A laminated material structure, a laminated material prepreg and a laminated material composite structure

By using a flexible fiber unit weaving structure and a laminated material design bonded with polymers, the problems of high cost and insufficient performance of plant fiber prepregs have been solved, enabling the low-cost production and application of high-performance fiber materials.

CN225013875UActive Publication Date: 2026-11-24FENSHIPU CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202522543488.9
Authority / Receiving Office
CN · China
Patent Type
Utility models(China)
Current Assignee / Owner
Priority Date
2025-03-21
Filing Date
2025-11-28
Publication Date
2026-11-24
Estimated Expiration
2035-11-28

AI Technical Summary

Technical Problem

Plant fiber prepregs have high production costs and insufficient performance, which limits their market promotion. Furthermore, there are challenges in applying the laminated structure of high-performance fiber materials.

Method used

The flexible fiber unit weaving structure within the flexible fiber layer forms a laminated material structure that combines flexibility and rigidity. The production process is simplified by bonding with a polymer layer.

Benefits of technology

It improves the flexibility and mechanical properties of prepregs, simplifies the production process, and reduces costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN225013875U_ABST
    Figure CN225013875U_ABST
Patent Text Reader

Abstract

This invention provides a laminated material structure, a laminated material prepreg, and a laminated material composite structure. The laminated material structure includes at least one flexible fiber layer, and any flexible fiber layer includes at least two strip-shaped flexible fiber units. The flexible fiber units are woven together to form a woven structure, thereby enabling the industrial production of fiber laminated material structures with high performance and strength, as well as corresponding prepregs and composite structures.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This utility model relates to the field of composite materials, and more specifically, to a laminated material structure, a laminated material prepreg, and a laminated material composite structure. Background Technology

[0002] The plant fiber prepreg market is one of the emerging markets in the composite materials field. With the increasing demand for sustainable materials and growing environmental awareness, the application of plant fiber prepregs in various industries is receiving increasing attention. However, compared with traditional synthetic fibers, the production cost of plant fiber prepregs remains high, and their performance is not as advantageous as that of man-made fibers, affecting market promotion. One of the main reasons is that natural plant fibers, especially high-performance bast fibers, are short fibers (centimeter-level). Producing continuous (several meters or even longer) plant fiber prepregs requires a complex production process. For example, the production process of currently high-performance bast fiber prepregs includes: harvesting, retting, breaking, scutching, hacking, modification, drying, laying and arranging, and resin impregnation. The production process involves several mechanical actions, inevitably causing damage to fiber strength. Furthermore, the numerous steps contribute to the high cost.

[0003] Even if the aforementioned technical problems are overcome and high-performance, high-strength fiber material laminates can be industrially produced, how to apply them will still be a new technical challenge in the industry. Utility Model Content

[0004] To address the problems in the aforementioned technologies, this utility model provides a laminated material structure, a laminated material prepreg, and a laminated material composite structure. Through the weaving structure of flexible fiber units within the flexible fiber layer, a prepreg that combines flexibility and rigidity is achieved.

[0005] This utility model provides a laminated material structure, including: At least one flexible fiber layer, the thickness of any flexible fiber layer is less than or equal to 0.25 mm, and the thickness of the laminated material structure is less than or equal to 0.5 mm; Any flexible fiber layer includes at least two strip-shaped flexible fiber units that are interwoven to form a woven structure.

[0006] Preferably, at least one surface of the flexible fiber unit or flexible fiber layer is attached with a polymer layer.

[0007] Preferably, any flexible fiber unit is wood fiber or wood paper.

[0008] Preferably, the tensile strength of the flexible fiber unit is 150-1000 MPa.

[0009] Preferably, the fiber extension directions of any two adjacent flexible fiber units are parallel or perpendicular.

[0010] This utility model also discloses a laminated material structure, including: At least one flexible fiber layer, with a sag of 0.5-50cm for the laminated material structure; Any flexible fiber layer includes at least two strip-shaped flexible fiber units that are interwoven to form a woven structure.

[0011] Preferably, at least one surface of the flexible fiber unit or flexible fiber layer is attached with a polymer layer.

[0012] Preferably, any flexible fiber unit is wood fiber or wood paper.

[0013] Preferably, the tensile strength of the flexible fiber unit is 150-1000 MPa.

[0014] Preferably, the fiber extension directions of any two adjacent flexible fiber units are parallel or perpendicular.

[0015] This utility model also discloses a laminated material structure, including: At least one flexible fiber layer, any flexible fiber layer includes at least two strip-shaped flexible fiber units, the flexible fiber units are woven together to form a woven structure; The tensile strength of the flexible fiber unit is 150-1000 MPa.

[0016] Preferably, at least one surface of the flexible fiber unit or flexible fiber layer is attached with a polymer layer.

[0017] Preferably, any flexible fiber unit is made of wood fiber or wood paper.

[0018] Preferably, the fiber extension directions of any two adjacent flexible fiber units are parallel or perpendicular.

[0019] This utility model also discloses a laminated material prepreg, comprising the laminated material structure as described above, wherein one or both sides of the laminated material structure are coated with a polymer layer.

[0020] This utility model also discloses a laminated material composite structure, including the laminated material structure as described above or the laminated material prepreg as described above, wherein adjacent laminated material structures are bonded together by a polymer.

[0021] The woven material made using the layered material structure proposed in this invention, combined with the weaving molding process, improves the flexibility and mechanical properties of prepregs made using the unidirectional layered material structure. The entire manufacturing process is simple and requires no complex operating equipment such as vacuum or pressurization. Attached Figure Description

[0022] Other features, objects, and advantages of this invention will become more apparent from the following detailed description of non-limiting embodiments with reference to the accompanying drawings.

[0023] Figure 1 This is a schematic diagram of a layered material structure according to an embodiment of the present invention. Detailed Implementation

[0024] Exemplary embodiments will now be described more fully with reference to the accompanying drawings. However, these exemplary embodiments can be implemented in many forms and should not be construed as limited to the embodiments set forth herein. Rather, these embodiments are provided so that this invention will be comprehensive and complete, and will fully convey the concept of the exemplary embodiments to those skilled in the art. The same reference numerals in the drawings denote the same or similar structures, and therefore repeated descriptions of them will be omitted. The directions described in this patent, such as up, down, lateral, and longitudinal, are descriptions of the relative positional relationships between components and do not limit the actual directions, nor are they intended to limit the scope of the claims.

[0025] See Figure 1 This diagram illustrates a structural schematic of a laminated material structure conforming to a preferred embodiment of the present invention. In this embodiment, the laminated material structure includes at least one flexible fiber layer. The flexible fiber layer can have unidirectional or bidirectional flexibility, giving the laminated material structure overall unidirectional or bidirectional flexibility. When multiple flexible fiber layers are used, the multiple flexible fiber layers are stacked and pressed together to form the laminated material structure (or woven). To ensure the flexibility, ductility, and stress resistance of the laminated material structure, each flexible fiber layer is configured such that at least one flexible fiber layer has a thickness less than or equal to 0.25 mm. When the number of flexible fiber layers is large, regardless of the number of layers selected, the total thickness of the final laminated material structure is less than or equal to 0.5 mm. With the above configuration, the total thickness of the laminated material structure is controllable. When the flexible fiber layer is controllable, the flexibility of the laminated material structure can be guaranteed at this thickness. When the width of the flexible fiber layer is 15 mm, the bending stiffness of the flexible fiber layer is 3000 N / mm. 2 At the same time, the layered material structure also has a certain degree of ductility, which can adapt to multiple application scenarios.

[0026] Furthermore, any flexible fiber layer includes at least two strip-shaped flexible fiber units, which are woven together to form a braided structure. That is, adjacent layers of flexible fiber units overlap vertically. For example, in two adjacent layers, the first layer is arranged side-by-side in one direction, and then a second layer of flexible fiber units is inserted into the first layer in an interlacing manner, with the insertion occurring above the preceding flexible fiber unit and below the following flexible fiber unit in a cyclical pattern. The other flexible fiber unit adjacent to this interlaced flexible fiber unit is inserted in a cyclical pattern, below the same preceding flexible fiber unit and above the same following flexible fiber unit, thus forming a braided structure. It can be understood that the woven single-layer flexible fiber layers can form a laminated material structure, or multiple woven flexible fiber layers can be stacked vertically to form a laminated material structure. With this laminated material structure, its axial stress resistance is stronger, and the gaps between adjacent flexible fiber units provide more bending space, offering higher flexibility to the laminated material structure.

[0027] In a preferred embodiment, the number of flexible fiber layers is greater than or equal to two, and the shapes of any flexible fiber layers may be the same or different. For example, the single-layer shape of all flexible fiber layers can be rectangular, making the shape of the laminated material structure rectangular, which can be applied to the surface of objects with regular shapes; for example, the single-layer shape of odd-numbered flexible fiber layers is rectangular, and the single-layer shape of even-numbered flexible fiber layers is spaced strips (i.e., within the spaced area, some positions have flexible fiber layers and some positions do not), making the thickness of the entire laminated material structure uneven (or staggered and uniform); as another example, the flexible fiber layers are circular, and in the axial direction, the radius of the flexible fiber layers gradually decreases or gradually increases, so that even with the same shape, the projected area covered by each flexible fiber layer is different, and the thickness of the laminated material structure is also uneven, in order to meet more application scenarios.

[0028] The flexible fiber layer can be a discontinuous, segmented layer, formed by arranging strip-shaped flexible fiber units side by side. When the above-mentioned flexible fiber layer is present, the number of flexible fiber layers can be greater than or equal to 2 layers. The arrangement direction of the flexible fiber units in each flexible fiber layer can be all the same, all different, or partially the same and partially different, depending on the application scenario and flexibility requirements.

[0029] Once the aforementioned flexible fiber layer is formed, it can be used alone as a laminated material structure. In applications requiring greater thickness, two or more woven flexible units can be stacked vertically to form a laminated material structure. For example, a polymer layer, such as a resin layer or PA layer, can be bonded between adjacent flexible fiber layers. This serves two purposes: fixing the structure and increasing flexibility and stress resistance. Alternatively, a polymer layer can be coated on one surface of the flexible fiber unit to facilitate weaving with other flexible fiber units. The resulting flexible fiber layer will then contain its own polymer.

[0030] In a preferred embodiment, any flexible fiber unit is wood fiber or wood paper.

[0031] In a preferred embodiment, the fiber extension directions of any two adjacent flexible fiber layers or flexible fiber units are parallel or perpendicular. It is understood that the more parallel the fiber extension directions in a given direction, the better the flexibility and bending ability in the direction perpendicular to that parallel direction. Furthermore, if the number of fibers arranged in the direction parallel to the fiber extension directions is approximately the same as the number arranged in the direction perpendicular to the fiber extension directions, then approximately the same flexibility and bending ability will be achieved in all directions.

[0032] In a preferred embodiment, the tensile strength of the flexible fiber unit is 150-1000 MPa.

[0033] This utility model also discloses a laminated material structure, including: at least one flexible fiber layer, the drape of the laminated material structure being 0.5-50cm (or the drape of any flexible fiber layer being 0.5-50cm); any flexible fiber layer including at least two strip-shaped flexible fiber units, the flexible fiber units being woven together to form a woven structure.

[0034] In a preferred embodiment, the number of flexible fiber layers is greater than or equal to 2.

[0035] In a preferred embodiment, at least one surface of the flexible fiber unit or flexible fiber layer is attached with a polymer layer.

[0036] In a preferred embodiment, any flexible fiber unit is wood fiber or wood paper.

[0037] In a preferred embodiment, the tensile strength of the flexible fiber unit is 150-1000 MPa.

[0038] This utility model also discloses a laminated material structure, including: at least one flexible fiber layer, any flexible fiber layer including at least two strip-shaped flexible fiber units, the flexible fiber units being woven together to form a woven structure; the tensile strength of the flexible fiber unit is 150-1000MPa.

[0039] In a preferred embodiment, the number of flexible fiber layers is greater than or equal to 2.

[0040] In a preferred embodiment, at least one surface of the flexible fiber unit is coated with a polymer layer.

[0041] In a preferred embodiment, any flexible fiber layer is made of wood fiber or wood paper.

[0042] In a preferred embodiment, the fiber extension directions of any two adjacent flexible fiber layers are parallel or perpendicular.

[0043] Those skilled in the art will understand that in any of the above embodiments, there are many ways to weave the flexible fiber units of any two adjacent layers, such as plain weave, twill weave, etc., and this utility model does not limit the weaving method.

[0044] This utility model also discloses a laminated material prepreg, including the laminated material structure as described above, wherein one or both sides of the laminated material structure are covered with a resin layer, and a polymer layer is also covered outside the resin layer, for example, by using a coating process, that is, coating the laminated material structure with a resin layer or directly coating it.

[0045] Preferably, an epoxy layer or a polyamide resin layer is provided between the laminated material structure and the resin layer, that is, an epoxy layer or a polyamide resin layer is coated before the resin layer is coated or the film is directly deposited.

[0046] This utility model also discloses a laminated material composite structure, including the laminated material structure as described above or the laminated material prepreg as described above, wherein adjacent laminated material structures are bonded together by a polymer.

[0047] It is understood that after the laminated material prepreg and / or laminated material composite structure in the above embodiments are prepared, their drape is also 0.5-50cm.

[0048] The following experimental process verifies various physical data of the laminated material structure.

[0049] - Flexibility The sag (sag length) constraint is 1-50 cm (at room temperature) as measured by ASTM D1388.

[0050] ASTM D1388 Description: A flexible fiber layer is cut into strips 25 cm wide. The ejection length is recorded when the front end of the strip droops under its own weight and contacts a ramp at a 41.5° angle to the platform. This length directly reflects the bending stiffness of the flexible fiber layer: a longer ejection length results in a stiffer fabric; a shorter ejection length results in a softer fabric. In the two embodiments of this invention, the ejection lengths are 8.35 cm and 22.7 cm, respectively.

[0051] It is understandable that the higher the resin content in the flexible fiber layer, the greater the stiffness of the resin at room temperature, the worse the flexibility of the laminated material structure with flexible fiber layers, and the longer the corresponding overhang length.

[0052] For epoxy resins that are not cured at room temperature, due to their softness, and PA (polyamide resin, a polymer containing amide groups (-CO-NH-) in its molecule) which has high stiffness at room temperature, the results of different ejection lengths in the examples show that, overall, the ejection length of PA is higher than that of epoxy prepreg. Furthermore, under the same conditions, the sparser the flexible fiber layer fabric and the better its flexibility, the shorter the ejection length; conversely, the thinner the flexible fiber layer and the smaller the sag of the laminated material structure, the shorter the ejection length.

[0053] - Mechanical properties A board is made by using a flexible fiber layer as a prepreg fabric under a pressure of 0.8 MPa, and then cut into bending test specimens according to ISO standards to measure the bending properties of the test specimens (instead of directly stretching the fabric to measure the properties).

[0054] The range of flexural properties includes: flexural strength: 100MPa-400MPa, flexural modulus: 8-30GPa. It is understood that flexural properties depend on the properties of the flexible fiber layer and the resin, with the properties of the flexible fiber layer having the greatest impact. Generally, epoxy resins perform better than PA resins. In the following examples, the properties of the flexible fiber layer are: tensile modulus approximately 50GPa; tensile strength approximately 450MPa.

[0055]

[0056] Table 1 shows the physical properties of a flexible fiber layer using PA in one embodiment.

[0057] Table 2 shows the physical properties of a flexible fiber layer using epoxy in Example 1. The implementation case test details include: all samples were selected from 4mm wide flexible fiber layers; all samples underwent a hot-pressing process followed by cutting and bending the specimens; and all samples were made of PA (a typical thermoplastic material).

[0058] Example 1: Thermoplastic Prepreg Raw materials: One-way wood veneer, approximately 0.1mm thick and 20cm wide, double-sided coated with PA (PA thickness approximately 0.015mm), then cut into 5mm wide strips, woven into fabric, and cut into 5 layers. These layers are placed in appropriate molds, molded, and then placed on a hot press. After molding and heating to 130℃, pressure is applied at 0.8MPa for 15 minutes. The temperature is then lowered to below 60℃ before demolding. Burrs and edges are removed, and the phone case weighs 0.72-0.75mm and has a thickness of 13.28g. For the same thickness and dimensions, the corresponding weight would be: 45# steel weighs 62.9g; 6061 aluminum weighs 21.7g; fiberglass composite material weighs 15.0g. It is evident that the laminated material under the woven structure in this invention is the lightest.

[0059] The test results for mechanical properties are as follows:

[0060] Table 3 shows the average bending performance measured under different conditions. Example 2: Thermosetting Prepreg Raw materials: Unidirectional wood veneer, approximately 0.1 mm thick and 20 cm wide, is coated on both sides with epoxy resin (approximately 0.03 mm thick on one side). It is then cut into narrow strips of 5 mm, 2 mm, and 10 mm wide, and woven into a plain weave fabric. The resulting fabric is then stacked and placed on a hot press, subjected to a pressure of 0.8 MPa, and held at 150°C for 30 minutes. The board is then removed, and samples are prepared according to the bending specimen dimensions required by ISO standards. Bending performance is tested according to ISO 14125 requirements.

[0061]

[0062] Table 4 shows the average bending performance measured under different conditions. The above description, in conjunction with specific preferred embodiments, provides a further detailed explanation of the present invention. It should not be construed that the specific implementation of the present invention is limited to these descriptions. For those skilled in the art, various simple deductions or substitutions can be made without departing from the concept of the present invention, and all such modifications and substitutions should be considered within the protection scope of the present invention.

Claims

1. A layered material structure, characterized in that, include: At least one flexible fiber layer, wherein the thickness of any of the flexible fiber layers is less than or equal to 0.25 mm, and the thickness of the laminated material structure is less than or equal to 0.5 mm; Any of the flexible fiber layers includes at least two strip-shaped flexible fiber units, which are interwoven to form a woven structure.

2. The laminated material structure as described in claim 1, characterized in that, At least one surface of the flexible fiber unit or flexible fiber layer is attached with a polymer layer.

3. The laminated material structure as described in claim 1, characterized in that, Any of the flexible fiber units can be wood fiber or wood paper.

4. The laminated material structure as described in claim 3, characterized in that, The tensile strength of the flexible fiber unit is 150-1000 MPa.

5. The laminated material structure as described in claim 1, characterized in that, The fiber extension directions of any two adjacent flexible fiber units are parallel or perpendicular.

6. A layered material structure, characterized in that, include: At least one flexible fiber layer, wherein the sag of the laminated material structure is 0.5-50cm; Any of the flexible fiber layers includes at least two strip-shaped flexible fiber units, which are interwoven to form a woven structure.

7. The laminated material structure as described in claim 6, characterized in that, At least one surface of the flexible fiber unit or flexible fiber layer is attached with a polymer layer.

8. The laminated material structure as described in claim 6, characterized in that, Any of the flexible fiber units can be wood fiber or wood paper.

9. The laminated material structure as described in claim 8, characterized in that, The tensile strength of the flexible fiber unit is 150-1000 MPa.

10. The laminated material structure as described in claim 7, characterized in that, The fiber extension directions of any two adjacent flexible fiber units are parallel or perpendicular.

11. A layered material structure, characterized in that, include: At least one flexible fiber layer, wherein any flexible fiber layer comprises at least two strip-shaped flexible fiber units, which are woven together to form a woven structure; The tensile strength of the flexible fiber unit is 150-1000 MPa.

12. The laminated material structure as described in claim 11, characterized in that, At least one surface of the flexible fiber unit or flexible fiber layer is attached with a polymer layer.

13. The laminated material structure as described in claim 11, characterized in that, Any of the flexible fiber units is made of wood fiber or wood paper.

14. The laminated material structure as described in claim 13, characterized in that, The fiber extension directions of any two adjacent flexible fiber units are parallel or perpendicular.

15. A laminated material prepreg, characterized in that, Includes the laminated material structure as described in any one of claims 1-14, wherein one or both sides of the laminated material structure are covered with a polymer layer.

16. A composite structure of laminated materials, characterized in that, Includes the laminated material structure as described in any one of claims 1-14 or the laminated material prepreg as described in claim 15, wherein adjacent laminated material structures are bonded together by a polymer.