A composite coating structure of a rotor permanent magnet and an intervention pump
By coating the rotor permanent magnet with a composite coating structure consisting of an electroplated metal layer, a biocompatible ceramic layer, and a polymer layer, the problem of easy corrosion of neodymium iron boron materials in blood is solved, achieving good biocompatibility and corrosion resistance.
Patent Information
- Application Number
- CN202522691069.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Utility models(China)
- Current Assignee / Owner
- Filing Date
- 2025-12-18
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2035-12-18
AI Technical Summary
Motor rotors made of neodymium iron boron are prone to rust and corrosion when working in blood, failing to meet biocompatibility requirements.
A composite coating structure is formed by depositing an electroplated metal layer, a biocompatible ceramic layer, and a polymer layer on the surface of the rotor permanent magnet. The electroplated metal layer improves the bonding strength, the biocompatible ceramic layer improves the corrosion resistance, and the polymer layer provides encapsulation and protection.
Significantly improved corrosion resistance and biocompatibility of NdFeB material, ensuring robust and durable intervention pump rotor.
Smart Images

Figure CN225006141U_ABST
Abstract
Description
Technical Field
[0001] This utility model belongs to the field of medical device technology, and in particular relates to a composite coating structure of a rotor permanent magnet and an interventional pump. Background Technology
[0002] Interventional catheter pumps (blood pumps), as a treatment for end-stage heart failure and cardiogenic shock, are characterized by minimal invasiveness and low surgical risk. They can restore cardiac function without causing physical damage to the heart and have good therapeutic effects on high-risk patients. The core component affecting the function of the left ventricular assist system catheter pump is a micromotor. By driving the micromotor to rotate at high speed, it drives the impeller to generate pressure, pumping blood from the left ventricle into the aorta. This ensures that heart failure patients can still generate the necessary circulating blood flow to maintain their vital signs even when their cardiac function is insufficient.
[0003] Because the catheter pump needs to operate in the bloodstream for extended periods, it must have an internal pathway capable of providing heparin perfusion. The micromotor is placed in the aorta, in direct contact with the blood. The perfusion fluid passes through the pump's infusion tubing, through the micromotor's interior, and finally enters the bloodstream from the micromotor's tip. The motor rotor, located inside the motor, is primarily made of neodymium iron boron (NdFeB) magnetic material. However, NdFeB is highly susceptible to rust and corrosion, failing to meet biocompatibility requirements. Therefore, the surface of the NdFeB motor rotor requires special treatment to ensure biocompatibility. Utility Model Content
[0004] To address the aforementioned technical problems, this invention provides a composite coating structure for a rotor permanent magnet and an intervention pump. By coating the surface of the rotor permanent magnet with the composite coating structure of this invention, which has excellent corrosion resistance and high bonding strength with NdFeB, the rotor made of NdFeB material can meet the requirements of good biocompatibility.
[0005] In a first aspect, this utility model discloses a composite coating structure for a rotor permanent magnet, comprising a first coating, a second coating, and a third coating disposed from the inside out on the surface of the rotor permanent magnet; the first coating is an electroplated metal layer used to improve the bonding strength between the rotor permanent magnet and the composite coating structure; the second coating is a biocompatible ceramic layer used to improve the corrosion resistance of the rotor permanent magnet; and the third coating is a polymer layer used to encapsulate and protect the rotor permanent magnet.
[0006] Furthermore, the first coating is at least one of an electroplated nickel layer, an electroplated chromium layer, an electroplated zinc layer, and an electroplated silver layer.
[0007] Furthermore, the thickness of the first coating is 1~3μm.
[0008] Furthermore, the second coating is a titanium nitride layer and / or a chromium nitride layer.
[0009] Furthermore, the thickness of the second coating is 1~3μm.
[0010] Furthermore, the third coating is a paraffin layer.
[0011] Furthermore, the thickness of the third coating is 5~7μm.
[0012] Furthermore, the composite coating structure also includes a connecting layer located between the second coating and the third coating to improve the bonding strength between the second coating and the third coating.
[0013] Furthermore, the connecting layer is a silane coupling agent layer.
[0014] Furthermore, the rotor permanent magnet is a neodymium iron boron permanent magnet.
[0015] Secondly, this utility model also discloses an intervention pump, including a motor, wherein the motor includes a composite coating structure of the rotor permanent magnet of the first aspect of this utility model.
[0016] Compared with the prior art, the present invention has at least the following beneficial effects: (1) The composite coating structure of this utility model can significantly improve the corrosion resistance of the NdFeB intervention pump rotor, thereby giving the intervention pump rotor good biocompatibility.
[0017] (2) The composite coating structure of this utility model has high bonding strength. The coating structure and the coating structure and the neodymium iron boron rotor have strong bonding force and good adhesion, thus ensuring that the intervention pump rotor is sturdy and durable and its excellent corrosion resistance can be maintained for a long time. Attached Figure Description
[0018] To more clearly illustrate the technical solutions of the embodiments of this application, the accompanying drawings used in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0019] Figure 1 This is a schematic diagram of the composite coating structure of the rotor permanent magnet of this utility model.
[0020] Figure 2 This is a photograph of the composite coating from Example 1 after a 5-day corrosion resistance test in 5% salt water.
[0021] Figure 3 This is a photograph of the composite coating of Comparative Example 1 after a 5-day corrosion resistance test in 5% salt water.
[0022] Figure 4 This is a photograph of the composite coating of Comparative Example 2 after a 5-day corrosion resistance test in 5% salt water.
[0023] Figure 5 This is a photograph of the composite coating of Comparative Example 3 after a 5-day corrosion resistance test in 5% salt water.
[0024] Explanation of reference numerals in the attached figures: Rotor permanent magnet 1, first coating 2, second coating 3, third coating 4, connecting layer 5. Detailed Implementation
[0025] The technical solutions of the embodiments of this application will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some, not all, of the embodiments of this application. All other embodiments obtained by those skilled in the art based on the embodiments of this application without creative effort are within the scope of protection of this application.
[0026] Unless otherwise specified, all temperatures mentioned herein are in degrees Celsius, and the preferred embodiments can be freely combined as needed. Those skilled in the art will understand that the data and parameters described in the embodiments are merely exemplary and do not constitute a limitation of this invention. All components used in the following embodiments and comparative examples are compounds known in the art, and all equipment used is equipment publicly known in the art. All components and equipment used in this invention can be obtained commercially or prepared using known techniques.
[0027] This invention provides a composite coating structure for a rotor permanent magnet, such as... Figure 1 As shown, the composite coating structure includes a first coating 2, a second coating 3, and a third coating 4 disposed from the inside out on the surface of the rotor permanent magnet 1; the rotor permanent magnet 1 is a neodymium iron boron permanent magnet; the first coating 2 is an electroplated metal layer used to improve the bonding strength between the rotor permanent magnet 1 and the composite coating structure; the second coating 3 is a biocompatible ceramic layer used to improve the corrosion resistance of the rotor permanent magnet 1; the third coating 4 is a polymer layer used to encapsulate and protect the rotor permanent magnet 1.
[0028] Preferably, the first coating 2 of this invention is at least one of an electroplated nickel layer, an electroplated chromium layer, an electroplated zinc layer, and an electroplated silver layer. The thickness of the first coating 2 of this invention can be 1~3μm, preferably 1~2μm. The metal electroplating layer of this invention not only acts as a connector between the NdFeB rotor and the biocompatible ceramic layer, improving the bonding strength between the rotor and the ceramic layer, but also, due to its own characteristics of being difficult to oxidize and corrosion resistant, can improve the corrosion resistance of the rotor permanent magnet 1 and the overall composite coating structure.
[0029] Preferably, the second coating 3 of this invention is a titanium nitride layer and / or a chromium nitride layer. The thickness of the second coating 3 can be 1~3μm, preferably 2~3μm. The second coating 3 not only has excellent biocompatibility, but also excellent corrosion resistance, thus further improving the corrosion resistance of the rotor permanent magnet 1 and the overall coating.
[0030] Preferably, the third coating 4 of this invention is a paraxylene layer. The thickness of the third coating 4 can be 5~7μm, preferably 5~6μm. The chemical name of paraxylene is parylene. The paraxylene layer of this invention is a high molecular polymer conformal coating polymerized from parylene monomers. It can form a uniform, pinhole-free, and transparent film on the surface of the rotor permanent magnet 1. It has properties such as moisture resistance, corrosion resistance, insulation, chemical corrosion resistance, and good biocompatibility. It can cover various complex surfaces, including tiny gaps. Therefore, using the paraxylene layer as the outermost layer of the composite coating structure can provide good encapsulation and protection for the rotor permanent magnet 1 and the overall coating, thereby enabling the rotor permanent magnet 1 to maintain good corrosion resistance and biocompatibility for a long time.
[0031] Preferably, the composite coating structure of this invention further includes a connecting layer 5 located between the second coating 3 and the third coating 4, used to improve the bonding strength between the second coating 3 and the third coating 4. The binder material of the connecting layer 5 should be a bifunctional compound, where one functional group or molecular portion can bond to the metal layer or metal nitride / metal oxide layer, for example, by reacting with hydroxyl groups on the surface of the metal or metal nitride / metal oxide layer; the other functional group or molecular portion can bond to parylene, thereby firmly connecting the inorganic metal layer or metal nitrogen / oxide layer to the organic parylene layer. This connection can be achieved through covalent bonds or other types of chemical bonds. As exemplary binders, silane compounds, thiols, phosphine derivatives, disulfides, and silanes having thiol, phosphine, or disulfide groups can be selected. The choice of binder depends on the type of inorganic metal layer or metal nitrogen / oxide layer, and different binder compounds are selected accordingly. As a connecting layer between the second coating 3 and the third coating 4 of this utility model, the connecting layer 5 is preferably a silane coupling agent, thereby forming a strong bond between the titanium nitride / chromium nitride layer of the second coating 3 and the parylene layer of the third coating 4.
[0032] The method for preparing a composite coating structure on the surface of a neodymium iron boron rotor according to this invention includes the following steps: S1. Preprocessing The surface of the rotor neodymium iron boron magnet is cleaned, including degreasing, rust removal, dust removal, and water washing. S2. Electroplating to form an electroplated metal layer The surface of the neodymium iron boron magnet is acid-washed with sulfuric acid. The acid washing is performed for 20-35 seconds using sulfuric acid with a mass concentration of 0.5%. A metal salt solution is used as the electrolyte, and a high instantaneous current is applied for an impact time of 7-21 minutes to form a metal electroplating layer with a coating thickness of 1-3 μm. The metal salt solution includes at least one of nickel salt solution, chromium salt solution, zinc salt solution, and silver salt solution. S3. Physical vapor deposition to form a metal nitride layer The rotor is placed on a base in the PVD coating furnace chamber for magnetron sputtering deposition of a metal nitride layer. The magnetron sputtering process conditions are as follows: titanium nitride or chromium nitride target is used; furnace temperature is 180~320℃; and furnace vacuum is 2.0~5.5×10⁻⁶. -4 Pa, pulse bias voltage 200V, nitrogen flow rate 280~430sccm, target and substrate distance 15~25cm, arc current 100A, deposit to form a titanium nitride or chromium nitride coating with a thickness of 1~3μm. After deposition, wait for the furnace temperature to drop to 90~100℃, then air cool to room temperature, and the rotor can be taken out. S4. Dip-deposit to form a silane coupling agent bonding layer The rotor is immersed in an isopropanol solution containing silane coupling agent for 40-90 minutes, then removed and dried at 60-70°C for 2 hours to form a silane coupling agent bonding layer. S5. Chemical vapor deposition to form a poly(p-xylene) layer The rotor is placed in the deposition chamber of the CVD coating machine, and the parylene powder is placed in the sublimation chamber. The vapor deposition process conditions are as follows: deposition chamber vacuum degree 12~17 mTorr, sublimation chamber temperature 150~200℃, activation time 10~18 min, pyrolysis temperature 650~700℃, deposition time 100~140 min, forming a parylene layer with a thickness of 5~7 μm, i.e., the phenelzine layer.
[0033] This utility model also provides an intervention pump, including a motor, wherein the motor includes a composite coating structure of the rotor permanent magnet of this utility model.
[0034] The present invention will now be described in more detail with reference to exemplary embodiments. The following embodiments or experimental data are intended to illustrate the present invention by way of example, and it should be understood by those skilled in the art that the present invention is not limited to these embodiments or experimental data.
[0035] Example 1 A composite coating structure consisting of a 2μm electroplated nickel layer, a 2μm titanium nitride layer, a silane coupling agent connecting layer, and a 6μm parylene layer was deposited on the surface of a neodymium iron boron magnet. The deposition method is as follows: S1. Preprocessing The surface of the neodymium iron boron magnet is cleaned, including degreasing, rust removal, dust removal, and water washing. S2. Electroplating to form an electroplated metal layer The surface of the neodymium iron boron magnet was pickled with sulfuric acid with a mass concentration of 0.5% for 30 seconds. A nickel salt solution was used as the electrolyte, and a high instantaneous current was applied for 14 minutes to form a nickel electroplating layer with a coating thickness of 2μm. S3. Physical vapor deposition to form a metal nitride layer The neodymium iron boron magnet was placed in the furnace cavity of the PVD coating equipment. The magnetron sputtering process conditions were as follows: titanium nitride target was used, furnace cavity temperature was 260℃, and furnace cavity vacuum degree was 3.5×10⁻⁶. -4 Pa, pulse bias voltage 200V, nitrogen flow rate 350sccm, target and substrate distance 20cm, arc current 100A, deposit a titanium nitride coating with a thickness of 2μm, after the furnace temperature drops to 100℃ and is air-cooled to room temperature, the magnet is taken out. S4. Dip-deposit to form a silane coupling agent bonding layer The neodymium iron boron magnet was immersed in an isopropanol solution containing silane coupling agent for 60 minutes, and then dried at 70°C for 2 hours to form a silane coupling agent bonding layer. S5. Chemical vapor deposition to form a poly(p-xylene) layer Neodymium iron boron magnets were placed in the deposition chamber of a CVD coating machine, and parylene powder was placed in the sublimation chamber. The vapor deposition process conditions were: deposition chamber vacuum of 15 mTorr, sublimation chamber temperature of 180℃, activation time of 14 min, pyrolysis temperature of 680℃, and deposition time of 120 min, forming a parylene layer with a thickness of 6 μm.
[0036] Example 2 A composite coating structure consisting of a 1μm electroplated zinc layer, a 3μm chromium nitride layer, a silane coupling agent connecting layer, and a 7μm parylene layer was deposited on the surface of a NdFeB magnet. The deposition method is as follows: S1. Preprocessing The surface of the neodymium iron boron magnet is cleaned, including degreasing, rust removal, dust removal, and water washing. S2. Electroplating to form an electroplated metal layer The surface of the neodymium iron boron magnet was pickled with sulfuric acid with a mass concentration of 0.5% for 30 seconds. A zinc salt solution was used as the electrolyte, and a high instantaneous current was applied for 7 minutes to form a zinc electroplating layer with a coating thickness of 1 μm. S3. Physical vapor deposition to form a metal nitride layer The neodymium iron boron magnet was placed in the furnace cavity of the PVD coating equipment. The magnetron sputtering process conditions were as follows: chromium nitride target was used, furnace cavity temperature was 260℃, and furnace cavity vacuum degree was 3.5×10⁻⁶. -4 Pa, pulse bias voltage 200V, nitrogen flow rate 350sccm, target and substrate distance 20cm, arc current 100A, deposit chromium nitride coating with a thickness of 3μm, after the furnace temperature drops to 100℃, air cool to room temperature, and then remove the magnet. S4. Dip-deposit to form a silane coupling agent bonding layer The neodymium iron boron magnet was immersed in an isopropanol solution containing silane coupling agent for 60 minutes, and then dried at 70°C for 2 hours to form a silane coupling agent bonding layer. S5. Chemical vapor deposition to form a poly(p-xylene) layer Neodymium iron boron magnets were placed in the deposition chamber of a CVD coating machine, and parylene powder was placed in the sublimation chamber. The vapor deposition process conditions were: deposition chamber vacuum of 15 mTorr, sublimation chamber temperature of 180℃, activation time of 14 min, pyrolysis temperature of 680℃, and deposition time of 140 min, forming a parylene layer with a thickness of 7 μm.
[0037] Example 3 A composite coating structure consisting of a 3μm electroplated chromium layer, a 1μm chromium nitride layer, a silane coupling agent connecting layer, and a 5μm parylene layer was deposited on the surface of a NdFeB magnet. The deposition method is as follows: S1. Preprocessing The surface of the neodymium iron boron magnet is cleaned, including degreasing, rust removal, dust removal, and water washing. S2. Electroplating to form an electroplated metal layer The surface of the neodymium iron boron magnet was pickled with sulfuric acid with a mass concentration of 0.5% for 30 seconds. A chromium salt solution was used as the electrolyte, and a high instantaneous current was applied for 21 minutes to form a chromium electroplating layer with a coating thickness of 3μm. S3. Physical vapor deposition to form a metal nitride layer The neodymium iron boron magnet was placed in the furnace cavity of the PVD coating equipment. The magnetron sputtering process conditions were as follows: chromium nitride target was used, furnace cavity temperature was 260℃, and furnace cavity vacuum degree was 3.5×10⁻⁶. -4 Pa, pulse bias voltage 200V, nitrogen flow rate 350sccm, target and substrate distance 20cm, arc current 100A, deposit chromium nitride coating with a thickness of 1μm, after the furnace temperature drops to 100℃, air cool to room temperature, and then remove the magnet. S4. Dip-deposit to form a silane coupling agent bonding layer The neodymium iron boron magnet was immersed in an isopropanol solution containing silane coupling agent for 60 minutes, and then dried at 70°C for 2 hours to form a silane coupling agent bonding layer. S5. Chemical vapor deposition to form a poly(p-xylene) layer Neodymium iron boron magnets were placed in the deposition chamber of a CVD coating machine, and parylene powder was placed in the sublimation chamber. The vapor deposition process conditions were: deposition chamber vacuum of 15 mTorr, sublimation chamber temperature of 180℃, activation time of 14 min, pyrolysis temperature of 680℃, and deposition time of 100 min, forming a parylene layer with a thickness of 5 μm.
[0038] Example 4 A composite coating structure consisting of a 2μm electroplated silver layer, a 3μm titanium nitride layer, a silane coupling agent connecting layer, and a 5μm parylene layer was deposited on the surface of a neodymium iron boron magnet. The deposition method is as follows: S1. Preprocessing The surface of the neodymium iron boron magnet is cleaned, including degreasing, rust removal, dust removal, and water washing. S2. Electroplating to form an electroplated metal layer The surface of the neodymium iron boron magnet was acid-washed with sulfuric acid with a mass concentration of 0.5% for 30 seconds. A silver salt solution was used as the electrolyte, and a high instantaneous current was applied for 14 minutes to form a silver electroplating layer with a coating thickness of 2μm. S3. Physical vapor deposition to form a metal nitride layer The neodymium iron boron magnet was placed in the furnace cavity of the PVD coating equipment. The magnetron sputtering process conditions were as follows: titanium nitride target was used, furnace cavity temperature was 260℃, and furnace cavity vacuum degree was 3.5×10⁻⁶. -4 Pa, pulse bias voltage 200V, nitrogen flow rate 350sccm, target and substrate distance 20cm, arc current 100A, deposit a titanium nitride coating with a thickness of 3μm, after the furnace temperature drops to 100℃, air cool to room temperature, and remove the magnet; S4. Dip-deposit to form a silane coupling agent bonding layer The neodymium iron boron magnet was immersed in an isopropanol solution containing silane coupling agent for 60 minutes, and then dried at 70°C for 2 hours to form a silane coupling agent bonding layer. S5. Chemical vapor deposition to form a poly(p-xylene) layer Neodymium iron boron magnets were placed in the deposition chamber of a CVD coating machine, and parylene powder was placed in the sublimation chamber. The vapor deposition process conditions were: deposition chamber vacuum of 15 mTorr, sublimation chamber temperature of 180℃, activation time of 14 min, pyrolysis temperature of 680℃, and deposition time of 100 min, forming a parylene layer with a thickness of 5 μm.
[0039] Comparative Example 1 A composite coating structure consisting of a 4μm titanium nitride layer, a silane coupling agent connecting layer, and a 6μm parylene layer was deposited on the surface of a neodymium iron boron magnet. The deposition method is as follows: S1. Preprocessing The surface of the neodymium iron boron magnet is cleaned, including degreasing, rust removal, dust removal, and water washing. S2. Formation of metal nitride layers by physical vapor deposition. The neodymium iron boron magnet was placed in the furnace cavity of the PVD coating equipment. The magnetron sputtering process conditions were as follows: titanium nitride target was used, furnace cavity temperature was 260℃, and furnace cavity vacuum degree was 3.5×10⁻⁶. -4 Pa, pulse bias voltage 200V, nitrogen flow rate 350sccm, target and substrate distance 20cm, arc current 100A, deposit a titanium nitride coating with a thickness of 4μm, after the furnace temperature drops to 100℃ and is air-cooled to room temperature, the magnet is taken out. S3. Dip-deposit to form a silane coupling agent bonding layer The neodymium iron boron magnet was immersed in an isopropanol solution containing silane coupling agent for 60 minutes, and then dried at 70°C for 2 hours to form a silane coupling agent bonding layer. S4. Chemical vapor deposition to form a poly(p-xylene) layer Neodymium iron boron magnets were placed in the deposition chamber of a CVD coating machine, and parylene powder was placed in the sublimation chamber. The vapor deposition process conditions were: deposition chamber vacuum of 15 mTorr, sublimation chamber temperature of 180℃, activation time of 14 min, pyrolysis temperature of 680℃, and deposition time of 120 min, forming a parylene layer with a thickness of 6 μm.
[0040] Comparative Example 2 A composite coating structure consisting of a 4μm electroplated nickel layer, a silane coupling agent connecting layer, and a 6μm parylene layer was deposited on the surface of a neodymium iron boron magnet. The deposition method is as follows: S1. Preprocessing The surface of the neodymium iron boron magnet is cleaned, including degreasing, rust removal, dust removal, and water washing. S2. Electroplating to form an electroplated metal layer The surface of the neodymium iron boron magnet was pickled with sulfuric acid with a mass concentration of 0.5% for 30 seconds. A nickel salt solution was used as the electrolyte, and a high instantaneous current was applied for 28 minutes to form a nickel electroplating layer with a coating thickness of 4 μm. S3. Dip-deposit to form a silane coupling agent bonding layer The neodymium iron boron magnet was immersed in an isopropanol solution containing silane coupling agent for 60 minutes, and then dried at 70°C for 2 hours to form a silane coupling agent bonding layer. S4. Chemical vapor deposition to form a poly(p-xylene) layer Neodymium iron boron magnets were placed in the deposition chamber of a CVD coating machine, and parylene powder was placed in the sublimation chamber. The vapor deposition process conditions were: deposition chamber vacuum of 15 mTorr, sublimation chamber temperature of 180℃, activation time of 14 min, pyrolysis temperature of 680℃, and deposition time of 120 min, forming a parylene layer with a thickness of 6 μm.
[0041] Comparative Example 3 A composite coating structure consisting of a 4μm electroplated zinc layer, a silane coupling agent connecting layer, and a 6μm parylene layer was deposited on the surface of a NdFeB magnet. The deposition method is as follows: S1. Preprocessing The surface of the neodymium iron boron magnet is cleaned, including degreasing, rust removal, dust removal, and water washing. S2. Electroplating to form an electroplated metal layer The surface of the neodymium iron boron magnet was pickled with sulfuric acid with a mass concentration of 0.5% for 30 seconds. A zinc salt solution was used as the electrolyte, and a high instantaneous current was applied for 28 minutes to form a zinc electroplating layer with a coating thickness of 4μm. S3. Dip-deposit to form a silane coupling agent bonding layer The neodymium iron boron magnet was immersed in an isopropanol solution containing silane coupling agent for 60 minutes, and then dried at 70°C for 2 hours to form a silane coupling agent bonding layer. S4. Chemical vapor deposition to form a poly(p-xylene) layer Neodymium iron boron magnets were placed in the deposition chamber of a CVD coating machine, and parylene powder was placed in the sublimation chamber. The vapor deposition process conditions were: deposition chamber vacuum of 15 mTorr, sublimation chamber temperature of 180℃, activation time of 14 min, pyrolysis temperature of 680℃, and deposition time of 120 min, forming a parylene layer with a thickness of 6 μm.
[0042] Comparative Example 4 A composite coating structure was deposited on the surface of a NdFeB magnet using the same deposition method as in Example 1, except that step S4 (immersion plating to form a silane coupling agent bonding layer) and step S5 (chemical vapor deposition to form a parylene layer) were omitted. The final result was a composite coating structure consisting of a 2μm electroplated nickel layer and a 2μm titanium nitride layer.
[0043] Comparative Example 5 A composite coating structure was deposited on the surface of a NdFeB magnet using the same deposition method as in Example 1, except that step S4, which involves immersion plating to form a silane coupling agent bonding layer, was omitted. The final result was a composite coating structure consisting of a 2μm electroplated nickel layer, a 2μm titanium nitride layer, and a 6μm parylene layer.
[0044] The composition of the composite coating structures in Examples 1-4 and Comparative Examples 1-5 is shown in Table 1.
[0045] Table 1. Composition of composite coating structures in each embodiment and comparative example.
[0046] Corrosion resistance test Prepare a 5wt% NaCl brine solution. Place the NdFeB magnets with composite coating structures deposited in Examples 1-4 and Comparative Examples 1-5 into the brine for corrosion resistance testing. Observe and record the surface corrosion after immersion for 2 days and 5 days. See Table 2 for details.
[0047] Table 2. Corrosion resistance test results of each embodiment and comparative example.
[0048] Performance test results analysis As shown in Table 2, after 2 days and 5 days of corrosion resistance tests, the surfaces of Examples 1-4 of this utility model showed no obvious changes. Figure 2The image shown is a physical photograph of the surface morphology of the NdFeB magnet in Example 1 after a 5-day corrosion resistance test. The surface of the NdFeB magnet is smooth and shows no obvious changes, indicating that the composite coating structure of this invention has a strong bond with the NdFeB magnet and significantly improves the corrosion resistance of the NdFeB magnet.
[0049] The composite coating in Comparative Example 1 lacked an electroplated metal layer. After 2 days of brine immersion, there was no obvious change on the surface. However, after 5 days of brine immersion, the coating changed significantly. Figure 3 As can be seen, the composite coating on the surface of the NdFeB magnet has severely peeled off, and there is obvious corrosion on the surface. The electroplated metal layer of this invention not only has corrosion resistance itself, but also improves the bonding force between the NdFeB magnet and the metal nitride ceramic layer. Therefore, the lack of an electroplated metal layer will significantly reduce the corrosion resistance of the rotor and the overall coating.
[0050] The composite coatings in Comparative Examples 2 and 3 lacked a metal nitride ceramic layer. After soaking in salt water for 2 days, slight coating peeling occurred. After soaking in salt water for 5 days, the surface coating peeling became more obvious, and the magnet surface showed obvious corrosion. Figure 4 and 5 The images shown are actual images of the surface morphology of the neodymium iron boron magnets in Comparative Examples 2 and 3 after 5 days of soaking in salt water. It can be seen that the coating on the surface of the magnets in Comparative Examples 2 and 3 has peeled off and there is obvious rust.
[0051] In Comparative Example 4, the composite coating lacked both a silane coupling agent layer and a pyrelin layer. The absence of the pyrelin layer's encapsulation and protection of the composite coating structure resulted in the electroplated nickel and titanium nitride layers being directly corroded by the salt water, exhibiting the most severe corrosion among all comparative examples. After just two days of salt water immersion, coating peeling and surface corrosion already occurred. After five days of salt water immersion, the magnet surface was severely corroded, demonstrating the crucial role of the pyrelin layer in improving the corrosion resistance of NdFeB magnets.
[0052] The composite coating of Comparative Example 5 lacks a silane coupling agent layer. Although the silane coupling agent layer does not directly improve corrosion resistance, it significantly enhances the bonding strength between the titanium nitride layer and the pyrene layer. As a result, the composite coating of the magnet in Comparative Example 5 began to peel off after 2 days of salt water immersion, and after 5 days of salt water immersion, the surface composite coating was severely peeled off, and the magnet surface was severely corroded. This demonstrates that the silane coupling agent layer plays an important role in improving the bonding strength between the titanium nitride layer and the pyrene layer.
[0053] The materials and equipment used in this utility model are all commercially available and can be purchased from the market. The above description is only a preferred embodiment of this utility model and is not intended to limit this utility model. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of this utility model should be included within the protection scope of this utility model.
Claims
1. A composite coating structure for a rotor permanent magnet, characterized in that, The system includes a first coating, a second coating, and a third coating disposed from the inside out on the surface of the rotor permanent magnet; the first coating is an electroplated metal layer used to improve the bonding strength between the rotor permanent magnet and the composite coating structure; the second coating is a biocompatible ceramic layer used to improve the corrosion resistance of the rotor permanent magnet; and the third coating is a polymer layer used to encapsulate and protect the rotor permanent magnet.
2. The composite coating structure of the rotor permanent magnet according to claim 1, characterized in that, The first coating is at least one of electroplated nickel, electroplated chromium, electroplated zinc, and electroplated silver.
3. The composite coating structure of the rotor permanent magnet according to claim 2, characterized in that, The thickness of the first coating is 1~3μm.
4. The composite coating structure of the rotor permanent magnet according to claim 1, characterized in that, The second coating is a titanium nitride layer and / or a chromium nitride layer.
5. The composite coating structure of the rotor permanent magnet according to claim 4, characterized in that, The thickness of the second coating is 1~3μm.
6. The composite coating structure of the rotor permanent magnet according to claim 1, characterized in that, The third coating is a paraffin layer.
7. The composite coating structure of the rotor permanent magnet according to claim 6, characterized in that, The thickness of the third coating is 5~7μm.
8. The composite coating structure of the rotor permanent magnet according to claim 1, characterized in that, The composite coating structure also includes a connecting layer located between the second coating and the third coating to improve the bonding strength between the second coating and the third coating.
9. The composite coating structure of the rotor permanent magnet according to claim 8, characterized in that, The connecting layer is a silane coupling agent layer.
10. The composite coating structure of the rotor permanent magnet according to any one of claims 1-9, characterized in that, The rotor permanent magnet is a neodymium iron boron permanent magnet.
11. An intervention pump, comprising a motor, characterized in that, The motor includes a composite coating structure for the rotor permanent magnet as described in any one of claims 1 to 10.