Glass fiber reinforced TPU
Patent Information
- Application Number
- DE502019012109
- Authority / Receiving Office
- DE · DE
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2018-07-12
- Filing Date
- 2019-07-11
- Publication Date
- 2024-10-02
- Estimated Expiration
- 2039-07-11
AI Technical Summary
Producing thermoplastic polyurethanes with high rigidity and excellent mechanical and low-temperature properties while being easy to process is challenging, especially in achieving elastic moduli greater than 10,000 MPa, due to the difficulty in obtaining stiff starting materials and achieving high glass fiber filling levels.
A composition containing a thermoplastic polyurethane (TPU-1) obtained by reacting a polyisocyanate composition with a polyol composition that includes specific chain extenders in a molar mixing ratio and a fibrous filler, optimizing the melting range and mechanical properties to produce glass fiber reinforced TPUs with elastic moduli above 10,000 MPa.
The solution enables the production of thermoplastic polyurethanes with improved property profiles, including high rigidity, good mechanical properties, and low-temperature performance, while being easy to process, by optimizing the polyol composition and using a fibrous filler, resulting in successful production of glass fiber reinforced TPUs with desired elastic moduli.
Description
[0001] The present invention relates to a composition comprising a thermoplastic polyurethane (TPU-1) obtained or produced by reacting a polyisocyanate composition (IZ) with a polyol composition (PZ), wherein the polyol composition (PZ) comprises at least one polyol (P1), a chain extender (KV1), and a chain extender (KV2); and a filler (F1), as well as a process for producing such compositions. The present invention further relates to the use of a composition according to the invention for producing a molded body, and to a molded body containing a composition according to the invention.
[0002] Filler-containing thermoplastic polyurethanes are disclosed, for example, in US 2016 / 264710A1, CN 104 212 159 A, WO 2017 / 195934A1, CN 106 366 286 A, WO 2007 / 118827 A1 or WO 2015 / 197515 A1.
[0003] Glass fiber reinforced thermoplastic polyurethanes are well-known. They are high-performance materials that combine excellent mechanical properties with very low coefficients of thermal expansion. These materials are highly resilient and are used in a wide variety of applications.
[0004] High-quality glass fiber reinforced thermoplastic polyurethanes can be manufactured, for example, from MDI-based thermoplastic polyurethanes. The MDI-based hard phase results in very good mechanical properties.
[0005] Also of interest are polyether-based, glass-fiber-reinforced TPUs, which exhibit very high impact strength, especially at low temperatures. These materials are used in sporting goods such as ski boots and skis for various functional components.
[0006] However, some applications require very stiff materials with Young's moduli greater than 10,000 MPa. Suitable materials are very difficult to produce, as they require both very stiff TPU starting materials and very high glass fiber filler levels.
[0007] One of the objectives of the present invention was therefore to provide reinforced thermoplastic polyurethanes that exhibit high stiffness. Furthermore, the thermoplastic polyurethanes should possess good mechanical properties, good low-temperature properties, and be easy to process.
[0008] According to the invention, this problem is solved by a composition containing (a) a thermoplastic polyurethane (TPU-1) obtained or obtainable by reacting a polyisocyanate composition (IZ) with a polyol composition (PZ), wherein the polyol composition (PZ) comprises at least one polyol (P1), a chain extender (KV1) and a chain extender (KV2), the chain extenders being used in a molar mixing ratio KV1:KV2 in the range of 20:1 to 3:1; and (b) a filler (F1), wherein the filler (F1) is fibrous.
[0009] Surprisingly, it was found that the combination of the thermoplastic polyurethane and the filler according to the invention yields compositions with an improved property profile. For example, the melting range of the very stiff TPU can be optimized by using the specific polyol composition according to the invention. Furthermore, it was found that the addition of a second chain extender during the synthesis of the very stiff TPU yields starting materials with which glass fiber-reinforced TPU with Young's moduli above 10,000 MPa can be produced.
[0010] The composition according to the invention comprises at least one filler (F1) and a thermoplastic polyurethane (TPU-1). The thermoplastic polyurethane (TPU-1) is obtained or produced within the scope of the present invention by reacting a polyisocyanate composition (IZ) with a polyol composition (PZ), wherein the polyol composition (PZ) comprises at least one polyol (P1), a chain extender (KV1) and a chain extender (KV2).
[0011] Thermoplastic polyurethanes are generally well-known. They are typically produced by reacting isocyanates, isocyanate-reactive compounds, and chain extenders, optionally in the presence of at least one catalyst and / or common auxiliary substances and / or additives. Isocyanates, isocyanate-reactive compounds, and chain extenders are also referred to individually or together as structural components.
[0012] According to the invention, the thermoplastic polyurethane (TPU-1) is obtainable by reacting a polyisocyanate composition (IZ) with a polyol composition (PZ). The polyol composition (PZ) contains at least one polyol (P1), a chain extender (KV1), and a chain extender (KV2). Within the scope of the present invention, the polyol composition may also contain further polyols.
[0013] Chain-extending agents (KV1) and (KV2) can be generally known aliphatic, araliphatic, aromatic, and / or cycloaliphatic compounds with a molecular weight, preferably an average molecular weight, of 50 g / mol to 499 g / mol, preferably di-functional compounds. Alkanediols with 2 to 10 carbon atoms in the alkylene residue are preferred, for example, 1,4-butanediol, 1,6-hexanediol, and / or di-, tri-, tetra-, penta-, hexa-, hepta-, octa-, nona-, and / or decaalkylene glycols with 3 to 8 carbon atoms; unbranched alkanediols, in particular 1,3-propanediol, 1,4-butanediol, and 1,6-hexanediol, are further preferred.
[0014] According to a further embodiment, the present invention also relates to a composition as described above, wherein the chain extender (KV1) and / or the chain extender (KV2) is selected from the group consisting of 1,2-ethanediol, 1,3-propanediol, 1,4-butanediol and 1,6-hexanediol, diethylene glycol, triethylene glycol, hydroquinone bis-2-hydroxyethyl ether and bis-2(hydroxy ethyl) terephthalate.
[0015] The chain extender (KV1) is, within the scope of the present invention, preferably selected from the group consisting of 1,2-ethanediol, 1,3-propanediol, 1,4-butanediol, and 1,6-hexanediol. According to a further embodiment, the present invention also relates to a composition as described above, wherein the chain extender (KV1) is 1,4-butanediol.
[0016] In the context of the present invention, 1,3-propanediol or 1,6-hexanediol is preferably used as the chain extender (KV2), and more preferably 1,3-propanediol is used as the chain extender (KV2). According to a further embodiment, the present invention therefore relates to a thermoplastic polyurethane as described above, wherein the chain extender (KV2) is 1,3-propanediol.
[0017] According to the invention, it is also possible to use a polyhydric alcohol, for example propanediol and / or another diol, which is at least partially derived from renewable raw materials. It is possible that the polyhydric alcohol is obtained partially or completely from renewable raw materials. According to the invention, at least one of the polyhydric alcohols used can be obtained at least partially from renewable raw materials.
[0018] So-called bio-1,3-propanediol can be obtained, for example, from corn and / or sugar. Another possibility is the conversion of glycerin waste from biodiesel production. According to a further preferred embodiment of the invention, the polyhydric alcohol is 1,3-propanediol, which is obtained at least partially from renewable raw materials.
[0019] According to a further embodiment, the present invention relates to a composition as described above, wherein the thermoplastic polyurethane is based on renewable raw materials to at least 30%. A suitable determination method is, for example, the C14 method.
[0020] According to the invention, further chain extenders can also be used in the polyol composition.
[0021] According to the invention, the polyol composition (PZ) contains at least the polyol (P1) as a compound reactive towards isocyanates. Within the scope of the present invention, in principle all suitable polyols can be used, for example, polyester ols, polyether ols, and / or polycarbonate diols. For example, the polyol used can have a molecular weight (Mn) in the range of 500 g / mol to 8000 g / mol and preferably an average functionality towards isocyanates of 1.8 to 2.3, more preferably 1.9 to 2.2, and particularly 2. The number-average molecular weight is determined according to DIN 55672-1 unless otherwise specified.
[0022] Preferably, the polyol (P1) used has a molecular weight in the range of 600 to 2000 Daltons, more preferably a molecular weight in the range of 750 to 1500 Daltons, and in particular a molecular weight of about 1000 Daltons.
[0023] Polyesterols can be polyesters based on diacids and diols. Diols with 2 to 10 carbon atoms are preferred, for example, ethanediol, butanediol, or hexanediol, especially 1,4-butanediol, or mixtures thereof. All known diacids can be used as diacids, for example, linear or branched-chain diacids with four to 12 carbon atoms, or mixtures thereof.
[0024] Furthermore, polyether polyols can be used within the scope of the present invention, for example those based on generally known starter substances and conventional alkylene oxides, preferably ethylene oxide, propylene oxide and / or butylene oxide, more preferably polyether ols based on propylene oxide-1,2 and ethylene oxide, and in particular polyoxytetramethylene glycols. The advantage of the polyether polyols lies, among other things, in their higher hydrolysis stability.
[0025] Low-unsaturated polyetherols are also suitable. Within the scope of this invention, low-unsaturated polyols are understood to be, in particular, polyether alcohols with an unsaturated compound content of less than 0.02 meq / g, preferably less than 0.01 meq / g. Such polyether alcohols are mostly produced by the addition of alkylene oxides, in particular ethylene oxide, propylene oxide, and mixtures thereof, to the diols or triols described above in the presence of highly active catalysts.
[0026] Such highly active catalysts are preferably cesium hydroxide and multimetal cyanide catalysts, also known as DMC catalysts. Zinc hexacyanocobaltate is a frequently and preferred DMC catalyst. The DMC catalyst can remain in the polyether alcohol after the reaction, but it is usually removed, for example by sedimentation or filtration.
[0027] Furthermore, polytetrahydrofurans can be used within the scope of the present invention, for example with an average molecular weight Mn in the range of 400 to 1800 g / mol, preferably from polytetrahydrofurans with an average molecular weight Mn in the range of 600 to 1500 g / mol, more preferably from polytetrahydrofurans with an average molecular weight Mn in the range of 750 to 1250 g / mol, for example in the range of 900 to 1100 g / mol.
[0028] It has been found that, particularly when using polyols with an average molecular weight in the range of 900 to 1100 g / mol, compositions are obtained that exhibit a particularly advantageous property profile. For example, the compositions according to the invention exhibit, on the one hand, a low melting point and, on the other hand, good low-temperature properties.
[0029] However, in the context of the present invention, the polyol composition can also include, in addition to the polyol (P1) and the chain extenders (KV1) and (KV2), other compounds reactive towards isocyanates. For example, the polyol composition can include further polyols with an average molecular weight Mn in the range of 800 to 1200 g / mol.
[0030] Suitable polycarbonate diols are, for example, polycarbonate diols based on alkane diols. Suitable polycarbonate diols are strictly difunctional OH-functional polycarbonate diols, preferably strictly difunctional OH-functional aliphatic polycarbonate diols. Suitable polycarbonate diols are based, for example, on 1,4-butanediol, 1,5-pentanediol, or 1,6-hexanediol, in particular 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 3-methylpentane-(1,5)-diol, or mixtures thereof, especially preferably 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, or mixtures thereof. Preferably, within the scope of the present invention, polycarbonate diols based on 1,4-butanediol and 1,6-hexanediol, polycarbonate diols based on 1,5-pentanediol and 1,6-hexanediol, polycarbonate diols based on 1,6-hexanediol, and mixtures of two or more of these polycarbonate diols are used. Suitable polycarbonate diols have, for example, an average molecular weight Mn in the range of 800 to 1200 g / mol.
[0031] It has been found that the use of polycarbonate diols yields compositions suitable for applications requiring good hydrolysis resistance and good aging resistance. Thus, when polycarbonate diols are used as polyols, the compositions according to the invention exhibit not only good low-temperature properties but also high hydrolysis resistance and good aging resistance.
[0032] Preferably, a polyetherol is used as the polyol (P1) in the present invention.
[0033] According to a further embodiment, the present invention also relates to a composition as described above, wherein the polyol (P1) is a polyether polyol.
[0034] In the present invention, the isocyanate composition (IZ) is used in the production of the thermoplastic polyurethane (TPU-1). The isocyanate composition contains at least one polyisocyanate, preferably at least one diisocyanate.
[0035] In principle, the commonly used organic isocyanates are suitable within the scope of the present invention. The organic isocyanates that can be used include aliphatic, cycloaliphatic, araliphatic and / or aromatic isocyanates, preferably tri-, tetra-, penta-, hexa-, hepta- and / or octamethylene diisocyanate, 2-methylpentamethylene diisocyanate-1,5, 2-ethylbutylene diisocyanate-1,4, pentamethylene diisocyanate-1,5, butylene diisocyanate-1,4, 1-isocyanato-3,3,5-trimethyl-5-isocyanatomethyl cyclohexane (isophorone diisocyanate, IPDI), 1,4- and / or 1,3-bis(isocyanatomethyl)cyclohexane (HXDI), 1,4-cyclohexane diisocyanate, 1-methyl-2,4- and / or -2,6-cyclohexane diisocyanate and / or 4,4'-, 2,4'- and 2,2'-Dicyclohexylmethane diisocyanate, 2,2`-, 2,4'- and / or 4,4'-Diphenylmethane diisocyanate (MDI), 1,5-Naphthylene diisocyanate (NDI), 2,4- and / or 2,6-Toluene diisocyanate (TDI), 3,3`-Dimethyl diphenyl diisocyanate, 1,2-Diphenylethane diisocyanate and / or Phenylene diisocyanate.Only 4.4'-MDI is preferred.
[0036] According to a further embodiment, the present invention therefore relates to a composition as described above, wherein the thermoplastic polyurethane is based on 4,4'-diphenylmethane diisocyanate.
[0037] Other suitable aliphatic isocyanates include, for example, hexamethylene diisocyanate (HDI) or 1-isocyanato-4-[(4-isocyanatocyclohexyl) methyl]cyclohexane (H12MDI).
[0038] Particularly preferred isocyanates according to the invention are hexamethylene diisocyanate (HDI), 2,2`-, 2,4'- and / or 4,4`-diphenylmethane diisocyanate (MDI) and 2,4- and / or 2,6-toluene diisocyanate (TDI), or 1-isocyanato-4-[(4-isocyanatocyclohexyl) methyl]cyclohexane (H12MDI), wherein 2,2`-, 2,4'- and / or 4,4`-diphenylmethane diisocyanate (MDI) is particularly preferred, especially 4,4`-diphenylmethane diisocyanate.
[0039] According to a further embodiment, the present invention also relates to a composition as described above, wherein the polyisocyanate composition (IZ) comprises a polyisocyanate (PI) selected from the group consisting of 1,2-, 1,3-, and / or 1,4-phenylene diisocyanate, triphenylmethane 4,4',4"-triisocyanate, naphthylene 1,5-diisocyanate (NDI), 2,4- and / or 2,6-toluene diisocyanate (TDI), 2,4'-, 4,4'- and / or 2,2-diphenyl diisocyanate, 2,2'-, 2,4'- and / or 4,4'-diphenylmethane diisocyanate (MDI), polyphenylpolymethylene polyisocyanate, 1,2-, 1,3- and / or 1,4-xylylene diisocyanate and m-tetramethylxylene diisocyanate (TMXDI).
[0040] In addition to the isocyanate composition (IZ) and the polyol composition (PZ), other components can be used to produce thermoplastic polyurethane (TPU1), such as suitable catalysts or auxiliaries.
[0041] Catalysts that accelerate, in particular, the reaction between the NCO groups of the diisocyanates and the hydroxyl groups of the compound reactive towards isocyanates and the chain-extending agent are, in a preferred embodiment, tertiary amines, in particular triethylamine, dimethylcyclohexylamine, N-methylmorpholine, N,N'-dimethylpiperazine, 2-(dimethylaminoethoxy)ethanol, diazabicyclo-(2,2,2)octane; in another preferred embodiment, these are organic metal compounds, such as titanium dioxide esters, iron compounds, preferably iron(III) acetylacetonate, tin compounds, preferably tin diacetate, tin dioctoate, tin dilaurate or the tin dialkyl salts of aliphatic carboxylic acids, preferably dibutyltin diacetate, dibutyltin dilaurate or bismuth salts in which bismuth is preferably present in oxidation states 2 or 3, in particular 3. Salts of carboxylic acids are preferred.Carboxylic acids with 6 to 14 carbon atoms, and especially those with 8 to 12 carbon atoms, are preferably used. Examples of suitable bismuth salts are bismuth(III) neodecanoate, bismuth 2-ethylhexanoate, and bismuth octanoate.
[0042] The catalysts are preferably used in amounts of 0.0001 to 0.1 parts by weight per 100 parts by weight of the compound reactive with isocyanates. Tin catalysts, especially tin dioctoate, are preferred.
[0043] In addition to catalysts, common additives can also be added. These include, for example, surfactants, fillers, further flame retardants, nucleating agents, oxidation stabilizers, sliding and demolding aids, dyes and pigments, possibly stabilizers (e.g., against hydrolysis, light, heat, or discoloration), inorganic and / or organic fillers, reinforcing agents, and plasticizers. Suitable additives and additives can be found, for example, in the Plastics Handbook, Volume VII, edited by Vieweg and Höchtlen, Carl Hanser Verlag, Munich 1966 (pp. 103–113).
[0044] Suitable manufacturing processes for thermoplastic polyurethanes are disclosed, for example, in EP 0 922 552 A1, DE 101 03 424 A1, or WO 2006 / 072461 A1. Production is usually carried out on a conveyor belt or a reaction extruder, but can also be performed on a laboratory scale, for example, by hand molding. Depending on the material properties of the components, these are either all mixed together directly or individual components are premixed and / or pre-reacted, e.g., to form prepolymers, and then polyadditionally added. In a further embodiment, a thermoplastic polyurethane is first produced from the structural components, optionally with a catalyst, into which auxiliary materials may also be incorporated. At least one filler is then introduced into this material and homogeneously distributed. This homogeneous distribution preferably takes place in an extruder, preferably a twin-screw extruder.According to the invention, it is preferred to add the filler in portions, for example, a portion at the extruder feed and another portion at a second dosing point, for example, a side pusher. To adjust the hardness of the TPU, the amounts of the build-up components (b) and (c) used can be varied over relatively wide molar ratios, with the hardness typically increasing with increasing content of chain extender.
[0045] According to the invention, the mixing ratio of the components used to produce the thermoplastic polyurethane can vary over a wide range. For example, the chain extenders and the polyol used can be employed in a molar mixing ratio in the range of 20:1 to 1:1, preferably in the range of 18:1 to 2:1, more preferably in the range of 17:1 to 3:1, and particularly preferably in the range of 15:1 to 4:1.
[0046] According to the invention, the chain extenders are used in a molar mixing ratio KV1:KV2 in the range of 20:1 to 3:1, preferably in the range of 15:1 to 4:1, more preferably in the range of 17:1 to 3:1, and particularly preferably in the range of 15:1 to 4:1.
[0047] The thermoplastic polyurethane used according to the invention preferably has a hardness in the range of 40D to 90D, determined according to DIN ISO 7619-1 (Shore hardness test A (3s)), preferably in the range of 50D to 90D, determined according to DIN ISO 7619-1, more preferably in the range of 60D to 90D, determined according to DIN ISO 7619-1, particularly preferably in the range of 70D to 90D, determined according to DIN ISO 7619-1.
[0048] According to a further embodiment, the present invention also relates to a composition as described above, wherein the thermoplastic polyurethane has a Shore hardness in the range of 40D to 90D, determined according to DIN ISO 7619-1.
[0049] To produce the thermoplastic polyurethanes according to the invention, the structural components are preferably reacted in the presence of catalysts and optionally auxiliaries and / or additives in such quantities that the equivalence ratio of NCO groups of the diisocyanates to the sum of the hydroxyl groups of the further structural components is 0.9 to 1.1 : 1, preferably 0.95 to 1.05 : 1 and in particular approximately 0.95 to 1.00 : 1.
[0050] The composition according to the invention contains the at least one thermoplastic polyurethane (TPU1) in an amount in the range of 40 wt.% to 60 wt.%, based on the total composition, in particular in the range of 45 wt.% to 55 wt.%, based on the total composition, preferably in the range of 48 wt.% to 52 wt.%, in each case based on the total composition.
[0051] According to a further embodiment, the present invention therefore relates to a composition as described above, wherein the proportion of thermoplastic polyurethane in the composition is in the range of 40 wt.% to 60 wt.%, based on the total composition.
[0052] The sum of all components of the composition each equals 100% by weight.
[0053] Preferably, thermoplastic polyurethanes are used according to the invention, in which the thermoplastic polyurethane has a mean molecular weight (MW) in the range of 50,000 to 500,000 Da. The upper limit for the mean molecular weight (MW) of the thermoplastic polyurethanes is generally determined by processability as well as the desired property spectrum. More preferably, the thermoplastic polyurethane has a mean molecular weight (MW) in the range of 50,000 to 250,000 Da, and particularly preferably in the range of 50,000 to 150,000 Da.
[0054] According to the invention, it is also possible that the composition contains two or more thermoplastic polyurethanes which differ, for example, in their average molecular weight or in their chemical composition.
[0055] The production of thermoplastic polyurethane can be carried out discontinuously or continuously using known methods, for example, with reaction extruders or the one-shot belt process. In these processes, the reacting components can be mixed sequentially or simultaneously, with the reaction starting immediately. In the extrusion process, the components are introduced into the extruder individually or as a mixture, preferably at temperatures of 100 °C to 280 °C, and more preferably at 140 °C to 250 °C. The resulting polyurethane is then extruded, cooled, and granulated.
[0056] The composition according to the invention further comprises a fibrous filler (F1). According to the invention, the chemical nature and shape of the filler (F1) can vary widely, as long as sufficient compatibility with the thermoplastic polyurethane (TPU-1) is ensured. The filler (F1) should be selected such that its shape and particle size allow for sufficient miscibility and uniform distribution within the composition.
[0057] Suitable fillers include, for example, glass fibers, carbon fibers, aramid fibers, potassium titanate fibers, fibers made of liquid-crystalline polymers, organic fibrous fillers, or inorganic reinforcing materials. Examples of organic fibrous fillers are cellulose fibers, hemp fibers, sisal, or kenaf. Examples of inorganic reinforcing materials are ceramic fillers, such as aluminum and boron nitride, or mineral fillers, such as asbestos, talc, wollastonite, microvit, silicates, chalk, calcined kaolin, mica, and quartz flour. According to the invention, the filler (F1) is preferably selected from the group consisting of glass fibers, carbon fibers, aramid fibers, potassium titanate fibers, fibers made of liquid-crystalline polymers, metal fibers, polyester fibers, polyamide fibers, organic fibrous fillers, and inorganic fibrous fillers.
[0058] According to a further embodiment, the present invention also relates to a composition as described above, wherein the filler (F1) is selected from the group consisting of glass fibers, carbon fibers, aramid fibers, potassium titanate fibers, fibers made of liquid crystalline polymers, metal fibers, polyester fibers, polyamide fibers, organic fibrous fillers and inorganic fibrous fillers.
[0059] The dimensions of the fillers used can vary within typical ranges. Preferably, the filler used has a length in the range of 3 mm to 4 mm and a diameter in the range of 1 µm to 20 µm, each determined according to ASTM D578-98. According to a further embodiment, the present invention also relates to a composition as described above, wherein the filler (F1) has a length in the range of 3 mm to 4 mm and a diameter in the range of 1 µm to 20 µm, each determined according to ASTM D578-98.
[0060] The fibrous fillers can be pretreated to improve compatibility with the thermoplastic material, for example with a silane compound.
[0061] Inorganic fibrous fillers are preferred. Using inorganic fibrous fillers results in a greater reinforcing effect and higher heat resistance.
[0062] According to the invention, the composition can also contain two or more fillers.
[0063] The proportion of the filler (F1) in the composition is, for example, in the range of 40 to 60 wt.% based on the total composition, preferably in the range of 45 to 55 wt.% based on the total composition, more preferably in the range of 48 to 52 wt.% based on the total composition.
[0064] According to a further embodiment, the present invention also relates to a composition as described above, wherein the filler (F1) is contained in an amount in the range of 40 to 60 wt.% based on the total composition.
[0065] According to the invention, the composition can contain, in addition to the thermoplastic polyurethane (TPU1) and the filler (F1), other components, such as demolding aids, UV protection, antioxidant or color pigments.
[0066] According to another aspect, the present invention also relates to a method for producing a composition comprising the step (i) Mixing the components (a) obtaining or obtaining a thermoplastic polyurethane (TPU-1) by reacting a polyisocyanate composition (IZ) with a polyol composition (PZ), wherein the polyol composition (PZ) comprises at least one polyol (P1), a chain extender (KV1) and a chain extender (KV2), the chain extenders being used in a molar mixing ratio KV1:KV2 in the range of 20:1 to 3:1; and (b) a filler (F1), wherein the filler (F1) is fibrous.
[0067] Regarding the preferred embodiments, reference is made to the above statements concerning the components preferably used.
[0068] Suitable methods for preparing the composition are known to those skilled in the art. Within the scope of the present invention, methods known per se are used for the compounding process.
[0069] For example, the composition can be produced in a known manner in an extruder, such as a twin-screw extruder. According to the invention, it is preferred to add the filler in portions, for example, a portion at the extruder feed and another portion at a second dosing point, such as a side pusher. The temperature is preferably in the range of 160 to 230°C. Within the scope of the present invention, the extruder can, for example, be operated at a speed in the range of 150 to 300 revolutions per minute.
[0070] The present invention further relates to a composition obtained or obtainable by a method according to the invention.
[0071] The present invention also relates to the use of the composition according to the invention or of a composition obtained or obtainable by a method according to the invention for the production of a molded body.
[0072] The product is preferably manufactured from granules by injection molding, calendering, powder sintering, or extrusion and / or by additional foaming of the composition according to the invention.
[0073] Furthermore, according to another aspect, the present invention also relates to molded bodies containing a composition according to the invention or a composition obtained or obtainable according to a method according to the invention.
[0074] The present invention also relates to the use of the composition according to the invention as described above for the production of molded bodies, for example parts of a shoe or parts of ski boots.
[0075] Further embodiments of the present invention can be found in the claims and examples. It is understood that the features of the subject matter / method or uses of the invention mentioned above and those explained below can be used not only in the combinations specified, but also in other combinations without departing from the scope of the invention. For example, the combination of a preferred feature with a particularly preferred feature, or of an uncharacterized feature with a particularly preferred feature, is implicitly included, even if this combination is not expressly mentioned.
[0076] The following examples serve to illustrate the invention, but are in no way limiting with regard to the subject matter of the present invention. Examples: 1. Materials used
[0077] Chopvantage HP3550 EC10-3.8: Fiberglass from PPG Industries Fiber Glass, Energieweg 3, 9608 PC Westerbroek, The Netherlands. E-glass, filament diameter 10µm, length 3.8mm.
[0078] TPU 1: TPU with Shore hardness 60D, based on polytetrahydrofuran (PTHF) with a molecular weight (Mn) of 1000 Dalton, 1,4-butanediol, MDI.
[0079] TPU 2: TPU with a Shore hardness of 83D, based on polytetrahydrofuran (PTHF) with a molecular weight (Mn) of 1000 Dalton, 1,4-butanediol, MDI.
[0080] TPU 3: TPU with a Shore hardness of 83D, based on polytetrahydrofuran (PTHF) with a molecular weight (Mn) of 1000 Dalton, 1,4-butanediol, 1,3-propanediol, MDI.
[0081] TPU 4: Glass fiber filled TPU of Shore hardness 70D produced by compounding 48% of the glass fiber Chopvantage HP3550 EC10-3.8 into TPU 1.
[0082] TPU 5: Glass fiber filled TPU of Shore hardness 75D produced by compounding 48% of the glass fiber Chopvantage HP3550 EC10-3.8 into TPU 2 (not producible, see Table 4).
[0083] TPU 6: Glass fiber filled TPU of Shore hardness 75D produced by compounding 48% of the glass fiber Chopvantage HP3550 EC10-3.8 into TPU 3. 2. Manufacturing examples 2.1 Manufacturing by hand casting process (TPU 1-3)
[0084] The quantity of polyol and chain extender specified in the underlying formula (Table 1) is weighed into the tin can and briefly covered with nitrogen. The can is then sealed with a lid and heated to approximately 90°C in a heating cabinet.
[0085] Another heating cabinet for tempering the rind is preheated to 80 °C. The Teflon tray is placed on the heating table, which is then set to 125 °C.
[0086] The calculated quantity of liquid isocyanate is determined by volumetric measurement. For this, the liquid isocyanate (MDI is measured at a temperature of approximately 48 °C) is weighed into a PE beaker and poured into another PE beaker within 10 seconds. The emptied beaker is then tared and filled with the calculated quantity of isocyanate. In the case of MDI, this is stored in a heating cabinet at approximately 48 °C.
[0087] Additives such as hydrolysis protection and antioxidants, which are present as solids at room temperature, are weighed in directly.
[0088] The preheated polyol is placed on a lifting platform under the stationary stirrer. The reaction vessel is then raised using the lifting platform until the stirring blades are completely immersed in the polyol.
[0089] Before switching on the mixing motor, ensure that the speed control is in the zero position. Then slowly increase the speed to ensure thorough mixing without incorporating air.
[0090] Then, additives such as antioxidants are added to the polyol.
[0091] The temperature of the reaction mixture is carefully adjusted to 80°C using a hot air gun.
[0092] If necessary, catalyst is dosed into the reaction mixture using a microliter syringe before the isocyanate is added. At 80 °C, the isocyanate is added by injecting the previously measured amount into the reaction mixture within 10 seconds. The weight is checked by weighing. Deviations greater or less than 0.2 g from the recipe quantity are documented. The stopwatch is started when the isocyanate is added. When the temperature reaches 110 °C, the reaction mixture is poured into the Teflon dishes, which have been preheated to 125 °C.
[0093] Ten minutes after the stopwatch starts, the rind is removed from the heating table and then stored in a heating cabinet at 80°C for 15 hours. The cooled rind is then shredded in a cutting mill. The granules are then dried at 110°C for 3 hours and stored in a dry place.
[0094] In principle, this process can be transferred to the reaction extruder or the belt process. Table 1: Formulations of TPU 1-3 TPU 1 TPU 2 TPU 3 PTHF 1000 [g] 393,2 100 100 Lupranat MET [g] 471,8 395,5 395,5 Butanediol-1.4 [g] 135,0 133,4 121,7 Propanediol - 1.3 [g] - - 9.8 Table 2: Properties of TPU 1-3 TPU 1 TPU 2 TPU 3 Tensile strength [MPa] DIN 53504-S2 50 70 67 Elongation at break [%] DIN 53504-S2 400 160 170 Shore Hardness [D] DIN ISO 7619-1 (3s) 60 85 83 E-modulus [MPa] DIN EN ISO 527 200 2000 2000 2.2 Production of TPU 4-6
[0095] Table 3 below lists compositions in which the individual ingredients are specified in weight fractions (Wt). The mixtures were each produced using a Berstorff ZE 40 A twin-shaft extruder with a process section length of 35 D, divided into 10 housings. Strand pelletizing was used. Table 3: Formulations of TPU 1-3 TPU 4 (VB) TPU 5 (VB) TPU 6 (EB) TPU 1 52 TPU 2 52 TPU 3 52 Chopvantage HP3550 EC10-3.8 48 48 48 Table 4: Properties of TPU 4-6 TPU 4 (VB) TPU 5 (VB) TPU 6 (EB) Tensile strength [MPa] DIN 53504-S2 93 Not producible. 244 Elongation at break [%] DIN 53504-S2 8 3 E-modulus [MPa] DIN EN ISO 527 4080 18300 3. Results
[0096] TPU 2 cannot be processed. The material has a very high melting point, making the production of the fiberglass compound impossible.
[0097] TPU 4 is manufacturable, but its modulus of elasticity is only 4080MPa.
[0098] Surprisingly, TPU 6 is manufacturable. Its elastic modulus is 18300 MPa. 4. Measurement methods
[0099] Shore hardness A: DIN ISO 7619-1, Shore hardness test A (3s) Tensile strength: DIN EN ISO 527 Elongation at break: DIN EN ISO 527 Tear resistance: DIN ISO 34-1, B (b Cited literature
[0100] Plastics Handbook, Volume VII, edited by Vieweg and Höchtlen, Carl Hanser Verlag, Munich 1966 (pp. 103-113) EP 0 922 552 A1 DE 101 03 424 A1 WO 2006 / 072461 A1
Claims
1. A composition comprising (a) a thermoplastic polyurethane (TPU-1) obtained or obtainable by reaction of a polyisocyanate composition (IZ) with a polyol composition (PZ), wherein the polyol composition (PZ) comprises at least one polyol (P1), a chain extender (KV1) and a chain extender (KV2), wherein the chain extenders are used in a molar ratio KV1:KV2 in the range from 20:1 to 3:1; and (b) a filler (F1), wherein the filler (F1) is fibrous.
2. The composition according to claim 1, wherein the chain extender (KV1) and / or the chain extender (KV2) is selected from the group consisting of 1,2-ethanediol, 1,3-propanediol, 1,4-butanediol and 1,6-hexanediol, diethylene glycol, triethylene glycol, hydroquinone bis-2-hydroxyethyl ether and bis(2-hydroxyethyl) terephthalate.
3. The composition according to claim 1 or 2, wherein the chain extender (KV1) is 1,4-butanediol.
4. The composition according to any of claims 1 to 3, wherein the polyol (P1) is a polyether polyol.
5. The composition according to any of claims 1 to 4, wherein the polyisocyanate composition (IZ) comprises a polyisocyanate (PI) selected from the group consisting of phenylene 1,2-, 1,3- and / or 1,4-diisocyanate, triphenylmethane 4,4',4"-triisocyanate, naphthylene 1,5-diisocyanate (NDI), tolylene 2,4- and / or 2,6-diisocyanate (TDI), biphenyl 2,4'-, 4,4'- and / or 2,2'-diisocyanate, diphenylmethane 2,2'-, 2,4'- and / or 4,4'-diisocyanate (MDI), polyphenylpolymethylene polyisocyanate, xylylene 1,2-, 1,3- and / or 1,4-diisocyanate and m-tetramethylxylylene diisocyanate (TMXDI).
6. The composition according to any of claims 1 to 5, wherein the filler (F1) is selected from the group consisting of glass fibers, carbon fibers, aramid fibers, potassium titanate fibers, fibers composed of liquid-crystal polymers, metal fibers, polyester fibers, polyamide fibers, organic fibrous fillers and inorganic fibrous fillers.
7. The composition according to any of claims 1 to 6, wherein the filler (F1) has a length in the range from 3 mm to 4 mm and a diameter in the range from 1 µm to 20 pm, in each case determined in accordance with ASTM D578-98.
8. The composition according to any of claims 1 to 7, wherein the filler (F1) is comprised in an amount in the range from 40 to 60% by weight based on the total composition.
9. The composition according to any of claims 1 to 8, wherein the thermoplastic polyurethane has a Shore hardness in the range from 40 D to 90 D, determined in accordance with DIN ISO 7619-1.
10. A process for producing a composition, which comprises the step (i) mixing of the components (a) a thermoplastic polyurethane (TPU-1) obtained or obtainable by reaction of a polyisocyanate composition (IZ) with a polyol composition (PZ), wherein the polyol composition (PZ) comprises at least one polyol (P1), a chain extender (KV1) and a chain extender (KV2), wherein the chain extenders are used in a molar ratio KV1:KV2 in the range from 20:1 to 3:1; and (b) a filler (F1), wherein the filler (F1) is fibrous.
11. A composition obtained or obtainable by a process according to claim 10.
12. The use of a composition according to any of claims 1 to 9 or of a composition obtained or obtainable by a process according to claim 10 for producing a shaped body.
13. A shaped body comprising a composition according to any of claims 1 to 9 or a composition obtained or obtainable by a process according to claim 10.