METHOD FOR PRODUCING A HYDRAULIC BINDER

DE502017016525D1Active Publication Date: 2024-11-21BAUMIT BETEILIGUNGEN GMBH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
DE502017016525
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Priority Date
2016-07-08
Filing Date
2017-07-05
Publication Date
2024-11-21
Estimated Expiration
2037-07-05

AI Technical Summary

Technical Problem

The existing processes for producing hydraulic binders from Al2O3-containing by-products in secondary aluminum production are costly due to the need for extensive salt separation and heavy metal removal, which often leaves unacceptable levels of contamination in the final product.

Method used

A method involving the simultaneous washing and burning of Al2O3-containing by-products with CaO-containing substances at high temperatures (1,500 °C to 2,000 °C) to drive off salts and heavy metals, which are then recovered from exhaust gases, eliminating the need for prior washing and reducing heavy metal contamination in the binder.

Benefits of technology

This approach reduces processing costs and heavy metal contamination in the binder, allowing for the production of high-quality hydraulic binders without prior treatment of the by-products, while enabling the recovery and reuse of salts in the aluminum industry.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader
Need to check novelty before this filing date? Find Prior Art

Description

Technical area

[0001] The present invention relates to a process for producing a hydraulic binder from a CaO-containing substance and an Al 2 O 3-containing by-product from secondary aluminum production. State of the art

[0002] Today's world requires fast-setting binders. These have a wide range of applications. Among them is the binder calcium aluminate / high-alumina cement. The fired or molten calcium aluminates are used as high-quality, fast-setting high-strength high-alumina cements, and in combination with Portland cement, they also form rapid-setting cements. The anhydrous calcium aluminates hydrate during the setting of cement (an exothermic process, similar to the slaking of CaO) and form various hydrates.

[0003] To recycle aluminum, aluminum scrap and dross are melted in rotary furnaces. "Drops" are a waste product from the processing of aluminum and the production of secondary aluminum. Dross is a mixture of aluminum metal and fine-grained oxide particles and is formed during the melting of aluminum at 800°C from the aluminum oxide produced by normal aluminum corrosion and as an oxidation product (oxide skin) when liquid aluminum comes into contact with atmospheric oxygen. To prevent aluminum oxide particles from entering the casting during aluminum casting, the dross is skimmed off the surface of the metal bath using scraping devices.

[0004] Due to the high aluminum metal content in the dross, it is recycled in a second step in smelting furnaces. The molten dross is coated with halide salts (approximately two-thirds NaCl, one-third KCl, and small amounts of calcium fluoride CaF2). This process produces salt slag as a byproduct.

[0005] There are many publications and patents on the utilization of salt slag, e.g. R. Feige and G. Merker: "SEROX - a synthetic Al-glass raw material", http: / / www.alumina.de / SEROX Al-Glasrohstoff DGG%20FA%20III.pdf. The most common method is washing the salt slag. The disadvantage of this process is that while the salts are removed sufficiently effectively, the heavy metals contained in the salt slag remain.

[0006] It is also known to burn Al2O3-containing by-products from secondary aluminum production (salt slag, aluminum dross) together with CaO and CaSO4 to produce a hydraulic binder. This means that the Al2O3-containing by-product is put to sensible use and does not have to be disposed of. There are numerous relevant publications; reference is made here to EP 0838443 A or JP H05 294685 A. All of these documents use a processed Al2O3-containing by-product. The problem is that the Al2O3-containing by-product is heavily contaminated, in particular it contains salts that must be separated during processing to prevent the quality of the produced binder from being impaired by the salts. However, this processing makes the process overall expensive. Nevertheless, the heavy metals that are not separated during processing remain in the binder, often in unacceptably high quantities.In KR 2011-0117353 A, aluminum dross is mentioned as an alternative to bauxite, but a precise process for aluminum dross is not described. According to US 2007 / 266902 A1, no hydraulic binder is produced, but rather a product for use in steel finishing, so impurities are less of a problem. According to JP H07 96265 A, the salts from aluminum dross are removed by heating the aluminum dross together with SiO2 (in an amount greater than the aluminum nitride contained in the dross) to at least 800°C. Brief description of the invention

[0007] The object of the present invention is to eliminate this additional effort caused by the processing of the scabies.

[0008] This object is achieved according to the invention by a process of the type mentioned at the outset in that the Al 2 O 3 -containing by-product is burned and melted together with the CaO-containing material at 1,500°C to 2,000°C, preferably at least 1,700°C, without prior washing, in which the salts would be removed, whereby the salts and heavy metals are expelled, and the volatile salts contained in the exhaust gases are recovered by cooling.

[0009] Within the scope of the present invention, it was found that the impurities in the Al 2 O 3 -containing by-product evaporate when burned or melted at 1,500°C to 2,000°C, preferably at least 1,700°C, so that the resulting binder contains only impurities within permissible limits. Not only do the salts evaporate at these temperatures, but also the heavy metals. These metals react with the existing salts to form halides (particularly chlorides), which are already gaseous at these temperatures and are thus also discharged with the exhaust gas stream. When the exhaust gas stream is cooled, the salts and the heavy metal halides condense, so that they can be easily removed from the exhaust gas stream and recovered.

[0010] Salt slag can therefore be used to produce a binder without pretreatment (without washing). This not only eliminates the expense of processing but also significantly reduces the heavy metal content of the binder. The salts can also be recovered here (as with processing) and reused in aluminum production.

[0011] The binder can be produced from mixtures of primary raw materials that conserve primary raw materials: the Al 2 O 3 is an existing by-product from secondary aluminum production and limestone is abundant; for example, limestone from limestone quarries can be used, but by-products containing CaO or CaCOs can also be used.

[0012] The material is preferably heated to 1,700°C and melted. This requires a melting unit with the appropriate flue gas purification systems. After a certain residence time, the molten material is drawn off at regular intervals (or continuously) and poured into molds.

[0013] To achieve the desired phase composition of the binder, the mixing ratio must be adjusted according to the chemical composition of the raw materials (see example). The salts generated during the melting process can be recycled to the aluminum industry.

[0014] It is advisable to conduct firing and melting under a reducing atmosphere. This promotes the formation of heavy metal halides.

[0015] Furthermore, it is beneficial to rapidly cool the fired or molten product using the rotating cup method or in a water bath, as this influences the properties of the fired or molten product. The functionality of the binder can be increased by adding sulfuric acid to the water bath. This results in an "amorphous" binder that sets particularly quickly.

[0016] Finally, after the recovery of valuable materials by cooling, it is advisable to additionally purify the exhaust gases using filtering media (e.g., activated carbon). While some of the heavy metals are removed along with the salts during cooling, to avoid environmental pollution, the heavy metals remaining in the exhaust gases should be removed by activated carbon filters before the exhaust gases are released into the environment.

[0017] Some of the heavy metals are separated along with the salts during cooling. Depending on the requirements of the recovered salt, a subsequent washing process can be carried out to reduce the heavy metal content. Description of the execution types

[0018] The present invention is explained in more detail using an example.

[0019] The following two raw materials are used (all figures are mass%): Table 1 Raw materials salt slag CaCO3 Loss on ignition 1000°C - 42,5 Al2O3 27,1 SiO2 3,0 1,0 Fe 2 O 3 0,85 0,2 CaO 1,6 54,5 MgO 3,5 0,9 K2O 10,5 Na2O 23,3 Cl 28,6

[0020] To produce a raw mixture, the salt slag is mixed with limestone flour (CaCO3) to obtain the highly reactive phase mayenite (C12A7), according to calculations. The raw mixture thus consists of 62.7% salt slag and 37.3% limestone flour.

[0021] The mixture is homogenized in the sample container, placed in a silicon carbide crucible at 950°C, and heated to over 1,700°C with a steady increase in temperature. The temperature ranges can be divided as follows: 1 hour at 950 to 1,250°C 1 hour at 1,250 to 1,450°C 1 hour at 1,450 to > 1,700°C

[0022] The long residence time serves to deacidify the limestone, thermally remove the salt components, and reduce the heavy metal content in the melt. After a residence time of three hours, the reactions that lead to the main phases mayenite, C12A7, monocalcium aluminate, CA, and gehlenite, CAS, in the calcium aluminate clinker are complete. Minor phases are spinel, MgAl2O4, and quartz, SiO2.

[0023] At approximately 1,400°C, the raw meal begins to liquefy. Turbulence in the melt leads to increased evaporation of the salts.

[0024] The liquid melt can be cooled by various methods.

[0025] To obtain a crystalline clinker, the melt is poured into a mold and cooled by mechanical crushing and the resulting increase in surface area through the ambient air.

[0026] To obtain an amorphous clinker structure, the melt is cooled by dry granulation on a granulation plate. The high cooling rate leads to a glassy solidification of the clinker. An amorphous structure leads to a higher activity potential of the clinker and thus to faster setting times and higher early strengths.

[0027] X-ray analysis of the resulting clinker shows an Al 2 O 3 content of 39 mass%. The chlorine content was reduced to 0.05 mass% by the melting process. Furthermore, the heavy metal content was significantly reduced by the removal of heavy metal chlorides. For example, 3,500 ppm Cu in the salt slag was reduced to 105 ppm Cu in the calcium aluminate clinker described.

[0028] When using other calcareous raw materials such as quicklime or fly ash, which have a different chemical composition, the specified weight ratios must be adjusted accordingly.

[0029] In various combustion tests, the following limit values ​​were always met (all values ​​in ppm): Table 2 V < 100 Cr < 200 Co < 200 Ni < 80 Cu < 500 Zn < 10

[0030] On an industrial scale, the salt slag is crushed (slag crusher, hammer mill) and classified. Aluminum is removed. The remaining salt slag is mixed with the CaO carrier without further processing, especially without washing, and fired or melted in a furnace. Cupola furnaces, shaft furnaces, induction furnaces, rotary drum furnaces, or electric arc furnaces can be used on an industrial scale. Fossil fuels (natural gas), also in combination with secondary fuels, or electricity (inductive, electric arc, etc.) can be used as energy sources. The salts melt at approximately 850°C; at 1,450°C, they evaporate. The heavy metals contained in the salt slag are partially volatilized under a reducing atmosphere if necessary, or heavy metal chlorides are formed and expelled. The melt is heated to 1,700°C.

[0031] After a certain holding time, both the salt loads and the heavy metals have largely evaporated, thus removing the remaining molten material. The melt is then poured out and cooled under specific conditions. If cooling occurs slowly, a calcium aluminate with high-alumina cement properties is formed. If the material is cooled very quickly, e.g., using the rotating cup process (dry granulation) or in a water bath, an "amorphous" structure is formed, significantly shortening the setting times. The cooling air is heated during dry granulation and can be used for recuperative energy recovery.

[0032] The exhaust gases / salt loads coming from the smelting plant are cooled, and the salts / heavy metal chlorides are separated in a first filter system. The heavy metal compounds remaining in the exhaust gases are bound and separated with activated carbon in a second filter system. By controlling the temperature of the exhaust gases, the chemical composition of the filter dust can be controlled.

[0033] The salts are returned to the aluminum industry, thus creating a complete cycle.

[0034] The heavy metals either remain in the salt (as heavy metal chlorides) and / or are removed in the second filter system with activated carbon.

[0035] The process according to the invention can be used to produce standard alumina cements (data in mass%): Table 3 ÖN EN 14647 Alumina content (as Al 2 O 3 ) 35%-58% Sulfide content (as S 2-< ) ≤ 0,10% Chloride content ≤ 0,10% Alkaline content (Na 2 O + 0.658 K 2 O) ≤ 0,4% Sulfate content (as SO 3 ) ≤ 0,5%

[0036] Possible compositions are (in mass%) Table 4 Al2O3 32-80 CaO 15-55 SiO2 0-7 Fe 2 O 3 0-1 MgO 0-6 SO3 0,0-0,2 Cl 0,0-0,2 TiO2 0,0-0,28

Claims

1. A method for the production of a hydraulic binder from a CaO containing substance and an Al2O3 containing by-product from secondary aluminium production, characterised in that the Al2O3 containing by-product is burned and melted together with the CaO containing substance at 1500°C to 2000°C, preferably at least 1700°C, without prior washing, in which the salts would have been removed, whereby the salts and heavy metals are expelled, and the volatile salts contained in the exhaust gases are recovered by cooling.

2. The method according to claim 1, characterised in that the burning and melting takes place under reduced atmosphere.

3. The method according to claim 1 or 2, characterised in that the properties of the burned or melted product are influenced by rapid cooling using the rotating cup method or in a water bath.

4. The method according to any of claims 1 to 3, characterised in that, after the resource recovery by cooling, the exhaust gases are additionally purified by filtering media, for example by adsorption using activated carbon.