THE COMPOSITE MATERIAL
Patent Information
- Application Number
- DE502017016454
- Authority / Receiving Office
- DE · DE
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2016-12-20
- Filing Date
- 2017-12-13
- Publication Date
- 2024-10-17
- Estimated Expiration
- 2037-12-13
AI Technical Summary
Current composite materials lack the ability to reversibly change their properties in response to external stimuli, limiting their adaptability and functionality.
A composite material comprising a hydrophilic matrix with cavities containing nanoparticles that can agglomerate in response to temperature changes, allowing for reversible changes in properties such as optical scattering, conductivity, and mechanical strength, through lipophilic surface modification and suitable solvent selection.
Enables reversible and repeatable changes in the composite material's properties, enhancing its adaptability and functionality by altering its optical, electrical, and mechanical characteristics in response to temperature stimuli.
Description
Field of the invention
[0001] The invention relates to a composite material comprising cavities containing nanoparticles. By changing the arrangement of the nanoparticles, in particular agglomeration of the nanoparticles, within the cavities, the properties of the system within the cavities and also the properties of the entire composite material change. If this process is reversible, the properties of the composite material can be reversibly changed. State of the art
[0002] Polymers in which conductive particles are embedded are known from the prior art. As the surrounding matrix expands, the distances between the particles change, and the conductivity of the polymer changes. This allows the conductivity of the polymer to be adjusted, for example, by changing the temperature.
[0003] E-Ink technology uses microcapsules with embedded pigments that can be moved within the capsules by applying an electric field. The microcapsules represent individual pixels of a display. The color change is based on the color of the individual particles, which migrate up or down within the capsule.
[0004] Materials are also known that contain encapsulated substances that are released when necessary, e.g. if the material is damaged.
[0005] CN105061759 discloses monodisperse Pd / PANI nanoparticles uniformly distributed in a polyaniline matrix (Example 1). The matrix lacks voids filled with solvent and nanoparticles.
[0006] EP1621574A1 discloses a polymer matrix in which the nanoparticles are incorporated. The differences in the optical properties result from the glass transition temperature of the polymer matrix. The matrix does not contain cavities filled with a solvent and nanoparticles.
[0007] US20110123589A1 discloses a polysaccharide matrix containing metallic nanoparticles uniformly distributed therein. The preparation, particularly the gelation, of the gels is described. Agglomeration of the particles does not occur. Task
[0008] The object of the invention is to provide a composite material whose properties can be modified by an external stimulus. A method for producing the composite material is also to be provided. Solution
[0009] This object is achieved by the inventions having the features of the independent claims. Advantageous developments of the inventions are characterized in the subclaims. The wording of all claims is hereby incorporated by reference into this description. The inventions also encompass all reasonable and, in particular, all mentioned combinations of independent and / or dependent claims.
[0010] The object is achieved by a composite material comprising a hydrophilic matrix and cavities, wherein the cavities comprise at least one type of nanoparticles, wherein at least one of the cavities can be converted from a first state to a second state by the action of temperature as an external stimulus on the composite material, wherein the first state differs from the second state in the arrangement of the nanoparticles within the at least one cavity and the nanoparticles are agglomerated in one of the two states, wherein the cavities comprise at least one type of nanoparticles and at least one non-polar solvent, wherein the at least one type of nanoparticle has a lipophilic surface modification, wherein the nanoparticles are dispersed in the solvent.
[0011] The term "cavity" in the context of the invention refers to a space spatially separated from the surrounding matrix, which has a different composition than the surrounding matrix. It often also differs in its physical properties. For example, the matrix is solid, while the composition within the cavity is liquid or viscous.
[0012] The two states preferably differ in a physical property of the composite material. For example, this property is selected from optical scattering, absorption, X-ray scattering, magnetic remanence, thermal conductivity, heat capacity, electrical conductivity, dielectric properties, mechanical strength, or viscoelastic properties, whereby several properties can also be changed simultaneously.
[0013] The change can, for example, lead to a change in the transparency, color and / or conductivity of the composite material.
[0014] The first and second states differ at least in the arrangement of the nanoparticles within the cavities. In one of the two states, the nanoparticles are agglomerated.
[0015] In a preferred embodiment of the invention, the conversion from a first to a second state is reversible, in particular multiply reversible, for example repeatable at least twice.
[0016] The external stimulus is temperature.
[0017] In one embodiment of the invention, the cavities comprise at least one means for influencing the arrangement of the nanoparticles upon exposure to the stimulus. This means can be selected accordingly depending on the chosen stimulus.
[0018] These can be agents that absorb the stimulus and transfer the energy to the nanoparticles, changing their arrangement. In the case of temperature, the agent can solidify and thus influence the arrangement of the nanoparticles dispersed within it.
[0019] The agents may also comprise nanoparticles, for example by absorbing the stimulus and transferring energy to the ligand shell or other components.
[0020] Preferred agents are those capable of interacting with the surface of the nanoparticles. These are preferably substances that contain at least one group with at least one heteroatom, a π bond, or an aromatic π system.
[0021] The nanoparticles according to the invention are nanoscale particles, i.e. the particle size is less than 500 nm. Unless otherwise stated, particle size here means the average particle diameter measured by TEM based on at least 60% of the particles. The average particle diameter is preferably not more than 200 nm, particularly preferably not more than 100 nm, e.g. 0.5 to 200, preferably 1 to 100 nm, e.g. 1 to 50 nm. Electron microscopic methods (e.g. via HR-TEM) can also be used to determine very small particles in this range. The particles can also be fibrous, if appropriate. In this case, the average particle size refers to the length, which can also be determined visually using microscopic methods, for example. Especially when optical properties play a role, the nanoparticles can be as small as 10 nm, in particular as small as 5 nm.
[0022] Sufficient nanoparticles must be arranged within a cavity so that the desired change in state is also achieved for the composite material. In the case of a change in optical properties, the absorption of the nanoparticles or their agglomerates must be sufficiently large. This can be easily determined by experiments with different cavity sizes.
[0023] For purely optical changes, it may be sufficient for the nanoparticles to be present in a proportion of 0.001 to 5 wt.%, preferably 0.01 to 2 wt.%, and especially 0.01 to 0.1 wt.%, based on the composition within the cavities. For gold nanoparticles, for example, concentrations as low as 0.05 wt.% are sufficient to detect a clearly visible change in the absorption of the composite material.
[0024] The nanoparticles are, in particular, nanoscale, inorganic solid particles. They are preferably metal nanoparticles, including metal alloys, metal or semi-metal compounds, in particular metal chalcogenides. All metals or semi-metals (hereinafter also abbreviated collectively as M) can be used for this purpose. Preferred metals or semi-metals M for the metal or semi-metal compounds are, for example, Mg, B, Al, Ga, In, Si, Ge, Sn, Pb, Y, Ti, Zr, V, Nb, Ta, Mo, W, Fe, Cu, Ag, Au, Pt, Pd, Zn, Cd, Ce and La or mixtures thereof. One type of nanoparticle or a mixture of nanoparticles can be used.
[0025] The nanoparticles can comprise a metal, mixtures of two or more metals, or an alloy of two or more metals, e.g., FePt. The metals are preferably selected from the metals of IUPAC groups 1 to 16, as well as the lanthanides, preferably from the metals of groups 4 to 16, in particular Au, Ag, Cu, Pt, Pd, Ni, Ru, In, Rh, Al, Pb, Bi, and Te. The nanoparticles can also comprise conductive or semiconductive oxides. Examples of such oxides, which can also be doped, are indium tin oxide (ITO) or antimony tin oxide (ATO). They can also be semiconductors of groups II-VI, III-V, or IV, or alloys of such semiconductors. Examples include CdS, CdSe, CdTe, InP, InAs, ZnS, ZnSe, ZnTe, HgTe, GaN, GaP, GaAs, GaSb, InSb, Si, Ge, AlAs, PbSe, or PbTe. They can also be non-metallic nanoparticles, for example, made of oxides, sulfides, or selenides of the aforementioned metals. Examples include Cu 2 S, Bi 2 S 3 , Sb 2 S 3 , SmO 3 , and PbS.Examples are (optionally hydrated) oxides such as ZnO, CdO, SiO 2 , GeO 2 , TiO 2 , ZrO 2 , CeO 2 , SnO 2 , Al 2 O 3 (in particular boehmite, AlO(OH), also as aluminum hydroxide), B 2 O 3 , In 2 O 3 , La 2 O 3 , Fe 2 O 3 , Fe 3 O 4 , Cu 2 O, Ta 2 O 5 , Nb 2 O 5 , V 2 O 5 , MoO 3 or WO 3 ; Phosphates, silicates, zirconates, aluminates, stannates of metals or semi-metals, and corresponding mixed oxides (e.g. indium tin oxide (ITO), antimony tin oxide (ATO), fluorine-doped tin oxide (FTO), luminescent pigments with Y- or Eu-containing compounds, spinels, ferrites or mixed oxides with perovskite structure such as BaTiO 3 and PbTiO 3 ).
[0026] Nanoscale particles can usually be prepared by various methods, including flame pyrolysis, plasma processes, colloidal techniques, sol-gel processes, controlled nucleation and growth processes, MOCVD processes, and emulsion processes. These processes are extensively described in the literature.
[0027] The nanoparticles can be spherical. They can also be rod-shaped, for example, with a length-to-diameter aspect ratio of 20:1 to 2:1, where the above-mentioned particle diameter refers to the longer dimension of the particles.
[0028] The nanoparticles can also be doped with at least one other metal or semimetal. In some cases, a non-metal is also suitable. Any suitable metal or semimetal compound can be added for doping during production of the nanoparticles, e.g. an oxide, a salt or a complex compound, e.g. halides, nitrates, sulfates, carboxylates (e.g. acetates) or acetylacetonates. The other metal can be present in the compound in any suitable oxidation precursor. Examples of suitable metals for doping are Mg, Ca, Y, Er, Sc, Ce, W, Mo, Zn, Cu, Ag, Au, Sn, In, Fe, Co, Ni, Mn, Ru, Al, Sb, V, Nb, Ir, Rh, Os, Pd and Pt.
[0029] The cavities contain a dispersing agent in which the nanoparticles are dispersed. This is a solvent. Preferably, this agent is mobile. This typically means that the agent is sufficiently viscous for the nanoparticles to migrate through the medium, changing their arrangement upon exposure.
[0030] These can be solvents, for example. They preferably have a boiling point above 80 °C, especially above 120 °C. This reduces the diffusion of the solvent from the cavities. They can also be a mixture of solvents.
[0031] It is a non-polar solvent. Examples of a polar solvent are water or mixtures containing water and organic, preferably water-soluble solvents. Polar solvents are particularly preferably water or mixtures of water and alcohols, aldehydes, and / or ketones, particularly preferably water or mixtures of water with mono- or polyhydric alcohols having up to four carbon atoms, such as methanol, ethanol, n-propanol, isopropanol, glycerol, or ethylene glycol, aldehydes having up to four carbon atoms, such as formaldehyde, and / or ketones having up to four carbon atoms, such as acetone or methyl ethyl ketone. However, polar organic solvents such as sulfonates or tetrahydrofuran can also be used.
[0032] Organic solvents are preferred as nonpolar solvents. These are preferably aromatic or aliphatic hydrocarbons with at least 5 carbon atoms, such as petroleum ether, hexane, heptane, decane, undecane, especially n-hexane, n-heptane, n-decane, n-undecane, toluene, benzene, cyclopentane, tetralin, or cyclohexane; halogenated aromatic or aliphatic hydrocarbons such as dichloromethane, dichloromethane, chloroform; alkyl acetates such as butyl acetate; and ketones such as acetophenone or cyclohexanone. Mixtures of these solvents can also be used.
[0033] The cavities are closed cavities within the matrix in which the nanoparticles are arranged. These cavities preferably have a maximum dimension of 500 µm, preferably up to 200 µm, in particular up to 100 µm. The minimum dimension of the cavities is preferably at least 100 nm, preferably 200 nm, and most preferably 500 nm. The cavities must be sufficiently large relative to the nanoparticles used so that a sufficient number of nanoparticles can be arranged within the respective cavity to respond to the stimulus. The size in the micrometer range can be determined using light microscopy.
[0034] The cavities remain closed during the transition between states. No nanoparticles leave the cavities. The change in properties is based on a change within the cavities.
[0035] To prevent nanoparticle diffusion, it is important to select the polarity of the matrix, the nanoparticles, and, if applicable, the dispersant in the cavities. In the case of a lipophilic matrix, such as organic polymers, the nanoparticles should be correspondingly lipophobic. Similarly, in a hydrophilic matrix, the nanoparticles should be hydrophobic. This can be achieved by appropriate surface modification of the nanoparticles.
[0036] In addition, the dispersant present in the cavities should also be lipophobic or hydrophobic, depending on the nanoparticles.
[0037] The concept of hydrophilicity / lipophilicity is well known to those skilled in the art. Lipophilic or hydrophobic groups tend not to penetrate and remain in water, while hydrophilic groups tend to penetrate and remain in water.
[0038] The properties of the nanoparticles can be adjusted through appropriate surface modification, for example, by compounds that introduce lipophilic residues onto the surface of the nanoparticles. Likewise, the nanoparticles can already contain corresponding groups from their production, for example, from a sol-gel process.
[0039] Lipophilic compounds or groups tend to disperse or dissolve in a non-polar medium, e.g., an organic solvent such as hexane or toluene, whereas hydrophilic compounds or groups tend to disperse or dissolve in a polar medium, e.g., water. Hydrophilic character can arise, for example, from hydroxyl, oxy, oxide, carboxylate, sulfate, sulfonate functions, generally ionic groups, or hydrophilic polyether chains, whereas lipophilic character is typically found in hydrocarbon residues such as alkyl or aromatic residues.
[0040] In order to achieve the dispersibility of the nanoparticles, as well as the responsiveness of the nanoparticles to the stimulus, the nanoparticles can have a corresponding surface modification.
[0041] The surface modification of the nanoparticles can be achieved simply by mixing the particles with the surface modifier. The reaction takes place in a solvent, if necessary, and by mechanical or thermal energy input and / or by adding a catalyst. The nanoparticles can also exhibit such modifications during their production.
[0042] Suitable surface modifiers are compounds that possess one or more groups that can react or interact with the surface of the nanoparticles or with reactive groups present thereon (such as OH groups). Surface modifiers can form, for example, covalent, coordinate (complex formation), and ionic (salt-like) bonds with the surface of the nanoparticles. Pure interactions include dipole-dipole interactions, hydrogen bonds, and van der Waals interactions. The formation of interactions or complexation is preferred.
[0043] The surface modifiers generally have a relatively low molecular weight. For example, the molecular weight can be less than 1,500, in particular less than 1,000, and preferably less than 700, and most preferably less than 500. However, a higher molecular weight, e.g., up to 2,000 or more, is also possible.
[0044] Inorganic and organic acids, bases, chelating agents, complexing agents such as β-diketones, amino acids or silanes can be used for the surface modification of the nanoparticles.
[0045] In a preferred embodiment, the surface modifier can be a complexing agent that forms the modification by complexing on the surface of the nanoparticles. Specific examples of surface modifiers are thiols, alcohols, phosphines, saturated or unsaturated mono- and polycarboxylic acids, the corresponding acid anhydrides, acid chlorides, esters and acid amides, amino acids, imines, nitriles, isonitriles, mono- and polyamines, β-dicarbonyl compounds such as β-diketones, oximes, alcohols, alkyl halides, and metal compounds that have a functional group that can react or interact with the surface of the particles, e.g., silanes with hydrolyzable groups or with at least one non-hydrolyzable group.
[0046] The nanoparticles have lipophilic groups on their surface.
[0047] The lipophilic groups located on the surface of the nanoparticles preferably comprise a lipophilic residue, wherein the lipophilic residue has in particular at least 4 and preferably at least 5 carbon atoms. Specific lipophilic groups are lipophilic alkyl, alkenyl, alkynyl, aryl, aralkyl, alkaryl, or ether residues, which have at least one group for binding to the surface of the nanoparticles. This can, for example, be at least one amino, alkylamino, thiol, hydroxyl, carboxylic acid, or phosphine group. The aforementioned lipophilic residues also include corresponding cyclic residues, such as cycloalkyloxy residues. In the case of phosphine, at least one residue on the phosphorus atom is a corresponding lipophilic residue.
[0048] The lipophilic radicals preferably have a saturated, unsaturated or aromatic, branched or unbranched hydrocarbon radical having at least 4 and preferably at least 5 carbon atoms, in particular at least 8 carbon atoms.
[0049] Examples of preferred alkyl groups are C 4 -C 30 alkyl, preferably C 5 -C 20 alkyl, such as n-butyl, i-butyl, sec-butyl, tert-butyl, linear or branched pentyl, hexyl, heptyl, octyl, such as 2-ethylhexyl, cyclohexyl, nonyl, decyl, undecyl, dodecyl, tridecyl, tetradecyl, pentadecyl, hexadecyl, heptadecyl, octadecyl, nonadecyl, eicosyl. The alkyl group can be branched or, preferably, linear. Examples of alkenyl groups are C 4 -C 30 alkenyl, preferably C 5 -C 20 alkenyl, such as butenyl, pentenyl, hexenyl, heptenyl, octenyl, nonenyl, decenyl, undecenyl, dodecenyl, tridecenyl, tetradecenyl, pentadecenyl, hexadecenyl, heptadecenyl, octadecenyl, and nonadecenyl. The alkenyl group can be branched or, preferably, linear; the double bond can be located at any position. More than one double bond can also be present. Examples of alkynyl groups are C 4 -C 30 alkynyl, preferably C 5 -C 20 alkynyl.
[0050] Lipophilic aryl, aralkyl, and alkaryl groups can have, for example, 6 to 30, preferably 6 to 15, carbon atoms. Examples are phenyl, naphthyl, tolyl, and benzyl. Suitable lipophilic ether groups have, for example, the general formula R 1< (-OR 2< ) x -, in which R 1< is a lipophilic alkyl group, R 2< is an alkylene group, e.g., having 1 to 4 carbon atoms, such as ethylene or propylene, and x is an integer from 1 to 4, preferably 1 or 2. The group R 1< is preferably a C 4 -C 20 alkyl group, such as butyl, pentyl, hexyl, cyclohexyl, heptyl, or octyl.
[0051] The lipophilic groups may be partially or fully fluorinated. Examples of fluorinated lipophilic C4-C20 alkyl groups include C2F5-CH2CH2, nC6F13-CH2CH2, nC8F17-CH2CH2, nC10F21-CH2CH2, iC3F7O-CH2CH2CH2, and nC6F13-CH2CH2. Optionally, other radicals may also be substituted by fluorine on at least one carbon atom. If the lipophilic group is such a fluorinated hydrocarbon chain, it may also comprise fewer than 4 carbon atoms, e.g., at least 1, and preferably at least 2, carbon atoms.
[0052] The surface modification can also include polymers that bind to the surface of the particles via the aforementioned groups. These can be, for example, polyethylene glycol derivatives, polyvinyl alcohol, polyacetylates, polyimides, polyvinyl ketones, polymethacrylates, dextrans, or biopolymers such as cellulose, chitosan, or heparin.
[0053] The choice of surface modification can be adapted to the nanoparticles. Mixtures of surface modifications can also be used.
[0054] The surface modification and the nanoparticles are selected depending on the chosen stimulus.
[0055] Preferably, the surface modification is applied in such a way that at least one dense monolayer forms on the surface of the particles. For a particle size of 4 nm, for example, this would be 300 to 1800 ligands per particle. The density of the ligands on the surface of the particles is, for example, 2-8 ligands / nm².
[0056] For example, surface modifications that decompose irreversibly are also possible, e.g., photolytically cleavable ligands, which can thus lead to an irreversible change in the arrangement, e.g., agglomeration. These can be groups based on photoinitiators, such as alpha-hydroxy ketones. They can also be thermally cleavable groups, such as azo initiators like AIBN or derivatives thereof, benzoyl peroxide.
[0057] Surface modification can involve combinations of ligands. For example, modification with functional silanes, such as aminosilanes, makes it possible to equip the surface of the nanoparticles with functional groups to which additional molecules, oligomers, or polymers can then be coupled.
[0058] It is also possible for the cavities to contain a separate stimulus acceptor, which transfers the energy to the nanoparticles that change the arrangement. These could, for example, be magnetic nanoparticles that can transmit a magnetic stimulus.
[0059] The nanoparticles themselves can also be suitable for absorbing a stimulus.
[0060] In the case of optical stimuli, these can be particles that absorb the corresponding wavelengths, such as plasmonic particles made of gold, silver, copper, platinum, and other coinage metals, as well as aluminum and other light metals; semiconductor nanoparticles that exhibit absorption and fluorescence as "quantum dots" due to their small size, such as cadmium selenide, cadmium sulfide, cadmium telluride, lead sulfide, silicon, and others; or doped oxide particles with intense absorption bands, such as metal and semiconductor oxides doped with transition metals. Further examples of such particles are mentioned under nanoparticles.
[0061] For magnetic stimuli, superparamagnetic particles made of iron oxides, nickel and other magnetic elements are particularly preferred.
[0062] For stimulation by microwaves and radio waves, nanoparticles of gold, silver, copper, and other coinage metals are particularly preferred, but all metals or highly doped semiconductors with sufficient charge carrier density and mobility are suitable, such as Fe 3 O 4 @SnO 2 :Er 3+< , Yb 3+< ).
[0063] Nanoparticles can also comprise more than one of the materials mentioned. For example, core-shell nanoparticles consist of different materials in the core and on the surface. Examples of these include "upconversion" nanoparticles, which comprise a doped oxide core and a metallic shell.
[0064] The absorption of the stimulus by absorption can, for example, cause local heating of the nanoparticles, as is the case with magnetic nanoparticles. In this case, all molecules that can be tightly bound to the nanoparticles and that, either alone or as a ligand shell, exhibit a temperature-dependent interaction with the surrounding solvent are preferred. Examples include self-assembled monolayers ("SAMs") of thiols or amines for coinage metals.
[0065] The stimulus can also change the charge of the nanoparticles or release free charge carriers. In this case, all molecules that can be tightly bound to the nanoparticles and that can absorb free charge carriers, either alone or as a ligand shell, are preferred as ligands. This, or the particle's charge, alters their interaction with the surrounding solvent.
[0066] The stimulus can also affect the surface modification, whereby the nanoparticle can act synergistically. In this case, all molecules that alter their interaction with the surrounding solvent through the stimulus, either alone or as a ligand shell, are preferred as ligands.
[0067] For example, the fluorescence of nanoparticles after absorption can excite photoactive ligands, which may change the arrangement of the nanoparticles through decomposition.
[0068] The stimulus can also release substances bound to the nanoparticles and / or their ligand shell. For example, by changing the charge or conformation, substances adsorbed in the ligand shell or non-covalently bound to it can be released into the solvent of the cavity. In the case of dyes, this can, for example, cause a color change.
[0069] In a preferred embodiment of the invention, the stimulus is temperature, ie the composite material is heated or cooled.
[0070] From Born et al. (Physical Review E 2013, 062313) and Geyer et al. (Physical Review Letters 2012, 109, 128302), it is known that the agglomeration of gold particles can be controlled by temperature-dependent ligand selection. For example, the temperature at which agglomerates form increases depending on the chain length of alkyl ligands.
[0071] Typically, this is achieved by the ligand shell around the nanoparticles changing as a function of temperature, thus altering the stability of the particle dispersion. This is achieved in nonpolar media with lipophilic surface modification, particularly for metallic particles. According to the invention, the cavities comprise at least one type of nanoparticle and at least one nonpolar solvent, with the at least one type of nanoparticle having a lipophilic surface modification. The matrix material is then preferably lipophobic.
[0072] Preferred surface modifications are lipophilic alkyl and alkenyl groups containing at least one thiol, amino, or hydroxyl group. Phosphines, such as triphenylphosphine, can also be used.
[0073] Whether a specific combination of modified nanoparticle and solvent allows transition between the two states at the desired temperature can be easily tested in the dispersion before the composite material is produced. Surprisingly, the results from the dispersion are transferable to the composite material.
[0074] Since the agglomeration of metallic particles in particular changes the surface plasmon, a color change of the composite material occurs, for example. Plasmonic nanoparticles, especially Au, Ag, or Cu, and especially Au, are therefore preferred.
[0075] The composite material also comprises a matrix. It can be organic, inorganic, or organically modified. These can be organic polymers or corresponding oligomers known to those skilled in the art, e.g., polyacrylates, polymethacrylates, polyolefins, e.g., polybutadiene, polystyrene, polyamides, polyimides, polyvinyl compounds such as polyvinyl chloride, polyvinyl alcohol, polyvinyl butyral, polyvinyl acetate, and corresponding copolymers, e.g., poly(ethylene-vinyl acetate), polyesters, e.g., polyethylene terephthalate or polydiallyl phthalate, polyarylates, polycarbonates, polyethers, e.g., polyoxymethylene, polyethylene oxide, or polyphenylene oxide, polyether ketones, polysulfones, polyepoxides, epoxy resins, and fluoropolymers, e.g., polytetrafluoroethylene. Functional groups can be present to adjust the lipophilicity or hydrophilicity of the matrix with respect to the interior of the cavities arranged in the matrix.
[0076] The matrix can be a polysaccharide matrix; preferably, the polysaccharides are selected from the group comprising cellulose esters, cellulose ethers, cellulose hydrate, agarose, chitin, chitosan, dextran, or combinations thereof. Optionally, the aforementioned polysaccharides can be cross-linked. The polysaccharide matrix can also be modified, for example, with the aforementioned polymers.
[0077] If optical transparency is required, it may be necessary to adjust the refractive index of the matrix and the interior of the cavities accordingly. This can be achieved, for example, by adding appropriate additives to the matrix, such as optically active fillers or solvents.
[0078] In a further embodiment of the invention, the cavities in the composite material are formed by microcapsules and / or nanocapsules. The production of microcapsules and / or nanocapsules is known in the art, for example, by interfacial polymerization. The capsules can then be incorporated into the matrix accordingly.
[0079] The invention also relates to a process for producing composite materials according to the invention. For this purpose, an emulsion comprising nanoparticles in the dispersive phase, wherein the nanoparticles have a lipophilic surface modification, is provided in the first step. A mixture of the hydrophilic matrix or a matrix precursor and the emulsion is then prepared, and the matrix is solidified, with the micelles of the emulsion forming cavities in the matrix that are filled with the dispersive phase of the emulsion.
[0080] Individual procedural steps are described in more detail below. The steps do not necessarily have to be performed in the order given, and the procedure described may also include additional steps not mentioned.
[0081] The emulsion also includes dispersants for stabilization. It can be an O / W or W / O emulsion. An O / W emulsion is preferred. The hydrophobic phase is the disperse phase.
[0082] An emulsion used preferably consists of an aqueous and an oily phase. Water or mixtures containing water and organic, preferably water-soluble solvents are preferred for the aqueous phase. The aqueous phase is particularly preferably water or mixtures of water and alcohols, aldehydes, and / or ketones, particularly preferably water or mixtures of water with mono- or polyhydric alcohols having up to four carbon atoms, such as methanol, ethanol, n-propanol, isopropanol, glycerol, or ethylene glycol, aldehydes having up to four carbon atoms, such as formaldehyde, and / or ketones having up to four carbon atoms, such as acetone or methyl ethyl ketone.
[0083] The oil phase preferably contains at least one organic solvent that is insoluble in the aqueous phase. These are preferably aromatic or aliphatic hydrocarbons having at least 5 carbon atoms, such as petroleum ether, hexane, heptane, decane, undecane, especially n-hexane, n-heptane, n-decane, n-undecane, toluene, benzene, cyclopentane, tetralin, or cyclohexane; halogenated aromatic or aliphatic hydrocarbons such as dichloromethane, dichloromethane, chloroform; alkyl acetates such as butyl acetate; and ketones such as acetophenone or cyclohexanone. Mixtures of the solvents can also be used. Preference is given to solvents with a boiling point above 80°C, especially above 120°C.
[0084] Solvents with a boiling point above 80 °C are preferred for both phases of the emulsion.
[0085] The matrix material represents the non-disperse phase of the emulsion. This means that the matrix material is preferably also lipophilic or hydrophilic. The nanoparticles, which may optionally be surface-modified as described above, are arranged in the disperse phase.
[0086] The preferred emulsion is a microemulsion or nanoemulsion. The disperse phase of the emulsion determines the shape of the cavities in the final composite material.
[0087] The disperse phase therefore already includes everything that is necessary for the later transformation from a first to a second state.
[0088] Those skilled in the art are aware of ways to influence the size of the micelles in an emulsion. This can be achieved, for example, by selectively evaporating the dispersed phase, by filtration, and / or by applying shear forces, such as with an Ultra Turrax. The process can also comprise several of these steps and combinations thereof.
[0089] The dispersant can be selected according to the emulsion and the nanoparticles. Examples of non-ionic dispersants are polyoxyethylene ethers, such as lauryl, oleyl, stearyl, or tridecyl ethers.
[0090] The dispersant is preferably used above the critical micelle concentration (CMC), particularly with respect to the selected temperature.
[0091] Transparent emulsions can be achieved either by using appropriately small micelles or by adjusting the refractive indices of the emulsion phases. Adjusting the refractive indices is preferred.
[0092] A mixture of the matrix or a precursor thereof and the emulsion is then prepared. A precursor of the matrix can be, for example, a monomer or oligomer that still needs to be cured by polymerization. It can also be the matrix material itself, for example, if it is liquid at elevated temperatures or only cures upon subsequent removal of solvent.
[0093] In the next step, the matrix is solidified. Depending on the matrix, this can be any physical or chemical reaction that stabilizes the matrix and thus encapsulates the micelles within it. This can involve cooling the matrix or polymerization reactions.
[0094] The process yields a composite material according to the invention, wherein the preferred embodiments mentioned above for the composite material also apply to the production process.
[0095] The composite material according to the invention can be used in many ways depending on the chosen stimulus.
[0096] For example, it can be used as a sensor material for the stimulus.
[0097] Further details and features will become apparent from the following description of preferred embodiments in conjunction with the subclaims. The respective features can be implemented individually or in combination with one another. The possibilities for solving the problem are not limited to the embodiments. For example, range specifications always include all intermediate values (not mentioned) and all conceivable subintervals.
[0098] The exemplary embodiments are illustrated schematically in the figures. Identical reference numerals in the individual figures denote identical or functionally identical elements, or elements that correspond to one another in terms of their functions. In detail: Fig. 1Schematic representation of the composite material in the first state (a) and in the second state (b); Fig. 2UV-Vis spectra of various particle dispersions at 10 °C and 50 °C, or 52 °C; Fig. 3UV-Vis spectra of various prepared composite materials at 10 °C and 50 °C; Fig. 4SAXS measurement of the particle dispersion of a) gold nanoparticles (3.62 nm) with PPh 3 and C 12 -thiol; c) the corresponding structure factor; b) SAXS measurement of gold nanoparticles (3.98 nm) with PPh 3 and C 12 -thiol; d) the corresponding structure factor; Fig. 5SAXS measurement of the particle dispersion of a) gold nanoparticles (1.88 nm) with C 6 -thiol; c) the corresponding structure factor; b) SAXS measurement of particle dispersions of gold nanoparticles (2.65 nm) with C 16 thiol; d) the corresponding structure factor; Fig.6SAXS measurement of the composites with a) gold nanoparticles (3.62 nm) with PPh 3 and C 12 -thiol; c) the corresponding structure factor; b) SAXS measurement of the composites with gold nanoparticles (3.98 nm) with PPh 3 and C 12 -thiol; d) the corresponding structure factor; Fig. 7SAXS measurement of the composite materials with a) gold nanoparticles (1.88 nm) with C 6 -thiol; b) the corresponding structure factor; Fig. 8SAXS measurement of the composite material 3.98 nm PPh 3 C16 for 5 temperature cycles (a) to (e); Fig. 9SAXS measurement of the composite material 3.62 nm PPh 3 C12 for 5 temperature cycles (a) to (e); .
[0099] Figure 1 shows a preferred embodiment of the invention. The composite material comprises a matrix material 100 in which cavities 110 are arranged. Nanoparticles 120 are arranged in these cavities ( Figure 1 a)). When an external stimulus 130 acts on the composite material, agglomerates 140 form within the cavities 110. This change also leads to a change in a property of the composite material. For example, absorption changes in a specific wavelength range. The stimulus must be transmitted through the matrix 100 to the nanoparticles 120, i.e., the matrix must be permeable to the stimulus or be able to transmit it accordingly.
[0100] Gold nanoparticles were used for the experiments. Agarose was used as the matrix material. Agarose is stable towards organic solvents and easy to handle. Materials and methods Small-Angle X-Ray Scattering (SAXS)
[0101] The measurements were recorded on a Xenocs Xeuss 2.0 equipped with a Dectris Pilatus 3 1 MR detector with a resolution of 981 x 1043 pixels and a pixel size of 172 x 172 µm². The sample distance to the detector was approximately 1240 mm. An additional structure factor can be measured when the nanoparticles agglomerate in the composite material. The data were analyzed using SASfit 0.94.6.
[0102] Polyimide capillaries were used to measure the dispersions. Pure solvent was measured as background. For the composite measurements, 1 mm thin strips were cut from the materials and measured. Samples without particles were measured as background. UV-Vis spectroscopy
[0103] The measurements were performed on an HR 2000+ High Resolution Spectrometer from Oceans Optics Inc. with a Mikropack DH-2000-BAL UV-VIS-NIR light source. Absorption and scattering (haze) were measured.
[0104] For the dispersion measurements, they were diluted. Pure solvent was measured as background. For composite materials, this was prepared directly in the cuvettes. Production of gold nanoparticles
[0105] The nanoparticles were prepared according to literature methods. An orange solution of HAuCl4 and oleylamine ((Z)-octadec-9-enylamine) in benzene, toluene, hexane, or pentane was mixed with an excess of tert-butylamine borane complex (TBAB) in oleylamine and benzene or hexane. The mixture was treated with ultrasound to dissolve the reducing agent TBAB. The proportion and type of organic solvent used influence the size distribution of the resulting particles. This reaction yields gold nanoparticles that are stabilized by the amines used.
[0106] To adjust the properties of the particles, the amino ligands can be exchanged for groups that bind more strongly to the surface of the gold particles, for example phosphines such as triphenylphosphine or thiols such as alkylthiols.
[0107] For example, a solution of 25 mg AuCl 4 in 2.5 ml oleylamine (70%) and 2.5 ml solvent was mixed with a solution of 15 mg TBAB, 1.5 ml oleylamine, and 1.5 ml solvent. The mixture was stirred at constant temperature for 60 minutes. The resulting particles were then precipitated by adding ethanol. The mixture was centrifuged at 4000 rpm at room temperature. The supernatant was removed, and the particles were suspended in pure solvent.
[0108] For ligand exchange, the suspension was heated to 90 °C and the new ligand, for example, thiol, phosphine, or a mixture of both, was added. In a mixture, the phosphine was added first. The suspension was cooled to room temperature, the particles precipitated, and resuspended in decane.
[0109] The ligands used were 1-hexanethiol (C6), 1-dodecanethiol (C12), 1-hexadecanethiol (C16), or triphenylphosphine, as well as mixtures. Decane was always used as the solvent for the particles.
[0110] The C16 thiols stabilize gold nanoparticles with a diameter of 2.65 nm. The transition temperature for agglomeration was 35 °C for hexane. In tetradecane, this temperature is 42 °C.
[0111] The transition temperature can be adjusted accordingly by selecting the ligand and solvent. An overview is shown in Table 1. + indicates the formation of agglomerates at the corresponding temperature, and - indicates the absence of agglomerates.
[0112] The systems can be divided into two types. If the melting temperature of the ligand shell of the nanoparticle is above the agglomeration temperature, the system is called ligand-dominated. If the agglomeration temperature is above the melting temperature of the ligand shell, the system is called particle-dominated. Of the systems used in Table 1, 3.98 nm and 2.65 nm are ligand-dominated, and 3.62 nm and 1.88 nm are particle-dominated. Emulsions
[0113] To produce the composite material, emulsions with micelles were first prepared according to the desired size of the cavities in the composite material.
[0114] Triton X165 (octylphenol ethoxylate) was used as the nonionic surfactant. This surfactant has a critical micelle concentration (CMC) of 570 ppm at 25 °C.
[0115] Transparent emulsions can be achieved either by using appropriately small micelles or by adjusting the refractive indices of the phases of the emulsion.
[0116] To prepare transparent emulsions containing small micelles, 14 ml of Millipore water and 2 ml of Trition X165 (6.25 CMC) were mixed. 4 ml of hexane and 100 µl of nanoparticle dispersion (6 mg gold / ml) in decane were added. The mixture was treated with Ultra Turrax at 24,000 rpm for 20 minutes. An emulsion with a micelle size of up to 25 µm was obtained. The emulsion was filtered through Chromafil RC 45 / 25 syringe filters (pore size 450 nm) and then Chromafil RC 20 / 25 syringe filters (pore size 200 nm). The resulting emulsion showed a maximum micelle size of 2 µm. The emulsion was heated to 60 °C and stirred at 1,000 rpm. Once a sufficiently small micelle size was reached, the emulsion became transparent.
[0117] To prepare transparent emulsions by index matching, a mixture of 4 ml water, 6 g glycerol (propanetriol), 1 ml Trition X165, and 1 ml gold nanoparticle dispersion in decane was stirred with a magnetic stirrer at 1600 rpm for 5 minutes. A homogeneous transparent emulsion was obtained.
[0118] Transparent emulsions from the dispersions shown in Table 1 for particles with 3.98 nm, 3.62 nm, and 1.88 nm were prepared by adjusting the refractive indices. For the emulsion with 2.65 nm particles, transparency was achieved by the formation of small micelles. Production of the composite material
[0119] 100 mg of agarose was added to 2 ml of the prepared emulsions. The mixture was stirred in a preheated aluminum block at 112 °C. The agarose was boiled for 4:30 minutes. For samples with refractive index adjustment, 120 mg of agarose and 2 ml of the respective emulsion were used. These mixtures were treated for 4:30 minutes at 125 °C. In the case of UV-Vis measurements, the mixture was heated directly in the measuring cuvettes.
[0120] The mixtures were then degassed in an ultrasonic bath (45 °C, 20 s). Results
[0121] All data in the figures refer to dispersions according to Table 1, as well as composite materials prepared with these dispersions. For characterization, the particle size and the ligand used are indicated.
[0122] Figure 2shows UV-Vis spectra (each normalized to 1) for different particle dispersions from Table 1 at 10 °C and 50 °C, or 52 °C. The particle diameters and the respective ligands are indicated in the spectrum. It can be seen that in all cases, there is a shift in the maximum of the spectrum. This indicates the formation of agglomerates. The cool dispersions also show higher absorption between 550 nm and 1100 nm. This also indicates the formation of agglomerates.
[0123] Figure 3 shows UV-Vis spectra of composites prepared with the corresponding dispersions. The shift of the maximum is also clearly visible in the composite.
[0124] The Figures 4 and 5show SAXS measurements of prepared particle dispersions at 10 °C and 50 °C, as well as the resulting structure factors. The structure factors clearly show that agglomerates form at low temperatures. A q-value of 0.07 Å -1< in Figure 4 d) corresponds to a distance of the particle centers of 8.9 nm on average. The q-values of 0.077 Ä and 0.147 Ä in Figure 4c ) correspond to distances of 8.15 nm and 4.27 nm, respectively. This indicates that in this case the particles in the agglomerate are partially arranged in an fcc lattice. A q-value of 0.126 Å 1< in Figure 5c ) represents a distance of 5.0 nm. The q-value of 0.092 Å -1< in Figure 5 d) represents a distance of 6.8 nm.
[0125] The Figures 6 and 7SAXS measurements of manufactured composite materials show that particle agglomerates also form within the composite materials. The q values are similar to those measured for the dispersions.
[0126] All composite materials could be heated and cooled several times, with the corresponding transformation of the nanoparticles being observed each time. To obtain a better signal for the 1.88 nm C6 composite, a higher concentration of particles in the emulsion was used for this sample.
[0127] More precise measurements of the structure factor revealed that for the 3.98 nm PPh 3 C16 system, the transition from agglomerate to free particles occurred at 42 °C upon heating, and the formation of agglomerates occurred at 35 °C upon cooling. For 3.62 nm PPh 3 C12, temperatures of 52 °C and 38 °C, respectively, were measured.
[0128] A significant color change of the composite material was observed upon formation of agglomerates.
[0129] Figure 8 shows several SAXS measurements for a composite material (3.98 nm PPh 3 C16) for several consecutive temperature cycles. The sample had already been stored at room temperature for 1.5 months. During heating, the sample was heated to 50 °C and held at this temperature for 25 minutes. 5 minutes after reaching this temperature, the measurement was started. The sample was then cooled to 10 °C and held at this temperature for 25 minutes, with the measurement starting after 5 minutes. During the first heating ( Figure 8 a )) not all agglomerates had dissolved at 50 °C. In the following cycles (Figure 8 b) to e)), the agglomerates clearly dissolved at the high temperature and reformed at the low temperature.
[0130] Figure 9shows several SAXS measurements for a composite material (3.62 nm PPh 3 C12) for several consecutive temperature cycles. The sample had already been stored at room temperature for 1.5 months. During heating, the sample was heated to 50 °C and the temperature was held for 25 minutes (approximately 35 minutes in the first cycle). Five minutes after reaching this temperature, the measurement began. The sample was then cooled to 10 °C and this temperature was held for 25 minutes, with the measurement starting after 5 minutes. During the first cycle (Figure 9 a)), complete deagglomeration was not yet observed. Figure 8 f) shows the change in the structure factor in the first cycle against time. It is clearly visible that deagglomeration is only complete after 30 minutes. Therefore, agglomerates were still present at the start of the measurement in the fifth minute. Table 1 Radius [nm] ligand solvent Agglomeration at 0 °C RT 50 °C 1,88 C6 dean + - - 2,65 C16 dean + + - 3,62 PPh 3 , C12 dean + + - 3,98 PPh 3 , C16 dean + + - Reference symbol
[0131] 100Matrix 110Cavities 120Nanoparticles 130Stimulus 140Agglomerates of nanoparticles cited literature
[0132] Born et al Physical Review E 2013, 062313 Geyer et al. Physical Review Letters 2012, 109, 128302
Claims
1. Composite material comprising a) a hydrophilic matrix; b) cavities, with the cavities comprising at least one kind of nanoparticles, characterized in that at least one of the cavities can be converted, by action of temperature on the composite material, from a first state into a second state, with the first state differing from the second state in the arrangement of the nanoparticles within the at least one cavity, and the nanoparticles are present in agglomerated form in one of the two states, with the cavities comprising at least one kind of nanoparticles and at least one non-polar solvent, with the at least one kind of nanoparticles having a lipophilic surface modification, with the nanoparticles being in dispersion in the solvent.
2. Composite material according to Claim 1, characterized in that the nanoparticles are plasmonic nanoparticles.
3. Composite material according to either of Claims 1 and 2, characterized in that the change between the two states is reversible.
4. Composite material according to any of Claims 1 to 3, characterized in that the matrix is solid, while the composition within the cavities is liquid or viscous.
5. Composite material according to any of Claims 1 to 4, characterized in that the nanoparticles are gold nanoparticles and the matrix is agarose.
6. Process for producing a composite material according to any of Claims 1 to 5, comprising the steps of a) providing an emulsion comprising nanoparticles in the dispersive phase, with the nanoparticles having a lipophilic surface modification; b) producing a mixture comprising hydrophilic matrix or a precursor thereof; c) solidifying the matrix, with the micelles of the emulsion forming cavities in the matrix that are filled with the dispersive phase of the emulsion.
7. Process according to Claim 6, characterized in that the emulsion is a microemulsion or nanoemulsion.
8. Process according to either of Claims 6 and 7, characterized in that the nanoparticles are gold nanoparticles and the matrix is agarose.