A system for producing nylon 66 industrial yarn
By adding a humidity control component and improving the filter assembly in the nylon 66 industrial yarn production system, the problems of lint and fuzz were solved, product quality was improved, and the needs of demanding customers were met.
Patent Information
- Application Number
- CN202522810755.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Utility models(China)
- Current Assignee / Owner
- Filing Date
- 2025-12-30
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2035-12-30
AI Technical Summary
In existing nylon 66 industrial yarn production systems, the number of clumps and filaments in the finished industrial yarn is relatively high, leading to frequent yarn bundle jamming, affecting the full twist rate and operating efficiency, and causing uneven glue spots on the fabric surface, which cannot meet the high requirements of customers.
In the production system of nylon 66 industrial yarn, a moisture conditioning component is added to adjust the moisture content of the chips. By improving the filter assembly and setting baffles at the side blowing device, the cooling environment of the yarn bundle is optimized to ensure the uniformity of the nylon 66 melt and the purity of the nascent fibers, thereby reducing the generation of fuzz and clumps.
By adjusting the moisture content of the slices and optimizing the cooling environment, the number of clumps and filaments per 10,000 meters was reduced, the quality of industrial yarn was improved, and higher customer demands were met.
Smart Images

Figure CN225013693U_ABST
Abstract
Description
Technical Field
[0001] This utility model relates to the field of textile and chemical fiber production technology, specifically to a production system for nylon 66 industrial yarn. Background Technology
[0002] Nylon 66 fiber is a commonly used synthetic fiber with wicking effect and excellent softness, making it highly favored in the clothing industry, especially in the manufacture of outdoor sports equipment, such as sportswear for mountaineering, hiking and other outdoor activities. In addition, due to its excellent properties such as high strength, high abrasion resistance and fatigue resistance, nylon 66 fiber is also often used in the field of rubber product performance enhancement, such as tires and hoses.
[0003] However, while the industrial yarn produced by current nylon 66 industrial yarn production systems possesses a certain strength, the finished industrial yarn has a high number of clumps and filaments. During production, when large clumps or filaments are present in the yarn bundle, the yarn bundle is prone to jamming as it passes through the yarn path, causing single-spindle shutdowns and affecting the full-bore twisting rate and start-up efficiency. Simultaneously, existing looms often have appearance inspection systems; when the size of filaments or clumps on the yarn bundle exceeds a certain standard, the system triggers a shutdown mechanism, which reduces the loom's start-up efficiency to some extent. Furthermore, a large number of relatively small filaments or clumps on the fabric surface also affects the appearance of the dipped tire cord fabric, resulting in uneven adhesive spots on the fabric surface, failing to meet the higher requirements of customers. Summary of the Invention
[0004] This invention aims to solve the problem of high clump and fuzz content in existing nylon 66 industrial yarn production systems. It provides a new nylon 66 industrial yarn production system that produces nylon 66 industrial yarn with fewer fuzz and clumps, thereby improving the overall quality of the nylon 66 industrial yarn and meeting the needs of customers with higher requirements.
[0005] The technical solution of this utility model is: a production system for nylon 66 industrial yarn, comprising a solid-phase thickening reactor, a screw extruder, a spinning assembly, a side-blowing device, a tunnel, an oiling device, a drawing assembly, and a winding machine arranged sequentially; a humidity conditioning assembly is provided between the solid-phase thickening reactor and the screw extruder, the humidity conditioning assembly including a finished product silo, a liquid storage tank, and a heating assembly, the heating assembly being used to heat the liquid in the liquid storage tank to turn it into steam, an air inlet on one side of the top of the liquid storage tank and an air outlet on the top of the liquid storage tank, an air inlet at the bottom of the finished product silo and an air outlet at the top of the finished product silo, the air inlet being connected to a protective gas source through a pipe, and the air outlet being connected to the air inlet being connected to the air inlet being through a pipe; the protective gas in the gas source enters the liquid storage tank through the air inlet, and drives the steam inside the liquid storage tank into the interior of the finished product silo, where it flows from bottom to top, humidifying the nylon 66 chips.
[0006] Furthermore, a raw material silo, a displacement silo, and a buffer silo are sequentially arranged before the solid-phase thickening reactor. Nylon 66 raw material chips fall into the raw material silo through the inlet end. The outlet end of the raw material silo is connected to the inlet end of the displacement silo, the outlet end of the displacement silo is connected to the inlet end of the buffer silo, and the outlet end of the buffer silo is connected to the inlet end of the solid-phase thickening reactor. The displacement silo is used to replace the nylon 66 chips with nitrogen, and the buffer silo is used to collect the nylon 66 chips after nitrogen replacement, thereby ensuring that the nylon 66 chips can be continuously added to the solid-phase thickening reactor.
[0007] Furthermore, the moisture content of the nylon 66 chips after being conditioned by the humidification component is 600ppm to 1200ppm.
[0008] Furthermore, the heating component is a heating wire installed inside the liquid reservoir. The heating wire is connected to an external power source via a power supply cable. One end of the power supply cable is connected to the heating wire, and the other end passes through the liquid reservoir and is connected to the external power source.
[0009] Furthermore, the humidity control component also includes a protective gas recovery device, wherein the inlet of the protective gas recovery device is connected to the outlet of the finished product silo, and the outlet is connected to the inlet of the liquid storage tank, thereby improving the utilization rate of nitrogen.
[0010] Furthermore, the nylon 66 nascent fibers ejected from the spinning assembly are separated from each other by partitions.
[0011] Furthermore, one end of the partition is connected to the end of the spinning assembly and the other end is connected to the beginning of the passageway, and the width direction of the partition is consistent with the blowing direction of the side blowing device, thereby avoiding mutual influence of cold air between the nylon 66 nascent fiber bundles.
[0012] Furthermore, the spinning assembly is provided with at least one set of filter screen assemblies, and when the number of filter screen assemblies is greater than one set, the filtration accuracy of different sets of filter screen assemblies increases sequentially from top to bottom. The filter screen assembly includes metal sand layers, multi-layer metal filter screens, and metal fiber sintered felt layers that are distributed vertically at intervals.
[0013] Furthermore, the metal filter screen has at least five layers, and the filtration accuracy of the metal filter screen increases sequentially from top to bottom. In each group of filter screen components, the filtration accuracy of the metal fiber sintered felt layer is higher than that of the metal filter screen in that group. The filtration accuracy of the bottom metal filter screen in the last group of filter screen components is 300 mesh, and the filtration accuracy of the metal fiber sintered felt layer is 20 μm.
[0014] Furthermore, the drafting assembly includes a feed roller and a drafting roller. The oiled nylon 66 material is introduced onto the drafting roller through the feed roller, and the drafting roller includes at least four pairs of rollers.
[0015] The beneficial effects of this utility model through the above technical solution are as follows: The production system disclosed in this utility model can adjust the moisture content of the chips after solid-phase thickening by adding a humidity control component, thereby ensuring the uniformity and stability of the nylon 66 melt. In addition, by improving the filter screen component, impurity particles in the nylon 66 melt can be effectively intercepted, further ensuring the purity of the nascent nylon 66 fibers. Furthermore, by adding a baffle at the side-blowing air window to isolate the filament bundle, the cooling environment of the filament bundle is optimized, avoiding the generation of fuzz and clumps caused by filament bundle adhesion and disturbance. The combined effect is that the produced industrial yarn can maintain core properties such as breaking strength while reducing the number of clumps and fuzz per 10,000 meters, thus improving product quality. Attached Figure Description
[0016] Figure 1 This is a schematic diagram of the distribution of this utility model; Figure 2 This is a schematic diagram showing the distribution of the humidity regulating components in this utility model; Figure 3 This is a schematic diagram showing the distribution of the raw material silo, the replacement silo, and the buffer silo in this utility model; Figure 4 This is one of the schematic diagrams showing the installation position of the partition plate in this utility model; Figure 5 This is the second schematic diagram of the installation position of the partition plate in this utility model; Figure 6 This is a schematic diagram of the installation position of the filter assembly in this utility model; Figure 7 This is a schematic diagram of the filter assembly in this utility model.
[0017] The attached diagram is labeled as follows: 1. Solid phase thickening reactor, 101. Raw material silo, 102. Displacement silo, 103. Buffer silo; 2. Humidity control components; 201. Finished product silo; 202. Liquid storage tank; 203. Protective gas recovery device; 3. Screw extruder; 4. Spinning assembly; 5. Side blowing device; 6. Chute; 7. Oiling device; 8. Drafting assembly, 801. Feed roller, 802. Drafting roller; 9. Winding machine; 10. Partition plate; 11. Metal sand; 12. Metal filter screen; 13. Metal fiber sintered felt; 14. Pre-spinning silo. Detailed Implementation
[0018] The present invention will be further described below with reference to the accompanying drawings and specific embodiments: like Figure 1 and Figure 2 As shown, a production system for nylon 66 industrial yarn includes a solid-phase thickening reactor 1, a screw extruder 3, a spinning assembly 4, a side-blowing device 5, a tunnel 6, an oiling device 7, a drawing assembly 8, and a winding machine 9 arranged in sequence; a humidity regulating assembly 2 is provided between the solid-phase thickening reactor 1 and the screw extruder 3.
[0019] The solid-phase thickening reactor 1 is used to thicken nylon 66 raw material chips to obtain high-viscosity nylon 66 chips. The humidity conditioning component 2 is used to condition the high-viscosity nylon 66 chips to adjust their moisture content. The screw extruder 3 is used to melt and compress the moisture-conditioned high-viscosity nylon 66 chips to obtain nylon 66 melt. The nylon 66 melt is then fed into the spinning component 4 and sprayed out by the spinning component 4 to form nylon 66 nascent fibers. The side blowing device 5 and the channel 6 are used to cool the nylon 66 nascent fibers. The oiling device 7 is used to oil the nylon 66 nascent fibers. The drawing component 8 is used to stretch and shape the oiled nylon 66 nascent fibers. The winding machine 8 is used to wind the stretched and shaped nylon 66 nascent fibers to produce nylon 66 industrial yarn.
[0020] The humidity control component 2 includes a finished product silo 201, a liquid storage tank 202, and a heating component. The heating component is used to heat the liquid in the liquid storage tank 202 to turn it into steam. The liquid storage tank 202 has an air inlet on one side of its top and an air outlet on its top. The finished product silo 201 has an air inlet at its lower part and an air outlet at its top. The air inlet is connected to a protective gas source through a pipe, and the air outlet is connected to the air inlet through a pipe.
[0021] Specifically, the protective gas is nitrogen, and the liquid storage tank 202 stores water. The nitrogen enters the liquid storage tank 202 through the air inlet, thereby driving the water vapor inside the liquid storage tank 202 from the lower part of the finished product silo 201 into the interior of the finished product silo 201, and flowing from bottom to top inside the finished product silo 201 to humidify the nylon 66 chips.
[0022] In one possible implementation, the heating component is a heating wire disposed inside the liquid reservoir 202. The heating wire is connected to an external power source via a power supply cable. One end of the power supply cable is connected to the heating wire, and the other end passes through the liquid reservoir 202 and is connected to the external power source.
[0023] Specifically, other existing heating components can also be used to heat the liquid in the reservoir 202. When the water is heated and evaporated to form water vapor, it enters the lower part of the finished product silo 201 under the drive of nitrogen gas introduced into the upper part of the reservoir 202, and flows from bottom to top in the finished product silo 201. When the water vapor comes into contact with the high-viscosity nylon 66 chips, it will condense into water droplets on the high-viscosity nylon 66 chips to humidify them, thereby achieving the adjustment of the moisture content of the high-viscosity nylon 66 chips.
[0024] Specifically, by controlling the residence time of the high-viscosity nylon 66 chips in the finished product silo 201, the moisture content of the high-viscosity nylon 66 chips can be adjusted. A residence time of 4-8 hours in the finished product silo results in a moisture content of 600-1200 ppm for the nylon 66 material after moisture conditioning by the moisture conditioning component 2. When the high-viscosity nylon 66 chips remain in the finished product silo 10 for 4 hours, their moisture content can reach 600-800 ppm; when they remain in the finished product silo 10 for 6 hours, their moisture content can reach 800-1000 ppm; and when they remain in the finished product silo 10 for 8 hours, their moisture content can reach 1000-1200 ppm.
[0025] As one possible implementation method, such as Figure 2 As shown, the humidity control component 2 also includes a protective gas recovery device 203, which can be an existing nitrogen recovery device. The inlet of the protective gas recovery device 203 is connected to the outlet of the finished product silo 201, and the outlet is connected to the inlet of the liquid storage tank 202, so as to recover the nitrogen discharged from the finished product silo 201 and reintroduce it into the liquid storage tank 202 through the inlet, thereby improving the utilization rate of nitrogen.
[0026] Specifically, the outlet of the protective gas recovery device 203 is connected to a pipe connecting the gas source and the inlet of the liquid storage tank 202. Valves are installed on both the outlet of the protective gas recovery device 203 and the pipe connecting the gas source and the inlet of the liquid storage tank 202. In use, nitrogen is first introduced into the liquid storage tank 202 from the gas source. Simultaneously, the protective gas recovery device 203 operates. Specifically, the amount of nitrogen introduced can be adjusted according to the size of the finished product silo 201. In this embodiment, 6 kg of nitrogen is introduced. After the nitrogen has largely covered the finished product silo 201, the valve at the gas source is closed, and the nitrogen is reused through the protective gas recovery device 203. To ensure that more water vapor can remain in the finished product silo 201, a condensing plate or existing condensing structure can be installed on the top of the finished product silo 201. When water vapor flows to the top of the finished product silo 201, it condenses into water droplets on the condensing plate or existing condensing structure, thus retaining more water vapor in the finished product silo 201.
[0027] As one possible implementation method, such as Figure 3 As shown, a raw material silo 101, a displacement silo 102, and a buffer silo 103 are sequentially arranged before the solid-phase thickening reactor 1. Nylon 66 raw material chips fall into the raw material silo 101 from the feed end. The discharge end of the raw material silo 101 is connected to the feed end of the displacement silo 102. The discharge end of the displacement silo 102 is connected to the feed end of the buffer silo 103. The discharge end of the buffer silo 103 is connected to the feed end of the solid-phase thickening reactor 1. The displacement silo 102 is used to replace the nylon 66 material with nitrogen, and the buffer silo 103 is used to collect the nylon 66 material, thereby ensuring that the nylon 66 material can be continuously added to the reactor 104.
[0028] Specifically, nylon 66 raw material chips with a formic acid relative viscosity of 37-45 are placed in the raw material silo 101. When the chips need to be thickened, they are first sent to the replacement silo 102 for nitrogen replacement. After nitrogen replacement, the chips fall into the buffer silo 103 and are then put into the solid phase thickening reactor 104. The chips are held at a temperature of 140℃-160℃ for 16h-24h to thicken them, so that the formic acid relative viscosity of the high-viscosity nylon 66 chips is 75-93. The formic acid relative viscosity refers to the relative viscosity of the high-viscosity nylon 66 chips measured in a 90% concentration formic acid solution, thus completing the thickening treatment.
[0029] As one possible implementation method, such as Figure 4 and Figure 5 As shown, the nylon 66 nascent fibers ejected from the spinning assembly 4 are separated from each other by a partition 10. The side blowing device 5 has a blowing temperature of 16℃~18℃, a wind speed of 0.5m / s~1.2m / s, and a wind humidity of 60%~80%.
[0030] As one possible implementation, one end of the partition 10 is connected to the end of the spinning assembly 4 and the other end is connected to the beginning of the passageway 6, and the width direction of the partition 10 is consistent with the blowing direction of the side blowing device 5, thereby avoiding mutual influence of cold air between the nylon 66 nascent fiber bundles.
[0031] As one possible implementation method, such as Figure 6 and Figure 7 As shown, the spinning assembly 4 may be provided with at least one set of filter screen assemblies. Each set of filter screen assemblies includes a metal sand layer 11, a multi-layer metal filter screen 12, and a metal fiber sintered felt layer 13 that are distributed vertically at intervals. When the number of filter screen assemblies is greater than one set, the filtration accuracy of different sets of filter screen assemblies increases sequentially from top to bottom.
[0032] As one possible implementation, the metal filter 12 has at least five layers, and the filtration accuracy of the metal filter 12 increases sequentially from top to bottom. In each group of filter components, the filtration accuracy of the metal fiber sintered felt layer 13 is higher than that of the metal filter 12 in that group.
[0033] In this embodiment, the metal filter 12 has five layers, such as... Figure 7 As shown, from top to bottom, the filtration accuracies of the metal filter 12 in the last filter assembly are 50 mesh, 100 mesh, 150 mesh, 200 mesh, and 300 mesh, respectively, and the filtration accuracies of the metal fiber sintered felt layer 13 in the last filter assembly are 20 μm. Since the metal fiber sintered felt layer 13 is relatively soft, an additional metal mesh can be set below it to support the metal fiber sintered felt layer 13. In this embodiment, the filtration accuracies of the metal mesh are 350 mesh.
[0034] Specifically, the high-viscosity nylon 66 chips, after being conditioned, are first fed into the pre-spinning silo 14, and then fed into the screw extruder 3 via the pre-spinning silo 14 for melt compression to obtain nylon 66 melt; by setting the pre-spinning silo 14, the feeding pressure of the screw extruder 3 can be ensured to be stable.
[0035] In one possible implementation, the drafting assembly 8 includes a feed roller 801 and a drafting roller 802. The nascent nylon 66 fibers after oiling are first bundled through a guide and then pre-networked to increase the tension of the nylon 66 nascent fiber bundles. Then, the bundles are introduced onto the drafting roller 802 through the feed roller 801. The feed roller 801 only serves a feeding function and is not heated. The drafting roller 802 includes at least four pairs of rollers, and existing guides and pre-networkers in the art can be used.
[0036] Specifically, when the stretching roller 802 consists of four pairs of rollers, from bottom to top, the first three pairs of rollers perform the stretching function, and the last pair of rollers performs the shaping function. The temperature of the first pair of rollers is 55℃~65℃, the temperature of the second pair of rollers is 185℃~210℃, the temperature of the third pair of rollers is 205℃~245℃, and the temperature of the fourth pair of rollers is 130℃~240℃.
[0037] Specifically, when the stretching roller 802 has 5 pairs of rollers, the first three pairs of rollers play a stretching role, and the last two pairs of rollers play a shaping role. The temperature of the first pair of rollers is 55℃~65℃, the temperature of the second pair of rollers is 185℃~210℃, the temperature of the third pair of rollers is 205℃~245℃, the temperature of the fourth pair of rollers is 180℃~215℃, and the temperature of the fifth pair of rollers is 130℃~180℃.
[0038] Specifically, the nascent nylon 66 fibers that have been stretched and shaped by the stretching assembly 8 are first processed by a networker, which can be an existing networker in the art, to produce high-quality nylon 66 industrial yarn. The industrial yarn is then fed to the winding machine 8 for winding, and finally wound into a yarn bobbin, thus completing the production of high-quality nylon 66 industrial yarn.
[0039] Specifically, the production system disclosed in this utility model produces high-quality nylon 66 industrial yarn with a breaking strength of 9.7 g / D to 11.0 g / D, a breaking elongation of 15.9% to 20.2%, a dry heat shrinkage rate of 3.5% to 8.1%, a clump count of 0.05 to 0.10 per 10,000 meters, and a filament count of 0.5 to 1.61 per 10,000 meters.
[0040] In this utility model, when in use: First, nylon 66 raw material chips are fed into a solid-phase viscosity-enhancing reactor 104 for viscosity-enhancing treatment to obtain high-viscosity nylon 66 chips. Then, the high-viscosity nylon 66 chips are fed into a humidity-conditioning component 2 for humidity-conditioning treatment to adjust their moisture content. Next, the humidity-conditioning high-viscosity nylon 66 chips are fed into a screw extruder 3 for melt compression to obtain nylon 66 melt. Then, the nylon 66 melt is quantitatively fed into a spinning component 4 and sprayed out through the spinning component 4 to form nylon 66 nascent fibers. Next, the nylon 66 nascent fibers are cooled sequentially through a side-blowing device 5 and a channel 6. Then, the cooled nylon 66 nascent fibers are oiled through an oiling device 7. Next, the oiled nylon 66 nascent fibers are fed into a drawing component 8 for stretching and shaping treatment. Finally, the stretched and shaped nylon 66 nascent fibers are conveyed to a winding machine 9 for winding to finally obtain nylon 66 industrial yarn.
[0041] Specifically, the application examples of the above production system are as follows: The total draw ratio refers to the ratio between the speed of the last pair of draw rolls and the speed of the first pair of draw rolls. The relaxation ratio is the ratio between the speed of the last pair of relaxation rolls and the speed of the last pair of draft rolls. The winding ratio is the ratio between the winding speed and the speed of the last pair of relaxation rolls; The number of tufts per 10,000 meters refers to the number of tufts within 10,000 meters of industrial yarn. The number of fibers per 10,000 meters refers to the number of fibers within 10,000 meters of industrial yarn.
[0042] The nylon 66 industrial yarn produced in Examples 1-4 is 1400 dtex industrial yarn. During production, the drawing rollers 802 consist of four pairs of rollers. From bottom to top, the first three pairs of rollers perform the drawing function, and the last pair performs the shaping function. The temperature of the first pair of rollers (referred to as 1G) is 55℃-65℃, the temperature of the second pair of rollers (referred to as 2G) is 185℃-210℃, the temperature of the third pair of rollers (referred to as 3G) is 205℃-245℃, and the temperature of the fourth pair of rollers (referred to as 4G) is 130℃-240℃. The specific parameter settings for each example are shown in Table 1. The nylon 66 industrial yarn produced in Comparative Examples 1 to 4 is 1400 dtex industrial yarn. The specific parameter settings for each comparative example are shown in Table 1.
[0043] Table 1. Specific parameters of Examples 1-4 and Comparative Examples 1-4, and the corresponding industrial yarn properties. As can be seen from Table 1, when the drawing roller 802 has 4 pairs of rollers during the production process, the nylon 66 industrial yarn produced by the production system of this utility model maintains key properties such as breaking strength and breaking elongation, while significantly reducing the number of clumps and filaments per 10,000 meters, thereby improving the quality of the product.
[0044] In the description of this utility model, it should be understood that the terms "upper", "lower", "front", "rear", "left", "right", "top", "bottom", "inner", "outer", etc., indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings. They are only for the convenience of describing this utility model and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, they should not be construed as limitations on this utility model.
[0045] The preferred embodiments of the present invention have been described in detail above with reference to the accompanying drawings. However, the present invention is not limited to the above embodiments. Any equivalent or equivalent modifications or substitutions to the technical solutions of the present invention without departing from the spirit of the present invention or the scope of disclosure shall fall within the protection scope of the present invention.
Claims
1. A production system for nylon 66 industrial yarn, comprising a solid-phase thickening reactor (1), a screw extruder (3), a spinning assembly (4), a side-blowing device (5), a duct (6), an oiling device (7), a drawing assembly (8), and a winding machine (9) arranged sequentially; characterized in that, A humidity conditioning component (2) is provided between the solid phase thickening reactor (1) and the screw extruder (3). The humidity conditioning component (2) includes a finished product silo (201), a liquid storage tank (202), and a heating component. The heating component is used to heat the liquid in the liquid storage tank (202) to make it into steam. The liquid storage tank (202) has an air inlet on one side of its top and an air outlet on its top. The finished product silo (201) has an air inlet at its lower part and an air outlet at its top. The air inlet is connected to the protective gas source through a pipe, and the air outlet is connected to the air inlet through a pipe.
2. The nylon 66 industrial yarn production system according to claim 1, characterized in that, Before the solid phase thickening reactor (1), there are also a raw material silo (101), a displacement silo (102) and a buffer silo (103) arranged in sequence. Nylon 66 raw material chips fall into the raw material silo (101) through the feed end. The discharge end of the raw material silo (101) is connected to the feed end of the replacement silo (102). The discharge end of the replacement silo (102) is connected to the feed end of the buffer silo (103). The discharge end of the buffer silo (103) is connected to the feed end of the solid phase thickening reactor (1).
3. The nylon 66 industrial yarn production system according to claim 1, characterized in that, The moisture content of the nylon 66 chips after the moisture conditioning component (2) is 600ppm to 1200ppm.
4. The nylon 66 industrial yarn production system according to claim 1, characterized in that, The heating component is a heating wire installed inside the reservoir (202). The heating wire is connected to an external power source via a power supply cable. One end of the power supply cable is connected to the heating wire, and the other end passes through the reservoir (202) and is connected to the external power source.
5. The nylon 66 industrial yarn production system according to claim 1, characterized in that, The humidity control component (2) also includes a protective gas recovery device (203), the air inlet of which is connected to the air outlet of the finished product silo (201), and the air outlet is connected to the air inlet of the liquid storage device (202).
6. The nylon 66 industrial yarn production system according to claim 1, characterized in that, The nylon 66 nascent fibers ejected by the spinning assembly (4) are separated from each other by a partition (10).
7. The nylon 66 industrial yarn production system according to claim 6, characterized in that, One end of the partition (10) is connected to the end of the spinning assembly (4), and the other end is connected to the beginning of the passage (6). The width direction of the partition (10) is consistent with the blowing direction of the side blowing device (5).
8. The nylon 66 industrial yarn production system according to claim 1, characterized in that, The spinning assembly (4) is provided with at least one set of filter screen assemblies. When the number of filter screen assemblies is greater than one set, the filtration accuracy of different sets of filter screen assemblies increases from top to bottom. The filter screen assembly includes a metal sand layer (11) with intervals between the upper and lower parts, a multi-layer metal filter screen (12), and a metal fiber sintered felt layer (13).
9. The nylon 66 industrial yarn production system according to claim 8, characterized in that, The metal filter (12) has at least five layers, and the filtration accuracy of the metal filter (12) increases sequentially from top to bottom. The filtration accuracy of the metal fiber sintered felt layer (13) in each group of filter components is higher than that of the metal filter (12) in that group. The filtration accuracy of the bottom metal filter (12) in the last group of filter components is 300 mesh, and the filtration accuracy of the metal fiber sintered felt layer (13) is 20 μm.
10. A production system for nylon 66 industrial yarn according to claim 1, characterized in that, The drafting assembly (8) includes a feed roller (801) and a drafting roller (802). The oiled nylon 66 nascent fiber is introduced onto the drafting roller (802) through the feed roller (801). The drafting roller (802) includes at least four pairs of rollers.