High performance hud freeform mirror

By employing a multi-layer film structure on the HUD reflector, the problems of low reflectivity and poor stability under extreme environments were solved, achieving high reflectivity and corrosion resistance in the high-performance HUD reflector.

CN225018472UActive Publication Date: 2026-11-24FUJIAN FULAN INTELLIGENT OPTICAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202620070718.6
Authority / Receiving Office
CN · China
Patent Type
Utility models(China)
Current Assignee / Owner
Filing Date
2026-01-20
Publication Date
2026-11-24
Estimated Expiration
2036-01-20

AI Technical Summary

Technical Problem

Traditional HUD freeform surface mirrors have low reflectivity and poor optical accuracy and dimensional stability in extreme environments, which cannot meet the requirements for high performance.

Method used

A PEI substrate is used, and Cr film, Al film, Al₂O₃ film, multilayer SiO₂ and Ti₃O₅ film and anti-fingerprint AF film are deposited on it in sequence. The multilayer film structure is formed by electron beam evaporation coating technology to improve reflectivity and corrosion resistance.

Benefits of technology

Achieving high reflectivity (94.54%–96.76%) and excellent corrosion resistance, the PEI substrate maintains optical precision and dimensional stability in extreme environments, and exhibits superior creep resistance and chemical resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN225018472U_ABST
    Figure CN225018472U_ABST
Patent Text Reader

Abstract

This utility model relates to the field of HUD reflector technology, specifically to a high-performance HUD freeform surface reflector, comprising a PEI substrate, on which are sequentially deposited a Cr film layer, an Al film layer, an Al2O3 film layer, a first SiO2 layer, a first Ti3O5 layer, a second SiO2 layer, a second Ti3O5 layer, a third SiO2 layer, a third Ti3O5 layer, a fourth SiO2 layer, and an anti-fingerprint AF film layer. The high-performance HUD freeform surface reflector provided by this utility model exhibits an average reflectivity of 94.54% in the 420nm–680nm wavelength band and a maximum reflectivity of 96.76% under incident angles of 6–55°, demonstrating high reflectivity; it also possesses advantages such as extreme heat resistance, excellent creep resistance, naturally high flame retardancy, and excellent chemical resistance, exhibiting superior corrosion resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This utility model relates to the field of HUD reflector technology, specifically to a high-performance HUD freeform surface reflector. Background Technology

[0002] With the continuous development of technology, HUD reflectors have been widely used in the automotive, aviation, and gaming industries. As a head-up display, the HUD is a key technology in modern automotive and aerospace industries for improving driving safety and interactive experience. Its core function is to project crucial information onto the user's line of sight, overlaying it with the real road scene to achieve a "eyes-on-the-road" driving state. The HUD reflector (usually a freeform mirror) is the core component of optical imaging, and its performance directly determines the quality and reliability of the HUD image. The HUD reflector is an optical element made by vacuum-depositing an aluminum film onto a substrate.

[0003] Traditional HUD freeform surface mirrors often use glass or PC as the substrate, which has low reflectivity and poor results in constant humidity and heat accelerated aging tests. Utility Model Content

[0004] The purpose of this invention is to provide a high-performance HUD freeform surface reflector.

[0005] This utility model provides the following technical solution: This invention proposes a high-performance HUD freeform surface reflector, comprising a PEI substrate, on which a Cr film layer, an Al film layer, an Al2O3 film layer, a first SiO2 layer, a first Ti3O5 layer, a second SiO2 layer, a second Ti3O5 layer, a third SiO2 layer, a third Ti3O5 layer, a fourth SiO2 layer, and an anti-fingerprint AF film layer are sequentially deposited.

[0006] Furthermore, the thickness of the Cr film layer is 35-50nm, the thickness of the Al film layer is 100nm-130nm, the thickness of the Al2O3 film layer is 20nm-25nm, the thickness of the first SiO2 layer is 50nm-55nm, the thickness of the first Ti3O5 layer is 45nm-50nm, the thickness of the second SiO2 layer is 80nm-90nm, the thickness of the second Ti3O5 layer is 1000nm-1100nm, the thickness of the third SiO2 layer is 35nm-45nm, the thickness of the third Ti3O5 layer is 90nm-95nm, the thickness of the fourth SiO2 layer is 65nm-70nm, and the thickness of the anti-fingerprint AF film layer is 10nm-20nm.

[0007] Furthermore, the thickness of the Cr film is 42 nm, the thickness of the Al film is 115 nm, the thickness of the Al2O3 film is 22 nm, the thickness of the first SiO2 layer is 52 nm, the thickness of the first Ti3O5 layer is 47 nm, the thickness of the second SiO2 layer is 85 nm, the thickness of the second Ti3O5 layer is 1050 nm, the thickness of the third SiO2 layer is 40 nm, the thickness of the third Ti3O5 layer is 92 nm, the thickness of the fourth SiO2 layer is 67 nm, and the thickness of the anti-fingerprint AF film is 15 nm.

[0008] Compared with existing technologies, the high-performance HUD freeform surface reflector provided by this invention has an average reflectivity of 94.54% in the 420nm-680nm wavelength band and a maximum reflectivity of 96.76% under incident light angles of 6-55°, demonstrating high reflectivity. Simultaneously, compared with traditional PC materials, the PEI substrate has an absolute advantage in maintaining optical precision and dimensional stability under extreme environments, exhibiting advantages such as extreme heat resistance, excellent creep resistance, natural high flame retardancy, and excellent chemical resistance. Furthermore, this invention performs exceptionally well under high temperature and pressure, thermal shock, and high-temperature storage conditions, demonstrating superior corrosion resistance. Attached Figure Description

[0009] Figure 1 This is a diagram showing the arrangement of the membrane layers of this utility model.

[0010] Figure 2 The reflectance diagrams of the light from this invention are shown at incident angles of 6°, 30°, and 55°.

[0011] 1-PEI substrate; 2-Cr film layer; 3-Al film layer; 4-Al2O3 film layer; 5-First SiO2 layer; 6-First Ti3O5 layer; 7-Second SiO2 layer; 8-Second Ti3O5 layer; 9-Third SiO2 layer; 10-Third Ti3O5 layer; 11-Fourth SiO2 layer; 12-Anti-fingerprint AF film layer. Detailed Implementation

[0012] The following is in conjunction with the appendix Figure 1 The present invention will be further described below.

[0013] In one embodiment of this utility model, a high-performance HUD freeform surface reflector is proposed, comprising a PEI substrate 1, on which are sequentially deposited a Cr film layer 2 (to improve the adhesion of the AL film and the corrosion resistance of the reflector), an Al film layer 3 (as the main reflective film layer, to achieve high reflectivity of the HUD reflector), an Al2O3 film layer 4 (to improve the corrosion resistance of the aluminum layer), a first SiO2 layer 5, a first Ti3O5 layer 6, a second SiO2 layer 7, a second Ti3O5 layer 8, a third SiO2 layer 9, a third Ti3O5 layer 10, a fourth SiO2 layer 11, and an anti-fingerprint AF film layer 12 (anti-fingerprint and to improve the scratch resistance of the film layer); the SiO2 layer and the Ti3O5 layer further waterproof and enhance the reflectivity of the aluminum layer.

[0014] In one embodiment of this utility model, the selected materials Ti3O5 have a refractive index of 2.41 to 2.45, SiO2 have a refractive index of 1.45 to 1.48, and Al2O3 have a refractive index of 1.65 to 1.69.

[0015] In one embodiment of this utility model, the thickness of the Cr film layer 2 is 35-50nm, the thickness of the Al film layer 3 is 100nm-130nm, the thickness of the Al2O3 film layer 4 is 20nm-25nm, the thickness of the first SiO2 layer 5 is 50nm-55nm, the thickness of the first Ti3O5 layer 6 is 45nm-50nm, the thickness of the second SiO2 layer 7 is 80nm-90nm, the thickness of the second Ti3O5 layer 8 is 1000nm-1100nm, the thickness of the third SiO2 layer 9 is 35nm-45nm, the thickness of the third Ti3O5 layer 10 is 90nm-95nm, the thickness of the fourth SiO2 layer 11 is 65nm-70nm, and the thickness of the anti-fingerprint AF film layer 12 is 10nm-20nm.

[0016] In one embodiment of this utility model, the thickness of the Cr film layer 2 is 42 nm, the thickness of the Al film layer 3 is 115 nm, the thickness of the Al2O3 film layer 4 is 22 nm, the thickness of the first SiO2 layer 5 is 52 nm, the thickness of the first Ti3O5 layer 6 is 47 nm, the thickness of the second SiO2 layer 7 is 85 nm, the thickness of the second Ti3O5 layer 8 is 1050 nm, the thickness of the third SiO2 layer 9 is 40 nm, the thickness of the third Ti3O5 layer 10 is 92 nm, the thickness of the fourth SiO2 layer 11 is 67 nm, and the thickness of the anti-fingerprint AF film layer 12 is 15 nm.

[0017] In practical applications, before plating, the PEI substrate is cleaned with an ultrasonic cleaner to remove surface dirt and foreign matter. Then, it is pre-baked to remove internal moisture and reduce the internal moisture content of the substrate to below 0.02%, release the internal stress of the PEI material, and improve the dimensional thermal stability of the substrate. The baking temperature is 150±5℃ and the baking time is 6 hours. The workshop maintains constant temperature and humidity (temperature 23±2℃, humidity 30%-45%RH). According to Table 1 below, electron beam evaporation coating equipment is used, and RF ion source is used to assist deposition to improve film adhesion. Electron beam heating method is used to evaporate the film material onto the PEI substrate. Cr film layer, Al film layer, Al2O3 film layer, first SiO2 layer, first Ti3O5 layer, second SiO2 layer, second Ti3O5 layer, third SiO2 layer, third Ti3O5 layer, fourth SiO2 layer, and anti-fingerprint AF film layer are sequentially deposited on the PEI substrate to obtain the HUD freeform surface reflector.

[0018] The vacuum level used during the coating process is 8.0 × 10⁻⁶. -4 Pa, a high vacuum environment can produce thin films with good density, high purity and uniform coating; coating chamber temperature: the ambient temperature of the vacuum chamber before the third layer is 70℃ and the temperature when the fourth layer begins to be deposited is 150℃.

[0019] Table 1

[0020] The HUD freeform surface mirror (hereinafter referred to as the product) prepared above was subjected to the following tests: ① High reflectivity: Actual product testing shows that, with incident angles of 6-55°, the average reflectivity in the 420nm-680nm wavelength band is 94.54%, with a maximum reflectivity of 96.76%. Specific reflectivity data is as follows: Figure 2 As shown.

[0021] ②PEI material can be efficiently manufactured through injection molding, making it easier to shape and allowing for mass production of HUD reflector substrates. PEI material maintains an absolute advantage in optical accuracy and dimensional stability under extreme environments (PEI substrates can be used as freeform surfaces to correct HUD aberrations and magnify virtual images; the core optical elements of HUDs are aspherical or freeform surfaces), making it more stable than PC.

[0022] ③ Excellent corrosion resistance: 1. High temperature and high humidity (65℃, 93%RH) environment: After 1200 hours of testing, the product appearance is normal. No corrosion is observed.

[0023] 2. After 1000 hours of testing in a thermal shock environment (high temperature 140±2℃ for 1 hour, then removed and placed at low temperature -40±2℃ for 1 hour within 30 seconds, which constitutes one cycle), the product showed normal appearance and no corrosion.

[0024] 3. High temperature storage (140℃): After 1200 hours of testing, the product appearance is normal and there is no corrosion.

[0025] The embodiments of this utility model are given for the purpose of illustration and description. Although embodiments of this utility model have been shown and described above, it is understood that the above embodiments are exemplary and should not be construed as limiting this utility model. Those skilled in the art can make changes, modifications, substitutions and variations to the above embodiments within the scope of this utility model.

Claims

1. A high-performance HUD freeform surface reflector, characterized in that: The PEI substrate includes a Cr film, an Al film, an Al2O3 film, a first SiO2 layer, a first Ti3O5 layer, a second SiO2 layer, a second Ti3O5 layer, a third SiO2 layer, a third Ti3O5 layer, a fourth SiO2 layer, and an anti-fingerprint AF film.

2. The high-performance HUD freeform surface reflector according to claim 1, characterized in that: The thickness of the Cr film is 35-50nm, the thickness of the Al film is 100nm-130nm, the thickness of the Al2O3 film is 20nm-25nm, the thickness of the first SiO2 layer is 50nm-55nm, the thickness of the first Ti3O5 layer is 45nm-50nm, the thickness of the second SiO2 layer is 80nm-90nm, the thickness of the second Ti3O5 layer is 1000nm-1100nm, the thickness of the third SiO2 layer is 35nm-45nm, the thickness of the third Ti3O5 layer is 90nm-95nm, the thickness of the fourth SiO2 layer is 65nm-70nm, and the thickness of the anti-fingerprint AF film is 10nm-20nm.

3. The high-performance HUD freeform surface reflector according to claim 1, characterized in that: The thickness of the Cr film is 42 nm, the thickness of the Al film is 115 nm, the thickness of the Al2O3 film is 22 nm, the thickness of the first SiO2 layer is 52 nm, the thickness of the first Ti3O5 layer is 47 nm, the thickness of the second SiO2 layer is 85 nm, the thickness of the second Ti3O5 layer is 1050 nm, the thickness of the third SiO2 layer is 40 nm, the thickness of the third Ti3O5 layer is 92 nm, the thickness of the fourth SiO2 layer is 67 nm, and the thickness of the anti-fingerprint AF film is 15 nm.