A non-uniform catalyst layer membrane electrode for asymmetric high pressure conditions
By designing a non-uniform catalyst layer membrane electrode in a proton exchange membrane water electrolyzer and optimizing the electrode flow channel structure, the stability and lifespan issues of the electrolyzer under asymmetric high-pressure conditions were solved, achieving better durability and adaptability.
Patent Information
- Application Number
- CN202522141769.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Utility models(China)
- Current Assignee / Owner
- Filing Date
- 2025-10-10
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2035-10-10
AI Technical Summary
Existing technologies have failed to effectively address the stability issues of proton exchange membrane water electrolyzers under asymmetric high-pressure conditions, leading to challenges in high-pressure hydrogen production and storage, and severe degradation of catalyst layer lifespan.
A non-uniform catalyst layer membrane electrode for asymmetric high-pressure conditions is designed, comprising an anode plate, a porous transport layer, a non-uniform anode catalyst layer, a proton exchange membrane, a non-uniform cathode catalyst layer, and a gas diffusion layer. By optimizing the electrode channel structure, irreversible damage to the membrane electrode is matched, and the increase in catalyst layer stress is reduced.
It improves the durability of the membrane electrode, avoids the rapid decay of the catalyst layer under asymmetric high pressure conditions, is suitable for asymmetric pressure scenarios, and enhances the stability and lifespan of the electrolyzer.
Smart Images

Figure CN225013629U_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of proton exchange membrane water electrolysis technology, and specifically relates to a non-uniform catalyst layer membrane electrode for asymmetric high-pressure conditions. Background Technology
[0002] Proton exchange membrane electrolysis (PEMWE) uses perfluorosulfonic acid proton exchange membranes as the solid electrolyte, which exhibit high selectivity for proton transport. This allows PEM electrolyzers to safely operate under asymmetric pressure between the cathode and anode (typically, the cathode is at high pressure and the anode at atmospheric pressure). This capability is crucial for the production, storage, and transportation of high-pressure hydrogen, as well as for rapidly responding to fluctuations in renewable electricity, and offers significant advantages in system integration and cost reduction. However, compared to traditional atmospheric or symmetric pressure operation, the stability of electrolyzers under asymmetric pressure operation still presents considerable challenges. Optimizing the membrane electrode assembly (MEA), the core component of the electrolyzer, is key to solving these problems.
[0003] Currently, there are few reports on the optimized design of membrane electrode assemblies (MEAs) under asymmetric high-pressure conditions in PEM electrolyzers. However, there are some reports on the optimized design of MEAs with non-uniform catalyst layers in the field of fuel cells. CN114566653B proposes a non-uniform catalyst layer, a MEA, and its preparation method, specifically involving at least two sequentially spliced first and second catalyst layer membranes in the direction of the reaction gas flow. The physical properties of the catalyst layer are used to address the non-uniform distribution of reactants and the reaction environment, ensuring a uniform distribution of electrode chemical reactions and their products within the catalyst layer. CN115939413A provides a method for preparing a non-uniform catalyst coating membrane (CCM), the coating membrane, and the MEA. Specifically, the catalyst layer is divided into sub-regions, including first and second catalyst layers on both sides of the proton exchange membrane. In this CCM and MEA, the cathode catalyst layer consists of multiple sub-regions, with different component compositions and proportions in each sub-region. The purpose is to address the non-uniform reaction environment, achieving uniform reaction and product distribution, thereby ensuring the long-term stability of the MEA and the fuel cell. The non-uniform membrane electrode provided by CN115911435A is a modular electrode. Its main feature is the non-uniformity of the catalyst coating on the membrane electrode, which solves the problem of excessive current density distribution at the interface and thus improves the durability of the membrane electrode.
[0004] However, the non-uniform catalyst layer membrane electrode structure provided by the above technology is mainly optimized for the non-uniform distribution of reactants or reaction environment in fuel cells, and cannot effectively solve the performance degradation under asymmetric high-pressure conditions in electrolyzers with different working principles.
[0005] Problems with existing technologies: 1. Most related technical reports do not consider the testing and operation of electrolyzers under asymmetric high-pressure conditions. This results in insufficient technical support for requirements such as high-pressure hydrogen production, storage and transportation, and rapid response to fluctuations. 2. Existing technologies mainly address the uneven distribution of reactants or reaction environments in fuel cells by designing and modifying the catalyst layer. However, these technologies do not significantly improve the severe degradation of membrane electrode activity and lifespan in electrolyzers under different principles and environments. Utility Model Content
[0006] In order to solve the above-mentioned problems in the existing technology, the purpose of this utility model is to provide a non-uniform catalyst layer membrane electrode for asymmetric high-pressure conditions, which can effectively alleviate the damage of stress to the catalyst layer structure and thus reduce the decline in the performance of the electrolyzer.
[0007] The technical solution adopted in this utility model is as follows: A non-uniform catalyst layer membrane electrode for asymmetric high-pressure conditions includes, from top to bottom, an anode plate, a porous transport layer, a non-uniform anode catalyst layer, a proton exchange membrane, a non-uniform cathode catalyst layer, a gas diffusion layer, and a cathode plate, wherein the non-uniform anode catalyst layer and the non-uniform cathode catalyst layer respectively cover both sides of the proton exchange membrane.
[0008] This invention relates to a proton exchange membrane with non-uniform anode catalyst layers and non-uniform cathode catalyst layers on both sides. Under asymmetric high-pressure conditions, this invention utilizes electrode flow channels to optimize and match the irreversible structural damage of the membrane electrode, resulting in better durability compared to other membrane electrode structures and making it more suitable for asymmetric applications (cathode at high pressure, anode at atmospheric pressure). This invention also avoids the problem of excessively rapid degradation caused by a significant increase in stress on the catalyst layer under asymmetric high-pressure conditions.
[0009] As a preferred embodiment of this utility model, the operating pressure of the cathode plate is 0.1-5 MPa, and the operating pressure of the anode plate is 0.1-5 MPa.
[0010] As a preferred embodiment of this utility model, the non-uniform anode catalyst layer and the non-uniform cathode catalyst layer are configured as parallel flow field, serpentine flow field, multi-serpentine flow field, interdigitated flow field, spiral flow field or mesh flow field.
[0011] As a preferred embodiment of this invention, the area of both the non-uniform anode catalyst layer and the non-uniform cathode catalyst layer is 16–3000 cm². 2 .
[0012] As a preferred embodiment of this utility model, the material of the non-uniform anode catalyst layer is at least one of elemental iridium, elemental ruthenium, iridium-ruthenium alloy, iridium oxide, ruthenium oxide, iridium supported catalyst, and ruthenium supported catalyst.
[0013] As a preferred embodiment of this utility model, the material of the non-uniform cathode catalyst layer is at least one of platinum catalyst, palladium catalyst, platinum-palladium alloy catalyst, carbon-supported platinum catalyst, carbon-supported palladium catalyst, and carbon-supported platinum-palladium alloy.
[0014] As a preferred embodiment of this utility model, the porous transport layer is sintered titanium, titanium fiber felt, titanium metal mesh, etched titanium plate, or surface-treated titanium.
[0015] As a preferred embodiment of this utility model, the gas diffusion layer is carbon paper, carbon cloth, carbon fiber, graphite felt, sintered titanium, titanium foam, or titanium fiber felt.
[0016] As a preferred embodiment of this utility model, the anode plate is made of coated stainless steel, pure titanium, titanium alloy, graphite composite material or metal composite material.
[0017] As a preferred embodiment of this utility model, the cathode plate is made of coated stainless steel, pure titanium, titanium alloy, graphite composite material or metal composite material.
[0018] The beneficial effects of this utility model are as follows: This invention relates to a proton exchange membrane with non-uniform anode catalyst layers and non-uniform cathode catalyst layers on both sides. Under asymmetric high-pressure conditions, this invention utilizes electrode flow channels to optimize and match the irreversible structural damage of the membrane electrode, resulting in better durability compared to other membrane electrode structures and making it more suitable for asymmetric applications (cathode at high pressure, anode at atmospheric pressure). This invention also avoids the problem of excessively rapid degradation caused by a significant increase in stress on the catalyst layer under asymmetric high-pressure conditions. Attached Figure Description
[0019] Figure 1 This is a diagram of the state of a non-uniform film electrode when it is not assembled and no cathode pressure is applied. Figure 2 This is a diagram showing the state of a non-uniform film electrode when it is assembled and subjected to cathode pressure. Figure 3 This is a diagram of the state of a uniform film electrode when it is not assembled and no cathode pressure is applied. Figure 4 This is a diagram showing the state of a uniform film electrode when it is assembled and subjected to cathode pressure. Figure 5 This is a schematic diagram of the parallel flow field structure; Figure 6 This is a schematic diagram of the serpentine flow field structure; Figure 7 This is a comparison chart of the initial performance test results of the electrolyzers in Example 1 and Comparative Example 1; Figure 8 This is a comparison chart of the initial performance test results of the electrolyzers in Example 2 and Comparative Example 2; Figure 9 This is a comparison chart of the initial performance test results of the electrolyzers in Example 3 and Comparative Example 3; Figure 10 This is a comparison chart of the durability test results of the electrolytic cells in Example 1 and Comparative Example 1; Figure 11 This is a comparison chart of the durability test results of the electrolytic cells in Example 2 and Comparative Example 2; Figure 12 This is a comparison chart of the durability test results of the electrolytic cells in Example 3 and Comparative Example 3.
[0020] In the figure: 1-Non-uniform anode catalyst layer; 2-Proton exchange membrane; 3-Non-uniform cathode catalyst layer; 4-Anode plate; 5-Porous transport layer; 6-Gas diffusion layer; 7-Cathode plate; 8-Uniform anode catalyst layer; 9-Uniform cathode catalyst layer. Detailed Implementation
[0021] To make the objectives, technical solutions, and advantages of the embodiments of this utility model clearer, the technical solutions of the embodiments of this utility model will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of this utility model, and not all embodiments. The components of the embodiments of this utility model described and shown in the accompanying drawings can generally be arranged and designed in various different configurations.
[0022] Therefore, the following detailed description of the embodiments of the present invention provided in the accompanying drawings is not intended to limit the scope of the claimed invention, but merely to illustrate selected embodiments of the invention. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without inventive effort are within the scope of protection of the present invention. It should be noted that, unless otherwise specified, the embodiments and features described in the embodiments of the present invention can be combined with each other.
[0023] like Figure 1 and Figure 2 As shown, the non-uniform catalyst layer membrane electrode of this utility model for asymmetric high-pressure conditions includes, from top to bottom, an anode plate 4, a porous transport layer 5, a non-uniform anode catalyst layer 1, a proton exchange membrane 2, a non-uniform cathode catalyst layer 3, a gas diffusion layer 6, and a cathode plate 7. The non-uniform anode catalyst layer 1 and the non-uniform cathode catalyst layer 3 respectively cover both sides of the proton exchange membrane 2.
[0024] The proton exchange membrane 2 of this invention is covered on both sides with a non-uniform anode catalyst layer 1 and a non-uniform cathode catalyst layer 3, respectively. Under asymmetric high-pressure conditions, this invention utilizes the electrode flow channels to match and optimize the irreversible structural damage of the membrane electrode, resulting in better durability compared to other membrane electrode structures and making it more suitable for asymmetric applications (cathode under high pressure, anode under normal pressure). This invention avoids the problem of excessively rapid degradation caused by a significant increase in stress on the catalyst layer under asymmetric high-pressure conditions.
[0025] The operating pressure of the cathode plate 7 is 0.1-5 MPa, and the operating pressure of the anode plate 4 is 0.1-5 MPa.
[0026] like Figure 5 and Figure 6 As shown, the non-uniform anode catalyst layer 1 and the non-uniform cathode catalyst layer 3 are configured as parallel flow fields, serpentine flow fields, multi-serpentine flow fields, interdigitated flow fields, spiral flow fields, or mesh flow fields.
[0027] The areas of both the non-uniform anode catalyst layer 1 and the non-uniform cathode catalyst layer 3 are 16–3000 cm². 2 .
[0028] The material of the non-uniform anode catalyst layer 1 is at least one of elemental iridium, elemental ruthenium, iridium-ruthenium alloy, iridium oxide, ruthenium oxide, iridium supported catalyst, and ruthenium supported catalyst.
[0029] The material of the non-uniform cathode catalyst layer 3 is at least one of platinum catalyst, palladium catalyst, platinum-palladium alloy catalyst, carbon-supported platinum catalyst, carbon-supported palladium catalyst, and carbon-supported platinum-palladium alloy.
[0030] The porous transport layer 5 is sintered titanium, titanium fiber felt, titanium metal mesh, etched titanium plate, or surface-treated titanium.
[0031] The gas diffusion layer 6 is made of carbon paper, carbon cloth, carbon fiber, graphite felt, sintered titanium, titanium foam, or titanium fiber felt.
[0032] The materials of the anode plate 4 and the cathode plate 7 are coated stainless steel, pure titanium, titanium alloy, graphite composite material or metal composite material.
[0033] The present invention relates to a method for preparing a non-uniform catalyst layer electrode for asymmetric high-voltage conditions: Anode slurry preparation: 50-2000 mg of anode catalyst is mixed with resin solution, dispersion and water, and then treated at 15-80℃ by conventional dispersion method for 0.1-8 h to form a uniformly dispersed anode slurry.
[0034] Cathode slurry preparation: 50-2000 mg of cathode catalyst is mixed with resin solution, dispersion and water, and then treated at 15-80℃ by conventional dispersion method for 0.1-8 h to form a uniformly dispersed cathode slurry.
[0035] Uniform anode catalyst layer 8: The above-mentioned anode slurry is used to prepare a uniform anode catalyst layer 8 on one side of the proton exchange membrane 2 using conventional catalyst layer preparation methods.
[0036] Uniform cathode catalyst layer 9: The above cathode slurry is prepared on one side of the proton exchange membrane 2 using conventional catalyst layer preparation methods to complete the preparation of uniform cathode catalyst layer 9, and finally form a membrane electrode with an effective area of 16 to 3000 cm2 uniform cathode catalyst layer 9.
[0037] Non-uniform mask fabrication: Based on specific bipolar plate flow channel types, including parallel flow fields, serpentine flow fields, multi-serpentine flow fields, interdigitated flow fields, spiral flow fields, and mesh flow fields, one of the following materials—polytetrafluoroethylene (PTFE), polyphenylene sulfide (PPS), polyethylene glycol diformate (PEN), polyetherimide (PEI), stainless steel, and quartz glass—is used as the mask substrate. Corresponding cutouts are made at the ridge positions of the flow channel types, resulting in an effective area of 16–3000 cm². 2 Mask plate required for fabrication of non-uniform catalyst layer film electrode.
[0038] Fabrication of a non-uniform catalyst layer membrane electrode: The above-mentioned mask is placed over the anode side of the uniform catalyst layer membrane electrode, and then a conventional anode catalyst layer preparation is performed; subsequently, the mask is placed over the cathode side of the uniform catalyst layer membrane electrode, and a conventional cathode catalyst layer preparation is performed, ultimately forming an effective area of 16–3000 cm². 2 Non-uniform catalyst layer film electrode.
[0039] Based on the above membrane electrode, the components are positioned, aligned, and stacked before assembly, according to... Figure 1 As shown, from top to bottom, they are: anode plate 4, porous transport layer 5, non-uniform anode catalyst layer 1, proton exchange membrane 2, non-uniform cathode catalyst layer 3, gas diffusion layer 6, and cathode plate 7.
[0040] Finally, after the electrolytic cell assembly was completed, the cathode operating pressure was controlled at 0.1–5 MPa and the anode operating pressure was controlled at 0.1–5 MPa, and an operational test was carried out.
[0041] The above-mentioned conventional dispersion methods include one or a combination of stirring, ball milling, ultrasonication, homogenization, and shearing.
[0042] The above-mentioned methods for preparing the catalyst layer include one of the following: spraying, coating, screen printing, transfer printing, blade coating, electrochemical deposition, and sputtering.
[0043] The above-mentioned resin solution includes: perfluorosulfonic acid resin, wherein the perfluorosulfonic acid resin is one or more of short-side-chain perfluorosulfonic acid resin, medium- and long-side-chain perfluorosulfonic acid resin and long-chain perfluorosulfonic acid resin in any proportion.
[0044] The dispersions described above include one or more of the following in any proportion: methanol, ethanol, isopropanol, n-propanol, tert-butanol, ethylene glycol, glycerol, propylene glycol, dimethylacetamide, and dimethylformamide.
[0045] Example 1: 800 mg of iridium oxide anode catalyst was mixed with perfluorosulfonic acid resin solution, n-propanol and water, and then dispersed at 20 °C by ultrasonication and ball milling for 4 h to form a uniformly dispersed anode slurry.
[0046] 1000 mg of platinum carbon cathode catalyst was mixed with perfluorosulfonic acid resin solution, isopropanol and water, and then treated at 15 °C by shearing and ultrasonic dispersion for 1 h to form a uniformly dispersed cathode slurry.
[0047] The above-mentioned anode slurry was used to prepare a uniform anode catalyst layer 8 on one side of the proton exchange membrane 2 by coating. The above-mentioned cathode slurry was used to prepare a uniform cathode catalyst layer 9 on the other side of the proton exchange membrane 2 using a coating method, ultimately forming an effective area of 1000 cm². 2 Uniform catalyst film electrode; Based on the bipolar plate parallel flow field channel type, polytetrafluoroethylene (PTFE) was used as the mask substrate. Corresponding cutouts were made at the ridge positions in the parallel flow field, resulting in an effective area of 1000 cm². 2 Mask plate required for fabrication of non-uniform catalyst layer film electrode.
[0048] Next, the aforementioned mask is placed over the anode side of the uniform catalyst layer membrane electrode, and an anode catalyst layer is prepared using a coating method. Subsequently, the mask is placed over the cathode side of the uniform catalyst layer membrane electrode, and a cathode catalyst layer is prepared using a coating method, ultimately forming an effective area of 1000 cm². 2 Non-uniform catalyst layer film electrode.
[0049] Based on the above membrane electrode, the components are positioned, aligned, and stacked before assembly, according to... Figure 1 As shown, from top to bottom, the components are: coated stainless steel anode plate 4, titanium fiber felt, non-uniform iridium oxide anode catalyst layer, proton exchange membrane 2, non-uniform platinum carbon cathode catalyst layer, carbon cloth, and titanium alloy cathode plate 7.
[0050] Finally, after the electrolytic cell assembly was completed, the cathode operating pressure was controlled at 3 MPa and the anode operating pressure at 0.1 MPa, and operational tests were conducted (e.g., Figure 2 (As shown).
[0051] Example 2: Example 2 is a modification based on Example 1. The difference between Example 2 and Example 1 is that the pressure operating condition of the cathode is changed from 3 MPa to 0.1 MPa.
[0052] Example 3: Example 3 is a modification of Example 1. The difference between Example 3 and Example 1 is that the configuration of the non-uniform film electrode and the shape of the electrode flow field are changed from a parallel flow field to a serpentine flow field. Figure 5 and Figure 6 ).
[0053] Comparative Example 1: Comparative Example 1 is a modification of Example 1. The difference between Comparative Example 1 and Example 1 is that the non-uniform film electrode is replaced with a uniform film electrode (e.g., ...). Figure 3 and Figure 4 (As shown). From Figure 4 It can be clearly seen that after applying a cathode-side pressure of 3 MPa, the catalyst layer is severely compressed, forming dead zones and losing active sites.
[0054] Comparative Example 2: Comparative Example 2 is an improvement on Comparative Example 1. The difference between Comparative Example 2 and Comparative Example 1 is that the pressure operating condition of the cathode is changed from 3 MPa to 0.1 MPa.
[0055] The performance and durability of the electrolytic cell were tested based on national standards GB-T 45541-2025 and GBT 45539-2025, and the results are as follows: Figures 7-12 As shown. From Figures 7-9 It can be seen that the initial performance of the electrolyzers assembled with the membrane electrodes in the examples and comparative examples is not significantly different. However, due to... Figures 10-12 The durability test results of the electrolyzers shown indicate that the electrolyzer with a non-uniform membrane electrode structure exhibits significantly better durability and lower degradation rate than the electrolyzer with a uniform membrane electrode structure. Furthermore, a comparison between Examples 1 and 2 shows that the improvement in electrolyzer durability due to the non-uniform membrane electrode structure is more pronounced under asymmetrical operating pressure (cathode 3 MPa, anode 0.1 MPa) than under symmetrical pressure conditions (cathode 0.1 MPa, anode 0.1 MPa). Secondly, a comparison between Examples 1 and 3 shows that both parallel and serpentine flow field types demonstrate the improvement in electrolyzer durability due to the non-uniform membrane electrode structure, indicating good versatility.
[0056] This utility model is not limited to the above-mentioned optional embodiments. Anyone can derive other forms of products under the guidance of this utility model. However, regardless of any changes made in its shape or structure, any technical solution that falls within the scope of the claims of this utility model shall be protected by this utility model.
Claims
1. A non-uniform catalyst layer film electrode for asymmetric high-voltage conditions, characterized in that: The anode plate (4), porous transport layer (5), non-uniform anode catalyst layer (1), proton exchange membrane (2), non-uniform cathode catalyst layer (3), gas diffusion layer (6) and cathode plate (7) are arranged sequentially from top to bottom. The non-uniform anode catalyst layer (1) and non-uniform cathode catalyst layer (3) cover both sides of the proton exchange membrane (2).
2. The non-uniform catalyst layer film electrode for asymmetric high-voltage conditions according to claim 1, characterized in that: The operating pressure of the cathode plate (7) is 0.1-5 MPa, and the operating pressure of the anode plate (4) is 0.1-5 MPa.
3. The non-uniform catalyst layer film electrode for asymmetric high-voltage conditions according to claim 1, characterized in that: The non-uniform anode catalyst layer (1) and the non-uniform cathode catalyst layer (3) are configured as parallel flow fields, serpentine flow fields, interdigitated flow fields, spiral flow fields, or mesh flow fields.
4. A non-uniform catalyst layer film electrode for asymmetric high-voltage conditions according to claim 1, characterized in that: The area of both the non-uniform anode catalyst layer (1) and the non-uniform cathode catalyst layer (3) is 16-3000 cm². 2 .
5. A non-uniform catalyst layer film electrode for asymmetric high-voltage conditions according to claim 1, characterized in that: The porous transport layer (5) is sintered titanium, titanium fiber felt, titanium metal mesh or etched titanium plate.
6. A non-uniform catalyst layer film electrode for asymmetric high-voltage conditions according to claim 1, characterized in that: The gas diffusion layer (6) is made of carbon paper, carbon cloth, carbon fiber, graphite felt, sintered titanium, titanium foam or titanium fiber felt.
7. A non-uniform catalyst layer film electrode for asymmetric high-voltage conditions according to claim 1, characterized in that: The anode plate (4) is made of coated stainless steel, pure titanium, titanium alloy or graphite composite material.
8. A non-uniform catalyst layer film electrode for asymmetric high-voltage conditions according to claim 1, characterized in that: The cathode plate (7) is made of coated stainless steel, pure titanium, titanium alloy or graphite composite material.
Citation Information
Patent Citations
A non-uniform catalyst layer, a membrane electrode and its preparation method
CN114566653B
Battery bipolar plate, battery stack and fuel cell
CN115911435A
Preparation method of non-uniform catalyst coating membrane, coating membrane and membrane electrode
CN115939413A