Non-aqueous electrolyte secondary battery and electronic device
Patent Information
- Application Number
- CN202580003035.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-02-26
- Publication Date
- 2026-11-24
AI Technical Summary
Existing lithium-ion batteries suffer from rapid electrolyte consumption, poor thermal stability, and safety issues due to the easy catalytic decomposition of the electrolyte by the lithium nickel cobalt manganese oxide cathode material during cycling. This also results in short cycle life.
A nickel-cobalt-manganese ternary material with a nickel molar content of ≥50% is used as the positive electrode active material, and combined with an electrolyte containing cyclic esters, linear esters and boron-containing additives. By forming a film of boron atoms on the surface of the positive electrode, the oxidation and decomposition of the electrolyte is slowed down, the lithium plating reaction is inhibited, and the chemical and thermal stability is improved.
It extends the cycle life of lithium-ion batteries, reduces the probability of heat generation due to lithium plating, and improves the safety performance of batteries.
Abstract
Description
Non-aqueous electrolyte secondary batteries and electronic devices Technical Field
[0001] This application relates to the field of electrochemical technology, and in particular to a non-aqueous electrolyte secondary battery and electronic device. Background Technology
[0002] Secondary batteries, such as lithium-ion batteries, are widely used in smartphones, wearable devices, consumer drones, and electric vehicles due to their advantages such as high energy density, long cycle life, and no memory effect. To further improve the energy density of secondary batteries and reduce their production costs, current technologies often use ternary lithium nickel cobalt manganese oxide as the positive electrode active material.
[0003] However, when using ternary nickel-cobalt-manganese lithium oxide as the positive electrode active material for secondary batteries, ternary nickel-cobalt-manganese lithium oxide has limitations due to the Ni content. 3+ / 4+ The eg orbital and O 2- The overlapping of the 2p orbitals makes it easier for oxygen to be released, which can easily catalyze electrolyte decomposition during cycling, accelerating electrolyte consumption and leading to insufficient electrolyte and lithium plating in the later stages of cycling. Lithium plating damages the solid electrolyte interphase (SEI) film, causing the solvent to be reduced in large quantities at the negative electrode, generating gas or heat. Furthermore, the rapid reaction between the deposited lithium and the electrolyte solvent also generates a large amount of heat and gas, ultimately resulting in poor thermal stability of the secondary battery, making it prone to thermal runaway and safety issues, and also contributing to its short cycle life. Therefore, how to achieve a longer cycle life while maintaining safety performance in secondary batteries has become a pressing technical problem for those skilled in the art. Summary of the Invention
[0004] The purpose of this application is to provide a non-aqueous electrolyte secondary battery and electronic device, so that the secondary battery can have a long cycle life while taking into account its safety performance.
[0005] It should be noted that while this application uses lithium-ion batteries as an example of secondary batteries to explain the invention, the secondary batteries in this application are not limited to lithium-ion batteries. The specific technical solution is as follows:
[0006] The first aspect of this application provides a non-aqueous electrolyte secondary battery, which includes a positive electrode and an electrolyte. The positive electrode includes a positive current collector and a positive active material layer disposed on at least one surface of the positive current collector. The positive active material layer includes a positive active material, which is a nickel-cobalt-manganese ternary material. Based on the total molar amount of the three elements, the molar percentage of nickel is ≥50%. The electrolyte includes a cyclic ester, a linear ester, and a boron-containing additive. Based on the mass of the electrolyte, the mass percentages of the cyclic ester (W1%), the linear ester (W2%), and the boron-containing additive (W3%) satisfy the following conditions: 15≤W1≤42, 45≤W2≤72, and 0.001≤W3≤2.8. The non-aqueous electrolyte secondary battery provided in the first aspect of this application utilizes a nickel-cobalt-manganese ternary material with a nickel molar percentage of ≥50% as the positive electrode active material, and an electrolyte containing cyclic esters, linear esters, and boron-containing additives, all within the range specified in this application. This allows the electrolyte and the positive electrode active material to work synergistically. The electron-deficient boron atoms in the boron-containing additive form a film on the surface of the positive electrode, combining with oxygen atoms to reduce the release of lattice oxygen. This slows down the oxidative decomposition of the electrolyte during the charge-discharge cycle of the secondary battery, reducing electrolyte consumption and lowering the probability of lithium plating due to insufficient electrolyte in the later stages of the cycle, thereby extending the cycle life of the secondary battery. The electrolyte of this application exhibits good chemical stability towards lithium, further mitigating the chemical reaction between the electrolyte solvent and metallic lithium after lithium plating, inhibiting heat and gas generation during the secondary battery reaction, improving the thermal stability of the secondary battery, and reducing the probability of safety problems caused by thermal runaway. In this way, the electrolyte and the positive electrode active material work synergistically, which can extend the cycle life of the secondary battery, reduce the probability of heat generation due to lithium plating, and improve the safety performance of the secondary battery. Therefore, the non-aqueous electrolyte secondary battery provided in the first aspect of this application can achieve both a long cycle life and good safety performance.
[0007] In one embodiment of this application, 0.2 ≤ W1 / W2 ≤ 0.7, and / or, 0.25 ≤ (W1 + 100W3) / W2 ≤ 4.1. These settings further improve the cycle life and safety performance of the secondary battery.
[0008] In one embodiment of this application, the positive electrode active material further includes other doping elements, including at least one of Al, Ta, Zr, B, Ti, or Y. Based on the total mass of nickel, cobalt, and manganese, the mass percentage of the other doping elements is z%, 0 ≤ z < 10. Introducing the above-mentioned types and amounts of other doping elements into the positive electrode active material can stabilize the structural stability of the positive electrode material and reduce the release of lattice oxygen.
[0009] In one embodiment of this application, the cyclic ester includes at least one of ethylene carbonate or propylene carbonate; the linear ester includes at least one of dimethyl carbonate, diethyl carbonate, methyl ethyl carbonate, methyl propyl carbonate, methyl formate, ethyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, or propyl propionate; and the boron-containing additive includes at least one of lithium tetrafluoroborate, lithium dioxalate borate, lithium difluorooxalate borate, triethyl borate, or tributyl borate. By selecting the above-mentioned types of cyclic esters, linear esters, and boron-containing additives, the secondary battery can achieve both a long cycle life and good safety performance.
[0010] In one embodiment of this application, the cyclic ester includes ethylene carbonate and propylene carbonate; the mass percentage of ethylene carbonate is W based on the mass of the electrolyte. 11 %, the mass percentage of propylene carbonate is W 12 %, 10≤W 11 ≤35, 0≤W 12 ≤25. Cyclic esters include ethylene carbonate and propylene carbonate, and controlling the mass percentage of ethylene carbonate and propylene carbonate within the above range can further improve the safety performance of secondary batteries while maintaining a longer cycle life.
[0011] In one embodiment of this application, 15 ≤ W 11 ≤25, and / or, 2≤W 12 ≤15. This allows secondary batteries to have a longer cycle life while further improving their safety performance.
[0012] In one embodiment of this application, the electrolyte further includes a sulfur-oxygen double bond compound, which includes at least one selected from 1,3-propanesulfonyl lactone, vinyl sulfate, propenesulfonyl lactone, 3-fluoro-1,3-propanesulfonyl lactone, 1,2-propanesulfonyl lactone, 1,4-butanesulfonyl lactone, 1,2-butanesulfonyl lactone, 1,3-butanesulfonyl lactone, 2,4-butanesulfonyl lactone, or 1,3-pentanesulfonyl lactone. Based on the mass of the electrolyte, the mass percentage of the sulfur-oxygen double bond compound is W4%, where 0.05 ≤ W4 ≤ 5, and W4 + W3 ≤ 6. By introducing the above-mentioned types and amounts of sulfur-oxygen double bond compounds into the electrolyte and controlling the mass percentage of the oxygen double bond compound W4% and the sum of its mass percentage with the boron-containing additive W3% (W4 + W3) within the above-mentioned range, the cycle life of the secondary battery is further extended while maintaining good safety performance.
[0013] In one embodiment of this application, 1 ≤ W4 ≤ 4, and / or 1.5 ≤ W4 + W3 ≤ 5. By controlling the mass percentage of the sulfur-oxygen double bond compound W4%, and / or the sum of the mass percentage of the sulfur-oxygen double bond compound W4% and the mass percentage of the boron-containing additive W3% W4 + W3 within the above range, the cycle life of the secondary battery is further extended while maintaining good safety performance.
[0014] In one embodiment of this application, the electrolyte further includes fluoroethylene carbonate, wherein the mass percentage of fluoroethylene carbonate is W5% based on the mass of the electrolyte, and 0.1 ≤ W5 ≤ 5%. Introducing fluoroethylene carbonate into the electrolyte and controlling its content within the aforementioned range further improves the safety performance of the secondary battery while maintaining a longer cycle life.
[0015] A second aspect of this application provides an electronic device comprising a non-aqueous electrolyte secondary battery as described in any of the foregoing embodiments. Therefore, the electronic device exhibits good performance.
[0016] The beneficial effects of this application are:
[0017] This application provides a non-aqueous electrolyte secondary battery and an electronic device. The non-aqueous electrolyte secondary battery includes a positive electrode and an electrolyte. The positive electrode includes a positive current collector and a positive active material layer disposed on at least one surface of the positive current collector. The positive active material layer includes a positive active material, which is a nickel-cobalt-manganese ternary material. Based on the total molar amount of the three elements, the molar percentage of nickel is ≥50%. The electrolyte includes a cyclic ester, a linear ester, and a boron-containing additive. Based on the mass of the electrolyte, the mass percentages of the cyclic ester (W1%), the linear ester (W2%), and the boron-containing additive (W3%) satisfy the following conditions: 15≤W1≤42, 45≤W2≤72, and 0.001≤W3≤2.8. Through the above configuration, the electrolyte and the positive electrode active material work synergistically. Electron-deficient boron atoms in the boron-containing additive form a film on the surface of the positive electrode, combining with oxygen atoms to reduce the release of lattice oxygen. This slows down the oxidative decomposition of the electrolyte during the charge-discharge cycle of the secondary battery, reducing electrolyte consumption and lowering the probability of lithium plating due to insufficient electrolyte in the later stages of the cycle, thereby extending the cycle life of the secondary battery. The electrolyte of this application exhibits good chemical stability towards lithium, further mitigating the chemical reaction between the electrolyte solvent and metallic lithium after lithium plating, inhibiting heat and gas generation during the secondary battery reaction, improving the thermal stability of the secondary battery, and reducing the probability of safety problems caused by thermal runaway. Thus, the synergistic effect between the electrolyte and the positive electrode active material extends the cycle life of the secondary battery and reduces the probability of heat generation due to lithium plating, improving the safety performance of the secondary battery. Therefore, the non-aqueous electrolyte secondary battery of this application can achieve both a long cycle life and good safety performance. The electronic device of this application has excellent performance characteristics. Detailed Implementation
[0018] To make the objectives, technical solutions, and advantages of this application clearer, the following embodiments are provided to further illustrate this application in detail. Obviously, the described embodiments are merely some embodiments of this application, and not all embodiments. All other embodiments obtained by those skilled in the art based on this application are within the scope of protection of this application.
[0019] It should be noted that, in the specific embodiments of this application, lithium-ion batteries are used as an example of non-aqueous electrolyte secondary batteries to explain this application, but the non-aqueous electrolyte secondary batteries of this application are not limited to lithium-ion batteries.
[0020] The first aspect of this application provides a non-aqueous electrolyte secondary battery, comprising a positive electrode and an electrolyte. The positive electrode includes a positive current collector and a positive active material layer disposed on at least one surface of the positive current collector. The phrase "positive active material layer disposed on at least one surface of the positive current collector" means that the positive active material layer can be disposed on one or both surfaces of the positive current collector, and the "surface" can be a partial or complete area of the surface of the positive current collector. The positive active material layer includes a positive active material, which is a nickel-cobalt-manganese ternary material. Based on the total molar amount of nickel, cobalt, and manganese, the molar percentage of nickel (Ni) element X ≥ 50%, and further, 50% ≤ X ≤ 99%. The electrolyte comprises cyclic esters, linear esters, and boron (B) additives. Based on the mass of the electrolyte, the mass percentages of the cyclic esters (W1%), linear esters (W2%), and boron additives (W3%) satisfy the following relationships: 15 ≤ W1 ≤ 42, 45 ≤ W2 ≤ 72, and 0.001 ≤ W3 ≤ 2.8. In some embodiments, the electrolyte comprises cyclic esters, linear esters, boron additives, and lithium salts.
[0021] For example, the molar percentage X of nickel can be 50%, 52%, 53%, 55%, 57%, 59%, 60%, 62%, 65%, 67%, 70%, 72%, 76%, 77%, 79%, 80%, 82%, 84%, 85%, 86%, 88%, 90%, 91%, 92%, 93%, 94%, 96%, 97%, 99%, or any value between any two of the above ranges. If the molar percentage of nickel is less than 50%, the molar percentage of cobalt and manganese will increase, raising the cost of nickel-cobalt-manganese ternary materials. Furthermore, these materials have lower specific capacity and specific energy. Using nickel-cobalt-manganese ternary materials with a nickel molar percentage of less than 50% as positive electrode active materials reduces the likelihood of improving the energy density of secondary batteries and also increases production costs.
[0022] For example, W1 can be 15, 17, 18, 20, 22, 24, 25, 26, 28, 30, 31, 32, 35, 37, 39, 40, 41.2, 42, or any value between any two of the above ranges. Cyclic esters exhibit good lithium chemical stability. Adding cyclic esters to the electrolyte can slow down the chemical reaction between lithium and metallic lithium after lithium deposition in the secondary battery and suppress heat generation from the reaction. If the mass percentage of cyclic ester W1% is less than 15%, the lithium chemical stability effect of the cyclic ester will be insignificant; if the mass percentage of cyclic ester W1% is greater than 42%, the excessive cyclic ester content will reduce the content of other components in the electrolyte, affecting the performance of the secondary battery. For example, if the lithium salt content in the electrolyte is too low, it will affect the charge-discharge performance of the secondary battery.
[0023] W2 can be 45, 46, 47, 49, 50, 52, 53, 54, 55, 57, 58, 59, 60, 62, 65, 67, 70, 72, or any value within any two of the above ranges. If the mass percentage of linear ester W2% is less than 45%, the electrolyte viscosity will increase, reducing the kinetic performance of the secondary battery and affecting its rate performance. If the mass percentage of linear ester W2% is greater than 72%, the content of linear ester will decrease the content of other components in the electrolyte, affecting the battery's performance. For example, if the lithium salt content in the electrolyte is too low, the charge-discharge performance of the secondary battery will be affected.
[0024] For example, W3 can be 0.001, 0.1, 0.3, 0.5, 0.6, 0.8, 1.0, 1.2, 1.3, 1.5, 1.6, 1.8, 1.9, 2.1, 2.2, 2.5, 2.6, 2.7, 2.8, or any value within any two of the above ranges. Boron atoms in the boron-containing additive form a film on the surface of the positive electrode, which can combine with oxygen atoms, reducing the release of lattice oxygen and thus slowing down the oxidative decomposition of the electrolyte during the charge-discharge cycle of the secondary battery, reducing the probability of lithium plating. If the mass percentage of the boron-containing additive W3% is less than 0.001%, it is too low to exert its function; if the mass percentage of the boron-containing additive W3% is greater than 2.8%, the film-forming resistance is too high, which will affect the cycle performance of the secondary battery.
[0025] The non-aqueous electrolyte secondary battery provided in the first aspect of this application utilizes a nickel-cobalt-manganese ternary material with a nickel molar percentage of ≥50% as the positive electrode active material, and an electrolyte containing cyclic esters, linear esters, and boron-containing additives, all within the scope of this application. This allows the electrolyte and the positive electrode active material to work synergistically. The electron-deficient boron atoms in the boron-containing additive form a film on the surface of the positive electrode, combining with oxygen atoms to reduce the release of lattice oxygen. This slows down the oxidative decomposition of the electrolyte during the charge-discharge cycle of the secondary battery, reducing electrolyte consumption and lowering the probability of lithium plating due to insufficient electrolyte in the later stages of the cycle, thereby extending the cycle life of the secondary battery. The electrolyte exhibits good chemical stability towards lithium, further mitigating the chemical reaction between the electrolyte solvent and metallic lithium after lithium plating, inhibiting heat and gas generation during the secondary battery reaction, improving the thermal stability of the secondary battery, and reducing the probability of safety problems caused by thermal runaway. In this way, the electrolyte and the positive electrode active material work synergistically, which can extend the cycle life of the secondary battery, reduce the probability of heat generation due to lithium plating, and improve the safety performance of the secondary battery. Therefore, the non-aqueous electrolyte secondary battery provided in the first aspect of this application can achieve both a long cycle life and good safety performance.
[0026] This application does not impose any particular restrictions on the type of nickel-cobalt-manganese ternary material. Those skilled in the art can choose according to actual needs, as long as it can achieve the purpose of this application. For example, nickel-cobalt-manganese ternary materials include LiNi. 0.5 Co 0.2 Mn 0.3 O2, LiNi 0.6 Co 0.1 Mn 0.3 O2, LiNi 0.6 Co 0.2 Mn 0.2 O2, LiNi 0.7 Co 0.1 Mn 0.2 O2, LiNi 0.71 Co 0.14 Mn 0.15 O2, LiNi 0.9 Co 0.05 Mn 0.05 O2, LiNi 0.91 Co 0.04 Mn 0.05 O2, LiNi 0.92 Co 0.03 Mn 0.05 O2, LiNi 0.93 Co 0.02 Mn 0.05 O2, LiNi 0.94 Co 0.01 Mn 0.05 O2, LiNi 0.95 Co 0.01 Mn 0.04 O2 or LiNi 0.8 Co 0.1 Mn 0.1 At least one of O2.
[0027] In one embodiment of this application, 0.2 ≤ W1 / W2 ≤ 0.7. For example, the value of W1 / W2 is 0.2, 0.22, 0.25, 0.26, 0.27, 0.29, 0.30, 0.31, 0.33, 0.34, 0.35, 0.37, 0.38, 0.40, 0.42, 0.43, 0.45, 0.46, 0.47, 0.49, 0.50, 0.52, 0.55, 0.57, 0.60, 0.62, 0.65, 0.67, 0.7, or any value between any two of the above ranges. By adjusting the value of W1 / W2 within the above range, the electrolyte exhibits good chemical stability towards lithium, which can further mitigate the chemical reaction between the electrolyte solvent and metallic lithium after lithium plating in the secondary battery, suppress the heat and gas generation of the secondary battery reaction, thereby further improving the cycle life and safety performance of the secondary battery.
[0028] In one embodiment of this application, 0.25 ≤ (W1 + 100W3) / W2 ≤ 4.1. For example, the value of (W1 + 100W3) / W2 is 0.25, 0.5, 0.65, 0.7, 0.8, 0.9, 1.2, 1.5, 1.6, 1.8, 2.0, 2.2, 2.5, 2.6, 2.8, 3.0, 3.2, 3.3, 3.5, 3.7, 4.0, 4.1 or any value between any two of the above ranges. By controlling the value of (W1+100W3) / W2 within the aforementioned range, the cyclic esters, linear esters, and boron-containing additives in the electrolyte work synergistically to give the electrolyte good chemical stability, reduce heat and gas generation during secondary battery reactions, and allow boron atoms in the electrolyte to combine with oxygen atoms, reducing the release of lattice oxygen, slowing down the oxidative decomposition of the electrolyte during secondary battery charge-discharge cycles, reducing the lithium plating rate of the secondary battery, and extending the cycle life of the secondary battery. Therefore, through the above settings, the cycle life and safety performance of the secondary battery can be further improved.
[0029] In one embodiment of this application, the positive electrode active material further includes other doping coating elements, which include at least one of Al, Ta, Zr, B, Ti, or Y. Based on the total mass of nickel, cobalt, and manganese, the mass percentage of the other doping coating elements is z%, 0 ≤ z < 10. The aforementioned "nickel, cobalt, and manganese" refers to nickel, cobalt, and manganese. For example, z can be 0, 0.1, 0.5, 0.6, 0.8, 1.0, 1.3, 1.6, 1.7, 1.8, 2.0, 2.2, 2.6, 2.7, 2.8, 3.0, 3.2, 3.3, 3.5, 3.7, 3.9, 4.0, 4.5, 4.8, 5.1, 5.5, 6.0, 6.7, 7.0, 7.2, 7.8, 8.0, 8.2, 8.5, 8.8, 9.0, 9.1, 9.5, 9.7, 9.9, or any value within any two of the above ranges. Introducing other doping elements of the above types and amounts into the positive electrode active material can further improve the structural stability of the positive electrode active material. Using positive electrode active materials with other doping elements in secondary batteries can improve the cycle life and safety performance of the secondary batteries.
[0030] In one embodiment of this application, the cyclic ester includes at least one of ethylene carbonate or propylene carbonate. The linear ester includes at least one of dimethyl carbonate, diethyl carbonate, methyl ethyl carbonate, methyl propyl carbonate, methyl formate, ethyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, or propyl propionate; preferably, the linear ester includes at least one of diethyl carbonate or methyl ethyl carbonate. The boron-containing additive includes at least one of lithium tetrafluoroborate, lithium dioxalate borate, lithium difluorooxalate borate, triethyl borate, or tributyl borate; preferably, the boron-containing additive includes at least one of lithium tetrafluoroborate, lithium dioxalate borate, or lithium difluorooxalate borate. By selecting the aforementioned types of cyclic esters, linear esters, and boron-containing additives, the electrolyte can possess good chemical stability, reduce heat generation during secondary battery reactions, and allow boron atoms in the electrolyte to combine with oxygen atoms, reducing the release of lattice oxygen, slowing down the oxidative decomposition of the electrolyte during secondary battery charge-discharge cycles, reducing the lithium plating rate of the secondary battery, and extending the cycle life of the secondary battery. Therefore, through the above-mentioned design, the secondary battery can achieve both a long cycle life and good safety performance.
[0031] In one embodiment of this application, the cyclic ester includes ethylene carbonate and propylene carbonate; the mass percentage of ethylene carbonate is W based on the mass of the electrolyte. 11 %, the mass percentage of propylene carbonate is W 12 %, 10≤W 11 ≤35, 0≤W 12 ≤25. For example, W 11It can be 10, 12, 13, 16, 17, 20, 21, 22, 25, 27, 28, 30, 31, 32, 35, or any value between any two of the above ranges. For example, W 12 The values are 0, 1, 2, 5, 7, 9, 10, 12, 13, 15, 17, 18, 20, 22, 25, or any value within any two of the above ranges. Cyclic esters include ethylene carbonate and propylene carbonate, and controlling the mass percentage of ethylene carbonate and propylene carbonate within the above ranges can further improve the chemical stability of cyclic esters for lithium, giving the electrolyte containing the above cyclic esters better chemical stability. This further slows down the chemical reaction between the electrolyte solvent and metallic lithium after lithium deposition in the secondary battery, thereby reducing the heat and gas generation from the reaction in the secondary battery, improving the thermal stability of the secondary battery, and reducing the probability of safety problems caused by thermal runaway. Therefore, the safety performance of the secondary battery can be further improved on the basis of a longer cycle life.
[0032] In one embodiment of this application, 15 ≤ W 11 ≤25. In another embodiment of this application, 2≤W 12 ≤15. In another embodiment of this application, 15≤W 11 ≤25, 2≤W 12 ≤15. For example, W 11 It can be any value between 15, 16, 17, 18, 19, 20, 21, 22, 25, or any two of the above ranges. For example, W 12 The value is 2, 5, 7, 9, 10, 12, 13, 15, or any value within any two of the above ranges. Cyclic esters include ethylene carbonate and propylene carbonate. Controlling the mass percentage of ethylene carbonate and propylene carbonate within the above ranges can further improve the chemical stability of cyclic esters for lithium, resulting in better chemical stability of the electrolyte containing these cyclic esters. This further slows down the chemical reaction between the electrolyte solvent and metallic lithium after lithium deposition in the secondary battery, thereby reducing heat and gas generation during the reaction, improving the thermal stability of the secondary battery, and lowering the probability of safety issues caused by thermal runaway. Therefore, the safety performance of the secondary battery can be further improved while maintaining a longer cycle life.
[0033] In one embodiment of this application, the electrolyte further includes a sulfur-oxygen double bond compound. In some embodiments, the electrolyte comprises a cyclic ester, a linear ester, a boron-containing additive, a sulfur-oxygen double bond compound, and a lithium salt. The sulfur-oxygen double bond compound includes at least one selected from 1,3-propanesulfonyl lactone, vinyl sulfate, propenesulfonyl lactone, 3-fluoro-1,3-propanesulfonyl lactone, 1,2-propanesulfonyl lactone, 1,4-butanesulfonyl lactone, 1,2-butanesulfonyl lactone, 1,3-butanesulfonyl lactone, 2,4-butanesulfonyl lactone, or 1,3-pentanesulfonyl lactone. Based on the mass of the electrolyte, the mass percentage of the sulfur-oxygen double bond compound is W4%, where 0.05 ≤ W4 ≤ 5%, and W4 + W3 ≤ 6%. For example, W4 is 0.05, 0.1, 0.3, 0.6, 0.9, 1, 1.3, 1.8, 2, 2.4, 2.7, 3.1, 3.5, 4.0, 4.2, 4.6, 5, or any value within any two of the above ranges. The value of W4+W3 is 0.05, 0.1, 0.3, 0.6, 0.9, 1, 1.3, 1.8, 2, 2.4, 2.7, 3.1, 3.5, 4.0, 4.2, 4.6, 5, 5.1, 5.3, 5.4, 5.6, 5.8, 6, or any value within any two of the above ranges. Sulfur-oxygen double bond compounds can form a film on the surface of the positive electrode to suppress oxygen release from the positive electrode active material. Introducing the aforementioned types and amounts of sulfur-oxygen double bond compounds into the electrolyte can further suppress oxygen release from the positive electrode active material, thereby reducing electrolyte consumption during secondary battery cycling and extending the cycle life of the secondary battery. By controlling the mass percentage of sulfur-oxygen double bond compounds (W4%) and the sum of W4+W3 (W3% of the boron-containing additive) within the aforementioned range, the sulfur-oxygen double bond compounds and the boron-containing additive work synergistically. The boron atoms introduced by the boron-containing additive combine with oxygen atoms to further reduce the release of lattice oxygen, slowing down the oxidative decomposition of the electrolyte during the secondary battery charge-discharge cycle. This further reduces electrolyte consumption and lowers the probability of lithium plating due to insufficient electrolyte in the later stages of the secondary battery cycle. Thus, the cycle life of the secondary battery can be further extended. Therefore, the cycle life of the secondary battery is further extended while maintaining good safety performance.
[0034] In one embodiment of this application, 1 ≤ W4 ≤ 4. In another embodiment of this application, 1.5 ≤ W4 + W3 ≤ 5. In yet another embodiment of this application, 1 ≤ W4 ≤ 4 and 1.5 ≤ W4 + W3 ≤ 5. For example, W4 is 1, 1.3, 1.5, 1.8, 2, 2.4, 2.6, 2.7, 2.9, 3.1, 3.3, 3.5, 3.7, 4, or any value between any two of the above ranges. The value of W4 + W3 is 1.5, 1.8, 2, 2.4, 2.6, 2.7, 2.9, 3.1, 3.2, 3.5, 3.7, 4.0, 4.2, 4.6, 5, or any value between any two of the above ranges. By controlling the mass percentage of the sulfur-oxygen double bond compound, W4%, and / or by adjusting the sum of W4% of the sulfur-oxygen double bond compound and W3% of the boron-containing additive, W4+W3, within the aforementioned range, oxygen release from the positive electrode surface is suppressed. Furthermore, the combination of boron atoms and oxygen atoms brought about by the boron-containing additive reduces the release of lattice oxygen, further slowing down the oxidative decomposition of the electrolyte during the charge-discharge cycle of the secondary battery. This further reduces electrolyte consumption and lowers the probability of lithium plating due to insufficient electrolyte in the later stages of the cycle. Thus, the cycle life of the secondary battery can be further extended. Therefore, the cycle life of the secondary battery is further extended while maintaining good safety performance.
[0035] In one embodiment of this application, the electrolyte further includes fluoroethylene carbonate, and the mass percentage of fluoroethylene carbonate is W5% based on the mass of the electrolyte, where 0.1 ≤ W5 ≤ 5. For example, W5 is 0.1, 0.5, 0.8, 1, 1.3, 1.5, 1.7, 1.9, 2.1, 2.5, 2.7, 2.9, 3.2, 3.4, 3.6, 3.8, 4.0, 4.2, 4.4, 4.6, 4.8, 5, or any value between any two of the above ranges. Fluoroethylene carbonate can passivate the lithium metal surface, reduce the reactivity of lithium metal, and thus inhibit the reaction between lithium metal and the solvent in the electrolyte. Introducing fluoroethylene carbonate into the electrolyte and controlling its content within the above range is beneficial for further mitigating the chemical reaction between the electrolyte solvent and metallic lithium after lithium plating in the secondary battery, inhibiting heat and gas generation from the secondary battery reaction, improving the thermal stability of the secondary battery, and reducing the probability of safety problems caused by thermal runaway in the secondary battery. This allows secondary batteries to not only have a longer cycle life but also improved safety performance.
[0036] In one embodiment of this application, the electrolyte comprises a cyclic ester, a linear ester, a boron-containing additive, a sulfur-oxygen double bond compound, fluoroethylene carbonate, and a lithium salt. In another embodiment of this application, the electrolyte comprises a cyclic ester, a linear ester, a boron-containing additive, fluoroethylene carbonate, and a lithium salt.
[0037] This application does not impose any particular limitation on the type of lithium salt, as long as it achieves the purpose of this application. For example, lithium salts include, but are not limited to, at least one of lithium hexafluorophosphate, lithium difluorophosphate, lithium tetrafluoroborate, lithium hexafluoroarsenate, lithium perchlorate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, lithium bis(oxalateborate), or lithium di(fluorooxalateborate). This application does not impose any particular limitation on the content of lithium salts, as long as it achieves the purpose of this application. For example, based on the mass of the electrolyte, the mass percentage of lithium salt is 8% to 16%.
[0038] This application does not impose any particular restrictions on the method of controlling the content of other doped and coated elements in the positive electrode active material, as long as the purpose of this application can be achieved. For example, it can be achieved by controlling the raw material ratio, temperature, etc.
[0039] This application does not impose any particular restrictions on the preparation method of positive electrode active materials containing other doped coating elements, as long as the purpose of this application can be achieved. For example, the preparation method of positive electrode active materials containing other doped coating elements includes, but is not limited to, the following steps: (1) preparing a hydroxide precursor containing Ni, Co, and Mn elements by hydrothermal method; (2) thoroughly mixing the prepared hydroxide precursor with a lithium source and a dopant compound, and then sintering at high temperature to obtain a positive electrode active material containing other doped coating elements. This application does not impose any particular restrictions on the type of hydroxide precursor mentioned above, as long as the purpose of this application can be achieved. For example, the hydroxide precursor may include, but is not limited to, Ni. 0.6 Co 0.1 Mn 0.3(OH)2. This application does not impose any particular restrictions on the type of lithium source, as long as it can achieve the purpose of this application. For example, the lithium source may include, but is not limited to, Li2CO3. This application does not impose any particular restrictions on the molar ratio of the hydroxide precursor and the lithium source. Those skilled in the art can select the appropriate ratio based on the chemical formula of the nickel-cobalt-manganese ternary material to be prepared, as long as it can achieve the purpose of this application. This application does not impose any particular restrictions on the amount of dopant compound added. Those skilled in the art can select the appropriate ratio based on the content of other doping and coating elements required, as long as it can achieve the purpose of this application. This application does not impose any particular restrictions on the process parameters of high-temperature sintering in step (2) above, as long as it can achieve the purpose of this application. For example, the high-temperature sintering temperature is 800℃ to 900℃, and the high-temperature sintering time is 10h to 14h. This application does not impose any particular restrictions on the positive electrode current collector, as long as it can achieve the purpose of this application. For example, the positive electrode current collector may contain aluminum foil or aluminum alloy foil, etc. In this application, there are no particular restrictions on the thickness of the positive electrode current collector and the positive electrode active material layer, as long as it can achieve the purpose of this application. For example, the thickness of the positive electrode current collector is 5 μm to 20 μm. The thickness of the single-layer positive electrode active material layer is 30 μm to 120 μm. Optionally, the positive electrode active material layer may also include at least one of a positive electrode conductive agent or a positive electrode binder. This application does not impose any particular limitation on the types of positive electrode conductive agents and positive electrode binders in the positive electrode active material layer, as long as the purpose of this application can be achieved. This application does not impose any particular limitation on the mass ratio of positive electrode active material, positive electrode conductive agent, and positive electrode binder in the positive electrode active material layer. Those skilled in the art can choose according to actual needs, as long as the purpose of this application can be achieved. For example, the mass ratio of positive electrode active material, positive electrode conductive agent, and positive electrode binder in the positive electrode active material layer is (97~97.9):(0.8~1.7):(1.0~2.0).
[0040] In one embodiment of this application, the secondary battery further includes a negative electrode sheet. This application does not impose any particular limitation on the negative electrode sheet, as long as it achieves the purpose of this application. In one embodiment, the negative electrode sheet includes a negative current collector and a negative active material layer. The negative active material layer is disposed on one or both surfaces of the negative current collector. The aforementioned "surface" can be a portion of the surface of the negative current collector or the entire surface of the negative current collector. This application does not impose any particular limitation on the negative current collector, as long as it achieves the purpose of this application. For example, the negative current collector can include copper foil, copper alloy foil, nickel foil, stainless steel foil, titanium foil, nickel foam, or copper foam, etc. The negative active material layer of this application includes a negative active material. This application does not impose any particular limitation on the type of negative active material, as long as it achieves the purpose of this application. For example, the negative active material can include natural graphite, artificial graphite, mesophase microcarbon spheres (MCMB), hard carbon, soft carbon, silicon, silicon-carbon composites, SiO₂, etc. x(0<x<2), Li-Sn alloy, Li-Sn-O alloy, Sn, SnO, SnO2, lithium titanate Li4Ti5O with spinel structure 12 at least one selected from Li-Al alloy and metallic lithium. In the present application, there are no particular limitations on the thicknesses of the negative electrode current collector and the negative electrode active material layer, as long as the object of the present application can be achieved. For example, the thickness of the negative electrode current collector is 6 μm to 10 μm, and the thickness of the negative electrode active material layer is 30 μm to 130 μm. Optionally, the negative electrode active material layer may further comprise at least one of a negative electrode conductive agent, a thickener, or a negative electrode binder. In the present application, there are no particular limitations on the types of the negative electrode conductive agent, thickener and negative electrode binder in the negative electrode active material layer, as long as the object of the present application can be achieved. In the present application, there are no particular limitations on the mass ratio of the negative electrode active material, the negative electrode conductive agent, the thickener and the negative electrode binder in the negative electrode active material layer, as long as the object of the present application can be achieved. For example, the mass ratio of the negative electrode active material, the negative electrode conductive agent, the thickener and the negative electrode binder in the negative electrode active material layer is (95~98):(0~1.5):(0~3.0):(1.0~2.0).
[0041] In an embodiment of the present application, the secondary battery further comprises a separator disposed between the positive electrode plate and the negative electrode plate. In the present application, there is no particular limitation on the separator, as long as the object of the present application can be achieved. For example, the material of the separator may include, but is not limited to, at least one of polyolefin (PO) based on polyethylene (PE) and polypropylene (PP), polyester (e.g., polyethylene terephthalate (PET) film), cellulose, polyimide (PI), polyamide (PA), spandex, and aramid. The type of the separator may include at least one of a woven film, a nonwoven film, a microporous membrane, a composite membrane, a calendered film, and a spun film. In the present application, there is no particular limitation on the thickness of the separator, as long as the object of the present application can be achieved.
[0042] In an embodiment of the present application, the secondary battery further comprises a packaging bag, and the positive electrode plate, the negative electrode plate, the separator and the electrolyte are accommodated in the packaging bag. In the present application, there is no particular limitation on the type of the packaging bag, as long as the object of the present application can be achieved.
[0043] The secondary battery of the present application is not particularly limited, and may include any device that undergoes an electrochemical reaction. For example, the secondary battery may include, but is not limited to: a lithium metal secondary battery, a lithium ion secondary battery (lithium ion battery), a lithium polymer secondary battery, or a lithium ion polymer secondary battery.
[0044] This application does not impose any particular limitation on the preparation method of the secondary battery. Any preparation method known in the art can be used, as long as it can achieve the purpose of this application. For example, the preparation method of the secondary battery includes, but is not limited to, the following steps: stacking the separator, positive electrode, separator and negative electrode in sequence, and winding, folding or other operations as needed to obtain a wound electrode assembly; placing the electrode assembly in a packaging bag; injecting electrolyte into the packaging bag and sealing it to obtain a secondary battery; or stacking the separator, positive electrode, separator and negative electrode in sequence, and then fixing the four corners of the entire stacked structure to obtain a stacked electrode assembly; placing the electrode assembly in a packaging bag; injecting electrolyte into the packaging bag and sealing it to obtain a secondary battery.
[0045] A second aspect of this application provides an electronic device comprising the secondary battery described in any of the foregoing embodiments. Therefore, the electronic device exhibits good performance.
[0046] The electronic device described in this application is not particularly limited and can be any electronic device known in the prior art. For example, the electronic device may include, but is not limited to: laptop computers, pen input computers, mobile computers, e-book players, portable telephones, portable fax machines, portable copiers, portable printers, stereo headphones, video recorders, LCD TVs, portable cleaners, portable CD players, mini CDs, transceivers, electronic notebooks, calculators, memory cards, portable recorders, radios, backup power supplies, motors, automobiles, motorcycles, electric bicycles, bicycles, lighting fixtures, toys, game consoles, clocks, power tools, flashlights, cameras, household large-capacity batteries, and lithium-ion capacitors.
[0047] Example
[0048] The embodiments and comparative examples provided below illustrate the implementation of this application in more detail. Various tests and evaluations were conducted according to the methods described below.
[0049] Test methods and equipment:
[0050] Testing of elemental content in nickel-cobalt-manganese ternary materials:
[0051] After discharging the lithium-ion battery to 3.0V at 0.5C, the positive electrode sheet is obtained. It is then soaked in high-purity anhydrous DMC for 8 hours and cleaned 3 times. After cleaning 3 times, it is left to stand in a vacuum drying oven for 12 hours. The material of the positive active material layer is scraped off from the positive electrode sheet and then tested by inductively coupled plasma atomic emission spectrometry (ICP) to obtain the content of each element in the nickel-cobalt-manganese ternary material.
[0052] Cycle life testing:
[0053] At 25℃, the lithium-ion battery was charged at a constant current of 1.2C to 4.2V, then charged at a constant voltage of 4.2V to a current of 0.7C, then charged at a constant current of 0.7C to 4.4V, and then charged at a constant voltage of 4.4V to a current of 0.05C. After resting for 5 minutes, it was discharged at a constant current of 0.5C to 3.0V. This was the first cycle, and the discharge capacity was recorded. Multiple cycles were performed following the above process, and the discharge capacity of the lithium-ion battery was measured after each cycle. Using the initial discharge capacity as 100%, the charge-discharge cycles were repeated until the discharge capacity retention rate decreased to 80% of the initial discharge capacity. The number of cycles was recorded as an indicator of the lithium-ion battery's capacity retention rate at room temperature.
[0054] Capacity retention rate = (Discharge capacity at the end of each cycle / Discharge capacity at the beginning of the first cycle) × 100%.
[0055] The cycle life of a lithium-ion battery is characterized by the number of cycles; the more cycles, the longer the cycle life.
[0056] Safety performance testing:
[0057] At 25℃, the lithium-ion battery was charged at a constant current of 1.2C to 4.2V, then charged at a constant voltage of 4.2V to a current of 0.7C, then charged at a constant current of 0.7C to 4.4V, and then charged at a constant voltage of 4.4V to a current of 0.05C. After resting for 5 minutes, it was discharged at a constant current of 0.5C to 3.0V. This was the first cycle, and the discharge capacity was recorded. Multiple cycles were performed following the above process, and the discharge capacity of the lithium-ion battery was measured after each cycle. The initial discharge capacity was taken as 100%, and the charge-discharge cycles were repeated until the discharge capacity retention rate decreased to 20% of the initial discharge capacity, at which point the test was stopped.
[0058] The lithium-ion battery was then charged at a constant current of 1.2C to 4.2V at 25℃, followed by constant voltage charging at 4.2V to a current of 0.7C, then constant current charging at 0.7C to 4.4V, and finally constant voltage charging at 4.4V to a current of 0.05C. The charged lithium-ion battery was then placed in a high-temperature furnace, with a temperature sensing wire attached to the battery body. The furnace was then heated to 200℃ at a rate of 5℃ / min and held at that temperature for 2 hours. The temperature at which the lithium-ion battery experienced a sudden temperature rise (the inflection point) was recorded; this temperature is the failure temperature and serves as an indicator for evaluating the safety performance of the lithium-ion battery.
[0059] Capacity retention rate = (Discharge capacity at the end of each cycle / Discharge capacity at the beginning of the first cycle) × 100%.
[0060] Failure temperature is used to characterize the safety performance of lithium-ion batteries; the higher the failure temperature, the better the safety performance of the lithium-ion battery.
[0061] Example 1-1
[0062] <Preparation of Electrolyte>
[0063] In an argon-atmospheric glove box with a water content of <10 ppm, cyclic esters ethylene carbonate, propylene carbonate, and linear ester diethyl carbonate were mixed to obtain a solvent. Then, a boron-containing additive, lithium tetrafluoroborate, and a lithium salt, LiPF6, were added to the base solvent, and the mixture was stirred until homogeneous to obtain an electrolyte. Based on the mass of the electrolyte, the lithium salt content was 12%, the boron-containing additive content was W3% by mass, and the remainder was the solvent, with the cyclic ester comprising W1% by mass and the linear ester comprising W2% by mass. The mass percentages of the boron additive, cyclic ester, and linear ester are shown in Table 1.
[0064] <Preparation of the positive electrode>
[0065] Nickel-cobalt-manganese ternary material (LiNi) 0.6 Co 0.1 Mn 0.3 O2), positive electrode conductive agent conductive carbon black (Super P), positive electrode binder polyvinylidene fluoride (PVDF, weight average molecular weight 5×10⁻⁶), and positive electrode binder polyvinylidene fluoride (PVDF, weight average molecular weight 5×10⁻⁶). 5 The materials were mixed at a mass ratio of 97:1.4:1.6, with N-methylpyrrolidone (NMP) added as a solvent. The mixture was stirred under vacuum until a homogeneous positive electrode slurry with a solid content of 72 wt% was obtained. The positive electrode slurry was uniformly coated onto one surface of a 6 μm thick aluminum foil used as a positive electrode current collector, and dried at 85°C to obtain a positive electrode sheet with a single-sided coating of the positive electrode active material layer. The above steps were then repeated on the other surface of the aluminum foil to obtain a positive electrode sheet with a double-sided coating of the positive electrode active material layer. After cold pressing and slitting, positive electrode sheets with dimensions of 74 mm × 867 mm were obtained for later use.
[0066] <Preparation of Negative Electrode Sheets>
[0067] Artificial graphite as the negative electrode active material and styrene-butadiene rubber (SBR) as the negative electrode binder (weight average molecular weight 5×10⁻⁶) are used. 6 Thickener sodium carboxymethyl cellulose was mixed at a mass ratio of 95:2:3, deionized water was added, and the mixture was stirred evenly under vacuum to obtain a negative electrode slurry with a solid content of 75 wt%. The negative electrode slurry was uniformly coated onto one surface of a 5 μm thick copper foil current collector, and the copper foil was dried at 85°C for 4 hours to obtain a negative electrode sheet with a single-sided coating of negative electrode active material. The above steps were repeated on the other surface of the copper foil to obtain a negative electrode sheet with a double-sided coating of negative electrode active material. After cold pressing, cutting, and slitting, a negative electrode sheet with a size of 76.6 mm × 875 mm was obtained.
[0068] <Preparation of the diaphragm>
[0069] The adhesive PVDF (weight average molecular weight of 5×10) 5 Inorganic alumina particles were mixed at a mass ratio of 1:2, and NMP was added as a solvent to prepare an inorganic layer slurry with a solid content of 12 wt%. The slurry was stirred evenly and then uniformly coated onto one surface of a 5 μm thick polyethylene substrate. The substrate was then dried at 85°C for 4 hours to obtain a diaphragm with a single-sided inorganic layer coating thickness of 2 μm. PVDF was then added to NMP solvent and stirred evenly to prepare a polymer layer slurry with a solid content of 25 wt%. This polymer layer slurry was then uniformly coated onto the surface of the inorganic layer, with a surface density of 0.15 mg / cm³. 2 Then, it is dried at 85℃ for 4 hours. Finally, a polymer layer slurry is uniformly coated on the other surface of the polyethylene substrate. The areal density of the polymer layer slurry is 0.15 mg / cm³. 2 Then, it is dried at 85°C for 4 hours to obtain a diaphragm with an inorganic layer and a polymer layer on one side and only a polymer layer on the other side.
[0070] <Preparation of Lithium-ion Batteries>
[0071] The prepared separator, positive electrode, and negative electrode are stacked in sequence, with the side of the separator coated with the inorganic layer and polymer layer facing the positive electrode, and the side coated only with the polymer layer facing the negative electrode. This places the separator between the positive and negative electrodes to act as a separator. The electrode assembly is then wound to obtain the electrode assembly. The electrode assembly is then placed in an aluminum-plastic film packaging bag and dried in an 85°C vacuum oven for 12 hours to remove moisture. The electrolyte is then injected, and after vacuum sealing, settling, formation, and shaping processes, a lithium-ion battery is obtained.
[0072] Examples 1-2 to Examples 1-15
[0073] Except for adjusting the relevant preparation parameters according to Table 1, the rest is the same as in Example 1-1.
[0074] When the mass percentage of at least one of the cyclic esters, linear esters, or boron-containing additives changes, the lithium salt content remains unchanged, and the sum of the mass percentages of lithium salts, cyclic esters, linear esters, and boron-containing additives is 100%.
[0075] Examples 1-16
[0076] Except for changing the nickel-cobalt-manganese ternary material to LiNi in the <Preparation of Positive Electrode Sheet> 0.5 Co 0.2 Mn 0.3 Except for O2, everything else is the same as in Example 1-1.
[0077] Examples 1-17
[0078] Except for changing the nickel-cobalt-manganese ternary material to LiNi in the <Preparation of Positive Electrode Sheet> 0.7 Co 0.1 Mn 0.2 Except for O2, everything else is the same as in Example 1-1.
[0079] Examples 1-18
[0080] Except for changing the nickel-cobalt-manganese ternary material to LiNi in the <Preparation of Positive Electrode Sheet> 0.9 Co 0.05 Mn 0.05 Except for O2, everything else is the same as in Example 1-1.
[0081] Examples 2-1 and 2-2
[0082] Except for adjusting the relevant preparation parameters according to Table 2, the rest is the same as in Examples 1-1.
[0083] Examples 2-3 and 2-4
[0084] Except for adjusting the mass percentage of boron-containing additives to 0.7% and the mass percentage of linear esters to 59.3% in the <Preparation of Electrolyte> section, and adjusting the types of boron-containing additives according to Table 2, the rest is the same as in Examples 1-1.
[0085] Example 3-1
[0086] <Preparation of Positive Electrode Active Materials>
[0087] According to the chemical formula LiNi 0.7 Co 0.1 Mn 0.2 O2 will react with the hydroxide precursor Ni 0.7 Co 0.1 Mn 0.2 After thoroughly mixing (OH)₂ and Li₂CO₃ (Li:transition metal molar ratio of 1.05, transition metals being Ni, Co, and Mn), Al₂O₃ is added and mixed evenly to obtain a mixture in which the total mass ratio of Al to Ni, Co, and Mn is 5:100. The resulting mixture is then placed in a tube furnace under a pure oxygen atmosphere at 500°C for 6 hours, heated to 850°C at a rate of 5°C / min and held for 12 hours. After cooling to room temperature, it is removed and ground to obtain LiNi doped with 5% Al. 0.7 Co 0.1 Mn 0.2 O2 powder sample.
[0088] Except for adjusting the type of positive electrode active material to the positive electrode active material prepared above, everything else is the same as in Example 1-1.
[0089] Example 3-2
[0090] <Preparation of Positive Electrode Active Materials>
[0091] According to the chemical formula LiNi 0.7 Co 0.1 Mn 0.2 O2 will react with the hydroxide precursor Ni 0.6 Co 0.1 Mn 0.3 After thoroughly mixing (OH)₂ and Li₂CO₃ (Li:transition metal molar ratio of 1.05, transition metals being Ni, Co, and Mn), ZrO₂ and TiO₂ are added and mixed evenly to obtain a mixture, wherein the total mass ratio of Zr, Ti to Ni, Co, and Mn is 2:100 and 3:100, respectively. The resulting mixture is then placed in a tube furnace under a pure oxygen atmosphere at 500℃ for 6 hours, heated to 850℃ at a rate of 5℃ / min and held for 12 hours, and then cooled to room temperature before being ground to obtain LiNi containing 2% Zr doping and 3% Ti doping. 0.7 Co 0.1 Mn 0.2 O2 powder sample.
[0092] Except for adjusting the type of positive electrode active material to the positive electrode active material prepared above, everything else is the same as in Example 1-1.
[0093] Example 3-3
[0094] <Preparation of Positive Electrode Active Materials>
[0095] According to the chemical formula LiNi 0.7 Co 0.1 Mn 0.2 O2 will react with the hydroxide precursor Ni 0.6 Co 0.1 Mn 0.3 After thoroughly mixing (OH)₂ and Li₂CO₃ (Li:transition metal molar ratio of 1.05, transition metals being Ni, Co, and Mn), Al₂O₃ is added and mixed evenly to obtain a mixture in which the total mass ratio of Al to Ni, Co, and Mn is 1:100. The resulting mixture is then placed in a tube furnace under a pure oxygen atmosphere at 500°C for 6 hours, heated to 850°C at a rate of 5°C / min and held for 12 hours. After cooling to room temperature, it is removed and ground to obtain LiNi doped with 1% Al. 0.7 Co 0.1 Mn 0.2 O2 powder sample.
[0096] Except for adjusting the type of positive electrode active material to the positive electrode active material prepared above, everything else is the same as in Example 1-1.
[0097] Examples 3-4
[0098] <Preparation of Positive Electrode Active Materials>
[0099] According to the chemical formula LiNi 0.7 Co 0.1 Mn 0.2 O2 will react with the hydroxide precursor Ni 0.6 Co 0.1 Mn 0.3 After thoroughly mixing (OH)₂ and Li₂CO₃ (Li:transition metal molar ratio of 1.05, transition metals being Ni, Co, and Mn), Al₂O₃ is added and mixed evenly to obtain a mixture in which the total mass ratio of Al to Ni, Co, and Mn is 9:100. The resulting mixture is then placed in a tube furnace under a pure oxygen atmosphere at 500°C for 6 hours, heated to 850°C at a rate of 5°C / min and held for 12 hours. After cooling to room temperature, it is removed and ground to obtain LiNi doped with 9% Al. 0.7 Co 0.1 Mn 0.2 O2 powder sample.
[0100] Except for adjusting the type of positive electrode active material to the positive electrode active material prepared above, everything else is the same as in Example 1-1.
[0101] Examples 3-5
[0102] <Preparation of Positive Electrode Active Materials>
[0103] According to the chemical formula LiNi 0.7 Co 0.1 Mn 0.2 O2 will react with the hydroxide precursor Ni 0.6 Co 0.1 Mn 0.3 After thoroughly mixing (OH)₂ and Li₂CO₃ (Li:transition metal molar ratio of 1.05, transition metals being Ni, Co, and Mn), Al₂O₃ is added and mixed evenly to obtain a mixture in which the total mass ratio of Al to Ni, Co, and Mn is 11:100. The resulting mixture is then placed in a tube furnace under a pure oxygen atmosphere at 500°C for 6 hours, heated to 850°C at a rate of 5°C / min and held for 12 hours. After cooling to room temperature, it is removed and ground to obtain LiNi doped with 11% Al. 0.7 Co 0.1 Mn 0.2 O2 powder sample.
[0104] Except for adjusting the type of positive electrode active material to the positive electrode active material prepared above, everything else is the same as in Example 1-1.
[0105] Examples 4-1 to 4-11
[0106] Except for the further introduction of sulfur-oxygen double bond compounds into the electrolyte and the adjustment of the relevant preparation parameters according to Table 4, the rest is the same as in Examples 1-1.
[0107] Among them, when the mass percentage of sulfur-oxygen double bond compounds changes, the mass percentage of linear esters changes accordingly, while the mass percentages of cyclic esters, boron-containing additives, and lithium salts remain unchanged. The sum of the mass percentages of sulfur-oxygen double bond compounds, lithium salts, cyclic esters, linear esters, and boron-containing additives is 100%.
[0108] Examples 5-1 to 5-4
[0109] Except for the further introduction of fluoroethylene carbonate into the electrolyte and the adjustment of the relevant preparation parameters according to Table 5, the rest is the same as in Examples 4-4.
[0110] Among them, when the mass percentage of fluoroethylene carbonate changes, the mass percentage of linear esters changes accordingly, while the mass percentages of sulfur-oxygen double bond compounds, cyclic esters, boron-containing additives, and lithium salts remain unchanged. The sum of the mass percentages of fluoroethylene carbonate, sulfur-oxygen double bond compounds, lithium salt cyclic esters, linear esters, and boron-containing additives is 100%.
[0111] Examples 5-5 to 5-8
[0112] Except for the further introduction of fluoroethylene carbonate into the electrolyte and the adjustment of the relevant preparation parameters according to Table 5, the rest is the same as in Example 1-1.
[0113] When the mass percentage of fluoroethylene carbonate changes, the mass percentage of linear esters changes accordingly, while the mass percentages of cyclic esters, boron-containing additives, and lithium salts remain unchanged. The sum of the mass percentages of fluoroethylene carbonate, lithium salt cyclic esters, linear esters, and boron-containing additives is 100%.
[0114] Comparative Examples 1 to 4
[0115] Except for adjusting the relevant preparation parameters according to Table 1, the rest is the same as in Example 1-1.
[0116] When the mass percentage of at least one of the cyclic esters, linear esters, or boron-containing additives changes, the lithium salt content remains unchanged, and the sum of the mass percentages of lithium salts, cyclic esters, linear esters, and boron-containing additives is 100%.
[0117] The preparation and performance parameters of each embodiment and comparative example are shown in Tables 1 to 5.
[0118] Table 1
[0119] As can be seen from Examples 1-1 to 1-18 and Comparative Examples 1 to 4, the secondary batteries of this application, by controlling the molar percentage content of nickel in the positive electrode active material to be ≥50% and the mass percentage content of cyclic esters, linear esters, and boron-containing additives in the electrolyte to be within the range of this application, achieve a higher number of cycle cycles and a higher hot box pass rate at a capacity retention rate of 80%, indicating that the secondary batteries can maintain a long cycle life while also ensuring safety performance. In contrast, the secondary batteries of the comparative examples, where the molar percentage content of nickel in the positive electrode active material is ≥50% or at least one of the contents of cyclic esters, linear esters, and boron-containing additives in the electrolyte is not within the range of this application, exhibit fewer cycle cycles and a lower hot box pass rate at a capacity retention rate of 80%, indicating that the comparative secondary batteries have a shorter cycle life and poorer safety performance.
[0120] The mass percentage (W1%) of cyclic esters typically affects the cycle life and safety performance of secondary batteries. As can be seen from Examples 1-1 to 1-4, Comparative Example 1, and Comparative Example 2, secondary batteries using cyclic esters with a mass percentage (W1%) within the scope of this application exhibit a higher number of cycle cycles and a higher hot box pass rate at 80% capacity retention, indicating that the secondary batteries have a longer cycle life and better safety performance.
[0121] The mass percentage (W2%) of linear esters typically affects the cycle life and safety performance of secondary batteries. As can be seen from Examples 1-1 to 1-6, Comparative Example 1, and Comparative Example 2, secondary batteries using linear esters with a mass percentage (W2%) within the scope of this application exhibit a higher number of cycle cycles and a higher hot box pass rate at 80% capacity retention, indicating that the secondary batteries have a longer cycle life and better safety performance.
[0122] The mass percentage (W3%) of boron-containing additives typically affects the cycle life and safety performance of secondary batteries. As can be seen from Examples 1-1, 1-7, and 1-8, and Comparative Examples 3 and 4, secondary batteries using boron-containing additives with a mass percentage (W3%) within the scope of this application exhibit a higher number of cycle cycles and a higher hot box pass rate at 80% capacity retention, indicating that the secondary batteries have a longer cycle life and better safety performance.
[0123] The value of W1 / W2 typically affects the cycle life and safety performance of secondary batteries. As can be seen from Examples 1-1 to 1-6, secondary batteries with W1 / W2 values selected within the scope of this application exhibit a higher number of cycle cycles and a higher hot box pass rate when the capacity retention rate is 80%, indicating that the secondary batteries have a longer cycle life and better safety performance.
[0124] The value of (W1+100W3) / W2 typically affects the cycle life and safety performance of secondary batteries. As can be seen from Examples 1-1 to 1-8, secondary batteries with a (W1+100W3) / W2 value within the scope of this application exhibit a higher number of cycle cycles and a higher hot box pass rate when the capacity retention rate is 80%, indicating that the secondary batteries have a longer cycle life and better safety performance.
[0125] When cyclic esters include ethylene carbonate and propylene carbonate, the mass percentage W of ethylene carbonate is... 11 % and mass percentage of propylene carbonate W 12 The percentage typically affects the cycle life and safety performance of secondary batteries. As can be seen from Examples 1-1, 1-9 to 1-15, the selected ethylene carbonate mass percentage W... 11 % and mass percentage of propylene carbonate W 12 The secondary batteries within the scope of this application have a high number of cycle cycles and a high hot box pass rate when the capacity retention rate is 80%, indicating that the secondary batteries have a long cycle life and good safety performance.
[0126] The type of cyclic ester typically affects the cycle life and safety performance of secondary batteries. As can be seen from Examples 1-9 to Examples 1-15, secondary batteries using cyclic esters within the scope of this application exhibit a higher number of cycle cycles and a higher hot box pass rate at a capacity retention rate of 80%, indicating that the secondary batteries have a longer cycle life and better safety performance.
[0127] The molar percentage of nickel in the positive electrode active material typically affects the cycle life and safety performance of secondary batteries. As can be seen from Examples 1-1, 1-16 to 1-18, secondary batteries using a nickel molar percentage in the positive electrode active material within the scope of this application exhibit a higher number of cycle cycles and a higher hot box pass rate at a capacity retention rate of 80%, indicating that the secondary batteries have a longer cycle life and better safety performance.
[0128] Table 2
[0129] The type of linear ester typically affects the cycle life and safety performance of secondary batteries. As can be seen from Examples 1-1, 2-1, and 2-2, secondary batteries using linear esters within the scope of this application exhibit a higher number of cycle cycles and a higher hot box pass rate at 80% capacity retention, indicating that the secondary batteries have a longer cycle life and better safety performance.
[0130] The type of boron-containing additives typically affects the cycle life and safety performance of secondary batteries. As can be seen from Examples 1-1, 2-3, and 2-4, secondary batteries using boron-containing additives within the scope of this application exhibit a higher number of cycle cycles and a higher hot box pass rate at 80% capacity retention, indicating that the secondary batteries have a longer cycle life and better safety performance.
[0131] Table 3
[0132] When the positive electrode active material includes other doped coating elements, the type and content of these other doped coating elements typically affect the cycle life and safety performance of the secondary battery. As can be seen from Examples 3-1 to 3-5, secondary batteries using other doped coating elements within the scope of this application exhibit a higher number of cycle cycles and a higher hot box pass rate at a capacity retention rate of 80%, indicating that the secondary batteries have a longer cycle life and better safety performance.
[0133] Table 4
[0134] Note: In Table 4, "\" indicates that there is no corresponding parameter.
[0135] When sulfur-oxygen double bond compounds are further introduced into the electrolyte, the mass percentage of the sulfur-oxygen double bond compound W4% and the sum of its mass percentage and the boron-containing additive W3% (W4+W3) typically affect the cycle life and safety performance of the secondary battery. As can be seen from Examples 1-1, 4-1 to 4-9, the secondary battery within the scope of this application, using the mass percentage of the sulfur-oxygen double bond compound W4% and the sum of its mass percentage and the boron-containing additive W3% (W4+W3), exhibits a higher number of cycle cycles and a higher hot box pass rate at 80% capacity retention, indicating a longer cycle life and better safety performance.
[0136] When sulfur-oxygen double bond compounds are further introduced into the electrolyte, the type of sulfur-oxygen double bond compound usually affects the cycle life and safety performance of the secondary battery. As can be seen from Examples 1-1, 4-10, and 4-11, the secondary batteries within the scope of this application that use sulfur-oxygen double bond compounds exhibit a higher number of cycle cycles and a higher hot box pass rate at 80% capacity retention, indicating that the secondary batteries have a longer cycle life and better safety performance.
[0137] Table 5
[0138] Note: In Table 5, "\" indicates that there is no corresponding parameter.
[0139] When fluoroethylene carbonate is further introduced into the electrolyte, the mass percentage W5% of fluoroethylene carbonate typically affects the cycle life and safety performance of the secondary battery. As can be seen from Examples 1-1, 4-1, 5-1 to 5-8, the secondary battery using fluoroethylene carbonate with a mass percentage W5% within the scope of this application exhibits a higher number of cycle cycles and a higher hot box pass rate at a capacity retention rate of 80%, indicating that the secondary battery has a longer cycle life and better safety performance.
[0140] It should be noted that, in this document, the terms “comprising,” “including,” or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, or article that comprises a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such a process, method, or article.
[0141] The various embodiments in this specification are described in a related manner. The same or similar parts between the various embodiments can be referred to each other. Each embodiment focuses on describing the differences from other embodiments.
[0142] The above description is only a preferred embodiment of this application and is not intended to limit this application. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of this application should be included within the scope of protection of this application.
Claims
1. A non-aqueous electrolyte secondary battery, comprising a positive electrode sheet and an electrolyte, wherein the positive electrode sheet comprises a positive current collector and a positive active material layer disposed on at least one surface of the positive current collector, the positive active material layer comprises a positive active material, wherein the positive active material is a nickel-cobalt-manganese ternary material, and based on the total molar amount of the three elements nickel, cobalt, and manganese, the molar percentage content of nickel is ≥50%; The electrolyte comprises cyclic esters, linear esters, and boron-containing additives. Based on the mass of the electrolyte, the mass percentages of the cyclic esters (W1%), linear esters (W2%), and boron-containing additives (W3%) satisfy the following relationships: 15 ≤ W1 ≤ 42, 45 ≤ W2 ≤ 72, and 0.001 ≤ W3 ≤ 2.
8.
2. The non-aqueous electrolyte secondary battery according to claim 1, wherein, 0.2≤W1 / W2≤0.7, and / or, 0.25≤(W1+100W3) / W2≤4.
1.
3. The non-aqueous electrolyte secondary battery according to claim 2, wherein, The positive electrode active material also includes other doping coating elements, which include at least one of Al, Ta, Zr, B, Ti or Y. Based on the total mass of the three elements nickel, cobalt and manganese, the mass percentage of the other doping coating elements is z%, 0≤z<10.
4. The non-aqueous electrolyte secondary battery according to claim 1, wherein, The cyclic ester includes at least one of ethylene carbonate or propylene carbonate; The linear esters include at least one of dimethyl carbonate, diethyl carbonate, methyl ethyl carbonate, methyl propyl carbonate, methyl formate, ethyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, or propyl propionate. The boron-containing additive includes at least one of lithium tetrafluoroborate, lithium dioxalate borate, lithium difluorooxalate borate, triethyl borate, or tributyl borate.
5. The non-aqueous electrolyte secondary battery according to any one of claims 1 to 4, wherein, The cyclic esters include ethylene carbonate and propylene carbonate; Based on the mass of the electrolyte, the mass percentage of ethylene carbonate is W. 11 The mass percentage of propylene carbonate is W. 12 %, 10≤W 11 ≤35, 0≤W 12 ≤25.
6. The non-aqueous electrolyte secondary battery according to claim 5, wherein, 15≤W 11 ≤25, and / or, 2≤W 12 ≤15.
7. The non-aqueous electrolyte secondary battery according to claim 1, wherein, The electrolyte further includes a sulfur-oxygen double bond compound, which includes at least one of 1,3-propanesulfonyl lactone, vinyl sulfate, propenesulfonyl lactone, 3-fluoro-1,3-propanesulfonyl lactone, 1,2-propanesulfonyl lactone, 1,4-butanesulfonyl lactone, 1,2-butanesulfonyl lactone, 1,3-butanesulfonyl lactone, 2,4-butanesulfonyl lactone, or 1,3-pentanesulfonyl lactone. Based on the mass of the electrolyte, the mass percentage of the sulfur-oxygen double bond compound is W4%, where 0.05 ≤ W4 ≤ 5, and W4 + W3 ≤ 6.
8. The non-aqueous electrolyte secondary battery according to claim 7, wherein, 1≤W4≤4, and / or, 1.5≤W4+W3≤5.
9. The non-aqueous electrolyte secondary battery according to claim 1 or 7, wherein, The electrolyte also includes fluoroethylene carbonate, and the mass percentage of fluoroethylene carbonate is W5% based on the mass of the electrolyte, where 0.1 ≤ W5 ≤ 5.