Electrochemical cell

CN123165705APending Publication Date: 2026-11-24DENSO CORP
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202580030158.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2024-04-26
Filing Date
2025-03-11
Publication Date
2026-11-24

Smart Images

  • Figure CN123165705A_ABST
    Figure CN123165705A_ABST
Patent Text Reader

Abstract

The electrochemical cell (1) sequentially comprises: a fuel electrode layer (2) serving as an electrode for which fuel is supplied; a solid electrolyte layer (3) having oxygen ion conductivity; and an air electrode layer (4) serving as an electrode paired with the fuel electrode layer (2). The solid electrolyte layer (3) has an electrolyte host layer (31) in contact with the fuel electrode layer (2). The electrolyte host layer (31) has a composite oxide phase comprising a first crystalline phase and a second crystalline phase, the first crystalline phase having a fluorite structure and being oriented with Ce. 1‑x (RE) x O 2‑x / 2 (Where x is greater than or equal to 0.05 and less than or equal to 0.2, and the RE element is at least one of Gd and Sm) is used to represent the second crystal phase, which is represented by (ZnO)(CeO). 2‑δ ) y (where δ > 0 and y is greater than 0.15 and less than 0.7) indicates.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] Cross-references to related applications

[0002] This application is based on Japanese Application No. 2024-072885, filed on April 26, 2024, the contents of which are incorporated herein by reference. Technical Field

[0003] This disclosure relates to electrochemical batteries. Background Technology

[0004] Previously, electrochemical cells using a solid electrolyte layer with oxygen ion conductivity as the electrolyte layer were known. Examples of such electrochemical cells include solid oxide fuel cells (SOFCs) and solid oxide electrolysis cells (SOECs).

[0005] For example, Patent Document 1 discloses a SOFC using a cerium oxide-based solid electrolyte, which is formed by forming an oxide layer with a perovskite-type crystal structure having an MCa(1-x)R(x)O(3-α) (M represents an alkaline earth element, R represents a rare earth element or Zn, Mn or In. Additionally, 0.05 ≤ x ≤ 0.20) on the surface of a cerium oxide-based substrate. This document describes how, by using the aforementioned cerium oxide-based solid electrolyte, the reduction of cerium is suppressed on the fuel electrode side in a particularly harsh environment exposed to reducing gases.

[0006] Existing technical documents

[0007] Patent documents

[0008] Patent Document 1: Japanese Patent Application Publication No. 2005-243473 Summary of the Invention

[0009] The existing technology has the following technical problems. In Patent Document 1, the Ce atom in the oxide layer with a perovskite-type crystal structure is tetravalent, and this Ce atom changes to trivalent when exposed to high temperature and a reducing atmosphere. Therefore, in the technology of Patent Document 1, the reduction expansion suppression effect of the solid electrolyte layer is insufficient, making it difficult to suppress the generation of cracks during operation. Furthermore, this material is also known as a proton conductor and is known to undergo chemical expansion due to hydration reactions. Therefore, it is even more difficult to suppress cracks during operation when exposed to reducing gases containing H2O.

[0010] The purpose of this disclosure is to provide an electrochemical battery that can suppress the generation of cracks in the electrolyte body layer in contact with the fuel electrode layer during operation.

[0011] One aspect of this disclosure lies in an electrochemical battery. The electrochemical cell sequentially comprises: a fuel electrode layer serving as an electrode for which fuel is supplied; a solid electrolyte layer having oxygen ion conductivity; and an air electrode layer serving as an electrode paired with the fuel electrode layer. The solid electrolyte layer has an electrolyte body layer in contact with the fuel electrode layer. The electrolyte host layer has a composite oxide phase comprising a first crystalline phase and a second crystalline phase, wherein the first crystalline phase has a fluorite structure and is predominantly Ce. 1-x (RE) x O 2-x / 2 (Where x is 0.05 to 0.2, and RE element is at least one of Gd and Sm) represents the second crystal phase as (ZnO)(CeO) 2-δ ) y (where δ > 0 and y is greater than 0.15 and less than 0.7) indicates.

[0012] The aforementioned electrochemical cell has the above-described configuration. Therefore, during operation, even when the electrolyte substrate in contact with the fuel electrode layer is exposed to high temperatures and a reducing atmosphere, the reducing expansion of the electrolyte substrate is reduced. Thus, the aforementioned electrochemical cell can suppress the formation of cracks in the electrolyte substrate during operation.

[0013] Furthermore, the reference numerals in parentheses in the claims indicate the correspondence with the specific means described in the following embodiments, and do not limit the technical scope of this disclosure. Attached Figure Description

[0014] The above-mentioned objects, other objects, features, and advantages of this disclosure will become more apparent with reference to the accompanying drawings and the following detailed description. The drawings are described below.

[0015] Figure 1 This is an illustrative diagram schematically showing an example of the stacked structure of the electrochemical cell involved in the embodiment.

[0016] Figure 2 This is an illustrative diagram schematically showing another example of the stacked structure of the electrochemical cell involved in the embodiment.

[0017] Figure 3 This is a SEM image showing the stacked structure of the electrochemical cell fabricated in the experimental example.

[0018] Figure 4 It is shown in magnification Figure 3 A magnified view of a portion of the SEM image shown.

[0019] Figure 5 This is a diagram showing the crystal phase identification results of the electrolyte host layer obtained in Experimental Example 1.

[0020] Figure 6 The graph shows the Zn mole fraction (ratio to Ce) in the composite oxide phase obtained in Experimental Example 1 (horizontal axis) and the linear expansion coefficient (×10) of the electrolyte bulk layer. -6 A graph showing the relationship between / K, 4% H2 (volume), and 650℃ (vertical axis).

[0021] Figure 7 The graph shows the Zn mole fraction (ratio to Ce) in the composite oxide phase obtained in Experimental Example 1 (horizontal axis) and the oxygen ion conductivity (×10) of the electrolyte bulk layer. -2 A graph showing the relationship between S / cm and temperature (650℃) (vertical axis).

[0022] Figure 8 This shows the temperature (°C) (horizontal axis) and the coefficient of linear expansion of the electrolyte bulk layer (×10) obtained in Experimental Example 2. -6 A graph showing the relationship between / K and 4%H2 (vertical axis). Detailed Implementation

[0023] use Figure 1 , Figure 2 The electrochemical cell of this embodiment will be described. Furthermore, in this disclosure, the lower and upper limits of the numerical range can be arbitrarily combined (hereinafter omitted).

[0024] like Figure 1 , Figure 2 As illustrated, the electrochemical cell 1 of this embodiment sequentially comprises a fuel electrode layer 2, a solid electrolyte layer 3, and an air electrode layer 4. Figure 1 , Figure 2 In this configuration, the fuel electrode layer 2 is disposed on one side of the solid electrolyte layer 3, and the air electrode layer 4 is disposed on the other side of the solid electrolyte layer 3. Figure 1 , Figure 2 Specifically, the diagram shows an example where a fuel electrode layer 2, a solid electrolyte layer 3, and an air electrode layer 4 are stacked sequentially, with the fuel electrode layer 2 and the solid electrolyte layer 3 bonded together, and the solid electrolyte layer 3 and the air electrode layer 4 bonded together via an intermediate layer 6 (described later). The fuel electrode layer 2 is the electrode to which fuel is supplied. That is, the fuel electrode layer 2 can be considered an electrode layer with electrode activity capable of functioning as a fuel electrode. The air electrode layer 4 is the electrode paired with the fuel electrode layer 2. That is, the air electrode layer 4 can be considered an electrode layer with electrode activity capable of functioning as an air electrode. Furthermore, the electrochemical cell 1 can be configured as follows... Figure 1 , Figure 2Although not illustrated, the battery structure with a flat plate shape can also be cylindrical. Furthermore, the electrochemical battery 1 of this embodiment can be any of the following structures: electrolyte-supported, electrode-supported (fuel electrode-supported, air electrode-supported), or metal-supported.

[0025] In the electrochemical cell 1, the solid electrolyte layer 3 has oxygen ion conductivity. The solid electrolyte layer 3 has an electrolyte host layer 31 in contact with the fuel electrode layer 2. The solid electrolyte layer 3 can be as follows: Figure 1 , Figure 2 Although not illustrated, a multi-layered structure can also be constructed from a single layer. Figure 1 , Figure 2 The diagram shows an example of a solid electrolyte layer 3 having two layers: an electrolyte host layer 31 and an electron blocking layer 32 formed on the surface of the electrolyte host layer 31 on the side of the air electrode layer 4. The electrolyte host layer 31 is the electrolyte layer constituting the main body of the solid electrolyte layer 3, and functions as the electrolyte in the electrochemical cell 1. Alternatively, if the solid electrolyte layer 3 is a single layer, that single layer becomes the electrolyte host layer 31. The electron blocking layer 32 is a layer used to impede electron movement. With the electron blocking layer 32, since electron movement can be impeded through the electron blocking layer 32, the electrolyte host layer 31 can exhibit electron conductivity in addition to oxygen ion conductivity, for example, under a reducing atmosphere. As described above, the solid electrolyte layer 3 has an electrolyte host layer 31 in contact with the fuel electrode layer 2, and its layer configuration is not particularly limited as long as it is configured to function as the electrolyte in the electrochemical cell 1.

[0026] Furthermore, electrochemical cell 1 can be like Figure 2 As illustrated, a fuel diffusion layer 5 is provided on the side of the fuel electrode layer 2 opposite to the solid electrolyte layer 3, in contact with the fuel electrode layer 2. The fuel diffusion layer 5 is a layer that functions to diffuse the fuel supplied to the fuel electrode layer 2. Furthermore, the fuel diffusion layer 5 can also function to diffuse electrons. With the fuel diffusion layer 5, diffused fuel can be supplied to the fuel electrode layer 2. In addition to its fuel diffusion function, such as diffusing fuel in a planar direction, the fuel diffusion layer 5 can also be configured to function as a support layer supporting the layers on the fuel electrode layer 2 side. Furthermore, the fuel diffusion layer 5 can also function as a current collector for the fuel electrode layer 2.

[0027] Furthermore, electrochemical cell 1 can be like Figure 1 , Figure 2 As illustrated, an intermediate layer 6 exists between the solid electrolyte layer 3 and the air electrode layer 4. The intermediate layer 6 primarily serves to suppress the reaction between the materials of the solid electrolyte layer 3 and the air electrode layer 4 (reaction inhibition layer). Figure 1 , Figure 2The image shows an example of an intermediate layer 6 contacting and bonding with the solid electrolyte layer 3 and the air electrode layer 4.

[0028] Furthermore, electrochemical cell 1 can be like Figure 2 As illustrated, an air electrode current collector layer 7 is provided on the side of the air electrode layer 4 opposite to the solid electrolyte layer 3. The air electrode current collector layer 7 is a layer that functions as a current collector for the air electrode layer 4.

[0029] In the electrochemical cell 1, the thickness of the fuel electrode layer 2 can be, for example, 10 μm to 100 μm. The thickness of the solid electrolyte layer 3 can be, for example, 2 μm to 20 μm. The thickness of the electrolyte host layer 31 can be, for example, 1 μm to 15 μm. The thickness of the electron blocking layer 32 can be, for example, 1 μm to 15 μm. The thickness of the air electrode layer 4 can be, for example, 10 μm to 100 μm. The thickness of the fuel diffusion layer 5 can be, for example, 100 μm to 800 μm. The thickness of the intermediate layer 6 can be, for example, 1 μm to 20 μm. The thickness of the air electrode current collector layer 7 can be, for example, 1 μm to 100 μm.

[0030] In the electrochemical cell 1 capable of having the above-described layered structure, the electrolyte host layer 31 has a composite oxide phase comprising a first crystalline phase and a second crystalline phase. In the composite oxide phase, the first crystalline phase has a fluorite structure and contains Ce. 1-x (RE) x O 2-x / 2 The first crystal phase represents the chemical composition of the crystal. In this first crystal phase, x is 0.05 to 0.2, and the RE element is at least one of Gd and Sm.

[0031] In the first crystal phase, from the viewpoint of obtaining high oxygen ion conductivity, x is preferably 0.06 or more and 0.18 or less, more preferably 0.08 or more and 0.15 or less. Furthermore, from the viewpoint of obtaining high oxygen ion conductivity at a relatively low cost, the RE element is preferably Gd.

[0032] In the composite oxide phase, the second crystalline phase is (ZnO)(CeO) 2-δ ) y The crystalline phase represents the chemical composition of the second crystalline phase. In this second phase, δ > 0, and y is between 0.15 and 0.7.

[0033] In the second crystal phase, from the viewpoint of suppressing reduction expansion, γ is preferably 0.3 or more, more preferably 0.4 or more, even more preferably 0.5 or more, and even more preferably 0.55 or more. Furthermore, from the viewpoint of suppressing reduction expansion, δ is preferably 0.1 or more, more preferably 0.3 or more, and even more preferably 0.7 or more.

[0034] The states of the first and second crystal phases in the composite oxide phase are not particularly limited, but examples can be given such as: the state in which the first crystal phase contains the second crystal phase (the state in which the first crystal phase is mixed with the second crystal phase, the state in which a portion of the second crystal phase is dissolved in the first crystal phase, the state in which the second crystal phase is dispersed in the first crystal phase, etc.), and the state in which the first crystal phase is the core and its surface is covered by the second crystal phase.

[0035] The electrolyte host layer 31 may also contain phases other than the composite oxide phase. Examples of other phases include phases containing elements constituting the electron blocking layer 32, partially stabilized ZrO2 phases, CeO2-ZrO2 solid solution phases, etc., used to improve the bonding force with the electron blocking layer 32. These may contain one or more phases.

[0036] In the composite oxide phase, the ratio of the number of moles of Zn to the number of moles of Ce contained in the first crystal phase (sometimes referred to in this disclosure as "Zn mole fraction (ratio to Ce)") is preferably 1.1 mol% or more. According to this configuration, compared to the case where the Zn mole fraction (ratio to Ce) is less than 1.1 mol%, the reduction expansion of the electrolyte host layer 31 can be suppressed more effectively, and crack avoidance during operation in the electrolyte host layer 31 can be achieved with a higher probability. From the viewpoint of making the above effects more reliable, the Zn mole fraction (ratio to Ce) is more preferably 1.3 mol% or more, further preferably 1.5 mol% or more, and even more preferably 1.8 mol% or more.

[0037] In the composite oxide phase, the Zn molar fraction (ratio to Ce) is preferably 4.6 mol% or less. According to this configuration, compared to cases where the Zn molar fraction (ratio to Ce) exceeds 4.6 mol%, it is possible to maintain a higher oxygen ion conductivity of the electrolyte host layer 31 while avoiding cracking during operation. Therefore, according to this configuration, the output of the electrochemical cell 1 can be easily improved. From the viewpoint of making the above effects more reliable, the Zn molar fraction (ratio to Ce) is more preferably 4.4 mol% or less, further preferably 4.2 mol% or less, and even more preferably 4.0 mol% or less.

[0038] Furthermore, the detailed composition of the composite oxide phase and the Zn mole fraction (relative to Ce) can be determined by Rietveld analysis of the X-ray diffraction (XRD) results. Details will be provided in the experimental examples.

[0039] When the electrochemical cell 1 is in operation, even when the electrolyte body layer 31, which is in contact with the fuel electrode layer 2, is exposed to high temperature and a reducing atmosphere, the reducing expansion of the electrolyte body layer 31 can be reduced. Therefore, even when using a cerium oxide-based solid electrolyte material, the electrochemical cell 1 can suppress the generation of cracks in the electrolyte body layer 31 during operation.

[0040] In addition, the electrochemical cell 1 of this embodiment has the following advantages.

[0041] As described above, in the electrochemical cell of Patent Document 1, an oxide layer with a perovskite-type crystal structure is formed on the surface of the cerium oxide-based substrate. The reduction expansion suppression effect of the electrolyte layer is insufficient, and it cannot suppress crack generation during operation. Therefore, the thin-film formation of the electrolyte layer is practically difficult. In contrast, electrochemical cell 1 can suppress crack generation caused by reduction expansion. Therefore, compared to the electrochemical cell of Patent Document 1, it is easier to achieve thin-film formation of the electrolyte substrate layer 31.

[0042] Furthermore, solid electrolyte materials with perovskite-type crystal structures have low oxygen ion conductivity. Therefore, as in the electrochemical cell of Patent Document 1, when an oxide layer with a perovskite-type crystal structure is formed on the surface of a cerium oxide-based substrate, this oxide layer becomes a resistive phase, reducing the cell's output. In contrast, in electrochemical cell 1, the composite oxide phase, in addition to a specific cerium oxide-based first crystal phase with a fluorite structure, also contains a specific second crystal phase containing Ce and Zn. This composite oxide phase is used in the electrolyte host layer 31, which is in contact with the fuel electrode layer 2. Therefore, compared to the electrochemical cell of Patent Document 1, electrochemical cell 1 more easily improves the cell's output.

[0043] Furthermore, solid electrolyte materials with a perovskite-type crystal structure are materials with hydrogen ion conductivity. Therefore, when the electrochemical cell of Patent Document 1 is used as an SOEC, the H2O generated by the electrolysis of H2O introduced into the fuel electrode... + A portion of the hydrogen flows through the electrolyte layer to the air electrode side, reducing hydrogen generation. In contrast, in electrochemical cell 1, the composite oxide phase, in addition to a specific cerium oxide-based first crystal phase with a fluorite structure, also contains a specific second crystal phase containing Ce and Zn. This composite oxide phase is used in the electrolyte host layer 31, which is in contact with the fuel electrode layer 2. Therefore, even when used as an SOEC (described later), electrochemical cell 1 can suppress the generation of hydrogen due to H2O electrolysis. + The decrease in hydrogen production is caused by a portion of it flowing out to the air pole side.

[0044] Furthermore, when replacing the technology in Patent Document 1 with a method that locally enriches rare earth elements on the surface of cerium oxide-based crystal particles, rare earth elements segregate near grain boundaries during the fabrication of the sintered body. This increases the amount of oxygen vacancies near the grain boundaries and decreases the amount of oxygen vacancies within the grains. Consequently, in this case, oxygen defect association and Schottky barriers occur near the grain boundaries, reducing oxygen ion conductivity and decreasing the battery output. Additionally, in this case, manufacturing is required at oxygen partial pressures higher than atmospheric pressure, increasing manufacturing costs. In contrast, in electrochemical cell 1, the reducing expansion of the electrolyte substrate layer 31 can be reduced without locally enriching rare earth elements on the surface of the cerium oxide-based crystal particles. Therefore, compared to the above case, electrochemical cell 1 more easily suppresses the decrease in battery output. Furthermore, the electrolyte substrate layer 31 can be manufactured under atmospheric pressure, thus, compared to the above case, electrochemical cell 1 is more easily cost-effective.

[0045] The electrochemical battery 1 described above can be configured as a solid oxide type battery using a material with oxygen ion conductivity as the electrolyte. There are no particular limitations on the materials and composition of the fuel electrode layer 2, solid electrolyte layer 3 (electron blocking layer 32, etc.), air electrode layer 4, fuel diffusion layer 5, intermediate layer 6, air electrode current collector layer 7, etc., other than the electrolyte body layer 31. Specifically, these layers can be configured as follows.

[0046] The fuel electrode layer 2 can contain the aforementioned composite oxide phase. In this case, the fuel electrode layer 2 specifically contains a fuel electrode catalyst phase, the aforementioned composite oxide phase, and voids. Based on these configurations, since reduction expansion in the fuel electrode layer 2 can also be suppressed, crack formation within the fuel electrode layer 2 can be suppressed.

[0047] When the fuel electrode layer 2 contains a composite oxide phase, it can be configured such that the molar fraction of Zn in the composite oxide phase (relative to Ce) in the fuel electrode layer 2 is less than the molar fraction of Zn in the composite oxide phase (relative to Ce) in the electrolyte bulk layer 31. Since the fuel electrode layer 2 contains voids, the reduction expansion is moderated compared to the dense electrolyte bulk layer 31, but reduction expansion still typically occurs. In contrast, according to the above configuration, it is possible to achieve high output due to improved electrode performance while suppressing crack formation caused by the reduction expansion of the fuel electrode layer 2.

[0048] In addition to the aforementioned composite oxide phase, the fuel electrode layer 2 may also include a fuel electrode electrolyte phase different from the composite oxide phase. Furthermore, the fuel electrode layer 2 may also be configured not to include the aforementioned composite oxide phase. In this case, the fuel electrode layer 2 may specifically be configured to include a fuel electrode catalyst phase, a fuel electrode electrolyte phase, and voids, without the aforementioned composite oxide phase. The fuel electrode catalyst phase may be composed of a fuel electrode catalyst material with electronic conductivity, or the like. The fuel electrode electrolyte phase may be composed of a solid electrolyte material with oxygen ion conductivity, or the like.

[0049] Examples of fuel electrode catalyst materials constituting the catalyst phase within the fuel electrode include electronic conductors (metals, alloys, hereinafter omitted) such as Ni, Ni alloys, Cu, Cu alloys, Co, Co alloys, etc., Ni oxides (NiO, etc.), Cu oxides, Co oxides, etc., which are reduced to electronic conductors (metal oxides, alloy oxides, hereinafter omitted). One or more of these can be used together. Among these, from the viewpoint of catalytic activity (electrode activity), Ni, Ni alloys, Ni oxides (NiO, etc.) are preferred, and Ni, NiO, etc. are more preferred. Furthermore, examples of solid electrolyte materials constituting the electrolyte phase within the fuel electrode include cerium oxide (CeO2) (hereinafter sometimes referred to as cerium oxide-based oxides) doped with one or more elements selected from Gd, Sm, Y, Sc, La, Nd, Yb, Ca, and Ho, cerium oxide, yttrium-stabilized zirconium oxide (YSZ), scandium oxide-stabilized zirconium oxide (ScSZ), etc. One or more of these can be used together. In addition, the fuel electrode layer 2 includes a fuel electrode internal catalyst phase composed of fuel electrode catalyst materials made of metals, alloys, their oxides, etc., as well as the aforementioned composite oxide phase, and can be described as a metal-ceramic electrode layer.

[0050] In, for example, Figure 1 When the solid electrolyte layer 3 is configured such that it includes an electron blocking layer 32 in addition to the electrolyte body layer 31, the electron blocking layer 32 can be made of a solid electrolyte material that is non-electronically conductive but oxygen-ion conductive under the oxygen partial pressure during operation. Examples of solid electrolyte materials that are non-electronically conductive but oxygen-ion conductive include yttrium-stabilized zirconium oxide (YSZ) and scandium oxide-stabilized zirconium oxide (ScSZ). One or more of these can be used together. Among these, yttrium-stabilized zirconium oxide (YSZ) is preferred from the viewpoint of being stable in a reducing atmosphere and not exhibiting electronic conductivity. In addition, the solid electrolyte layer 3 is usually formed as a dense material in a gas-impermeable manner.

[0051] Specifically, the air electrode layer 4 can include an air electrode internal catalyst phase, an air electrode internal electrolyte phase, and voids. The air electrode internal catalyst phase can be composed of an air electrode catalyst material with electron conductivity and oxygen ion conductivity. The air electrode internal electrolyte phase can be composed of a solid electrolyte material with oxygen ion conductivity.

[0052] Examples of perovskite catalyst materials constituting the catalyst phase within the air electrode include perovskite oxides containing La, Sr, and Co; perovskite oxides containing Pr, Ba, and Co; perovskite oxides containing Gd, Ba, and Co; and perovskite oxides containing Nd, Ba, and Co. One or more of these can be used in combination. From the viewpoint of excellent mixed conductivity (coexisting with both electronic and oxygen ion conductivity) and high air electrode catalytic activity, perovskite oxides containing La, Sr, and Co are suitable as air electrode catalyst materials. Specifically, examples of the aforementioned perovskite oxides containing La, Sr, and Co include La... 0.6 Sr 0.4 CoO3 and other components with La 1-x Sr x CoO 3-δ Metal oxides, etc., represented by (0 < x ≤ 1, preferably 0.1 ≤ x ≤ 0.5). Specifically, perovskite oxides containing Pr, Ba, and Co can be exemplified by Pr... 2-x Ba x Co2O 5+δ Metal oxides, etc., expressed as (0.7≤x≤1.3, preferably 0.8≤x≤1). Specifically, perovskite oxides containing Gd, Ba, and Co can be exemplified by those containing Gd... 2-x Ba x Co2O 5+δ Metal oxides, etc., expressed as (0.7≤x≤1.3, preferably 0.8≤x≤1). Specifically, perovskite oxides containing Nd, Ba, and Co can be exemplified by those containing Nd... 2- x Ba x Co2O 5+δ Metal oxides, etc., represented by (0.7≤x≤1.3, preferably 0.8≤x≤1). Furthermore, the aforementioned oxides may or may not have an indefinite oxygen ratio.

[0053] Examples of solid electrolyte materials constituting the electrolyte phase within the air electrode include the aforementioned cerium oxide-based oxides and cerium oxide. One or more of these can be used together. From the viewpoint of excellent oxygen ion conductivity at relatively low temperatures of around 700°C, cerium oxide doped with at least one of Gd and Sm is preferred as the solid electrolyte material constituting the electrolyte phase within the air electrode; cerium oxide doped with Gd is more preferred.

[0054] The fuel diffusion layer 5 can be configured as a porous material with voids and / or through-holes to avoid hindering fuel supply to the fuel electrode layer 2. The fuel diffusion layer 5 can contain the aforementioned composite oxide phase. In this case, the fuel diffusion layer 5 specifically contains an electron-conducting phase, the aforementioned composite oxide phase, and voids. Based on these configurations, since reduction expansion in the fuel diffusion layer 5 can also be suppressed, crack formation within the fuel diffusion layer 5 can be suppressed.

[0055] When the fuel diffusion layer 5 contains a composite oxide phase, it can be configured such that the molar fraction of Zn in the composite oxide phase (relative to Ce) is less than the molar fraction of Zn in the composite oxide phase (relative to Ce) in the electrolyte host layer 31. According to this configuration, crack formation caused by reduction expansion of the fuel diffusion layer 5 can be suppressed. Furthermore, in the fuel diffusion layer 5, electronic conductivity is more important than oxygen ion conductivity. Therefore, by configuring it as having a lower molar fraction of Zn (relative to Ce) as described above, the proportion of Ce changing from +4 to +3 valence can be increased, and the accompanying reduction in electronic resistance due to hole conduction can also be expected.

[0056] In addition to the aforementioned composite oxide phase, the fuel diffusion layer 5 may also include an internal oxide phase different from the composite oxide phase. Furthermore, the fuel diffusion layer 5 may also be configured not to contain the aforementioned composite oxide phase. In this case, the fuel diffusion layer 5 may specifically be configured to contain an electronically conductive phase, an internal oxide phase, and voids, without the aforementioned composite oxide phase. The electronically conductive phase may be composed of an electronically conductive material or the like. The internal oxide phase may be composed of various oxide materials or the like.

[0057] Examples of electronically conductive materials constituting the electronically conductive phase include electronic conductors such as Ni, Ni alloys, Cu, Cu alloys, Co, and Co alloys, as well as oxides of electronic conductors such as Ni oxides (NiO, etc.), Cu oxides, and Co oxides that are reduced to electronic conductors. One or more of these can be used together. Furthermore, the electronically conductive material constituting the electronically conductive phase may or may not have catalytic activity. From the viewpoint of catalytic activity (electrode activity), Ni, Ni alloys, and Ni oxides (NiO, etc.) are preferred, and Ni and NiO are more preferred. Additionally, examples of oxide materials constituting the oxide phase within the diffusion layer include solid electrolyte materials such as cerium oxide-based oxides, cerium oxide, yttrium-stabilized zirconium oxide (YSZ), and scandium oxide-stabilized zirconium oxide (ScSZ), and various oxides that are not solid electrolyte materials such as CaO and MgO. One or more of these can be used together. Furthermore, the fuel diffusion layer 5, comprising an electronically conductive phase composed of metals, alloys, and their oxides, as well as the aforementioned composite oxide phase and the oxide phase within the diffusion layer, can be considered a metal-ceramic layer.

[0058] In addition to the above, the fuel diffusion layer 5 can also be made of metal (including alloys, hereinafter omitted) or the like. Furthermore, the electrochemical cell 1 can be supported, for example, by a metal support (not shown) disposed on the side of the fuel diffusion layer 5 opposite to the fuel electrode layer 2.

[0059] As a metallic material constituting the fuel diffusion layer 5 and the metal support, Fe-based alloys can be exemplified, for example. Furthermore, Fe-based alloys are made by adding alloying elements to Fe as a base. The alloying elements include at least one metallic element, and in addition to metallic elements, at least one non-metallic element may also be included. Furthermore, Fe is not included in the alloying elements. In addition, the aforementioned metallic elements may include half-metallic elements. Examples of metallic elements included in the alloying elements include Cr, Mn, Ti, Ni, Al, Cu, Mo, Nb, V, La, Ta, Hf, Zr, Si, and B. One or more of these can be used together. Specifically, the metallic elements included in the alloying elements may include at least Cr, and more specifically, at least Cr and at least one selected from the group consisting of Mn, Ti, Ni, Al, Cu, Mo, Nb, V, La, Ta, Hf, Zr, Si, and B. The most abundant metallic element among the metallic elements included in the Fe-based alloys may be, for example, one selected from the group consisting of Cr, Mn, and Ti. Furthermore, Fe-based alloys containing Cr as the largest additive metal element can be called Fe-Cr alloys. Similarly, Fe-based alloys containing Mn as the largest additive metal element can be called Fe-Mn alloys, and Fe-based alloys containing Ti as the largest additive metal element can be called Fe-Ti alloys.

[0060] The intermediate layer 6 can contain the aforementioned composite oxide phase. In this case, the intermediate layer 6 can specifically be composed of the aforementioned composite oxide phase, or it can contain the aforementioned composite oxide phase and an air electrode material phase composed of part or all of the air electrode material forming the air electrode layer 4 (such as the air electrode catalyst material constituting the air electrode internal catalyst phase, the solid electrolyte material constituting the air electrode internal electrolyte phase, etc.). In the electrochemical cell 1, the intermediate layer 6 is separated from the fuel electrode layer 2 by the solid electrolyte layer 3, so it is usually not exposed to a reducing atmosphere and does not undergo reducing expansion. However, when the aforementioned composite oxide phase is included, it is easy to match the coefficients of thermal expansion in the electrochemical cell 1, thus suppressing the generation of cracks caused by the difference in thermal expansion between the layers.

[0061] In addition to the aforementioned composite oxide phase, the intermediate layer 6 may also contain an intralayer electrolyte phase different from the composite oxide phase. Furthermore, the intermediate layer 6 may also be configured not to contain the aforementioned composite oxide phase. In this case, the intermediate layer 6 specifically does not contain the aforementioned composite oxide phase and may be composed of an intralayer electrolyte phase, or it may contain both an intralayer electrolyte phase and an air electrode material phase.

[0062] The electrolyte phase within the intermediate layer can be composed of a solid electrolyte material or the like that which has oxygen ion conductivity. Examples of solid electrolyte materials constituting the electrolyte phase within the intermediate layer include, for example, the aforementioned cerium oxide-based oxides, cerium oxide, yttrium oxide-stabilized zirconium oxide (YSZ), and scandium oxide-stabilized zirconium oxide (ScSZ). One or more of these can be used together.

[0063] The air electrode current collector layer 7 can be made of an air electrode current collector material with electronic conductivity suitable for current collection on the air electrode side exposed to a high-temperature oxidizing atmosphere.

[0064] Examples of air electrode current collectors include metallic materials such as Pt, Pt alloys, Ag, Ag alloys, and Au; perovskite oxides containing La, Sr, and Co; and perovskite oxides containing La, Ni, and Fe, all of which possess electronic conductivity. One or more of these can be used in combination. Among these, from the viewpoint of being difficult to oxidize in high-temperature oxidizing atmospheres and possessing high electronic conductivity, Pt and Pt alloys are preferred in the case of metallic materials, and perovskite oxides containing La, Sr, and Co are preferred in the case of electronically conductive oxides.

[0065] Electrochemical cell 1 can be used as at least one of a single-cell solid oxide fuel cell (SOFC) and a solid oxide electrolyzer (SOEC). That is, electrochemical cell 1 can be operated as an SOFC or as an SOEC, and can be configured to switch between SOFC mode as an SOFC and SOEC mode as an SOEC, so that it can operate as both SOFC and SOEC.

[0066] Specifically, when the electrochemical cell 1 operates as a SOFC, hydrogen-containing gases such as hydrogen can be supplied to the fuel electrode layer 2 as fuel gas. In this case, oxygen-containing gases such as air and oxygen can be supplied to the air electrode layer 4. On the other hand, when the electrochemical cell 1 operates as an SOEC, the fuel electrode layer 2 can function as a hydrogen electrode. Water vapor or water-containing gases (H2O) can be supplied to the fuel electrode layer 2 as fuel gas. In this case, the air electrode layer 4 can function as an oxygen electrode. Gases such as air can be supplied to the air electrode layer 4, or no gas can be supplied. In addition, the aforementioned hydrogen-containing gas can contain water vapor for humidification, etc., and the water-containing gas can contain reducing gases such as hydrogen. Furthermore, when it operates as a co-electrolyte, the fuel gas can also contain carbon dioxide (CO2) in addition to water.

[0067] The operating temperature of the electrochemical cell 1 is preferably 500°C or higher, more preferably 600°C or higher, and even more preferably 650°C or higher, from the viewpoint of reducing battery resistance and obtaining higher output. Furthermore, the operating temperature of the electrochemical cell 1 is preferably 825°C or lower, more preferably 800°C or lower, and even more preferably 775°C or lower, from the viewpoint of easily suppressing reduction expansion.

[0068] In particular, when the operating temperature of the electrochemical cell 1 is below 755°C, the electrochemical cell 1 can operate within a range that easily suppresses the rapid reduction expansion in the electrolyte host layer 31, thus having the advantage of easily achieving high output of the electrochemical cell 1.

[0069] (Experimental Example)

[0070] The electrochemical cell of this disclosure will now be described in detail using experimental examples. In the experimental examples shown below, a cell was fabricated as follows... Figure 3 and Figure 4 The illustrated electrochemical cell 1 has a stacked structure in which a fuel diffusion layer 5, a fuel electrode layer 2, a solid electrolyte layer 3, an intermediate layer 6, an air electrode layer 4, and an air electrode current collector layer 7 are stacked sequentially. In this electrochemical cell 1, the solid electrolyte layer 3 is composed of an electrolyte bulk layer 31 and an electron blocking layer 32. Furthermore, Figure 3 and Figure 4 This is a diagram of the electrochemical cell of sample 13 prepared in Experimental Example 3 described later.

[0071] (Experimental Example 1)

[0072] <Materials Preparation>

[0073] -GDC powder-

[0074] Ce was prepared as a Gd-doped cerium oxide powder. 0.9 Gd 0.1 O 1.95 (Hereinafter referred to as GDC) powder. Specifically, GDC powder is produced by weighing CeO2 as a Ce source and Gd2O3 as a Gd source in a manner that makes up the chemical composition specified above, calcining these at 800°C, and then pulverizing them.

[0075] -Zn source-

[0076] ZnO powder (average particle size: 0.1 μm) was prepared as the Zn source for forming the composite oxide phase. The average particle size mentioned above is the particle size (diameter) d50 at 50% of the cumulative frequency distribution based on volume, determined by laser diffraction-scattering method (the same applies below).

[0077] In this experimental example, ZnO was used as the Zn source starting material. However, zinc acetate, zinc acetate dihydrate, zinc nitrate, zinc nitrate hexahydrate, and zinc oxide nanoparticle suspensions can also be used. Among these, when using materials other than zinc oxide nanoparticle suspensions, voids may form due to the volatilization of acetic acid and nitric acid during firing. Therefore, when using these materials as starting materials for forming layers requiring density, such as the electrolyte body layer and intermediate layer, it is preferable to weigh the required amount of zinc nitrate, dissolve it in water, add GDC powder, mix using a ball mill, spread the recovered slurry on a tray, and dry the powder at approximately 100°C. When using zinc acetate as a starting material, it is preferable to use the material after further heating at approximately 250°C to 300°C. This pretreatment before preparing the slurry for the specified layer formation allows for the pre-decomposition and volatilization of acetic acid and nitric acid. When using these materials as Zn sources for fuel electrode layers and fuel diffusion layers, since they can also be used as pore-forming components, this pretreatment is sometimes unnecessary.

[0078] -Fuel diffusion layer-

[0079] A slurry was prepared by mixing NiO powder (average particle size: 0.5 μm), GDC powder (average particle size: 0.5 μm), acrylic resin (pore-forming agent), polyvinyl butyral, isoamyl acetate, and 1-butanol using a ball mill. The mass ratio of NiO powder to GDC powder was set to 65:35. The slurry was coated onto a resin sheet in a layered manner using a doctor blade method. After drying, the resin sheet was peeled off, thereby preparing sheets for forming the fuel diffusion layer of samples 1 to 6 and sample 1C, respectively.

[0080] -Fuel polar layer-

[0081] A slurry was prepared by mixing NiO powder (average particle size: 0.5 μm), GDC powder (average particle size: 0.5 μm), acrylic resin (pore-forming agent), polyvinyl butyral, isoamyl acetate, and 1-butanol using a ball mill. The mass ratio of NiO powder to GDC powder was set to 50:50. Furthermore, the pore-forming dosage in the fuel electrode layer forming sheet was set to be less than that in the fuel diffusion layer forming sheet. Subsequently, fuel electrode layer forming sheets for samples 1 to 6 and sample 1C were prepared in the same manner as the preparation of the fuel diffusion layer forming sheet.

[0082] -Electrolyte host layer-

[0083] A slurry was prepared by mixing GDC powder (average particle size: 0.5 μm), ZnO powder (average particle size: 0.1 μm), polyvinyl butyral, isoamyl acetate, 2-butanol, and ethanol using a ball mill. At this time, GDC powder and ZnO powder were weighed and added in a specified molar ratio. Then, in the same manner as the preparation of the sheet for forming the fuel diffusion layer, sheets for forming the electrolyte host layer for samples 1 to 6 were prepared. Furthermore, except that ZnO powder was not added, a sheet for forming the electrolyte host layer for sample 1C was also prepared.

[0084] Furthermore, in this experimental example, the process of mixing GDC powder with a Zn source is used to attempt to form a composite oxide phase, which differs from the process of weighing CeO2, Gd2O3, and ZnO to prepare a composite oxide containing Ce, Gd, and Zn and using it as a raw material. In addition, this experimental example does not involve fabricating the electrolyte host layer as a glass material containing SiO2, B2O3, etc., in addition to ZnO.

[0085] -Electron blocking layer-

[0086] A slurry was prepared by mixing yttrium-stabilized zirconium oxide (hereinafter, 8YSZ) (average particle size: 0.5 μm) containing 8 mol% Y₂O₃, polyvinyl butyral, isoamyl acetate, 2-butanol, and ethanol using a ball mill. Subsequently, in the same manner as the preparation of the sheet for forming the fuel diffusion layer, sheets for forming the electron blocking layer were prepared for samples 1 to 6 and sample 1C, respectively.

[0087] -Middle Layer-

[0088] A slurry was prepared by mixing GDC powder (average particle size: 0.5 μm), polyvinyl butyral, isoamyl acetate, 2-butanol, and ethanol using a ball mill. Subsequently, sheets for forming the intermediate layer of samples 1–6 and sample 1C were prepared in the same manner as those for forming the fuel diffusion layer.

[0089] -Atmosphere-

[0090] La 0.6 Sr 0.4 CoO3 powder (hereinafter, LSC) (average particle size: 0.8 μm) and GDC powder (average particle size: 0.3 μm) were weighed at a volume ratio of 8:2. Carbon (pore-forming agent), ethyl cellulose and terpineol were added to the mixture, and the mixture was mixed using a ball mill to prepare pastes for forming air electrode layers for samples 1 to 6 and sample 1C, respectively.

[0091] -Air Electrode Current Collector-

[0092] LSC powder (average particle size: 0.8 μm), carbon (pore-forming agent), ethyl cellulose and terpineol were added and mixed using a ball mill to prepare pastes for forming air electrode current collector layers for samples 1 to 6 and sample 1C, respectively.

[0093] <The Construction of Electrochemical Cells>

[0094] A specified sheet for forming a fuel diffusion layer, a sheet for forming a fuel electrode layer, a sheet for forming an electrolyte substrate layer, a sheet for forming an electron blocking layer, and a sheet for forming an intermediate layer are sequentially stacked to obtain a laminate. The resulting laminate is then pressed using a hot isostatic pressing (WIP) method and degreased. The WIP forming conditions are set at a temperature of 80°C, a pressure of 50 MPa, and a pressing time of 10 minutes. Next, the resulting laminate is cut into specified sizes. Then, the laminate is sintered in atmospheric atmosphere at a specified temperature (selected from the range of 1000°C to 1370°C) for 2 hours. This yields a specified ceramic substrate (sintered body) consisting of a fuel diffusion layer (200 μm thick), a fuel electrode layer (40 μm thick), an electrolyte substrate layer (5 μm thick), an electron blocking layer (5 μm thick), and an intermediate layer (5 μm thick).

[0095] Next, a specified air electrode layer forming paste is applied to the surface of the intermediate layer in the obtained ceramic substrate by screen printing, and then fired (sintered) at 1125°C for 10 minutes in an atmospheric atmosphere to form an air electrode layer (thickness 50 μm). At this time, the shape of the air electrode layer is formed to be smaller than that of the fuel electrode layer.

[0096] Next, a paste for forming the specified air electrode current collector layer is applied to the surface of the air electrode layer by screen printing, and then fired (bonded) at 900°C for 1 hour in an atmospheric atmosphere to form the air electrode current collector layer (thickness 50μm).

[0097] Based on the above, flat electrochemical cells (single cells) of samples 1 to 6 and sample 1C as shown in Table 1 were fabricated.

[0098] <Identification of the crystal phase of the electrolyte matrix and the molar fraction of Zn (relative to Ce)>

[0099] Unwanted layers, excluding the electrolyte matrix, were removed from the electrochemical cells of each sample beforehand. Only the analytical material was collected from the electrolyte matrix and pulverized in a mortar to prepare analytical powder for XRD. Next, XRD analysis was performed on the analytical powder of each sample in a large synchrotron radiation facility (SPring-8, beamline: BL19B2) under the following conditions. Furthermore, Rietveld analysis was performed using the obtained XRD results. Through this process, the crystalline phases of the electrolyte matrix were identified, and the mass proportions of each crystalline phase were calculated. Additionally, the Zn mole fraction (ratio to Ce) was calculated based on the information from the Rietveld analysis.

[0100] X-ray diffraction equipment: High-throughput powder X-ray diffractometer

[0101] X-ray wavelength: 0.7 Å

[0102] Measurement range: 2.1°~84.8°

[0103] Step interval: 0.005°

[0104] Crystal phase analysis software: PDXL (manufactured by Rigaku Corporation)

[0105] Structural analysis software: RIETAN-FP (peak shape function: extended pseudo-Voigt function)

[0106] In this experimental example, XRD measurements were performed using a synchrotron radiation apparatus, but XRD measurements can also be performed using experimental equipment. In this case, Rigaku's "RINT2000" or "SmartLab" powder X-ray diffraction apparatus can be used. Furthermore, the measurement conditions can be set as follows: X-ray source: Cu tube bulb, tube voltage: 40 kV, tube current: 30 mA, measurement range: 10°–90°, step interval: 0.01°, etc.

[0107] Figure 5 The crystal phase identification results of the electrolyte host layer are shown. Additionally, in Figure 5 The results for samples 2, 4, 6, and 1C are shown in the table below, as representative examples. Figure 5 (See also Table 1 below) as shown, the use in Ce 0.9 Gd 0.1 O 1.95 The electrolyte host layer of the electrochemical cells of samples 2, 4, and 6, which contain ZnO-added raw materials, has a composite oxide phase. This composite oxide phase comprises: a fluorite structure and Ce... 0.9 Gd 0.1 O 1.95 The first crystalline phase is represented by (ZnO)(CeO). 1.695 )0.5625 The second crystalline phase is indicated. Table 1 summarizes the Zn molar fraction (ratio relative to Ce) of the composite oxide phase in the electrolyte host layer. On the other hand, it was confirmed that the use of a phase not in Ce... 0.9 Gd 0.1 O 1.95 The electrolyte host layer of a 1C electrochemical cell containing ZnO-added raw materials did not form (ZnO)(CeO). 1.695 ) 0.5625 The second crystalline phase is represented by Ce. 0.9 Gd 0.1 O 1.95 It is a single phase and does not have a complex oxide phase.

[0108] In addition, Figure 5 In this example, results for samples 2, 4, 6, and 1C are shown as representative samples, but the same results were obtained for samples 1, 3, and 5. Furthermore, in this experimental example, Ce was used to form the electrolyte substrate layer. 0.9 Gd 0.1 O 1.95 Powder, but based on the above results, if Ce is used... 1-x (RE) x O 2-x / 2 (Where x is between 0.05 and 0.2, and RE element is at least one of Gd and Sm) powder, a composite oxide phase containing a first crystalline phase will be generated, which has a fluorite structure and is dominated by Ce. 1-x (RE) x O 2-x / 2 (Where x is 0.05 to 0.2, and RE element is at least one of Gd and Sm). Furthermore, in this experimental example, as the second crystalline phase in the composite oxide phase, (ZnO)(CeO) is generated. 1.695 ) 0.5625 The second crystalline phase is represented by (ZnO)(CeO), but by changing the amount of Zn source such as ZnO added, the firing temperature, and the initial state of Zn source such as ZnO, other phases with the crystalline structure (ZnO)(CeO) can be generated. 2-δ ) y The second crystalline phase is represented by δ > 0 and y = 0.15 to 0.7.

[0109] <Coefficient of linear expansion of the electrolyte bulk layer>

[0110] The slurry prepared during the fabrication of the electrolyte substrate sheet is dried, and the resulting powder is pressed into a molded body. Next, the molded body is fired at the same specified firing temperature and time as that used in the fabrication of an electrochemical cell, thereby producing an electrolyte substrate sample. Then, a strip sample measuring 4 mm wide × 2 mm high × 10 mm long is collected from the electrolyte substrate sample by grinding. Next, using a DIL402 Expedis Select & Supreme thermal expansion apparatus (manufactured by Netzsch), the temperature is increased from room temperature to 800°C while 4% by volume of hydrogen-Ar gas is flowing through the strip sample. The relationship between temperature and the linear expansion coefficient of the electrolyte substrate is measured, and the linear expansion coefficient of the electrolyte substrate at 650°C is determined.

[0111] <Oxygen ion conductivity of the electrolyte host layer>

[0112] The slurry prepared during the fabrication of the electrolyte substrate sheet was dried, and the resulting powder was pressed into a molded body. Next, the molded body was fired at the same specified firing temperature and time as that used in the fabrication of an electrochemical cell, thereby producing an electrolyte substrate sample. Then, the surface of the electrolyte substrate sample was ground, and Au was sputtered on both sides to form a pair of electrodes. Impedance measurements were then performed on this electrolyte substrate sample using an E4990A impedance analyzer (manufactured by Keysight Corporation), a high-temperature, high-frequency corresponding sample rod HT-Z2-HF-ROD (manufactured by Toyo Teknica Corporation), and an HT-Z2-HF type high-frequency corresponding heating furnace system (manufactured by Toyo Teknica Corporation). The impedance measurements were performed every 50°C between 450°C and 700°C. The obtained data were analyzed using Z-View, and the oxygen ion conductivity at 650°C was calculated by combining the electrode area and the thickness of the electrolyte substrate sample.

[0113] <Cracking during operation>

[0114] Glass rings were placed on both sides of the electrochemical cell and melted at high temperature to form a gas-sealed structure. Next, the fuel electrode layer and fuel diffusion layer underwent reduction treatment. Then, using an SOFC fuel cell evaluation device (manufactured by Nishiyama Corporation), an electrolysis test (operating temperature: 650°C) was conducted with humidified N2 (50ml) and H2 (50ml) introduced into the fuel electrode layer at 80°C, and air (100ml) introduced into the air electrode layer, and the IV characteristics were measured. At this time, with the electrolyte bulk layer cracked, the open-circuit voltage (OCV) deviated significantly from the theoretical value. Furthermore, H2 reacted with O2 and burned, causing the thermocouple installed near the cell to detect a temperature rise. Essentially, these conditions were used to determine whether there was cracking in the electrolyte bulk layer during operation. The above evaluation was performed three times at each level. The results are recorded in Table 1 below using the notation X / 3 (X=0, no cracking occurred in any of the three tests; X=1, cracking occurred once in the three tests; X=2, cracking occurred twice in the three tests; X=3, cracking occurred three times in the three tests). Furthermore, as a precaution, the electrolyte substrate was observed using SEM to confirm the presence of any cracks that would occur during operation. Additionally, the current density required to scan up to 1.3V was determined as needed.

[0115] Table 1 summarizes the details and evaluation results of Experiment Example 1 above. Furthermore, Figure 6 The relationship between the Zn mole fraction (ratio to Ce) in the composite oxide phase and the linear expansion coefficient of the electrolyte bulk layer is shown. Figure 7 The relationship between the Zn molar fraction (ratio to Ce) in the composite oxide phase and the oxygen ion conductivity of the electrolyte host layer is shown.

[0116] Table 1

[0117] According to Table 1, Figure 6 , Figure 7 The following can be observed. In sample 1C, the electrolyte bulk layer in contact with the fuel electrode layer does not contain oxides containing Zn and Ce, i.e., (ZnO)(CeO). 2-δ ) y The second crystalline phase is represented. Therefore, when sample 1C is in operation, under conditions where the electrolyte substrate is exposed to high temperature and a reducing atmosphere, it cannot reduce the reducing expansion of the electrolyte substrate and fails to suppress the generation of cracks in the electrolyte substrate during operation.

[0118] In contrast, in samples 1 to 6, the electrolyte substrate layer in contact with the fuel electrode layer has a composite oxide phase, which includes: a fluorite structure and Ce 1-x (RE) xO 2-x / 2 (where x is 0.05 to 0.2, and RE element is at least one of Gd and Sm) represents the first crystalline phase; and oxides containing Zn and Ce, namely (ZnO) and (CeO) 2-δ ) y The second crystal phase (where δ > 0 and y is 0.15 or greater than 0.7) represents the second crystal phase. Therefore, it has been confirmed that samples 1 to 6, when in operation, can reduce the reducing expansion of the electrolyte substrate layer and suppress the generation of cracks in the electrolyte substrate layer during operation, even when the electrolyte substrate layer is exposed to high temperature and a reducing atmosphere.

[0119] It is speculated that the reduction expansion of the electrolyte bulk layer is reduced for the following reasons: Cerium oxide-based electrolyte materials, when exposed to low oxygen partial pressure (low P), exhibit reduced reductive expansion. O2 At high temperatures, oxygen atoms detach. This is accompanied by the formation of CeO₂. 4+ →Ce 3+ The change in price. Ce 4+ The ionic radius of Ce is 0.97 Å. 3+ The ionic radius is 1.14 Å. The aforementioned valence change increases the ionic radius, resulting in lattice expansion. It can be considered that exposure to low P... O2 Before entering a high-temperature environment, pre-treat a portion of Ce. 4+ With Ce 3+ The state of ZnO in solid solution can reduce exposure to low P. O2 Ce changes under high temperature conditions 4+ The amount of [amount] is such that, as a result, the reducing expansion of the electrolyte bulk layer can be reduced.

[0120] In addition, according to Figure 6 As shown in Table 1, when the Zn mole fraction (ratio to Ce) is above 1.1 mol%, it can more effectively suppress the reducing expansion of the electrolyte substrate compared to when the Zn mole fraction (ratio to Ce) is less than 1.1 mol%, and can achieve crack avoidance in the electrolyte substrate during operation with a higher probability.

[0121] In addition, according to Figure 7 As shown in Table 1, when the Zn molar fraction (ratio to Ce) is below 4.6 mol%, compared with the case where the Zn molar fraction (ratio to Ce) exceeds 4.6 mol%, it can avoid cracks in the electrolyte host layer during operation and maintain a high oxygen ion conductivity of the electrolyte host layer, which makes it easier to improve the output of the electrochemical cell.

[0122] (Experimental Example 2)

[0123] Similar to the preparation of the electrochemical cell for sample 3 in Experimental Example 1, six electrochemical cells were prepared. Then, in this experimental example, the electrochemical cells prepared above were the same as in Experimental Example 1. Sample 7 operated at 600°C, Sample 8 operated at 650°C, Sample 9 operated at 700°C, Sample 10 operated at 750°C, Sample 11 operated at 755°C, and Sample 12 operated at 760°C. Cracking during operation was confirmed for each sample. Furthermore, the electrolyte substrate layer of the electrochemical cells for Samples 7 to 12 all contained the aforementioned specific composite oxide phase. Table 2 summarizes the results. In addition, similar to Experimental Example 1, the coefficient of linear expansion of the electrolyte substrate layer was measured for the electrochemical cells of Samples 3 and 1C within a temperature range of 400°C to 800°C. Figure 8 The results are shown.

[0124] Table 2

[0125] According to Table 2, Figure 8 It is known that when the operating temperature of an electrochemical battery is below 755℃, the battery can operate within a range where rapid reduction and expansion in the electrolyte bulk layer can be easily suppressed. Therefore, it can be concluded that high output of an electrochemical battery can be easily achieved when the operating temperature is below 755℃.

[0126] (Experimental Example 3)

[0127] An electrochemical cell was fabricated in the same manner as that used for sample 3 in Experimental Example 1. In this experimental example, the electrochemical cell fabricated above was used as the electrochemical cell for sample 13. Furthermore, the electrolyte substrate layer of the electrochemical cell for sample 13 contains the aforementioned specific composite oxide phase, but the fuel electrode layer and fuel diffusion layer do not contain the aforementioned specific composite oxide phase.

[0128] A slurry was prepared by mixing NiO powder (average particle size: 0.5 μm), GDC powder (average particle size: 0.5 μm), ZnO powder (average particle size: 0.1 μm), acrylic resin (pore-forming agent), polyvinyl butyral, isoamyl acetate, and 1-butanol using a ball mill. GDC powder and ZnO powder were weighed and added in a specified molar ratio. The mass ratio of NiO powder to GDC powder was set to 65:35. The slurry was coated onto a resin sheet in a layered manner using a doctor blade. After drying, the resin sheet was peeled off, thus preparing sheets for forming the fuel diffusion layer in samples 14 and 15, respectively.

[0129] A slurry was prepared by mixing NiO powder (average particle size: 0.5 μm), GDC powder (average particle size: 0.5 μm), ZnO powder (average particle size: 0.1 μm), acrylic resin (pore-forming agent), polyvinyl butyral, isoamyl acetate, and 1-butanol using a ball mill. GDC powder and ZnO powder were weighed and added in a predetermined molar ratio. The mass ratio of NiO powder to GDC powder was set to 50:50. Furthermore, the pore-forming dosage in the fuel electrode layer forming sheet was set to a smaller amount compared to the pore-forming dosage in the aforementioned fuel diffusion layer forming sheet. Then, in the same manner as the preparation of the aforementioned fuel diffusion layer forming sheet, fuel electrode layer forming sheets for samples 14 and 15 were prepared, respectively.

[0130] In the fabrication of the electrochemical cell of sample 3 in Experimental Example 1, the electrochemical cell of sample 14 was fabricated in the same manner, except that the sheet for forming the fuel diffusion layer and the sheet for forming the fuel electrode layer of sample 14 were used as described above. Furthermore, the electrolyte body layer, fuel electrode layer, and fuel diffusion layer of the electrochemical cell of sample 14 all contain the aforementioned specific composite oxide phase.

[0131] In the fabrication of the electrochemical cell of sample 3 in Experimental Example 1, the electrochemical cell of sample 15 was fabricated in the same manner, except that the sheet for forming the fuel diffusion layer and the sheet for forming the fuel electrode layer of sample 15 were used as described above. Furthermore, the electrolyte body layer, fuel electrode layer, and fuel diffusion layer of the electrochemical cell of sample 15 all contain the aforementioned specific composite oxide phase.

[0132] For the electrochemical cells of samples 13 to 15, electrolysis tests were conducted in the same manner as in Experimental Example 1 (operating temperature: 650°C), and the current density was measured. Furthermore, no cracking was confirmed during operation in any of the electrochemical cells of samples 13 to 15. Table 3 summarizes the results.

[0133] Table 3

[0134] Table 3 reveals the following: The fuel electrode layer and fuel diffusion layer require electronic conductivity. Cerium oxide-based solid electrolyte materials are reduced to Ce during operation. 4+ →Ce 3+ Since it exhibits electronic conductivity, it can be concluded that setting the molar amount of Zn to a smaller value and making Ce... 4+ Partial reduction can achieve a higher current density.

[0135] This disclosure is not limited to the above-described embodiments and experimental examples, and various modifications can be made without departing from its spirit. Furthermore, the components shown in the above-described embodiments and experimental examples can be arbitrarily combined. That is, although this disclosure is described based on embodiments, it should be understood as not being limited to those embodiments, structures, etc. This disclosure also includes various modifications and equivalent variations. In addition, various combinations and methods, and further combinations and methods including only one element, more elements, or fewer elements, also fall within the scope and concept of this disclosure.

[0136] The features of this disclosure are as follows.

[0137] [1]

[0138] An electrochemical battery, The electrochemical cell (1) sequentially comprises: a fuel electrode layer (2) serving as an electrode to which fuel is supplied; a solid electrolyte layer (3) having oxygen ion conductivity; and an air electrode layer (4) serving as an electrode paired with the fuel electrode layer. The solid electrolyte layer has an electrolyte body layer (31) in contact with the fuel electrode layer. The electrolyte host layer has a composite oxide phase comprising a first crystalline phase and a second crystalline phase, wherein the first crystalline phase has a fluorite structure and is predominantly Ce. 1-x (RE) x O 2-x / 2 (Where x is 0.05 to 0.2, and RE element is at least one of Gd and Sm) represents the second crystal phase as (ZnO)(CeO) 2-δ ) y (where δ > 0 and y is greater than 0.15 and less than 0.7) indicates.

[0139] [2]

[0140] According to the electrochemical cell described in [1], In the composite oxide phase, the molar ratio of Zn to Ce in the first crystalline phase is 1.1 mol% or more.

[0141] [3]

[0142] According to the electrochemical cells described in [1] or [2], In the composite oxide phase, the molar ratio of Zn to Ce in the first crystalline phase is less than 4.6 mol%.

[0143] [4]

[0144] According to any one of the electrochemical cells described in [1] to [3], The operating temperature is below 755℃.

[0145] [5]

[0146] According to any one of the electrochemical cells described in [1] to [4], The fuel electrode layer contains the composite oxide phase.

[0147] [6]

[0148] According to any one of the electrochemical cells described in [1] to [5], A fuel diffusion layer (5) is provided on the side of the fuel electrode layer opposite to the solid electrolyte layer side, which is in contact with the fuel electrode layer. The fuel diffusion layer contains the composite oxide phase.

[0149] [7]

[0150] According to the electrochemical cell described in [5], The ratio of the number of moles of Zn in the composite oxide phase contained in the fuel electrode layer to the number of moles of Ce contained in the first crystalline phase is less than the ratio of the number of moles of Zn in the composite oxide phase contained in the electrolyte host layer to the number of moles of Ce contained in the first crystalline phase.

[0151] [8]

[0152] According to the electrochemical cell described in [6], The ratio of the number of moles of Zn in the composite oxide phase contained in the fuel diffusion layer to the number of moles of Ce contained in the first crystalline phase is less than the ratio of the number of moles of Zn in the composite oxide phase contained in the electrolyte host layer to the number of moles of Ce contained in the first crystalline phase.

[0153] [9]

[0154] According to any one of the electrochemical cells described in [1] to [8], An intermediate layer (6) is provided between the solid electrolyte layer and the air electrode layer. The intermediate layer contains the composite oxide phase.

[0155]

[10]

[0156] According to any one of the electrochemical cells described in [1] to [9], Used as at least one of a single solid oxide fuel cell and a solid oxide electrolyzer.

Claims

1. An electrochemical battery, The electrochemical cell (1) sequentially comprises: a fuel electrode layer (2) serving as an electrode to which fuel is supplied; a solid electrolyte layer (3) having oxygen ion conductivity; and an air electrode layer (4) serving as an electrode paired with the fuel electrode layer. The solid electrolyte layer has an electrolyte body layer (31) in contact with the fuel electrode layer. The electrolyte host layer has a composite oxide phase comprising a first crystalline phase and a second crystalline phase, wherein the first crystalline phase has a fluorite structure and is predominantly Ce. 1-x (RE) x O 2-x / 2 It means that, among them, x is 0.05 to 0.2, RE element is at least one of Gd and Sm, and the second crystal phase is (ZnO)(CeO) 2-δ ) y This indicates that δ > 0 and y is between 0.15 and 0.

7.

2. The electrochemical battery according to claim 1, characterized in that, In the composite oxide phase, the molar ratio of Zn to Ce in the first crystalline phase is 1.1 mol% or more.

3. The electrochemical battery according to claim 1 or 2, characterized in that, In the composite oxide phase, the molar ratio of Zn to Ce in the first crystalline phase is less than 4.6 mol%.

4. The electrochemical battery according to claim 1 or 2, characterized in that, The operating temperature is below 755℃.

5. The electrochemical battery according to claim 1 or 2, characterized in that, The fuel electrode layer contains the composite oxide phase.

6. The electrochemical battery according to claim 1 or 2, characterized in that, A fuel diffusion layer (5) is provided on the side of the fuel electrode layer opposite to the solid electrolyte layer side, which is in contact with the fuel electrode layer. The fuel diffusion layer contains the composite oxide phase.

7. The electrochemical battery according to claim 5, characterized in that, The ratio of the number of moles of Zn in the composite oxide phase contained in the fuel electrode layer to the number of moles of Ce contained in the first crystalline phase is less than the ratio of the number of moles of Zn in the composite oxide phase contained in the electrolyte host layer to the number of moles of Ce contained in the first crystalline phase.

8. The electrochemical battery according to claim 6, characterized in that, The ratio of the number of moles of Zn in the composite oxide phase contained in the fuel diffusion layer to the number of moles of Ce contained in the first crystalline phase is less than the ratio of the number of moles of Zn in the composite oxide phase contained in the electrolyte host layer to the number of moles of Ce contained in the first crystalline phase.

9. The electrochemical battery according to claim 1 or 2, characterized in that, An intermediate layer (6) is provided between the solid electrolyte layer and the air electrode layer. The intermediate layer contains the composite oxide phase.

10. The electrochemical battery according to claim 1 or 2, characterized in that, Used as at least one of a single solid oxide fuel cell and a solid oxide electrolyzer.

Citation Information

Patent Citations

  • Cerium based solid electrolyte and its manufacturing method

    JP2005243473A

  • Oral composition