POLYALKYL ENTEREPHTHALATE COMPOSITIONS

DE502016016769D1Active Publication Date: 2024-11-21ENVALIOR DEUTSCHLAND GMBH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
DE502016016769
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Filing Date
2016-09-06
Publication Date
2024-11-21
Estimated Expiration
2036-09-06

AI Technical Summary

Technical Problem

Polyalkylene terephthalate molding compounds experience a decrease in melt stability and flowability due to the addition of reactive additives with multiple epoxy, anhydride, or carbodiimide groups, leading to increased melt viscosity and processing issues, such as specks and blockages in injection molding systems, while existing solutions like hydroxyapatite can degrade polymer chains and reduce mechanical properties.

Method used

A composition comprising polyalkylene terephthalate, a copolymer of olefin and acrylic acid ester with a melt flow index of at least 50 g/10 min, and an epoxidized natural oil with multiple epoxy groups, which maintains melt stability and flowability without the adverse effects of reactive additives, ensuring high hydrolysis resistance and mechanical properties.

Benefits of technology

The solution provides polyalkylene terephthalate-based compositions with stable melt viscosity, good flow behavior, and enhanced hydrolysis resistance, maintaining mechanical properties and surface quality even when a flow agent is added, thus addressing the limitations of existing technologies.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The invention relates to novel, optionally reinforced compositions based on a) polyalkylene terephthalates, preferably polybutylene terephthalate, b) at least one copolymer of at least one olefin and at least one (meth)acrylic acid ester of an aliphatic alcohol, and c) at least one additive based on molecules having 2 or more epoxy, anhydride or carbodiimide groups per molecule, molding compositions to be produced therefrom, and hydrolysis-stable products to be produced from the molding compositions having good surfaces and, at the same time, good mechanical properties.

[0002] Polyalkylene terephthalates are generally characterized by good processability, good mechanical properties, temperature stability, and chemical stability. They are used in numerous applications, primarily in injection molding, film production, or fiber production. Preferred products based on polyalkylene terephthalates include switches, housings, connectors, sensors, and other applications in the electrical and electronics sectors.

[0003] What is important for polyalkylene terephthalates in the above-mentioned applications is problem-free processing, particularly with regard to hot runner systems, and the highest possible melt stability at elevated temperatures, whereby the person skilled in the art understands elevated temperatures to be those in the range >260°C, but below the decomposition temperature.

[0004] Melt stability describes the change in melt viscosity at elevated temperatures over time. For a polyalkylene terephthalate without additives, the melt viscosity decreases over time. However, reactive, chain-extending additives, such as molecules containing two or more epoxy groups, can also increase the melt viscosity. This is disadvantageous because it reduces the flowability of the melt, which can, among other things, lead to lower processing speeds. Furthermore, an increase in melt viscosity can lead to specks or solidification of the injection molding compound in the nozzle used during injection molding, or to blockages or closures in the sprue system (hot runner) of an injection molding system.Therefore, molding compounds with high melt stability are defined below as those that exhibit no increase in melt viscosity even after residence times of > 5 minutes significantly above the melting point of the molding compound, preferably > 260°C. For such melt-stable molding compounds, as is known to those skilled in the art, a slight reduction in melt viscosity is usually observed during processing.

[0005] According to https: / / de.wikipedia.org / wiki / Stippe_(Kunststoff), a speck is a surface defect on an injection-molded part. The present invention considers organic specks consisting of cracked, i.e., thermally decomposed, polymer.

[0006] The non-increase in melt viscosity during processing of a molding compound contributes to reducing specks and improving surface quality, thus reducing scrap in the injection molding process.

[0007] The use of additives containing two or more epoxy, anhydride, or carbodiimide groups in molding compounds generally leads to a reduction in flowability by increasing melt viscosity. Furthermore, at elevated temperatures, melt viscosity can increase during processing, causing significant processing problems.

[0008] WO2014 / 035472 A1 shows that polyester blends containing, for example, epoxy stabilizers tend to increase viscosity at high temperatures. The addition of hydroxyapatite to polyester blends containing additives containing reactive components (with two or more epoxy functionalities per molecule) leads to an increase in melt stability. However, WO2014 / 035472 A1 deliberately adds a chain-degrading mineral substance, which, under unfavorable conditions, can also lead to excessive degradation of the polymer chains and thus to a loss of mechanical properties in the final product. This significantly complicates its correct use in practice.

[0009] EP 1 992 662 A2 discloses molding compositions based on a thermoplastic polyester and at least one copolymer of at least one α-olefin with at least one methacrylic acid ester of an aliphatic alcohol, wherein the MFI (melt flow index) of the copolymer is not less than 100 g / 10 min.

[0010] The object of this invention was to provide polyalkylene terephthalate mixtures in the form of compositions and molding compounds according to the invention with high melt stability under processing conditions that do not exhibit any increase in melt viscosity during or as a result of processing. At the same time, the molding compounds according to the invention should exhibit low melt viscosity, good flow behavior during processing, and the products manufactured therefrom should exhibit high hydrolysis resistance, which does not decrease upon addition of a flow agent. The solution to the problem and the subject matter of the present invention are compositions, molding compounds, and products containing a) at least one polyalkylene terephthalate, b) at least one copolymer of at least one olefin and at least one acrylic acid ester or methacrylic acid ester of an aliphatic alcohol, wherein the melt flow index (MFI) of the copolymer, to be determined according to ISO 1133, is not less than 50 g / 10 min, preferably 150 g / 10 min, and is measured or determined at 190°C and a test weight of 2.16 kg, and c) at least one additive based on molecules with 2 or more epoxy groups per molecule, which is at least one epoxidized natural oil.

[0011] Surprisingly, the combination of components b) and c) leads to polyalkylene terephthalate-based compositions according to the invention and molding compositions to be produced therefrom which exhibit high melt stability under processing conditions, ie no build-up of melt viscosity, wherein products to be manufactured from the molding compositions are characterized by good surfaces and good mechanical properties and exhibit high hydrolysis resistance which does not decrease upon addition of a flow agent, as shown in the examples. Definitions

[0012] In one embodiment, the present invention relates to reinforced compositions, molding materials or products which are characterized by the presence of at least one filler or reinforcing material.

[0013] Melt-stable molding compounds are those that exhibit no increase in melt viscosity even after residence times of >5 minutes, well above the melting point, preferably above 260°C but below the decomposition temperature. A slight reduction in melt viscosity, as is known to the person skilled in the art and always observed for polyalkylene terephthalates under such conditions, is the desired state according to the invention.

[0014] Melt stability is determined by time-resolved MVR measurements according to ISO 1133 at 260°C and a test weight of 2.16 kg. The MVR value is determined after 5 and 20 minutes of residence time at 260°C. A decrease in the MVR value indicates an increase in melt viscosity. Consequently, a molding compound with a slight increase in the MVR value upon prolonged residence at 260°C can be considered melt-stable.

[0015] In the context of this application, the melt viscosity was determined according to ISO 11443 as a function of the shear viscosity (unit of measurement Pa•s). Good flow behavior is characterized by a low melt viscosity at typical shear rates corresponding to the processing (e.g., Eta = 1500 s -1< ).

[0016] Good mechanical properties within the meaning of the present invention are characterized in the case of products according to the invention by high values ​​of Izod impact strength. Impact strength describes the ability of a material to absorb shock and impact energy without breaking. The Izod impact strength test according to ISO 180 is a standard method for determining the impact strength of materials. In this test, an arm of a pendulum impact tester is first held at a certain height (= constant potential energy) and then released. The arm strikes the sample, causing it to break. The impact energy is determined from the energy absorbed by the sample. Impact strength is calculated as the ratio of impact energy to sample cross-section (unit of measurement kJ / m²). For the purposes of the present invention, impact strength was determined according to ISO 180-1U at 23°C.

[0017] The surface quality of products based on compositions according to the invention was examined and visually assessed within the scope of the present invention on test specimens measuring 60 mm x 60 mm x 2 mm. The decisive criteria for the assessment were gloss, smoothness, color, and uniform surface structure. Preferred embodiments of the invention

[0018] The compositions, moulding materials or products contain a) at least one polyalkylene terephthalate, b) at least one copolymer of an olefin and of an acrylic acid ester of an aliphatic alcohol, wherein the melt flow index (MFI) of the copolymer, to be determined according to ISO 1133, is not less than 50 g / 10 min, preferably 150 g / 10 min and is measured or determined at 190°C and a test weight of 2.16 kg, and c) at least one additive based on epoxidized natural oils with 2 or more epoxy groups per molecule.

[0019] The present invention preferably relates to compositions, molding materials or products containing a) polybutylene terephthalate, b) at least one copolymer of an olefin and of an acrylic acid ester of an aliphatic alcohol, wherein the melt flow index (MFI) of the copolymer, to be determined according to ISO 1133, is not less than 50 g / 10 min, preferably 150 g / 10 min and is measured or determined at 190°C and a test weight of 2.16 kg, and c) at least one additive based on epoxidized natural oils with 2 or more epoxy groups per molecule.

[0020] The present invention preferably relates to compositions, molding materials or products containing, in addition to components a), b) and c), component d) at least one filler and / or reinforcing material.

[0021] The present invention preferably relates to compositions, molding materials or products containing, in addition to components a), b), c) and d), or instead of d), at least one impact modifier.

[0022] The present invention preferably relates to compositions, molding materials or products containing, in addition to components a), b), c), d) and e), or instead of d) and / or e), also f), at least one further additive different from components b) to e).

[0023] The present invention preferably relates to compositions, molding materials or products comprising, per 100 parts by mass of component a), component b) in amounts in the range from 0.1 to 35 parts by mass and component c) in amounts in the range from 0.1 to 25 parts by mass.

[0024] The present invention preferably relates to compositions, molding materials or products containing component d) in amounts in the range from 5 to 150 parts by mass per 100 parts by mass of component a).

[0025] The present invention preferably relates to compositions, molding materials or products containing component e) in amounts in the range from 5 to 50 parts by mass per 100 parts by mass of component a).

[0026] The present invention preferably relates to compositions, molding materials or products comprising component f) in amounts ranging from 0 to 100 parts by mass per 100 parts by mass of component a).

[0027] The invention also relates to the use of compositions comprising components a), b) and c) and optionally d) and / or e) and / or f) for producing molding materials or products.

[0028] The invention further relates to a process for increasing the melt stability of polyalkylene terephthalate-based molding compositions or products to be produced therefrom, preferably PBT-based products, by adding at least one copolymer of at least one olefin and at least one methacrylic acid ester or acrylic acid ester of an aliphatic alcohol, wherein the melt flow index (MFI) of the copolymer, to be determined according to ISO 1133, is not less than 50 g / 10 min, preferably 150 g / 10 min, and is measured or determined at 190°C and a test weight of 2.16 kg, and at least one additive based on molecules with 2 or more epoxy groups per molecule, which is at least one epoxidized natural oil.

[0029] In one embodiment, the invention relates to a process for increasing the hydrolysis stability of polyalkylene terephthalate-based products, preferably PBT-based products, by adding at least one copolymer of at least one olefin and at least one methacrylic acid ester or acrylic acid ester of an aliphatic alcohol, wherein the melt flow index (MFI) of the copolymer, to be determined according to ISO 1133, is not less than 50 g / 10 min, preferably 150 g / 10 min, and is measured or determined at 190°C and a test weight of 2.16 kg, and at least one additive based on molecules with 2 or more epoxy, anhydride or carbodiimide groups per molecule.

[0030] For the sake of clarity, it should be noted that the scope of the present invention encompasses all definitions and parameters listed below, general or in preferred ranges, in any combination. The present invention relates to the compositions according to the invention, molding compositions to be produced therefrom, and products to be produced from the molding compositions, comprising at least one composition according to the invention. Cited standards apply in the version valid on the date of filing, unless otherwise stated. Although DIN EN ISO 10927 specifies a general method for determining the average molar mass and the molar mass distribution of polymers in a molar mass range from 2000 g / mol to 20,000 g / mol by matrix-assisted laser desorption / ionization time-of-flight mass spectrometry, in the context of the present invention it also provides reliable values ​​for component c) in the molar mass range from 500 g / mol to 1000 g / mol and is or iswas therefore applied accordingly. (Meth)acrylic acid esters in the context of the present invention mean methacrylic acid esters and / or acrylic acid esters.

[0031] The preparation of compositions according to the invention for the production of melt-stable molding compounds for further use in the manufacture of products, preferably by injection molding, extrusion, or blow molding, is carried out by mixing the individual components in at least one mixing unit, preferably a compounder, particularly preferably a co-rotating twin-screw extruder. This results in the intermediate products obtained from the invention, melt-stable molding compounds. These molding compounds—also referred to as thermoplastic molding compounds—can either consist exclusively of components a), b), and c), or additionally contain at least one of components d), e), or f). The compositions, molding compounds, or products according to the invention may contain components d), e), and f), but they may also not contain them. According to the invention, the following combinations result for the compositions, molding compounds, or products: a), b), c) a), b), c), d) a), b), c), e) a), b), c), f) a). b), c) d), e) a), b), c), d), f) a), b), c), d), e), f) Component a)

[0032] Polyalkylene terephthalates in the sense of the invention are reaction products of aromatic dicarboxylic acids or their reactive derivatives, preferably dimethyl esters or anhydrides, and aliphatic, cycloaliphatic or araliphatic diols and mixtures of these reaction products.

[0033] Preferred polyalkylene terephthalates can be prepared from terephthalic acid (or its reactive derivatives) and aliphatic or cycloaliphatic diols with 2 to 10 C atoms by known methods ( Plastics Handbook, Vol. VIII, p. 695 ff, Karl-Hanser-Verlag, Munich 1973 ).

[0034] Preferred polyalkylene terephthalates contain at least 80 mol%, preferably 90 mol%, based on the dicarboxylic acid, of terephthalic acid residues and at least 80 mol%, preferably at least 90 mol%, based on the diol component, of ethylene glycol and / or propane-1,3-diol and / or butane-1,4-diol residues.

[0035] The preferred polyalkylene terephthalates may contain, in addition to terephthalic acid residues, up to 20 mol% of residues of other aromatic dicarboxylic acids having 8 to 14 C atoms or residues of aliphatic dicarboxylic acids having 4 to 12 C atoms, such as residues of phthalic acid, isophthalic acid, naphthalene-2,6-dicarboxylic acid, 4,4'-diphenyldicarboxylic acid, succinic acid, adipic acid, sebacic acid, azelaic acid, cyclohexanediacetic acid, cyclohexanedicarboxylic acid.

[0036] The preferred polyalkylene terephthalates can be used in addition to ethylene or propanediol-1,3- or. Butanediol-1,4-glycol residues contain up to 20 mol% of other aliphatic diols having 3 to 12 C atoms or cycloaliphatic diols having 6 to 21 C atoms, in particular residues of propanediol-1,3, 2-ethylpropanediol-1,3, neopentyl glycol, pentanediol-1,5, hexanediol-1,6, cyclohexane-dimethanol-1,4, 3-methylpentanediol-2,4, 2-methylpentanediol-2,4, 2,2,4-trimethylpentanediol-1,3 and -1,6,2-ethylhexanediol-1,3, 2,2-diethylpropanediol-1,3, hexanediol-2,5, 1,4-di-(β-hydroxyethoxy)-benzene, 2,2-bis-(4-hydroxycyclohexyl)-propane, 2,4-Dihydroxy-1,1,3,3-tetramethylcyclobutane, 2,2-bis-(3-β-hydroxyethoxyphenyl)-propane and 2,2-bis-(4-hydroxypropoxyphenyl)-propane (DE-A 24 07 674 , DE-A 24 07 776 , DE-A 27 15 932 ).

[0037] The polyalkylene terephthalates can be branched by incorporating relatively small amounts of tri- or tetrahydric alcohols or tri- or tetrabasic carboxylic acids, as described, for example, in DE-A 19 00 270. Preferred branching agents are trimesic acid, trimellitic acid, trimethylolethane and propane, and pentaerythritol.

[0038] It is advisable not to use more than 1 mol% of the branching agent based on the acid component.

[0039] Particularly preferred are polyalkylene terephthalates which are produced solely from terephthalic acid and its reactive derivatives, preferably its dialkyl esters, and ethylene glycol and / or 1,3-propanediol and / or 1,4-butanediol and / or 1,4-cyclohexane dimethanol, in particular polyethylene and polybutylene terephthalate, and mixtures of these polyalkylene terephthalates.

[0040] Preferred polyalkylene terephthalates are also copolyalkylene terephthalates which are prepared from at least two of the above-mentioned acid components and / or from at least two of the above-mentioned alcohol components; particularly preferred copolyalkylene terephthalates are poly(ethylene glycol / butane-1,4-diol) terephthalates.

[0041] The thermoplastic polyalkylene terephthalates to be used according to the invention can also be used in a mixture with other polyalkylene terephthalates and / or other polymers.

[0042] The polybutylene terephthalate (PBT) [CAS No. 24968-12-5] preferably used as component a) according to the invention is prepared from terephthalic acid or its reactive derivatives and butanediol by known methods (Kunststoff-Handbuch, Vol. VIII, p. 695 ff, Karl Hanser Verlag, Munich 1973).

[0043] The PBT to be used as component a) preferably contains at least 80 mol%, preferably at least 90 mol%, based on the dicarboxylic acid, of terephthalic acid residues.

[0044] The PBT preferably used as component a) according to the invention can, in one embodiment, contain, in addition to terephthalic acid residues, up to 20 mol% of residues of other aromatic dicarboxylic acids having 8 to 14 C atoms or residues of aliphatic dicarboxylic acids having 4 to 12 C atoms, in particular residues of phthalic acid, isophthalic acid, naphthalene-2,6-dicarboxylic acid, 4,4'-diphenyldicarboxylic acid, succinic acid, adipic acid, sebacic acid, azelaic acid, cyclohexanediacetic acid, cyclohexanedicarboxylic acid, 2,5-furandicarboxylic acid.

[0045] The PBT preferably used as component a) according to the invention can, in one embodiment, contain, in addition to butanediol, up to 20 mol% of other aliphatic diols having 3 to 12 C atoms or up to 20 mol% of cycloaliphatic diols having 6 to 21 C atoms, preferably residues of 1,3-propanediol, 2-ethyl-1,3-propanediol, neopentyl glycol, 1,5-pentanediol, 1,6-hexanediol, 1,4-cyclohexanedimethanol, 3-methyl-2,4-pentanediol, 2-methyl-2,4-pentanediol, 2,2,4-trimethyl-1,3-pentanediol, 2,2,4-trimethyl-1,5-pentanediol, 2-ethyl-1,3-hexanediol, 2,2-diethyl-1,3-propanediol, 2,5-hexanediol, 1,4-Di-(β-hydroxyethoxy)-benzene, 2,2-bis-(4-hydroxycyclohexyl)-propane, 2,4-dihydroxy-1,1,3,3-tetramethyl-cyclobutane, 2,2-bis-(3-β-hydroxyethoxyphenyl)-propane and 2,2-bis-(4-hydroxypropoxy-phenyl)-propane.

[0046] PBT preferably used as component a) preferably has an intrinsic viscosity according to EN-ISO 1628 / 5 in the range from 40 to 170 cm 3 / g, particularly preferably in the range from 50 to 150 cm 3 / g, most preferably in the range from 65 to 135 cm 3 / g, in each case measured in an Ubbelohde viscometer in phenol / o-dichlorobenzene (1:1 parts by weight) at 25°C. The intrinsic viscosity iV,Also known as the Staudinger index or intrinsic viscosity, it is proportional to the average molecular weight according to the Mark-Houwink equation and is the extrapolation of the viscosity number VN for the case of vanishing polymer concentrations. It can be estimated from series of measurements or by using suitable approximate methods (e.g., Billmeyer). The VN [ml / g] is obtained from measuring the solution viscosity in a capillary viscometer, for example, an Ubbelohde viscometer. The solution viscosity is a measure of the average molecular weight of a plastic. It is determined on the dissolved polymer using different solvents, preferably m-cresol, tetrachloroethane, phenol, 1,2-dichlorobenzene, and concentrations. The viscosity number VN makes it possible to monitor the processing and usage properties of plastics. See also: http: / / de.wikipedia.org / wiki / Viskosimetrie and "http: / / de.wikipedia.org / wiki / Mark-Houwink-Gleichung".

[0047] The PBT preferably used as component a) according to the invention can also be used in a mixture with other polymers, preferably with polyethylene terephthalate and / or polycyclohexylenedimethylene terephthalate. Such PBT blends for use according to the invention are produced by compounding. During such compounding, conventional additives, in particular mold release agents or elastomers, can also be mixed in the melt, thereby improving the properties of the blends.

[0048] PBT to be used according to the invention can be obtained as Pocan ®< B 1300 from Lanxess Deutschland GmbH, Cologne. Component b)

[0049] As component b), the compositions according to the invention contain at least one copolymer of at least one olefin, preferably an α-olefin, and at least one methacrylic ester or an acrylic ester of an aliphatic alcohol, wherein the MFI of copolymer b) is not less than 50 g / 10 min, preferably 150 g / 10 min. Preferably, the copolymer to be used as component b) contains no further constituents, i.e., only the two components olefin and (meth)acrylic ester.

[0050] In a preferred embodiment, component b) is a copolymer of an olefin, preferably α-olefin, and of an acrylic acid ester of an aliphatic alcohol, wherein the MFI of the copolymer b) is not less than 50 g / 10 min, preferably 150 g / 10 min.

[0051] Component b) preferably contains less than 4% by weight, based on 100% by weight of component b), particularly preferably less than 1.5% by weight and very particularly preferably 0% by weight, of monomer units which contain further reactive functional groups, preferably selected from the group comprising oxetanes, imides, aziridines, furans, acids, amines, oxazolines.

[0052] Preferred olefins, especially α-olefins, as constituents of component b) have carbon atoms in a number ranging from 2 to 10. Preferred olefins may be unsubstituted or substituted by one or more aliphatic, cycloaliphatic, or aromatic groups.

[0053] Preferred olefins are selected from the group comprising ethene, propene, 1-butene, 1-pentene, 1-hexene, 1-octene, and 3-methyl-1-pentene. Particularly preferred olefins are ethene and propene, with ethene being most preferred.

[0054] Mixtures of the described olefins are also suitable.

[0055] In a further preferred embodiment, the further reactive functional groups, selected from the group comprising oxetanes, imides, aziridines, furans, acids, amines, oxazolines, of component b) are introduced into the copolymer exclusively via the olefin.

[0056] The olefin content of the copolymer is preferably in the range from 50 to 90% by weight, particularly preferably in the range from 55 to 75% by weight, based on 100% by weight of component b).

[0057] The copolymer is further defined by the second component, in addition to the olefin. Suitable second components are alkyl or arylalkyl esters of methacrylic acid or acrylic acid, whose alkyl or arylalkyl group consists of 1 to 30 carbon atoms, preferably 3 to 20 carbon atoms. The alkyl or arylalkyl group can be linear or branched and contain cycloaliphatic or aromatic groups, and can also be substituted by one or more ether or thioether functions.

[0058] Preferably, the alkyl or arylalkyl group of the methacrylic acid ester or the acrylic acid ester is selected from the group comprising 1-propyl, 1-butyl, 1-pentyl, 1-hexyl, 2-hexyl, 3-hexyl, 1-heptyl, 3-heptyl, 1-octyl, 1-(2-ethyl)hexyl, 1-nonyl, 1-decyl, 1-dodecyl, 1-lauryl, or 1-octadecyl. Alkyl or arylalkyl groups having 3 to 20 carbon atoms are preferred.

[0059] Mixtures of the described acrylic acid or methacrylic acid esters are also suitable.

[0060] According to the invention, the use of more than 60 parts by mass, particularly preferably more than parts by mass and very particularly preferably the use of 100 parts by mass of acrylate (2-ethyl)hexyl ester based on the total amount of 100 parts by mass of component b) is particularly preferred.

[0061] In a further preferred embodiment, the further reactive functional groups, selected from the group comprising oxetanes, imides, aziridines, furans, acids, amines, oxazolines, of the copolymer b) are introduced into the copolymer b) exclusively via the methacrylic acid ester or the acrylic acid ester. The content of the methacrylic acid ester or the acrylic acid ester in the copolymer b) is in the range from 10 to 50 parts by mass, preferably in the range from 25 to 45 parts by mass, based on 100 parts by mass of component b).

[0062] Copolymers b) to be used according to the invention are characterized not only by their chemical composition but also by their low molecular weight. Accordingly, only copolymers b) that have an MFI value measured at 190°C and a load of 2.16 kg of at least 50 g / 10 min, preferably at least 150 g / 10 min, and particularly preferably 300 g / 10 min are suitable for the compositions according to the invention. According to the invention, the copolymer of ethene and 2-ethylhexyl acrylate [CAS No. 26984-27-0], which is available under the trademark Lotryl® from Arkema Group, France, is very particularly preferred as component b).

[0063] The copolymers to be used as component b) can also act as flow agents in the molding compositions according to the invention. Component c)

[0064] Component c) comprises at least one additive based on molecules with two or more epoxy groups per molecule, which is an epoxidized natural oil. Additives of component c) particularly preferably have at least one terminal epoxy group, but a total of at least two epoxy groups per molecule.

[0065] Preferred epoxidized natural oils are based on at least one oil from the group consisting of olive oil, linseed oil, peanut oil, palm oil, soybean oil, and cod liver oil. Linseed oil or soybean oil is particularly preferred, and linseed oil is most preferred.

[0066] The average molecular weight of the epoxidized natural oils to be used as component c) is preferably in the range of 500 to 1000 g / mol and is determined by matrix-assisted laser desorption / ionization time-of-flight mass spectrometry according to DIN EN ISO 10927. Linseed or soybean oils to be used with preference according to the invention are mixtures of trifatty acid glycerides, with the C 18 carboxylic acid portion predominating.

[0067] Epoxidized natural oils are generally prepared by methods familiar to a person skilled in the art; see Angew. Chem. 2000, 112, 2292 - 2310 .

[0068] Preferred epoxidized fatty acid esters is obtained from saturated or unsaturated aliphatic carboxylic acids having 10 to 40 C atoms, preferably 16 to 22 C atoms, by reaction with aliphatic saturated alcohols having 2 to 40 C atoms, preferably 2 to 6 C atoms.

[0069] These are preferably mono- or divalent carboxylic acids. Particularly preferably, at least one carboxylic acid is selected from the group consisting of pelargonic acid, palmitic acid, lauric acid, margaric acid, dodecanedioic acid, behenic acid, stearic acid, capric acid, montanic acid, linoleic acid, linolenic acid, and oleic acid.

[0070] Preferably used aliphatic saturated alcohols are monohydric to tetrahydric. Particularly preferred is at least one alcohol selected from the group consisting of n-butanol, n-octanol, stearyl alcohol, ethylene glycol, propylene glycol, neopentyl glycol, pentaerythritol, and glycerol. Glycerol is especially preferred.

[0071] Mixtures of different esters and / or oils can also be used.

[0072] The introduction of the epoxide function into the aforementioned esters and / or oils is carried out by reacting them with epoxidizing agents, preferably with peracids, especially peracetic acid. Such reactions are well known to those skilled in the art.

[0073] The production synthetic epoxidized compounds is also known to the person skilled in the art. Preferred synthetic epoxidized compounds are polyglycidyl or poly(beta-methylglycidyl) ethers obtainable by reacting a compound having at least two free alcoholic or phenolic hydroxy groups and / or by reacting phenolic hydroxy groups with a substituted epichlorohydrin, preferably under alkaline conditions or in the presence of an acidic catalyst followed by alkali treatment.

[0074] Preferred polyglycidyl or poly(beta-methylglycidyl) ethers are derived from acyclic alcohols, in particular ethylene glycol, diethylene glycol and higher poly(oxyethylene) glycols, propane-1,2-diol or poly(oxypropylene) glycols, propane-1,3-diol, butane-1,4-diol, poly(oxytetramethylene) glycols, pentane-1,5-diol, hexane-1,6-diol, hexane-2,4,6-triol, glycerol, 1,1,1-trimethylpropane, bistrimethylolpropane, pentaerythritol, sorbitol and polyepichlorohydrins.

[0075] Alternatively preferred polyglycidyl or poly(beta-methylglycidyl) ethers are derived from cycloaliphatic alcohols, in particular 1,3- or 1,4-dihydroxycyclohexane, bis(4-hydroxycyclohexyl)methane, 2,2-bis(4-hydroxycyclohexyl)propane or 1,1-bis(hydroxymethyl)cyclohex-3-ene, or they have aromatic nuclei based on N,N-bis-8,2-hydroxyethyl)aniline or p,p'-bis(2-hydroxyethylamino)diphenylmethane.

[0076] Preferred synthetic epoxidized compounds are also based on mononuclear phenols, on polynuclear phenols, or on condensation products of phenols with formaldehyde obtained under acidic conditions.

[0077] Preferred mononuclear phenols are resorcinol or hydroquinone.

[0078] Preferred polynuclear phenols are bis(4hydroxyphenyl)methane, 2,2-bis(4-hydroxyphenyl)propane, 2,2-bis(3,5-dibromo-4-hydroxyphenyl)propane or 4,4'-dihydroxydiphenylsulfone.

[0079] Preferred condensation products of phenols with formaldehyde are phenol novolaks.

[0080] Preferred aromatic epoxy compounds have two terminal epoxy functions.

[0081] Preferred aromatic epoxy compound with 2 terminal epoxy functions is an oligomeric reaction product of bisphenol A with epichlorohydrin of the formula (I), with n in the range from 0 to 10, preferably with n in the range from 1 to 8, particularly preferably with n in the range from 1 to 6, where n is the average number of units in formula (I).

[0082] A synthetic epoxy compound to be used according to the invention preferably has a Mettler softening point according to DIN 51920 in the range from 0 to 150°C, particularly preferably from 50°C to 120°C, most preferably from 60°C to 110°C, and especially from 75°C to 95°C. The Mettler softening point is the temperature at which the sample flows out of a cylindrical nipple with an outlet opening of 6.35 mm in diameter, interrupting a light barrier located 19 mm below. For this purpose, the sample is heated in air under constant conditions.

[0083] Synthetic epoxy compounds to be used preferably have an average epoxy equivalent weight (EEW, grams of resin containing one mole of epoxide-bound oxygen) via titration according to DIN16945 in the range from 160 to 2000 g / eq, preferably in the range from 250 to 1200 g / eq, particularly preferably in the range from 350 to 1000 g / eq and especially preferably in the range from 450 to 800 g / eq.

[0084] Particularly preferred as component c) is a poly(bisphenol A-co-epichlorohydrin) [CAS No. 25068-38-6], preferably with a number average molecular weight (M n ) in the range from 600 to 1800 g / mol, to be determined by MALDI-TOF mass spectrometry by matrix-assisted laser desorption / ionization time-of-flight mass spectrometry according to EN ISO 10927, available as Epilox ®< from Leuna Harze GmbH, Leuna.

[0085] In a preferred embodiment of the present invention, the compositions, molding materials and products do not contain any further components besides components a), b) and c). Component d)

[0086] Preferably, at least one filler or reinforcing material is used as component d). Preferably, as component d) at least one filler or reinforcing material from the group consisting of carbon fibers, glass beads, ground glass, amorphous silica, calcium silicate [CAS No. 1344-95-2], calcium metasilicate [CAS No. 10101-39-0], magnesium carbonate [CAS No. 546-93-0], kaolin [CAS No. 1332-58-7], calcined kaolin [CAS No. 92704-41-1], chalk [CAS No. 1317-65-3], powdered or ground quartz [CAS No. 14808-60-7], mica [CAS No. 1318-94-1], phlogopite [CAS No. 12251-00-2], barium sulfate [CAS No. 7727-43-7], feldspar [CAS No. 68476-25-5], wollastonite [CAS No. 13983-17-0], montmorillonite [CAS No. 67479-91-8], and glass fibers [CAS No. 65997-17-3] are used. Glass fibers are particularly preferred, especially E-glass fibers.

[0087] The particularly preferred Glass fiberspreferably have a fiber diameter in the range of 7 to 18 µm, particularly preferably in the range of 9 to 15 µm, and are added as continuous fibers or as chopped or ground glass fibers.

[0088] According to "http: / / de.wikipedia.org / wiki / Faser-Kunststoff-Verbund," a distinction is made between a) chopped fibers, also known as short fibers, with a length in the range of 0.1 to 1 mm, b) long fibers with a length in the range of 1 to 50 mm, and c) continuous fibers with a length L > 50 mm. Fiber lengths can be determined, for example, using microfocus X-ray computed tomography (µ-CT); DGZfP Annual Conference 2007 - Lecture 47.

[0089] The fibers are preferably treated with a sizing system or an adhesion promoter or adhesion promoter system, particularly preferably based on silane.

[0090] Particularly preferred silane-based adhesion promoters for pretreatment are silane compounds of the general formula (II) (X-(CH 2 ) q ) k -Si-(OC r H 2r+1 ) 4-k (II) in which the substituents have the following meaning: X: NH 2 -, HO-, q: an integer from 2 to 10, preferably 3 to 4, r: an integer from 1 to 5, preferably 1 to 2, k: an integer from 1 to 3, preferably 1.

[0091] Particularly preferred adhesion promoters are silane compounds from the group aminopropyltrimethoxysilane, aminobutyltrimethoxysilane, aminopropyltriethoxysilane, aminobutyltriethoxysilane and the corresponding silanes which contain a glycidyl group as substituent X.

[0092] For the finishing of the glass fibers, the silane compounds are preferably used in amounts in the range of 0.05 to 2 parts by mass, particularly preferably in the range of 0.25 to 1.5 parts by mass and in particular in the range of 0.5 to 1 part by mass based on 100 parts by mass of glass fibers for the surface coating.

[0093] Due to the processing into the molding compound (compounding) or the resulting product, the glass fibers in the molding compound or product may have a lower d97 or d50 value than the originally used glass fibers. Due to the processing into the molding compound or the final product, the glass fibers in the molding compound or product may have shorter length distributions than originally used.

[0094] In a preferred embodiment of the present invention, the compositions, molding materials and products do not contain any further components besides components a), b), c) and d). Component e)

[0095] Impact modifiers preferably used according to the invention include, among others, one or more graft polymers of E.1 5 to 95 parts by mass, preferably 30 to 90 parts by mass, of at least one vinyl monomer on E.2 95 to 5 parts by mass, preferably 70 to 10 parts by mass, of one or more graft bases with glass transition temperatures < 10°C, preferably < 0°C, particularly preferably <-20°C, in each case based on 100 parts by mass of component e).

[0096] The graft base E.2 generally has an average particle size (d50 value) in the range from 0.05 to 10 µm, preferably in the range from 0.1 to 5 µm, particularly preferably in the range from 0.15 to 1 µm.

[0097] Monomers E.1 are preferably (meth)acrylic acid (C 1 -C 8 ) alkyl esters, in particular methacrylic acid (C 1 -C 8 ) alkyl esters, in particular methyl methacrylate, ethyl methacrylate and / or glycidyl methacrylate, n-butyl acrylate, t-butyl acrylate, and / or derivatives, in particular anhydrides and imides of unsaturated carboxylic acids, in particular maleic anhydride or N-phenyl maleimide. Preferred monomer E.1 is methyl methacrylate. Also suitable monomers E.1 are mixtures of

[0098] E.1.1 50 to 99 parts by mass of vinylaromatics and / or nucleus-substituted vinylaromatics, in particular styrene, α-methylstyrene, p-methylstyrene, p-chlorostyrene, and / or methacrylic acid (C 1 -C 8 )-alkyl esters, in particular methyl methacrylate, ethyl methacrylate and

[0099] E.1.2 1 to 50 parts by mass of vinyl cyanides, in particular unsaturated nitriles such as acrylonitrile and methacrylonitrile, and / or (meth)acrylic acid (C 1 -C 8 ) alkyl esters, in particular methyl methacrylate, glycidyl methacrylate, n-butyl acrylate, t-butyl acrylate, and / or derivatives, in particular anhydrides and imides of unsaturated carboxylic acids, in particular maleic anhydride or N-phenyl maleimide.

[0100] Preferred monomers E.1.1 are selected from at least one of the monomers styrene, α-methylstyrene and methyl methacrylate, preferred monomers E.1.2 are selected from at least one of the monomers acrylonitrile, maleic anhydride, glycidyl methacrylate and methyl methacrylate.

[0101] Suitable graft bases E.2 for the graft polymers used in the elastomer modifiers include, for example, acrylate rubbers, diene rubbers, EPDM rubbers (i.e., those based on ethylene / propylene and optionally diene), as well as polyurethane, silicone, chloroprene, and ethylene / vinyl acetate rubbers. EPDM stands for ethylene-propylene-diene rubber.

[0102] Preferred graft bases E.2 are acrylate rubbers based on graft bases E.2, which are preferably polymers of alkyl acrylic esters, optionally with up to 40 wt. %, based on E.2, of other polymerizable, ethylenically unsaturated monomers. Preferred polymerizable acrylic esters include C 1 -C 8 -alkyl esters, preferably methyl, ethyl, butyl, n-octyl, and 2-ethylhexyl esters; haloalkyl esters, preferably halo-C 1 -C 8 -alkyl esters, preferably chloroethyl acrylate, glycidyl esters, and mixtures of these monomers. Graft polymers with butyl acrylate as the core and methyl methacrylates as the shell are particularly preferred.

[0103] For crosslinking, monomers with more than one polymerizable double bond can be copolymerized. Preferred examples of crosslinking monomers are esters of unsaturated monocarboxylic acids with 3 to 8 C atoms and unsaturated monohydric alcohols with 3 to 12 C atoms, or saturated polyols with 2 to 4 OH groups and 2 to 20 C atoms, preferably ethylene glycol dimethacrylate, allyl methacrylate; polyunsaturated heterocyclic compounds, preferably trivinyl and triallyl cyanurate; polyfunctional vinyl compounds, preferably di- and trivinylbenzenes; but also triallyl phosphate and diallyl phthalate.

[0104] Preferred crosslinking monomers are allyl methacrylate, ethylene glycol dimethacrylate, diallyl phthalate and heterocyclic compounds having at least 3 ethylenically unsaturated groups.

[0105] Particularly preferred crosslinking monomers are the cyclic monomers triallyl cyanurate, triallyl isocyanurate, triacryloylhexahydro-s-triazine, and triallylbenzenes. The amount of crosslinked monomers is preferably 0.02 to 5 parts by mass, in particular 0.05 to 2 parts by mass, based on the graft base E.2.

[0106] For cyclic crosslinking monomers with at least 3 ethylenically unsaturated groups, it is advantageous to limit the amount to less than 1 mass fraction of the graft base E.2.

[0107] Preferred "other" polymerizable, ethylenically unsaturated monomers that can optionally be used in addition to the acrylic acid esters to prepare the graft base E.2 are acrylonitrile, styrene, α-methylstyrene, acrylamides, vinyl C 1 -C 8 alkyl ethers, methyl methacrylate, glycidyl methacrylate, and butadiene. Preferred acrylate rubbers as the graft base E.2 are emulsion polymers with a gel content of at least 60 parts by mass.

[0108] Likewise suitable grafting bases E.2 are diene rubbers, in particular based on butadiene, isoprene, etc., or mixtures of diene rubbers or copolymers of diene rubbers or mixtures thereof with further copolymerizable monomers, in particular according to E.1.1 and E.1.2, with the proviso that the glass transition temperature of component E.2 is <10°C, preferably <0°C, particularly preferably <-10°C.

[0109] Suitable grafting bases E.2 are preferably ABS polymers (emulsion, bulk and suspension ABS), where ABS stands for acrylonitrile butadiene styrene, as described, for example, in DE-A 2 035 390 or in DE-A 2 248 242 or in Ullmann, Enzyklopädie der Technischen Chemie, Vol. 19 (1980), p. 280 ff. .The gel content of the graft base E.2 is preferably at least 30 parts by mass, particularly preferably at least 40 parts by mass (measured in toluene). A rubber based on an acrylonitrile-butadiene-styrene copolymer is very particularly preferred. The elastomer modifiers or graft polymers are prepared by free-radical polymerization, preferably by emulsion, suspension, solution, or bulk polymerization, in particular by emulsion or bulk polymerization.

[0110] Since, as is known, the graft monomers are not necessarily completely grafted onto the graft base during the grafting reaction, graft polymers are also understood according to the invention to include products which are obtained by (co)polymerization of the graft monomers in the presence of the graft base and which are also obtained during the processing.

[0111] Further preferably suitable grafting bases according to E.2 are silicone rubbers with grafting-active sites, as described in DE-A 3 704 657, DE-A 3 704 655, DE-A 3 631 540 and DE-A 3 631 539.

[0112] In addition to elastomer modifiers based on graft polymers, elastomer modifiers not based on graft polymers can also be used, which have glass transition temperatures < 10°C, preferably < 0°C, particularly preferably < -20°C. These preferably include elastomers with a block copolymer structure as well as thermoplastically meltable elastomers, in particular EPM, EPDM and / or SEBS rubbers (EPM = ethylene-propylene copolymer, EPDM = ethylene-propylene-diene rubber and SEBS = styrene-ethene-butene-styrene copolymer).

[0113] In a preferred embodiment of the present invention, the compositions, molding materials and products contain no further components besides components a), b), c), d) and e), or the compositions, molding materials and products contain no further components besides components a), b), c) and e). Component f)

[0114] In one embodiment, the compositions according to the invention contain, in addition to components a) to c) or in addition to components a) to d), at least one additive f) different from components b, c), d) and e) from the group consisting of phosphite stabilizers, mold release agents, UV stabilizers, thermal stabilizers, gamma ray stabilizers, antistatic agents, flow aids, flame retardants, fire protection additives, emulsifiers, nucleating agents, plasticizers, lubricants, dyes and pigments.

[0115] The above-mentioned and other suitable additives are described, for example, in Gächter, Müller, Kunststoff-Additive, 3rd Edition, Hanser-Verlag, Munich, Vienna, 1989 and in the Plastics Additives Handbook, 5th Edition, Hanser-Verlag, Munich, 2001 . The additives to be used as component f) can be used individually or in mixtures or in the form of masterbatches.

[0116] Preferably, as component f) at least one Phosphite stabilizerPreference is given to using at least one phosphite stabilizer from the series tris(2,4-ditert-butylphenyl)phosphite (Irgafos®< 168, BASF SE, [CAS No. 31570-04-4]), bis(2,4-di-tert-butylphenyl)pentaerythritol diphosphite (Ultranox®< 626, Chemtura, [CAS No. 26741-53-7]), bis(2,6-di-tert-butyl-4-methylphenyl)pentaerythritol diphosphite (ADK Stab PEP-36, Adeka, [CAS No. 80693-00-1]), bis(2,4-dicumylphenyl)pentaerythritol diphosphite (Doverphos®< S-9228, Dover Chemical Corporation, [CAS No. 154862-43-8]), tris(nonylphenyl)phosphite (Irgafos ®< TNPP, BASF SE, [CAS No. 26523-78-4]), (2,4,6-tri-t-butylphenol)2-butyl-2-ethyl-1,3-propanediol phosphite (Ultranox ®< 641, Chemtura, [CAS No. 161717-32-4]) or Hostanox ®< P-EPQ.

[0117] Preferably, as component f) at least one mold release agentPreferred mold release agents are at least one selected from the group consisting of ester wax(es), pentaerythritol tetrastearate (PETS), long-chain fatty acids, salt(s) of long-chain fatty acids, amide derivative(s) of long-chain fatty acids, montan waxes, and low-molecular-weight polyethylene or polypropylene wax(es) or ethylene homopolymer wax(es).

[0118] Preferred long-chain fatty acids are stearic acid or behenic acid. Preferred salts of long-chain fatty acids are calcium stearate or zinc stearate. The preferred amide derivative of long-chain fatty acids is ethylenebisstearylamide. Preferred montan waxes are mixtures of straight-chain, saturated carboxylic acids with chain lengths of 28 to 32 carbon atoms.

[0119] As Thermo- or UV stabilizersPreferably, sterically hindered phenols, hydroquinones, aromatic secondary amines such as diphenylamines, substituted resorcinols, salicylates, benzotriazoles and benzophenones, as well as variously substituted representatives of these groups or mixtures thereof are used.

[0120] As plasticizers Dioctyl phthalate, dibenzyl phthalate, butylbenzyl phthalate, hydrocarbon oils or N-(n-butyl)benzenesulfonamide are preferably used.

[0121] Nucleating agents to be used as component f) according to the invention are preferably sodium or potassium salts of acetate, salicylate, steareate, saccharinate, as well as partially saponified montan waxes and ionomers, sodium or calcium phenylphosphinate, aluminum oxide, silicon dioxide, or talc. Talc [CAS No. 14807-96-6], in particular microcrystalline talc, is particularly preferably used as the nucleating agent. Talc, also referred to as talc, is a layered silicate with the chemical composition Mg 3 [Si 4 O 10 (OH) 2 ], which, depending on the modification, crystallizes as Talc-1A in the triclinic or as Talc-2M in the monoclinic crystal system (http: / / de.wikipedia.org / wiki / Talkum). Talc to be used according to the invention can be obtained, for example, as Mistron®< R10 from Imerys Talc Group, Toulouse, France (Rio Tinto Group). use

[0122] The present invention further relates to the use of at least one copolymer of at least one olefin and at least one acrylic acid ester or methacrylic acid ester of an aliphatic alcohol, wherein the melt flow index (MFI) of the copolymer, to be determined according to ISO 1133, does not fall below 50 g / 10 min and is measured or determined at 190°C and a test weight of 2.16 kg, and at least one additive based on molecules having two or more epoxy groups per molecule, which additive is at least one epoxidized natural oil, in at least one polyalkylene terephthalate for producing polyalkylene terephthalate-based compositions, molding compounds, or products.

[0123] The invention preferably relates to the use of components b) and c) for providing polyalkylene terephthalate-based molding compositions with high melt stability under processing conditions which do not show any build-up of melt viscosity during or as a result of processing and which have a low melt viscosity and good flow behavior during their processing.

[0124] The invention particularly preferably relates to the use of components b) and c) for providing polyalkylene terephthalate-based products with high hydrolysis resistance, which preferably does not decrease even when a flow agent is added. Proceedings

[0125] The preparation of compositions according to the invention for the production of molding compounds for further use in injection molding or extrusion is carried out by mixing the individual components in at least one mixing unit, preferably a compounder. To produce a polyalkylene terephthalate-based product, the molding compounds are subjected to further processing, preferably an injection molding process or extrusion. The injection molding and extrusion processes of thermoplastic molding compounds are known to those skilled in the art.

[0126] The present invention therefore relates to a process for producing products, preferably hydrolysis-stable products, particularly preferably hydrolysis-stable products without the hydrolysis stability decreasing due to the addition of a flow agent, by processing compositions comprising components a), b) and c) in at least one mixing unit, preferably a compounder, to form molding compositions and subjecting these to further processing, preferably an injection molding process or extrusion.

[0127] Processes according to the invention for producing polyalkylene terephthalate-based products by extrusion or injection molding are carried out at melting temperatures in the range from 230 to 330°C, preferably in the range from 250 to 300°C and optionally additionally at pressures of not more than 2500 bar, preferably at pressures of not more than 2000 bar, particularly preferably at pressures of not more than 1500 bar and very particularly preferably at pressures of not more than 750 bar.

[0128] Extrusion is primarily divided into profile extrusion and sequential coextrusion. In sequential coextrusion, two different materials are extruded one after the other in alternating sequence. This creates a preform with a different material composition in sections along the extrusion direction. By selecting the appropriate material, specific sections of the product can be equipped with specifically required properties, for example, for products with soft ends and a hard middle section or integrated soft bellows sections. ( Thielen, Hartwig, Gust, "Blow molding of hollow plastic bodies", Carl Hanser Verlag, Munich 2006, pages 127-129 ).

[0129] The injection molding process is characterized by the fact that the raw material, preferably in granular form, is melted (plasticized) in a heated cylindrical cavity and injected under pressure into a temperature-controlled cavity as an injection molding compound. The raw material used is a composition according to the invention, which has preferably already been compounded into a molding compound, which in turn has preferably been processed into granules. After the molding compound injected into the temperature-controlled cavity has cooled (solidified), the injection-molded part is removed from the mold. A distinction is made

[0130] 1. Plasticizing / melting 2. Injection phase (filling process) 3. Holding pressure phase (due to thermal contraction during crystallization) 4. Demolding

[0131] An injection molding machine consists of a clamping unit, the injection unit, the drive, and the control system. The clamping unit includes fixed and movable mold clamping plates, a face plate, and columns and the drive for the movable mold clamping plate (toggle joint or hydraulic clamping unit).

[0132] An injection unit comprises the electrically heated cylinder, the screw drive (motor, gear), and the hydraulics for moving the screw and injection unit. The injection unit's task is to melt, meter, inject, and repress the powder or granules (due to contraction). The problem of melt backflow within the screw (leakage flow) is solved by non-return valves.

[0133] The incoming melt is then dissolved and cooled in the injection mold, thus producing the final product. This always requires two mold halves. Injection molding distinguishes between the following functional complexes: Gate system Mold-forming inserts Ventilation Machine and force absorption Demolding system and motion transmission Tempering

[0134] In contrast to injection molding, extrusion involves inserting a continuously formed plastic strand, here made from a molding compound according to the invention, into the extruder, whereby the extruder is a machine for the production of thermoplastic molded parts / products.

[0135] Single-screw extruders and twin-screw extruders as well as the respective subgroups of conventional single-screw extruders, conveying-effective single-screw extruders, counter-rotating twin-screw extruders and co-rotating twin-screw extruders.

[0136] Extrusion lines consist of an extruder, a tool, downstream equipment, and extrusion blow molding. Extrusion lines for producing profiles consist of an extruder, a profile tool, calibration, a cooling section, a caterpillar and roller haul-off system, a separating device, and a tipping chute.

[0137] Products obtainable according to the invention are preferably materials that are exposed to aqueous media, atmospheric humidity, or splash water. The automotive industry's requirements for components used in motor vehicles are continually increasing, thus creating new challenges for the materials used. Plugs, connectors, and housing components used under the hood of cars must therefore pass increasingly stringent tests. Cycle tests in the temperature range of -40 to +150°C under humid conditions are not uncommon and require materials treated with special hydrolysis stabilizers. For example, PBT is produced by a polycondensation reaction between terephthalic acid or dimethyl terephthalate and 1,4-butanediol with the elimination of water. However, this polycondensation is reversible by hydrolysis at high temperatures and high relative humidity (RH).When PBT reacts with water, the polymer chain is cleaved, forming fragments with shorter chain lengths, including the reactants terephthalic acid and 1,4-butanediol. This means that the esterification is reversed (deesterification). Even a hydrolyzed fraction of 0.01% can significantly reduce viscosity and molecular weight. Compared to thermo-oxidative or thermal degradation, the destruction of a polymer through hydrolysis can be accelerated by a thousand or ten thousand times by catalytic additives. Various stabilizers can be added to halt or at least slow down hydrolysis. Common stabilizers can, on the one hand, capture the water, but, on the other hand, they can also rebuild already destroyed polymer chains. The hydrolysis of inventive products based on polyalkylene terephthalates is halted or at least slowed down by adding components b) and c).

[0138] Such hydrolysis-stabilized products are found in particular in motor vehicles, in the electronics, telecommunications, information technology or computer industries, as well as in household, sports, medicine or the entertainment industry.

[0139] According to the invention, preferred compositions and molding compositions and products to be produced therefrom contain a) PBT, b) copolymer of ethene and 2-ethylhexyl acrylate and c) epoxidized linseed oil or oligomeric 2,2-bis(4-(2,3-epoxypropoxy)phenyl)propane or a phenol-epichlorohydrin reaction product.

[0140] According to the invention, preferred compositions and molding compositions and products to be produced therefrom contain a) PBT, b) copolymer of ethene and 2-ethylhexyl acrylate, c) epoxidized linseed oil or oligomeric 2,2-bis(4-(2,3-epoxypropoxy)phenyl)propane or a phenol-epichlorohydrin reaction product and d) glass fibers.

[0141] According to the invention, preferred compositions and molding compositions and products to be produced therefrom contain a) PBT, b) copolymer of ethene and 2-ethylhexyl acrylate, c) epoxidized linseed oil or oligomeric 2,2-bis(4-(2,3-epoxypropoxy)phenyl)propane or a phenol-epichlorohydrin reaction product, d) glass fibers and e) methyl methacrylate-butyl acrylate graft copolymer.

[0142] According to the invention, preferred compositions and molding compositions and products to be produced therefrom contain a) PBT, b) copolymer of ethene and 2-ethylhexyl acrylate, c) epoxidized linseed oil or oligomeric 2,2-bis(4-(2,3-epoxypropoxy)phenyl)propane or a phenol-epichlorohydrin reaction product, d) glass fibers, e) methyl methacrylate-butyl acrylate graft copolymer and f) talc.

[0143] According to the invention, preferred compositions and molding compositions and products to be produced therefrom contain a) PBT, b) copolymer of ethene and 2-ethylhexyl acrylate, c) epoxidized linseed oil or oligomeric 2,2-bis(4-(2,3-epoxypropoxy)phenyl)propane or a phenol-epichlorohydrin reaction product, d) glass fibers, e) methyl methacrylate-butyl acrylate graft copolymer and f) phosphite stabilizer.

[0144] According to the invention, preference is given to compositions and molding compositions and products to be produced therefrom comprising a) PBT, b) copolymer of ethene and 2-ethylhexyl acrylate, c) epoxidized linseed oil or oligomeric 2,2-bis(4-(2,3-epoxypropoxy)phenyl)propane or a phenol-epichlorohydrin reaction product, d) glass fibers, e) methyl methacrylate-butyl acrylate graft copolymer and f) talc and phosphite stabilizer.

[0145] According to the invention, preference is given to compositions and molding compositions and products to be produced therefrom comprising a) PBT, b) copolymer of ethene and 2-ethylhexyl acrylate, c) epoxidized linseed oil or oligomeric 2,2-bis(4-(2,3-epoxypropoxy)phenyl)propane or a phenol-epichlorohydrin reaction product, d) glass fibers, e) methyl methacrylate-butyl acrylate graft copolymer and f) at least one fatty acid ester.

[0146] According to the invention, preference is given to compositions and molding compositions and products to be produced therefrom comprising a) PBT, b) copolymer of ethene and 2-ethylhexyl acrylate, c) epoxidized linseed oil or oligomeric 2,2-bis(4-(2,3-epoxypropoxy)phenyl)propane or a phenol-epichlorohydrin reaction product, d) glass fibers, e) methyl methacrylate-butyl acrylate graft copolymer and f) talc and at least one fatty acid ester.

[0147] According to the invention, preferred compositions and molding compositions and products to be produced therefrom contain a) PBT, b) copolymer of ethene and 2-ethylhexyl acrylate, c) epoxidized linseed oil or oligomeric 2,2-bis(4-(2,3-epoxypropoxy)phenyl)propane or a phenol-epichlorohydrin reaction product, d) glass fibers, e) methyl methacrylate-butyl acrylate graft copolymer and f) talc, phosphite stabilizer and at least one fatty acid ester. Examples

[0148] To produce inventive products based on inventive compositions, the individual components were melt-mixed in a twin-screw extruder (ZSK 32 Mega Compounder from Coperion Werner & Pfleiderer, Stuttgart, Germany) at temperatures ranging from 260 to 300°C, extruded as a strand, cooled in a water bath until granulatable, and granulated. Before further steps, the granules were dried at 120°C in a vacuum drying cabinet for approximately 4 hours.

[0149] The plates and test specimens for the Tables 1 to 3 The tests listed were carried out on a commercially available injection moulding machine of the type Arburg 320-210-500 at a melt temperature in the range of 250 to 270°C and a mould temperature in the range of 75 to 85°C. Test bars 80x10x4 mm (according to ISO 178) Color sample plates: 60x40x2 mm

[0150] Except for the melt viscosity measurements and the melt indices measurements, all tests listed in Tables 1 to 3 were carried out on the above-mentioned test specimens. Impact strength

[0151] The impact strength of the products manufactured from the compositions according to the invention in the form of test specimens measuring 80 × 100 × 4 mm 3< was determined in the impact test according to ISO 180-1U (IZOD) at 23°C (unit kJ / m 2< ). Melt viscosity

[0152] For the purposes of the present invention, the melt viscosity was determined according to ISO 11443 at the specified (apparent) shear rate and temperature using a Malvern RH7-900 instrument (cylinder diameter = 15 mm; capillary diameter = 1 mm; capillary length = 32 mm) after drying the granules at 120°C for 4 hours in a vacuum dryer. The measurement yielded the apparent viscosity in Pa•s. Melt index MVR (melt volume flow rate)

[0153] As a measure of melt stability, MVR measurements were performed according to ISO 1133 using a Zwick / Roell B4106.200 extrusion plastometer after 5 and 20 minutes of dwell time. The measurement results are expressed in cm3 / 10 min.

[0154] Reactive polyester blends can increase chain length and thus viscosity over time due to exposure to temperature. In contrast, in standard polyester, exposure to temperature leads to slight chain degradation.

[0155] The test after a 5-minute residence time in the flow tester allowed a comparative assessment of the chain and viscosity degradation in the melt during the preceding compounding in the twin-screw extruder. The test after a 20-minute residence time finally provided a direct comparison of the buildup or degradation of the composition in the melt and could therefore be transferred, for example, to processing steps in the melt after compounding (e.g., injection molding, hot runner). In this case, a "non-stable melt" was characterized by a buildup and thus by an increase in melt viscosity and, consequently, a lower MVR value. hydrolysis

[0156] To measure hydrolysis resistance, test specimens produced from molding compounds according to the invention containing the compositions according to the invention were stored in a steam sterilizer at 100°C and 100% humidity. After 15 days of exposure to humidity (hydrolysis), the impact strength of the stored products was determined in an impact test according to ISO 180-1U at 23°C, and the values ​​were determined according to Table 1. The impact strength is given as a relative percentage (%) of the initial value. surface

[0157] The surface was inspected and visually assessed using test specimens measuring 60 mm x 60 mm x 2 mm. The decisive criteria for the assessment were gloss, smoothness, color, and uniform surface structure. reactants

[0158] Component a): PBT, Linear polybutylene terephthalate with an intrinsic viscosity of 93 g / cm 3< measured in phenol : 1,2-dichlorobenzene = 1:1 at 25°C; (Pocan ®< B1300, commercial product of Lanxess Deutschland GmbH, Cologne)

[0159] Component b) : Copolymer of ethylene and 2-ethylhexyl acrylate with an ethylene content of 63 wt.% and an MFI of 550 (Lotryl ®< 37 EH 550 from Arkema France) [CAS No. 26984-27-0]

[0160] Component c1): Oligomeric reaction product of bisphenol A and epichlorohydrin (see formula (I)), with an epoxy equivalent weight (DIN 16945) of 500 to 700 g / eq and a softening point (Mettler, DIN 51920) between 75 and 90°C. [CAS No. 25068-38-6]

[0161] Component c2): Epoxidized linseed oil (epoxide content 8-10%). Edenol B 316 Spezial from Emery Oligochemicals, Malaysia

[0162] Component d):Glass fiber coated with silane-containing compounds with a diameter of 10 µm (CS 7967, commercial product of Bayer Antwerpen NV, Antwerp, Belgium)

[0163] Component e): Methyl methacrylate / butyl acrylate copolymer, consisting of a butyl acrylate core and a grafted MMA shell (70 / 30), Paraloid EXL 3300, DOW Chemical AG, USA.

[0164] Component f): The following components commonly used in thermoplastic polyesters were used as additional additives: Nucleating agent: Talc [CAS No. 14807-96-6] in amounts of 0.01 to 0.55 parts by mass relative to 100 parts by mass of component a) Thermostabilizer: Common stabilizers based on phenyl phosphites in amounts of 0.01 to 0.55 parts by mass relative to 100 parts by mass of component a) Mold release agent: Commercially available fatty acid esters in amounts of 0.1 to 0.50 parts by mass relative to 100 parts by mass of component a) Pigments:Carbon black, organic dyes in amounts of 0 to 0.85 parts by mass in relation to 100 parts by mass of component a) Table 1 Comparison 1 Comparison 2 Example 1 Example 2 Example 3 Component a) 100 100 100 100 100 Component b) - 10 10 10 Component c1) - 3 3 3 Component c2) 9 Component d) 43 47 49 52 43 Component e) - 6 7 Component f) 1 1 1 1 1 MVR (260°C, 2.16 kg) - 5 min 17 11 17 13 18 MVR (260°C, 2.16 kg) - 20 min 24 8 23 17 19 Melt stability ++ - ++ ++ + Melt viscosity 260°C, Eta = 1500s -1< 138 120 85 90 and Izod impact strength and + + + and Retention of impact strength (Izod) after 15 d 100°C, 100% humidity 13 42 68 55 55 Surface quality color sample plate [60 × 40 × 2 mm] + and + and and (Quantities in assenantelles)

[0165] Examples 1 and 2 are reference examples.

[0166] Comparison 1 shows the results measured within the scope of the present invention using a standard PBT with 30 mass fractions of glass fibers. The measurements confirmed that the melt stability of such a standard molding compound made of PBT and 30 mass fractions of glass fibers is very good (++), as evidenced by the increase in MVR with longer residence times at 260°C. Pocan®< B3235 from Lanxess Deutschland GmbH, Cologne, was used as the standard PBT GF 30.

[0167] Comparison 2In contrast, the melt stability of a molding compound made of PBT, glass fibers, a reactive epoxy resin, and an impact modifier (acrylate copolymer based on a methyl methacrylate / butyl acrylate copolymer) was not melt stable (--). This is evident from the decrease in the MVR after a residence time of 20 minutes at 260°C compared to a residence time of 5 minutes.

[0168] In comparison, molding compositions according to the invention according to Examples 1 to 3 made of a) PBT, b) an acrylate copolymer based on ethylhexyl acrylate and ethene, c) a reactive epoxy resin and d) glass fibers, again showed very good melt stabilities - comparable to Comparison 1 - on.

[0169] In addition, products made from these molding compositions according to the invention showed a higher hydrolysis stability than products based on molding compositions from Comparative Examples 1 and 2!

[0170] Likewise, the melt viscosity test results for Examples 1 and 2 were significantly lower than the melt viscosity values ​​for the molding compounds of Comparative Examples 1 and 2. The excellent flow behavior was reflected in a low melt viscosity and shear viscosity at high shear rates (1500 s -1< ), which roughly corresponded to the shear rate during processing. The flowability of the molding compounds made from the inventive compositions exceeded the flowability of a standard PBT GF 30.

[0171] Furthermore, the mechanical properties (Izod impact strength) according to ISO 180 of products based on the molding compounds according to the invention and the surface quality were comparable to a standard PBT from Comparison 1 , which is known to experts for its good properties in terms of surface and mechanics.

[0172] Surprisingly for the expert, Example 2the fact that the addition of component b) to a Comparison 2 described, actually not melt-stable mixture of PBT, despite everything, resulted in good melt stability. Furthermore, improved hydrolytic stability and a reduced melt viscosity were also observed here, compared to Comparison 2, given.

[0173] Example 3 shows that in a molding composition according to the invention, other epoxy sources, in this case epoxidized linseed oil, can be used instead of a phenol-epichlorohydrin-based epoxy resin for an additive to be used as component c).

[0174] Table 1 shows that compositions or molding materials according to the invention and products to be produced therefrom according to the Examples 1 to 3all the requirements set out in the task of the present invention were met. The blends of PBT with the combination of components b) and c) used according to the invention exhibited excellent melt stability, the molding compounds exhibited excellent flow behavior, and the products produced therefrom were characterized by good hydrolysis resistance, good mechanical properties, and a good surface.

Claims

1. Compositions, moulding materials and articles of manufacture containing a) at least one polyalkylene terephthalate, b) at least one copolymer of at least one olefin and at least one acrylic ester or methacrylic ester of an aliphatic alcohol, wherein the melt flow index according to ISO 1133 of the copolymer is not less than 50 g / 10 min and said index is measured / determined at 190°C and a test weight of 2.16 kg, and c) at least one additive based on molecules having 2 or more epoxy groups per molecule, wherein said additive is at least one epoxidized natural oil.

2. Compositions, moulding materials and articles of manufacture according to Claim 1, characterized in that the epoxidized natural oils are based on at least one oil from the group of olive oil, linseed oil, peanut oil, palm oil, soybean oil and cod liver oil.

3. Compositions, moulding materials and articles of manufacture according to Claim 1 or 2, characterized in that as component c) linseed oil or soybean oil, in particular linseed oil, is employed.

4. Compositions, moulding materials and articles of manufacture according to Claim 2 or 3, characterized in that the average molecular weight of the epoxidized natural oils employable as component c) is in the range from 500 to 1000 g / mol and is determined by matrix-assisted laser desorption / ionization time-of-flight mass spectrometry according to DIN EN ISO 10927.

5. Process for producing articles of manufacture, characterized in that it comprises processing compositions according to any of Claims 1 to 4 in at least one mixing assembly to afford moulding materials and subjecting these to further processing, preferably to an injection moulding process or an extrusion.

6. Use of at least one copolymer of at least one olefin and at least one acrylic ester or methacrylic ester of an aliphatic alcohol, wherein the melt flow index (MFI) according to ISO 1133 of the copolymer is not less than 50 g / 10 min and said index is measured / determined at 190°C and a test weight of 2.16 kg, and at least one additive based on molecules having 2 or more epoxy groups per molecule, wherein said additive is at least one epoxidized natural oil, for producing polyalkylene terephthalate-based compositions, moulding materials or articles of manufacture.