Leather materials, vehicle interior and vehicle
Patent Information
- Application Number
- CN202522599701.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Utility models(China)
- Current Assignee / Owner
- Filing Date
- 2025-12-05
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2035-12-05
Smart Images

Figure CN224952688U_ABST
Abstract
Description
Technical Field
[0001] This utility model belongs to the field of leather material technology, specifically relating to leather materials, vehicle interiors, and vehicles. Background Technology
[0002] Currently, leather materials are widely used in automotive interiors and the clothing industry. The appearance color of leather is something people can immediately see, and as people's living standards continue to improve, their demands for the aesthetic appeal of leather colors are also increasing. Leather with changeable appearance color has attracted considerable attention. Some studies have introduced photosensitive and temperature-sensitive units into the leather manufacturing process, using light or temperature as a control method to switch the leather's appearance color. However, using light and temperature as control methods is susceptible to interference from the external environment (temperature or light), making active control impossible. Electrical control has the advantage of precise control (time, location), belonging to active control methods. However, current color-changing leather relying on electrical control requires relatively high voltages (e.g., 100V~250V), posing a high safety risk for human interaction, hindering the application of electrical control in color-changing leather. Utility Model Content
[0003] This invention aims to at least partially solve one of the technical problems in related technologies. To this end, this invention proposes a leather material with actively adjustable color and high safety for human interaction, as well as a vehicle interior and vehicle.
[0004] In a first aspect, this application provides a leather material. According to an embodiment of this application, the leather material includes: a base layer; a first electrode disposed on one side of the base layer; an electrochromic layer disposed on the side of the first electrode away from the base layer, the electrochromic layer comprising electronic ink microcapsules; a second transparent electrode disposed on the side of the electrochromic layer away from the base layer; and a first transparent surface layer disposed on the side of the second transparent electrode away from the base layer. In this leather material, the first transparent surface layer can provide a textured effect, the first and second transparent electrodes provide conductivity, the electrochromic layer provides a color-changing effect under the action of an electric field, and the base layer provides insulation, a tactile feel, and mechanical properties. The electrochromic layer utilizes electronic ink microcapsules. The charged color-changing particles within these microcapsules migrate in different directions after electrophoresis under an electric field, achieving color changes on the leather material surface at low voltages (≤10 V). Specifically, the electronic ink microcapsules can drive charged particles to move in a transparent liquid using an electric field. When an electric field is applied, charged particles of the corresponding polarity migrate to the side of the microcapsule closest to the second transparent electrode, reflecting ambient light to display the corresponding color. After power is off, the charged particles maintain their position and do not change, demonstrating stable color change and achieving bistable display. This results in extremely low power consumption, reducing operating voltage and improving safety. Furthermore, the electronic ink capsules can contain a variety of selectable charged particles, enabling switching between multiple colors and providing excellent color-changing effects.
[0005] According to embodiments of this application, the electronic ink microcapsules satisfy at least one of the following conditions: The average particle size of the electronic ink microcapsules is 5μm~70μm; The electronic ink microcapsules include at least one of the following: microcapsules containing monochromatic particles, microcapsules containing dual-color particles, and microcapsules containing multicolor particles.
[0006] According to embodiments of this application, the microcapsules containing bicolor particles include microcapsules containing charged titanium dioxide and charged carbon black.
[0007] According to embodiments of this application, the leather material satisfies at least one of the following conditions: The first transparent surface layer has a first predetermined pattern; The electrochromic layer has a second predetermined pattern.
[0008] According to embodiments of this application, the leather material satisfies at least one of the following conditions: The thickness of the first electrode is 5μm~25μm; The thickness of the first transparent layer is 20μm~50μm; The thickness of the second transparent electrode is 5μm~25μm; The thickness of the electrochromic layer is 5μm~150μm; The first electrode comprises a conductive polymer, silver nanowires, or carbon nanoparticles; The second transparent electrode comprises a conductive polymer, silver nanowires, or carbon nanoparticles; The first transparent surface layer comprises polyurethane resin or polyvinyl chloride resin.
[0009] According to an embodiment of this application, the leather material further includes an adhesive layer disposed between the electrochromic layer and the first electrode.
[0010] According to embodiments of this application, the adhesive layer satisfies at least one of the following conditions: The thickness of the adhesive layer is 50μm~400μm; The adhesive layer includes natural adhesives, epoxy resin adhesives, polyurethane adhesives, or polyvinyl alcohol adhesives.
[0011] According to an embodiment of this application, the substrate layer includes: a second surface layer disposed on the side of the first electrode away from the electrochromic layer; a foam layer disposed on the side of the second surface layer away from the electrochromic layer; and a base fabric layer disposed on the side of the foam layer away from the electrochromic layer.
[0012] According to embodiments of this application, the leather material satisfies at least one of the following conditions: The thickness of the second surface layer is 20μm~50μm; The thickness of the foamed layer is 100μm~700μm; The thickness of the base fabric layer is 200μm~3000μm; The second surface layer comprises polyurethane resin or polyvinyl chloride resin; The foaming layer includes polyurethane foam; The base fabric layer may include at least one of knitted fabric, woven fabric, nonwoven fabric, and 3D Mesh.
[0013] In another aspect, this application provides a vehicle interior trim. According to an embodiment of this application, the vehicle interior trim includes the leather material described above. Therefore, the vehicle interior trim can actively change color, resulting in a richer and more diverse appearance, while also providing higher safety.
[0014] In another aspect, this application provides a vehicle. According to an embodiment of this application, the vehicle includes the leather material or the vehicle interior described above. Therefore, the vehicle can actively change color, resulting in a richer and more diverse appearance, while also offering higher safety. Attached Figure Description
[0015] Figure 1 This is a schematic diagram of the structure of a leather material according to an embodiment of this application.
[0016] Figure 2 This is a schematic diagram of the structure of a leather material according to another embodiment of this application.
[0017] Figure 3 This is a schematic diagram of the structure of a leather material according to another embodiment of this application.
[0018] Figure label: 10: Base layer; 11: Second surface layer; 12: Foaming layer; 13: Base fabric layer; 21: First electrode; 22: Electrochromic layer; 23: First transparent electrode; 30: First transparent surface layer; 40: Adhesive layer. Detailed Implementation The embodiments of the present invention are described in detail below, examples of which are shown in the accompanying drawings. The embodiments described below with reference to the accompanying drawings are exemplary and intended to explain the present invention, and should not be construed as limiting the present invention.
[0019] This utility model is based on the inventor's discovery and understanding of the following facts and problems: As mentioned earlier, compared to control methods such as light and temperature, electrical control has the advantage of precise control (time and location), belonging to active control methods. Compared to light and temperature, using electricity as a control method can broaden the application scenarios of products. Currently, the electrically controlled active color-changing leather material uses ZnS-based light-emitting units, which belongs to the intrinsic electroluminescence mechanism, meaning that when an external voltage is applied, the electric field strength exceeds 10. 4 At a voltage of V / cm, electrons are accelerated at high speed and gain kinetic energy, colliding with impurity or defect energy levels at the luminescence center. This triggers an electron transition from the excited state to the ground state, releasing a photon and thus producing visible light. Because the band structure and luminescence mechanism of ZnS require electrons to gain sufficient kinetic energy before the collision to overcome the energy barrier inside the material, the voltage required for this material to emit light is as high as 100V~250V.
[0020] In response to the above situation, the inventors of this utility model attempted to develop a leather material that can actively control color change under low pressure. Through research and exploration, the inventors discovered that by using electronic ink microcapsules, and utilizing the principle that charged color-changing particles inside the electronic ink microcapsules migrate in different directions after electrophoresis under the action of an electric field, it is possible to change the surface color of the leather material under low pressure (≤10 V), effectively improving the safety of use.
[0021] In view of the above, in a first aspect, this application provides a leather material. According to an embodiment of this application, referring to... Figure 1The leather material includes: a base layer 10; a first electrode 21 disposed on one side of the base layer 10; an electrochromic layer 22 disposed on the side of the first electrode 21 away from the base layer 10, the electrochromic layer 22 comprising electronic ink microcapsules; a second transparent electrode 23 disposed on the side of the electrochromic layer 22 away from the base layer 10; and a first transparent surface layer 30 disposed on the side of the second transparent electrode 23 away from the base layer 10. In this leather material, the first transparent surface layer can provide a textured effect, the first and second transparent electrodes provide conductivity, the electrochromic layer provides a color-changing effect under the action of an electric field, and the base layer provides insulation, a tactile feel, and mechanical properties. The electrochromic layer utilizes electronic ink microcapsules. The charged color-changing particles within these microcapsules migrate in different directions after electrophoresis under an electric field, achieving color changes on the leather material surface at low voltages (≤10 V). Specifically, the electronic ink microcapsules can drive charged particles to move in a transparent liquid using an electric field. When an electric field is applied, charged particles of the corresponding polarity migrate to the side of the microcapsule closest to the second transparent electrode, reflecting ambient light to display the corresponding color. After power is off, the charged particles maintain their position and do not change, demonstrating stable color change and achieving bistable display. This results in extremely low power consumption, reducing operating voltage and improving safety. Furthermore, the electronic ink capsules can contain a variety of selectable charged particles, enabling switching between multiple colors and providing excellent color-changing effects.
[0022] In this article, electronic ink microcapsules refer to tiny spherical capsules encapsulating charged pigment particles in a transparent insulating liquid. Visual displays can be achieved by controlling the movement of the internal particles through an electric field. Generally, the outer shell of electronic ink microcapsules is a transparent polymer film, providing mechanical protection and electrical insulation. The internal substances include charged pigment particles and a transparent suspension. The charged pigment particles include, but are not limited to, negatively charged white titanium dioxide particles, positively charged black carbon particles, organic pigment particles (azo pigments, phthalocyanine pigments, quinacridones, perylene pigments, etc.), inorganic pigment particles (such as metal oxides, sulfides, etc.), and composite structure particles. The transparent suspension includes, but is not limited to, dielectric liquids (such as paraffin oil), which serve as a medium for particle movement, reducing frictional resistance.
[0023] It is understandable that electronic ink microcapsules containing charged pigment particles of different colors can be selected based on the desired aesthetic effect. For example, charged pigment particles include, but are not limited to, white particles (such as positively charged modified titanium dioxide), black particles (such as negatively charged carbon black), red particles (such as nano-red powder encapsulated in polyethylene film), blue particles (such as lake pigments, phthalocyanine blue), green particles (such as phthalocyanine green G), yellow particles (such as Hansa Yellow 10G), and brown particles (such as azo and heterocyclic organic pigments).
[0024] According to embodiments of this application, the electronic ink microcapsules may include at least one of microcapsules containing monochromatic particles, microcapsules containing dichromatic particles, and microcapsules containing multichromatic particles (i.e., three or more colors). Thus, leather materials can achieve monochromatic, dichromatic, or multichromatic apparent colors, improving the appearance of the leather material.
[0025] According to embodiments of this application, the microcapsules containing dual-color particles include microcapsules containing charged titanium dioxide and charged carbon black. This satisfies color-changing requirements in most cases, and the process is mature and cost-effective.
[0026] According to embodiments of this application, the average particle size of the electronic ink microcapsules is 5μm to 70μm, specifically within the range of 5μm, 10μm, 15μm, 20μm, 25μm, 30μm, 35μm, 40μm, 45μm, 50μm, 55μm, 60μm, 65μm, 70μm, or any two of these ranges. Within this particle size range, higher resolution and better display effects can be achieved, while also being easier to prepare, with a suitable microcapsule wall thickness ratio and superior optical performance.
[0027] According to embodiments of this application, the thickness of the electrochromic layer is 5μm to 150μm, specifically within the range of 5μm, 30μm, 55μm, 80μm, 105μm, 130μm, 150μm, or any two of these ranges. Within this thickness range, a single layer of electronic ink microcapsules can be fully coated, which is beneficial for improving the color-changing effect.
[0028] According to embodiments of this application, in order to achieve more diverse aesthetic effects, the first transparent surface layer has a first predetermined pattern. This allows for personalized display requirements and the achievement of richer aesthetic effects.
[0029] Specifically, there are no particular restrictions on the first predetermined pattern, which can be flexibly selected as needed, such as including but not limited to geometric shapes, animal and plant patterns, landscape patterns, etc. The first predetermined pattern can be formed on the first transparent surface layer in various ways, and this application has no particular restrictions.
[0030] According to an embodiment of this application, the electrochromic layer has a second predetermined pattern. This allows for personalized display requirements and achieves richer aesthetic effects. Furthermore, it can be superimposed with a first predetermined pattern to further enhance the aesthetic effect.
[0031] Specifically, there are no particular restrictions on the second predetermined pattern, which can be flexibly selected as needed, such as including but not limited to geometric shapes, animal and plant patterns, landscape patterns, etc. The second predetermined pattern can be formed on the electrochromic layer in various ways, or the electrochromic layer can be directly prepared into the shape of the second predetermined pattern, for example, an electrochromic layer with the shape of the second predetermined pattern can be prepared by screen printing.
[0032] According to embodiments of this application, the thickness of the first electrode is 5μm to 25μm, specifically within the range of 5μm, 8μm, 10μm, 12μm, 15μm, 18μm, 20μm, or any two of these ranges. Within this thickness range, it exhibits good conductivity while maintaining a relatively thin and light leather material, resulting in better performance.
[0033] According to embodiments of this application, the first electrode comprises a conductive polymer, silver nanowires, or carbon nanoparticles (such as carbon nanotubes, graphene, etc.). These materials exhibit superior conductivity and are easy to fabricate.
[0034] According to embodiments of this application, the thickness of the first transparent layer is 20μm to 50μm, specifically within the range of 20μm, 25μm, 30μm, 35μm, 40μm, 45μm, 50μm, or any two of these ranges. Within this thickness range, it exhibits high transparency, which is beneficial for enhancing the color-changing effect and facilitates the creation of various textures and patterns, thereby enriching the overall appearance.
[0035] According to embodiments of this application, the first transparent surface layer comprises polyurethane resin or polyvinyl chloride resin. This facilitates the creation of a wide variety of textures and patterns, improving the appearance and providing higher transparency for a better visual effect.
[0036] According to embodiments of this application, the thickness of the second transparent electrode is 5μm to 25μm, specifically 5μm, 8μm, 10μm, 12μm, 15μm, 18μm, 20μm, or any combination thereof. Within this thickness range, it exhibits good conductivity while maintaining high transparency, which enhances the appearance and keeps the leather material relatively thin, resulting in better performance.
[0037] According to embodiments of this application, the second transparent electrode comprises a conductive polymer, silver nanowires, or carbon nanoparticles (such as carbon nanotubes, graphene, etc.). Therefore, it possesses high transparency while exhibiting excellent conductivity.
[0038] According to the embodiments of this application, referring to Figure 2 The leather material also includes an adhesive layer 40, which is disposed between the electrochromic layer 22 and the first electrode 21. Thus, by providing the adhesive layer, it serves two purposes: firstly, it acts as a dielectric, preventing the electrochromic layer from being broken down; secondly, it allows the structures on both sides of the adhesive layer to be formed separately during the fabrication process, and then the first electrode and the electrochromic layer are bonded together using the adhesive layer. This avoids damage to the electronic ink microcapsules caused by the high-temperature environment during substrate fabrication, effectively improving product yield and ensuring the color-changing effect.
[0039] According to embodiments of this application, the thickness of the adhesive layer is 50 μm to 400 μm, specifically 50 μm, 100 μm, 150 μm, 200 μm, 250 μm, 300 μm, 350 μm, 400 μm, or any range between two of these. This thickness range provides good dielectric properties, protecting the electrochromic layer and ensuring safe use, without affecting the migration speed of the color-changing particles in the electronic ink microcapsules, thus guaranteeing a fast response time.
[0040] According to embodiments of this application, the adhesive layer comprises a natural adhesive, an epoxy resin adhesive, a polyurethane adhesive, or a polyvinyl alcohol adhesive. Therefore, it provides both good adhesion and good dielectric properties.
[0041] According to the embodiments of this application, referring to Figure 3 The base layer 10 includes: a second surface layer 11 disposed on the side of the first electrode 21 away from the electrochromic layer 22; a foam layer 12 disposed on the side of the second surface layer 11 away from the electrochromic layer 22; and a base fabric layer 13 disposed on the side of the foam layer 12 away from the electrochromic layer 22. Thus, the base layer can meet different functional needs. Specifically, the second surface layer can provide better insulation, the foam layer can impart softness, elasticity, and breathability to the leather material, and the base fabric layer can provide better mechanical properties, thereby further improving the overall performance of the leather material.
[0042] According to embodiments of this application, the thickness of the second surface layer is 20μm to 50μm, specifically 20μm, 25μm, 30μm, 35μm, 40μm, 45μm, 50μm, or any combination thereof. This results in better insulation while allowing for a suitable thickness of the leather material, leading to improved performance.
[0043] According to an embodiment of this application, the second surface layer comprises polyurethane resin or polyvinyl chloride resin.
[0044] According to embodiments of this application, the thickness of the foamed layer is 100μm to 700μm, specifically within the ranges of 100μm, 150μm, 200μm, 250μm, 300μm, 350μm, 400μm, 450μm, 500μm, 550μm, 600μm, 650μm, 700μm, or any two of these ranges. Within the aforementioned thickness range, the leather material can possess suitable softness, elasticity, breathability, sound insulation, and mechanical strength, thereby improving the overall performance of the leather material.
[0045] According to an embodiment of this application, the foaming layer comprises polyurethane foam. Thus, polyurethane foam possesses advantages such as high elasticity and resilience, strong wear and scratch resistance, tear and impact resistance, and a good feel, thereby giving the leather material superior overall performance, good environmental friendliness, and high degree of hand-feel simulation.
[0046] According to embodiments of this application, the thickness of the base fabric layer is 200μm to 3000μm, specifically within the ranges of 200μm, 500μm, 800μm, 1000μm, 1200μm, 1500μm, 1800μm, 2000μm, 2200μm, 2500μm, 2800μm, 3000μm, or any two of these ranges. This thickness range allows the leather material to possess suitable mechanical strength, comfortable feel, and breathability, while also providing good three-dimensionality, appropriate weight and cost, thus improving the overall performance of the leather material.
[0047] According to embodiments of this application, the base fabric layer includes at least one of knitted fabric, woven fabric, nonwoven fabric, and 3D Mesh. As an example, the base fabric layer may include knitted fabric, woven fabric, nonwoven fabric, and 3D Mesh made of polyester (PET) or nylon (PA). Thus, the leather material possesses superior mechanical strength, hand comfort, functional properties, and durability.
[0048] In this article, 3D Mesh (three-dimensional mesh / spacer fabric) is a three-dimensional structure fabric formed through a three-dimensional weaving process, commonly known as extra-thick sandwich mesh or 3D spacer fabric. Its core structure consists of two independent fabric surface layers and intermediate connecting fibers, forming a porous three-dimensional material with thickness-direction support.
[0049] In another aspect, this application provides a method for preparing the aforementioned leather material. According to an embodiment of this application, the method includes: S1. The first transparent surface layer paste is coated on the surface of the first release paper and dried to obtain the first transparent surface layer.
[0050] In some embodiments, polyurethane resin or polyvinyl chloride resin (PVC resin) and solvent can be mixed to prepare the first transparent topcoat slurry. As an example, the raw materials of the first transparent topcoat slurry can be mixed and stirred at 500-1000 rpm for 5-10 min to control the viscosity to 3000-7000 cps.
[0051] As an example, the first transparent topcoat slurry may include 80-120 parts by weight of polyurethane resin, 30-80 parts by weight of solvent, 0-2 parts by weight of wetting agent, 0-1 parts by weight of defoamer, 0-3 parts by weight of thickener, and 0-5 parts by weight of curing agent. The polyurethane resin may be either solvent-based polyurethane or waterborne polyurethane; the solvent-based polyurethane may be one or a mixture of two or more types of polycarbonate, polyether, or polyester. The solvent, wetting agent, defoamer, thickener, and curing agent are not particularly limited in this application and can be flexibly selected according to actual needs.
[0052] In some embodiments, silicone resin, silica, matting resin, etc., may be added to the first transparent surface layer slurry as needed to further improve the feel and gloss of the leather material, and further enhance the overall performance of the leather material.
[0053] In some embodiments, the specific coating and drying steps are not particularly limited and can be selected as needed. As an example, the coating thickness of the first transparent topcoat slurry can be 100 μm to 400 μm, the drying temperature can be 100 to 140 °C, and the drying time can be 10 to 15 min.
[0054] S2. The second transparent electrode paste is coated on the side of the first transparent surface layer away from the first release paper, and then dried to obtain the second transparent electrode.
[0055] In some embodiments, the second transparent electrode paste may be a polyaniline:polystyrene sulfonate solution with a solid content of 1-6 wt%, or a poly(3,4)-poly(2 ... Ethylene dioxythiophene: a polystyrene sulfonate solution, or an aqueous solution of silver nanowires with a concentration of 5-15 mg / mL, an aqueous dispersion of single-walled carbon nanotubes and / or graphene, wherein the solid content of the aqueous dispersion can be 1-6 wt%.
[0056] In some embodiments, the coating thickness of the second transparent electrode paste can be 50 μm to 300 μm; the drying temperature can be 100 to 140 °C, and the drying time can be 10 to 15 min.
[0057] S3. The electrochromic layer paste is coated on the side of the second transparent electrode away from the first release paper, and then dried to obtain the electrochromic layer.
[0058] According to embodiments of this application, the electrochromic layer slurry may include an adhesive and an electronic ink microcapsule dispersion.
[0059] In some embodiments, the adhesive may be one or a combination of natural adhesives, epoxy resin adhesives, polyurethane adhesives, and polyvinyl alcohol adhesives.
[0060] As an example, the electrochromic layer slurry is formed by mixing the above-mentioned adhesive with an electronic ink capsule dispersion, specifically comprising: 80-100 parts by weight of the adhesive and 40-300 parts by weight of the electronic ink capsule dispersion.
[0061] In some embodiments, the preparation method of the electrochromic layer slurry can be as follows: the electronic ink microcapsule dispersion is concentrated by centrifugation to obtain an electronic ink microcapsule concentrate, wherein the centrifugation speed is 500~1000 rpm and the centrifugation time is 10~15 min; then the electronic ink microcapsule concentrate is mixed evenly with the adhesive slurry, wherein the stirring speed is 300~500 rpm and the stirring time is 10~15 min.
[0062] In some embodiments, the electrochromic layer slurry can be vacuum degassed before coating to avoid the negative impact of air bubbles on display performance such as resolution and color uniformity.
[0063] In some embodiments, the coating thickness of the electrochromic layer slurry can be 30 μm to 500 μm; the drying temperature can be 25 to 60 °C, and the drying time can be 0.5 to 24 h.
[0064] S4. Take the second release paper, coat the surface of the second surface layer slurry with the second surface layer slurry, and dry it to obtain the second surface layer.
[0065] As an example, polyurethane resin or polyvinyl chloride resin (PVC resin) can be mixed with a solvent to prepare a second surface layer slurry. In some embodiments, silicone resin, silica, matting resin, etc., can also be added to the second surface layer slurry as needed to further improve the feel, gloss, etc. of the leather material, and further enhance the overall performance of the leather material.
[0066] As an example, the second topcoat slurry may include 80-120 parts by weight of polyurethane resin, 30-80 parts by weight of solvent, 0-2 parts by weight of wetting agent, 0-1 parts by weight of defoamer, 0-3 parts by weight of thickener, and 0-5 parts by weight of curing agent. The polyurethane resin may be either solvent-based polyurethane or waterborne polyurethane; the solvent-based polyurethane may be one or a mixture of two or more types of polycarbonate, polyether, or polyester. There are no particular limitations on the solvent, wetting agent, defoamer, thickener, and curing agent in this application, and they can be flexibly selected according to actual needs.
[0067] In some embodiments, the preparation method of the second surface layer slurry can be as follows: the raw materials of the second surface layer slurry are mixed and stirred evenly, and the viscosity is controlled to be 3000~7000 cps; the stirring speed is 500~1000 rpm and the stirring time is 5~10 min.
[0068] In some embodiments, the coating thickness of the second surface layer slurry can be 100μm~400μm; the drying temperature can be 100~140 ℃, and the drying time can be 10~15 min.
[0069] S5. Apply the foaming layer slurry to the side of the second surface layer away from the second release paper, and dry it for the first time until it can be bonded to the base fabric layer. After bonding the base fabric layer to the side of the foaming layer away from the second release paper, dry it for the second time and peel the whole thing off the release paper to obtain the semi-finished product 1.
[0070] According to embodiments of this application, the foaming layer slurry may include a polyol component A, an isocyanate component B, a catalyst, and a flame retardant. As an example, the foaming layer slurry comprises: 80-120 parts by weight of polyester polyol component A; 85-140 parts by weight of isocyanate component B; 0.001-0.2 parts by weight of an organometallic catalyst; 0.001-0.2 parts by weight of an organic amine catalyst; and 0.01-1.5 parts by weight of a phosphorus-based flame retardant.
[0071] In some embodiments, the preparation method of the foaming layer slurry can be as follows: first, the polyester polyol component A, organometallic catalyst, organic amine catalyst, and phosphorus flame retardant are mixed evenly at a stirring speed of 500-1000 rpm for 10-15 min; then, isocyanate component B is added to the above slurry and mixed evenly at a stirring speed of 1000 rpm for 1-2 min.
[0072] In some embodiments, the coating thickness of the foaming layer slurry can be 100μm~700μm; the temperature of the first and second drying treatments can be 120~140 ℃, the first drying time can be 1~7 min, and the second drying time can be 20~30 min.
[0073] S6. The first electrode paste is coated on the side of the semi-finished product 1 away from the base fabric layer, and then dried to obtain the semi-finished product 2.
[0074] In some embodiments, the first electrode paste may be a polyaniline:polystyrene sulfonate solution with a solid content of 1-6 wt%, or a poly(3,4)-poly(2 ... Ethylene dioxythiophene: a polystyrene sulfonate solution or an aqueous dispersion of silver nanowires, single-walled carbon nanotubes and / or graphene with a concentration of 5-15 mg / mL, wherein the solid content of the aqueous dispersion can be 1-6 wt%.
[0075] In some embodiments, the coating thickness of the first electrode slurry can be 50 μm to 300 μm; the drying temperature can be 100 to 140 °C, and the drying time can be 10 to 15 min.
[0076] S7. Apply the adhesive paste to the side of the electrochromic layer away from the first release paper, and then bond it to the side of the semi-finished product 2 away from the base fabric layer. After drying, peel off the first release paper to obtain a leather material that can actively control color change under low pressure.
[0077] According to embodiments of this application, the adhesive layer paste may include an adhesive and a solvent. As an example, the adhesive may be one or a combination of natural adhesives, epoxy resin adhesives, polyurethane adhesives, and polyvinyl alcohol adhesives.
[0078] According to embodiments of this application, the adhesive layer slurry can be vacuum degassed before coating to avoid the negative impact of air bubbles on display performance such as resolution and color uniformity.
[0079] In some embodiments, the coating thickness of the adhesive slurry can be 50 μm to 500 μm; the drying temperature can be 25 to 60 °C, and the drying time can be 0.5 to 12 h.
[0080] According to embodiments of this application, in addition to bonding the semi-finished product 2 and the electrochromic layer with an adhesive layer, they can also be laminated by hot pressing to further simplify the product manufacturing process.
[0081] In another aspect, this application provides a vehicle interior trim. According to an embodiment of this application, the vehicle interior trim includes the leather material described above. Therefore, the vehicle interior trim can actively change color, resulting in a richer and more diverse appearance, while also providing higher safety.
[0082] It is understandable that there are no particular restrictions on the specific types of automotive interiors, including but not limited to at least one of the following: seats, door panels, dashboard, steering wheel, and headliner.
[0083] In another aspect, this application provides a vehicle. According to an embodiment of this application, the vehicle includes the leather material or the vehicle interior described above. Therefore, the vehicle can actively change color, resulting in a richer and more diverse appearance, while also offering higher safety.
[0084] The embodiments of this application are described in detail below.
[0085] Example 1: S1. Weigh 100 g of polycarbonate polyurethane and 60 g of DMF, mix them evenly at room temperature by mechanical stirring (1000 rpm for 10 min), then coat them on the surface of release paper by roller coating (coating thickness of 200 μm), and dry them (120 ℃ for 10 min) to obtain the first transparent surface layer. S2. Prepare a 5 wt% polyaniline:polystyrene sulfonate solution (5 g of polyaniline:polystyrene sulfonate is added to 95 g of water and stirred at 1000 rpm for 10 min). Coat the second transparent electrode slurry onto the side of the first transparent layer away from the release paper (coating thickness is 300 μm). After drying (140 ℃, 10 min), the second transparent electrode is obtained. S3. The electronic ink microcapsule dispersion containing black / white bicolor charged particles is concentrated by centrifugation (500 rpm, 10 min) to obtain an electronic ink microcapsule concentrate; the electronic ink microcapsule concentrate is then mixed evenly with 15 wt% aqueous polyurethane adhesive (500 rpm, 10 min) to obtain an electrochromic layer slurry; the above electrochromic layer slurry is coated (coating thickness of 300 μm) on the side of the second transparent electrode away from the release paper, and then dried (60 ℃, 6 h) to obtain an electrochromic layer. S4. Weigh 100 g of polycarbonate polyurethane and 60 g of DMF, mix them evenly at room temperature by mechanical stirring (1000 rpm for 10 min), take another release paper, coat it with a roller (coating thickness of 200 μm) on the surface of the release paper, and dry it (120 ℃ for 10 min) to obtain the second surface layer. S5. Prepare the foaming layer slurry (weigh 50 g of polyester polyol component A, 53 g of isocyanate component B, 0.025 g of organometallic catalyst, 0.325 g of organic amine catalyst, and 15 g of aluminum hypophosphite flame retardant, and mix them by mechanical stirring at 1000 rpm for 1 min). Coat the foaming layer slurry on the side of the second surface away from the release paper (coating thickness of 400 μm). After the first drying (120 ℃, 2-3 min), it is ready to be bonded to the base fabric. After bonding the knitted fabric to the side of the foaming layer away from the release paper, it is dried a second time (140 ℃, 20 min). The whole thing is then peeled off from the release paper to obtain semi-finished product 1. S6. Prepare a 5 wt% single-walled carbon nanotube dispersion (5 g of single-walled carbon nanotubes are added to 95 g of water and stirred at 1000 rpm for 10 min), coat it (coating thickness is 300 μm) on the side of the semi-finished product 1 away from the base fabric, and dry it (140 ℃, 10 min) to form the first electrode and obtain the semi-finished product 2. S7. Prepare 15 wt% water-based polyurethane adhesive, apply the adhesive slurry (coating thickness of 300 μm) to the side of the electrochromic layer away from the release paper, and then bond it to the side of the semi-finished product 2 away from the base fabric. After drying treatment (60 ℃, 4h), the release paper is peeled off to obtain a leather material that can actively control color change under low pressure.
[0086] Example 2: Same as Example 1, except that: S3, the electronic ink microcapsule dispersion containing yellow / white bicolor particles is concentrated by centrifugation (500 rpm, 10 min) to obtain electronic ink microcapsule concentrate; then the electronic ink microcapsule concentrate is mixed evenly with 15 wt% waterborne polyurethane adhesive (500 rpm, 10 min) to obtain electrochromic layer slurry; the above electrochromic layer slurry is coated (coating thickness is 300 μm) on the side of the second transparent electrode away from the release paper, and dried (60 ℃, 6 h) to obtain electrochromic layer.
[0087] Example 3: Same as Example 1, except that: S3, the electronic ink microcapsule dispersion containing black / white bicolor particles is concentrated by centrifugation (500 rpm, 10 min) to obtain electronic ink microcapsule concentrate; then the electronic ink microcapsule concentrate is mixed evenly with 10 wt% PVA adhesive (10 g PVA added to 90 g water, stirred at 500 rpm for 1 h at 90 ℃, and then cooled to room temperature) (500 rpm, 10 min) to obtain electrochromic layer slurry; the above electrochromic layer slurry is coated (coating thickness of 300 μm) on the side of the second transparent electrode away from the release paper, and dried (60 ℃, 6 h) to obtain electrochromic layer.
[0088] S7. Prepare 10 wt% PVA adhesive (10 g PVA is added to 90 g water, stirred at 500 rpm for 1 h at 90 ℃, and then cooled to room temperature). Apply the adhesive slurry (coating thickness is 300 μm) to the side of the electrochromic layer away from the release paper, and then bond it to the side of the semi-finished product 2 away from the base fabric. After drying (60 ℃, 4 h), the release paper is peeled off to obtain a leather material that can actively control color change under low pressure.
[0089] Example 4: Same as Example 1, except that: S2, prepare a silver nanowire aqueous solution with a concentration of 15 mg / mL (1.5 g silver nanowires are added to 100 mL of water and stirred at 1000 rpm for 10 min), coat the second transparent electrode slurry on the side of the first transparent surface away from the release paper (coating thickness is 150 μm), and dry it (140 ℃, 10 min) to obtain the second transparent electrode.
[0090] Example 5: Same as Example 1, except that: S1, 100 g of polyester polyurethane and 60 g of DMF are weighed and mixed evenly at room temperature by mechanical stirring (1000 rpm for 10 min), and then coated on the surface of release paper by roller coating (coating thickness of 200 μm), and dried (120 ℃ for 10 min) to obtain the first transparent surface layer. S3. The electronic ink microcapsule dispersion containing white / red bicolor particles is concentrated by centrifugation (500 rpm, 10 min) to obtain an electronic ink microcapsule concentrate; the electronic ink microcapsule concentrate is then mixed evenly with 15 wt% of water-based polyurethane adhesive (500 rpm, 10 min) to obtain an electrochromic layer slurry; the above electrochromic layer slurry is coated (coating thickness of 300 μm) on the side of the second transparent electrode away from the release paper, and dried (60 ℃, 6 h) to obtain an electrochromic layer; S4. Weigh 100 g of polyester polyurethane and 60 g of DMF, mix them evenly at room temperature by mechanical stirring (1000 rpm for 10 min), take another release paper, coat it with a roller (coating thickness of 200 μm) on the surface of the release paper, and dry it (120 ℃ for 10 min) to obtain the second surface layer.
[0091] Example 6: S1. Weigh 100 g of polycarbonate polyurethane and 60 g of DMF, mix them evenly at room temperature by mechanical stirring (1000 rpm for 10 min), then coat them on the surface of release paper by roller coating (coating thickness of 200 μm), and dry them (120 ℃ for 10 min) to obtain the first transparent surface layer. S2. Prepare a 5 wt% polyaniline:polystyrene sulfonate solution (5 g of polyaniline:polystyrene sulfonate is added to 95 g of water and stirred at 1000 rpm for 10 min). Coat the second transparent electrode slurry onto the side of the first transparent layer away from the release paper (coating thickness is 300 μm). After drying (140 ℃, 10 min), the second transparent electrode is obtained. S3. The electronic ink microcapsule dispersion containing black / white bicolor particles is concentrated by centrifugation (500 rpm, 10 min) to obtain an electronic ink microcapsule concentrate; the electronic ink microcapsule concentrate is then mixed evenly with 15 wt% of water-based polyurethane adhesive (500 rpm, 10 min) to obtain an electrochromic layer slurry; the electrochromic layer slurry is coated (coating thickness of 300 μm) on the side of the second transparent electrode away from the release paper, and then dried (60 ℃, 6 h) to obtain an electrochromic layer; S4. Prepare 15 wt% water-based polyurethane adhesive, apply the adhesive slurry (coating thickness of 300 μm) to the side of the electrochromic layer away from the release paper, and dry it (60 ℃, 4 h) to obtain the adhesive layer.
[0092] S5. Prepare a 5 wt% single-walled carbon nanotube dispersion (5 g of single-walled carbon nanotubes are added to 95 g of water and stirred at 1000 rpm for 10 min), coat it (coating thickness is 300 μm) on the side of the above adhesive layer away from the release paper, and dry it (140 ℃, 10 min) to obtain the first electrode. S6. Weigh 100 g of polycarbonate polyurethane and 60 g of DMF, mix them evenly at room temperature by mechanical stirring (1000 rpm for 10 min), coat them with a roller (coating thickness of 200 μm) on the side of the first electrode away from the release paper, and dry them (120 °C for 10 min) to obtain the second surface layer. S7. Prepare the foaming layer slurry (weigh 50 g of polyester polyol component A, 53 g of isocyanate component B, 0.025 g of organometallic catalyst, 0.325 g of organic amine catalyst, and 15 g of aluminum hypophosphite flame retardant, and mix them by mechanical stirring at 1000 rpm for 1 min). Coat the foaming layer slurry on the side of the second surface layer away from the release paper (coating thickness of 400 μm). Dry it for the first time (120 ℃, 2-3 min) until it can be bonded to the base fabric. After bonding the knitted fabric to the side of the foaming layer away from the release paper, dry it for the second time (140 ℃, 20 min) and peel the whole thing off the release paper to obtain the leather material.
[0093] Example 7: S1. Weigh 100 g of polycarbonate polyurethane and 60 g of DMF, mix them evenly at room temperature by mechanical stirring (1000 rpm for 10 min), then coat them on the surface of release paper by roller coating (coating thickness of 200 μm), and dry them (120 ℃ for 10 min) to obtain the first transparent surface layer. S2. Prepare a 5 wt% polyaniline:polystyrene sulfonate solution (5 g of polyaniline:polystyrene sulfonate is added to 95 g of water and stirred at 1000 rpm for 10 min). Coat the second transparent electrode slurry onto the side of the first transparent layer away from the release paper (coating thickness is 300 μm). After drying (140 ℃, 10 min), the second transparent electrode is obtained. S3. Weigh 100 g of polycarbonate polyurethane and 60 g of DMF, mix them evenly at room temperature by mechanical stirring (1000 rpm for 10 min), take another release paper, coat it with a roller (coating thickness of 200 μm) on the surface of the release paper, and dry it (120 ℃ for 10 min) to obtain the second surface layer. S4. Prepare the foaming layer slurry (weigh 50 g of polyester polyol component A, 53 g of isocyanate component B, 0.025 g of organometallic catalyst, 0.325 g of organic amine catalyst, and 15 g of aluminum hypophosphite flame retardant, and mix them by mechanical stirring at 1000 rpm for 1 min). Coat the foaming layer slurry on the side of the second surface away from the release paper (coating thickness of 400 μm). After the first drying (120 ℃, 2-3 min), it is ready to be bonded to the base fabric. After bonding the knitted fabric to the side of the foaming layer away from the release paper, it is dried a second time (140 ℃, 20 min). The whole thing is then peeled off from the release paper to obtain semi-finished product 1. S5. Prepare a 5 wt% single-walled carbon nanotube dispersion (5 g of single-walled carbon nanotubes are added to 95 g of water and stirred at 1000 rpm for 10 min), coat it (coating thickness is 300 μm) on the side of the semi-finished product 1 away from the base fabric, and dry it (140 ℃, 10 min) to obtain the semi-finished product 2. S6. The electronic ink microcapsule dispersion containing black / white bicolor particles is concentrated by centrifugation (500 rpm, 10 min) to obtain an electronic ink microcapsule concentrate; the electronic ink microcapsule concentrate is then mixed evenly with 15 wt% water-based polyurethane adhesive (500 rpm, 10 min) to obtain an electrochromic layer slurry; the electrochromic layer slurry is coated (coating thickness of 300 μm) on the side of the second transparent electrode away from the release paper; it is then bonded to the side of the semi-finished product 2 away from the base fabric, dried (60 ℃, 6 h), and then the whole thing is peeled off from the release paper to obtain the leather material.
[0094] Comparative Example 1: Same as Example 7, except that: S6, ZnS is mixed evenly with 15 wt% of water-based polyurethane adhesive (500 rpm, 10 min) to obtain an electrochromic layer slurry; the above electrochromic layer slurry is coated (coating thickness is 300 μm) on the side of the second transparent electrode away from the release paper; then it is bonded to the side of the semi-finished product 2 away from the base fabric, dried (60 ℃, 6 h), and then the whole thing is peeled off from the release paper to obtain the leather material.
[0095] Performance testing: Color-changing ability under low voltage: At room temperature, the positive and negative terminals of the power supply were connected to the second transparent electrode / first electrode of the leather material via wires. The power supply voltage was set to 10 V. The apparent color of the leather, whether the color changed, and the uniformity of the color were observed under the adjusted potential direction. The number of color change cycles was recorded (if the color-changing effect was black-to-white, the number of cycles from white to black was 1, the number of cycles from white to black to white to black was 2, and so on). The apparent color, whether the color changed, the uniformity of the color, and the number of color change cycles were observed by the human eye. The test results are shown in Table 1.
[0096] Table 1
[0097] The data above shows that electronic ink microcapsules can achieve good color-changing effects under low voltage.
[0098] In the description of this utility model, it should be understood that the terms "first" and "second" are used for descriptive purposes only and should not be construed as indicating or implying relative importance or implicitly specifying the number of indicated technical features. Therefore, a feature defined as "first" or "second" may explicitly or implicitly include at least one of that feature. In the description of this utility model, "multiple" means at least two, such as two, three, etc., unless otherwise explicitly specified.
[0099] In the description of this specification, the references to terms such as "one embodiment," "some embodiments," "example," "specific example," or "some examples," etc., indicate that a specific feature, structure, material, or characteristic described in connection with that embodiment or example is included in at least one embodiment or example of the present invention. In this specification, the illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples. Moreover, without contradiction, those skilled in the art can combine and integrate the different embodiments or examples described in this specification, as well as the features of different embodiments or examples.
[0100] Although embodiments of the present invention have been shown and described above, it is understood that the above embodiments are exemplary and should not be construed as limiting the present invention. Those skilled in the art can make changes, modifications, substitutions and variations to the above embodiments within the scope of the present invention.
Claims
1. A leather material, characterized in that, include: basal layer; A first electrode is disposed on one side of the substrate layer; An electrochromic layer is disposed on the side of the first electrode away from the substrate layer, and the electrochromic layer includes electronic ink microcapsules; A second transparent electrode is disposed on the side of the electrochromic layer away from the substrate layer; A first transparent layer is disposed on the side of the second transparent electrode away from the substrate layer.
2. The leather material according to claim 1, characterized in that, The electronic ink microcapsules satisfy at least one of the following conditions: The average particle size of the electronic ink microcapsules is 5μm~70μm; The electronic ink microcapsules include at least one of the following: microcapsules containing monochromatic particles, microcapsules containing dual-color particles, and microcapsules containing multicolor particles.
3. The leather material according to claim 2, characterized in that, The microcapsules containing dual-color particles include microcapsules containing charged titanium dioxide and charged carbon black.
4. The leather material according to claim 1, characterized in that, At least one of the following conditions must be met: The first transparent surface layer has a first predetermined pattern; The electrochromic layer has a second predetermined pattern.
5. The leather material according to claim 1, characterized in that, At least one of the following conditions must be met: The thickness of the first electrode is 5μm~25μm; The thickness of the first transparent layer is 20μm~50μm; The thickness of the second transparent electrode is 5μm~25μm; The thickness of the electrochromic layer is 5μm~150μm; The first electrode comprises a conductive polymer, silver nanowires, or carbon nanoparticles; The second transparent electrode comprises a conductive polymer, silver nanowires, or carbon nanoparticles; The first transparent surface layer comprises polyurethane resin or polyvinyl chloride resin.
6. The leather material according to any one of claims 1 to 5, characterized in that, It also includes an adhesive layer disposed between the electrochromic layer and the first electrode.
7. The leather material according to claim 6, characterized in that, The adhesive layer satisfies at least one of the following conditions: The thickness of the adhesive layer is 50μm~400μm; The adhesive layer includes natural adhesives, epoxy resin adhesives, polyurethane adhesives, or polyvinyl alcohol adhesives.
8. The leather material according to claim 1, characterized in that, The base layer includes: A second surface layer is disposed on the side of the first electrode away from the electrochromic layer; A foamed layer is disposed on the side of the second surface layer away from the electrochromic layer; A base fabric layer is disposed on the side of the foam layer away from the electrochromic layer.
9. The leather material according to claim 8, characterized in that, At least one of the following conditions must be met: The thickness of the second surface layer is 20μm~50μm; The thickness of the foamed layer is 100μm~700μm; The thickness of the base fabric layer is 200μm~3000μm; The second surface layer comprises polyurethane resin or polyvinyl chloride resin; The foaming layer includes polyurethane foam; The base fabric layer may include at least one of knitted fabric, woven fabric, nonwoven fabric, and 3D Mesh.
10. A vehicle interior, characterized in that, The leather material includes any one of claims 1 to 9.