USE OF Toughness Improvers to Increase the Maximum Linear Expansion of One-Component Heat-Curing Epoxy Resin Compounds
Patent Information
- Application Number
- DE502018015261
- Authority / Receiving Office
- DE · DE
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2017-12-19
- Filing Date
- 2018-12-18
- Publication Date
- 2024-11-14
- Estimated Expiration
- 2038-12-18
AI Technical Summary
Heat-curing epoxy resin compositions fail to maintain structural connections between substrates with different thermal expansion coefficients, leading to stress and potential failure during the curing process due to differential expansion and contraction.
A one-component thermosetting epoxy resin composition is developed, incorporating a toughness improver, such as a terminally blocked polyurethane prepolymer, with a specific weight ratio to the epoxy resin, which enhances the maximum linear expansion and mechanical properties, allowing the composition to withstand thermal stresses without bond failure.
The composition exhibits improved mechanical properties and increased maximum linear expansion, enabling it to maintain structural integrity and withstand high stresses during heat curing, thus ensuring a durable adhesive connection.
Description
Technical area
[0001] The invention relates to the field of heat-curing epoxy resin compositions, in particular for bonding substrates with different thermal expansion coefficients, in particular in the bodyshell of means of transport or white goods. State of the art
[0002] Heat-curing epoxy resin compositions have been known for a long time. An important application for heat-curing epoxy resin compositions is in vehicle construction, particularly for bonding the body shell of transport vehicles or white goods. In both cases, after the epoxy resin composition is applied, the bonded object is heated in an oven, which also cures the heat-curing epoxy resin composition.
[0003] When two substrates with different coefficients of thermal expansion are bonded together by structural bonding, the curing step in the oven at temperatures of 120–220°C causes the two substrates to expand to different lengths. During the subsequent cooling, this creates high stresses in the cured epoxy resin composition, which can lead to either failure of the adhesive bond, deformation of the substrates, or a so-called "freezing" of the stress in the bond. Such "freezing" makes the bond significantly more sensitive to static, dynamic, and impact loads over its lifetime, which can lead to weakening of the bond.
[0004] EP1916272 A1 and EP1916270 A1 describe heat-curing epoxy resin compositions containing a terminally blocked polyurethane prepolymer as an impact modifier. The disclosed compositions exhibit improved impact strength, good mechanical properties, and a high glass transition temperature. EP 2110397 A1 discloses impact modifiers obtained by reacting amphiphilic block copolymers and suitable for use in heat-curing epoxy resin adhesives.
[0005] There is therefore a need for heat-curing epoxy resin compositions for the structural bonding of substrates with different thermal expansion coefficients, which on the one hand have sufficient mechanical properties for structural bonding and on the other hand can withstand the high stresses occurring during heat curing without failure of the structural bond. Description of the invention
[0006] The object of the present invention is therefore to provide heat-curing epoxy resin compositions suitable for the structural bonding of substrates with different thermal expansion coefficients, which on the one hand have sufficient mechanical properties for structural bonding and on the other hand ensure the bond despite the high stresses occurring during heat curing without failure of the structural bond.
[0007] This object could surprisingly be achieved by an inventive use according to claim 1.
[0008] Further aspects of the invention are the subject of further independent claims. Particularly preferred embodiments of the invention are the subject of the dependent claims. Ways to implement the invention
[0009] The present invention relates to the use of at least one toughener D,to increase the maximum length expansion Max. stretch a one-component heat-curing epoxy resin composition, the one-component heat-curing epoxy resin composition comprising: a) at least one epoxy resin A with an average of more than one epoxy group per molecule; b) at least one latent hardener for epoxy resins B; wherein the weight ratio of the at least one epoxy resin A with an average of more than one epoxy group per molecule to which at least one toughener D of 0.3 - 2.2, and wherein the toughener is D is a terminally blocked polyurethane prepolymer of formula (I); where R 1< represents a p-valent radical of a linear or branched polyurethane prepolymer terminated with isocyanate groups after removal of the terminal isocyanate groups; p represents a value from 2 to 8; and R 2< represents a blocking group which splits off at a temperature above 100°C, where R 2< does not represent a substituent selected from the group consisting of R 12< represents an alkylene group having 2 to 5 carbon atoms, which may contain double bonds or be substituted, or a phenylene group or a hydrogenated phenylene group, in particular ε-caprolactam after removal of the NH proton. R 19< represents bisphenols, after removal of a hydroxyl group, in particular bisphenol-A, bisphenol-F, and 2,2'-diallylbisphenol-A.
[0010] The maximum length Max. stretchis determined in a tensile shear test during the cooling of a heated, cured tensile shear specimen.
[0011] In this document, the use of the term "independently of one another" in connection with substituents, residues or groups is to be interpreted as meaning that in the same molecule the substituents, residues or groups with the same name can occur simultaneously with different meanings.
[0012] In this document, a "toughness improver" is understood to mean an additive to an epoxy resin matrix which, even at low additions of ≥ 5 wt.%, in particular ≥ 10 wt.%, based on the total weight of the epoxy resin compositions, causes a significant increase in toughness and is thus able to absorb higher bending, tensile, impact or shock loads before the matrix tears or breaks.
[0013] In this document, the prefix "poly" in substance names such as "polyol", "polyisocyanate", "polyether" or "polyamine" indicates that the respective substance formally contains more than one of the functional groups mentioned in its name per molecule.
[0014] In this document, "molecular weight" refers to the molar mass (in grams per mole) of a molecule. "Mean molecular weight" refers to the number-average molecular weight Mn of an oligomeric or polymeric mixture of molecules, which is usually determined by GPC against polystyrene as a standard.
[0015] A "primary hydroxyl group" is an OH group that is bonded to a C atom with two hydrogens.
[0016] In this document, the term "primary amino group" refers to an NH2 group bonded to an organic residue, while the term "secondary amino group" refers to an NH group bonded to two organic residues, which may also together be part of a ring. Accordingly, an amine containing a primary amino group is referred to as a "primary amine," one containing a secondary amino group is referred to as a "secondary amine," and one containing a tertiary amino group is referred to as a "tertiary amine."
[0017] In this document, "room temperature" is defined as 23°C. Description Measurement method for maximum length extension (Max. Elongation) and maximum force
[0018] When two substrates, such as metals or fiber-reinforced plastics, with different coefficients of thermal expansion (Δα) are bonded together by structural bonding, particularly in body shell construction, the curing step in the oven at temperatures of 120–220°C, for example, when passing through a convection oven, causes the two substrates to expand to different lengths. During subsequent cooling, for example, when passing through cooling zones, this creates high stress in the cured epoxy resin composition, which leads either to failure of the adhesive bond, deformation of the substrates, or a so-called "freezing" of the stress in the adhesive bond.
[0019] In order to better investigate the behavior of cured epoxy resin compositions, a laboratory method was developed to evaluate their tolerance to "Δα induced" stresses.
[0020] Instead of inducing stress through thermal linear expansion, which would require specimens with dimensions similar to real car body components, the laboratory method applied the "Δα stress" to a tensile shear specimen using a tensile testing machine. The temperature profile in the convection oven was simulated by two thermocouples, allowing the tensile shear specimen to be tempered in the area of the bonding surface at defined heating and cooling rates. Since the cooling phase is the most critical, stress was applied via the tensile testing machine only during cooling in this test. Depending on the tensile speed setting on the tensile testing machine, variable stress drops that would occur with different substrate combinations can be simulated. Test specimens used and their preparation
[0021] For the simulation of "Δα induced" stresses, tensile shear test specimens were used, which were made of galvanized steel sheet (1.5 mm thickness, yield strength 420 MPa) as follows: Preparation:
[0022] 1.) Clean the steel sheet (25 mm x 100 mm x 1.5 mm) with heptane and then apply a defined amount of 3 g / m² of Anticorit PL3802-39S (deep-drawing oil, FUCHS Schmierstoffe GmbH). 2.) Limit the bonding surface (10 mm x 25 mm) with a Teflon spacer (1.5 mm thick) and apply the epoxy resin composition. 3.) Join the sheets and secure each bonding surface with a clamp. 4.) Heat the tensile shear specimens to 180°C for 35 minutes (dwell time) to cure the epoxy resin composition. 5.) After the specimens have cooled, remove the Teflon spacer. Parameter determination
[0023] As already mentioned, this test method allows for the simulation of various Δα-induced stress drops by adjusting the speed at which the tensile shear specimen is pulled. The following example illustrates the results of a material combination consisting of aluminum and steel (Δα = 13 * 10 -6< K -1< ), the necessary train speed can be calculated, taking into account equations (1) and (2).
[0024] Thermal expansion of solid bodies in linear approximation Δ L = L 0 ∗ α ∗ Δ T Δ T = T 2 − T 1
[0025] The initial length L 0 of both joining partners should be 1000mm. According to common temperature profiles in convection ovens, the heating and cooling of the samples was carried out using the Figure 1 shown temperature profile. This results in start and end temperatures T 1 / T 2 and the temperature difference Δ THeating and cooling rates were also chosen at 40°C / min, which is typical in the automotive industry. L 0 = 1000 mm α Stahl = 10.8 ∗ 10 − 6 K − 1 α Alu = 23.8 ∗ 10 − 6 K − 1 Δ T = 165 K T 2 = 190 ° C T 1 = 25 ° C Δ L Stahl = 1000 mm ∗ 10.8 ∗ 10 − 6 K − 1 ∗ 165 K = 1.782 mm Δ L Alu = 1000 mm ∗ 23.8 ∗ 10 − 6 K − 1 ∗ 165 K = 3.927 mm
[0026] The thermal expansion coefficients for steel α steel and aluminum α Alu were taken from the literature. Inserting the defined values into equations 1 and 2, one obtains the thermal expansion Δ L for steel and aluminum according to equations 4 and 5. This results in a linear expansion difference of 2.145 mm during the heating phase, by which aluminum expands more than steel. Accordingly, the cured epoxy resin composition, which forms a material bond, must compensate for a shrinkage difference of 2.145 mm during the cooling phase. Taking into account the cooling rate VA of 40°C / min, according to equations 6 and 7, a pulling speed V train of 0.52mm / min. V Zug = 3.927 mm − 1.782 mm ∗ 40 min ° C 190 ° C − 25 ° C = 0.52 mm / min Carrying out a measurement:
[0027] 1.) A tensile shear specimen prepared according to the preparation instructions described above is clamped into a tensile testing machine. Initially, however, only the lower clamping jaw is secured. The clamping length is 100 mm. 2.) Both thermocouples are pressed against the specimen so that they are in contact with the adhesive surface. 3.) The start and end temperatures are set to 25°C and 190°C on the control unit. 40°C / min is entered for the heating and cooling rates. 4.) The heating phase begins. 5.) When the final temperature of 190°C is reached, a countdown is used to hold the temperature for 2 minutes to ensure even heating of the adhesive surface. 6.) 30 seconds before the end of the countdown, the tensile shear specimen is also secured by the upper clamping jaw. 7.) When the countdown is over, the cooling phase begins automatically. At the same time, a tensile shear test is carried out manually using the control software of the tensile testing machine with a tensile speed of 0.52mm / min started. . Measurement results and evaluation
[0028] The measurement result is the force required to deform the tensile shear specimen to failure while cooling it from 190°C to 25°C. A triplicate determination is performed for each epoxy resin composition. The linear expansion Max. stretch is determined based on the traverse path traveled. To evaluate the measurement, the mean values of the maximum linear expansion are taken from the measurement report. Max. stretch ( ε M 2) at maximum force ( σ M 2) was used.
[0029] The higher the maximum length expansion achieved Max. stretch, the more "Δα tolerant" the epoxy resin composition can be considered. Furthermore, it is advantageous for a "Δα tolerant" epoxy resin composition if a low maximum force must be applied. Such epoxy resin compositions particularly preferably have a high maximum linear expansion. Max. stretchand a low maximum force required.
[0030] Also of interest is the time of failure. If this occurs before the end of the cooling phase, ie a fracture occurs at a tensile speed V train of 0.52mm / min before reaching a length extension of 2.145mm, the "Δ α Tolerance" of the epoxy resin composition is considered disadvantageous, since such an epoxy resin composition in a real application with ( L 0 = 1000 mm and Δ α = 13 * 10 -6< K -1< would lead to component failure. In contrast, if the fracture occurs at strains ≥2.145mm, this is considered the preferred "Δ α Tolerance". The higher the linear expansion, the better the "Δ α Tolerance".
[0031] Another interesting parameter is the force level at the end of the cooling phase, i.e., when a length of 2,145 mm is reached. The higher the force level, the more likely frozen stresses in the epoxy resin composition and irreversible deformations in the substrates are to be expected. Accordingly, the lowest possible force level is a favorable result here.
[0032] The maximum linear elongation Max. elongation is determined in a tensile shear test during the cooling of a heated, cured tensile shear specimen.
[0033] The maximum linear elongation Max. elongation is measured in a tensile shear test at a tensile speed V tensile of 0.52 mm / min.
[0034] The maximum linear elongation Max. elongation is determined as the linear elongation at the maximum force measured in the tensile shear test (maximum force).
[0035] The maximum linear extension Max. elongation is determined in the tensile shear test based on the traveled crosshead path.
[0036] The temperature of the tensile shear specimen for the tensile shear test is 190°C at the start of the measurement. At the start of the measurement, the tensile shear specimen is cooled to a temperature of 25°C at a cooling rate of 40°C / min and then left at this temperature. Preferably, the tensile shear specimen is heated to a temperature of 190°C at a heating rate of 40°C / min before the start of the measurement.
[0037] The tensile shear test is a tensile shear test for determining the tensile shear strength according to DIN EN 1465.
[0038] The tensile shear test is a tensile shear test with tensile shear test specimens that have the following characteristics: Steel sheets measuring 25mm x 100mm x 1.5mm, bonding surface of the cured one-component heat-curing epoxy resin composition measuring 10mm x 25mm with a thickness of 1.5mm, preferably 1.0mm.
[0039] The steel sheets used are preferably hot-dip galvanized steel. Furthermore, they preferably have a yield strength of at least 420 MPa to minimize the influence of substrate deformation.
[0040] The maximum length Max. stretch is determined based on the traverse path covered.
[0041] Preferably, the steel sheets are cleaned with heptane before applying the one-component heat-curing epoxy resin composition and then oiled with a deep-drawing oil, in particular Anticorit PL3802-39S, at a concentration of 3g / m 2<.
[0042] Preferably, the one-component heat-curing epoxy resin composition is cured at 180°C for 35 minutes.
[0043] The maximum linear expansion Max. expansion is ≥ 2.145 mm, preferably ≥ 2.2 mm, preferably ≥ 2.5 mm, preferably ≥ 2.8 mm, preferably ≥ 3.0 mm, preferably ≥ 3.5 mm, preferably ≥ 4.0 mm.
[0044] Preferably, the measured maximum force is ≤ 6000 N, preferably ≤ 5000 N, preferably ≤ 4500 N, preferably ≤ 4000 N, preferably ≤ 3500 N, preferably ≤ 3000 N, preferably ≤ 2500 N, preferably ≤ 2000 N.
[0045] Preferably, the measured force when reaching the maximum linear extension Max. extension of 2,145 mm is ≤ 4,000 N, preferably ≤ 3,000 N, preferably ≤ 2,500 N, preferably ≤ 2,000 N, preferably ≤ 1,500 N, preferably ≤ 1,000 N, preferably ≤ 800 N, preferably ≤ 700 N.
[0046] The epoxy resin AWith an average of more than one epoxy group per molecule, it is preferably a liquid epoxy resin or a solid epoxy resin. The term "solid epoxy resin" is well known to epoxy experts and is used in contrast to "liquid epoxy resins." The glass transition temperature of solid resins is above room temperature, meaning they can be ground into pourable powders at room temperature.
[0047] Preferred epoxy resins have the formula (II)
[0048] Here, the substituents R' and R" independently represent either H or CH 3 .
[0049] For solid epoxy resins, the index s stands for a value of > 1.5, in particular from 2 to 12.
[0050] Such solid epoxy resins are commercially available, for example from Dow, Huntsman or Hexion.
[0051] Compounds of formula (II) with an index s of 1 to 1.5 are referred to by those skilled in the art as semisolid epoxy resins. For the purposes of the present invention, they are also considered solid resins. However, preferred solid epoxy resins are epoxy resins in the narrower sense, i.e., where the index s has a value of > 1.5.
[0052] For liquid epoxy resins, the index s represents a value less than 1. Preferably, s represents a value less than 0.2.
[0053] These are therefore preferably diglycidyl ethers of bisphenol A (DGEBA), bisphenol F, and bisphenol A / F. Such liquid resins are available, for example, as Araldite ®< GY 250, Araldite ®< PY 304, Araldite ®< GY 282 (Huntsman), DER ™< 331 or DER ™< 330 (Dow), or Epikote 828 (Hexion).
[0054] Also suitable as epoxy resin A are so-called epoxy novolaks. These have the following formula: withR2= or CH 2 , R1 = H or methyl and z = 0 to 7.
[0055] In particular, these are phenol or cresol epoxy novolaks ( R2 = CH2).
[0056] Such epoxy resins are commercially available under the trade names EPN or ECN as well as Tactix ®< from Huntsman or under the DEN ™< product range from Dow Chemical.
[0057] Preferably, the epoxy resin A an epoxy liquid resin of formula (II).
[0058] In a particularly preferred embodiment, the heat-curing epoxy resin composition contains both at least one liquid epoxy resin of the formula (II) with s < 1, in particular less than 0.2, and at least one solid epoxy resin of the formula (II) with s > 1.5, in particular from 2 to 12.
[0059] The proportion of epoxy resin Ais preferably 10 - 60 wt.%, in particular 30 - 50 wt.%, based on the total weight of the epoxy resin composition.
[0060] Furthermore, it is advantageous if 60-100 wt.%, in particular 60-80 wt.%, of the epoxy resin A is a previously mentioned epoxy liquid resin.
[0061] Furthermore, it is advantageous if 0-40 wt.%, in particular 20-40 wt.%, of the epoxy resin A is a previously mentioned solid epoxy resin.
[0062] The heat-curing epoxy resin composition contains at least one latent hardener B for epoxy resins. This is activated by elevated temperatures, preferably at temperatures of 70°C or more.
[0063] This is preferably a hardener selected from the group consisting of dicyandiamide; guanidines; anhydrides of polybasic carboxylic acids; dihydrazides and aminoguanidines.
[0064] The hardener is particularly preferred B Dicyandiamide.
[0065] The amount of latent hardener B for epoxy resins, is advantageously 0.1 - 30 wt.%, in particular 0.2 - 10 wt.%, preferably 1 - 10 wt.%, particularly preferably 5 - 10 wt.%, based on the weight of the epoxy resin A.
[0066] Preferably, the heat-curing epoxy resin composition additionally contains at least one accelerator Cfor epoxy resins. Such accelerating hardeners are preferably substituted ureas, such as 3-(3-chloro-4-methylphenyl)-1,1-dimethylurea (chlorotoluron) or phenyldimethylureas, especially p-chlorophenyl-N,N-dimethylurea (monuron), 3-phenyl-1,1-dimethylurea (fenuron), or 3,4-dichlorophenyl-N,N-dimethylurea (diuron). Furthermore, compounds from the imidazole class, such as 2-isopropylimidazole or 2-hydroxy-N-(2-(2-(2-hydroxyphenyl)-4,5-dihydroimidazol-1-yl)ethyl)benzamide, imidazolines, and amine complexes, can be used.
[0067] Preferably, the accelerator C for epoxy resins selected from the list consisting of substituted ureas, imidazoles, imidazolines and amine complexes.
[0068] The accelerator is particularly preferred Cfor epoxy resins selected from the list consisting of substituted ureas and amine complexes, especially when the latent hardener B is a guanidine, in particular dicyandiamide.
[0069] The one-component heat-curing epoxy resin composition contains at least one toughener D. The toughness improvers D can be solid or liquid.
[0070] The toughness improver is D a terminally blocked polyurethane polymer of formula (I).
[0071] Here, R 1< represents a p-valent radical of a linear or branched polyurethane prepolymer terminated with isocyanate groups after removal of the terminal isocyanate groups and p represents a value from 2 to 8.
[0072] Furthermore, R 2< represents a blocking group which splits off at a temperature above 100°C, where R 2< does not represent a substituent selected from the group consisting of where R 12< represents an alkylene group having 2 to 5 carbon atoms, which may contain double bonds or be substituted, or a phenylene group or a hydrogenated phenylene group, in particular ε-caprolactam after removal of the NH proton; and R 19< represents bisphenols, after removal of a hydroxyl group, in particular bisphenol-A, bisphenol-F, and 2,2'-diallylbisphenol-A, particularly preferably bisphenol-A and bisphenol-F. In this context, the term "bisphenols" preferably refers to compounds which, as a common structural feature, contain two phenol rings linked via a carbon atom.
[0073] Surprisingly, it was found that the above-mentioned substituents insufficient values for the maximum length extension Max. stretch This can be seen, for example, in the comparison of Examples 8 and 9 in Table 4 with the examples in Table 3.
[0074] Preferably, R 2< independently represent a substituent selected from the group consisting of where R 5< , R 6< , R 7< and R 8< each independently represent an alkyl or cycloalkyl or aralkyl or arylalkyl group or R 5< together with R 6< , or R 7< together with R 8< , form part of a 4- to 7-membered ring which is optionally substituted; R 9< , R 9'< and R 10< each independently represent an alkyl or aralkyl or arylalkyl group or an alkyloxy or aryloxy or aralkyloxy group; R 11< stands for an alkyl group, R 13< and R 14< each independently represent an alkylene group having 2 to 5 C atoms, which may optionally have double bonds or be substituted, or a phenylene group or a hydrogenated phenylene group; R 15< , R 16< and R 17< each independently represent H or an alkyl group or an aryl group or an aralkyl group;and R 18< represents an aralkyl group having a substituted or unsubstituted aromatic group or a mononuclear substituted or unsubstituted aromatic group which optionally contains aromatic hydroxyl groups; R 4< represents a residue of an aliphatic, cycloaliphatic, aromatic or araliphatic epoxide containing a primary or secondary hydroxyl group after removal of the hydroxy and epoxide groups; and m represents a value of 1, 2 or 3. ;
[0075] Particularly preferably, R 2< independently of one another represent a substituent which is selected from the group consisting of in particular preferably and ---OR 18< , particularly preferred ---OR 18< and most preferred for ---OR 18< .
[0076] Surprisingly, it was found that this resulted in higher values for the Young's modulus, tensile strength, elongation at break, tensile shear strength, angle peel strength, and impact peel strength. This can be seen, for example, in Table 3 when comparing Examples 1-7.
[0077] Phenols after removal of a hydroxyl group are particularly to be considered as R 18<. Preferred examples of such phenols are selected in particular from the list consisting of phenol, cresol, 4-methoxyphenol (HQMME), resorcinol, pyrocatechol, cardanol (3-pentadecenylphenol (from cashew nut shell oil)), and nonylphenol.
[0078] On the other hand, hydroxybenzyl alcohol and benzyl alcohol after removal of a hydroxyl group are to be considered as R 18<.
[0079] As a substituent of the formula ---OR 18<, monophenols are preferred after removal of a phenolic hydrogen atom. Particularly preferred examples of such radicals R 2< are radicals selected from the group consisting of and preferred
[0080] The radical Y here represents a saturated, aromatic, or olefinically unsaturated hydrocarbon radical having 1 to 20 carbon atoms, in particular having 1 to 15 carbon atoms. Particularly preferred Ys are allyl, methyl, nonyl, dodecyl, phenyl, alkyl ethers, in particular methyl ethers, carboxylic acid esters, or an unsaturated C15-alkyl radical having 1 to 3 double bonds. Most preferably, Y is selected from the group consisting of alkyl ethers, in particular methyl ethers, and unsaturated C15-alkyl radicals having 1 to 3 double bonds.
[0081] Particularly preferably, R 18< is a phenol after removal of a hydroxyl group, particularly preferred examples of such phenols are selected from the list consisting of 4-methoxyphenol (HQMME) and cardanol (3-pentadecenylphenol (from cashew nut shell oil)).
[0082] If R 5< , R 6< , R 7< , R 8< , R 9< , R 9'< , R 10< , R 11< , R 15< , R 16< or R 17< represents an alkyl group, this is in particular a linear or branched C 1 -C 20 alkyl group.
[0083] If R 5< , R 6< , R 7< , R 8< , R 9< , R 9'< , R 10< , R 15< , R 16< or R 17< represents an aralkyl group, this group is in particular an aromatic group bonded via methylene, in particular a benzyl group.
[0084] If R 5< , R 6< , R 7< , R 8< , R 9< , R 9'< or R 10< represents an alkylaryl group, this is in particular a C 1 to C 20 alkyl group bonded via phenylene, such as, for example, tolyl or xylyl.
[0085] The terminally blocked polyurethane prepolymer of formula (I) is prepared from the isocyanate-terminated linear or branched polyurethane prepolymer with one or more isocyanate-reactive compounds R 2< H. If several such isocyanate-reactive compounds are used, the reaction can be carried out sequentially or with a mixture of these compounds.
[0086] The polyurethane prepolymer with isocyanate end groups on which R 1< is based can be prepared in particular from at least one diisocyanate or triisocyanate and from a polymer Q PM with terminal amino, thiol or hydroxyl groups.
[0087] Suitable diisocyanates are aliphatic, cycloaliphatic, aromatic, or araliphatic diisocyanates, especially commercially available products such as methylenediphenyl diisocyanate (MDI), hexamethylene diisocyanate (HDI), toluene diisocyanate (TDI), tolidine diisocyanate (TODI), isophorone diisocyanate (IPDI), trimethylhexamethylene diisocyanate (TMDI), 2,5- or 2,6-bis(isocyanatomethyl)bicyclo[2.2.1]heptane, 1,5-naphthalene diisocyanate (NDI), dicyclohexylmethyl diisocyanate (H12MDI), p-phenylene diisocyanate (PPDI), m-tetramethylxylylene diisocyanate (TMXDI), etc., as well as their dimers. HDI, IPDI, MDI, or TDI are preferred.
[0088] Suitable triisocyanates are trimers or biurets of aliphatic, cycloaliphatic, aromatic, or araliphatic diisocyanates, especially the isocyanurates and biurets of the diisocyanates described in the previous paragraph. Suitable mixtures of di- or triisocyanates can also be used.
[0089] As polymers Q PM with terminal amino, thiol or hydroxyl groups are particularly suitable polymers Q PM with two or three terminal amino, thiol or hydroxyl groups.
[0090] The polymers Q PM advantageously have an equivalent weight of 300 - 6000, in particular 600 - 4000, preferably 700 - 2200 g / equivalent of NCO-reactive groups.
[0091] As polymers Q PM Preferred are polyols having average molecular weights between 600 and 6000 Daltons selected from the group consisting of polyethylene glycols, polypropylene glycols, polyethylene glycol-polypropylene glycol block polymers, polybutylene glycols, polytetramethylene ether glycols, hydroxyl-terminated polybutadienes, hydroxyl-terminated butadiene-acrylonitrile copolymers and mixtures thereof, particularly preferred are polytetramethylene ether glycols and hydroxyl-terminated polybutadienes.
[0092] One or more polytetramethylene ether glycols can be used. Polytetramethylene ether glycol is also known as polytetrahydrofuran or PTMEG. PTMEG can be produced, for example, by polymerizing tetrahydrofuran, e.g., via acid catalysis. Polytetramethylene ether glycols are primarily diols.
[0093] Polytetramethylene ether glycols are commercially available, e.g. the PolyTHF ®< products from BASF such as PolyTHF ®< 2000, PolyTHF ®< 2500 CO or PolyTHF ®< 3000 CO, the Terathane ®< products from Invista BV or the Polymeg ®< products from LyondellBasell.
[0094] The OH functionality of the polytetramethylene ether glycol used is preferably in the range of about 2, e.g., in the range of 1.9 to 2.1. This is due to the cationic polymerization of the starting monomer tetrahydrofuran.
[0095] Polytetramethylene ether glycols with OH numbers between 170 mg / KOH g and 35 mg KOH / g are advantageous, preferably in the range from 100 mg KOH / g to 40 mg KOH / g, and most preferably from 70 to 50 mg KOH / g. Unless otherwise stated, the OH number is determined titrimetrically in accordance with DIN 53240 in this application. The hydroxyl number is determined by acetylation with acetic anhydride and subsequent titration of the excess acetic anhydride with alcoholic potassium hydroxide solution.
[0096] With knowledge of the difunctionality, the OH equivalent weights or the average molecular weight of the polytetramethylene ether glycol used can be determined from the titrimetrically determined hydroxyl numbers.
[0097] Polytetramethylene ether glycols advantageously used in the present invention preferably have an average molecular weight in the range from 600 to 5000 g / mol, more preferably 1000 to 3000 g / mol and particularly preferably in the range from 1500 to 2500 g / mol, in particular about 2000 g / mol.
[0098] One or more hydroxy-terminated polybutadienes can be used. Mixtures of two or more hydroxy-terminated polybutadienes can also be used.
[0099] Suitable hydroxy-terminated polybutadienes include, in particular, those produced by radical polymerization of 1,3-butadiene, using, for example, an azonitrile or hydrogen peroxide as an initiator. Hydroxy-terminated polybutadienes are commercially available, for example, the Poly bd ®< products from Cray Valley such as Poly bd ®< R45V, Polyvest ®< HT from Evonik, and Hypro ®< 2800X95HTB from Emerald Performance Materials LLC.
[0100] The hydroxy-terminated polybutadiene preferably has an average molecular weight of less than 5,000, preferably in the range of 2,000 to 4,000 g / mol. The OH functionality of the hydroxy-terminated polybutadiene is preferably in the range of 1.7 to 2.8, preferably 2.4 to 2.8.
[0101] Further preferred are hydroxy-terminated polybutadienes with an acrylonitrile content of less than 15%, preferably less than 5%, particularly preferably less than 1%, particularly preferably less than 0.1%. Most preferred are hydroxy-terminated polybutadienes free of acrylonitrile.
[0102] Based on the total weight of the polyols used to produce the isocyanate-terminated polymer, the total proportion of polytetramethylene ether glycol and hydroxy-terminated polybutadiene is preferably at least 95 wt.% and more preferably at least 98 wt.%. In a preferred embodiment, only polytetramethylene ether glycol and / or hydroxy-terminated polybutadiene are used as polyols.
[0103] The weight ratio of polytetramethylene ether glycol to hydroxy-terminated polybutadiene is preferably in the range of 100 / 0 to 70 / 30, more preferably 100 / 0 to 60 / 40, more preferably 100 / 0 to 90 / 10, and most preferably 100 / 0.
[0104] This is advantageous in that it results in higher values for the Young's modulus, tensile strength, elongation at break, tensile shear strength, angle peel strength, and impact peel strength. This can be seen, for example, in the comparison of Examples 2 and 3 in Table 3.
[0105] In a preferred embodiment, the polyurethane prepolymer is made from at least one diisocyanate or triisocyanate and from a polymer Q PM with terminal amino, thiol or hydroxyl groups. The polyurethane prepolymer is prepared in a manner known to the polyurethane expert, in particular by adding the diisocyanate or triisocyanate in a stoichiometric excess with respect to the amino, thiol or hydroxyl groups of the polymer. Q PM is used.
[0106] The polyurethane prepolymer with isocyanate end groups preferably has an elastic character. It preferably exhibits a glass transition temperature (Tg) of less than 0°C.
[0107] The weight ratio of at least one epoxy resin A with an average of more than one epoxy group per molecule to which at least one toughener D is from 0.3 - 2.2.
[0108] A weight ratio of less than 0.3 is disadvantageous in that the compositions cure very slowly or not at all. Furthermore, particularly low values for elastic modulus, tensile strength, and angle peel strength are obtained.
[0109] A weight ratio of more than 2.2 is disadvantageous in that it results in compositions which have low values for impact peel strength and maximum linear expansion.
[0110] This can be seen, for example, in Table 6.
[0111] Preferably, the weight ratio of the at least one epoxy resin A with an average of more than one epoxy group per molecule to which at least one toughener D of 0.4 - 2.0, particularly preferably 0.5 - 1.8, most preferably 0.6 - 1.4. This is advantageous in that the compositions exhibit high values for angle peel strength and impact peel strength.
[0112] Furthermore, it may be advantageous if the weight ratio is 0.3 - 2.2, in particular 0.4 - 2.2, 0.6 - 2.2, 1.0 - 2.2, 1.4 - 2.2, preferably 1.8 - 2.2. This is advantageous in that the compositions exhibit high values for elastic modulus and tensile strength.
[0113] If the weight ratio is 0.4 - 2.0, in particular 0.4 - 1.8, preferably 0.4 - 1.4, particularly preferably 0.4 - 1.0, this is advantageous in that the compositions thereby have high values for the impact peel strength at -30°C, if R 2< is selected from the group consisting of ---OR 18< and most preferably ---OR 18< .
[0114] Furthermore, it may be advantageous if the weight ratio is 0.3 - 2.0, in particular 0.3 - 1.8, 0.3 - 1.4, 0.3 - 1.0, 0.3 - 0.6, preferably 0.3 - 0.4. This results in compositions with high values for the maximum linear expansion. Max. stretch and get maximum power.
[0115] In a further preferred embodiment, the composition additionally contains at least one filler F.These are preferably mica, talc, kaolin, wollastonite, feldspar, syenite, chlorite, bentonite, montmorillonite, calcium carbonate (precipitated or ground), dolomite, quartz, silica (pyrogenic or precipitated), cristobalite, calcium oxide, aluminum hydroxide, magnesium oxide, hollow ceramic spheres, hollow glass spheres, organic hollow spheres, glass spheres, color pigments.
[0116] Advantageously, the total proportion of the total filler is F 5 - 40% by weight, preferably 10 - 30% by weight, based on the total weight of the epoxy resin composition.
[0117] In a further embodiment, the composition may contain a physical or chemical blowing agent, such as is available, for example, under the trade name Expancel™ from Akzo Nobel or Celogen™ from Chemtura, or under the trade name Luvopor® from Lehmann & Voss. The proportion of the blowing agent is typically 0.1-3 wt.%, based on the total weight of the epoxy resin composition. Preferably, the composition contains less than 1 wt.%, more preferably less than 0.5 wt.%, more preferably less than 0.3 wt.%, and most preferably less than 0.1 wt.% of physical or chemical blowing agent, based on the total weight of the epoxy resin composition.
[0118] In a further preferred embodiment, the composition additionally contains at least one reactive diluent carrying epoxy groups G.Such reactive diluents are known to those skilled in the art. Preferred examples of reactive diluents containing epoxy groups are: Glycidyl ethers of monofunctional saturated or unsaturated, branched or unbranched, cyclic or open-chain C 4 - C 30 alcohols, e.g. butanol glycidyl ether, hexanol glycidyl ether, 2-ethylhexanol glycidyl ether, allyl glycidyl ether, tetrahydrofurfuryl and furfuryl glycidyl ether, trimethoxysilyl glycidyl ether, etc. Glycidyl ethers of difunctional saturated or unsaturated, branched or unbranched, cyclic or open-chain C 2 - C 30 alcohols, e.g. ethylene glycol, butanediol, hexanediol, octanediol glycidyl ether, cyclohexanedimethanol diglycidyl ether, neopentyl glycol diglycidyl ether, etc. Glycidyl ethers of tri- or polyfunctional, saturated or unsaturated, branched or unbranched, cyclic or open-chain alcohols such as epoxidized castor oil, epoxidized trimethylolpropane, epoxidized pentaerythrol or polyglycidyl ethers of aliphatic polyols such as sorbitol, glycerin, trimethylolpropane, etc.Glycidyl ethers of phenol and aniline compounds such as phenyl glycidyl ether, cresyl glycidyl ether, p-tert-butylphenyl glycidyl ether, nonylphenol glycidyl ether, 3-n-pentadecenyl glycidyl ether (from cashew nut shell oil), N,N-diglycidylaniline etc. Epoxidized amines such as N,N-diglycidylcyclohexylamine etc. Epoxidized mono- or dicarboxylic acids such as neodecanoic acid glycidyl ester, methacrylic acid glycidyl ester, benzoic acid glycidyl ester, phthalic acid, tetra- and hexahydrophthalic acid diglycidyl esters, diglycidyl esters of dimeric fatty acids etc. Epoxidized di- or trifunctional, low to high molecular weight polyether polyols such as polyethylene glycol diglycidyl ether, polypropylene glycol diglycidyl ether etc.
[0119] Particularly preferred are hexanediol diglycidyl ether, cresyl glycidyl ether, p-tert-butylphenyl glycidyl ether, polypropylene glycol diglycidyl ether and polyethylene glycol diglycidyl ether.
[0120] Advantageously, the total proportion of the epoxy group-bearing reactive diluent is G 0.1 - 15% by weight, preferably 0.1 - 5% by weight, particularly preferably 0.1 - 2% by weight, particularly preferably 0.2 - 1% by weight, based on the total weight of the epoxy resin composition.
[0121] The composition may comprise further components, in particular catalysts, stabilizers, in particular heat and / or light stabilizers, thixotropic agents, plasticizers, solvents, mineral or organic fillers, blowing agents, dyes and pigments, corrosion inhibitors, surfactants, defoamers and adhesion promoters.
[0122] Phenol alkylsulfonic acid esters or benzenesulfonic acid N-butylamide, which are commercially available as Mesamoll ®< or Dellatol BBS from Bayer, are particularly suitable as plasticizers.
[0123] Suitable stabilizers are, in particular, optionally substituted phenols such as BHT or Wingstay ®< T (Elikem), sterically hindered amines or N-oxyl compounds such as TEMPO (Evonik).
[0124] A particularly preferred one-component epoxy resin composition comprises: 10 - 60 wt.%, in particular 20 - 40 wt.%, based on the total weight of the epoxy resin composition, epoxy resin A with an average of more than one epoxy group per molecule; preferably 60-100 wt.%, in particular 60-80 wt.%, of the epoxy resin A an epoxy liquid resin and at 0-40 wt.%, in particular 20-40 wt.%, of the epoxy resin A a solid epoxy resin; . at least one latent hardener for epoxy resins B,preferably selected from dicyandiamide, guanidines, anhydrides of polybasic carboxylic acids, dihydrazides, and aminoguanidines, as well as their derivatives, with dicyandiamide being preferred; preferably at least one accelerator C, selected from the list consisting of substituted ureas, imidazoles, imidazolines and amine complexes, in particular selected from the list consisting of substituted ureas and amine complexes, particularly preferably substituted ureas; at least one aforementioned toughener D, Preferred are those which have been previously described as preferred tougheners D described, preferably the proportion of toughener is D20-60 wt.%, 25-55 wt.%, 30-50 wt.%, particularly preferably 30-40 wt.%, based on the total weight of the epoxy resin composition; preferably 5-40 wt.%, preferably 10-30 wt.%, based on the total weight of the epoxy resin composition, of a filler F selected preferably from the group consisting of wollastonite, calcium carbonate, calcium oxide, color pigments, in particular carbon black, and pyrogenic silicas, in particular calcium carbonate, calcium oxide and pyrogenic silicas; preferably 0.1 - 15% by weight, preferably 0.1 - 5% by weight, particularly preferably 0.1 - 2% by weight, particularly preferably 0.2 - 1% by weight, based on the total weight of the epoxy resin composition, of an epoxy group-bearing reactive diluent G; wherein the weight ratio of the at least one epoxy resin A with an average of more than one epoxy group per molecule to which at least one toughener Dof 0.3 - 2.2, 0.4 - 2.0, particularly preferably 1.0 - 1.8.
[0125] Furthermore, it may be advantageous if the preferred one-component epoxy resin composition consists of more than 80% by weight, preferably more than 90% by weight, in particular more than 95% by weight, particularly preferably more than 98% by weight, most preferably more than 99% by weight, based on the total weight of the epoxy resin composition, of the aforementioned components.
[0126] An example of a particularly preferred composition is, for example, Example 13 in Table 5.
[0127] It is advantageous if the epoxy resin composition according to the invention has a viscosity at 25°C of 100–10,000 Pa*s, in particular 500–5,000 Pa*s, preferably 1,000–3,000 Pa*s. This is advantageous in that it ensures good applicability. The viscosity is preferably measured as described in the examples.
[0128] Particularly preferred are heat-curing epoxy resin compositions which, in the cured state: a tensile shear strength, in particular measured according to DIN EN 1465, particularly preferably as described in the example section, of more than 10 MPa, more than 15 MPa, more than 20 MPa, and / or a tensile strength, in particular measured according to DIN EN ISO 527, particularly preferably as described in the example section, of more than 10 MPa, more than 15 MPa, more than 20 MPa, and / or an elongation at break, in particular measured according to DIN EN ISO 527, particularly preferably as described in the example section, of more than 10%, more than 20%, more than 30%, in particular 30 - 200%, particularly preferably 30 - 150%, and / or an E-modulus, in particular measured according to DIN EN ISO 527, particularly preferably as described in the example section, of 300 - 1000 MPa, in particular 500 - 800 MPa.an impact peel strength, in particular measured according to ISO 11343, particularly preferably as described in the examples, of more than 30 N / mm, more than 40 N / mm, more than 60 N / mm at 23°C, and / or an angle peel strength, in particular measured according to DIN 53281, particularly preferably as described in the examples, of more than 5 N / mm, more than 8 N / mm, more than 10 N / mm.
[0129] The invention comprises the use of at least one toughener D, to increase the maximum length expansion Max. stretch a previously mentioned one-component heat-curing epoxy resin composition.
[0130] The increase in the maximum length Max. stretch refers to the comparison with a one-component thermosetting epoxy resin composition, which in particular does not: the inventive weight ratio of the at least one epoxy resin Awith an average of more than one epoxy group per molecule to which at least one toughener D and / or a toughener according to the invention D has.
[0131] Preferably, in the use according to the invention, the increase in the maximum length extension is Max. stretch, compared to a one-component thermosetting epoxy resin composition, which in particular does not: the inventive weight ratio of the at least one epoxy resin A with an average of more than one epoxy group per molecule to which at least one toughener D and / or a toughener according to the invention D has, more than 20%, more than 30%, in particular more than 40%, more than 50%, particularly preferably more than 75%, particularly preferably more than 100%.
[0132] It has further been shown that the described heat-curing epoxy resin compositions are particularly suitable for use as one-component heat-curing adhesives, in particular as heat-curing one-component adhesives in vehicle construction and sandwich panel construction. Such a one-component adhesive has a wide range of applications. In particular, heat-curing one-component adhesives can be realized with them that are characterized by high impact strength, both at elevated temperatures and at low temperatures. Such adhesives are required for bonding heat-stable materials. Heat-stable materials are understood to be materials that are dimensionally stable at a curing temperature of 100–220°C, preferably 120–200°C, at least during the curing time.In particular, these include metals and plastics such as ABS, polyamide, epoxy resin, polyester resin, polyphenylene ether, and fiber-reinforced plastics such as glass fiber and carbon fiber reinforced plastics. Fiber-reinforced plastics are particularly preferred as plastics. The preferred application is one in which at least one material is a metal. A particularly preferred use is the bonding of different metals, in particular metals with different coefficients of thermal expansion (Δα) and / or the bonding of metals with fiber-reinforced plastics, particularly in bodyshell construction in the automotive industry. The preferred metals are primarily steel, in particular electrogalvanized, hot-dip galvanized, oiled steel, Bonazink-coated steel, and subsequently phosphated steel, as well as aluminum, particularly in the variants typically found in automotive construction.
[0133] Such an adhesive is in particular first contacted with the materials to be bonded at a temperature of between 10°C and 80°C, in particular between 10°C and 60°C, and later cured at a temperature of typically 130 - 220°C, preferably 140 - 200°C, particularly preferably 150 - 190°C.
[0134] Such a use as mentioned above results in a bonded article. Such an article is preferably a vehicle or a part of a vehicle.
[0135] A further aspect of the present invention therefore relates to a bonded article obtained from the aforementioned use. Of course, in addition to heat-curing adhesives, a composition according to the invention can also be used to produce sealants. Furthermore, the compositions according to the invention are suitable not only for automotive construction but also for other areas of application. Particular mention should be made of related applications in the construction of means of transport, such as ships, trucks, buses, or rail vehicles, or in the construction of consumer goods, such as washing machines.
[0136] The materials bonded by means of an aforementioned composition are used at temperatures between typically 120°C and -40°C, preferably between 100°C and -40°C, in particular between 80°C and -40°C. Examples
[0137] The following are some examples which further illustrate the invention but are not intended to limit the scope of the invention in any way. Determination of isocyanate content
[0138] The isocyanate content was determined in wt. % by back titration with an excess of di-n-butylamine and 0.1 M hydrochloric acid. All determinations were performed semi-manually on a Mettler-Toledo DL50 Graphix titrator with automatic potentiometric endpoint determination. For this purpose, 600–800 mg of the sample to be determined were dissolved, with heating, in a mixture of 10 ml of isopropanol and 40 ml of xylene and then reacted with a solution of dibutylamine in xylene. Excess di-n-butylamine was titrated with 0.1 M hydrochloric acid, and the isocyanate content was calculated from this. Maximum elongation (Max. elongation) and maximum force (Max. force)
[0139] The maximum linear extension (Max. Extension) and the maximum force (Max. Force) were determined as described above under "Description of the Measurement Method for Maximum Linear Extension (Max. Extension) and Maximum Force." A triplicate determination was performed for each epoxy resin composition. The maximum linear extension Max. stretch was determined based on the traverse path. To evaluate the measurement, the mean values of the maximum linear expansion were taken from the measurement protocol. Max. stretch ( ε M 2) at maximum force ( σ M 2) was used. Tensile strength, elongation at break and modulus of elasticity (DIN EN ISO 527)
[0140] An adhesive sample was pressed between two sheets of Teflon paper to a thickness of 2 mm. After 35 minutes of curing at 175°C, the Teflon paper was removed and the test specimens were punched out according to DIN standards. The test specimens were measured under standard conditions at a tensile speed of 2 mm / min. Tensile strength, elongation at break, and the 0.05-0.25% Young's modulus were determined according to DIN EN ISO 527. Lap shear strength (LSS) (DIN EN 1465)
[0141] Cleaned and re-oiled with Anticorit PL 3802-39S, H420+Z steel test panels (1.2 mm thick) were bonded to a 25 × 10 mm bonding area with glass beads as spacers in a layer thickness of 1.5 mm and cured under the specified curing conditions. Curing conditions: a) 35 min at 175°C oven temperature.
[0142] The tensile shear strength was determined on a tensile machine at a tensile speed of 10 mm / min in a triplicate determination according to DIN EN 1465. Angle peel strength (T-Peel) (DIN 53281)
[0143] Test panels measuring 130 x 25 mm were prepared from DC-04+ZE steel (0.8 mm thick). The test panels were unrolled to a height of 30 mm using a suitable punching machine (90°). The cleaned and re-oiled 100 x 25 mm surfaces, measuring 0.3 mm thick with Anticorit PL 3802-39S, were bonded with the adhesive using glass beads as spacers and cured for a 35-minute dwell time after reaching an oven temperature of 175 °C. The angle peel strength was determined on a tensile test machine at a tensile speed of 100 mm / min in a double determination as a peel force in N / mm over a range of 1 / 6 to 5 / 6 of the crosshead travel. Impact peel strength (according to ISO 11343)
[0144] The test specimens were manufactured using the adhesive and steel DC04+ZE, measuring 90 x 20 x 0.8 mm. The bonding area was 20 x 30 mm, with a layer thickness of 0.3 mm, and glass beads were used as spacers. The impact peel strength was measured in triplicate at the specified temperatures (RT = 23 °C, -30 °C) using a Zwick 450 impact pendulum at 2 m / s. The impact peel strength is expressed as the average force in N / mm under the measurement curve from 25% to 90% according to ISO 11343.
[0145] The adhesives were cured at 175°C oven temperature for 35 min. viscosity
[0146] Viscosity measurements on the adhesives were carried out 1 day after production on an Anton Paar MCR 101 rheometer using an oscillatory plate-plate geometry at a temperature of 25°C or 50°C with the following parameters: 5 Hz, 1 mm gap, plate-plate distance 25 mm, 1% deformation.
[0147] The following commercial products were used to produce impact modifiers 1 to 9: Table 1: Connection Description Manufacturer BHT (Ionol ®< CP) Stabilizer butylhydroxytoluene Evonik PolyTHF ®< 2000 difunctional polytetramethylene ether glycol with a molecular weight of 2000 g / mol BASF Poly bd ®< R45V Hydroxyl terminated polybutadiene with a molecular weight of 2800 g / mol, OH functionality approx. 2.4-2.6 Cray Valley Vestanat IPDI Isophorone diisocyanate Evonik Dibutyltin dilaurate catalyst Thorson 4-Methoxyphenol Blocking agents Solvay phenol Blocking agents Sigma-Aldrich Caprolactam Blocking agents Sigma-Aldrich Methylethylketoxime Blocking agents Sigma-Aldrich 2-Benzoxazolinone Blocking agents Synthesia 3,5-Dimethylpyrazole Blocking agents Chemtura 2,2-Diallylbisphenol A Blocking agents Sigma-Aldrich Example 1: Impact modifier SM1 (phenol [1.2 eq.] as blocking agent, PolyTHF2000 / Poly BD R45HTLO backbone)
[0148] 225 g of PolyTHF 2000, 225 g of Poly bd R45V, and 2.25 g of BHT as a stabilizer were dehydrated for 1 h under vacuum at 90°C with minimal stirring. Subsequently, 90.83 g of isophorone diisocyanate (IPDI) and 0.059 g of dibutyltin dilaurate (DBTDL) were added. The reaction was carried out for 2 h under vacuum at 90°C with moderate stirring to obtain an isocyanate-terminated polymer: Measured free NCO content: 3.05%.
[0149] 0.117 g of dibutyltin dilaurate (DBTDL) and 44.35 g of phenol were added to the resulting NCO-terminated polymer, and the isocyanate groups were removed by reaction under vacuum at 110°C for 5 h. Measured free NCO content: 0.53% (immediately after preparation), 0.24% (1 day after preparation). Example 2: Impact modifier SM2 (4-methoxyphenol [1.2 eq.] as blocking agent, PolyTHF2000 / PolyBD R45V as backbone)
[0150] 200 g of PolyTHF 2000, 200 g of Poly bd R45V, and 2.00 g of BHT as a stabilizer were dehydrated for 1 h under vacuum at 90 °C with minimal stirring. Subsequently, 80.64 g of isophorone diisocyanate (IPDI) and 0.053 g of dibutyltin dilaurate (DBTDL) were added. The reaction was carried out for 2 h under vacuum at 90 °C with moderate stirring to obtain an isocyanate-terminated polymer: Measured free NCO content: 2.81%.
[0151] 0.106 g of dibutyltin dilaurate (DBTDL) and 47.93 g of 4-methoxyphenol (HQMME) were added to the resulting NCO-terminated polymer, and the isocyanate groups were removed by reaction under vacuum at 110°C for 5 h. Measured free NCO content: 2.82% (immediately after preparation), 0.09% (1 day after preparation). Example 3: Impact modifier SM3 (4-methoxyphenol [1.2eq.] as blocking agent, PolyTHF 2000 as backbone)
[0152] 350 g of PolyTHF 2000 and 3.50 g of BHT as a stabilizer were dehydrated for 1 h under vacuum at 90°C with minimal stirring. Subsequently, 77.82 g of isophorone diisocyanate (IPDI) and 0.048 g of dibutyltin dilaurate (DBTDL) were added. The reaction was carried out for 2 h under vacuum at 90°C with moderate stirring to obtain an isocyanate-terminated polymer: Measured free NCO content: 3.35%.
[0153] 0.096 g of dibutyltin dilaurate (DBTDL) and 50.76 g of 4-methoxyphenol (HQMME) were added to the resulting NCO-terminated polymer, and the isocyanate groups were removed by reaction under vacuum at 110°C for 5 h. The measured free NCO content was 0.48% (immediately after preparation), 0.23% (one day after preparation).
[0154] Viscosity (1 day after production): 422 Pa*s at 25°C, 82 Pa*s at 50°C. Example 4: Impact modifier SM4 (2-benzoxazolinone [1.2eq.] as blocking agent, PolyTHF 2000 as backbone)
[0155] 400 g of PolyTHF 2000 and 4.50 g of BHT as a stabilizer were dehydrated for 1 h under vacuum at 90°C with minimal stirring. Subsequently, 88.62 g of isophorone diisocyanate (IPDI) and 0.055 g of dibutyltin dilaurate (DBTDL) were added. The reaction was carried out for 2 h under vacuum at 90°C with moderate stirring to obtain an isocyanate-terminated polymer: Measured free NCO content: 3.61%.
[0156] 0.110 g of dibutyltin dilaurate (DBTDL) and 59.64 g of benzoxazolinone were added to the resulting NCO-terminated polymer, and the isocyanate groups were reacted for 3 h under vacuum at 110°C. Measured free NCO content: 0.24%. Example 5: Impact modifier SM5 (3,5-dimethylpyrazole [1.2eq.] as blocking agent, PolyTHF 2000, Poly bd R45V as backbone)
[0157] 225 g of PolyTHF 2000, 225 g of Poly bd R45V, and 2.25 g of BHT as a stabilizer were dehydrated for 1 h under vacuum at 90°C with minimal stirring. Subsequently, 77.82 g of isophorone diisocyanate (IPDI) and 0.058 g of dibutyltin dilaurate (DBTDL) were added. The reaction was carried out for 2 h under vacuum at 90°C with moderate stirring to obtain an isocyanate-terminated polymer: Measured free NCO content: 3.08%.
[0158] 0.116 g of dibutyltin dilaurate (DBTDL) and 38.11 g of 3,5-dimethylpyrazole were added to the resulting NCO-terminated polymer, and the isocyanate groups were removed by reaction under vacuum at 110°C for 2 h. Measured free NCO content: 0.0% Example 6: Impact modifier SM6 (dibutylamine [1.0 eq.] as blocking agent, PolyTHF 2000, Poly bd R45V as backbone)
[0159] 175 g of PolyTHF 2000, 175 g of Poly bd R45V, and 1.75 g of BHT as a stabilizer were dehydrated for 1 h under vacuum at 90°C with minimal stirring. Subsequently, 70.56 g of isophorone diisocyanate (IPDI) and 0.046 g of dibutyltin dilaurate (DBTDL) were added. The reaction was carried out for 2 h under vacuum at 90°C with moderate stirring to obtain an isocyanate-terminated polymer: Measured free NCO content: 2.90%.
[0160] 0.92 g of dibutyltin dilaurate (DBTDL) and 37.52 g of dibutylamine were added to the resulting NCO-terminated polymer, and the isocyanate groups were removed by reaction under vacuum at 70°C for 3 h. Measured free NCO content: 0.0% Example 7: Impact modifier SM7 (MEKO [1.2 eq.] as blocking agent)
[0161] 200 g of PolyTHF 2000, 200 g of Poly BD R45V, and 2.00 g of BHT as a stabilizer were dehydrated for 1 h under vacuum at 90°C with minimal stirring. Subsequently, 80.74 g of isophorone diisocyanate (IPDI) and 0.052 g of dibutyltin dilaurate (DBTDL) were added. The reaction was carried out for 2 h under vacuum at 90°C with moderate stirring to obtain an isocyanate-terminated polymer: Measured free NCO content: 2.91%.
[0162] 0.104 g of dibutyltin dilaurate (DBTDL) and 34.82 g of 2-butane oxime (MEKO) were added to the resulting NCO-terminated polymer, and the isocyanate groups were removed by reaction under vacuum at 110°C for 1 h. Measured free NCO content: 0.00%. Example 8: Impact modifier SM8 (2,2-diallylbisphenol A [1.2 eq.] as blocking agent)
[0163] 290 g of PolyTHF 2000 and 2.90 g of BHT as a stabilizer were dehydrated for 1 h under vacuum at 90°C with minimal stirring. Subsequently, 64.25 g of isophorone diisocyanate (IPDI) and 0.046 g of dibutyltin dilaurate (DBTDL) were added. The reaction was carried out for 2 h under vacuum at 90°C with moderate stirring to obtain an isocyanate-terminated polymer: Measured free NCO content: 3.36%.
[0164] 0.092 g of dibutyltin dilaurate (DBTDL) and 104.76 g of 2,2-diallylbisphenol were added to the resulting NCO-terminated polymer, and the isocyanate groups were reacted for 5 h under vacuum at 110°C. Measured free NCO content after 5 h: 0.74%.
[0165] Measured free NCO content next day at RT: 0.36%. Example 9: Impact modifier SM9 (caprolactam [1.2 eq.] as blocking agent)
[0166] 200 g of PolyTHF 2000, 200 g of Poly bd R45V, and 2.00 g of BHT as a stabilizer were dehydrated for 1 h under vacuum at 90°C with minimal stirring. Subsequently, 80.74 g of isophorone diisocyanate (IPDI) and 0.053 g of dibutyltin dilaurate (DBTDL) were added. The reaction was carried out for 2 h under vacuum at 90°C with moderate stirring to obtain an isocyanate-terminated polymer: Measured free NCO content: 3.026%.
[0167] 0.106 g of dibutyltin dilaurate (DBTDL) and 47.01 g of caprolactam were added to the resulting NCO-terminated polymer, and the isocyanate groups were removed by reaction under vacuum at 110°C for 3 h. Measured free NCO content: 0.00%. Example adhesives 1 to 9
[0168] The impact modifiers SM1 to SM9 prepared in Examples 1 to 9 were each used to prepare epoxy resin compositions according to Table 2.
[0169] Compositions and proportions for epoxy resin compositions containing any of the impact modifiers 1 to 9 are summarized in Table 2. SM-X refers to the impact modifiers SM1, SM2, etc. prepared above. Table 2 parts by weight Chemical composition function 23,0 Epoxy resin based on bisphenol A, liquid Epoxy resin matrix 12,0 Epoxy resin based on bisphenol A, solid Epoxy resin matrix 0,5 p-Tert-butylphenyl glycidyl ether Reactive thinner 50,0 Blocked polyurethane, SM-X Impact modifier 2,43 Dicyandiamide Hardener 0,13 Urone Hardener Accelerator 5,0 CaCO3 filler 6,0 Calcium oxide Moisture catcher 8,0 Fumed silica Thixotropic agents In total: 107,06 Dicy Index: 5.50 mol EP / Dicy
[0170] The respective epoxy resin compositions were mixed in a 350 g batch size in a planetary mixer. The mixing container was filled with the liquid components followed by the solid components, and the mixture was mixed under vacuum at 70°C. During the mixing process (approximately 45 minutes), the vacuum was broken several times and the mixing tool was wiped clean. After obtaining a homogeneous mixture, the epoxy resin composition was filled into cartridges and stored at room temperature.
[0171] Tables 3 and 4 show the results of the evaluation of the obtained epoxy resin compositions with the impact modifiers SM1-9. Table 3: (Positive examples) composition 1 2 3 4 5 6 7 Impact modifier SM1 SM2 SM3 SM4 SM5 SM6 SM7 Blocking agents phenol HQMME HQMME 2-Benzoxazolinone 3.5-Dimethylpyrazole Dibutylamine MEKO Backbone PolyTHF2000 Poly bd R45V PolyTHF2000 Poly bd R45V PolyTHF2000 PolyTHF2000 PolyTHF2000Poly bd R45V PolyTHF2000Poly bd R45V PolyTHF 2000 PolyBD R45V Max. elongation [mm] 2.5 3.2 3.8 4.0 3.1 3.5 3.2 Max. force [N] 3151 1933 2304 3972 1178 2025 2503 Young's modulus [MPa] 336 236 256 433 156 183 264 Tensile strength [MPa] 16,5 12,9 15,0 16,4 5,6 7,9 10,6 Elongation at break [%] 141 108 154 115 40 83 47 LSS [MPa] 17,1 16,1 17,1 14,6 12,1 15,2 15,8 T-peel [N / mm] 14,6 10,5 13,6 11,3 8,1 13,0 11,0 I-Peel [N / mm] 54,2 42,4 62,8 36,5 36,4 53,7 46,0 Viscosity [Pa*s] 25°C 1738 1583 1470 1319 1716 1534 1636 50°C 559 497 559 452 603 530 553 Table 4: (Negative examples) composition 8 9 Impact modifier SM8 SM9 Blocking agents Diallylbisphenol A Caprolactam Backbone PolyTHF2000 PolyTHF 2000 PolyBD R45V Max. elongation [mm] 0.5 0.4 Max. force [N] 166 179 Young's modulus [MPa] 402 299 Tensile strength [MPa] 17,4 16,6 Elongation at break [%] 95 53 LSS [MPa] 17,8 15,3 T-peel [N / mm] 7,6 5,9 I-Peel [N / mm] RT 49,4 31,0 Viscosity [Pa*s] 25° 6387 1652 Viscosity [Pa*s] 50°C 1326 511 Compositions 10-24
[0172] The impact modifiers SM2, SM3, and SM4 were used in different concentrations to produce adhesives according to Table 5. The epoxy resin used, "bisphenol A epoxy resin," is a mixture of 2 parts liquid epoxy resin based on bisphenol A and 1 part solid epoxy resin based on bisphenol A.
[0173] Tables 6-8 show the results of the evaluation of the obtained adhesives 10-25 with the impact modifiers SM2, SM3 and SM4.
[0174] The maximum linear expansion depending on the proportion of impact modifier is given in the Figures 2 to 4 shown. Table 5: Concentration series with SM2, SM3, SM4, *Weight ratio epoxy resin A / toughener SM composition 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 parts by weight Bisphenol A epoxy resin 70 60 55 46 30 10 60 55 46 30 10 60 46 30 10 Impact modifier SM2 10 20 25 34 50 70 -- -- -- -- -- -- -- -- -- Impact modifier SM3 - -- -- -- -- -- 20 25 34 50 70 -- -- -- -- Impact modifier SM4 -- -- -- -- -- -- -- -- -- -- -- 20 34 50 70 Calcium carbonate 7 7 7 7 7 7 7 7 7 7 7 7 7 7 7 Calcium oxide 5 5 5 5 5 5 5 5 5 5 5 5 5 5 5 Fumed silica 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 Dicyandiamide 5.77 4.95 4.54 3.79 2.47 0.82 4.95 4.54 3.79 2.47 0.82 4.95 3.79 2.47 0.82 Urone 0.30 0.26 0.24 0.20 0.13 0.04 0.26 0.24 0.20 0.13 0.04 0.26 0.20 0.13 0.04 A / SM* 7 3 2.2 1.4 0.6 0.2 3 2.2 1.4 0.6 0.2 3 1.4 0.6 0.2 Table 6: Results of compositions 10-15 with SM2 composition 10 11 12 13 14 15 SM2 parts by weight 10% 20% 25% 34% 50% 70% Max. elongation [mm] 1.40 1.70 2.16 2.40 330 5.20 Max. force [N] 3415 4164 4390 4072 3010 265 Young's modulus [MPa] 1860 1560 1320 966 291 2 Tensile strength [MPa] 38.5 34.5 29.8 25.5 15 1.8 Elongation at break [%] 4 8 8 19 121 262 T-peel [N / mm] 2.6 8.9 10.9 11.4 11.3 4.8 I-Peel [N / mm] 23°C 10.4 27.5 40.8 41.6 43.2 22.4 I-Peel [N / mm] -30°C 4.8 26.4 33.5 44.3 51.7 41.3 Table 7: Results of compositions 16-20 with SM3 composition 16 17 18 19 20 SM3 parts by weight 20% 25% 34% 50% 70% Max. elongation [mm] 16 21 23 3.8 Composition not cured Max. force [N] 2439 4459 3537 2303 Young's modulus [MPa] 1430 1340 913 256 Tensile strength [MPa] 29.4 28.3 20.7 15 Elongation at break [%] 6 8 14 154 T-peel [N / mm] 4.9 12.2 12.9 13.6 I-Peel [N / mm] 23°C 34.1 448 52.7 62.8 I-Peel [N / mm] -30°C 10.7 31.6 42.1 61.1 Table 8: Results of compositions 21-24 with SM4 composition 21 22 22 23 24 SM4 parts by weight 20% 25% 34% 50% 70% Max. elongation [mm] 1.6 19 2.2 3.2 Composition not cured Max. force [N] 3261 4047 3974 3971 Young's modulus [MPa] 1200 1190 914 433 Tensile strength [MPa] 25.9 28.4 25.8 16.4 Elongation at break [%] 7 11 21 115 T-peel [N / mm] 2.6 3.4 7.9 11.3 I-Peel [N / mm] 23°C 15.2 30.2 379 36.5 I-Peel [N / mm] -30°C 6.3 30.5 41.6 33.8
Claims
1. Use of at least one toughness improver D for increasing the maximum linear expansion Max. elongation of a one-component thermosetting epoxy resin composition, wherein the one-component thermosetting epoxy resin composition comprises: a) at least one epoxy resin A having an average of more than one epoxy group per molecule; b) at least one latent curing agent for epoxy resins B; where the weight ratio of the at least one epoxy resin A having an average of more than one epoxy group per molecule to the at least one toughness improver D is 0.3-2.2, and wherein the toughness improver D is a terminally blocked polyurethane prepolymer of the formula (I): where R1 is a p-valent radical of a linear or branched polyurethane prepolymer terminated by isocyanate groups after the removal of the terminal isocyanate groups; p has a value of 2 to 8; and R2 is a blocking group which is detached at a temperature above 100°C, where R2 is not a substituent selected from the group consisting of where R12 is an alkylene group which has 2 to 5 carbon atoms and optionally has double bonds or is substituted, or is a phenylene group or a hydrogenated phenylene group, especially ε-caprolactam after removal of the NH proton; and R19 represents bisphenols, after removal of a hydroxyl group, especially bisphenol A, bisphenol F and 2,2'-diallylbisphenol A, and wherein the maximum linear expansion Max. elongation is determined in a lap shear test during the cooling of a heated cured lap shear specimen, and wherein the maximum linear expansion Max. elongation is ≥ 2.145 mm, preferably ≥ 2.2 mm, preferably ≥ 2.5 mm, preferably ≥ 2.8 mm, preferably ≥ 3.0 mm, preferably ≥ 3.5 mm, preferably ≥ 4.0 mm, where the exact test method is defined in the description.
2. Use according to Claim 1, wherein R2 is independently a substituent selected from the group consisting of where R5, R6, R7 and R8 are each independently an alkyl or cycloalkyl or aralkyl or arylalkyl group or R5 together with R6, or R7 together with R8, form part of a 4- to 7-membered, optionally substituted ring; R9, R9' and R10 are each independently an alkyl or aralkyl or arylalkyl group or an alkyloxy or aryloxy or aralkyloxy group; R11 is an alkyl group, R13 and R14 are each independently an alkylene group which has 2 to 5 carbon atoms and optionally has double bonds or is substituted, or a phenylene group or a hydrogenated phenylene group; R15, R16 and R17 are each independently H or an alkyl group or an aryl group or an aralkyl group; and R18 is an aralkyl group or is a mono- or polycyclic, substituted or unsubstituted aromatic group optionally having aromatic hydroxyl groups; R4 is a radical of an aliphatic, cycloaliphatic, aromatic or araliphatic epoxide containing a primary or secondary hydroxyl group after the removal of the hydroxyl and epoxy groups; and m has a value of 1, 2 or 3.
3. Use according to Claim 1 or 2, wherein R2 is independently a substituent selected from the group consisting of and ---O-R18, where R5, R6, R7 and R8 are each independently an alkyl or cycloalkyl or aralkyl or arylalkyl group or R5 together with R6, or R7 together with R8, form part of a 4- to 7-membered, optionally substituted ring; R15, R16 and R17 are each independently H or an alkyl group or an aryl group or an aralkyl group; and R18 is an aralkyl group or is a mono- or polycyclic, substituted or unsubstituted aromatic group optionally having aromatic hydroxyl groups; R2 is preferably selected from the group consisting of and ---O-R18, R2 is especially selected from the group consisting of and ---O-R18, R2 is more preferably selected from the group consisting of and ---O-R18 R2 is most preferably ---O-R18.
4. Use according to any of the preceding claims, wherein the weight ratio of the at least one epoxy resin A having an average of more than one epoxy group per molecule to the at least one toughness improver D is 0.4-2.0, more preferably 0.5-1.8.
5. Use according to any of the preceding claims, wherein R1 is a p-valent radical of a linear or branched polyurethane prepolymer terminated by isocyanate groups after the removal of the terminal isocyanate groups, and the polyurethane prepolymer is prepared from at least one diisocyanate or triisocyanate and from a polymer QPM having terminal amino, thiol or hydroxyl groups.
6. Use according to Claim 5, wherein the polymer QPM having terminal amino, thiol or hydroxyl groups comprises polyols having average molecular weights between 600 and 6000 daltons, selected from the group consisting of polyethylene glycols, polypropylene glycols, polyethylene glycol-polypropylene glycol block polymers, polybutylene glycols, polytetramethylene ether glycols, hydroxyl-terminated polybutadienes, hydroxyl-terminated butadiene-acrylonitrile copolymers and mixtures thereof, especially preferably polytetramethylene ether glycols and hydroxyl-terminated polybutadienes.
7. Use according to Claim 6, wherein the polymer QPM having terminal amino, thiol or hydroxyl groups comprises polyols having average molecular weights between 600 and 6000 daltons, selected from the group consisting of polytetramethylene ether glycols and hydroxyl-terminated polybutadienes, wherein the weight ratio of polytetramethylene ether glycol to hydroxyl-terminated polybutadiene is in the range from 100 / 0 to 70 / 30, more preferably from 100 / 0 to 60 / 40, more preferably from 100 / 0 to 90 / 10 and most preferably 100 / 0.
8. Use according to any of the preceding claims, wherein the maximum linear expansion Max. elongation is measured in a lap shear test at a strain rate Vst of 0.52 mm / min.
9. Use according to any of the preceding claims, wherein the temperature of the lap shear specimen in the lap shear test is 190°C at the start of the measurement and the lap shear specimen is cooled at the start of the measurement at a cooling rate of 40°C / min to a temperature of 25°C and then left at that temperature.
10. Use according to any of the preceding claims, wherein the lap shear test is a lap shear test having lap shear test specimens having the following features: - steel sheets having the dimensions of 25 mm x 100 mm x 1.5 mm, - bonding area of the cured one-component thermosetting epoxy resin composition having the dimensions of 10 mm x 25 mm with a thickness of 1.5 mm, preferably 1.0 mm.
11. Use according to any of the preceding claims, wherein the maximum force measured is ≤ 6000 N, preferably ≤ 5000 N, preferably ≤ 4500 N, preferably ≤ 4000 N, preferably ≤ 3500 N, preferably ≤ 3000 N, preferably ≤ 2500 N, preferably ≤ 2000 N.
12. Use according to any of the preceding claims, wherein the force measured on attainment of the maximum linear expansion Max. elongation of 2.145 mm is ≤ 4000 N, preferably ≤ 3000 N, preferably ≤ 2500 N, preferably ≤ 2000 N, preferably ≤ 1500 N, preferably ≤ 1000 N, preferably ≤ 800 N, preferably ≤ 700 N.
13. Use according to any of the preceding claims, wherein the latent curing agent for epoxy resins B is selected from the group consisting of dicyandiamide, guanidines, anhydrides of polybasic carboxylic acids, dihydrazides and aminoguanidines, preference being given to dicyandiamide.
14. Use according to any of the preceding claims, wherein the one-component thermosetting epoxy resin composition is a thermosetting epoxy resin adhesive, especially for motor vehicle construction and sandwich panel construction.