METHOD FOR THE PRODUCTION OF POLYURETHANE / POLYISOCYANURATE (PUR / PIR) RIGID FOAM
Patent Information
- Application Number
- DE502019012187
- Authority / Receiving Office
- DE · DE
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2018-04-13
- Filing Date
- 2019-04-09
- Publication Date
- 2024-10-17
- Estimated Expiration
- 2039-04-09
AI Technical Summary
The production of polyurethane/polyisocyanurate (PUR/PIR) rigid foams faces challenges in achieving optimal foam properties such as foam pressure and curing without increasing the amount of flammable hydrocarbons, while also avoiding the use of formic acid and water as blowing agents to prevent corrosion and carbon monoxide formation.
A process for producing PUR/PIR rigid foams using a reaction mixture with a polyisocyanate component, an isocyanate-reactive component comprising polyester polyols and polyetherester polyols, a catalyst component with potassium formate, and a physical blowing agent, where the mixture contains minimal or no formic acid and water, and an isocyanate index of ≥ 150 to 600, optimizing foam properties without the need for higher hydrocarbon quantities.
This process improves foam pressure and curing efficiency while reducing the use of flammable hydrocarbons and minimizing corrosion risks, achieving stable and effective PUR/PIR foam production for applications like cold storage facilities.
Description
[0001] The invention relates to a process for the production of polyurethane / polyisocyanurate (PUR / PIR) rigid foams comprising the step i) reacting a reaction mixture containing A) a polyisocyanate component and B) an isocyanate-reactive component comprising B1) a polyol component, B2) a catalyst component, B3) optionally auxiliaries and additives, and C) a physical blowing agent characterized by that the catalyst component contains potassium formate B2.a), and that component B) of the reaction mixture contains 50.0 to 90.0 wt.% of at least one polyester polyol and / or polyether ester polyol B1.a) having a hydroxyl number in the range from 80 mg KOH / g to 290 mg KOH / g determined according to DIN 53240, and 1.0 to 10.0 wt.% of at least one polyol component B1.b) selected from the group consisting of polyether polyols, polycarbonate polyols and polyether-polycarbonate polyols having a hydroxyl number in the range from 300 mg KOH / g to 600 mg KOH / g determined according to DIN 53240, and optionally further isocyanate-reactive components B1.c), wherein the data in wt.% are in each case based on the total weight of the composition B), and that the reaction mixture from step i) contains less than 0.3 wt.% water and less than 0.2 wt.% formic acid, and wherein the reaction mixture from step i) has an isocyanate index of ≥ 150 to 600.
[0002] Polyurethane / polyisocyanurate (PUR / PIR) rigid foams are well-known. Their production is typically achieved by reacting an excess of polyisocyanates with compounds containing hydrogen atoms reactive toward isocyanate groups, particularly polyols. The excess isocyanate, usually with an isocyanate index of at least 150 or higher, results in the formation of urethane structures, which are formed by reacting isocyanates with compounds containing reactive hydrogen atoms, and further structures by reacting the isocyanate groups with each other or with other groups, such as polyurethane groups.
[0003] PUR / PIR rigid foams exhibit desirable properties with regard to thermal insulation and fire performance. This is particularly true for polyester-based PUR / PIR rigid foams (i.e., PUR / PIR rigid foams manufactured with > 40 wt.%, in particular > 50 wt.%, and most especially > 55 wt.%, of polyester polyols or polyetherester polyols based on the total weight of the isocyanate-reactive components). Due to these properties, they are used for insulating composite elements, such as metal sandwich elements, for example, for use in industrial hall construction. Composite elements are particularly used in the construction of cold storage facilities.
[0004] To achieve the desired foam properties, such as bulk density and thermal insulation properties of PUR / PIR rigid foams, physical blowing agents are added to the reaction mixture. While hydrocarbons offer advantages such as a favorable effect on the lambda value, they also have disadvantages, particularly their high flammability.
[0005] One goal in the production of hydrocarbon-blown PUR / PIR rigid foams is therefore to keep the amount of flammable hydrocarbons used as low as possible without negatively influencing other properties associated with the blowing agent, such as foam pressure, dimensional stability, density and shrinkage.
[0006] Composite elements used in the construction of cold storage facilities are often permanently exposed to low temperatures ranging from 0 °C to -30 °C. However, it has been shown that composite elements shrink in thickness when used continuously under these conditions. This shrinkage then leads, among other things, to undesirable stresses in the buildings constructed with the composite elements and to misalignment between individual composite elements, resulting in associated visual defects.
[0007] Catalyst components suitable for catalyzing the blowing reaction, the urethane reaction, and / or the isocyanurate reaction (trimerization) are typically added to the PUR / PIR reaction mixture. Amine-based catalyst systems are often used for both reactions; the use of potassium salts, especially potassium acetate, as trimerization catalysts is also known.
[0008] WO 07 / 25888 A describes the use of a catalyst system consisting of certain aminoethyl ethers or aminoethyl alcohols and salts of aromatic or aliphatic carboxylic acids, including potassium formate, in PUR / PIR systems. When such catalyst systems are used, a positive effect on the surface of formic acid / water-blown PUR / PIR foams is observed. WO 07 / 25888 describes, and also demonstrates in experiments, that formic acid as a blowing agent leads to PUR / PIR foams with long curing times. The solution proposed by WO 07 / 25888 is the use of the aforementioned catalyst system. When using this catalyst system, better curing times are found with formic acid (ibid., Table 2) than when omitting the aminoethyl ether (and replacing it with an aliphatically substituted tertiary amine).However, if the use of formic acid / water is omitted and replaced with a water / dipropylene glycol mixture, a significantly poorer foam (brittle, increased number of surface defects) is obtained. Overall, WO 07 / 25888 discloses good results only for the use of formic acid in combination with the catalyst system potassium formate / aminoethyl ether.
[0009] US Pat. No. 4,277,571 A describes the production of potassium formate-catalyzed polyisocyanurate foams based on a polyhydroxy compound containing naphthenic acids or their derivatives and a hydroxy-functional amine. The foams are said to exhibit good physical properties, particularly compression and dimensional stability.
[0010] However, it is also known that the use of naphthenic acids in general and / or formic acid and / or formic acid / water mixtures as blowing agents can lead to corrosion problems in the system and poses the risk of carbon monoxide formation (see, for example, "Reactive Polymers Fundamentals and Applications", 2nd Edition, 2013, Johannes Karl Fink, ISBN: 978-1-4557-3149-7). The use of formic acid causes increased urea formation, which in turn increases brittleness and negatively affects adhesion to the cover layers compared to purely physically blown foams.
[0011] Based on the described prior art, the aim of this application is to provide a process for the production of PUR / PIR rigid foams containing physical blowing agents, which improves the known PUR / PIR systems with regard to foam pressure and curing without having to use higher amounts of the physical blowing agent, but at the same time largely or even completely dispenses with the use of formic acid and / or water as blowing agents.
[0012] The above-mentioned object has now surprisingly been achieved by a process for producing a PUR / PIR rigid foam comprising the step i) the reaction of a reaction mixture containing A) a polyisocyanate component B) an isocyanate-reactive component comprising B1) a polyol component, B2) a catalyst component, B3) optionally auxiliaries and additives, C) a physical blowing agent, characterized in that component B) of the reaction mixture contains 50.0 to 90.0 wt.% of at least one polyester polyol and / or polyether ester polyol B1.a) having a hydroxyl number in the range from 80 mg KOH / g to 290 mg KOH / g determined according to DIN 53240, and 1.0 to 10.0 wt.% of at least one polyol component B1.b) selected from the group consisting of polyether polyols, polycarbonate polyols and polyether-polycarbonate polyols having a hydroxyl number in the range from 300 mg KOH / g to 600 mg KOH / g determined according to DIN 53240, and optionally further isocyanate-reactive components B1.c), the data in wt.% being based in each case on the total weight of the composition B), and in that the reaction mixture from step i) contains less than 0.3 wt.% (preferably 0.2 wt.%, particularly preferably less than 0.15 % wt.) water and less than 0.2 wt.% (preferably less than 0.1 wt.-% formic acid, particularly preferably no formic acid) and wherein the reaction mixture from step i) has an isocyanate index of ≥ 150 to 600. .
[0013] Preferably, the reaction mixture further contains no or only small amounts of naphthenic acids. In a particularly preferred embodiment, the reaction mixture contains less than 0.2 wt.% naphthenic acids (preferably less than 0.1 wt.% naphthenic acids, particularly preferably no naphthenic acids).
[0014] In further very preferred embodiments, the reaction mixture contains no naphthenic acids and less than 0.2 wt.% formic acid, in particular less than 0.1 wt.% formic acid, very particularly preferably no formic acid) and less than 0.3 wt.% (preferably less than 0.2 wt.%, and very particularly preferably less than 0.15 wt.%) water.
[0015] The polyol component B1.a) is one or more polyols selected from the group consisting of polyester polyols and polyetherester polyols.
[0016] The proportion of polyol component B1.a) is, based on the total weight of component B1), at least 50.0 - 90.0 wt.% and particularly preferably 55 - 90.0 wt.%.
[0017] Suitable polyester polyols include polycondensates of di-, tri-, and tetraols, and di-, tri-, and tetracarboxylic acids, or hydroxycarboxylic acids or lactones. Instead of free polycarboxylic acids, the corresponding polycarboxylic acid anhydrides or corresponding polycarboxylic acid esters of lower alcohols can also be used to produce the polyesters.
[0018] Examples of suitable diols include ethylene glycol, butylene glycol, diethylene glycol, triethylene glycol, polyalkylene glycols such as polyethylene glycols, 1,2-propanediol, 1,3-propanediol, 1,3- and 1,4-butanediol, 1,6-hexanediol and isomers, neopentyl glycol, or neopentyl glycol hydroxypivalate. Polyols such as trimethylolpropane, glycerin, erythritol, pentaerythritol, trimethylolbenzene, or trishydroxyethyl isocyanurate can also be used. Monohydric alkanols can also be used.
[0019] Examples of polycarboxylic acids that can be used include phthalic acid, isophthalic acid, terephthalic acid, tetrahydrophthalic acid, hexahydrophthalic acid, cyclohexanedicarboxylic acid, adipic acid, azelaic acid, sebacic acid, glutaric acid, tetrachlorophthalic acid, maleic acid, fumaric acid, itaconic acid, malonic acid, suberic acid, succinic acid, 2-methylsuccinic acid, 3,3-diethylglutaric acid, 2,2-dimethylsuccinic acid, dodecanedioic acid, endomethylenetetrahydrophthalic acid, dimer fatty acid, trimer fatty acid, citric acid, or trimellitic acid. In certain embodiments, the use of polyesters containing aliphatic dicarboxylic acids (e.g., glutaric acid, adipic acid, succinic acid) is preferred, particularly the use of purely aliphatic polyesters (without aromatic groups). The corresponding anhydrides can also be used as acid sources. Monocarboxylic acids such as benzoic acid and alkanecarboxylic acids can also be used.
[0020] Hydroxycarboxylic acids that can be used as reactants in the production of a polyester polyol with terminal hydroxyl groups include hydroxycaproic acid, hydroxybutyric acid, hydroxydecanoic acid, and hydroxystearic acid. Suitable lactones include caprolactone, butyrolactone, and homologues. Bio-based starting materials and / or their derivatives are also particularly suitable for the production of polyester polyols, such as:Castor oil, polyhydroxy fatty acids, ricinoleic acid, hydroxyl-modified oils, grape seed oil, black cumin oil, pumpkin seed oil, borage seed oil, soybean oil, wheat seed oil, rapeseed oil, sunflower seed oil, peanut oil, apricot kernel oil, pistachio oil, almond oil, olive oil, macadamia nut oil, avocado oil, sea buckthorn oil, sesame oil, hemp oil, hazelnut oil, primrose oil, rosehip oil, safflower oil, walnut oil, fatty acids, hydroxyl-modified and epoxidized fatty acids and fatty acid esters, for example based on myristoleic acid, palmitoleic acid, oleic acid, vaccenic acid, petroselinic acid, gadoleic acid, erucic acid, nervonic acid, linoleic acid, alpha- and gamma-linolenic acid, stearidonic acid, arachidonic acid, timnodonic acid, clupanodonic acid and cervonic acid. Particularly preferred are esters of ricinoleic acid with polyfunctional alcohols, e.g., glycerin. The use of mixtures of such bio-based acids with other carboxylic acids, e.g., phthalic acids, is also preferred.
[0021] The polyester polyols preferably have an acid number of 0-5 mg KOH / g. This ensures that blocking of amine catalysts by conversion to ammonium salts occurs only to a limited extent and that the reaction kinetics of the foaming reaction are minimally affected.
[0022] Suitable polyetherester polyols are compounds containing ether groups, ester groups, and OH groups. Organic dicarboxylic acids with up to 12 carbon atoms are suitable for producing the polyetherester polyols, preferably aliphatic dicarboxylic acids with ≥ 4 to ≤ 6 carbon atoms or aromatic dicarboxylic acids, which are used individually or in mixtures. Examples include suberic acid, azelaic acid, decanedicarboxylic acid, maleic acid, malonic acid, phthalic acid, pimelic acid, and sebacic acid, as well as, in particular, glutaric acid, fumaric acid, succinic acid, adipic acid, phthalic acid, terephthalic acid, and isoterephthalic acid. In addition to organic dicarboxylic acids, derivatives of these acids, for example, their anhydrides, as well as their esters and half-esters with low-molecular-weight, monofunctional alcohols with ≥ 1 to ≤ 4 carbon atoms, can also be used. The proportional use of the above-mentioned bio-based raw materials, in particular fatty acids orFatty acid derivatives (oleic acid, soybean oil) are also possible and can offer advantages, e.g. with regard to storage stability of the polyol formulation, dimensional stability, fire behavior and compressive strength of the foams.
[0023] Polyether polyols, which are obtained by alkoxylating starter molecules such as polyhydric alcohols, are used as a further component in the production of polyetherester polyols. The starter molecules are at least difunctional, but may optionally also contain portions of higher-functionality, particularly trifunctional, starter molecules.
[0024] Starter molecules are, for example, diols with number-average molecular weights Mn of preferably ≥ 18 g / mol to ≤ 400 g / mol, preferably ≥ 62 g / mol to ≤ 200 g / mol, such as 1,2-ethanediol, 1,3-propanediol, 1,2-propanediol, 1,4-butanediol, 1,5-pentenediol, 1,5-pentanediol, neopentyl glycol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,10-decanediol, 2-methyl-1,3-propanediol, 2,2-dimethyl-1,3-propanediol, 3-methyl-1,5-pentanediol, 2-butyl-2-ethyl-1,3-propanediol, 2-butene-1,4-diol and 2-butyne-1,4-diol, ether diols such as diethylene glycol, triethylene glycol, tetraethylene glycol, dibutylene glycol, tributylene glycol, tetrabutylene glycol, dihexylene glycol, trihexylene glycol, tetrahexylene glycol, and oligomer mixtures of alkylene glycols, such as diethylene glycol. Starter molecules with functionalities other than OH can also be used alone or in mixtures.
[0025] In addition to the diols, compounds with > 2 Zerewitinoff-active hydrogens, in particular with number-average functionalities of > 2 to ≤ 8, in particular from ≥ 3 to ≤ 6, can also be used as starter molecules for the production of the polyethers, for example 1,1,1-trimethylolpropane, triethanolamine, glycerol, sorbitan and pentaerythritol as well as polyethylene oxide polyols started on triols or tetraols with average molar masses Mn of preferably ≥ 62 g / mol to ≤ 400 g / mol, in particular from ≥ 92 g / mol to ≤ 200 g / mol.
[0026] Polyetherester polyols can also be prepared by alkoxylation, particularly by ethoxylation and / or propoxylation, of reaction products obtained by reacting organic dicarboxylic acids and their derivatives, as well as components containing Zerewitinoff-active hydrogens, particularly diols and polyols. Derivatives of these acids can include, for example, their anhydrides, such as phthalic anhydride.
[0027] Polyol production processes have been described, for example, by Ionescu in "Chemistry and Technology of Polyols for Polyurethanes", Rapra Technology Limited, Shawbury 2005, p. 55 ff. (Chapter 4: Oligo-Polyols for Elastic Polyurethanes), p. 263 ff. (Chapter 8: Polyester Polyols for Elastic Polyurethanes), and in particular on p. 321 ff. (Chapter 13: Polyether Polyols for Rigid Polyurethane Foams) and p. 419 ff. (Chapter 16: Polyester Polyols for Rigid Polyurethane Foams). It is also possible to obtain polyester and polyether polyols via glycolysis of suitable polymer recyclates. Suitable polyether-polycarbonate polyols and their production are described, for example, in EP 2910585 A,
[0024] -
[0041] . Examples of polycarbonate polyols and their preparation can be found, inter alia, in EP 1359177 A. The preparation of suitable polyetherester polyols is described, inter alia, in WO 2010 / 043624 A and in EP 1 923 417 A.
[0028] The polyester polyols and / or polyetherester polyols B1.a) have functionalities of preferably ≥1.2 to ≤3.5, in particular ≥1.6 to ≤2.4, and a hydroxyl number between 80 and 290 mg KOH / g, particularly preferably 150 to 270 mg KOH / g, and especially preferably 160 to 260 mg KOH / g. The polyester polyols and polyetherester polyols preferably contain more than 70 mol%, preferably more than 80 mol%, in particular more than 90 mol%, of primary OH groups.
[0029] The number-average molar mass M n (also: molecular weight) is determined in the context of this invention by gel permeation chromatography according to DIN 55672-1 of August 2007.
[0030] The "hydroxyl number" indicates the amount of potassium hydroxide in milligrams equivalent to the amount of acetic acid bound during the acetylation of one gram of substance. It is determined in the context of this invention according to the standard DIN 53240-2 (1998).
[0031] The "acid number" is determined in the context of the present invention according to the standard DIN EN ISO 2114:2002-06.
[0032] In the context of the present invention, "functionality" refers to the theoretical average functionality (number of functions in the molecule that are reactive towards isocyanates or polyols) calculated from the known starting materials and their quantitative ratios.
[0033] For the purposes of this application, "a polyester polyol" can also be a mixture of different polyester polyols, in which case the mixture of polyester polyols as a whole has the stated OH number. This applies analogously to the other polyols listed here and their key figures.
[0034] In addition to the polyols of polyol component B1.a) described above, other isocyanate-reactive components are also used in the isocyanate-reactive component B).
[0035] For this purpose, in particular, further polyols B1.b) selected from the group consisting of polyether polyols, polycarbonate polyols, and polyethercarbonate polyols are used. Very particular preference is given to using one or more polyether polyols in addition to the one or more polyols B1.a). Component B) contains 1.0 to 10.0 wt. % of at least one polyol component B1.b) selected from the group consisting of polyether polyols, polycarbonate polyols, and polyether-polycarbonate polyols with a hydroxyl number in the range of 300 mg KOH / g to 600 mg KOH / g, determined according to DIN 53240.
[0036] The addition of long-chain polyols, especially polyether polyols, can improve the flowability of the reaction mixture and the emulsifiability of the blowing agent-containing formulation. For the manufacture of composite elements, these can enable the continuous production of elements with flexible or rigid cover layers.
[0037] These long-chain polyols have functionalities of ≥ 1.2 to ≤ 3.5 and a hydroxyl number between 10 and 100 mg KOH / g, preferably between 20 and 50 mg KOH / g. They have more than 70 mol%, preferably more than 80 mol%, in particular more than 90 mol% primary OH groups. The long-chain polyols are preferably polyether polyols with functionalities of ≥ 1.2 to ≤ 3.5 and a hydroxyl number between 10 and 100 mg KOH / g.
[0038] The addition of medium-chain polyols, particularly polyether polyols, and low-molecular-weight isocyanate-reactive compounds can improve the adhesion and dimensional stability of the resulting foam. For the production of composite elements using the process according to the invention, these medium-chain polyols can enable the continuous production of elements with flexible or rigid cover layers. The medium-chain polyols, which are particularly polyether polyols, have functionalities of ≥ 2 to ≤ 6 and a hydroxyl number between 300 and 700 mg KOH / g.
[0039] The polyether polyols used are the polyether polyols known to the person skilled in the art and usable in polyurethane synthesis with the features mentioned.
[0040] Examples of suitable polyether polyols are polytetramethylene glycol polyethers, which are obtained by polymerization of tetrahydrofuran by cationic ring opening.
[0041] Also suitable polyether polyols are addition products of styrene oxide, ethylene oxide, propylene oxide, butylene oxide, and / or epichlorohydrin to di- or polyfunctional starter molecules. The addition of ethylene oxide and propylene oxide is particularly preferred. Suitable starter molecules include, for example, water, ethylene glycol, diethylene glycol, butyldiglycol, glycerol, diethylene glycol, trimethylolpropane, propylene glycol, pentaerythritol, sorbitol, sucrose, ethylenediamine, toluenediamine, triethanolamine, bisphenols, in particular 4,4'-methylenebisphenol, 4,4'-(1-methylethylidene)bisphenol, 1,4-butanediol, 1,6-hexanediol, as well as low-molecular-weight, hydroxyl-containing esters of such polyols with dicarboxylic acids, and oligoethers of such polyols.
[0042] Suitable polycarbonate polyols are polycarbonates containing hydroxyl groups, such as polycarbonatediols. These are formed by reacting carbonic acid derivatives, such as diphenyl carbonate, dimethyl carbonate, or phosgene, with polyols, preferably diols.
[0043] Examples of such diols are ethylene glycol, 1,2- and 1,3-propanediol, 1,3- and 1,4-butanediol, 1,6-hexanediol, 1,8-octanediol, neopentyl glycol, 1,4-bishydroxymethylcyclohexane, 2-methyl-1,3-propanediol, 2,2,4-trimethylpentanediol-1,3, dipropylene glycol, polypropylene glycols, dibutylene glycol, polybutylene glycols, bisphenols and lactone-modified diols of the type mentioned above.
[0044] Instead of or in addition to pure polycarbonate diols, polyether polycarbonate diols can also be used, which are obtainable, for example, by copolymerization of alkylene oxides, such as propylene oxide, with CO 2 .
[0045] Furthermore, the polyol component B1) may contain, in addition to the polyols described, other isocyanate-reactive compounds B1.c), in particular polyamines, polyols, polyamino alcohols, and polythiols. Of course, the described isocyanate-reactive components also include compounds with mixed functionalities.
[0046] In preferred embodiments of component B1), it also contains low molecular weight isocyanate-reactive compounds, in particular di- or trifunctional amines and alcohols, particularly preferably diols and / or triols with molecular weights M n of less than 400 g / mol, preferably from 60 to 300 g / mol. Examples of compounds used are triethanolamine, diethylene glycol, ethylene glycol, glycerol and low molecular weight esters or half-esters of these alcohols, e.g. the half-esters of phthalic anhydride and diethylene glycol. If such low molecular weight isocyanate-reactive compounds are used to produce the PUR / PIR rigid foams, e.g. in the function as chain extenders and / or crosslinking agents, they are expediently used in an amount of at most 5% by weight, based on the total weight of component B1). Compounds which, due to their structure, fall within the definition of component B1.c) and also fall under one of the definitions of the polyol compounds B1.a) or B1.b) described above, are counted quantitatively as component B1.a) or B1.b) and not as component B1.c).
[0047] A preferred polyol component B1) for the foams produced by this process contains 50.0 to 90.0 wt.% of the polyol component B1.a), which is selected from one or more polyols from the group consisting of polyester polyols and polyether ester polyols in a hydroxyl number range between 100 to 290 mg KOH / g and with functionalities of ≥ 1.2 to ≤ 3.5, in particular ≥1.6 to ≤ 2.4, and 1.0 to 10.0 wt.%, in particular 1.0 to 6 wt.%, of medium-chain polyether polyols with functionalities of ≥ 2 to ≤ 6 and a hydroxyl number between 300 and 600 mg KOH / g (B1.b) and furthermore 0 to 25 wt.%, preferably 1 to 20 wt.%, of long-chain polyether polyols with a functionality of ≥ 1.2 to ≤ 3.5 and a hydroxyl number between 10 and 100 mg KOH / g (B1.c), and 0 to 10 wt.%, in particular 1 to 5 wt.%, of low-molecular-weight isocyanate-reactive compounds with a molar mass M n of less than 400 g / mol (B1.c).
[0048] The isocyanate-reactive component B) or the reaction mixture may contain auxiliaries and additives B3). These are either initially added with the other components or added to the mixture of components during the production of the PUR / PIR rigid foams.
[0049] The auxiliaries and additives B3) preferably comprise emulsifiers (B3.a). Suitable emulsifiers, which also serve as foam stabilizers, include, for example, all commercially available silicone oligomers modified with polyether side chains, which are also used for the production of conventional polyurethane foams. If emulsifiers are used, they are used in amounts of preferably up to 8 wt. %, particularly preferably from 0.5 to 7.0 wt. %, in each case based on the total weight of the isocyanate-reactive composition. Preferred emulsifiers are polyetherpolysiloxane copolymers. These are commercially available, for example, under the names Tegostab®< B84504 and B8443 from Evonik, Niax* L-5111 from Momentive Performance Materials, AK8830 from Maystar, and Struksilon 8031 from Schill and Seilacher. Silicone-free stabilizers, such as LK 443 from Air Products, can also be used.
[0050] To improve fire resistance, flame retardants (B3.b) are also added to the isocyanate-reactive compositions. Such flame retardants are known in principle to the person skilled in the art and are described, for example, in "Kunststoffhandbuch", Volume 7 "Polyurethanes", Chapter 6.1. These can be, for example, halogenated polyesters and polyols, bromine- and chlorine-containing paraffins, or phosphorus compounds, such as the esters of orthophosphoric acid and metaphosphoric acid, which may also contain halogen. Flame retardants that are liquid at room temperature are preferably selected. Examples are triethyl phosphate, diethyl ethanephosphonate, cresyl diphenyl phosphate, dimethylpropanephosphonate, and tris((3-chloroisopropyl)phosphate). Particular preference is given to flame retardants selected from the group consisting of tris(chloro-2-propyl)phosphate (TCPP) and triethyl phosphate (TEP) and mixtures thereof. Flame retardants are preferably used in an amount of 1 to 30 wt.-%, particularly preferably 5 to 30 wt. %, based on the total weight of the isocyanate-reactive composition B). To achieve specific property profiles (viscosity, brittleness, flammability, halogen content), it may also be advantageous to combine different flame retardants. In certain embodiments, the presence of triethyl phosphate (TEP) in the flame retardant mixture or as the sole flame retardant is particularly advantageous.
[0051] Furthermore, component B3) also includes all other additives (B3.c) that can be added to isocyanate-reactive compositions. Examples of such additives include cell regulators, thixotropic agents, plasticizers, and dyes.
[0052] According to the invention, catalyst component B2) contains potassium formate B2.a). This is often used as a solution, e.g., in diethylene glycol / monoethylene glycol. Potassium formate is preferably used in a concentration of 0.2-4.0 wt.%, more preferably 0.4-2.0 wt.% (based on the mass of pure potassium formate in component B).
[0053] In addition, other catalysts may be present in B2), for example, to catalyze the blowing reaction, the urethane reaction, and / or the isocyanurate reaction (trimerization). The catalyst components can be added to the reaction mixture or, in whole or in part, pre-mixed with the isocyanate-reactive component B).
[0054] In addition to potassium formate, one or more catalytically active compounds selected from the following groups are particularly suitable: B2.b) Aminic catalysts, e.g. amidines, such as 2,3-dimethyl-3,4,5,6-tetrahydropyrimidine, and / or tertiary amines, such as triethylamine, tributylamine, dimethylcyclohexylamine, dimethylbenzylamine, N-methyl-, N-ethyl-, N-cyclohexylmorpholine, N,N,N',N'-tetramethylethylenediamine, N,N,N',N'-tetramethylbutanediamine, N,N,N',N'-tetramethylhexane-1,6-diamine, pentamethyldiethylenetriamine, bis(2-dimethylaminoethyl)ether, bis(dimethylaminopropyl)urea, dimethylpiperazine, 1,2-dimethylimidazole, N,N',N"-tris-(dimethylaminopropyl)hexahydrotriazine, bis[2-(N,N-dimethylamino)ethyl] ether, 1-aza-bicyclo-(3,3,0)-octane and 1,4-diaza-bi-cyclo-(2,2,2)-octane, and alkanolamine compounds such as triethanolamine, triisopropanolamine, N-methyl- and N-ethyl-diethanolamine, N,N-dimethylaminoethoxyethanol, N,N,N'-trimethylaminoethyl-ethanolamine and dimethylethanolamine.Particularly suitable compounds are selected from the group comprising tertiary amines, such as triethylamine, tributylamine, dimethylcyclohexylamine, dimethylbenzylamine, N,N,N',N'-tetramethylethylenediamine, pentamethyldiethylenetriamine, bis(2-dimethylaminoethyl)ether, dimethylpiperazine, 1,2-dimethylimidazole and alkanolamine compounds, such as tris(dimethylaminomethyl)phenol, triethanolamine, triisopropanolamine, N-methyl- and N-ethyldiethanolamine, N,N-dimethylaminoethoxyethanol, N,N,N'-trimethylaminoethylethanolamine and dimethylethanolamine.
[0055] In a likewise preferred embodiment, one or more aminic compounds according to the following structure are used in the catalyst component: (CH 3 ) 2 N-CH 2 -CH 2 -X-CH 2 -CH 2 -Y where Y = NR 2 or OH, preferably Y = N(CH 3 ) 2 or OH, particularly preferably Y = N(CH 3 ) 2 and where X = NR or O, preferably X = N-CH 3 or O, particularly preferably X = N-CH 3 . Each R can be selected independently of any other R and represents an organic radical of any structure having at least one C atom. R is preferably an alkyl group having 1 to 12 C atoms, in particular C1 to C6 alkyl, particularly preferably methyl and ethyl, in particular methyl.
[0056] Component B2.b) preferably contains dimethylbenzylamine (DMBA, N,N-dimethyl-1-phenylmethanamine according to IUPAC) and / or dimethylcyclohexylamine (DMCHA, N,N-dimethylcyclohexanamine according to IUPAC), especially dimethylcyclohexylamine. In particular, component B2.b) contains no other amine catalysts besides dimethylbenzylamine and / or dimethylcyclohexylamine.
[0057] In addition to the above-mentioned catalyst components, one or more catalytically active compounds selected from B2.c) metal carboxylates other than potassium formate, in particular alkali or alkaline earth metals, in particular sodium acetate, sodium octoate, potassium acetate, potassium octoate, as well as tin carboxylates, e.g. tin(II) acetate, tin(II) octoate, tin(II) ethylhexoate, tin(II) laurate, dibutyltin diacetate, dibutyltin dilaurate, dibutyltin maleate, and dioctyltin diacetate, and ammonium carboxylates are particularly suitable. Sodium, potassium, and ammonium carboxylates are particularly preferred. Preferred carboxylates are ethylhexanoates (=octoates), propionates, and acetates.
[0058] The catalyst components can be added to the reaction mixture or can be introduced wholly or partly into the isocyanate-reactive component B).
[0059] The reactivity of the reaction mixture is generally tailored to requirements using the catalyst component. For example, the production of thin panels requires a reaction mixture with higher reactivity than the production of thicker panels. Typical parameters are the start time and the setting time, which measure the time at which the reaction mixture begins to react and the point in time at which a sufficiently stable polymer network is formed. In a preferred embodiment, the catalysts B2.a), B2.b) and, if appropriate, B2.c) required to produce the rigid foam are used in such quantities that, for example, elements with flexible and rigid cover layers can be produced on continuously producing systems at speeds of up to 80 m / min, depending on the element thickness.
[0060] In particular, a combination of the catalyst components potassium formate B2.a) and amine catalysts B2.b) in a molar ratio n(potassium formate) / n(amine) between 0.1 and 80, in particular between 0.5 and 20, is preferably used in the reaction mixture. Short setting times can be achieved, for example, with more than 0.2 wt.% potassium formate based on all components of the reaction mixture.
[0061] The proportion of pure potassium formate in the catalyst mixture is preferably 15-100 wt.%, particularly preferably 30-100 wt.%. Preferably, no other catalysts, particularly those catalyzing the trimerization reaction, are used besides potassium formate. Particularly preferably, the catalyst mixture contains no other metal carboxylates besides potassium formate.
[0062] The reaction mixture further contains as much blowing agent C) as is necessary to achieve a dimensionally stable foam matrix and the desired bulk density. This is generally 0.5 - 30.0 parts by weight of blowing agent based on 100.0 parts by weight of component B. The blowing agents used are preferably physical blowing agents selected from at least one member of the group consisting of hydrocarbons, halogenated ethers, and perfluorinated and partially fluorinated hydrocarbons having 1 to 8 carbon atoms. In the context of the present invention, "physical blowing agents" are understood to mean compounds which, due to their physical properties, are highly volatile and do not react with the polyisocyanate component. The physical blowing agents to be used according to the invention are preferably selected from hydrocarbons (e.g., n-pentane, isopentane, cyclopentane, butane, isobutane, propane), ethers (e.g.,Methylal), halogenated ethers, (per)fluorinated hydrocarbons having 1 to 8 carbon atoms (e.g. perfluorohexane), and mixtures thereof. Also preferred is the use of (hydro)fluorinated olefins, such as HFO 1233zd(E) (trans-1-chloro-3,3,3-trifluoro-1-propene) or HFO 1336mzz(Z) (cis-1,1,1,4,4,4-hexafluoro-2-butene) or additives such as FA 188 from 3M (1,1,1,2,3,4,5,5,5-nonafluoro-4-(trifluoromethyl)pent-2-ene), as well as the use of combinations of these blowing agents. In particularly preferred embodiments, a pentane isomer or a mixture of different pentane isomers is used as blowing agent C). With extraordinary particular preference, a mixture of cyclopentane and isopentane is used as blowing agent C). Further examples of preferred fluorocarbons are HFC 245fa (1,1,1,3,3-pentafluoropropane), HFC 365mfc (1,1,1,3,3-pentafluorobutane), HFC 134a or mixtures thereof.Different propellant classes can also be combined.
[0063] Particularly preferred is the use of (hydro)fluorinated olefins, such as HFO 1233zd(E) (trans-1-chloro-3,3,3-trifluoro-1-propene) or HFO 1336mzz(Z) (cis-1,1,1,4,4,4-hexafluoro-2-butene) or additives such as FA 188 from 3M (1,1,1,2,3,4,5,5,5-nonafluoro-4(or2)-(trifluoromethyl)pent-2-ene and / or 1,1,1,3,4,4,5,5,5-nonafluoro-4(or2)-(trifluoromethyl)pent-2-ene), alone or in combination with other blowing agents. These have the advantage of having a particularly low ozone depletion potential (ODP) and a particularly low global warming potential (GWP).
[0064] Chemical blowing agents may also be included, provided that the reaction mixture less than 0.20 wt.%, preferably less than 0.10 wt.%, particularly preferably no (0.00 wt.%) formic acid and less than 0.30 wt.%, preferably 0.20 wt.%, particularly preferably less than 0.15 wt.%, water contains.
[0065] Particularly preferably, the reaction mixture does not contain any free carboxylic acids.
[0066] This means, in particular, that component B) preferably contains no additional water beyond the residual moisture that is unavoidable in technical products (e.g., by deliberately adding effective amounts of water). Surprisingly, a reduction in the tack-free time was observed only for these foams with very low water content.
[0067] In a preferred embodiment, the reaction mixture contains, in addition to the above-mentioned blowing agents, a carbamate capable of releasing carbon dioxide under reaction conditions. The use of 2-hydroxypropyl carbamate, for example, is preferred. Surprisingly, it has been found that the positive effect on both foam pressure and curing is particularly pronounced in the presence of carbamate.
[0068] Component A) is a polyisocyanate, i.e. an isocyanate with an NCO functionality of ≥ 2. Examples of such suitable polyisocyanates are 1,4-butylene diisocyanate, 1,5-pentane diisocyanate, 1,6-hexamethylene diisocyanate (HDI), isophorone diisocyanate (IPDI), 2,2,4- and / or 2,4,4-trimethylhexamethylene diisocyanate, the isomeric bis(4,4'-isocyanatocyclohexyl)methanes or their mixtures of any isomer content, 1,4-cyclohexylene diisocyanate, 1,4-phenylene diisocyanate, 2,4- and / or 2,6-tolylene diisocyanate (TDI), 1,5-naphthylene diisocyanate, 2,2'- and / or 2,4'- and / or 4,4'-diphenylmethane diisocyanate (MDI) and / or higher homologues, 1,3- and / or 1,4-bis-(2-isocyanato-prop-2-yl)-benzene (TMXDI), 1,3-bis-(isocyanatomethyl)benzene (XDI), and alkyl 2,6-diisocyanatohexanoates (lysine diisocyanates) with C1 to C6 alkyl groups.
[0069] As polyisocyanate component A), mixtures of the isomers of diphenylmethane diisocyanate ("monomeric MDI", abbreviated "mMDI") and its oligomers ("oligomeric MDI") are preferably used. Mixtures of monomeric MDI and oligomeric MDI are generally referred to as "polymeric MDI" (pMDI). The oligomers of MDI are polyphenyl polymethylene polyisocyanates with a higher ring core, i.e. mixtures of the homologues with a higher ring core of diphenyl methylene diisocyanate, which have an NCO functionality f > 2 and can be described by the following empirical formula: C 15 H 10 N 2 O 2 [C 8 H 5 NO] n , where n = integer > 0, preferably n = 1, 2, 3 and 4. Higher-nuclear homologues C 15 H 10 N 2 O 2 [C 8 H 5 NO] m , m = integer ≥ 4) can also be present in the mixture of organic polyisocyanates A). Further preferred polyisocyanate components A) are mixtures of mMDI and / or pMDI with a maximum of up to 20 wt.%, more preferably a maximum of 10 wt.%.-% of other aliphatic, cycloaliphatic and especially aromatic polyisocyanates known for the production of polyurethanes, especially TDI.
[0070] The polyisocyanate component A) is further characterized in that it preferably has a functionality of at least 2, in particular at least 2.2, particularly preferably at least 2.4, and very particularly preferably at least 2.7.
[0071] For use as polyisocyanate components in rigid foam, polymeric MDI types are particularly preferred over monomeric isocyanates.
[0072] The NCO content of the polyisocyanate component A) is preferably from ≥ 29.0 wt.% to ≤ 33.0 wt.%, and preferably has a viscosity at 25 °C of ≥ 80 mPas to ≤ 2900 mPas, particularly preferably from ≥ 95 mPas to ≤ 850 mPas at 25 °C.
[0073] The NCO value (also known as NCO content or isocyanate content) is determined using EN ISO 11909:2007. Unless otherwise stated, the values are given at 25°C.
[0074] Viscosity data refer to the dynamic viscosity, determined according to DIN EN ISO 3219:1994-10 "Plastics - Polymers / resins in liquid, emulsified or dispersed state".
[0075] In addition to the polyisocyanates mentioned above, modified diisocyanates with uretdione, isocyanurate, urethane, carbodiimide, uretonimine, allophanate, biuret, amide, iminooxadiazinedione and / or oxadiazinetrione structure as well as unmodified polyisocyanate with more than 2 NCO groups per molecule, such as 4-isocyanatomethyl-1,8-octane diisocyanate (nonane triisocyanate) or triphenylmethane-4,4',4"-triisocyanate, can also be used proportionally.
[0076] Instead of or in addition to the above-mentioned polyisocyanates, suitable NCO prepolymers can also be used as organic polyisocyanate component A). The prepolymers can be prepared by reacting one or more polyisocyanates with one or more polyols, corresponding to the polyols described under component A). It is possible that the isocyanate is a prepolymer obtainable by reacting an isocyanate with an NCO functionality of ≥ 2 and polyols with a molecular weight Mn of ≥ 62 g / mol to ≤ 8000 g / mol and OH functionalities of ≥ 1.5 to ≤ 6.0.
[0077] A reaction mixture is created by mixing the isocyanate-reactive component B) and the polyisocyanate component A), which results in the PUR / PIR rigid foam. Production generally occurs by mixing all components using conventional high- or low-pressure mixing heads.
[0078] The isocyanate index (also called index or isocyanate number) is the quotient of the actual amount of isocyanate groups used [mol] and the actual amount of isocyanate-reactive groups used [mol], multiplied by 100: Index = (mole isocyanate groups / mole isocyanate-reactive groups) * 100
[0079] In the reaction mixture, the number of NCO groups in the isocyanate and the number of isocyanate-reactive groups are adjusted to result in an index of 150 to 600. The index is preferably in a range of > 180 to < 450.
[0080] In a preferred embodiment, the present invention relates to a polyurethane / polyisocyanurate (PUR / PIR) rigid foam obtainable from the reaction of a reaction mixture of B) an isocyanate-reactive composition comprising B1.a) 50.0 to 90.0 wt.% of at least one polyester polyol and / or polyether ester polyol having a hydroxyl number in the range from 80 mg KOH / g to 290 mg KOH / g, B1.b) 1.0 to 20.0 wt.% of at least one polyether polyol having a hydroxyl number in the range from 300 mg KOH / g to 600 mg KOH / g, preferably comprising a polyether polyol initiated with an aromatic amine. B1.c) 0.0 to 5.0 wt.%, in particular 1.0 - 5.0 wt.%, of low molecular weight isocyanate-reactive compounds having a molar mass Mn of less than 400 g / mol B3.b) 1.0 to 30.0 wt.% of at least one flame retardant, B2.a) 0.1 to 4.0 wt.% potassium formate, the wt.% being based in each case on all components of the isocyanate-reactive composition B); with A) a mixture of diphenylmethane-4,4'-diisocyanate with isomers and higher-functional homologues, the isocyanate index being ≥ 150 to ≤ 450, in the presence of C) a physical blowing agent, 。 wherein the reaction mixture contains less than 0.30 wt% water and less than 0.20 wt% formic acid.
[0081] In one embodiment of the PUR / PIR rigid foams according to the invention, these have a core density of ≥ 30 kg / m 3 < to ≤ 50 kg / m 3 <. The density is determined according to DIN EN ISO 3386-1-98. The density is preferably in a range from ≥ 33 kg / m 3 < to ≤ 45 kg / m 3 <, and particularly preferably from ≥ 36 kg / m 3 < to ≤ 42 kg / m 3 <.
[0082] The present invention further relates to the use of the PUR / PIR foams according to the invention for the production of composite elements, in particular metal composite elements. For details of individual embodiments, reference is made to the explanations of the process according to the invention to avoid unnecessary repetition.
[0083] Metal composite elements are sandwich composite elements consisting of at least two cover layers and a core layer between them. In particular, metal-foam composite elements consist of at least two cover layers made of metal and a core layer made of a foam, e.g., a polyurethane (PUR) rigid foam or a polyurethane / polyisocyanurate (PUR / PIR) rigid foam. Such metal-foam composite elements are well known in the art and are also referred to as metal composite elements. In addition to coated steel sheets, stainless steel, copper, or aluminum sheets are also used as cover layers. Additional layers can be provided between the core layer and the cover layers. For example, the cover layers can be coated, e.g., with a paint.
[0084] Examples of the application of such metal composite elements include flat or lined wall elements and profiled roof elements for industrial halls and cold storage buildings as well as for truck bodies, hall doors or transport containers.
[0085] These metal composite elements can be manufactured continuously (preferred) or discontinuously. Devices for continuous production are known, for example, from DE 1 609 668 A or DE 1 247 612 A. Continuous application occurs using double-belt systems. In the prior art double-belt process, the reaction mixture is applied to the lower cover layer, for example, using oscillating application devices, e.g., pouring rakes, or one or more stationary pouring devices, e.g., pouring rakes with holes or other bores, or using nozzles with gaps and / or slots, or using multi-finger technology. See, for example, EP 2 216 156 A1, WO 2013 / 107742 A, WO 2013 / 107739 A, and WO 2017 / 021463 A.
[0086] The following embodiment is not according to the invention and serves merely for illustration and relates to a method for producing a composite element, wherein a reaction mixture according to the invention is applied to a moving cover layer by means of a casting device. Examples
[0087] The following compounds are used to produce PUR / PIR rigid foams: B1.a-P1 Polyester polyol made from phthalic anhydride, adipic acid, monoethylene glycol and diethylene glycol, OH number 240 mg KOH / g from Covestro Deutschland AG, B 1.a-P2 Stepanpol PS 2412, aromatic polyester polyol based on phthalic anhydride and diethylene glycol, containing 3-10 wt-% TCPP, OH number 240 mg KOH / g from Stepan, B 1.a-P3 Aliphatic polyester polyol produced by reacting a mixture of adipic acid, succinic acid and glutaric acid with ethylene glycol, OH number 216 mg KOH / g from Covestro Deutschland AG, B 1.b-P4 Polyether polyol based on ortho-toluenediamine, ethylene oxide and propylene oxide with an OH number of 415 mg KOH / g from Covestro Deutschland AG, B1.c-P5 Polyether polyol based on propylene glycol, propylene oxide and ethylene oxide with 90% primary OH groups and an OH number of 28 mg KOH / g from Covestro Deutschland AG, B3.b-1 Tris(1-chloro-2-propyl) phosphate (TCPP) from Lanxess GmbH B3.b-2 Triethyl phosphate (TEP) from Lanxess GmbH B3.a-1 Polyetherpolysiloxane copolymer Tegostab ®< B8443 from Evonik. B 1.c-P6 Half ester of phthalic anhydride and diethylene glycol, OH number 795 mg KOH / g from Covestro Deutschland AG, A-1 Desmodur ®< 44V70L polymeric PolyA-1 based on 4,4-diphenylmethane diisocyanate with an NCO content of approximately 31.5 wt.% Covestro Deutschland AG Carbamate 2-Hydroxypropylcarbamic acid salt, 40-60% in ethanediol, carbon dioxide-releasing additive from Covestro Deutschland AG B2.b-1 Dimethylbenzylamine, Covestro Deutschland AG B2.c-1 Potassium acetate (according to IUPAC: potassium ethanoate), 25 wt-% in diethylene glycol (DEG) B2.c-2 12.5 wt-% potassium acetate (according to IUPAC: potassium ethanoate) and 25 wt-% potassium 2-ethylhexanoate in diethylene glycol (DEG) B2.c-3 Potassium 2-ethylhexanoate, 50 wt% in DEG:NMP (=1:2) B2.a-1 Potassium formate (according to IUPAC: potassium methanoate), 36 wt-% in monoethylene glycol C-1 n-Pentane [F+;Xn;N] Measurement of the reaction and product properties of the manufactured PUR / PIR rigid foams:
[0088] The foam pressure and flow properties during the foam reaction can be determined in a rigid foam tube using methods known to those skilled in the art. For this purpose, the reaction mixture is prepared in a paper cup as described above, and the filled paper cup is inserted into a temperature-controlled tube from below. The rise profile and the developing foam pressure are continuously recorded during the reaction.
[0089] The measurement of the bulk density was carried out according to DIN EN ISO 845 (October 2009). Measuring the setting time:
[0090] The setting time is generally the time required, for example, in the polyaddition reaction between a polyol and a polyisocyanate, to produce a theoretically infinitely expanded polymer (transition from the liquid to the solid state). The setting time can be determined experimentally by dipping a thin wooden stick at short intervals into the foaming reaction mixture, prepared here in a test package with a base area of 20 x 20 cm². The time from mixing the components until the point at which threads remain attached to the stick upon withdrawal is the setting time. Measurement of the tack-free time:
[0091] After discharge, the tack-free time of the foam surface is determined according to TM 1014:2013 (FEICA). Measuring the indentation depth:
[0092] The indentation depth of freshly produced laboratory foams in test packages with a base area of 20×20 cm 2< is determined by measuring the penetration depth of a stamp with a defined stamp pressure after the specified time periods during the curing phase. Examples 1 - 4): Production of pentane-blown foams, with potassium carboxylate catalysts, without amine catalyst
[0093] All foams are produced by hand mixing on a laboratory scale in test packages with a base area of 20 x 20 cm² (see Table 1 for formulations and reaction properties). The polyol component containing the polyols, additives, and catalysts is initially introduced. Shortly before mixing, the polyol component is heated to 23–25°C, while the polyisocyanate component is kept at a constant temperature of 30–35°C. The polyisocyanate component is then added to the polyol mixture while stirring, to which the amount of pentane required to achieve a core density of 37–38 kg / m³ has been previously weighed. The mixing time is 6 seconds, and the mixing speed of the Pendraulik stirrer is 4200 rpm. After 2.5 and 5 minutes, respectively, the foam hardness is determined using the indentation method, and after 8–10 minutes, the maximum core temperature is determined. The foam is then stored for a further 24 hours at 23°C to allow it to react. Table 1: Preparation and properties of pentane-blown foams, with potassium carboxylate catalysts, without amine catalyst Formulation, reaction properties Unit Example 1* Example 2* Example 3* Example 4 B1.a-P1 pbw 66,5 66,5 66,5 66,5 B1.b-P4 pbw 5,2 5,2 5,2 5,2 B3.b-1 pbw 20,8 20,8 20,8 20,8 B3.b-2 pbw 5,2 5,2 5,2 5,2 B 1.c-P6 pbw 2,3 2,3 2,3 2,3 B3.a-1 pbw 3,0 3,0 3,0 3,0 B2.c-1 pbw 4,300 B2.c-2 pbw 4,300 B2.c-3 pbw 3,800 B2.a-1 pbw 2,900 A-1 pbw 189,2 189,0 167,4 190,8 C-1 pbw 14,6 14,6 13,5 13,7 C-1 wt-% 4,7 4,7 4,7 4,4 index 330,0 330,0 330,0 330,0 Start time s 16 15 12 14 Setting time s 46 46 45 46 Tack-free time s 65 69 92 55 Core density kg / m 3 37,0 37,3 37,7 37,5 Foam pressure hPa 266,0 248,0 192,0 382,0 Maximum core temperature °C 170,1 170,3 166,0 175,3 Impression depth after 2.5 min mm 9,0 9,5 13,0 7,0 Impression depth after 5 min mm 10,0 10,5 13,5 7,5
[0094] Table 1 shows that when using potassium formate as a blowing agent, less pentane is required to achieve the target bulk density of approximately 37 kg / m³. At the same time, inventive example 4, using potassium formate as the PIR catalyst, is characterized by higher foam pressures and higher core temperatures at the time of foaming reaction. Furthermore, it is evident that the flow behavior can be optimized in the presence of potassium formate as a catalyst compared to potassium acetate. This is reflected in shorter starting times with otherwise identical setting times (Comparative Examples 1* and 2* vs. inventive example 4).
[0095] Only when potassium formate is used can higher foam pressures and improved flow behavior be simultaneously observed. In the case of potassium 2-ethylhexanoate (Comparative Example 3*), although shorter start times are also observed, the foams exhibit lower foam pressures. Furthermore, foams produced with potassium formate exhibit improved curing (quantified by the indentation depth of a weight after 2.5 and 5 minutes). Examples 5 - 12): Production of pentane-blown foams, with potassium carboxylate catalysts, with amine catalyst
[0096] These foams were produced analogously to Examples 1 - 4) by hand mixing on a laboratory scale (formulations and reaction properties see Table 2).
[0097] Examples 5 - 9) are adjusted to approximately the same core density of approximately 38 kg / m³ by adjusting the amount of pentane. In Examples 9) and 10) as well as in Examples 11) and 12), other polyol formulations were used which differ in the composition of the main polyol (Polyol P2 = aromatic polyester, Polyol P3 = aliphatic polyester). It can be seen in each case that when potassium formate (Examples 10) and 12)) is used instead of potassium acetate, the density of the rigid foam decreases by 1.5 to 2.1 kg / m³ at a constant amount of blowing agent and, at the same time, the foam pressure increases by approximately 35 or 70 hPa. Furthermore, it can be seen that foams produced using potassium formate have improved curing properties (see indentation depth) at lower densities than those of PUR / PIR foams catalyzed with potassium acetate. Table 2: Preparation and properties of pentane-blown foams, with potassium carboxylate catalysts, with amine catalyst formulation Unit Example 5* Example 6* Example 7* Example 8 Example 9* Example 10 Example 11* Example 12 B1.a-P1 pbw 66,5 66,5 66,5 66,5 B 1.a-P2 pbw 83,0 83,0 B1.a-P3 pbw 83,0 83,0 B1.b-P4 pbw 5,2 5,2 5,2 5,2 5,2 5,2 5,2 5,2 B3.b-1 pbw 20,8 20,8 20,8 20,8 9,5 9,5 9,5 9,5 B3.b-2 pbw 5,2 5,2 5,2 5,2 B1.c-P6 pbw 2,3 2,3 2,3 2,3 2,3 2,3 2,3 2,3 B3.a-1 pbw 3,0 3,0 3,0 3,0 3,0 3,0 3,0 3,0 B2.b-1 pbw 1,2 1,2 1,2 1,2 1,2 1,2 1,2 1,2 B2.c-1 pbw 3,5 4,20 4,60 B2.c-2 pbw 3,6 B2.c-3 pbw 3,5 B2.a-1 pbw 1,9 2,50 3,00 A-1 pbw 184,1 184,6 167,0 180,9 200,0 200,0 200,0 200,0 C-1 pbw 14,4 14,4 13,6 13,3 14,9 14,9 14,9 14,9 C-1 wt-% 4,7 4,7 4,7 4,4 4,6 4,6 4,6 4,6 index 330,0 330,0 330,0 330,0 305,6 310,5 325,9 328,0 Start time s 13 13 11 12 13 11 14 12 Setting time s 46 47 47 46 37 36 37 38 Tack-free time s 90 92 126 84 48 44 47 45 Core density kg / m^3 38,5 37,6 38,4 38,3 39,8 38,2 38,9 36,8 Foam pressure hPa 228,0 188 173 247 242 278 286 355 Maximum core temperature °C 166,2 166,3 165 167,2 175,4 177,7 171 174,2 Impression depth after 2.5 min mm 13,5 16,5 18 11,5 4,2 3,9 6,0 5,8 Impression depth after 5 min mm 14,5 17,5 19,5 12,0 5,0 4,8 7,0 6,3 Examples 13 - 15): Preparation of pentane-blown foams, with potassium carboxylate catalysts, without amine catalyst and carbamate
[0098] These foams were produced analogously to Examples 1-4 by hand mixing on a laboratory scale (see Table 3 for formulations and reaction properties). It can be seen that the positive effect on both foam pressure and curing is particularly strong in the presence of carbamate. Table 3: Preparation and properties of pentane-blown foams with potassium carboxylate catalysts, with 2-hydroxyethyl carbamate Formulation, reaction properties Unit Example 13* Example 14* Example 15* Example 16 B1.a-P1 pbw 66,5 66,5 66,5 66,5 B1.b-P4 pbw 5,2 5,2 5,2 5,2 B3.b-1 pbw 20,8 20,8 20,8 20,8 B3.b-2 pbw 5,2 5,2 5,2 5,2 B 1.c-P6 pbw 2,3 2,3 2,3 2,3 B3.a-1 pbw 3,0 3,0 3,0 3,0 Carbamate pbw 1,5 1,5 1,5 1,5 B2.c-1 pbw 4,800 B2.c-2 pbw 4,800 B2.c-3 pbw 4,200 B2.a-1 pbw 3,400 A-1 pbw 211,2 211,0 186,9 214,7 C-1 pbw 15,5 15,5 14,3 14,7 C-1 wt-% 4,6 4,6 4,6 4,4 index 330,0 330,0 330,0 330,0 Start time s 14 12 11 13 Setting time s 47 46 46 45 Tack-free time s 62 67 88 54 Core density kg / m^3 36,7 36,3 36,8 37,2 Foam pressure hPa 308 287 237 392 Max. core temperature °C 173,9 174,4 169,8 179,4 Impression depth after 2.5 min mm 9,5 10,5 12,0 6,0 Impression depth after 5 min mm 10,5 11,5 13,0 6,5
[0099] All examples according to the invention exhibit a reduction in tack-free time compared to other potassium carboxylate-catalyzed foams. Surprisingly, this can only be observed with foams blown without water or almost without water, as demonstrated by the following Comparative Examples 17* and 18* (Table 4). Examples 17 - 18): Preparation of pentane-blown foams, with potassium carboxylate catalysts, water-containing (not according to the invention)
[0100] These foams were produced analogously to Examples 1 - 4) by hand mixing on a laboratory scale (formulations and reaction properties see Table 4). Table 4: Preparation and properties of pentane-blown foams with potassium carboxylate catalysts, water-containing Formulation, reaction properties Unit Example 17* Example 18* B 1.a-P3 pbw 73,0 73 B1.c-P5 pbw 12,0 12 B3.b-1 pbw 15 15 Water pbw 0,80 0,80 B3.a-1 pbw 3,00 3,00 B2.b-1 pbw 1,20 1,20 B2.c-1 pbw 3,50 B2.a-1 pbw 2,3 A-1 pbw 202,75 201,87 C-1 pbw 13,30 12,30 C-1 wt-% 4,10 3,80 index 350,0 350,0 Start time s 13 13 Setting time s 38 38 Tack-free time s 43 45 Core density kg / m^3 40,2 40,7
[0101] In comparative examples 17* and 18* (water-containing), an increased foam pressure can be found when using potassium formate, but no shortening of the tack-free time.
Claims
1. Process for producing rigid polyurethane / polyisocyanurate (PUR / PIR) foams comprising the step of i) reacting a reaction mixture containing A) a polyisocyanate component and B) an isocyanate-reactive component comprising B1) a polyol component, B2) a catalyst component, B3) optionally auxiliary and additive substances, and C) a physical blowing agent, characterized in that the catalyst component contains potassium formate B2.a), and in that the component B) of the reaction mixture contains - 50.0% to 90.0% by weight of at least one polyester polyol and / or polyether ester polyol B1.a) having a hydroxyl number in the range from 80 mg KOH / g to 290 mg KOH / g determined according to DIN 53240, and - 1.0% to 10.0% by weight of at least one polyol component B1.b) selected from the group consisting of polyether polyols, polycarbonate polyols and polyether-polycarbonate polyols having a hydroxyl number in the range from 300 mg KOH / g to 600 mg KOH / g determined according to DIN 53240, and - optionally further isocyanate-reactive components B1.c), wherein the reported % by weight values are in each case based on the total weight of the composition B), and in that the reaction mixture from step i) contains less than 0.3% by weight of water and less than 0.2% by weight of formic acid, and wherein the reaction mixture from step i) has an isocyanate index of ≥ 150 to 600.
2. Process according to Claim 1, wherein the reaction mixture further contains less than 0.20% by weight of naphthenic acids.
3. Process according to Claim 1 or 2, characterized in that based on its total weight the component B) of the reaction mixture contains at least 55% by weight of a polyol B1.a) selected from the group consisting of polyester polyols and polyether ester polyols.
4. Process according to any of the preceding claims, wherein based on its total weight the component B) contains 0.1-4.0% by weight of potassium formate B2.a).
5. Process according to Claim 1 or 2, characterized in that the component B) of the reaction mixture contains - 50.0% to 90.0% by weight of at least one polyester polyol and / or polyether ester polyol B1.a) having a hydroxyl number in the range from 80 mg KOH / g to 290 mg KOH / g determined according to DIN 53240, - 1.0% to 10.0% by weight of at least one polyether polyol B1.b) having a hydroxyl number in the range from 300 mg KOH / g to 600 mg KOH / g determined according to DIN 53240, - 0.0% to 5.0% by weight of low molecular weight isocyanate-reactive compounds B1.c) having a molar mass Mn of less than 400 g / mol, - 1.0% to 30.0% by weight of at least one flame retardant B.3), - 0.1% to 4.0% by weight of potassium formate B.2a) wherein the reported % by weight values are in each case based on all components of the isocyanate-reactive component B), and the component A) contains a mixture of diphenylmethane 4,4'-diisocyanate with isomeric and higher-functional homologs, and the reaction mixture has an isocyanate index of ≥ 150 to ≤ 450.
6. Process according to any of the preceding claims, characterized in that the catalyst component B2) contains 15-100% by weight of potassium formate and 0-85% by weight of an aminic catalyst B2.b).
7. Process according to any of the preceding claims, wherein the reaction mixture further contains a carbamate.
8. Process according to any of the preceding claims, characterized in that the reaction mixture contains a flame retardant selected from the group consisting of tris(chloro-2-propyl) phosphate (TCPP), triethyl phosphate (TEP) and mixtures thereof.
9. Process according to any of the preceding claims, characterized in that the blowing agent C) is a physical blowing agent selected from one or more compounds of the group containing hydrocarbons, halogenated ethers and (per)fluorinated hydrocarbons, in particular pentane isomers and / or (hydro)fluorinated olefins.
10. Process according to any of the preceding claims, further comprising the step of ii) applying the reaction mixture onto a moving outerlayer using a curtain coater, especially in continuous production.
11. Rigid polyurethane / polyisocyanurate foam obtainable by a process according to any of Claims 1-10.
12. Composite elements containing one or two outerlayers and a rigid polyurethane / polyisocyanurate foam according to Claim 11.
13. Use of a composite element according to Claim 12, characterized in that at least one outerlayer is made of metal, for the production of flat wall elements or wall elements having linear features or profiled roof elements for construction of industrial buildings and of cold stores or for truck bodies, industrial doors or transport containers.