methods described below: -a) Anionic polymerization of 1,3-diene or copolymerization of 1,3-diene with a second vinyl aromatic compound initiated by a dilithium compound (e.g., the adduct of diisopropenylbenzene and sec-butyllithium described in document EP1237941, or 1,1,4,4-tetraphenyl-1,4-dilithiumbutane), followed by polymerization of the first vinyl aromatic compound to form a triblock polymer, can be synthesized by sequentially continuing the polymerization of 1,3-diene and, where appropriate, continuing the polymerization of the second vinyl aromatic compound and the first vinyl aromatic compound; -b) Anionic polymerization of a first vinyl aromatic compound initiated by a monolithiated compound (e.g., butyllithium), followed by polymerization of 1,3-diene or copolymerization of 1,3-diene with a second vinyl aromatic compound, and then reaction with a coupling agent (e.g., dichlorosilane) to form a triblock, can be synthesized by sequentially continuing the polymerization of the first vinyl aromatic compound and the polymerization of 1,3-diene, and, where appropriate, continuing the polymerization of the second vinyl aromatic compound before the coupling reaction; Those skilled in the art will understand that the methods for preparing the starting block polymer can produce mixtures comprising the starting block polymer. Those skilled in the art will understand that the method for preparing the starting block polymer according to method b) can result in the formation of a mixture comprising the starting block polymer, polyvinyl aromatics, and diblocks (formed during the third and first steps of the method, respectively). Similarly, those skilled in the art will understand that method a) can produce a mixture comprising the starting block polymer and a homopolymer or copolymer of 1,3-diene formed during the first step.
[0037] For the modification of vinyl aromatic monomer units, please refer to, for example, literature WO 2010010290; for hydrogenation reactions, please refer to, for example, literature WO 03008467.
[0038] Alternatively, the ionomer, i.e. the block polymer of formula (I), can be prepared from a commercial product, such as the one obtained by Kraton Corporation under the name "Kraton G" or the one obtained by Kuraray Corporation under the trade name "SEPTON". This commercial product is a hydrogenated block polymer, which differs from the ionomer in that it does not contain quaternary ammonium groups.
[0039] When one of these methods for preparing the starting block polymer results in a mixture containing the starting block polymer, the mixture containing the starting block polymer is typically subjected to hydrogenation and modification of the vinyl aromatic monomer units. In the case of hydrogenation and modification of the mixture containing the starting block polymer of vinyl aromatic monomer units, the ionomer is obtained as a mixture and is generally usable without separation from the mixture.
[0040] Ionomers are in the form of thin films before crosslinking by electron beam irradiation. The ionomers are formed into thin films prior to electron beam irradiation. It is known that polymers can be coated to form thin films. It is also known, for example, from patent application WO2019010290, that ionomers having quaternary amines as ionic groups are very poorly soluble, or even insoluble, in many solvents. Due to this low solubility or insolubility, forming thin films from ionomers by coating solutions of ionomers can be problematic. To overcome this problem, films are typically prepared by coating their precursors (i.e., halogenated polymers) rather than by coating the ionomers themselves.
[0041] Halogenated polymers can be used to form films by depositing a solution of the halogenated polymer onto a carrier surface to cover it, followed by drying and evaporation of the solvent constituting the solution or dispersion. Typically, a solution of the halogenated polymer is prepared, which can be spread on a flat surface of the carrier to form a polymer layer by coating the carrier. The coating temperature is selected by those skilled in the art, specifically based on the viscosity of the halogenated polymer solution and the boiling point of the solvent of the halogenated polymer solution. Coating is preferably carried out at a temperature close to ambient temperature, typically 20°C to 25°C, or at a temperature above ambient temperature but below the boiling point of the solvent of the halogenated polymer solution. The concentration of the polymer solution is adjusted by those skilled in the art, specifically based on the solubility of the halogenated polymer in the solvent of the solution and according to the viscosity of the solution. The solvent of the halogenated polymer solution is selected by those skilled in the art, specifically based on the solubility of the halogenated polymer in the solvent and according to its boiling point temperature. The concentration range of the halogenated polymer solution is typically 1% to 15% by mass of solids. The solvent for the halogenated polymer solution preferably has a relatively low boiling point temperature, typically less than or equal to 100°C, so that it can be easily removed from the polymer layer, particularly by evaporation under vacuum, in an air stream, or inert gas stream such as nitrogen or argon. Suitable solvents include, for example, ethers, mixtures of ethers and alcohols, and halogenated solvents. The solvent is preferably selected from tetrahydrofuran, mixtures of tetrahydrofuran and alcohols, and chloroform, wherein the alcohol is preferably ethanol. Drying to remove the solvent from the halogenated polymer solution is typically carried out under vacuum, in an air stream, or inert gas stream such as nitrogen or argon, preferably at a temperature in the range of ambient temperature (23°C) to the boiling point temperature of the solvent, and preferably at a temperature 15°C lower than the boiling point temperature under an air stream or inert gas stream. The thickness of the spread layer after drying is preferably less than or equal to 110 micrometers, more preferably less than or equal to 90 micrometers. The thickness is preferably greater than or equal to 50 micrometers.
[0042] Once the halogenated polymer is in film form, it is immersed in a bath of tertiary amine solution to modify the vinyl aromatic monomer units, thereby forming an ionomer in film form. Preferably, the ionomer is then rinsed and dried. After recovery, it is subjected to electron beam irradiation, thereby crosslinking the ionomer.
[0043] During electron beam irradiation, the crosslinking of the ionomer is caused by the radiochemical effects of the irradiation. Electron beam irradiation is preferably performed in the absence of a chemical curing agent. The electron beam irradiation dose can vary over a wide range and can be adjusted by those skilled in the art based on the thickness of the film and the required trade-offs according to the film's properties (i.e., lifetime, water absorption, and ionic conductivity). Preferably, the electron beam irradiation dose is greater than 50 kGy and less than 5000 kGy. More preferably, the electron beam irradiation dose is greater than 100 kGy and less than 3000 kGy, and more preferably less than 2000 kGy. Electron beam irradiation can be performed in air or in an inert atmosphere (typically nitrogen), preferably in an inert atmosphere, and more preferably in nitrogen. Depending on the power of the electron beam irradiation equipment used, the dose can be delivered in a single irradiation sequence or in several consecutive irradiation sequences. Electron beam irradiation produces crosslinked ionomers in the form of a thin film.
[0044] Another subject of this invention is a crosslinked ionomer, which is a block polymer crosslinked by electron beam irradiation, said block polymer being any of the block polymers of formula (I) defined in the method for preparing anion exchange polymer membranes according to the invention. The crosslinked ionomer constitutes all or part, preferably all, of a membrane intended for use in a fuel cell or electrolyzer. The electron beam irradiation-crosslinked ionomer results in membranes containing it exhibiting improved performance in terms of water absorption and lifespan, while maintaining ionic conductivity.
[0045] As another subject of the present invention, and the membrane that can be obtained by the method according to the present invention, is an anion exchange polymer membrane comprising cross-linked ionomers.
[0046] In summary, the present invention is advantageously implemented according to any one of the following embodiments 1 to 36: Implementation Scheme 1: A method for preparing anion exchange polymer membrane comprising a crosslinked ionomer, the method comprising electron beam irradiation of the ionomer in thin film form, the ionomer being a block polymer of formula (I), (AB) n -A (I), Symbol A represents a polyvinyl aromatic block containing a quaternary ammonium group. The symbol B represents a hydrogenated block of poly(1,3-diene) or a hydrogenated block of a copolymer containing monomer units of 1,3-diene and vinyl aromatic monomers. n is an integer equal to or greater than 1.
[0047] Implementation Scheme 2: The method according to Implementation Scheme 1, wherein the block polymer of formula (I) is linear.
[0048] Implementation Scheme 3: The method according to Implementation Scheme 1 or 2, wherein the block polymer of Formula (I) is a triblock.
[0049] Implementation Scheme 4: The method according to any one of Implementation Schemes 1 to 3, wherein the 1,3-diene is 1,3-butadiene, isoprene, or a mixture thereof.
[0050] Implementation Scheme 5: The method according to any one of Implementation Schemes 1 to 4, wherein the polyvinyl aromatic block is a polystyrene block, a poly(α-methylstyrene) block, or a styrene / α-methylstyrene copolymer block.
[0051] Implementation Scheme 6: The method according to any one of Implementation Schemes 1 to 5, wherein the poly(1,3-diene) is a homopolymer of 1,3-butadiene.
[0052] Implementation Scheme 7: The method according to any one of Implementation Schemes 1 to 6, wherein the copolymer comprising monomer units of 1,3-diene and vinyl aromatic monomers is a copolymer of 1,3-diene and vinyl aromatic monomers, wherein some or all of the vinyl aromatic monomer units have aryl groups substituted by alkyl chains replaced by quaternary ammonium groups.
[0053] Implementation Scheme 8: The method according to Implementation Scheme 7, wherein the aryl group is phenyl.
[0054] Implementation Scheme 9: The method according to any one of Implementation Schemes 1 to 8, wherein the molar content of the vinyl aromatic monomer unit and the quaternary ammonium group-containing vinyl aromatic monomer unit in the hydrogenated block of the copolymer comprising 1,3-diene and vinyl aromatic monomer units varies in the range of 1% to 25%, preferably 5% to 20%, of the repeating unit constituting the hydrogenated block.
[0055] Implementation Scheme 10: The method according to any one of Implementation Schemes 1 to 9, wherein the 1,3-diene and vinyl aromatic monomers of the copolymer comprising monomer units of 1,3-diene and vinyl aromatic monomers are 1,3-butadiene and styrene, respectively.
[0056] Implementation Scheme 11: The method according to any one of Implementation Schemes 1 to 10, wherein the block represented by the symbol B accounts for 50% to 90% of the total mass of the block polymer of Formula (I), preferably 60% to 80% of the total mass of the block polymer of Formula (I).
[0057] Implementation Scheme 12: The method according to any one of Implementation Schemes 1 to 11, wherein the block represented by the symbol B is a hydrogenated block of a 1,3-butadiene homopolymer or a hydrogenated block of a copolymer of 1,3-butadiene and styrene, wherein all or part of the styrene monomer units have phenyl groups substituted by alkyl chains replaced by quaternary ammonium groups.
[0058] Implementation Scheme 13: The method according to any one of Implementation Schemes 1 to 12, wherein the content of quaternary ammonium groups in the block polymer of formula (I) is greater than or equal to 0.1 meq / g of the block polymer of formula (I) and less than or equal to 1 meq / g of the block polymer of formula (I).
[0059] Implementation Scheme 14: The method according to any one of Implementation Schemes 1 to 13, wherein the quaternary ammonium group is N-alkylpiperidinium.
[0060] Implementation Scheme 15: The method according to any one of Implementation Schemes 1 to 14, wherein the quaternary ammonium group is N-methylpiperidinium.
[0061] Implementation Scheme 16: The method according to any one of Implementation Schemes 1 to 15, wherein electron beam irradiation is carried out in the absence of a chemical curing agent.
[0062] Implementation Scheme 17: The method according to any one of Implementation Schemes 1 to 16, wherein the electron beam irradiation dose is greater than 50 kGy and less than 5000 kGy.
[0063] Implementation Scheme 18: The method according to any one of Implementation Schemes 1 to 17, wherein the electron beam irradiation dose is greater than 100 kGy and less than 3000 kGy.
[0064] Implementation Scheme 19: The method according to Implementation Scheme 18, wherein the electron beam irradiation dose is less than 2000 kGy.
[0065] Implementation Scheme 20: An anion exchange polymer membrane comprising a crosslinked ionomer, wherein the crosslinked ionomer is a block polymer of formula (I) crosslinked by electron beam irradiation. (AB) n -A (I), Symbol A represents a polyvinyl aromatic block containing a quaternary ammonium group. The symbol B represents a hydrogenated block of poly(1,3-diene) or a hydrogenated block of a copolymer containing monomer units of 1,3-diene and vinyl aromatic monomers. n is an integer equal to or greater than 1.
[0066] Implementation Scheme 21: The membrane according to Implementation Scheme 20, wherein the block polymer of Formula (I) is linear.
[0067] Implementation Scheme 22: The membrane according to Implementation Scheme 20 or 21, wherein the block polymer of Formula (I) is a triblock.
[0068] Implementation Scheme 23: The membrane according to any one of Implementation Schemes 20 to 22, wherein the 1,3-diene is 1,3-butadiene, isoprene, or a mixture thereof.
[0069] Implementation Scheme 24: The membrane according to any one of Implementation Schemes 20 to 23, wherein the polyvinyl aromatic block is a polystyrene block, a poly(α-methylstyrene) block, or a styrene / α-methylstyrene copolymer block.
[0070] Implementation Scheme 25: The membrane according to any one of Implementation Schemes 20 to 24, wherein the poly(1,3-diene) is a homopolymer of 1,3-butadiene.
[0071] Implementation Scheme 26: The membrane according to any one of Implementation Schemes 20 to 25, wherein the copolymer comprising monomer units of 1,3-diene and vinyl aromatic monomers is a copolymer of 1,3-diene and vinyl aromatic monomers, wherein some or all of the vinyl aromatic monomer units have aryl groups substituted by alkyl chains replaced by quaternary ammonium groups.
[0072] Implementation Scheme 27: The membrane according to any one of Implementation Schemes 20 to 26, wherein the aryl group is phenyl.
[0073] Implementation Scheme 28: The membrane according to any one of Implementation Schemes 20 to 27, wherein the molar content of vinyl aromatic monomer units and quaternary ammonium-containing vinyl aromatic monomer units in the hydrogenated block of the copolymer comprising 1,3-diene and vinyl aromatic monomer units varies in the range of 1% to 25%, preferably 5% to 20%, of the repeating units constituting the hydrogenated block.
[0074] Implementation Scheme 29: The membrane according to any one of Implementation Schemes 20 to 28, wherein the 1,3-diene and vinyl aromatic monomers of the copolymer comprising monomer units of 1,3-diene and vinyl aromatic monomers are 1,3-butadiene and styrene, respectively.
[0075] Implementation Scheme 30: The membrane according to any one of Implementation Schemes 20 to 29, wherein the block represented by the symbol B accounts for 50% to 90% of the total mass of the block polymer of Formula (I), preferably 60% to 80% of the total mass of the block polymer of Formula (I).
[0076] Implementation Scheme 31: The membrane according to any one of Implementation Schemes 20 to 30, wherein the block represented by the symbol B is a hydrogenated block of a 1,3-butadiene homopolymer or a hydrogenated block of a copolymer of 1,3-butadiene and styrene, wherein all or part of the styrene monomer units have phenyl groups substituted by alkyl chains replaced by quaternary ammonium groups.
[0077] Implementation Scheme 32: The membrane according to any one of Implementation Schemes 20 to 31, wherein the content of quaternary ammonium groups in the block polymer of Formula (I) is greater than or equal to 0.1 meq / g of the block polymer of Formula (I) and less than or equal to 1 meq / g of the block polymer of Formula (I).
[0078] Implementation Scheme 33: The membrane according to any one of Implementation Schemes 20 to 32, wherein the quaternary ammonium group is N-alkylpiperidinium.
[0079] Implementation Scheme 34: The membrane according to any one of Implementation Schemes 20 to 22, wherein the quaternary ammonium group is N-methylpiperidinium.
[0080] Implementation Scheme 35: A cross-linked ionomer, which is a block polymer of formula (I) cross-linked by electron beam irradiation. (AB) n -A (I), Symbol A represents a polyvinyl aromatic block containing a quaternary ammonium group. The symbol B represents a hydrogenated block of poly(1,3-diene) or a hydrogenated block of a copolymer containing monomer units of 1,3-diene and vinyl aromatic monomers. n is an integer equal to or greater than 1.
[0081] Implementation Scheme 36: A fuel cell or electrolyzer comprising a membrane as defined in any one of Implementation Schemes 20 to 34 or comprising a membrane obtainable by any one of Implementation Schemes 1 to 19. Detailed Implementation
[0082] The above and other features of the invention will be better understood by reading the following description of several exemplary embodiments of the invention, which are given by way of illustration.
[0083] Example The crosslinked ionomer constituting the membrane according to the invention is prepared from a commercial product according to the following steps in sequence: 1) Commercial products are brominated and alkylated to prepare brominated polymers, wherein vinyl aromatic monomer units are replaced by alkyl groups substituted with bromine atoms. 2) A thin film of brominated polymer is formed by coating. 3) Tertiary amines react with brominated polymers in thin film form to form ionomers in thin film form. 4) Irradiate the thin film obtained at the end of step 3 with an electron beam.
[0084] The commercial product “G1652” from Kraton is a triblock hydrogenated block polymer, wherein the central block is polybutadiene and the terminal block is polystyrene, and the hydrogenation rate of the butadiene unit is greater than 99%. Table 1 shows the composition and macroscopic structure of the commercial product (number-average molar mass Mn measured by size exclusion chromatography and PS calibration).
[0085] Table 1: Step 1: The commercial product is brominated and alkylated according to the following procedure: Place the polymer and solvent dichloromethane into a bottle and stir until completely dissolved (approximately 2 hours at ambient temperature (23°C)). Then place the bottle at 5°C for 12 hours. Nitrogen gas was bubbled into the polymer solution at 5°C for 10 minutes. Cool the solution to 0°C in an ice bath and maintain for 30 minutes; While stirring, add trifluoroacetic acid (0.6 acid / styrene equivalent) (yellow / orange) dropwise over 1 minute at 0°C. Stir at 0°C for 30 minutes (yellow / orange); After the stirring time is over, allow the solution to return to ambient temperature. The olefin 6-bromo-1-hexene was added dropwise over 45 minutes using a syringe pump (the solution turned red), while stirring. Stir for another 90 minutes at ambient temperature (23°C) (the color will turn dark red); Add methanol as a reaction terminator (for medium decolorization). Neutralize by adding KOH in batches of methanol solution (1 M) until the pH reaches 7-8 (a small amount of precipitate forms and the color changes from grayish-white to purplish-red). Methanol was rapidly added dropwise into the vortex, solidified in methanol (three times the reaction volume), and then the polymer was recovered using a filter. The polymer is poured into a deionized water bath and stirred for 10 minutes (to remove salt) to clean the polymer, which is then recovered using a filter. The polymer was recovered and dried in an oven at 40°C and 150 mbar for 24 hours.
[0086] The contents of ethylene, butene, styrene, and substituted styrene units in the brominated polymer were measured by NMR analysis and are shown in Table 2; the term "substituted styrene" refers to styrene units substituted with alkyl groups by bromine atoms.
[0087] Table 2: Step 2: A thin film of brominated polymer is formed by coating: Five thin films, F1 to F5, were prepared according to the following procedure: a) Prepare a toluene solution containing the brominated polymer. b) Pour the solution onto a flat polytetrafluoroethylene (PTFE) carrier with two 1200-micron-high pads on both sides, and form a 1200-micron-thickness solution layer using a scraper. c) Evaporate the solvent at ambient temperature for 120 minutes, while simultaneously rinsing with air to dry the layer. d) Recover the film on the carrier and peel the film off its carrier.
[0088] The thickness of the film ranges from 90 micrometers to 110 micrometers.
[0089] Step 3: The reaction of tertiary amines with brominated polymers in thin film form: Prepare a 20 wt% deionized aqueous solution of N-methylpiperidine; In a glass container (such as a beaker, crystallizing dish, or wide-mouth bottle), pour the solution to 3 / 4 of its volume; Carefully dip the film in using tweezers to avoid forming air bubbles and / or the film folding itself. Place a glass lens on the container to isolate it from the external environment; Immerse the film at ambient temperature for 72 hours; Replace the solution with deionized water to clean the membrane. Change the water twice a day for two consecutive days. The membrane was placed on a PTFE support, and the assembly was then placed in an oven at 40°C and 150 mbar overnight.
[0090] The contents of ethylene, butene, styrene, and substituted styrene units in the ionomers were determined by NMR analysis of the brominated polymer contents, as shown in Table 2.
[0091] Step 4: Electron beam irradiation of ionomers in thin film form: Except for film F1, all other films were irradiated with an electron beam (using an EBLab200 from manufacturer Skan Stein AG). The absorbed irradiation dose for each film is shown in Table 3. The dose is expressed in kilograys (kGy). Since the device can irradiate up to 300 kGy in a single pass, films were irradiated multiple times for doses greater than 300 kGy. For dose 2: one dose of 300 kGy plus one dose of 200 kGy; For dose 3: 3 times 300 kGy; For dose 4: four 300 kGy doses plus one 200 kGy dose.
[0092] Table 3: The other five films, F6 through F10, were obtained from Dioxide Materials. They consist of a commercial ionomer, specifically the T-grade Sustainion 37-50, described in "Energy Technol. 2017, 5, 929-936," which is a reaction product between 1-methylimidazolium and copolymers of styrene and chloromethylstyrene. It is not a block copolymer of formula (I).
[0093] Table 4 shows the solvents used and the mass concentrations of the polymers in the solutions for films F1 to F5. Films F6 to F10 consist of "Sustaining" films with a thickness of 50 micrometers.
[0094] Table 4: Membranes F2 to F5, F7 to F8, and F1 and F6 were subjected to alkaline degradation under the following conditions to evaluate their lifespan as anion exchange membranes. Their water absorption and anion conductivity were also measured. The results are shown in Table 5.
[0095] The stability of films F9 and F10 could not be evaluated because electron beam irradiation caused them to crack.
[0096] Alkaline degradation conditions: The membrane was immersed in an aqueous solution of potassium hydroxide, in which hydroxide ions (HO ions) were present. - The active substance was considered to be KOH. Degradation conditions were achieved by stirring in a 500 mL reaction volume, at a KOH concentration of 5 mol / L, and at 80 °C. The residual mass of the membrane after 300 hours of soaking was used to estimate the membrane degradation rate.
[0097] Measurement of ionic conductivity: To determine the ionic conductivity of the prepared membrane, its electrochemical impedance across the membrane plane was measured at 30 °C and 30% relative humidity, with the measurement parameters being an amplitude change of 50 mV and an applied potential of 0 V.
[0098] To measure conductivity, the halide equilibrium ions are replaced with hydroxide anions according to the following procedure: The cross-linked ionomer, which forms a thin film and thus a membrane, was immersed in a 1 M potassium hydroxide demineralized aqueous solution at ambient temperature (23°C) for 24 hours to facilitate ion exchange between bromide and hydroxide ions. It was then soaked in the demineralized aqueous solution for 15 minutes to remove excess hydroxide ions.
[0099] It absorbs 100% water by mass.
[0100] Then the ionic conductivity was measured.
[0101] Table 5: Films F2 to F5 are films according to the invention and they are prepared according to the method of the invention. Films F6 to F10 are not films according to the invention, and they are not prepared according to the method of the invention, as the ionomers constituting the films do not conform to formula (I). Film F1 is not a film according to the invention because film F1 has not been irradiated with an electron beam. Film F6 is also not a film according to the invention for two reasons: the ionomer does not conform to formula (I) and the film has not been irradiated with an electron beam.
[0102] Compared to non-inventory membranes that have not been irradiated by an electron beam, the membranes according to the invention exhibit significantly less alkali degradation and offer a better trade-off between properties such as water absorption, ionic conductivity, and resistance to alkali degradation. "Sustainion" membranes subjected to electron beam irradiation under the same conditions as the membranes according to the invention exhibit poor resistance to alkali degradation or even become too fragile to be used for alkali degradation testing.
Claims
1. A method for preparing anion-exchange polymer membrane comprising a crosslinked ionomer, the method comprising electron beam irradiation of the ionomer in the form of a thin film, said ionomer being a block polymer of formula (I), (A-B) n -A (I), Symbol A represents a polyvinyl aromatic block containing a quaternary ammonium group. The symbol B represents a hydrogenated block of poly(1,3-diene) or a hydrogenated block of a copolymer containing monomer units of 1,3-diene and vinyl aromatic monomers. n is an integer equal to or greater than 1.
2. The method according to claim 1, wherein, The block polymer of formula (I) is linear.
3. The method according to claim 1 or 2, wherein, The block polymer of formula (I) is a triblock.
4. The method according to any one of claims 1 to 3, wherein, The polyvinyl aromatic block is a polystyrene block, a poly(α-methylstyrene) block, or a styrene / α-methylstyrene copolymer block.
5. The method according to any one of claims 1 to 4, wherein, The poly(1,3-diene) is a homopolymer of 1,3-butadiene.
6. The method according to any one of claims 1 to 5, wherein, A copolymer comprising monomer units of 1,3-diene and vinyl aromatic monomers is a copolymer of 1,3-diene and vinyl aromatic monomers, wherein some or all of the vinyl aromatic monomer units have aryl groups substituted by alkyl chains replaced by quaternary ammonium groups.
7. The method according to any one of claims 1 to 6, wherein, In the hydrogenated block of a copolymer comprising monomer units of 1,3-diene and vinyl aromatic monomers, the molar content of vinyl aromatic monomer units and vinyl aromatic monomer units with quaternary ammonium groups varies from 1% to 25%, preferably 5% to 20%, of the repeating units constituting the hydrogenated block.
8. The method according to any one of claims 1 to 7, wherein, The copolymers comprising monomer units of 1,3-diene and vinyl aromatic monomers contain 1,3-butadiene and styrene, respectively.
9. The method according to any one of claims 1 to 8, wherein, The block represented by the symbol B accounts for 50% to 90% of the total mass of the block polymer of formula (I), preferably 60% to 80% of the total mass of the block polymer of formula (I).
10. The method according to any one of claims 1 to 9, wherein, The content of quaternary ammonium groups in the block polymer of formula (I) is greater than or equal to 0.1 meq / g of the block polymer of formula (I) and less than or equal to 1 meq / g of the block polymer of formula (I).
11. The method according to any one of claims 1 to 10, wherein, The quaternary ammonium group is N-alkylpiperidinium, preferably N-methylpiperidinium.
12. The method according to any one of claims 1 to 11, wherein, Electron beam irradiation is performed in the absence of chemical curing agents.
13. An anion exchange polymer membrane comprising a crosslinked ionomer, said crosslinked ionomer being a block polymer of formula (I) crosslinked by electron beam irradiation. (A-B) n -A (I), Symbol A represents a polyvinyl aromatic block containing a quaternary ammonium group. The symbol B represents a hydrogenated block of poly(1,3-diene) or a hydrogenated block of a copolymer containing monomer units of 1,3-diene and vinyl aromatic monomers. n is an integer equal to or greater than 1. The membrane can be obtained by the method defined in any one of claims 1 to 12.
14. A cross-linked ionomer, which is a block polymer of formula (I) cross-linked by electron beam irradiation, (A-B) n -A (I), Symbol A represents a polyvinyl aromatic block containing a quaternary ammonium group. The symbol B represents a hydrogenated block of poly(1,3-diene) or a hydrogenated block of a copolymer containing monomer units of 1,3-diene and vinyl aromatic monomers. n is an integer equal to or greater than 1.
15. A fuel cell or electrolyzer comprising a membrane as defined in claim 13 or comprising a membrane obtainable by any one of the methods defined in claims 1 to 12.
Citation Information
Patent Citations
Method for preparing a dilithium initiator and anionic polymerisation method
EP1237941A1
Polymer electrolyte membrane for solid polymer fuel cell, membrane-electrode assembly and fuel cell
EP1840993B1
Sulfonated block copolymers, method for making same, and various uses for such block copolymers
US20070021569A1
Sulfonated block copolymers
US5239010A
Fuel cell incorporating novel ion-conducting membrane
US5468574A