A silicon carbide crystal growth apparatus

By introducing inert gas and nitrogen into the silicon carbide crystal growth apparatus, the growth environment was optimized, and the problems of radial temperature difference and excessive evaporation of silicon vapor caused by induction coil heating were solved, thus achieving stable growth of high-quality silicon carbide crystals.

CN225013677UActive Publication Date: 2026-11-24BEIJING TIANKE HEDA SEMICON CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202522826400.4
Authority / Receiving Office
CN · China
Patent Type
Utility models(China)
Current Assignee / Owner
Filing Date
2025-12-31
Publication Date
2026-11-24
Estimated Expiration
2035-12-31

AI Technical Summary

Technical Problem

In the existing technology, the induction coil heating method causes high temperature at the edge of the crucible during the growth of silicon carbide crystals, resulting in radial temperature difference and thermal stress, which leads to crystal cracking and dislocation proliferation. Furthermore, the problems of excessive silicon vapor evaporation and uneven nitrogen doping in the early stage of growth are difficult to solve.

Method used

Inert gas and nitrogen are introduced around the crucible. Inert gas and nitrogen are introduced into the gap between the graphite cylinder and the crucible through the gas path assembly to adjust the pressure and temperature, optimize the growth environment, reduce the edge temperature, suppress silicon vapor evaporation, and uniformly distribute the dopant.

Benefits of technology

It effectively reduces radial temperature difference, decreases thermal stress, inhibits excessive silicon vapor evaporation, improves nitrogen doping uniformity, and achieves stable growth of high-quality silicon carbide crystals.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN225013677U_ABST
    Figure CN225013677U_ABST
Patent Text Reader

Abstract

This invention provides a silicon carbide crystal growth apparatus, comprising a crucible, a graphite cylinder, a seed crystal holder, and a gas path assembly. The crucible is heated by an induction coil. The graphite cylinder is placed inside the crucible with a gap between it and the crucible. The graphite cylinder contains a raw material zone and a crystal growth zone. The raw material zone holds silicon carbide powder, and the crystal growth zone grows silicon carbide crystals. Through-holes are provided on the side wall of the graphite cylinder. The seed crystal holder is used to fix the silicon carbide seed crystal and is connected to the tops of both the crucible and the graphite cylinder. The gas path assembly passes through the seed crystal holder, with one end placed in the gap and the other end extending out of the crucible, for introducing inert gas and nitrogen into the gap. The inert gas and nitrogen can enter the graphite cylinder through the through-holes. This apparatus effectively reduces radial temperature differences and suppresses excessive silicon vapor evaporation in the early stages of growth, achieving stable growth of high-quality silicon carbide crystals.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This utility model belongs to the field of silicon carbide crystal growth technology, and specifically relates to a silicon carbide crystal growth device. Background Technology

[0002] Silicon carbide (SiC), as a third-generation wide-bandgap semiconductor material, possesses excellent properties such as high breakdown electric field, high thermal conductivity, and high electron mobility, making it irreplaceable in high-end fields such as new energy vehicles, 5G communications, and aerospace. Currently, induction coil heating methods (such as physical vapor transport, PVT) are the mainstream technology for preparing high-quality silicon carbide single crystals in industry. The principle is to heat the silicon carbide raw material in a crucible using an alternating magnetic field generated by an induction coil, causing the raw material to sublimate into Si-C vapor. Under the influence of a temperature gradient, the vapor is transported towards the seed crystal and deposited to grow into a single crystal.

[0003] However, due to the edge effect of the magnetic field distribution of the induction coil, the heating intensity of the edge region of the crucible and the raw materials inside is higher than that of the center region. This results in a huge radial temperature gradient inside the crucible, causing the temperature of the edge region of the grown crystal to be much higher than that of the center region. The uneven temperature field will generate huge thermal stress inside the crystal, which can easily lead to defects such as crystal cracking and dislocation multiplication, seriously reducing crystal quality and yield.

[0004] In existing technologies, attempts are usually made to improve temperature distribution by adjusting the number of turns of the induction coil and optimizing the furnace insulation structure. However, these methods cannot fundamentally solve the problem of high temperature at the crucible edge. In addition, ventilation at the top / bottom of the furnace is also used to try to solve the problem of high temperature at the crucible edge. However, due to the influence of the insulation graphite felt on the outside of the crucible, these methods are difficult to directly solve the problem of high temperature at the crucible edge, and are also difficult to simultaneously achieve the suppression of silicon vapor and the improvement of nitrogen doping uniformity.

[0005] Therefore, how to effectively reduce radial temperature difference, suppress excessive silicon vapor evaporation in the early stage of growth, and improve the uniformity of nitrogen doping to achieve stable growth of high-quality silicon carbide crystals is a technical problem that needs to be solved by those skilled in the art. Utility Model Content

[0006] In view of this, the purpose of this utility model is to provide a silicon carbide crystal growth device that can effectively reduce radial temperature difference, suppress excessive evaporation of silicon vapor in the early stage of growth, improve the uniformity of nitrogen doping, and achieve stable growth of high-quality silicon carbide crystals.

[0007] To achieve the above objectives, this utility model provides the following technical solution:

[0008] A silicon carbide crystal growth apparatus, comprising:

[0009] The crucible is heated by an induction coil;

[0010] A graphite cylinder is disposed inside the crucible, and there is a gap between the graphite cylinder and the crucible. The graphite cylinder is provided with a raw material area and a crystal growth area. The raw material area is used to place silicon carbide powder, and the crystal growth area is used for silicon carbide crystal growth. The side wall of the graphite cylinder is provided with through holes.

[0011] A seed crystal holder is used to fix a silicon carbide seed crystal, and the seed crystal holder is connected to the top of the crucible and the graphite cylinder respectively;

[0012] A gas passage assembly passes through the seed crystal holder, with one end of the gas passage assembly placed in the gap and the other end extending out of the crucible, for introducing inert gas and nitrogen into the gap. The inert gas and nitrogen can enter the graphite cylinder through the through hole.

[0013] Optionally, the flow rate of the inert gas introduced into the gap is 200 sccm-600 sccm, and the flow rate of the nitrogen gas introduced into the gap is 15 sccm-25 sccm.

[0014] Optionally, the seed crystal holder is threadedly connected to the crucible and the graphite cylinder, or snap-fit ​​connected.

[0015] Optionally, the graphite cylinder and the crucible are detachably connected.

[0016] Optionally, the inner diameter of the graphite tube is R1, the outer diameter of the graphite tube is R2, and the diameter of the silicon carbide seed crystal is R3, where 0.1mm≤R1-R3≤0.5mm and 10mm≤R2-R3≤80mm.

[0017] Optionally, the plurality of through holes are evenly arranged along the wall of the graphite cylinder, and the distances from the through holes to the bottom end face of the graphite cylinder are equal, and / or,

[0018] The diameter of the through hole is 1mm-5mm.

[0019] Optionally, the length of the gas path assembly extending into the crucible is L1, where 20mm ≤ L1 ≤ 50mm, and / or,

[0020] The distance between the through hole and the surface of the seed crystal holder is L2, where 10mm≤L2≤100mm.

[0021] Optionally, the gas path assembly includes a first inlet pipe and a second inlet pipe, wherein the first inlet pipe is used to introduce nitrogen gas and the second inlet pipe is used to introduce the inert gas.

[0022] The first air inlet pipe and the second air inlet pipe are at the same height from the bottom of the crucible.

[0023] Optionally, the seed crystal holder is further provided with mounting holes for mounting the gas path assembly and exhaust holes for the inert gas and the nitrogen flow.

[0024] Both the mounting hole and the vent hole are provided corresponding to the gap, and there is a preset distance between the vent hole and the mounting hole.

[0025] Optionally, the number of vent holes is 1-3;

[0026] The diameter of the exhaust port is 2mm-5mm.

[0027] As can be seen from the above technical solution, firstly, silicon carbide powder is placed in the raw material area of ​​the graphite cylinder, and the silicon carbide seed crystal is fixed on the seed crystal holder. The seed crystal holder is connected to the top of the crucible and the graphite cylinder respectively. Then, the furnace is cleaned. After cleaning, the pressure of the graphite cylinder is maintained at a first preset pressure value. The induction coil is activated to heat the crucible and the graphite cylinder placed inside the crucible, causing the inside of the graphite cylinder to gradually heat up. During the heating process, inert gas is continuously introduced into the gap between the graphite cylinder and the crucible through the gas path assembly. The inert gas enters the graphite cylinder through the through hole. During the heating process, the pressure inside the graphite cylinder is maintained at the first preset pressure value. When the temperature inside the graphite cylinder reaches the first preset pressure value... When the temperature is set, maintain it for a first preset time. Then, under the first preset temperature condition, reduce the first preset pressure value to a second preset pressure value and maintain it for a second preset time. Under the second preset pressure value condition, introduce nitrogen gas into the gap between the graphite cylinder and the crucible, mix it with the inert gas, and let the nitrogen gas enter the graphite cylinder through the through hole to carry out crystal growth. During this stage, maintain the first preset temperature. After the silicon carbide crystal growth is completed, stop heating, turn off the nitrogen gas, and continue to introduce inert gas to keep the pressure inside the graphite cylinder at a third preset pressure value until the temperature inside the graphite cylinder drops to room temperature. Then continue to introduce inert gas until the pressure rises to atmospheric pressure, and then take out the silicon carbide crystal.

[0028] Compared with the prior art, the silicon carbide crystal growth apparatus disclosed in this embodiment of the present invention can achieve multi-dimensional optimization of the crystal growth environment by introducing an inert gas around the crucible, specifically in the following three aspects:

[0029] 1) It can reduce the edge temperature of silicon carbide crystals, reduce the radial temperature difference, and reduce the thermal stress during the growth of silicon carbide crystals;

[0030] 2) It can reduce the edge temperature of the raw material zone, suppress excessive evaporation of silicon vapor in the early stage of growth, and the introduction of inert gas can effectively suppress the escape rate of silicon vapor and maintain the balance of silicon-carbon ratio of raw materials.

[0031] 3) The introduction of inert gas can instantly disperse and uniformly mix the introduced nitrogen dopant in the entire atmosphere, avoiding excessively high or low local concentrations, thereby effectively enhancing the uniformity of wafer resistivity and achieving stable growth of high-quality silicon carbide crystals. Attached Figure Description

[0032] To more clearly illustrate the technical solutions in the embodiments of this utility model or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of this utility model. For those skilled in the art, other drawings can be obtained based on the provided drawings without creative effort.

[0033] Figure 1 This is a schematic diagram of the silicon carbide crystal growth apparatus disclosed in the embodiments of this utility model.

[0034] Figure 2 This is a schematic diagram of the seed crystal holder structure disclosed in the embodiments of this utility model;

[0035] Figure 3 This is a stress diagram of a crystal grown using the silicon carbide crystal growth apparatus disclosed in this embodiment of the invention after it has been processed into a wafer.

[0036] Figure 4 This is a dark field encapsulation image of a silicon carbide crystal grown using the silicon carbide crystal growth apparatus disclosed in this embodiment of the invention after it has been processed into a wafer.

[0037] Figure 5 The stress diagram is shown for a silicon carbide crystal grown using a silicon carbide crystal growth apparatus disclosed in the prior art, after being processed into a wafer.

[0038] Figure 6 This is a dark field encapsulation image of a silicon carbide crystal grown using a silicon carbide crystal growth apparatus disclosed in the prior art, after being processed into a wafer.

[0039] Explanation of reference numerals in the attached figures:

[0040] 100-Crucible,

[0041] 200 - Graphite tube, 201 - Through hole, 202 - Raw material area, 203 - Crystal growth area

[0042] 300 - Seed crystal holder, 301 - Mounting hole, 302 - Vent hole

[0043] 400-First Intake Pipe

[0044] 500 - Second intake pipe,

[0045] 600-gap. Detailed Implementation

[0046] In view of this, the core of this utility model is to provide a silicon carbide crystal growth device that can effectively reduce radial temperature difference, suppress excessive evaporation of silicon vapor in the early stage of growth, and improve the uniformity of nitrogen doping, so as to achieve stable growth of high-quality silicon carbide crystals.

[0047] The technical solutions of the present utility model will be clearly and completely described below with reference to the accompanying drawings of the embodiments. Obviously, the described embodiments are only some embodiments of the present utility model, and not all embodiments. Based on the embodiments of the present utility model, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present utility model. Please refer to... Figures 1-6 .

[0048] Please refer to Figure 1 The silicon carbide crystal growth apparatus disclosed in this embodiment includes a crucible 100, a graphite cylinder 200, a seed crystal holder 300, and a gas path assembly. The crucible 100 is heated by an induction coil. The graphite cylinder 200 is disposed within the crucible 100, with a gap 600 between the graphite cylinder 200 and the crucible 100. The graphite cylinder 200 contains a raw material zone 202 and a crystal growth zone 203. The raw material zone 202 is used to hold silicon carbide powder, and the crystal growth zone 203... For silicon carbide crystal growth, a through hole 201 is provided on the side wall of the graphite cylinder 200; a seed crystal holder 300 is used to fix the silicon carbide seed crystal, and the seed crystal holder 300 is connected to the top of the crucible 100 and the graphite cylinder 200 respectively; a gas passage assembly passes through the seed crystal holder 300, one end of the gas passage assembly is placed in the gap 600, and the other end extends out of the crucible 100, for introducing inert gas and nitrogen into the gap 600, and the inert gas and nitrogen can enter the graphite cylinder 200 through the through hole 201.

[0049] First, silicon carbide powder is placed in the raw material area 202 of the graphite cylinder 200. A silicon carbide seed crystal is fixed on the seed crystal holder 300. The seed crystal holder 300 is connected to the top of both the crucible 100 and the graphite cylinder 200. Then, the furnace is cleaned. After cleaning, the pressure in the graphite cylinder 200 is maintained at a first preset pressure value. The induction coil is activated to heat the crucible 100 and the graphite cylinder 200 placed inside the crucible 100, causing the interior of the graphite cylinder 200 to gradually heat up. During the heating process, inert gas is continuously introduced into the gap 600 between the graphite cylinder 200 and the crucible 100 through the gas path assembly. The inert gas enters the graphite cylinder 200 through the through-hole 201. During the heating process, the pressure inside the graphite cylinder 200 is maintained at the first preset pressure value. When the graphite cylinder 200… When the temperature inside the graphite cylinder 200 reaches the first preset temperature, it is maintained for the first preset time. Then, under the first preset temperature condition, the first preset pressure value is reduced to the second preset pressure value and maintained for the second preset time. Under the second preset pressure value condition, nitrogen gas is introduced into the gap 600 between the graphite cylinder 200 and the crucible 100 and mixed with inert gas. The nitrogen gas enters the graphite cylinder 200 through the through hole 201 to carry out crystal growth. During this stage, the first preset temperature is maintained. After the silicon carbide crystal growth is completed, heating is stopped, nitrogen gas is turned off, and inert gas is continuously introduced to keep the pressure inside the graphite cylinder 200 at the third preset pressure value until the temperature inside the graphite cylinder 200 drops to room temperature. Then, inert gas is introduced again until the pressure rises to atmospheric pressure, and the silicon carbide crystal is taken out.

[0050] Compared with the prior art, the silicon carbide crystal growth apparatus disclosed in this utility model can achieve multi-dimensional optimization of the silicon carbide crystal growth environment by introducing an inert gas around the crucible, specifically in the following three aspects:

[0051] 1) It can reduce the edge temperature of silicon carbide crystals, reduce the radial temperature difference, and reduce the thermal stress during the growth of silicon carbide crystals;

[0052] 2) It can reduce the edge temperature of the raw material zone 202, suppress the excessive evaporation of silicon vapor in the early stage of growth, and the introduction of inert gas can effectively suppress the escape rate of silicon vapor and maintain the balance of silicon-carbon ratio of raw materials.

[0053] 3) The introduction of inert gas can instantly disperse and uniformly mix the introduced nitrogen dopant in the entire atmosphere, avoiding excessively high or low local concentrations, thereby effectively enhancing the uniformity of wafer resistivity and achieving stable growth of high-quality silicon carbide crystals.

[0054] It should be noted that an insulating graphite felt is provided on the outside of the crucible 100, and an induction coil is provided on the outside of the insulating graphite felt.

[0055] It should be explained that the top of crucible 100 and graphite cylinder 200 refers to the end away from the raw material zone 202.

[0056] As a further embodiment, in the silicon carbide crystal growth apparatus disclosed in this utility model embodiment, the flow rate of the inert gas introduced into the gap 600 is 200 sccm-600 sccm. For example, the flow rate of the inert gas can be specifically 200 sccm, 400 sccm, or 600 sccm.

[0057] If the flow rate of the inert gas is too low, it may not be able to form effective forced convection cooling in the high-temperature zone at the edge of the crucible 100, resulting in the raw material edge temperature remaining too high. The root cause of excessive Si vapor evaporation is not suppressed, and the silicon-carbon ratio in the gas phase is difficult to maintain balance, which will still cause defects such as polymorphic inclusions and inclusions in the crystal. However, the flow rate range of 200 sccm-600 sccm disclosed in this embodiment can form stable and directional forced convection during crystal growth, achieving the best balance between suppressing excessive evaporation of raw materials, optimizing the temperature field, homogenizing dopants, and maintaining growth stability.

[0058] As a further embodiment, in the silicon carbide crystal growth apparatus disclosed in this utility model embodiment, the flow rate of nitrogen gas introduced through the gap 600 is 15 sccm - 25 sccm. For example, the flow rate of nitrogen gas can be specifically 15 sccm, 20 sccm, or 25 sccm.

[0059] This utility model embodiment does not limit the specific connection relationship between the crucible 100, the graphite cylinder 200 and the seed crystal holder 300. The seed crystal holder 300 can be threaded to the crucible 100 and the graphite cylinder 200 respectively, or it can be snapped to the crucible 100 and the graphite cylinder 200 respectively. Any structure that meets the requirements of the utility model is within the protection scope of this utility model. Those skilled in the art can make selections according to actual needs.

[0060] It should be noted that the graphite cylinder 200 and the crucible 100 disclosed in this embodiment of the present invention are detachably connected, which facilitates the replacement of the graphite cylinder 200.

[0061] Specifically, the graphite cylinder 200 and the crucible 100 can be connected by threads, snap-fit, or other connection structures. Those skilled in the art can choose the specific connection method according to actual needs.

[0062] As a further embodiment, in the silicon carbide crystal growth apparatus disclosed in this utility model embodiment, the inner diameter of the graphite cylinder 200 is R1, the outer diameter of the graphite cylinder 200 is R2, and the diameter of the silicon carbide seed crystal is R3, where 0.1mm≤R1-R3≤0.5mm and 10mm≤R2-R3≤80mm. For example, R1-R3 can specifically be 0.1mm, 0.3mm, or 0.5mm; R2-R3 can specifically be 10mm, 30mm, 50mm, 60mm, or 80mm.

[0063] The range of 0.1mm≤R1-R3≤0.5mm mainly takes into account the processing tolerances and the protection of the silicon carbide seed crystal during assembly.

[0064] The setting of the range 10mm≤R2-R3≤80mm determines the wall thickness of the graphite cylinder 200. This wall thickness determines the thermal resistance of the graphite cylinder 200 itself, enabling it to effectively construct and maintain the axial temperature gradient required for seed crystal growth. This gradient is the guarantee of stable crystal growth. Furthermore, the size of this wall thickness determines the amount of material loaded, ensuring that there is sufficient raw material to meet the requirements of large-size and long-thick crystals.

[0065] As a further embodiment, in the silicon carbide crystal growth apparatus disclosed in this utility model embodiment, the through holes 201 are uniformly arranged along the wall of the graphite cylinder 200, and the distance between the through holes 201 and the bottom end face of the graphite cylinder 200 is equal. This arrangement ensures that inert gas and nitrogen gas are injected simultaneously and in equal amounts from all directions of the graphite cylinder 200, thereby effectively preventing the formation of vortices or localized high-speed / low-speed zones in the airflow within the chamber of the graphite cylinder 200, and further preventing disturbances in the temperature field.

[0066] The diameter of the through hole 201 is 1mm-5mm. For example, the diameter of the through hole 201 can be 1mm, 3mm, or 5mm.

[0067] As a further embodiment, in the silicon carbide crystal growth apparatus disclosed in this utility model embodiment, the length of the gas path component entering the crucible 100 is L1, where 20mm≤L1≤50mm. For example, L1 can specifically be 20mm, 25mm, 30mm, 35mm, 40mm, or 50mm.

[0068] As a further embodiment, in the silicon carbide crystal growth apparatus disclosed in this utility model embodiment, the distance between the through hole 201 and the surface of the seed crystal holder 300 is L2, where 10mm≤L2≤100mm. For example, L2 can specifically be 10mm, 20mm, 30mm, 50mm, 80mm, or 100mm.

[0069] It should be noted that the silicon carbide crystal growth apparatus disclosed in this embodiment of the present invention includes a gas path assembly comprising a first gas inlet pipe 400 and a second gas inlet pipe 500. The first gas inlet pipe 400 is used to introduce nitrogen gas, and the second gas inlet pipe 500 is used to introduce argon gas.

[0070] The first inlet pipe 400 and the second inlet pipe 500 are at the same height from the bottom of the crucible 100. This arrangement allows the two gases to mix rapidly upon introduction, and the inert gas can quickly disperse and evenly mix the nitrogen gas throughout the atmosphere, effectively improving resistivity uniformity.

[0071] As a further embodiment, please refer to Figure 2 The silicon carbide crystal growth apparatus disclosed in this embodiment of the invention includes a seed crystal holder 300 with a mounting hole 301 for mounting gas path components and an exhaust hole 302 for the outflow of inert gas and nitrogen. Both the mounting hole 301 and the exhaust hole 302 are correspondingly positioned to correspond to a gap 600, and a predetermined distance exists between the exhaust hole 302 and the mounting hole 301. With this configuration, after the inert gas and nitrogen mix within the gap 600, a portion enters the crucible 100, and a portion flows out through the exhaust hole 302.

[0072] In this embodiment of the present invention, the number of exhaust holes 302 is 1-3, and the diameter of the exhaust holes 302 is 2mm-5mm. For example, the exhaust holes 302 can be 2mm, 3mm, or 5mm.

[0073] This utility model does not limit the specific type of inert gas. Any inert gas that meets the requirements of this utility model is within the protection scope of this utility model.

[0074] As a specific embodiment of this utility model, the inert gas disclosed in this utility model embodiment is preferably argon.

[0075] The following is a comparison of the crystal surface after silicon carbide crystal growth using the silicon carbide crystal growth apparatus of this utility model and the crystal surface after crystal growth using the prior art:

[0076] Please refer to Figure 3 and Figure 4 , adopt as Figure 1 , 2The disclosed silicon carbide crystal growth apparatus uses induction coils for heating and graphite felt as the insulation medium. A 190mm diameter 4H-SiC seed crystal is selected, with the C-side chosen as the growth surface, and is bonded to the seed crystal holder 300 using organic adhesive. The seed crystal holder 300 has a diameter of 240mm and is connected to the crucible 100 and graphite cylinder 200 via threads. The seed crystal holder 300 passes through a first inlet pipe 400 for introducing inert gas and a second inlet pipe 500 for introducing nitrogen gas. Three exhaust holes 302 with a diameter of 3mm are provided on the other side. The graphite cylinder 200 has an inner diameter of 190.1mm and an outer diameter of 210mm, with a ring of 2mm diameter through holes 201 on its side. The through holes 201 are 3mm away from the surface of the seed crystal. The height of the graphite cylinder 200 is 230mm. Silicon carbide powder is placed in the lower middle part of the graphite cylinder 200, with a loading height of 160mm. After cleaning the furnace, the pressure inside the graphite cylinder 200 is maintained at 50Kpa. The induction coil is started to heat the temperature to 2100℃-2500℃ and held for 3 hours. During the heating process, a large flow of argon gas (300sccm) is continuously introduced, and the pressure is maintained at 50Kpa. Then the pressure is reduced to 700Pa, and the temperature is still maintained at 2100℃-2500℃. Nitrogen gas (16sccm) is introduced and held for 200 hours to carry out the crystal growth process. After the growth is completed for 200 hours, the nitrogen gas is turned off and the heating is stopped. The argon gas remains unchanged, and the pressure is maintained at 50Kpa until the temperature drops to room temperature. Then the pressure is increased to atmospheric pressure and the crystal is removed.

[0077] Please refer to the following for details. Figure 3 and Figure 4 ,in, Figure 3 From left to right, (a), (b), and (c) are stress diagrams from the end of junior high school. Figure 4 From left to right, (a), (b), and (c) are dark-field wrapping diagrams from the end of junior high school.

[0078] After removing the crystal, observation of the crystal surface revealed the following:

[0079] 1) The crystal surface is smooth, free from defects such as cracks and microtubules.

[0080] 2) The crystal was cut and processed into 500-micrometer-thick SiC wafers. Stress (stress meter), resistivity (non-contact sheet resistance meter), and dark-field encapsulation (fully automated microscope) were tested on silicon carbide wafers from the early, middle, and late growth stages. The results are as follows:

[0081] Initial wafer: resistivity uniformity 0.86%, average stress across the entire aperture 2.43 MPa, 40 dark field wraps;

[0082] Mid-term wafer: resistivity uniformity 0.91%, average stress across the entire aperture 2.01 MPa, 41 dark field wrappers;

[0083] Final wafer: resistivity uniformity 0.98%, average stress across the entire aperture 1.9 MPa, 56 dark field wraps.

[0084] Please refer to Figure 5 and Figure 6 Heating is achieved through induction coil heating, using the existing technology of bottom ventilation in the furnace chamber, with graphite felt as the insulation medium. A 190mm 4H-SiC seed crystal is taken, with the C-side selected as the growth surface, and is bonded to the seed crystal holder of the silicon carbide growth device disclosed in the prior art using organic adhesive. The diameter of the seed crystal holder is 240mm, and it is connected to the graphite crucible by threads. The height of the graphite crucible is 230mm, and silicon carbide powder is placed in the lower middle part of the graphite crucible with a loading height of 160mm. After cleaning the furnace, maintain the pressure inside the graphite cylinder at 50 kPa. Start the induction coil to raise the temperature to 2100℃-2500℃ and hold for 3 hours. During the heating process, continuously introduce a large flow of argon gas at 300 sccm and maintain the pressure at 50 kPa. Then reduce the pressure to 700 Pa and maintain the temperature at 2100℃-2500℃. Introduce nitrogen gas at 16 sccm and hold for 200 hours to carry out the crystal growth process. After 200 hours of growth, turn off the nitrogen gas and stop heating. Keep the argon gas constant and maintain the pressure at 50 kPa until the temperature drops to room temperature. Then, purge the gas to atmospheric pressure and remove the crystal.

[0085] Observations on the crystal surface revealed:

[0086] 1) A few microtubules appear on the crystal surface;

[0087] 2) The crystal was cut and processed into 500-micrometer-thick SiC wafers. Stress (stress meter), resistivity (non-contact sheet resistance meter), and dark-field encapsulation (fully automated microscope) were tested on silicon carbide wafers from the early, middle, and late growth stages. The results are as follows:

[0088] Initial wafer: resistivity uniformity 6.42%, average stress across the entire aperture 5.13 MPa, 181 dark field wraps;

[0089] Mid-term wafer: resistivity uniformity 7.65%, average stress across the entire aperture 5.08 MPa, 306 dark field wraps;

[0090] Final wafer: resistivity uniformity 8.03%, average stress across the entire aperture 5.01 MPa, 720 dark field wrappers.

[0091] Finally, it should be noted that in this document, relational terms such as "first" and "second" are used only to distinguish one entity or operation from another, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Furthermore, the term "comprising" or any other variation thereof is intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that comprises a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such a process, method, article, or apparatus.

[0092] The various embodiments in this specification are described in a progressive manner, with each embodiment focusing on the differences from other embodiments. The same or similar parts between the various embodiments can be referred to each other.

[0093] The above description of the disclosed embodiments enables those skilled in the art to make or use the present invention. Various modifications to these embodiments will be readily apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention is not to be limited to the embodiments shown herein, but is to be accorded the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A silicon carbide crystal growth apparatus, characterized in that, include: The crucible is heated by an induction coil; A graphite cylinder is disposed inside the crucible, and there is a gap between the graphite cylinder and the crucible. The graphite cylinder is provided with a raw material area and a crystal growth area. The raw material area is used to place silicon carbide powder, and the crystal growth area is used for silicon carbide crystal growth. The side wall of the graphite cylinder is provided with through holes. A seed crystal holder is used to fix a silicon carbide seed crystal, and the seed crystal holder is connected to the top of the crucible and the graphite cylinder respectively; A gas passage assembly passes through the seed crystal holder, with one end of the gas passage assembly placed in the gap and the other end extending out of the crucible, for introducing inert gas and nitrogen into the gap. The inert gas and nitrogen can enter the graphite cylinder through the through hole.

2. The silicon carbide crystal growth apparatus according to claim 1, characterized in that, The flow rate of the inert gas introduced into the gap is 200 sccm-600 sccm, and the flow rate of the nitrogen gas introduced into the gap is 15 sccm-25 sccm.

3. The silicon carbide crystal growth apparatus according to claim 1, characterized in that, The seed crystal holder is threadedly connected to the crucible and the graphite cylinder, or snap-fitted together.

4. The silicon carbide crystal growth apparatus according to claim 1, characterized in that, The graphite cylinder and the crucible are detachably connected.

5. The silicon carbide crystal growth apparatus according to claim 1, characterized in that, The inner diameter of the graphite tube is R1, the outer diameter of the graphite tube is R2, and the diameter of the silicon carbide seed crystal is R3. 0.1mm≤R1-R3≤0.5mm, 10mm≤R2-R3≤80mm.

6. The silicon carbide crystal growth apparatus according to claim 5, characterized in that, The plurality of through holes are evenly arranged along the wall of the graphite cylinder, and the distances from the through holes to the bottom end face of the graphite cylinder are equal, and / or, The diameter of the through hole is 1mm-5mm.

7. The silicon carbide crystal growth apparatus according to claim 1, characterized in that, The length of the gas passage assembly extending into the crucible is L1, where 20mm ≤ L1 ≤ 50mm, and / or, The distance between the through hole and the surface of the seed crystal holder is L2, where 10mm ≤ L2 ≤ 100mm.

8. The silicon carbide crystal growth apparatus according to claim 1, characterized in that, The gas path assembly includes a first inlet pipe and a second inlet pipe, wherein the first inlet pipe is used to introduce nitrogen gas and the second inlet pipe is used to introduce the inert gas. The first air inlet pipe and the second air inlet pipe are at the same height from the bottom of the crucible.

9. The silicon carbide crystal growth apparatus according to claim 1, characterized in that, The seed crystal holder is also provided with mounting holes for mounting the gas path assembly and exhaust holes for the inert gas and the nitrogen flow. Both the mounting hole and the vent hole are provided corresponding to the gap, and there is a preset distance between the vent hole and the mounting hole.

10. The silicon carbide crystal growth apparatus according to claim 9, characterized in that, The number of exhaust holes is 1-3; The diameter of the exhaust port is 2mm-5mm.