METHOD FOR CHANGING THE MORPHOLOGY OF A SUPERABSORBENT POLYMER, NAMELY A SAP POLYMERGEL, USING A SINGLE-SHAFT EXTRUDER

DE502017016521D1Active Publication Date: 2024-11-14BASF SE
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
DE502017016521
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Priority Date
2016-12-21
Filing Date
2017-12-15
Publication Date
2024-11-14
Estimated Expiration
2037-12-15

AI Technical Summary

Technical Problem

Existing methods for producing superabsorbent polymer gels using single-screw extruders often result in undesirable morphology changes or destruction of the desired morphology, particularly at high throughput, leading to compromised water absorption and centrifuge retention capacities.

Method used

A single-screw extruder design with adaptive geometry, including varying pitch values and increasing shaft diameter along the conduit, is used to minimize specific mechanical energy input while maintaining high throughput, promoting a desired morphology that enhances water absorption and permeability of the SAP polymer gel.

Benefits of technology

The method allows for high throughput of SAP polymer gel with improved water absorption and centrifuge retention capacity, maintaining desired morphology and reducing energy consumption, thereby producing durable and efficient water-absorbing polymer particles.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The present invention relates to a method according to the preamble of claim 1 for changing a morphology of a superabsorbent SAP polymer gel using a single-screw extruder.

[0002] WO 2014 / 118024 A1 describes a process for producing water-absorbing polymer particles with high swelling rates and high centrifuge retention capacity, coupled with high permeability of the swollen gel bed, by polymerizing an aqueous monomer solution in a polymerization reactor with at least two axially parallel rotating shafts (kneader). The resulting polymer gel is then subjected to extrusion at high temperatures and thermal surface post-crosslinking. The polymer gel has a temperature greater than 80°C during extrusion, and less than 60 kWh / t of specific mechanical energy is introduced during extrusion. The specific mechanical energy (SME) introduced during extrusion can be influenced, for example, by the ratio of the internal length to the internal diameter of the extruder (L / D).The specific mechanical energy (SME) is the extruder motor power in kW divided by the polymer gel throughput in t / h. Short extruders are advantageously used. This avoids excessive pressures during extrusion. During extrusion, the polymer gel is forced through the holes of a die plate. The properties of water-absorbing polymer particles can be improved if more highly cross-linked polymer gels produced in a polymerization reactor with at least two shafts rotating parallel to the axis are additionally extruded at higher temperatures. The resulting shear forces lead to rougher polymer particles, which, after thermal surface post-crosslinking, exhibit a high swelling rate (FSR) and a high centrifuge retention capacity (CRC). However, excessive energy inputs during extrusion lead to a deterioration in the swelling rate (FSR) and the centrifuge retention capacity (CRC) and should therefore be avoided.The teaching and content of patent application WO 2014 / 118024 A1 known from WO 2014 / 118024 A1 are part of this text and are incorporated herein by reference to WO 2014 / 118024 A1.

[0003] JP2001 079829 A2 describes a process for producing a water-absorbent resin with excellent physical properties by safely blending a fine powder with a water-containing gel-like polymer, thereby producing the water-absorbent polymer with high efficiency. Fine powder of a water-absorbent gel-like polymer with a size smaller than a specified range, which is produced in the production process of the water-absorbent resin, and fine powder of an additive for improving various properties of a water-absorbent resin with the coarsely ground, water-containing gel-like polymer, are fed from a feed port of a screw extruder; they are kneaded in a constant-pressure section of a barrel of the screw extruder.Then, the hydrous gel-like polymer is extruded while increasing the compression force on the hydrous gel-like polymer in a compression section of the screw extruder barrel near an extrusion orifice provided with a porous plate. That is, a method is used in which fine powder is added to a hydrous gel prior to fine pulverization, and then the entire mixture is kneaded using a screw extruder to continuously extrude a hydrous gel until a compression force is increased near the extrusion orifice of the screw extruder.

[0004] Specifically, the housing has a cylindrical shape, and a FIG. 1The screw shown in JP2001 079829 A2 is arranged within the housing along the longitudinal direction of the housing. At one end of the cylindrical housing, the extrusion opening for extruding and granulating the water-containing gel is provided. In particular, as shown in FIG. 1 As shown in JP2001 079829 A2, the hydrous gel and the fine powder are fed from the feed opening into the casing without being sufficiently mixed. The hydrous gel and the fine powder fed into the casing are mixed (kneaded) by the rotation of the screw. When the screw is rotated, since the water is conveyed to the side of the extrusion opening rather than mixing, an external force is exerted on the hydrous gel. Therefore, a uniform pressure is exerted on the hydrous gel to such an extent that the hydrous gel does not compress. In addition, as shown in FIG. 1As shown in JP2001 079829 A2, a large part of the casing, in which such uniform pressure is exerted on the hydrous gel, is used as a pressure equalizing part. On the other hand, since the perforated plate is provided in the extrusion opening, the hydrous gel near the extrusion opening is not easily pushed out but is compressed by the rotation of the screw. In addition, as described above, since the hydrous gel and the fine powder in the casing are conveyed to the extrusion opening by the rotation of the screw, the compression force is further increased. As a result, the hydrous gel and the fine powder are stirred and mixed while being compressed and extruded from the extrusion opening of the perforated plate. FIG. 1As shown in JP2001 079829 A2, the area around the extrusion orifice, to which such a compression force is applied, is defined as the compression section. This allows the dried fine powder to be uniformly mixed with the hydrous gel. This method allows the fine powder to be safely and sufficiently mixed into the hydrous gel-like polymer, forming it into fine granules. The granulated hydrous gel is dried with hot air.

[0005] The invention uses a single-screw extruder for changing a morphology of superabsorbent polymer gel (SAP polymer gel), namely comprising: an inlet opening for supplying SAP polymer gel, a conduit connected to the inlet opening, a screw shaft arranged in the conduit for conveying and changing the morphology of the SAP polymer gel, and an outlet opening connected to the conduit, preferably also for changing the morphology, for discharging the SAP polymer gel with changed morphology.

[0006] The screw shaft has a shaft and a screw arranged on the shaft and is arranged and designed to transport the SAP polymer gel from the inlet opening to the outlet opening by means of the screw.

[0007] The duct has an inlet zone arranged at or near the inlet opening, an outlet zone arranged at or near the outlet opening and a conveying zone extending along the duct from the inlet zone to the outlet zone.

[0008] Such single-screw extruders are generally known from the state of the art and are used, among other things, to convey solid or viscous masses according to the functional principle of a screw conveyor and to give the mass a shape.

[0009] Such single-screw extruders have, for example, a screw shaft arranged in a housing, which is typically rotated about its longitudinal axis by a drive motor. The screw shaft has a screw and a shaft. The screw extends along a longitudinal axis of the shaft. The housing is typically cylindrical, so that the screw of the screw shaft is adjacent to the housing wall. The interior of the housing can be divided into an inlet zone, a conveyor zone, and an outlet zone, known as the dosing zone. Material is typically fed into the inlet zone of the single-screw extruder via a hopper through an inlet opening. When the single-screw extruder is filled with material, the rotation of the screw shaft conveys the material along the housing from the inlet zone via the conveyor zone to the outlet zone.Furthermore, friction is generated between the rotating mass and the stationary housing wall, whereby pressure can be built up and extrusion or pressing out through a shaping outlet opening at the end of the outlet zone, i.e. behind the dosing zone, of the single-screw extruder is enabled.

[0010] Such a screw as mentioned above has, among other parameters, a pitch G or lead, a shaft diameter d, and an outer screw diameter D. The pitch corresponds to the distance between two screw turns. Screws can be categorized by the ratio of shaft diameter d to outer screw diameter D, i.e. a value d / D. A d / D ratio between 0.3 and 0.5 is what is known as a deep-cut screw, which enables high throughput. A d / D ratio between 0.7 and 0.9 is what is known as a shallow-cut screw, which enables high pressure but has a lower throughput than the deep-cut screw.

[0011] EP 1 510 317 B1 shows in its Fig.1a screw extruder with an upwardly opening feed opening, a cylindrical tube, and a screw section. The screw section is driven by a motor and rotates within the cylindrical tube section. At the front end of the tube section is a perforated extrusion plate with a multitude of small holes. The screw section conveys cut pieces along the tube section to the perforated extrusion plate. The pieces are pushed through the extrusion plate and formed into hydrogel particles. The pitch of the screw is adjusted according to this Fig.1 larger in the input zone than in the conveyor zone.

[0012] EP 2 557 095 A1 shows in its Fig.1a screw extruder with a cylindrical housing, a base, a screw, a feed opening, a hopper, an extrusion opening, a perforated nozzle, a rotating blade, a ring, a backflow prevention part, and a motor. Hydrogel is fed into the housing via the hopper of the feed opening from above. The screw is arranged in the housing. The rotating blade can be arranged on the screw. The motor drives the screw. The screw is used to convey the hydrogel along the screw extruder, which then extrudes it from the extrusion opening through the perforated nozzle and the rotating blade. The pitch of the screw is according to this Fig.1 larger in the input zone than in the conveyor zone.

[0013] JP 2005-272653 A shows a screw extruder for processing a hydrogel, comprising, among other things, a screw housing, a screw shaft, a filling opening, an exit opening, and a screw. The screw shaft of the screw extruder is designed to prevent backflow of water-containing gel to the feed side. For this purpose, the screw shaft has side section lengths corresponding to the ratio C=(B / A)x100, where C lies in a range between 100% and 500%. A corresponds to the side section length between the proximal end of the screw and the distal end of the filling opening, and B corresponds to the side section length between the distal end of the filling opening and the distal end of the screw.

[0014] JP 2002-177807 A shows a screw extruder for processing a hydrogel, comprising a housing, a feed opening, a screw, a rotating blade, and a perforated plate. Raw material is fed into the housing through the feed opening. The raw material is conveyed along the housing by means of the screw. The rotating blade is positioned at the end of the screw, between it and the perforated plate, allowing the raw material to be cut and extruded through it.

[0015] The book "Applied Plastics Engineering Handbook: Processing and Materials," by Myer Kutz, 1st edition 2011, pages 227 to 267, defines the screw geometry parameters of extruders for plastics processing. Typical screws have a constant helix angle of 17.7° and a constant pitch. Figure 15.22 of the book shows the structure of a screw with a constant helix angle and a constant pitch. The screw has a shaft diameter that increases along its longitudinal axis and a constant outer screw diameter. Another screw with three constant pitch sections has a constant pitch in each zone: a constant pitch with a helix angle of 17.7° in an entry zone, a larger constant pitch in a feed zone, and a constant pitch with a helix angle of 17.7° in the exit zone.

[0016] JP 2001 301006 A2 describes a method in which a thermoplastic resin composition is fed to a multi-part extruder and melted in a first part of the extruder and thereafter, in a second part of the extruder, a non-reactive gas in a high-pressure state is fed to the extruder (in a first cylinder section having a deep groove section 21b) to dissolve a non-reactive gas in the molten resin, and then a part of the gas is discharged (in an unfilled resin section 21c where the screw pitch is widened) while reducing a pressure, and then a molded body is formed in a third part of the extruder.

[0017] As in FIG. 1 As shown in JP 2001 301006 A2, the extruder uses a single screw shaft with a screw arranged in a cylinder. The shaft type can be cylindrical or conical.

[0018] The first part of the extruder is formed with a resin metering section 21a. In the second part of the extruder, the first cylinder section is formed with the deep groove section 21b, in which the screw groove depth is deep. This is followed by a tapered shaft section. Only then is the second cylinder section formed with the unfilled resin section 21c, where the screw pitch is widened and the shaft section is cylindrical; that is, in this order, the second cylinder section follows the first cylinder section in the second part of the extruder.

[0019] Thereby, the resin transportability at the position where the gas discharge device is connected (the unfilled resin portion 21c) becomes larger than the resin transportability at an upstream side of the position where the gas discharge device is connected.

[0020] The object of the invention is to provide a method for changing the morphology of a superabsorbent polymer, namely an SAP polymer gel, using an improved single-screw extruder, in which the lowest possible specific mechanical energy consumption (SME) has to be used for the highest possible throughput.

[0021] This object is achieved according to the invention by a method using a single-screw extruder for changing the morphology of superabsorbent polymer gel (SAP polymer gel), which extruder has an inlet opening, a feed channel, a screw shaft, and an outlet opening. The inlet opening is designed to feed SAP polymer gel. The feed channel is connected to the inlet opening. The screw shaft is arranged in the feed channel and is designed to convey and change the morphology of the SAP polymer gel. The outlet opening is connected to the feed channel, preferably for changing the morphology, for discharging the SAP polymer gel with the changed morphology. The screw shaft has a shaft and a screw arranged on the shaft and is arranged and designed to convey the SAP polymer gel from the inlet opening to the outlet opening by means of the screw.The duct has an inlet zone arranged at or near the inlet opening, an outlet zone arranged at or near the outlet opening and a conveying zone extending along the duct from the inlet zone to the outlet zone.

[0022] According to the invention, it is provided that the screw shaft has a first pitch value of a pitch of the screw along the conveying zone of the conduit channel and has a second pitch value of the pitch of the screw along the conveying zone of the conduit channel following in the conveying direction, and wherein the second pitch value is lower than the first pitch value according to the invention.

[0023] The SAP polymer gel can, for example, contain a superabsorbent such as a copolymer of acrylic acid and sodium acrylate. In its dry state, the superabsorbent polymer (SAP) is in powder form. A dry state here describes a state in which the SAP has not come into contact with liquid or has been dried. If the SAP comes into contact with liquid, it swells and forms a hydrogel or polymer gel. The single-screw extruder is designed to convey an SAP polymer gel, for example, resulting from a polymerization process, and to change its morphology. The SAP polymer gel is therefore in a state in which the SAP has come into contact with liquid.

[0024] The invention recognizes that high throughput of SAP polymer gel through prior art single-screw extruders could typically produce an undesirable morphology or destroy a preferred morphology of the SAP polymer gel. A desirable morphology of the SAP polymer gel involves improving water absorption, particularly by increasing the surface porosity and / or permeability of the SAP polymer gel. It has been difficult to increase throughput without losing the desired morphology of the SAP polymer gel. One aspect of the invention is that a relatively high throughput of SAP polymer gel through the single-screw extruder is possible while simultaneously producing SAP polymer gel with a desired morphology.

[0025] The invention includes the discovery that it is advantageous to adapt the geometry of the screw of the single-screw extruder to the SAP polymer gel to be conveyed and morphologically modified, so that the lowest possible specific mechanical energy input is required. The single-screw extruder is designed to produce a desired morphology that improves water absorption without introducing a large amount of specific mechanical energy (SME) into the SAP polymer gel. A further aspect of the invention is that the invention enables a high throughput of SAP polymer gel. Furthermore, the invention enables the production of durable SAP polymer gel. In particular, the invention can improve the conveying properties of the SAP polymer gel along the feed channel.Furthermore, a favorable polymer morphology can be achieved or maintained while increasing the throughput of SAP polymer gel through the feed channel. Another aspect is that lower energy consumption per material is required, as higher conveying efficiency is possible, and consequently, higher throughput is enabled. As a result, a smaller and more cost-effective single-screw extruder can be provided.

[0026] After the morphology has been altered using the single-screw extruder and the desired morphology of the SAP polymer gel is achieved, the SAP polymer gel can be subjected to a drying process, for example. Preferably, the morphology of the SAP polymer gel should be altered in such a way that the water absorption and / or absorption rate of the SAP polymer gel is increased. This is possible, for example, by increasing the surface porosity and / or permeability. Overall, the water-absorbing polymer particles should exhibit a high swelling rate and high centrifuge retention capacity while simultaneously maintaining high permeability.

[0027] Further process steps can be applied to the SAP. For example, the SAP dried in the drying process can be ground in a mill to produce SAP particles of various sizes. These can then be sieved out, for example, using sieves with different pore openings, whereby SAP particles of various sizes can be separated. The SAP particles of various sizes separated in this way can then be remixed, for example according to the desired size mixtures, to obtain an SAP particle mixture with desired properties, such as a specific particle size distribution (PSD). Subsequently, further process steps, such as surface cross-linking (SXL), can be carried out to further improve the properties of the SAP particle mixture.In SXL, additional substances are applied to the surface of each SAP particle. When the SAP particle mixture is heated with the substances present on the surface, a network forms on the surface of the respective particles. This network can, for example, help maintain the shape of the particles in a swollen state—i.e., when the SAP particle mixture has come into contact with a liquid and has taken on the form of an SAP polymer gel—and thus increase the holding capacity or centrifuge retention capacity when liquid is absorbed. In particular, the additional surface network can increase the holding capacity under increased pressure on the SAP polymer gel.

[0028] Advantageous further developments of the invention can be found in the dependent claims and specify in detail advantageous possibilities for realizing the concept explained above within the scope of the task and with regard to further advantages.

[0029] In a preferred development, the screw shaft has at least three different pitch values ​​of the screw along the guide channel. For example, the screw can have three different pitch values, of which the first pitch value is the largest. In this case, the second pitch value is preferably the second largest and the third pitch value is the smallest. For example, the first pitch value can lie in the inlet zone and the other two pitch values ​​in the conveying zone. However, all three different pitch values ​​can also lie in the conveying zone, wherein a first pitch value in the conveying direction along the guide channel can be, for example, greater than a third pitch value in the conveying direction along the guide channel, but smaller than a second pitch value in the conveying direction along the guide channel.The pitch can therefore first increase and then decrease again, or first decrease and then increase again. For example, the screw shaft can also have four different pitch values ​​along the conveyor channel, e.g., two different pitch values ​​along the entry zone and two different pitch values ​​along the conveying zone. This means that a first pitch value in the entry zone can already be greater than a second pitch value following in the conveying direction. The screw shaft can also have different pitch values ​​in the exit zone. In particular, a first pitch value in the exit zone can also be greater than a second pitch value following in the conveying direction.

[0030] In a further development, the screw shaft has a screw pitch that changes at least twice along the conveying zone of the duct.

[0031] In a further preferred development, the pitch of the screw decreases along the conveying zone of the conduit channel, i.e. a first pitch value located at the transition between the inlet zone and the conveying zone is greater than a subsequent pitch value in the conveying direction, and the pitch value located at the transition between the conveying zone and the exit zone is the smallest along the conveying zone. The pitch in the conveying zone can decrease, for example, linearly, exponentially, or stepwise along the conveying direction. This makes it possible to reduce the volume in which the SAP polymer gel is located along the conveying zone. As a result, the pressure acting on the SAP polymer gel along the conveying zone between the inlet opening and the exit opening can be increased.

[0032] Preferably, the screw pitch decreases continuously along the conveying zone of the feed channel. This allows for a continuous increase in the pressure acting on the SAP polymer gel along the conveying zone between the inlet and outlet openings. A continuous pressure change enables more homogeneous SAP polymer gel production and can improve conveying behavior.

[0033] In a further development, the single-screw extruder can have a screw with at least one pitch value of the screw that lies between 30 mm and 800 mm, for example between 350 mm and 500 mm. The screw can, for example, have a first pitch value of 500 mm, a second pitch value of 460 mm, and a third pitch value of 350 mm. The screw can, for example, also have just two different pitch values, for example 600 mm and 500 mm. The pitch values ​​of the screw can also change continuously along the duct between 800 mm and 30 mm, in particular between 500 mm and 350 mm. For example, the pitch can change continuously along the duct by the pitch value decreasing from 500 mm near the inlet opening to 350 mm near the outlet opening.

[0034] According to the invention, the diameter of the screw shaft increases along the feed channel. This allows the free transport volume to be reduced and thus the pressure acting on the SAP polymer gel to be increased.

[0035] Preferably, the single-screw extruder has a screw running width value between 4 mm and 80 mm, for example 40 mm.

[0036] In a further development, the single-screw extruder can have at least one value of a conveying chamber height between the shaft of the screw shaft and a wall of the duct between 25 mm and 500 mm, for example between 270 mm and 310 mm.

[0037] The single-screw extruder preferably has an outer screw diameter between 60 mm and 1000 mm, for example, 650 mm. The single-screw extruder preferably has at least one shaft diameter between 25 mm and 500 mm, for example, between 340 mm and 380 mm. The screw shaft can have multiple diameters, for example, if the diameter changes continuously along the feed channel, for example, continuously increases. The diameter can also increase in steps, for example.

[0038] In a preferred embodiment, the ratio between shaft diameter and outer screw diameter increases along the feed channel. The ratio between shaft diameter and outer screw diameter along the feed channel can, for example, increase between values ​​of 0.3 and 0.9 and preferably between 0.4 and 0.6. Particularly preferably, the ratio between shaft diameter and outer screw diameter increases along the feed channel from 0.449 at the inlet opening to 0.577 at the outlet opening or from 0.52 at the inlet opening to 0.58 at the outlet opening. The ratio of the shaft diameter to the outer screw diameter determines the relationship between throughput and the pressure acting on the SAP polymer gel. When the screw shaft is in operation, screw chambers defined by the pitch between the screw flights are formed, with free transport volumes decreasing along the feed channel.The decreasing free transport volumes are a result of the decreasing ratio between the shaft diameter and the outer screw diameter. Increasing the ratio of the shaft diameter to the outer screw diameter therefore results in higher pressure and lower throughput. By increasing the ratio along the feed channel, SAP polymer gel can be fed into the feed channel at the inlet opening at a high throughput. This can further increase the pressure in the conveying zone because a large amount of SAP polymer gel is subsequently supplied. This allows a relatively high throughput at the outlet opening to be achieved at increased pressure.

[0039] The single-screw extruder preferably has a shaft diameter to outer screw diameter ratio between 0.4 and 0.6, for example between 0.449 and 0.577 or, for example, between 0.52 and 0.58. The single-screw extruder can also have a shaft diameter to outer screw diameter ratio between 0.3 and 0.9.

[0040] In a preferred embodiment, the pitch decreases along the conveying zone from a pitch of 500 mm near the inlet zone to a pitch of 350 mm near the outlet zone. The decreasing pitch allows the pressure acting on the SAP polymer gel to be increased, as the free transport volume of the screw chambers is reduced.

[0041] In a further preferred embodiment, the screw shaft has a lowest pitch value along the conduit channel that is at most between 20% and 80% of a highest pitch value along the conduit channel. The screw shaft can also have a pitch value near the entrance zone that is at most between 20% and 80% of a pitch value near the exit zone. Limiting the change in pitch along the conduit channel reduces the risk of an undesirable morphological change in the SAP polymer gel, since an excessive decrease in pitch could introduce too much specific mechanical energy (SME) into the SAP polymer gel.

[0042] In a further development, the worm shaft has a lowest value of a shaft diameter along the guide channel that is at most between 20% and 80% of a highest value of a shaft diameter along the guide channel. The worm shaft can also have a shaft diameter near the inlet zone that is at most between 20% and 80% of a shaft diameter near the outlet zone.

[0043] Preferably, the single-screw extruder is designed to produce an SAP polymer gel with a desired morphology that increases the water absorption of the SAP and with a throughput of at least 23 tons per hour. The single-screw extruder is dimensioned accordingly as a production version, meaning that, among other things, the feed channel and the screw shaft are of an appropriate size.

[0044] In a preferred embodiment, the single-screw extruder has at least one mixing element arrangement that extends into the feed channel of the single-screw extruder and is designed to mix the SAP polymer gel. The mixing element arrangement can extend or be arranged along part of the feed channel or over the entire length of the feed channel. Preferably, the mixing element arrangement extends at least along the conveying zone or is arranged along it. The mixing element arrangement is preferably arranged at least partially around the circumference of the screw shaft.

[0045] The mixing element arrangement can, for example, have one or more pin arrangements projecting into the interior of the line channel, which are distributed along the entire length of the line channel, for example, at several points along the axis of the screw shaft - a pin arrangement can have pins, bolts or the like that are distributed circumferentially around the screw shaft at the point along the axis of the screw shaft. Alternatively or additionally, a mixing element arrangement can have one or more recesses in the screw of the screw shaft, distributed along the entire length of the line channel, for example, arranged at several points along the axis of the screw shaft. The pins, bolts or the like of the pin arrangement can engage in these recesses at the corresponding point along the axis of the screw shaft.The pins, bolts, or similar mixing elements of a pin arrangement and corresponding recesses in the screw shaft serve to mix and increase the shear of the SAP polymer gel conveyed along the interior of the conduit at the location of the pin arrangement. The pins are preferably arranged in a wall of the conduit channel, secured, and extend into the interior of the conduit channel.

[0046] Particularly preferably, the mixing element arrangement comprises at least one pin extending into an interior of the conduit channel and at least one recess along the screw. The at least one pin preferably extends into the at least one recess of the screw when the screw is rotated during operation, so that rotation of the screw shaft is possible without the pin touching the screw. The further development of the mixing element with pins in recesses of the screw makes it possible to change the morphology of the SAP polymer gel in the single-screw extruder. This creates a desired morphology that has a sufficiently high porosity so that water absorption can be improved ("surface activation"). The pins in the recesses increase mixing, particularly for larger single-screw extruders, especially production versions of the single-screw extruder.For smaller dimensioned single-screw extruders, especially laboratory versions of a single-screw extruder, a smaller but still significant improvement in mixing and a slight increase in shear can be observed.

[0047] In a preferred development, the guide channel has at least two pins arranged along the guide channel in the conveying direction at a mixing element spacing. A value of the mixing element spacing is preferably adapted to a pitch value of the screw pitch. The mixing element spacing is preferably adapted to the pitch such that a larger value of the mixing element spacing is provided when a smaller pitch value is provided and a smaller value of the mixing element spacing is provided when a larger pitch value is provided. Preferably, several pins are arranged around the circumference of a shaft so that a guide channel chamber is formed in the space between each two separately arranged pins. A screw chamber is formed between two screw turns, i.e. with the length of the pitch. The length of the guide channel chamber can be adapted to the length of the screw chamber.Preferably, the lengths are in opposite directions, i.e., as the pitch decreases, the length of the conduit chamber increases. In a further development, the length of the conduit chamber increases along the conveying zone in the conveying direction, for example, linearly, exponentially, or similarly.

[0048] In a particularly preferred embodiment, the single-screw extruder comprises a drive motor and / or a heating device. The drive motor is preferably designed to rotate the screw shaft at up to 150 revolutions per minute, for example at 75 revolutions per minute and preferably at 30 revolutions per minute.

[0049] The heating device is preferably designed to heat the duct so that it has a temperature between 85°C and 140°C, at least in the inlet zone. The heating device can, for example, extend along the length of the duct and enclose it, allowing uniform heating. Alternatively, the heating device can extend only over parts of the duct. The heating device can also be arranged and designed in such a way that it can create different temperature zones.

[0050] The heating device is preferably arranged and configured such that, during operation of the single-screw extruder, the temperature of the SAP polymer gel in the duct increases along the conveying direction up to an exit zone, preferably by a temperature in the range of 20°C to 40°C. The temperature increases with energy input, in particular also by increasing pressure and shear forces along the conveying direction. The SAP polymer gel preferably has a further reduced temperature of between 90°C and 110°C directly after the exit opening, once the SAP polymer gel has cooled down again.

[0051] Preferably, the heating device comprises an oil having a temperature of up to 150°C. The heating device can also be designed for cooling and, for example, comprise an oil having a temperature lower than the temperature of the SAP polymer gel.

[0052] In a further development, the conduit has a length between 200 mm and 4000 mm. Preferably, the conduit has a length of at least 3000 mm, so that the screw has a working length of 3000 mm. The conduit can, for example, have an inner diameter between 50 mm and 750 mm. Preferably, the conduit has an inner diameter of 650 mm.

[0053] In a preferred embodiment, the outlet opening has a nozzle, preferably also for changing the morphology, for discharging the SAP polymer gel with the changed morphology. The nozzle can have one through-opening or hole or several through-openings or holes, or it can generally have a number of through-openings or holes in the range between 60 and 90 - in this case, this is a preferred number of holes for the laboratory version of the single-screw extruder. Preferably, the nozzle in a production version has many more holes. Particularly preferably, the nozzle has more than 1000 holes, for example 3600 holes. In the production version of the single-screw extruder, the nozzle 34 preferably has a number of holes in the range between 3000 and 4000 holes.

[0054] The holes can, for example, have diameters between 4 mm and 12 mm. The holes preferably have a diameter of 8 mm. Preferably, 10% of the nozzle surface is open, i.e., 10% of the surface is made up of passage openings or holes.

[0055] In a preferred embodiment, the exit opening comprises a nozzle with 3000 holes, each with a diameter of 8 mm. In this case, 10% of the nozzle area is particularly preferably open.

[0056] In a preferred embodiment, the single-screw extruder is designed to generate a maximum pressure of 50 bar. The single-screw extruder can be designed to generate a throughput of 30 t per hour. The single-screw extruder can also be designed to absorb a specific mechanical energy of up to 60 kWh per ton. Furthermore, the single-screw extruder can be designed to operate with an input power of up to 18.5 kW.

[0057] The invention relates to a method for changing the morphology of a superabsorbent polymer, namely a polymer gel (SAP polymer gel), using the single-screw extruder of the invention or one of its further developments. The method comprises the following steps: Feeding the SAP polymer gel from a polymerization process into the single-screw extruder, operating the single-screw extruder to change the morphology of the SAP polymer gel, discharging the SAP polymer gel with changed morphology from the single-screw extruder to a drying process.

[0058] In a further development of the process, the drying process comprises the following steps: Spreading the SAP polymer gel with modified morphology on drying trays and heating the SAP polymer gel with modified morphology on the drying trays in a convection oven or circulating air oven.

[0059] The drying trays can be filled with varying amounts of SAP polymer gel with modified morphology, resulting in a filling level that depends on the area of ​​the drying tray and the amount of SAP polymer gel with modified morphology filled onto the drying tray. The drying temperature and drying time depend on the filling level; for example, with a filling of 0.91 g / cm²<, a drying temperature of 175°C can be used for 70 minutes. The drying trays can have a sieve bottom, for example, with 250 µm mesh openings, so that the liquid can also escape through the sieve bottom. The sieve bottom can be formed, for example, from wires with a diameter of 130 µm each.

[0060] In a further training, the procedure includes the additional step: Feeding the dried SAP to a milling process.

[0061] Preferably, the dried SAP is ground by a mill to produce SAP particles of different sizes.

[0062] The method may further comprise the following step: Feeding the ground SAP to a screening or sorting process.

[0063] Preferably, the ground SAP is sieved or sorted using a sieving or sorting process so that SAP particles of different sizes are separated from one another.

[0064] The method may further comprise the following step: Feeding sorted SAP particles to a mixing process.

[0065] Preferably, in the mixing process, SAP particles of different sizes are mixed according to a predetermined mixing ratio in order to obtain desired properties of the SAP particle mixture.

[0066] Furthermore, the method may comprise the following step: Feeding the SAP particle mixture to a surface cross linking (SXL) process.

[0067] Preferably, a surface crosslinking agent, which may contain, for example, isopropanol, water, and / or aluminum lactate, is applied to the surface of the SAP particles. The SAP particles coated with the surface crosslinking agent are then heated, preferably at a temperature of 185°C, so that a surface crosslinking is formed on the respective SAP particles. Surface crosslinking enables the SAP particles to retain their shape in the swollen state—i.e., when the SAP particles have absorbed liquid and are present as a polymer gel. In particular, surface crosslinking can increase the holding capacity of absorbed liquid under pressure.

[0068] The invention relates to a use of the single-screw extruder of the invention or one of the further developments for changing a morphology of superabsorbent polymer gel (SAP polymer gel).

[0069] Embodiments of the invention are now described below with reference to the drawing. These are not necessarily intended to represent the embodiments to scale; rather, where useful for explanation, the drawing is schematic and / or slightly distorted. With regard to additions to the teachings immediately apparent from the drawing, reference is made to the relevant prior art. It should be noted that numerous modifications and changes to the form and detail of an embodiment can be made without deviating from the general idea of ​​the invention. The features of the invention disclosed in the description, in the drawing and in the claims can be essential for the further development of the invention, both individually and in any combination.Furthermore, all combinations of at least two of the features disclosed in the description, the drawings and / or the claims fall within the scope of the invention. The general idea of ​​the invention is not limited to the exact form or detail of the preferred embodiments shown and described below, or limited to an object that would be more limited than the object claimed in the claims. In the case of specified dimensioning ranges, values ​​within the stated limits are also intended to be disclosed as limit values ​​and to be used and claimed as desired. For the sake of simplicity, the same reference numerals are used below for identical or similar parts or parts with identical or similar functions.

[0070] Further advantages, features and details of the invention will become apparent from the following description of the preferred embodiments and from the drawing, which shows:Fig. 1 is a schematic representation of a section of an exemplary single-screw extruder with a screw shaft with parameter definitions according to an embodiment of the invention; Fig. 2 is a schematic representation of an embodiment of a single-screw extruder not belonging to the invention; Fig. 3 is a schematic representation of an example of a screw shaft of a single-screw extruder not belonging to the invention; Fig. 4 is a schematic representation of a first preferred embodiment according to the concept of the invention with a screw shaft of a single-screw extruder; Fig. 5 is a schematic representation of an embodiment of a screw shaft of a single-screw extruder not belonging to the invention; Fig. 6 is a schematic representation of a second preferred embodiment according to the concept of the invention with a single-screw extruder with a mixing element arrangement;7in views (A1, A2), (B1, B2) and (C) preferred variants of pin arrangements with pins for a in . Fig.6 Fig. 8 shows a mixing element arrangement in the second preferred embodiment according to the concept of the invention; Fig. 8 shows a first preferred embodiment according to the concept of the invention for a first preferred method for changing a morphology of a superabsorbent polymer gel (SAP polymer gel) using a single-screw extruder; Fig. 9 shows a second preferred embodiment according to the concept of the invention for a second preferred method for changing a morphology of a superabsorbent polymer gel (SAP polymer gel) using a single-screw extruder.

[0071] Fig.1 shows a section of a single-screw extruder 10 with a screw shaft 12. The screw shaft 12 has a shaft 13 and a screw 14 extending along the shaft 13 and is arranged in an interior space 17 of a duct 16. The Fig.1The section shown shows a section of the screw shaft 12 arranged in a conveying zone 18. The conveying direction 20 along the conveying zone 18 runs from left to right in this illustration.

[0072] During operation of the screw shaft 12, the shaft 13 is rotated about its longitudinal axis, so that the screw 14 is also rotated and the screw threads 22 material, such as SAP polymer gel 24 (see Fig.2 ), along the conduit 16 in the conveying direction 20. The material, for example SAP polymer gel 24, is pushed by the screw 14 and the wall of the conduit 16 on the one hand, but also pulled on the other, so that a complex flow behavior develops. The conveying zone 18 thus functions as a pump, conveying material, such as SAP polymer gel 24, from an inlet zone 26 to an outlet zone 28 (see Fig.2). In the exit zone 28, a pressure value is advantageous that is high enough to force the SAP polymer gel 24 out of the exit opening 30 through a perforated disk 32 and a nozzle 34 (see Fig.2 ); i.e., preferably for changing the morphology of the SAP polymer gel 24. The level of the required pressure value depends, among other things, on the amount of material, the viscoelastic properties of the material, for example the SAP polymer gel 24, and its temperature.

[0073] Depending on the parameters of the screw shaft 12, in particular of shaft 13 and screw 14, the pressure and throughput of the material, for example, SAP polymer gel 24, can be adjusted. Furthermore, the throughput and pressure also depend, among other things, on the rotational speed of the screw shaft 13. Certain advantageous pressures are required to change the morphology of the SAP polymer gel 24. Therefore, it may be necessary to adjust the parameters of the screw shaft 12, in particular of shaft 13 and screw 14, such that a sufficiently high pressure is achieved.

[0074] Parameters of the single-screw extruder 10 are the shaft diameter d (root diameter), the outer screw diameter D (diameter), the lead pitch G (lead or pitch), the channel width W (channel width e), the metering depth H (feed chamber height), the helix angle φ (helix angle), and the distance δ from the wall of the feed channel 16 (flight clearance). These parameters are explained in more detail below.

[0075] The shaft 13 of the worm shaft 12 has the shaft diameter d (root diameter). The worm 14 has the outer screw diameter D (diameter). The worm 14 of the worm shaft 12 can be categorized depending on the ratio between the shaft diameter d and the outer screw diameter D, i.e. a value d / D. A value of d / D between 0.3 and 0.5 is what is known as a deep-cut worm, which enables a high throughput. A value of d / D between 0.7 and 0.9 is what is known as a shallow-cut worm, which enables high pressure but has a lower throughput than the deep-cut worm. The throughput of the worm 14, and in particular of a shallow-cut worm, can be increased by increasing the rotational speed of the shaft 13 of the worm shaft 12.Thus, a shallow-cut screw can achieve high pressure at a relatively high throughput. However, this requires a relatively high energy input to provide the necessary high rotational speeds of the screw shaft 13 and 12.

[0076] The pitch G specifies the distance between the proximal end of a first screw turn 22a and the proximal end of a second screw turn 22b of the screw 14. The pitch W specifies the distance between the distal end of a first screw turn 22a and the proximal end of a second screw turn 22b of the screw 14. The run width e specifies the width of the screw 14. The conveying chamber height H specifies the distance between the wall of the feed channel 16 and the surface of the shaft 13. The helix angle φ specifies the angle at which the screw 14 is inclined. The distance δ to the wall of the feed channel 16 specifies the distance between the outer surface of the screw 14 and the wall of the feed channel 16. A minimum distance δ from the wall of the duct 16 must be maintained, since otherwise the screw 14 would rotate into the wall of the duct 16 during operation and would damage it.However, the distance δ to the wall of the duct 16 is very small compared to the other dimensions, for example less than 1 mm.

[0077] Fig.2shows a preferred embodiment of a single-screw extruder 10. This can be dimensioned in different ways, for example, as a large production version of the single-screw extruder 10, which is suitable for industrial production, and as a small laboratory version of the single-screw extruder 10, which is used for experimental purposes. The basic structure of the two versions of the single-screw extruder 10 is similar or identical. The single-screw extruders 10 differ primarily in their dimensions; in particular, the large production version of the single-screw extruder 10 is designed for a throughput of up to 30 t / h (tons per hour), while the laboratory version of the single-screw extruder 10 is only designed for a throughput of up to 340 kg per hour.The laboratory version of the embodiment of the single-screw extruder 10 is a scaled-down version of the production version of the embodiment of the single-screw extruder 10 and can be used in particular for experimental purposes, for example to carry out comparative measurements for different screw shafts 12 (cf. measured values ​​for the laboratory versions of the embodiments of the single-screw extruder 10 in Tables 5 and 7).

[0078] The single-screw extruder 10 has an inlet opening 36, a feed channel 16, a screw shaft 12, and an outlet opening 30. The feed channel 16 has an interior 17, which is assigned an inlet zone 26, a conveying zone 18, and an outlet zone 28 and extends between the inlet opening 36 and the outlet opening 30. The single-screw extruder 10 can be used to convey a superabsorbent polymer gel (SAP polymer gel 24) in the conveying direction 20 and to change the morphology of the SAP polymer gel 24. In particular, the single-screw extruder 10 can be used to increase the surface porosity of the particles of the SAP polymer gel in order to increase the water absorption capacity of the SAP polymer gel.

[0079] The SAP polymer gel 24 is produced in a polymerization process 38. The so-called base polymer on which the SAP polymer gel 24 is based is used for the Fig.2The preferred embodiment shown was prepared according to the formulation given in Table 1. Table 1: reactor ORP 250 solid components 42.7% by weight Degree of neutralization 71 mol% Base polymer fine dosing 7.7% by weight baP (polymer-based) hydrogen peroxide 0.0008 wt% baA (based on acrylic acid) Ascorbic acid 0.0023 wt% baA Sodium persulfate 0.128 wt% baA Core networker 0.39 wt% baA (Laromer PO9044V) Monomer temperature 35°C Throughput 800 kg / h Dam height 160 mm

[0080] The single-screw extruder 10 of the Fig.2 is not limited to the processing of SAP polymer gel 24 with the composition of Table 1 and can also be used for other compositions of SAP polymer gel 24.

[0081] The SAP polymer gel 24 produced in the polymerization process 38 is fed to the single-screw extruder 10 via the inlet opening 36. The inlet opening 36 is connected to the interior 17 of the conduit 16 and borders the inlet zone 26. During operation of the single-screw extruder 10, the SAP polymer gel 24 is fed via the inlet opening 36 to the inlet zone 26 of the interior 17 of the conduit 16.

[0082] The screw shaft 12, which has a shaft 13 with a screw 14, is arranged in the interior 17 of the conduit 16. When the single-screw extruder 10 is operated, the shaft 13 of the screw shaft 12 rotates about its longitudinal axis. For this purpose, a drive motor 40 is provided, which is connected to the shaft 13 of the screw shaft 12. In this exemplary embodiment, the drive motor 40 can rotate the shaft 13 of the screw shaft 12 at up to 150 revolutions per minute. During operation, depending on the dimensions of the single-screw extruder 10, the shaft 13 is preferably rotated at a rotation speed between 30 revolutions per minute for the production version of the single-screw extruder 10 and 75 revolutions per minute for the laboratory version of the single-screw extruder 10.The screw shaft 12 serves to convey the SAP polymer gel 24 from the inlet opening 36 along the conveying zone 18 to the outlet opening 30 with the aid of the screw 14 and the wall of the conduit 16 and to change the morphology of the SAP polymer gel 24.

[0083] In this exemplary embodiment, the conduit 16 of the single-screw extruder 10 is completely enclosed by a heating device 42. Alternatively, only a portion of the conduit 16 may be enclosed by the heating device 42, or no heating device 42 may be present at all (not shown). Preferably, the laboratory version of the single-screw extruder 10 is enclosed by a heating device 42, while the production version of the single-screw extruder 10 is preferably designed without a heating device 42. The heating device 42 serves to heat the conduit 16. For this purpose, an oil is arranged in the heating device 42, which can have a temperature of up to 200°C.

[0084] The heating device 42 is preferably operated such that the temperature of an SAP polymer gel 24 in the conduit 16, at least in the inlet zone 26, is between 85°C and 100°C in the laboratory version of the single-screw extruder 10 and / or somewhat higher in the production version. In the production version of the single-screw extruder 10, the temperature in the conduit 16, at least in the inlet area, is preferably between 90°C and 140°C. The temperature increases with energy input, in particular by increasing pressure and shear forces along the conveying direction 20. This temperature increase along the conveying direction 20 up to an exit zone 28 can be between 20°C and 40°C compared to the inlet zone.

[0085] Preferably, the SAP polymer gel 24 directly after the exit opening 30 has a temperature which is again lower as a result of cooling, between 78°C and 110°C, preferably between 90°C and 110°C.

[0086] The heating device 42 can also be used for cooling, for example when it is filled with an oil whose temperature is lower than the temperature of the conducting channel 16 and / or the SAP polymer gel 24. The heating device 42 can in principle also serve the purpose of temperature control.

[0087] The outlet opening 30 is connected to the interior space 17 of the conduit 16 and borders the outlet zone 28. The outlet opening 30 has a perforated disk 32 and a nozzle 34 arranged downstream of the perforated disk 32. The outlet opening 30 serves to change the morphology of the SAP polymer gel 24 and to discharge the SAP polymer gel 44 with the changed morphology. For this purpose, the conveying mechanism of the screw 14 and the wall of the conduit 16 force the SAP polymer gel 24 through the perforated disk 32 and through the nozzle 34.

[0088] In this exemplary embodiment, the nozzle 34 has 66 through-holes or, in principle, can have a number of through-holes in the range between 60 and 90—in this case, this is a preferred number of holes for the laboratory version of the single-screw extruder 10. The nozzle 34 can also have only one through-hole or one hole, or a different number of holes. For example, in any case, for the production version of a single-screw extruder, a preferred number of holes is at least 1,000, for example, 3,600. In the production version of the single-screw extruder 10, the nozzle 34 has a number of holes in the range between 3,000 and 4,000.

[0089] The holes each have a diameter of 8 mm. Alternatively, the holes can also have a diameter between 4 mm and 12 mm. Holes of equal or different diameters can be arranged next to each other. In this exemplary embodiment, for the laboratory version of the single-screw extruder 10, approximately 66% of the area of ​​the nozzle 34 is open. Alternatively, for example, between 5% and 66% of the area of ​​the nozzle 34 can be open (not shown). In the production version of the single-screw extruder 10, 10% of the area of ​​the nozzle is open (not shown).

[0090] The single-screw extruder 10 may additionally or alternatively comprise an adapter, a holder, a matrix, or a combination of these components (not shown) in addition to the orifice plate 32 and the nozzle 34 at the exit opening 30. One or more of the aforementioned components may, for example, be arranged at the distal end of the screw shafts 12.

[0091] The SAP polymer gel 44 with modified morphology discharged from the outlet opening 30 is fed to a drying process 46. The drying process 46 serves to remove the liquid from the SAP polymer gel 44 with modified morphology in order to dry it. Various drying processes 46 are conceivable and known to the person skilled in the art. Within the scope of the Fig.7 A possible drying process 46 is explained in more detail in the process described. The drying process 46 may be followed by further process steps (not shown).

[0092] Further details of the screw 14 and shaft 13 of the screw shaft 12 of this embodiment of the single-screw extruder 10 are explained below.

[0093] The screw 14 of the screw shaft 12 has a pitch G that decreases along the conveying zone 18 of the feed channel 16. The pitch can also change continuously, for example, preferably decrease continuously (not shown). Between the respective sections of the screw turns 22 of the screw 14 shown, it can be seen that the different pitch values ​​G1, G2, G3, and G4 result.

[0094] In this embodiment, the first pitch value G1 of the pitch is 70 mm for the laboratory version of the single-screw extruder and the fourth pitch value G4 is 46 mm, so that the pitch G decreases along the conveying zone from a pitch value of 70 mm near the inlet zone to a pitch value of 46 mm near the outlet zone.

[0095] For the production version of the single-screw extruder 10, the first pitch value G1 is 500 mm and the fourth pitch value G4 is 350 mm. The second and third pitch values ​​G2 and G3 lie between these values. In an alternative embodiment not shown, the pitches G can also lie between pitch values ​​of 800 mm and 30 mm, for example.

[0096] The different pitch values ​​G1, G2, G3, G4 of the pitch are accompanied by different steep helix angles φ1, φ2, φ3 and φ4 (not shown).

[0097] In this exemplary embodiment, the value of the running width e of the screw 14 is a constant 6 mm for the laboratory version of the single-screw extruder 10 and a constant 40 mm for the production version of the single-screw extruder 10. Alternatively, the running width of the screw 14 can also have values ​​between 4 mm and 80 mm, for example, and can vary along the guide channel 16, for example, increasing.

[0098] In this exemplary embodiment, the shaft 13 of the screw shaft 12 has a constant shaft diameter d at least along the conveying zone 18, preferably also across the inlet zone 26 and / or outlet zone 28. The constant shaft diameter d has a value of 35 mm for the laboratory version of the single-screw extruder 10, or the constant shaft diameter d has a value of 340 mm for the production version of the single-screw extruder 10. In particular, the shaft diameter d can also have values ​​between 25 mm and 500 mm, for example, between 340 mm and 380 mm.

[0099] In this embodiment, the value of the screw outer diameter D is 78 mm for the laboratory version of the single-screw extruder 10 or 650 mm for the production version of the single-screw extruder 10. In particular, the screw outer diameter D can also have values ​​between 60 mm and 1000 mm, for example between 600 mm and 700 mm.

[0100] In this embodiment, the ratio of the shaft diameter d to the screw outer diameter D is constant and amounts to approximately 0.449 for the laboratory version of the single-screw extruder 10 and 0.52 for the production version of the single-screw extruder 10. In particular, the ratio of the screw shaft diameter d to the screw outer diameter D can also be between 0.4 and 0.6, for example 0.449 and 0.577 or, for example, between 0.52 and 0.58. The ratio of the shaft diameter d to the screw outer diameter D can also change, namely increase (see Fig.4 ).

[0101] The value of the conveying chamber height H between the shaft 13 of the screw shaft 12 and a wall of the duct 16 in this embodiment is 43 mm for the laboratory version of the single-screw extruder 10 and 310 mm for the production version of the single-screw extruder 10. In particular, the conveying chamber height H can also have values ​​between 25 mm and 500 mm, for example between 270 mm and 310 mm.

[0102] The laboratory version of the single-screw extruder 10 is based on an ECT EXR T80. Table 2 below provides an overview of the parameters of the laboratory version of the single-screw extruder 10 and the production version of the single-screw extruder 10, as well as information on preferred parameter ranges for the single-screw extruder 10. Table 2: parameter ECT EXR T80 (laboratory version) Single-screw extruder (production version Parameter range Screw working length (SAL) 300 mm 3000 mm 200 mm to 4000 mm Duct inner diameter (LID) 80 mm 650 mm 50 mm to 750 mm LI D / SAL 3,75 4,6 2.22 to 8 Maximum pressure 50 bar 50 bar 30 to 70 bar Rotational speed during operation 75 revolutions / minute 30 revolutions / minute 15 rpm to 150 rpm Nozzle thickness 33 mm 33 mm 20 mm to 45 mm Nozzle hole diameter 8 mm 8 mm 4 mm to 12 mm Number of nozzle holes 66 3600 1 to 4000 Relatively open area of ​​the nozzle 66% 10% 5% to 66% Max. throughput -340 kg / h 30 t / h 200 kg / h to 30 t / h Max. specific mechanical energy absorption -60 kWh / t -60 kWh / t 20 kWh / t to 100 kWh / t Heating oil temperature 150°C without oil heating 80°C to 200°C Temperature in the duct ~85-95°C 95-140 °C SAP polymer gel temperature at the exit opening ~78-90°C 90-110°C

[0103] The single-screw extruder 10 is not limited to the parameters given in Table 2; these merely represent a preferred parameter range.

[0104] In Fig.3 a section of an example of a laboratory version of a single-screw extruder 10 is shown. Fig.3 shows an example of a worm shaft 12 with a shaft 13 and a worm 14. In this example, the worm 14 has a constant pitch G along the conveying direction 20. The value of the shaft diameter d increases; ie, here it increases from d1 to d2 along the conveying direction, while the value of the outer screw diameter D=78 mm remains constant. In this example, the pitch G has a constant pitch value G1=46 mm. The shaft diameter increases from a value of d1=35 mm to a value of d2=45 mm. Therefore, the ratio d / D also increases from 0.445 to 0.577.

[0105] In the Fig.4and Fig.5 Preferred embodiments of screw shafts 12 according to the concept of the invention are shown, which, like the screw shaft 12 of the embodiment of the single-screw extruder 10 of the Fig.2 can be used in the single-screw extruder 10. The screw shaft 12 can be dimensioned in different ways, for example, as a large production version of the screw shaft 12, which is suitable for industrial production, and a small laboratory version of the screw shaft 12, which is used for experimental purposes. The structure of the two versions of the screw shaft 12 is identical. The screw shafts 12 differ in their dimensions; in particular, the large production version of the screw shaft 12 is designed for a throughput of up to 30 t / h (tons per hour), while the laboratory version of the screw shaft 12 is only designed for a throughput of up to 340 kg / h (kilograms per hour).

[0106] The worm shaft 12 of the Fig.4 has a shaft 13 and a worm 14. In this exemplary embodiment, the worm 14 has a pitch G that decreases from G1 to G2. The worm shaft diameter d increases; ie, here it increases from a value d1 to d2 along the conveying direction 20, while the outer screw diameter has a constant value D=78 mm for the laboratory version of the worm shaft 12 and D=650 mm for the production version of the worm shaft 12. The shaft diameter d of the shaft 13 of the worm shaft 12 therefore increases along the guide channel 16 in this exemplary embodiment.

[0107] In this exemplary embodiment, the first pitch value G1=70 mm and the second pitch value G2=46 mm for the laboratory version of the worm shaft 12. For the production version of the worm shaft 12, the first pitch value G1=500 mm and the second pitch value G2=350 mm. The shaft diameter increases from a value d1=35 mm to d2=45 mm for the laboratory version of the worm shaft 12. For the production version of the worm shaft, the shaft diameter increases from a value d1=340 mm to d2=380 mm. Therefore, the ratio d / D also increases from 0.445 to 0.577 for the laboratory version of the worm shaft 12 and from 0.52 to 0.58 for the production version of the worm shaft 12. In this embodiment, the ratio d / D between shaft diameter d and screw outer diameter D increases along the guide channel 16. Thus, on the one hand, the ratio d / D increases and on the other hand, the pitch G decreases.This allows the transport properties of the screw 14 for the SAP polymer gel 24 to be improved. This makes it possible to achieve a higher throughput with less energy consumption and simultaneously maintain the product properties, in particular a desired morphology of the SAP polymer gel, which could otherwise only be achieved with higher energy consumption and / or lower throughput.

[0108] Fig.5 shows a section of a single-screw extruder 10 with a second embodiment of a screw shaft 12 according to the concept of the invention. This can also be dimensioned according to a laboratory version of the screw shaft 12 and a production version of the screw shaft 12. The screw shaft 12 has a shaft 13 and a screw 14. The screw 14 has a decreasing pitch G in this embodiment. Compared to the embodiment of the Fig.4However, the shaft diameter has a constant value of d=35 mm along the conveying direction for the laboratory version of the worm shaft 12 and d=340 mm for the production version of the worm shaft 12. The outer screw diameter also remains constant with a value of D=78 mm for the laboratory version of the worm shaft 12 and D=650 mm for the production version of the worm shaft 12.

[0109] In this embodiment, the pitch has a first pitch value G1=70 mm and a second pitch value G2=46 mm for the laboratory version of the worm shaft 12 and first pitch value G1=500 mm and second pitch value G2=350 mm for the production version of the worm shaft 12. Thus, in this embodiment, in contrast to the embodiment of the Fig.4 only the pitch G. This allows the transport properties of the screw 14 for the SAP polymer gel 24 compared to, for example, the screw shaft 12 of the Fig.3However, the worm shaft 12 of the embodiment of the Fig.5 behind the improvement by the additional increase of the ratio d / D of the embodiment of the worm shaft 12 of the Fig.4 back (see Tables 5 and 7 for the comparison of measured values ​​for the laboratory versions of the screw shafts 12 in the laboratory version of the single-screw extruder 10).

[0110] Fig.6 shows a second preferred embodiment of a single-screw extruder 10. The single-screw extruder 10 preferably relates to a production version. The single-screw extruder 10 can also be designed as a laboratory version (not shown). The single-screw extruder 10 of the second embodiment is similar to the single-screw extruder 10 shown in Fig.2The first embodiment of the single-screw extruder 10 shown in the drawing is similar, and thus, for the sake of simplicity, the same reference numerals are used for similar or identical parts or parts with similar or identical functions. The conveying direction 20 along the conveying zone 18 again runs from left to right in this illustration.

[0111] The single-screw extruder 10 has an inlet opening 36, a feed channel 16, a screw shaft 12, and an outlet opening 30. The feed channel 16 has an interior space 17, which is assigned an inlet zone 26, a conveying zone 18, and an outlet zone 28 and which extends between the inlet opening 36 and the outlet opening 30. The single-screw extruder 10 can be used to convey a superabsorbent polymer gel (SAP polymer gel 24) in the conveying direction 20 and to change a morphology of the SAP polymer gel 24.

[0112] In this embodiment, the conduit 16 of the single-screw extruder 10 is also completely enclosed by a heating device 42. The heating device 42 can be filled with an oil at a predetermined temperature in order to set a desired temperature in the interior 17 of the conduit 16.

[0113] Like the single-screw extruder 10 of the first preferred embodiment of the Fig.2 The single-screw extruder 10 of the second preferred embodiment of the Fig.6 filled with SAP polymer gel 24, which originates from a polymerization process 38. This is fed via the inlet opening 36 into the interior 17 of the single-screw extruder 10 and conveyed by the screw flights 22 of the screw 14 of the screw shaft 12 along the conduit 16 in the conveying direction 20.

[0114] During transport along the conduit 16, the morphology of the SAP polymer gel is altered, in particular, the porosity of the surface of the SAP polymer gel particles is increased. At the exit opening 30, the SAP polymer gel is forced through the schematically illustrated perforated disk 32 and the nozzle 34, and the morphology is further altered, producing an SAP polymer gel 44 with altered morphology. The SAP polymer gel 44 with altered morphology is then fed to a drying process 46. Further processes for treating the SAP polymer gel 44 may follow the drying process 46, such as milling and / or sieving (not shown).

[0115] The second embodiment of the single-screw extruder 10 of the Fig.6 differs essentially from the first embodiment of the single-screw extruder 10 of the Fig.2that the single-screw extruder 10 has a mixing element arrangement 49 with two mixing elements shown here in the form of pins 48.1 and 48.2 of a pin arrangement 48 and the shaft diameter d of the shaft 13 changes along the line channel 16 - in this exemplary case, the diameter d shown schematically in Fig.4 shown screw shaft 12. Here, the shaft 13 of the screw shaft 12 has an increasing shaft diameter d along the conveying zone 18, preferably additionally also over the inlet zone 26 and / or outlet zone 28.

[0116] An embodiment of a single-screw extruder 10 of the Fig.6 --without mixing element arrangement 49 but in principle with a screw thread 22 of the screw 14 of the screw shaft 12 along the channel 16 in the conveying direction 20 as in Fig.4 or Fig.5 -- is not explicitly shown here but also according to the general concept of the invention. A single-screw extruder 10 of the Fig.2 --with a shaft diameter d increasing in any case along the conveying zone 18, preferably additionally also over the inlet zone 26 and / or outlet zone 28, and in principle with a screw thread 22 of the screw 14 of the screw shaft 12 along the duct 16 in the conveying direction 20 as in Fig.4 or Fig.5 -- is not explicitly shown here but also according to the general concept of the invention.

[0117] In the second embodiment of the single-screw extruder 10 of the Fig.6 In addition, the mixing element arrangement 49 has four pin arrangements 48 with pins 48.1, 48.2 shown here in the channel 16 -- and, if necessary, recesses 50 in the screw 14 of the screw shaft 12--. Variants of the pin arrangements 48 are shown in Fig.7explained by way of example. In this embodiment of the single-screw extruder 10, the pins 48.1, 48.2 are fastened in the wall of the conduit 16 and protrude into the interior 17 of the conduit 16. The pins 48.1, 48.2 of a pin arrangement are arranged around the entire circumference of the conduit 16, so that a ring of pins is formed around the circumference, of which two pins 48.1, 48.2 are shown here.

[0118] A duct chamber is formed between each two of the pin rings of a pin arrangement 48 with pins 48.1, 48.2, which are arranged separately along the conveying direction 20 with a mixing element spacing K.

[0119] The length of the respective conduit chamber is defined by the value of the pin spacings K1, K2, K3, K4, K5 and is different in this exemplary embodiment because the pin arrangements 48 are arranged with different pin spacings K. The first conduit chamber along the conveying direction 20 has a value of the mixing element spacing K1 and is formed by a wall of the conduit 16 and the first pin ring of a pin arrangement 48 with pins 48.1 and 48.2. The first conduit chamber extends from the inlet zone 26 into the conveying zone 18. The conduit chambers following in the conveying direction 20 are formed between the respective pin rings of a further pin arrangement 48 (not designated in more detail but recognizable) consisting of further pins 48.1, 48.2 (not designated in more detail but recognizable) in the conveying zone 18 and have the values ​​K2, K3 and K4.The duct chamber at the exit zone 28 of the duct 16 is formed between the last pin arrangement 48 in the conveying direction 20 and the perforated disc 32.

[0120] Which also in Fig.7 The visible recesses 50 in the screw 14 are arranged such that, during operation, when the shaft 13 is rotated by the drive motor 40, the pins 48.1, 48.2 pass through the recesses 50 during the rotation of the shaft 13 without the pins 48 touching the screw 14. The recesses 50 thus represent interruptions in the screw 14.

[0121] The pins 48.1, 48.2 of a pin arrangement 48 and the recesses 50 serve to mix and shear the SAP polymer gel 24. Improved mixing and increased shear are particularly evident in a production version of the single-screw extruder 10, i.e., a version with larger dimensions. For a laboratory version with smaller dimensions, the mixing element arrangement 49 has a lesser effect.

[0122] In this embodiment of the single-screw extruder 10, the shaft 13 of the screw shaft 12 is divided into six shaft segments W1, W2.1 and W2.2, W3, W4, W5, and W6. Shaft segment W1 is located in the input zone 26, shaft segments W2, W3, W4, and W5 are located in the conveying zone 18, and shaft segment W6 is located in the output zone 28. Shaft segments W1 and W2.1 have a shaft diameter d, and shaft segment W2.2 has a shaft diameter with a first value d1=340 mm. Shaft segment W3 has a shaft diameter that continuously changes from the first value d1=340 mm to a second value d2=380 mm—i.e., by Δd. In shaft segments W4 and W5, the shaft diameter initially has a value of d2=380 mm and then remains at d2 or (as here) continues to increase to d3>380 mm. In shaft segment W6, i.e., in exit zone 28, the shaft diameter d continuously decreases from the value d2=380 mm or d3>380 to a value of d4=120 mm.

[0123] The exit zone 28 thus has a larger transport volume, which makes it possible to push a larger amount of SAP polymer gel through the exit opening 30 under lower pressure.

[0124] In this exemplary embodiment, the screw shaft 12 has a lowest value of a shaft diameter d1 along the conduit 16, which is approximately 32% of the highest value of the shaft diameter d2 or d3 along the conduit 16. The lowest value of the shaft diameter d along the conduit 16 can also be at most between 20% and 80% of a highest value of a shaft diameter along the conduit 16. The value of the screw outer diameter D is constant along the conduit 16 and amounts to 650 mm. Thus, along the conveying zone 18 of the conduit 16, the ratio d / D of the shaft diameter d to the screw outer diameter D changes from 0.52 to 0.58.

[0125] In this exemplary embodiment, the pitch G noticeably decreases from a first pitch value of G1=500 mm. In the shaft segment W2.1 and W2.2, the worm 14 has a second pitch value of G2=460 mm. This means that in this exemplary embodiment, the pitch G noticeably decreases from G1=500 mm to G2=460 mm to G3=350 mm and then (as here) possibly further to G4 and G5<350 mm. This means that the lowest pitch value along the guide channel is 70% of the highest pitch value or even lower. The lowest pitch value along the guide channel can also be between 20% and 80% of the highest pitch value along the guide channel.

[0126] In the shaft segment W3, the pitch G decreases on the one hand, and the shaft diameter d increases on the other. This leads to an increase in pressure and a reduction in transport volume along the conduit 16 in the conveying direction 20.

[0127] In a first variant, this can be maintained over the shaft segments W4 and W5 (not shown) or (as here) the tendency can be further increased in the shaft segments W4 and W5 by further increasing the shaft diameter d (to d2 and then d3) and further reducing the pitch G (to G4 and then G5).

[0128] In this exemplary embodiment, the values ​​of the mixing element spacing K2, K3, K4, and K5 are adapted to the pitch values ​​G2, G3, G4, and G5 of the pitch G of the screw 14. While the values ​​of the pin spacings decrease from K2 to K5, the pitch values ​​also decrease from G2 to G5. The change in the mixing element spacing K therefore runs in the same direction as the change in the pitch G. This leads to a comparatively high introduction of pressure and shear forces as a result of the increase in pressure and reduction in transport volume, and to improved mixing and increased shear in the conveying direction 20 toward the exit zone 28 of the single-screw extruder 10.

[0129] In a modification not shown here, the change in the mixing element spacing K can also be designed in the opposite direction to the change in the pitch G. The reference numerals of the Fig.6In such a modified embodiment, the values ​​of the mixing element spacing K2, K3, K4, and K5 would be adapted in opposite directions to the pitch values ​​G2 and G3 of the pitch G of the screw 14. While the values ​​of the pin spacing increased in the case of the modified embodiment from K2 to K5 (not shown), the pitch values ​​decreased in the opposite direction from G2 to G5 (shown). This led to a comparatively moderate introduction of pressure and shear forces as a result, on the one hand, of the increase in pressure and the reduction in transport volume, and, on the other hand, of improved but not increased mixing, i.e. a rather decreasing shear in the conveying direction 20 towards the exit zone 28 of the single-screw extruder 10.

[0130] The following Table 3 summarizes the parameters of the example of a laboratory version of a worm shaft 12 analogous to the Fig.3and the parameters of the examples of a laboratory version of the worm shaft 12 analogous to the Fig. 4 and Fig.5 , as well as the parameters of the design example of a production version of the worm shaft analogous to the Fig.6 together. Table 3: Properties of the worm shaft and worm Example of a worm shaft of the Fig.3 (Laboratory version) Example of the worm shaft of the Fig.4 (Laboratory version) Example of the worm shaft of the Fig.5 (Laboratory version) Example of the worm shaft of the Fig.6 (production version) Gear width (W) W W1 to W2 W1 to W2 100*W1 to 100*W2 Running width (e) 6 mm 6 mm 6 mm 40 mm Pitch (G=π(De)tanφ) 46 mm 70 mm to 70 mm to 46 mm 500 mm to 46 mm 350 mm Screw outer diameter (D) 78 mm 78 mm 78 mm 650 mm Conveying chamber height (H) 43 mm to 43 mm to 43 mm 310 mm to 33 mm 33 mm 270 mm Shaft diameter (d) 35 mm to 35 mm to 35 mm 340 mm to 45 mm 45 mm 380 mm d / D 0.45 to 0.58 0.45 to 0.58 0,45 0.52 to 0.58 Distance between housing wall and screw (δ) δ δ δ 5δ Helix angle (φ) φ φ1 to φ2 φ1 to φ2 φ1 to φ2

[0131] Fig.7 shows in views (A1, A2), (B1, B2) and (C) preferred variants of pin arrangements 48 with pins for a Fig.6shown mixing element arrangement; the pin assemblies are designated 48.A1, 48.A2, 48.B1, 48.B2, and 48.C, respectively. The pin assemblies 48.A1 and 48.A2 each have two pins 481, 482 arranged opposite one another on a diametrical axis A. The pin assemblies 48.A1 and 48.A2 differ in the orientation of the diametrical axis, with the pins 481, 482 each at a 12 o'clock position and a 6 o'clock position (view A1) and with the pins 481, 482 each at a 3 o'clock position and a 9 o'clock position (view A2).

[0132] In view A1, the length L of a pin 481, 482 is also shown as an example in the range of approximately L=300mm and the distance I of a pin end from the surface of the shaft 13 482 is shown as an example in the range of approximately I=10mm; the latter distance I can, for example, be in the range of 10-25mm. The length L of a pin 481, 482 can be in the range of approximately L=270mm to 330mm.

[0133] Thus, the length L of the pin projecting into the interior 17 of the conduit 16 is preferably approximately 90% to 99% of the free conveying chamber height H of the conduit 16. The conveying chamber height H indicates the distance between the wall of the conduit 16 and the surface of the shaft 13 and is 310 mm here. The diameter Q of a preferably round (but also possible oval or square) cross-section of a pin is approximately Q = 1 - 8 cm, preferably 2 - 6 cm, particularly preferably 4 cm. These pin arrangements 48.A1 and 48.A2 can also be combined for a mixing element arrangement 49 along the conveying direction of the single-screw extruder 10, e.g., alternating.

[0134] The pin assemblies 48.B1 and 48.B2 each have four pins 481, 482 and 483, 484 arranged in pairs opposite one another on a first and second diametrical axis A1, A2. The pin assemblies 48.B1 and 48.B2 differ in the orientation of the diametrical axes A1, A2 with the pins 481, 482, 483, 484 each at a 12 o'clock position and 6 o'clock position as well as 3 o'clock position and 9 o'clock position (view B1) and with the pins 481, 482, 483, 484 each at a 2 o'clock position and 8 o'clock position as well as 5 o'clock position and 11 o'clock position (view B2). These pin assemblies 48.B1 and 48.B2 can also be combined, e.g., alternated, for a mixing element arrangement 49 along the conveying direction of the single-screw extruder 10. The dimensions of the pins of pin assemblies 48.B1 and 48.B2 can be selected in the same way as those of the pins of pin assemblies 48.A1 and 48.A2.

[0135] The pin arrangement 48.C has eight pins 481, 482 and 483, 484, as well as 485, 486 and 487, 488, arranged in opposite pairs—it is essentially an overlay of the pin arrangements 48.B1 and 48.B2. This pin arrangement 48.C can also be combined with the pin arrangements 48.B1 and 48.B2 and / or the pin arrangements 48.A1 and 48.A2 for a mixing element arrangement 49 along the conveying direction of the single-screw extruder 10.

[0136] In principle, other angular arrangements for the alignment of the pins in a pin arrangement 48 for a mixing element arrangement 49 can also be selected.

[0137] Fig.8 shows an embodiment of a method for changing the morphology of a superabsorbent polymer, namely a polymer gel (SAP polymer gel 24) using a single-screw extruder 10. The method comprises the steps: 100Feeding the SAP polymer gel 24 from a polymerization process 38 into the single-screw extruder 10, 200Operating the single-screw extruder 10 to change the morphology of the SAP polymer gel 24, and 300Discharging the SAP polymer gel 44 with changed morphology from the single-screw extruder 10 to a drying process 46.

[0138] The polymerization process of step 100 produces a so-called base polymer as the basis for the SAP polymer gel 24 according to the formulation of Table 1. Other formulations may alternatively be used.

[0139] The single-screw extruder 10 is operated according to step 200, in which the drive motor 40 rotates the shaft 13 of the screw shaft 12 and conveys SAP polymer gel 24 from the inlet opening 36 to the outlet opening 30. As the SAP polymer gel 24 is conveyed along the conveying zone 18, the morphology of the SAP polymer gel 24 can be changed. The conveying zone 18 also serves as a feed zone to the outlet zone 28, which serves as a metering zone for the outlet opening 30. Depending on the supply of SAP polymer gel 24 to the outlet zone 28, which depends, among other things, on the parameters of the screw shaft 12 and its rotational speed, a specific amount of SAP polymer gel 24 is provided in the outlet zone 28. This specific amount can then be discharged through the outlet opening 30 at a specific pressure. The exit opening 30 has shaping components that change the morphology of the SAP polymer gel 24. In the embodiment of the method according to Fig.8The exit opening 30 has a perforated disk 32 and a subsequent nozzle 34. Alternatively or additionally, other components, such as a matrix or other components that change the morphology of the SAP polymer gel 24, can be arranged at the exit opening 30.

[0140] The drying process 46 according to step 300 has in this embodiment of the method of Fig.8 the following steps: Spreading the SAP polymer gel 44 with altered morphology on drying trays and heating the SAP polymer gel 44 with altered morphology on the drying trays in a convection oven or circulating air oven.

[0141] The drying trays can be filled with various amounts of SAP polymer gel 44 with modified morphology, resulting in a filling level dependent on the area of ​​the drying tray and the amount of SAP polymer gel 44 with modified morphology filled onto the drying tray. The drying temperature and drying time depend on the filling level. In this exemplary embodiment, with a filling of 0.91 g / cm², a drying temperature of 175°C is used for 70 minutes. In this exemplary embodiment, the drying trays have a sieve bottom with 250 µm mesh openings so that the liquid can also escape through the sieve bottom. In this exemplary embodiment, the sieve bottom is formed from wires each with a diameter of 130 µm.

[0142] Fig.9shows a further preferred embodiment of a method for changing the morphology of a superabsorbent polymer, namely a polymer gel (SAP polymer gel 24) with a single-screw extruder 10. The method comprises the steps: 100 Feeding the SAP polymer gel 24 from a polymerization process 38 into the single-screw extruder 10. 200 Operating the single-screw extruder 10 to change the morphology of the SAP polymer gel 24. 300 Discharge of the SAP polymer gel 44 with modified morphology from the single-screw extruder 10 to a drying process 46. 400 Feeding the dried SAP to a milling process to grind the SAP. 500 Feeding the ground SAP to a screening or sorting process to screen or sort the SAP. 600 Feeding sorted SAP particles to a mixing process to mix the SAP particles. 700 Feeding the SAP particle mixture to a surface cross linking (SXL) process to perform surface cross linking on the surfaces of the SAP particles.

[0143] Steps 100, 200 and 300 of the procedure are identical to those in Fig.8 described steps of the embodiment of the method for changing the morphology of a superabsorbent polymer, namely a polymer gel (SAP polymer gel 24) with a single-screw extruder 10.

[0144] The dried SAP is ground by a mill in the milling process in step 400, resulting in SAP particles of different sizes.

[0145] The ground SAP is sieved or sorted in the sieving or sorting process of step 500 so that SAP particles of different sizes are separated from each other.

[0146] In the mixing process of step 600, SAP particles of different sizes are mixed according to a predetermined mixing ratio to obtain desired properties of the SAP particle mixture. In this exemplary embodiment, an SAP particle mixture with a particle size distribution (psd) according to Table 4 was produced. Table 4: Screening area > 710 µm 710-600 µm 600-500 µm 500-300 µm 300-200 µm 200-150 µm < 150 µm In total Percentage (weight%) 0 10,6 27,9 42,7 13,8 5,0 0 100,0

[0147] For the method of the embodiment of the Fig.9For the SAP particle mixtures produced without step 700, measured values ​​for various parameters are given in Table 5 below. These parameters include the flow rate swelling rate (FSR) and the centrifuge retention capacity (CRC) listed in Table 5, the gel strength estimated here at 0.3 psi as the absorbency against pressure (AAP) of the polymer gel, and, most importantly, the specific mechanical energy (SME) introduced during extrusion.

[0148] Centrifuge retention capacity (CRC) is determined according to EDANA recommended test method No. WSP 241.3(10) "Fluid Retention Capacity in Saline, After Centrifugation".

[0149] The Absorbency Against Pressure (AAP) or absorption under load is determined here under a pressure of 21.0 g / cm 2 < = 0.3 psi (AUL0.3psi) according to the EDANA recommended test method No. WSP 242.2-05 "Absorption Under Pressure, Gravimetric Determination".

[0150] To determine the flow rate of swelling (FSR), 1.00 g (= W 1 ) of the water-absorbing polymer particles is weighed into a 25 ml beaker and evenly distributed over the bottom. Then, 20 ml of a 0.9 wt. % saline solution is metered into a second beaker using a dispenser, and the contents of this beaker are quickly added to the first, and a stopwatch is started. As soon as the last drop of saline solution is absorbed, which can be seen by the disappearance of the reflection on the liquid surface, the stopwatch is stopped. The exact amount of liquid poured from the second beaker and absorbed by the polymer in the first beaker is determined by backweighing the second beaker (= W 2 ). The time required for absorption, measured with the stopwatch, is referred to as t. The disappearance of the last drop of liquid from the surface is determined as time t.

[0151] The swelling rate (FSR) is calculated as follows: FSR g / g s = W 2 / W 1 × t

[0152] However, if the moisture content of the water-absorbing polymer particles exceeds 3 wt.%, the weight W 1 must be adjusted for this moisture content. The throughput in kg / h was measured gravimetrically. The torque in N*m was measured as a function of the motor input power. The specific mechanical energy (SME) is calculated using the following formula: SME = Drehmoment N * m * 2 * π * N min − 1 m ′ * 60 kg / h kW * h / t

[0153] The measured values ​​in Table 5 refer to the laboratory versions of the screw shaft 12 examples and are used to determine which screw shaft 12 delivers the best measured values. In particular, a high throughput with low specific mechanical energy (SME) is aimed for in order to produce a desired morphology of the SAP polymer gel at high throughput. Table 5: Pro be Tendon shaft CRC [g / g] AAP 0.3 psi [g / g] FSR [g / (g* s)] Humidity [%] extractable fractions [%] P min Pmax Throughput [kg / h] Torque [N+m] SME [kW*h / t] 1 Fig.5 33,1 17,1 0,29 1,08 13,3 18 24 201 894 34,9 2 Fig.3 33,8 15,6 0,28 1,05 13,3 8 10 138 615 35,0 3 Fig.3 32,5 17,9 0,26 1,6 11,6 4 9 124 570 36,1 4 Fig.4 35,8 11,6 0,28 1,21 14,7 18 23 249 918 28,9 5 Fig.3 34,8 12,7 0,33 1,59 14,1 6 7 120 555 36,3 6 Fig.4 33,9 14,5 0,28 0,89 13,8 16 24 237 990 32,8

[0154] In the surface post-crosslinking process (SXL process) of step 700, a surface crosslinking agent is applied to the surface of the SAP particles. The surface crosslinking agent in this embodiment was prepared according to the formulation shown in Table 6 below: Table 6: liquid portion 4.54% by weight baP (Isopropanol / water=30.9 / 69.1) Heonon / 1,3-PG 0.07 / 0.07 wt% baP 1,2-PG 0.7% by weight baP Isopropanol 0.99% by weight baP Span 20 40 ppm baP Aluminum lactate 0.5% by weight baP (as 22% by weight liquid solution Lohtragon AL 220) temperature 185°C

[0155] Heonon corresponds to 2-hydroxyethyl-2-oxazolidinone. As an alternative to the formulation in Table 6, other formulations can also be used to produce the surface crosslinker. For example, alternative surface crosslinkers can contain heonon, isopropanol, aluminum lactate, and / or aluminum sulfate.

[0156] The SAP particles coated with a surface crosslinking agent are heated to a temperature of 185°C, resulting in the formation of a surface crosslink on the respective SAP particles. Surface crosslinking allows the SAP particles to retain their shape in the swollen state—that is, when the SAP particles have absorbed liquid and are present as a polymer gel. In particular, surface crosslinking can increase the holding capacity of absorbed liquid under pressure.

[0157] Table 7 shows the values ​​of the measured values ​​for the Fig.9For the SAP particle mixtures produced after performing step 700 of the process, measured values ​​for various parameters are given. These parameters include the permeability listed in Table 7 as "Saline Flow Conductivity" (SFC) (for 1.5 g), the swelling rate (FSR), the centrifuge retention capacity (CRC), and the gel strength estimated here at 0.7 psi as Absorbency Against Pressure (AAP), as well as derived values ​​of the polymer gel and, primarily, the specific mechanical energy (SME) introduced during extrusion. The introduced specific mechanical energy (SME) can be measured as SME = Drehmoment N * m * 2 * π * N min − 1 m ′ * 60 kg / h kW * h / t , where T represents the torque and the speed of the extruder shaft, N, and m' represents the extruder's polymer gel throughput. The specific mechanical energy (SME) is thus the extruder's motor power in kW divided by the polymer gel throughput in t / h.

[0158] How the centrifuge retention capacity (CRC) and the flow rate swelling rate (FSR) are determined is given above.

[0159] The Absorbency Against Pressure (AAP) or absorption under pressure (Absorbency under Load) is determined here under a pressure of 49.2 g / cm 2 < = 0.7 psi (AUL0.7psi) analogous to the test method no. WSP 242.3 "Absorption Under Pressure, Gravimetric Determination" recommended by EDANA, whereby a pressure of 49.2 g / cm 2 < (AUL0.7psi) is set instead of a pressure of 21.0 g / cm 2 < (AUL0.3psi).

[0160] The saline flow conductivity (SFC) is determined for a swollen gel layer under a pressure load of 0.3 psi (2070 Pa), as described in EP 2 535 698 A1, namely with a sample weight of 1.5 g of water-absorbing polymer particles as a urine permeability measurement (UPM) of a swollen gel layer. The flow is recorded automatically. The saline flow conductivity (SFC) is calculated as follows: SFC cm 3 s / g = Fg t = 0 × L0 / d × A × WP , where Fg(t=0) is the flow rate of NaCl solution in g / s obtained from a linear regression analysis of the data Fg(t) of the flow determinations by extrapolation to t=0, L0 is the thickness of the gel layer in cm, d is the density of the NaCl solution in g / cm 3< , A is the area of ​​the gel layer in cm 2< and WP is the hydrostatic pressure above the gel layer in dyne / cm 2< .

[0161] The measured values ​​in Table 7 refer to the laboratory versions of the worm shaft 12 design examples. Table 7: Pro be Worm shaft SFC 1.5g (CRC+ AAP) / 2 FSR CRC AAP 0.7psi [g / g] P min Pmax Throughput [kg / h] Torque T [N*m ] SME [kW* h / t] 1 Fig.5 110 24,5 0,25 25,3 23,8 18 24 201 894 34,9 2 Fig.3 94 26,1 0,23 27,2 25,0 8 10 138 615 35,0 3 Fig.3 94 26,2 0,28 26,9 25,5 4 9 124 570 36,1 4 Fig.4 99 25,4 0,25 26,4 24,4 18 23 249 918 28,9 5 Fig.3 97 25,9 0,25 27,0 24,8 6 7 120 555 36,3 6 Fig.4 93 25,7 0,26 26,4 25,0 16 24 237 990 32,8

[0162] Table 7 shows that the worm shaft 12 of the embodiment of the Fig.4 has the lowest specific mechanical energy (SME) compared to the other worm shafts 12. Therefore, the worm shaft 12 according to the embodiment of the Fig.4 The preferred design of the screw shaft 12 for the single-screw extruder 10 is to achieve a high throughput with the lowest possible energy consumption and to produce a high-quality SAP polymer gel. The laboratory versions represent a scaled-down version of the production versions of the screw shafts 12 and single-screw extruder 10. The measured values ​​can be transferred to the production versions. Therefore, the screw shaft 12 of the embodiment of the Fig.4 the preferred version. List of reference symbols

[0163] 10Single-screw extruder 12Screw shaft 13Shaft 14Screw 16Feed channel 17Interior of the feed channel 18Conveying zone 20Conveying direction 22Screw flight 24SAP polymer gel 26Inlet zone 28Exit zone 30Exit opening 32Perforated disc 34Nozzle 36Inlet opening 38Polymerization process 40Drive motor 42Heating device 44SAP polymer gel with modified morphology 46Drying process 48.1, 48.2 pins 481, 482, 483, 484 pins 485, 486, 487, 488 pins 48 pin arrangement 49 mixing element arrangement 50 recess diametrical axis of the pins G pitch (G=π(De)tanφ) G1, G2, G3, G4 pitch value d, Δd shaft diameter d1, d2, d3 value of the shaft diameter D screw outer diameter H conveying chamber height L length of a pin I distance of a pin from the surface of the shaft 13 Q diameter of a cross section of a pin K mixing element spacing K1, K2, K3, K4 value of the mixing element spacing W pitch W1, W2, W3, W4, W5, W6 shaft segment e running width δ distance between the wall of the duct and Screw φHelix angle.

Claims

1. A process for changing the morphology of a superabsorbent polymer gel (SAP polymer gel) (24) with a single-screw extruder (10) for changing the morphology of superabsorbent polymer gel (SAP polymer gel) (24), having: - an input aperture (36) for the introduction of SAP polymer gel (24), - connected to the input aperture (36), a channel (16), - arranged in the channel (16), a screw (12) for conveying, and changing the morphology of, the SAP polymer gel (24) and - connected to the channel (16), an output aperture (30) for the discharge of the SAP polymer gel (44) with changed morphology, where the screw (12) has a shank (13) and has screw flights (14) arranged on the shank (13) and is arranged and configured to convey the SAP polymer gel (24) from the input aperture (36) to the output aperture (30) by means of the screw flights (14), where the channel (16) has an input zone (26) arranged at, or in the vicinity of, the input aperture (36), an output zone (28) arranged at, or in the vicinity of, the output aperture (30), and a conveying zone (18) extending along the channel (16) from the input zone (26) to the output zone (28), wherein - the screw (12) has a first pitch value (G1) of a pitch (G) of the screw flights (14) along the conveying zone (18) of the channel (16) and, following in conveying direction (20), has a second pitch value (G2) of the pitch (G) of the screw flights (14) along the conveying zone (18) of the channel (16), and where the second pitch value (G2) is smaller than the first pitch value (G1), and - a shank diameter (d) of the shank (13) of the screw (12) increases along the channel (16), where the process has the following steps: - introduction of the SAP polymer gel (24) from a polymerization process (38) into the single-screw extruder (10), - operation of the single-screw extruder (10) in order to change the morphology of the SAP polymer gel (24), and - discharge of the SAP polymer gel (44) with changed morphology from the single-screw extruder (10) to a drying process (46).

2. The process according to claim 1, where the single-screw extruder (10) has a drive motor (40) and / or a heating device (42), where - the drive motor (40) is configured to rotate the shank (13) of the screw (12) at up to 150 revolutions per minute, and / or - the heating device (42) is configured to heat the channel (16) so that the temperature thereof is between 85°C and 140°C, at least in the input zone (26), and during operation of the single-screw extruder (10) the temperature of the SAP polymer gel (24) in the channel (16) increases along the conveying direction (20) as far as an output zone (28).

3. The process according to claim 2, where - the temperature of the SAP polymer gel (24) in the channel (16) increases along the conveying direction (20) as far as an output zone (28) by a temperature in the range from 20°C to 40°C, and preferably - moreover directly after the output aperture (30) the cooled SAP polymer gel (24) has a reduced temperature between 90°C and 110°C.

4. The process according to any of claims 1 to 3, where the screw (12) has, along the conveying zone (18) of the channel (16), at least three different pitch values (G1, G2, G3, G4) of the screw flights (14).

5. The process according to any of claims 1 to 4, where the pitch (G) of the screw flights (14) decreases along the conveying zone (18) of the channel (16).

6. The process according to any of claims 1 to 5, where - the pitch (G) of the screw flights (14) decreases continuously along the conveying zone (18) of the channel (16), and / or - the shank diameter (d) of the shank (13) of the screw (12) increases continuously along the conveying zone (18) of the channel (16).

7. The process according to any of claims 1 to 6, where a ratio (d / D) between the shank diameter (d) and an external screw flight diameter (D) increases along the channel (16), and / or a ratio (d / D) between the shank diameter (d) and an external screw flight diameter (D) is between 0.4 and 0.6.

8. The process according to any of claims 1 to 7, where - the screw (12) has, along the channel (16), a smallest pitch value (G4) that is at most between 20% and 80% of a largest pitch value (G1) along the channel (16), and / or - the screw (12) has, along the channel (16), a smallest value of a shank diameter (d2) that is at most between 20% and 80% of a largest value of a shank diameter (d1) along the channel (16).

9. The process according to any of claims 1 to 8, where an SAP polymer gel (24) with a desired morphology that increases the water absorption of the SAP and / or with elevated throughput, especially of at least 23 metric tons per hour, is produced.

10. The process according to any of claims 1 to 9, where the single-screw extruder (10) is characterized by at least one mixing-element arrangement (49) with at least one mixing element which protrudes into the channel (16) of the single-screw extruder and which is configured for the mixing of the SAP polymer gel (24).

11. The process according to claim 10, where the mixing-element arrangement (49) has a pin arrangement (48) comprising at least one pin (48.1, 48.2) extending into an internal space (17) of the channel (16), and has at least one cutout (50) along the screw flights (14), the at least one pin (48.1, 48.2) extending into the at least one cutout (50) of the screw flights (14) when the screw flights (14) are rotated during operation, rotation of the shank (13) of the screw (12) therefore being possible without contact between the pin (48.1, 48.2) and the screw flights (14).

12. The process according to any of claims 1 to 11, where the channel (16) has at least two pins (48) arranged along the channel (16) in the conveying direction (20) and separated from one another by a mixing-element separation (K), and there is positive or negative correlation between a value of the mixing-element separation (K1, K2, K3, K4) and a pitch value (G1, G2, G3) of the pitch (G) of the screw flights (14), where - the negative correlation between the mixing-element separation (K) and the pitch (G) is such that a larger value of the mixing-element separation (K1, K2, K3, K4) is provided when a smaller pitch value (G1, G2, G3) is provided, and a smaller value of the mixing-element separation (K1, K2, K3, K4) is provided when a larger pitch value (G1, G2, G3) is provided, or - the positive correlation between the mixing-element separation (K) and the pitch (G) is such that a larger value of the mixing-element separation (K1, K2, K3, K4) is provided when a larger pitch value (G1, G2, G3) is provided, and a smaller value of the mixing-element separation (K1, K2, K3, K4) is provided when a smaller pitch value (G1, G2, G3) is provided.