POLYESTER COMPOSITIONS

DE502019012414D1Active Publication Date: 2024-11-14ENVALIOR DEUTSCHLAND GMBH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
DE502019012414
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Priority Date
2018-12-20
Filing Date
2019-12-16
Publication Date
2024-11-14
Estimated Expiration
2039-12-16

AI Technical Summary

Technical Problem

Aluminum oxide, due to its high Mohs hardness and thermodynamic stability, causes significant wear in processing machines and embrittlement in polyester-based products, leading to poor mechanical properties such as low elongation at break and impact strength, making it unsuitable for thermally conductive plastic compositions.

Method used

Surface-treating aluminum oxide with at least one aminosilane and/or epoxysilane before incorporating it into polyester compositions reduces abrasiveness and improves mechanical properties, resulting in thermally conductive and electrically insulating polyester compositions with enhanced processing behavior.

Benefits of technology

The surface-treated aluminum oxide significantly reduces abrasion on processing machines while maintaining or exceeding the mechanical properties of the original polyester compositions, ensuring acceptable thermal conductivity and improved processing efficiency.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The present invention relates to a process for reducing the abrasiveness of aluminum oxide-containing polyester compositions or to the use of aluminum oxide surface-treated with at least one aminosilane and / or epoxysilane in thermally conductive polyester compositions for reducing abrasion in processing machines and processing tools and to corresponding compositions, molding compounds to be produced therefrom and products based thereon. State of the art

[0002] Those skilled in the art are familiar with the use of aluminum oxide as an abrasive. Aluminum oxide is extracted from bauxite by digesting it with caustic soda using the Bayer process. Aluminum oxide is obtained by removing the water, for example, through firing, sintering, or calcination. A distinction is made between cubic γ-Al 2 O 3 , so-called alumina, which serves as a starting material for ceramic and aluminum production, and rhombohedral / trigonal α-Al 2 O 3 , known as the mineral corundum, sapphire, or, when doped with chromium, as ruby.

[0003] Due to its thermodynamic stability, α-Al 2 O 3 with a density of 3.98, a Mohs hardness of 9 and a melting point of 2053°C is preferably used as an abrasive.

[0004] US 5,718,971 A describes a polyester film containing aluminum oxide surface-treated with an aminosilane or epoxysilane. US 2003 / 194549 A1 describes a composition of binder and aluminum oxide particles pretreated with silanes, including aminosilanes and epoxysilanes. Alpha aluminum oxide is preferably used. Polyester is described as a binder, among other materials. CN 108 178 909 A discloses modified polyesters with nano-aluminum oxide particles, a coupling agent, and a flame retardant. Aminosilanes and phosphite stabilizers are listed, among others.

[0005] In WO2010 / 025857A1, the aluminum oxide used to produce abrasives is surface-treated with organic silane and incorporated into a synthetic resin matrix. The examples explicitly mention 3-aminopropyltriethoxysilane and 3-methacryloxypropyltrimethoxysilane as silanes.

[0006] The increase in thermal conductivity of polyester-based molding compounds and products produced therefrom by adding aluminum oxide (Al 2 O 3 ) is known to those skilled in the art from WO2009 / 019186 A1. However, due to its Mohs hardness of 9 and the resulting high wear in processing machines, particularly injection molding machine tools, aluminum oxide has not yet been widely adopted for the production of thermally conductive plastic compositions. In addition, it has been found that the use of aluminum oxide leads to significant embrittlement of a compound or products produced therefrom and also has a negative impact on the deformation resistance or elongation at break, as well as the impact strength of polyester-based products.

[0007] US 2003 / 194549 A1 describes a composition of binder and aluminum oxide particles which have been pretreated with silanes.

[0008] CN 108178909 A discloses a modified polyester with nano-alumina particles, coupling agent and flame retardant.

[0009] The elongation at break is a material property that indicates the permanent extension of a sample after fracture, relative to the initial gauge length, and is therefore an important parameter for characterising the deformability or ductility of a material (see: http: / / de.wikipedia.org / wiki / Bruchdehnung). Elongation at break is measured in a tensile test according to ISO527, e.g., on injection-molded specimens. Impact strength, on the other hand, describes the ability of a material to absorb impact energy and shock energy without breaking. Impact strength is calculated as the ratio of impact energy to the specimen cross-section (unit of measurement: kJ / m 2< ). Impact strength can be determined using various types of impact tests (Charpy, Izod). Impact strength is measured according to ISO180-1U, e.g., on injection-molded specimens. (See: http: / / de.wikipedia.org / wiki / Schlagz%C3%A4higkeit ). Object of the present invention

[0010] The object of the present invention was therefore to provide thermally conductive and electrically insulating polyester compositions containing aluminum oxide for this purpose, with improved mechanical properties compared to the above-cited WO 2009 / 019186 A1 and acceptable or optionally improved thermal conductivity as well as improved abrasion behavior with an otherwise comparable composition with regard to further additives.

[0011] The wear behaviour of processing machines, hereinafter referred to as "abrasion", in particular in extruders and injection moulding machines, was investigated in the context of the present invention based on the wear test of the German Plastics Institute DKI Darmstadt ( Publication by the Plastics Research Group, "New and further development of model testing methods for corrosive / abrasive wear in plastics processing", Project No. AiF 12245N (DKI 18 / 0-87), duration 01.12.1999 to 28.02.2003 recreated.

[0012] A low wear or a good wear behavior (=abrasion) in processing machines or processing tools means in the context of the present invention that only a technically justifiable material removal during injection molding of the polyester composition to be investigated of 100 shots (1 shot = 3D), with an injection speed v from v = 30 mm / s and a screw diameter D of D = 35 mm, at a melt temperature of 270°C through a nozzle consisting of two metal plates (steel: 1.2738) with the slot width b = 12 mm, the slot length l = 12 mm and the slot height h = 0.4 mm can be observed. V describes the volume flow that passes through the platelets during the spraying process. Material removal from the steel 1.2738 (abbreviated name 40CrMnNiMo8-6-4 and It) used in the present invention. Data sheet Dörrenberg Edelstahl GmbH, Engelskirchen, from 02 / 2017with the chemical composition C = 0.4%, Mn = 1.5%, Cr = 1.9%, Ni = 1.0%, Mo = 0.2%) of less than 200 mg is considered technically justifiable in the sense of the present invention in order to enable the user / processor, when using a suitably hardened and optionally surface-coated steel, to technically process polyester compositions containing aluminum oxide in the injection molding process. Fig.2 and Fig.3 show schematic representations of the wear apparatus used according to the invention to determine the abrasion as well as the plate arrangement and geometry of the measuring device used according to the invention.

[0013] If the specialist knows the number of shots, the shot speed and the shot quantity (shot quantity = screw feed = 3D = 3 times screw diameter), he can calculate a V = volume V = 3 D ⋅ π ⋅ D 2 2 which defines the amount of force forced through the metal slot. The apparent shear rate γ̇ ap the expert can use the formula γ ˙ ap = 6 ⋅ V ˙ b ⋅ h 2 with the V = volume melt flow V ˙ = v ⋅ π D 2 2 , the slot width b, the slot height h, the screw diameter D and the injection speed v also be calculated. The material removal can be determined by differential weighing of the metal plates before and after the test.

[0014] Good mechanical properties within the meaning of the present invention mean an elongation at break of at least 1.5%, measured according to ISO 527 on freshly molded test specimens at 150 parts by mass of aluminum oxide relative to 100 parts by mass of polyester. The elongation at break is the last recorded elongation value before a stress drop to less than or equal to 10% of the strength value occurs. The elongation at break is expressed as a quantity of dimension 1 or in percent (%). For fractures above the yield point, the nominal elongation at break is given. This is the last recorded nominal elongation value before a stress drop to less than or equal to 10% of the strength value occurs. The nominal elongation is determined from the measured values ​​between the clamps. See: https: / / de.wikipedia.org / wiki / Bruchdehnung?veaction=edit§ion=6#Definition_2

[0015] High impact strength within the meaning of the present invention means an impact strength of at least 18 kJ / m²< measured according to ISO 180-1U on freshly molded test specimens at 150 parts by mass of aluminum oxide relative to 100 parts by mass of polyester. An acceptable thermal conductivity for a product according to the invention within the scope of the present invention is a thermal conductivity measured according to ISO 22007-4 of at least 0.7 W / m²K on freshly molded test specimens, both in and perpendicular to the flow direction of the test specimen, at 150 parts by mass of aluminum oxide relative to 100 parts by mass of polyester.

[0016] Electrically insulating in the sense of the present invention means that the volume resistance of freshly molded test specimens measured according to IEC60093 is above 10 9< Ohm.m.

[0017] Surprisingly, it was found that polyester compositions and products produced therefrom, whose thermal conductivity is improved by a high aluminum oxide content, exhibit significantly lower abrasion on the tools during injection molding in processing machines while retaining their mechanical properties if the aluminum oxide is surface-treated with at least one aminosilane and / or epoxysilane before being processed into a molding compound in the polyester. Since the skilled person knows that abrasion depends on the filler content of a compound, the inventive effect must be tested on compositions that, apart from the aluminum oxide, otherwise contain the same amounts of additives. Solution to the task:

[0018] The present invention relates to a process for reducing the abrasiveness of thermally conductive, electrically insulating polyester compositions and molding compositions to be produced therefrom, characterized in that the aluminum oxide to be used, the surface of which is surface-treated with at least one aminosilane and / or epoxysilane, is brought into contact with a polyester composition.

[0019] The invention further relates to the use of aluminum oxide surface-treated with at least one aminosilane and / or epoxysilane to reduce abrasion in processing machines during the processing of polyester compositions and polyester molding compounds based thereon. For the purposes of the present invention, aluminum oxide without surface treatment is considered as the reference.

[0020] The invention also relates to compositions, molding materials to be produced therefrom and products based thereon containing a) 100 parts by mass of at least one polyester, b) 70 to 600 parts by mass, preferably 125 to 400 parts by mass, particularly preferably 150 to 300 parts by mass, of aluminum oxide (Al 2 O 3 ) surface-treated with at least one aminosilane and / or epoxysilane, and c) 0.017 to 12.5 parts by mass of at least one phosphite stabilizer.

[0021] In one embodiment, compositions according to the invention and the molding compositions to be produced therefrom, as well as products, contain, in addition to components a), b) and c), at least one mold release agent and / or nucleating agent. Thus, the present invention relates to compositions and molding compositions to be produced therefrom, and products based thereon, wherein a) 100 parts by mass of at least one polyester, b) 70 to 600 parts by mass, preferably 125 to 400 parts by mass, particularly preferably 150 to 300 parts by mass, of aluminum oxide (Al 2 O 3 ) surface-treated with at least one aminosilane and / or epoxysilane, c) 0.017 to 12.5 parts by mass of at least one phosphite stabilizer, and d) 0.001 to 10 parts by mass of at least one mold-release agent and / or nucleating agent.

[0022] In one embodiment, compositions according to the invention and the molding compositions to be produced therefrom, as well as products, comprise at least one additive other than components b), c) and d). Thus, the present invention relates to compositions and molding compositions to be produced therefrom, and products based thereon, wherein a) 100 parts by mass of at least one polyester, b) 70 to 600 parts by mass, preferably 125 to 400 parts by mass, particularly preferably 150 to 300 parts by mass, of aluminum oxide surface-treated with at least one aminosilane and / or epoxysilane, c) 0.017 to 12.5 parts by mass of at least one phosphite stabilizer, d) 0.001 to 10 parts by mass of at least one mold release agent and / or nucleating agent, and e) 0.001 to 150 parts by mass of at least one additive other than components b), c) and d).

[0023] In one embodiment, the present invention relates to compositions and molding materials to be produced therefrom and products based thereon, wherein a) 100 parts by mass of at least one polyester, b) 70 to 600 parts by mass, preferably 125 to 400 parts by mass, particularly preferably 150 to 300 parts by mass, of aluminum oxide surface-treated with at least one aminosilane and / or epoxysilane, c) 0.017 to 12.5 parts by mass of at least one phosphite stabilizer, d) 0.001 to 10 parts by mass of talc and / or at least one mold release agent, and e) 0.001 to 150 parts by mass of at least one further additive different from components b), c) and d).

[0024] Preferably, a composition according to the invention or molding compositions to be produced therefrom and products based thereon have a thermal conductivity to be determined according to ISO 22007-4 in the range from 0.4 to 10 W / mK, particularly preferably in the range from 0.8 to 8 W / mK, very particularly preferably in the range from 1 to 6 W / mK, both in and perpendicular to the flow direction of the test specimen to be examined.

[0025] The compositions according to the invention are prepared for further use by mixing the components a) and b) to be used as starting materials, and optionally the further components c) to e), in at least one mixing tool. This produces molding compositions based on the compositions according to the invention as intermediates. These molding compositions can either consist exclusively of the aforementioned components or contain further components in addition to the aforementioned components.

[0026] In the context of the present invention, "alkyl" refers to a straight-chain or branched saturated hydrocarbon group. For example, if an alkyl group with 1 to 4 carbon atoms is used, this can be referred to as a "lower alkyl group" and preferably includes methyl (Me), ethyl (Et), propyl, especially n-propyl and isopropyl, butyl, especially n-butyl, isobutyl, sec-butyl, and tert-butyl.

[0027] "Cycloalkyl" is derived from cycloalkanes, a group of ring-shaped, saturated hydrocarbons. The rings can bear side chains. In the systematics of organic chemistry, they are classified as alicyclic compounds. Cycloalkanes without side chains form a homologous series with the general molecular formula C n H 2n , where n ≥ 3. Thus, the smallest occurring cycloalkane is cyclopropane. Accordingly, the molecular formula for an unsubstituted cycloalkyl residue without a side chain is C n H 2n-1 .

[0028] For the sake of clarity, it should be noted that the scope of this invention encompasses all definitions and parameters listed, whether general or in preferred ranges, in any combination. This expressly also applies to the combinations of the processes and uses described within the scope of the present invention with the mass fractions of the components as specified for the compositions and the molding compositions to be produced therefrom and the products based thereon.

[0029] Unless otherwise stated, cited standards apply in the version valid on the filing date. Unless otherwise stated, percentages are by weight. Preferred embodiments of the invention Component a)

[0030] The polyesters to be used according to the invention are preferably polyalkylene terephthalates (PAT). Preferred polyalkylene terephthalates are selected from the group consisting of polyethylene terephthalate (PET), polytrimethylene terephthalate (PTT), polybutylene terephthalate (PBT), polypentamethylene terephthalate (PPT), polyhexamethylene terephthalate (PHT), and polyoctamethylene terephthalate (POT).

[0031] According to the invention, component a) is at least one polyalkylene terephthalate, preferably at least polybutylene terephthalate (PBT), polyethylene terephthalate (PET) or a blend of PBT and PET, in particular blends of PBT and PET, wherein the PET content, based on the sum of all polyesters contained, is in the range from 50 to 99.9% by weight.

[0032] According to the invention, component a) is preferably polybutylene terephthalate (PBT) or polyethylene terephthalate (PET) or a blend of PBT and PET, in particular blends of PBT and PET, in which the PET content, based on the sum of all polyesters contained, is in the range from 50 to 99.9% by weight.

[0033] The polyalkylene terephthalates PBT and PET, which are preferably used according to the invention, are reaction products of aromatic dicarboxylic acids or their reactive derivatives, preferably dimethyl esters or anhydrides, and the corresponding aliphatic diols. They can be prepared from terephthalic acid (or its reactive derivatives) and the respective aliphatic diols with 4 or 2 carbon atoms by known methods ( Plastics Handbook, Vol. VIII, p. 695 - 743, Karl-Hanser-Verlag, Munich 1973).

[0034] PET preferably used as polyester contains at least 80 mol%, preferably at least 90 mol%, based on the dicarboxylic acid, of terephthalic acid residues and at least 80 mol%, preferably at least 90 mol%, based on the diol component, of ethylene glycol residues.

[0035] PBT preferably used as polyester contains at least 80 mol%, preferably at least 90 mol%, based on the dicarboxylic acid, of terephthalic acid residues and at least 80 mol%, preferably at least 90 mol%, based on the diol component, of 1,4-butanediol residues.

[0036] The preferred polyesters PBT and PET can contain, in addition to ethylene or 1,4-butanediol residues, up to 20 mol% of other aliphatic diols with 3 to 12 C atoms or cycloaliphatic diols with 6 to 21 C atoms. Preferred are residues of 1,3-propanediol, 2-ethyl-1,3-propanediol, neopentyl glycol, 1,5-pentanediol, 1,6-hexanediol, 3-methyl-2,4-pentanediol, 2-methyl-2,4-pentanediol, 2,2,4-trimethyl-1,3-pentanediol, 1,6,2-ethyl-1,3-hexanediol, or 2,2-Bis-(4-hydroxypropoxyphenyl)propane (DE-A 24 07 674 DE-A 24 07 776 , DE-A 27 15 932 ).

[0037] In one embodiment, the preferred polyesters can be branched by incorporating relatively small amounts of tri- or tetrahydric alcohols or tri- or tetrabasic carboxylic acids, as described, for example, in DE-A 19 00 270. Preferred branching agents are trimesic acid, trimellitic acid, trimethylolethane and trimethylolpropane, and pentaerythritol.

[0038] To characterize the average molecular weight of the polyester used as component a), the solution viscosity, also called intrinsic or limiting viscosity (SV or IV), is often used. The polyesters preferably used according to the invention preferably have an intrinsic viscosity in the range from 30 cm 3 / g to 150 cm 3 / g, particularly preferably in the range from 40 cm 3 / g to 130 cm 3 / g, especially preferably in the range from 50 cm 3 / g to 110 cm 3 / g, in each case measured in phenol / o-dichlorobenzene (1:1 parts by weight) at 25°C using an Ubbelohde viscometer according to ISO 1628 (see: Viscosity Manual, SI Analytics GmbH / Xylem Inc. 11 / 2015 ).

[0039] The intrinsic viscosity [η] is also called the limiting viscosity number or Staudinger index because, firstly, it is a constant and, secondly, it is related to the molecular weight. It indicates how the viscosity of the solvent is influenced by the dissolved substance. The following definition is used to determine the intrinsic viscosity: η = lim c → 0 η sp c = lim c → 0 1 c ln η η 0 where c is the concentration of the solute in g / ml, n 0 is the viscosity of the pure solvent and n sp = n / n 0 -1 is the specific viscosity.

[0040] If a blend of PET and PBT is used, a blend is preferred in which the PET content, based on the sum of all polyesters contained in component a), is in the range of 50 to 99.9 wt.%. Component b)

[0041] Preferably, an α-Al 2 O 3 surface-treated with at least one aminosilane and / or at least one epoxysilane is used as component b).

[0042] For component b), Al 2 O 3 [CAS 1344-28-1] with a monomodal, volume-average particle size distribution determined by laser diffraction according to ISO 13320 is particularly preferred. The evaluation of the data obtained by laser diffraction is carried out using a volume-related histogram with a logarithmic abscissa. For this purpose, the particle sizes are divided into size classes. Each decade is divided into 18 size classes over a measuring range of 0.01 µm to 10000 µm. This results in 108 size classes, the width of which corresponds to the size class y of the formula y = 0,01 ⋅ e ln 10 ⋅ x 18 − 0,01 ⋅ e ln 10 ⋅ x − 1 18 where x is the consecutive number of size classes in the range from 1 to 108.

[0043] For the definition of the term "monomodal" see: https: / / de.wikipedia.org / wiki / Partikelgr%C3%B6%C3%9Fenverteilung

[0044] According to the invention, a monomodal particle size distribution exists when the plot of the volume of the aluminum oxide particle sizes in [%] (= Y-axis in the histogram) against the size class in micrometers [µm] (= X-axis in the histogram) preferably forms only one maximum in the form of a Gaussian curve, and any additional maxima that may occur do not exceed a volume of 1%. Particularly preferably, the one maximum of the Gaussian curve to be considered in the histogram lies in the range from 0.1 to 15 µm, most preferably in the range from 0.1 to 10 µm.

[0045] An aluminum oxide powder used in the present invention with a monomodal, volume-average particle size distribution determined by laser diffraction according to ISO 13320 is CT 3000 SG from Almatis GmbH with a d50 value of 0.5 µm and a BET surface area of ​​7.8 m 2 < / g.

[0046] Fig. 1shows a histogram with the monomodal particle size distribution determined by laser diffraction according to ISO 13320 of another surface-treated aluminum oxide used in the present invention, for which 3-aminopropyltrimethoxysilane was used. However, 3-aminopropyltriethoxysilane can also be used. In the histogram of the Fig. 1 The size classes in µm (x-axis) are plotted against the volume in %. The d10 is 0.582 µm, the d50 is 1.95 µm, and the d90 is 4.79 µm. Monomodal aluminum oxides are also marketed by Nabaltec AG, Schwandorf, under the brand name Nabalox ®.

[0047] The term "particle size distribution" is borrowed from statistics. There, frequencies and frequency distributions of any characteristic, such as manufacturing tolerances, are considered. In the field of particle technology and particle metrology, or dispersity analysis, the equivalent diameter of a particle is chosen as the characteristic. The general frequency distribution of statistics thus becomes the particle size distribution, which is often also referred to as the grain size distribution. The density distribution of particle sizes usually exhibits the shape of a Gaussian bell curve. If the density distribution of particle sizes has only one maximum, it is called a monomodal distribution. If there are two maxima, the distribution is bimodal. The abscissa value of the largest maximum is called the modal value. The particle size distribution is determined using laser diffraction according to ISO 13320.For the measurement, the optical material data for aluminum oxide were used in the present invention and evaluated according to the Mie theory. See: . https: / / de.wikipedia.org / wiki / Laserbeugungs-Partikelgr%C3%B6%C3%9Fenanalyse. d10, d50 and d90 are the diameters where 10%, 50% (median) and 90% of the particles have a smaller diameter relative to the total volume.

[0048] The technical aluminum oxide preferably used in the present invention has a proportion of α-Al 2 O 3 of more than 70%. It is particularly preferred to use an aluminum oxide with an α-Al 2 O 3 proportion of more than 90%. It is very particularly preferred to use an aluminum oxide with an α-Al 2 O 3 proportion of more than 95%. According to the invention, α-Al 2 O 3 with less than 5% by weight of impurities is particularly preferred, and very particularly preferred with less than 1% by weight of impurities.

[0049] For component b), a surface-treated aluminum oxide in powder form is preferably used. Preferred powders have a volume-average particle size d50 of at most 100 µm, determined by laser diffraction according to ISO 13320, preferably a volume-average particle size d50 in the range of 0.1 to 50 µm, particularly preferably a volume-average particle size d50 in the range of 0.5 to 10 µm, and most preferably a volume-average particle size d50 in the range of 0.5 to 5 µm.

[0050] The particle size d10 for component b), which is to be determined by laser diffraction according to ISO13320, is preferably in the range from 0.01 to 20 µm, particularly preferably from 0.05 to 10 µm, very particularly preferably in the range from 0.1 to 5 µm and especially preferably in the range between 0.5 and 2 µm.

[0051] The particle size d90 for component b), which is to be determined by laser diffraction according to ISO13320, is preferably at most 200 µm, particularly preferably in the range from 1 to 100 µm, very particularly preferably in the range from 1.5 to 50 µm, especially preferably in the range from 2 to 10 µm.

[0052] Preferably, an aluminum oxide having a volume-average particle size distribution determined by laser diffraction according to ISO 13320 with a d50 of not more than 100 µm, a d10 in the range from 0.01 to 20 µm, and a d90 of not more than 200 µm is used for component b). The invention therefore preferably relates to compositions and molding compounds and products produced therefrom, with the proviso that an aluminum oxide having a volume-average particle size distribution determined by laser diffraction according to ISO 13320 with a d50 of not more than 100 µm, a d10 in the range from 0.01 to 20 µm, and a d90 of not more than 200 µm is used as component b).

[0053] For component b), an aluminum oxide having a monomodal, volume-average particle size distribution, determined by laser diffraction in accordance with ISO 13320, with a d50 of not more than 100 µm, a d10 in the range from 0.01 to 20 µm, and a d90 in the range from 1 to 100 µm is particularly preferably used. The invention therefore particularly preferably relates to compositions and molding compounds and products to be produced therefrom, with the proviso that an aluminum oxide having a monomodal, volume-average particle size distribution, determined by laser diffraction in accordance with ISO 13320, with a d50 of not more than 100 µm, a d10 in the range from 0.01 to 20 µm, and a d90 in the range from 1 to 100 µm is used.

[0054] For component b), very particular preference is given to using an aluminum oxide having a monomodal, volume-average particle size distribution, determined according to ISO 13320 by laser diffraction, with a d50 in the range from 0.1 to 50 µm, a d10 in the range from 0.01 to 20 µm, and a d90 in the range from 1 to 100 µm. The invention therefore very particularly preferably relates to compositions and molding compounds and products to be produced therefrom, with the proviso that an aluminum oxide having a monomodal, volume-average particle size distribution, determined according to ISO 13320 by laser diffraction, with a d50 in the range from 0.1 to 50 µm, a d10 in the range from 0.01 to 20 µm, and a d90 in the range from 1 to 100 µm is used.

[0055] In particular, very particular preference is given to using an aluminum oxide having a monomodal, volume-average particle size distribution, determined according to ISO 13320 by laser diffraction, with a d50 in the range from 0.5 to 5 µm, a d10 in the range from 0.5 to 2 µm, and a d90 in the range from 2 to 10 µm. The invention therefore particularly preferably relates to compositions and molding compounds and products to be produced therefrom, with the proviso that an aluminum oxide having a monomodal, volume-average particle size distribution, determined according to ISO 13320 by laser diffraction, with a d50 in the range from 0.5 to 5 µm, a d10 in the range from 0.5 to 2 µm, and a d90 in the range from 2 to 10 µm is used as component b).

[0056] The Al 2 O 3 particles to be used according to the invention for component b) can be present in different shapes, which can be described by the aspect ratio. Preference is given to using particles with an aspect ratio of 1 to 100, more preferably 1 to 30, and most preferably 1 to 10. EP 3 164 694 A1 describes some methods for determining the aspect ratio. In camera-based methods, the particles are imaged as two-dimensional images onto the camera sensor. If the sensor is a CCD matrix or a CMOS image sensor, appropriate image analysis software is used to determine the particle shape. DE 198 02 141 C1 describes a solution with a matrix camera and EP 1 972 921 A1 describes a solution with two cameras. If the sensor is a CCD line, the imaged particle area is composed of the measured chord lengths at a known particle velocity.Corresponding devices and methods are described in DE 10 2009 056 503 A1 (with a sensor line), DE 10 2004 056 520 A1 (with a CCD line), DE 43 13 688 A1 (with a CCD line), DE 41 19 240 C2 (with a CCD line), DD 278 859 A1 (with a CCD line sensor), DD 260 764 A1 (with a CCD line sensor), and DD 232760 A1 (with a single-line television camera). DE 196 28 348 C1 proposes determining particle shape using a line of individual optical fibers, with a second optical fiber line being used to determine velocity. Diffraction-based methods utilize the dependence of the particle diffraction pattern on the particle shape. The particles are irradiated with coherent light, and the light intensity distribution of the diffraction pattern is measured with a suitable receiver. The distribution of light intensity in the diffraction pattern depends on the shape of the particles. Solutions for this can be found in DE 694 06 683 T2 (with a ring sensor) and DE 102 18 413 B4. .DE 41 29105 A1 discloses a particle shape determination using scattered light measurement. Since the methods mentioned differ only in their complexity, the skilled person can freely choose from the methods mentioned in the prior art.

[0057] Al 2 O 3 to be used according to the invention for component b) is provided with at least one surface modification based on at least one aminosilane and / or epoxysilane, preferably epoxysilane. Silane-based organic coupling agents are referred to as surface modifications, which are intended to improve the bond to the thermoplastic matrix.

[0058] Preferably, at least one aminosilane having the general molecular formula (RO) 3 -Si-(CH 2 ) n -X is used for the surface treatment or surface modification of the aluminum oxide, in which R represents an organic radical selected from the group consisting of methyl, ethyl, i-propyl and methoxymethyl, n represents an integer from 0 to 12 (including end values), and X represents a radical NR 1< R 2< and R 1< and R 2< each independently represent hydrogen, a C 1 -C 6 alkyl radical or a C 5 -C 9 cycloalkyl radical.

[0059] An aminosilane preferably used for the surface treatment or surface modification of the aluminum oxide is selected from the group consisting of 3-aminopropyltriethoxysilane [CAS 919-30-2], 3-aminopropyltrimethoxysilane [CAS 13822-56-5], N-(2-aminoethyl)-3-aminopropyltrimethoxysilane [CAS 1760-24-3], N-(2-aminoethyl)-3-aminopropyltriethoxysilane [CAS 5089-72-5], 3-(N-cyclohexylamino)propyltrimethoxysilane [CAS 3068-78-8], and N,N-(diethylaminomethyl)triethoxysilane [CAS 15180-47-9].

[0060] For the surface treatment or surface modification of the aluminum oxide, at least one epoxysilane having the general empirical formula ER 3< -Si(R 4< ) a -(OR 5< ) 3-a is preferably used, in which E stands for a glycidyl group, a glycidyloxy group or an epoxycyclohexyl group or a mixture thereof, R 3< stands for a C 1 -C 4 alkylene group, R 4< and R 5< each independently stand for C 1 -C 4 alkyl groups and a stands for 0, 1 or 2.

[0061] Particularly preferably, at least one epoxysilane is selected from the group 2-(3,4-Epoxycyclohexyl)ethyltrimethoxysilane [CAS 3388-04-3], (3-Glycidoxypropyl)trimethoxysilane [CAS 2530-83-8], (3-Glycidoxypropyl)methyldiethoxysilane [CAS 2897-60-1], 5,6-Epoxyhexyltriethoxysilane [CAS 86138-01-4], 2-(3,4-Epoxycyclohexyl)ethylmethyldiethoxysilane [CAS 3388-04-3], (3-Glycidoxypropyl)triethoxysilane [CAS 2602-34-8], 2-(3,4-Epoxycyclohexyl)ethyltriethoxysilane [CAS 10217-34-2] and (3-Glycidoxypropyl)methyldimethoxysilane [CAS 65799-47-5].

[0062] Silane-based surface modifications according to the invention and their preparation are known to the person skilled in the art in principle from US 7,547,743 B2 or DE 69317121 T2, the contents of which with regard to the preparation of silanes to be used according to the invention disclosed therein are fully encompassed by the present application.

[0063] The aminosilane or epoxysilane to be used for the surface treatment is preferably applied in amounts in the range of 0.05 to 5 parts by mass, particularly preferably in amounts in the range of 0.1 to 1 part by mass, based on 100 parts by mass of aluminum oxide.

[0064] The surface treatment or surface modification of the aluminum oxide with aminosilane and / or epoxysilane can be carried out immediately before the use of the aluminum oxide, or previously surface-treated aluminum oxide can be used. The silanes used react upon contact with the aluminum oxide to form silanols, and the respective alcohol residue is split off. Fig.1 The discussed 3-aminopropyltrimethoxysilane and 3-aminopropyltriethoxysilane are both converted to 3-aminopropylsilanol upon contact with aluminum oxide, and the alcohol residue is eliminated. The same applies to the alternative epoxysilanes.

[0065] According to the invention, the aminosilane is applied to the aluminum oxide in the manner described in WO 2009 / 156342 A1, by first placing the aminosilane in deionized water (DE = fully demineralized water) to form the silanol and stirring the mixture at a temperature in the range of 23 to 27 °C (room temperature). The amounts used are based on the mass fractions stated above. The aluminum oxide is then added, the suspension is stirred at temperatures in the range of 75 to 100 °C, the surface-treated aluminum oxide is filtered off with suction and washed with deionized water. The mixture is then dried at temperatures of approximately 120 °C and tempered at 200 °C. A technical method for the surface treatment of aluminum oxide with silanes is described in EP 1 628 916 B1, the content of which is fully encompassed by the present application.In this process, pyrogenic aluminum oxide is sprayed with the surface modifier at room temperature, and the mixture is then thermally treated at a temperature of 50 to 400 °C for a period of 1 to 6 hours. Alternatively, the pyrogenic aluminum oxide is treated with the surface modifier in vapor form, and the mixture is then thermally exposed to a temperature in the range of 50 to 800 °C for a period of 0.5 to 6 hours. The thermal treatment can be carried out under a protective gas, such as nitrogen. The surface treatment according to EP 1 628 916 B1 can be carried out continuously or discontinuously in heatable mixers and dryers with spray devices. Suitable devices include, for example, ploughshare mixers or plate, cyclone, or fluidized-bed dryers. Component c)

[0066] According to the invention, at least one phosphite stabilizer is used as component c). Preference is given to at least one phosphite stabilizer from the series tris(2,4-ditert-butylphenyl)phosphite (Irgafos®< 168, BASF SE, [CAS 31570-04-4]), bis(2,4-di-tert-butylphenyl)pentaerythritol diphosphite (Ultranox®< 626, Chemtura, [CAS 26741-53-7]), bis(2,6-di-tert-butyl-4-methylphenyl)pentaerythritol diphosphite (ADK Stab PEP-36, Adeka, [CAS 80693-00-1]), bis(2,4-dicumylphenyl)pentaerythritol diphosphite (Doverphos®< S-9228, Dover Chemical Corporation, [CAS 154862-43-8]), Tris(nonylphenyl)phosphite (Irgafos ®< TNPP, BASF SE, [CAS 26523-78-4]), (2,4,6-tri-t-butylphenol)2-butyl-2-ethyl-1,3-propanediol phosphite (Ultranox ®< 641, Chemtura, [CAS 161717-32-4]), Hostanox ®< P-EPQ [CAS 119345-01-6] or polymeric phosphorous acid esters according to EP 1 523 520 B1 - preferably polymeric phosphorous acid esters,which contain oxetane groups and of which 50% or more of all molecules contain at least four monomers from the group of a di- or polyhydric phenol and / or esters of phosphorous acid.

[0067] According to the invention, preference is given to compositions, molding compositions to be produced therefrom and products based thereon containing a) 100 parts by mass of at least one polyester, b) 70 to 600 parts by mass, preferably 125 to 400 parts by mass, particularly preferably 150 to 300 parts by mass, of Al 2 O 3 surface-treated with at least one aminosilane and / or epoxysilane, and c) 0.017 to 12.5 parts by mass of at least one phosphite stabilizer from the group tris(2,4-ditert-butylphenyl)phosphite, bis(2,4-di-tert-butylphenyl)pentaerythritol diphosphite, bis(2,6-di-tert-butyl-4-methylphenyl)pentaerythritol diphosphite, bis(2,4-dicumylphenyl)pentaerythritol diphosphite, tris(nonylphenyl)phosphite, (2,4,6-tri-t-butylphenol)2-butyl-2-ethyl-1,3-propanediol phosphite, tetrakis(2,4-di-tert-butylphenyl)-1,1-biphenyl-4,4'-diylbisphosphonite and polymeric phosphorous acid esters containing oxetane groups and of which 50% or more of all molecules contain at least four monomers from the group of a di- or polyhydric phenol and / or esters of phosphorous acid.

[0068] Particularly preferred phosphite stabilizer is Hostanox®< P-EPQ [CAS 119345-01-6] from Clariant International Ltd., Muttenz, Switzerland. This contains tetrakis(2,4-di-tert-butylphenyl)-1,1-biphenyl-4,4'-diylbisphosphonite [CAS 38613-77-3], which is particularly preferred as component c) according to the invention.

[0069] Particularly preferred according to the invention are compositions, molding compositions to be produced therefrom and products based thereon containing a) 100 parts by mass of at least one polyester, b) 70 to 600 parts by mass, preferably 125 to 400 parts by mass, particularly preferably 150 to 300 parts by mass, of Al 2 O 3 surface-treated with at least one aminosilane and / or epoxysilane, and c) 0.017 to 12.5 parts by mass of tetrakis(2,4-di-tert-butylphenyl)-1,1-biphenyl-4,4'-diylbisphosphonite.

[0070] The invention particularly preferably relates to a method for reducing the abrasiveness of thermally conductive polyester compositions, characterized in that the Al 2 O 3 to be used, the surface of which is surface-treated with at least one amino- and / or epoxysilane, is brought into contact with a polyester composition which contains at least one phosphite stabilizer from the group tris(2,4-ditert-butylphenyl)phosphite, bis(2,4-di-tert-butylphenyl)pentaerythritol diphosphite, bis(2,6-di-tert-butyl-4-methylphenyl)pentaerythritol diphosphite, bis(2,4-dicumylphenyl)pentaerythritol diphosphite, tris(nonylphenyl)phosphite, (2,4,6-tri-t-butylphenol)2-butyl-2-ethyl-1,3-propanediol phosphite, Tetrakis(2,4-di-tert-butylphenyl)-1,1-biphenyl-4,4'-diylbisphosphonite and polymeric phosphorous acid esters,which contain oxetane groups and of which 50% or more of all molecules contain at least four monomers from the group of a di- or polyhydric phenol and / or esters of phosphorous acid.

[0071] The invention further relates to the use of Al 2 O 3 surface-treated with at least one aminosilane and / or epoxysilane for reducing abrasion in processing machines for processing polyester compositions, wherein the aluminum oxide is used in combination with at least one phosphite stabilizer from the group tris(2,4-ditert-butylphenyl)phosphite, bis(2,4-di-tert-butylphenyl)pentaerythritol diphosphite, bis(2,6-di-tert-butyl-4-methylphenyl)pentaerythritol diphosphite, bis(2,4-dicumylphenyl)pentaerythritol diphosphite, tris(nonylphenyl)phosphite, (2,4,6-tri-t-butylphenol)2-butyl-2-ethyl-1,3-propanediol phosphite, Tetrakis(2,4-di-tert-butylphenyl)-1,1-biphenyl-4,4'-diylbisphosphonite and polymeric phosphorous acid esters containing oxetane groups and of which 50% or more of all molecules contain at least four monomers from the group of a di- or polyhydric phenol and / or esters of phosphorous acid. Component d)

[0072] In one embodiment, at least one mold release agent or at least one nucleating agent is used as component d).

[0073] Nucleating agents preferably used as component d) according to the invention are sodium or calcium phenylphosphinate, silicon dioxide, or talc, particularly preferably talc. Talc is a magnesium silicate hydrate with the chemical composition Mg 3 [Si 4 O 10 (OH) 2 ].

[0074] Mold release agents preferably used as component d) according to the invention are long-chain fatty acids, their salts, as well as their ester derivatives or amide derivatives, montan wax esters, and low-molecular-weight polyethylene or polypropylene waxes in oxidized and non-oxidized form.

[0075] The preferred fatty acid is stearic acid. Preferred fatty acid salts are calcium stearate or zinc stearate. Preferred ester derivatives of fatty acids are stearyl stearate or glycerol tristearate. Preferred montan wax esters are esters of montanic acids with polyfunctional alcohols, especially with ethylene glycol.

[0076] Preferred lubricants and / or mold release agents according to the invention are also the group of esters or amides of saturated or unsaturated aliphatic carboxylic acids having 8 to 40 C atoms with aliphatic saturated alcohols or amines having 2 to 40 C atoms.

[0077] In a further preferred embodiment, the molding compositions according to the invention contain mixtures of the above-mentioned lubricants and / or mold-release agents. The montan wax esters and their salts, which are particularly preferred, improve the flowability of plastics such as polyesters solely through their internal lubrication effect, without reducing the molecular weight of the polymer. Particularly preferred are esters of montan acid with multifunctional alcohols, which are offered by Clariant GmbH as Licowax®< E [CAS 73138-45-1].

[0078] In one embodiment, the present invention relates to compositions and molding materials to be produced therefrom and products based thereon containing a) 100 parts by mass of at least one polyester, b) 70 to 600 parts by mass, preferably 125 to 400 parts by mass, particularly preferably 150 to 300 parts by mass, of Al 2 O 3 surface-treated with at least one aminosilane and / or epoxysilane, c) 0.017 to 12.5 parts by mass of at least one phosphite stabilizer selected from the group tris(2,4-ditert-butylphenyl)phosphite, bis(2,4-di-tert-butylphenyl)pentaerythritol diphosphite, bis(2,6-di-tert-butyl-4-methylphenyl)pentaerythritol diphosphite, bis(2,4-dicumylphenyl)pentaerythritol diphosphite, tris(nonylphenyl)phosphite, (2,4,6-tri-t-butylphenol)2-butyl-2-ethyl-1,3-propanediol phosphite, tetrakis(2,4-di-tert-butylphenyl)-1,1-biphenyl-4,4'-diylbisphosphonite and polymeric phosphorous acid esters containing oxetane groups and of which 50% or more of all molecules contain at least four monomers from the group of a di- or polyhydric phenol and / or esters of phosphorous acid, and d) 0,001 to 10 parts by mass of at least one ester of montanic acid with multifunctional alcohols or talc.

[0079] According to the invention, preference is given to compositions, molding compositions to be produced therefrom and products based thereon containing a) 100 parts by mass of at least one polyester, b) 70 to 600 parts by mass, preferably 125 to 400 parts by mass, particularly preferably 150 to 300 parts by mass, of Al 2 O 3 surface-treated with at least one aminosilane and / or epoxysilane, and c) 0.017 to 12.5 parts by mass of tetrakis(2,4-di-tert-butylphenyl)-1,1-biphenyl-4,4'-diylbisphosphonite, and d) 0.001 to 10 parts by mass of at least one ester of montanic acid with multifunctional alcohols or talc.

[0080] In one embodiment, the present invention relates to compositions and molding materials to be produced therefrom and products based thereon, wherein a) 100 parts by mass of PBT, b) 70 to 600 parts by mass, preferably 125 to 400 parts by mass, particularly preferably 150 to 300 parts by mass, of Al 2 O 3 surface-treated with at least one aminosilane and / or epoxysilane, c) 0.017 to 12.5 parts by mass of at least one phosphite stabilizer selected from the group tris(2,4-ditert-butylphenyl)phosphite, bis(2,4-di-tert-butylphenyl)pentaerythritol diphosphite, bis(2,6-di-tert-butyl-4-methylphenyl)pentaerythritol diphosphite, bis(2,4-dicumylphenyl)pentaerythritol diphosphite, tris(nonylphenyl)phosphite, (2,4,6-tri-t-butylphenol)2-butyl-2-ethyl-1,3-propanediol phosphite, tetrakis(2,4-di-tert-butylphenyl)-1,1-biphenyl-4,4'-diylbisphosphonite and polymeric phosphorous acid esters containing oxetane groups and of which 50% or more of all molecules contain at least four monomers from the group of a di- or polyhydric phenol and / or esters of phosphorous acid, d) 0,0.001 to 10 parts by mass of at least one ester of montanic acid with multifunctional alcohols or talc, and e) 0.001 to 150 parts by mass of at least one further additive different from components b), c) and d).

[0081] According to the invention, preference is given to compositions, molding compositions to be produced therefrom and products based thereon containing a) 100 parts by mass of PBT, b) 70 to 600 parts by mass, preferably 125 to 400 parts by mass, particularly preferably 150 to 300 parts by mass, of Al 2 O 3 surface-treated with at least one aminosilane and / or epoxysilane, and c) 0.017 to 12.5 parts by mass of tetrakis(2,4-di-tert-butylphenyl)-1,1-biphenyl-4,4'-diylbisphosphonite, and d) 0.001 to 10 parts by mass of at least one ester of montanic acid with multifunctional alcohols and talc.

[0082] In one embodiment, the present invention relates to compositions and molding materials to be produced therefrom and products based thereon, wherein a) 100 parts by mass of PBT, b) 70 to 600 parts by mass, preferably 125 to 400 parts by mass, particularly preferably 150 to 300 parts by mass, of Al 2 O 3 surface-treated with at least one aminosilane, c) 0.017 to 12.5 parts by mass of at least one phosphite stabilizer selected from the group tris(2,4-ditert-butylphenyl)phosphite, bis(2,4-di-tert-butylphenyl)pentaerythritol diphosphite, bis(2,6-di-tert-butyl-4-methylphenyl)pentaerythritol diphosphite, bis(2,4-dicumylphenyl)pentaerythritol diphosphite, tris(nonylphenyl)phosphite, (2,4,6-tri-t-butylphenol)2-butyl-2-ethyl-1,3-propanediol phosphite, tetrakis(2,4-di-tert-butylphenyl)-1,1-biphenyl-4,4'-diylbisphosphonite and polymeric phosphorous acid esters containing oxetane groups and of which 50% or more of all molecules contain at least four monomers from the group of a di- or polyhydric phenol and / or esters of phosphorous acid, d) 0,0.001 to 10 parts by mass of at least one ester of montanic acid with multifunctional alcohols and talc, and e) 0.001 to 150 parts by mass of at least one further additive other than components b), c) and d) are used.

[0083] In one embodiment, the present invention relates to compositions and molding materials to be produced therefrom and products based thereon, wherein a) 100 parts by mass of PBT, b) 70 to 600 parts by mass, preferably 125 to 400 parts by mass, particularly preferably 150 to 300 parts by mass, of Al 2 O 3 surface-treated with at least one aminosilane, c) 0.017 to 12.5 parts by mass of tetrakis (2,4-di-tert-butylphenyl)-1,1-biphenyl-4,4'-diylbisphosphonite, d) 0.001 to 10 parts by mass of at least one ester of montanic acid with multifunctional alcohols and talc, and e) 0.001 to 150 parts by mass of at least one further additive different from components b), c) and d).

[0084] In one embodiment, component d) can be omitted. In this case, a composition, molding compound, or product contains components a), b), c), and e). Component e)

[0085] Optionally, further additives to be used as component e) are substances other than components b), c), and d) from the group of UV stabilizers, gamma-ray stabilizers, hydrolysis stabilizers, antistatic agents, emulsifiers, plasticizers, processing aids, impact modifiers or elastomer modifiers, fillers and reinforcing agents, lubricants, dyes, flame retardants, or pigments. These and other suitable additives are state of the art and can be found by the skilled person, for example, in the Plastics Additives Handbook, 5th Edition, Hanser-Verlag, Munich, 2001, pages 80-84, 546-547, 688, 872-874, 938, 966. The additives to be used as component e) can be used alone or in a mixture or in the form of masterbatches.

[0086] UV stabilizers preferably used as component e) according to the invention are substituted resorcinols, salicylates, benzotriazoles or benzophenones.

[0087] Impact modifiers or elastomer modifiers to be used as component e) according to the invention are copolymers preferably composed of at least two monomers from the group consisting of ethylene, propylene, butadiene, isobutene, isoprene, chloroprene, vinyl acetate, styrene, acrylonitrile, and acrylic acid esters or methacrylic acid esters with 1 to 18 carbon atoms in the alcohol component. The copolymers may contain compatibilizing groups, preferably maleic anhydride or epoxide.

[0088] Dyes or pigments to be used according to the invention as component e) are inorganic pigments, particularly preferably titanium dioxide, ultramarine blue, iron oxide, zinc sulfide, or carbon black, as well as organic pigments, particularly preferably phthalocyanines, quinacridones, perylenes, and dyes, particularly preferably nigrosine or anthraquinones as colorants, as well as other colorants. Carbon black and / or nigrosine are particularly preferred.

[0089] Fillers and reinforcing materials to be used as component e) according to the invention are fibrous, acicular, or particulate fillers and reinforcing materials other than aluminum oxide. Particular preference is given to carbon fibers, glass spheres, amorphous silica, calcium silicate, calcium metasilicate, magnesium carbonate, kaolin, calcined kaolin, chalk, powdered quartz, mica, phlogopite, barium sulfate, feldspar, wollastonite, kyanite or aluminum silicate, montmorillonite, magnesium oxide, zinc oxide, boron nitride, graphite, carbon nanotubes, graphene, iron oxides, ferrites, magnetite, copper, aluminum, titanium dioxide, or glass fibers, very particularly preferably glass fibers, especially preferably glass fibers made of E-glass. In a preferred embodiment, the fibrous or particulate reinforcing materials are provided with suitable surface modifications, in particular surface modifications containing silane compounds, for improved compatibility with thermoplastics.

[0090] Thermal conductivity additives to be used according to the invention as component e) are preferably selected from the group consisting of aluminum silicate, in particular kyanite, montmorillonite, magnesium oxide, zinc oxide, boron nitride, graphite, carbon nanotubes, graphene, iron oxides, ferrites, magnetite, copper, aluminum and titanium dioxide.

[0091] Flame retardants to be used according to the invention as component e) are preferably mineral flame retardants, nitrogen-containing flame retardants or phosphorus-containing flame retardants.

[0092] Preferred nitrogen-containing flame retardants are the reaction products of trichlorotriazine, piperazine, and morpholine [CAS 1078142-02-5], particularly MCA PPM Triazine HF from MCA Technologies GmbH, Biel-Benken, Switzerland, as well as melamine cyanurate and condensation products of melamine such as melem, melam, melon, and higher-condensed compounds of this type. Preferred inorganic nitrogen-containing compounds are ammonium salts.

[0093] Furthermore, salts of aliphatic and aromatic sulfonic acids and mineral flame retardant additives, preferably aluminum hydroxide, Ca-Mg carbonate hydrates (e.g. DE-A 4 236 122 ) or magnesium hydroxide can be used as a flame retardant for component e).

[0094] Among the mineral flame retardants, magnesium hydroxide is particularly preferred. Magnesium hydroxide [CAS 1309-42-8] can be contaminated due to its origin and method of production. Typical impurities include silicon-, iron-, calcium-, and / or aluminum-containing species, which can be embedded, for example, in the form of oxides in the magnesium hydroxide crystals. The surface of the magnesium hydroxide used according to the invention as a flame retardant in component e) can be uncoated or coated, where a coating is understood to be an impregnating liquid for imparting specific properties to the surface of a material. The magnesium hydroxide is preferably coated with coatings based on stearates or aminosiloxanes, particularly preferably with aminosiloxanes.Magnesium hydroxide to be used preferably has an average particle size d50 in the range from 0.5 µm to 6 µm, with a d50 in the range from 0.7 µm to 3.8 µm being preferred and a d50 in the range from 1.0 µm to 2.6 µm being particularly preferred, and the average particle size is determined by laser diffractometry in accordance with ISO 13320. Magnesium hydroxide types suitable according to the invention are, for example, Magnifin®< H5IV from Martinswerk GmbH, Bergheim, Germany, or Hidromag®< Q2015 TC from Penoles, Mexico City, Mexico.

[0095] Also suitable for component e) are flame retardant synergists from the group of oxygen-, nitrogen- or sulphur-containing metal compounds, with zinc-free compounds, in particular molybdenum oxide, magnesium oxide, magnesium carbonate, calcium carbonate, calcium oxide, titanium nitride, magnesium nitride, calcium phosphate, calcium borate, magnesium borate or mixtures thereof, being particularly preferred.

[0096] In an alternative embodiment, zinc-containing compounds can also be used as component e) - if required. These preferably include zinc oxide, zinc borate, zinc stannate, zinc hydroxystannate, zinc sulfide, and zinc nitride, or mixtures thereof.

[0097] Preferred phosphorus-containing flame retardants to be used as component e) are organic metal phosphinates, in particular aluminum tris(diethylphosphinate), aluminum salts of phosphonic acid, red phosphorus, inorganic metal hypophosphites, in particular aluminum hypophosphite, other metal phosphonates, in particular calcium phosphonate, derivatives of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxides (DOPO derivatives), resorcinol bis(diphenyl phosphate) (RDP), including oligomers, and bisphenol A bisdiphenyl phosphate (BDP) including oligomers, furthermore melamine pyrophosphate and melamine polyphosphate, furthermore melamine poly(aluminum phosphate), melamine poly(zinc phosphate) or phenoxyphosphazene oligomers and mixtures thereof.

[0098] Other flame retardants to be used as component e) are carbon formers, particularly preferably phenol-formaldehyde resins, polycarbonates, polyimides, polysulfones, polyethersulfones or polyether ketones and anti-drip agents, in particular tetrafluoroethylene polymers.

[0099] The flame retardants to be used as component e) can be added in pure form, as well as via masterbatches or compacts.

[0100] In an alternative embodiment, halogen-containing flame retardants can also be used as component e). Preferred halogen-containing flame retardants are commercially available organic halogen compounds, particularly preferably ethylene-1,2-bistetrabromophthalimide, decabromodiphenylethane, tetrabromobisphenol A epoxy oligomer, tetrabromobisphenol A oligocarbonate, tetrachlorobisphenol A oligocarbonate, polypentabromobenzyl acrylate, brominated polystyrene, or brominated polyphenylene ethers, which can be used alone or in combination with synergists, in particular antimony trioxide or antimony pentoxide. Among the halogen-containing flame retardants, brominated polystyrene is particularly preferred. Brominated polystyrene is commercially available in various product grades. Examples of this are Firemaster ®< PBS64 from Lanxess, Cologne, Germany and Saytex ®< HP-3010 from Albemarle, Baton Rouge, USA.

[0101] Among the flame retardants to be used as component e), aluminum tris(diethylphosphinate)] [CAS 225789-38-8] and the combination of aluminum tris(diethylphosphinate) and melamine polyphosphate or the combination of aluminum tris(diethylphosphinate) and at least one aluminum salt of phosphonic acid are very particularly preferred, the latter combination being particularly preferred.

[0102] Suitable aluminum tris(diethylphosphinate)s include Exolit®< OP1230 or Exolit®< OP1240 from Clariant International Ltd., Muttenz, Switzerland. Melamine polyphosphate is commercially available in various product grades. Examples include Melapur®< 200 / 70 from BASF, Ludwigshafen, Germany, and Budit®< 3141 from Budenheim, Budenheim, Germany.

[0103] Preferred aluminum salts of phosphonic acid are selected from the group of primary aluminum phosphonate [Al(H 2 PO 3 ) 3 ], basic aluminum phosphonate [Al(OH)H 2 PO 3 ) 2 ·2H 2 O], Al 2 (HPO 3 ) 3 ·x Al 2 O 3 ·n H 2 O with x in the range from 2.27 to 1 and n in the range from 0 to 4, Al 2 (HPO 3 ) 3 · (H 2 O) q (Z1) with q in the range from 0 to 4, in particular aluminum phosphonate tetrahydrate [Al 2 (HPO 3 ) 3 ·4H 2 O] or secondary aluminum phosphonate [Al 2 (HPO 3 ) 3 ], Al 2 M z (HPO 3 ) y (OH) v · (H 2 O) w (Z2) wherein M is at least one alkali metal ion and z is in the range from 0.01 to 1.5, y is in the range from 2.63 - 3.5, v is in the range from 0 to 2 and w is in the range from 0 to 4, and Al 2 (HPO 3 ) u (H 2 PO 3 ) t · (H 2 O) s (Z3) where u is in the range from 2 to 2.99, t is in the range from 2 to 0.01 and s is in the range from 0 to 4, where in formula (Z2) z, y and v and in formula (Z3) u and t can only assume numbers such that the corresponding aluminum salt of phosphonic acid as a whole is uncharged. Preferred alkali metals in formula (Z2) are sodium and potassium.The described aluminum salts of phosphonic acid can be used individually or in mixtures. Particularly preferred aluminum salts of phosphonic acid are selected from the group of primary aluminum phosphonate [Al(H 2 PO 3 ) 3 ], secondary aluminum phosphonate [Al 2 (HPO 3 ) 3 ], basic aluminum phosphonate [Al(OH)H 2 PO 3 ) 2 ·2H 2 O], aluminum phosphonate tetrahydrate [Al 2 (HPO 3 ) 3 ·4H 2 O] and Al 2 (HPO 3 ) 3 ·xAl 2 O 3 ·n H 2 O with x in the range from 2.27 to 1 and n in the range from 0 to 4. Very particular preference is given to secondary aluminum phosphonate [Al 2 (HPO 3 ) 3 , [CAS 71449-76-8] and secondary aluminum phosphonate tetrahydrate [Al 2 (HPO 3 ) 3 ·4H 2 O, [CAS 156024-71-4], particularly preferred is secondary aluminum phosphonate [Al 2 (HPO 3 ) 3 ]. The preparation of the aluminum salts of phosphonic acid used as flame retardants of component e) is described, for example, in WO 2013 / 083247 A1.The present invention further provides a process for producing molding compositions according to the invention, wherein components a) to c) and optionally d) and optionally e) are mixed or blended in appropriate mass proportions in at least one mixing unit. The components to be used are preferably kneaded, compounded, extruded, or rolled to form a molding composition. This is preferably carried out at a temperature in the range from 230 to 400°C, particularly preferably by compounding on a co-rotating twin-screw extruder or Buss kneader. It may be advantageous to premix individual components.

[0104] The present application also relates to the use or processing of the molding compositions to be produced from the components to be used according to the invention in the extrusion process, in blow molding processes or in injection molding for the production of products, preferably molded parts or semi-finished products.

[0105] Processes according to the invention for producing products by means of extrusion, blow molding or injection molding are carried out at melt temperatures in the range from 230 to 330°C, preferably from 250 to 300°C and optionally additionally at pressures of not more than 2500 bar, preferably at pressures of not more than 2000 bar, particularly preferably at pressures of not more than 1500 bar and very particularly preferably at pressures of not more than 750 bar.

[0106] During extrusion, also known as extrusion, solid to viscous, curable thermoplastic molding materials are continuously pressed out of a molding opening, preferably called a die, matrix, or mouthpiece, under pressure. This produces products with the cross-section of the opening in theoretically any length ( http: / / de.wikipedia.org / wiki / Extrusion_(Verfahrenstechnik ). The basic process steps of the profile extrusion process, a form of extrusion, are: 1. Plasticizing and preparing the thermoplastic melt in an extruder, 2. Extrusion of the thermoplastic melt strand through a calibration sleeve which has the cross-section of the profile to be extruded, 3. Cooling of the extruded profile in a calibration table, 4. Further transport of the profile with a take-off behind the calibration table, 5. Cutting of the previously endless profile to length in a cutting system, 6. Collecting the cut profiles on a collection table.

[0107] A description of the extrusion of polyalkylene terephthalates is given in Kunststoff-Handbuch Volume VIII, Polyester, Carl Hanser Verlag, Munich 1973, pages 730-731 .

[0108] The blow molding process is used, for example, in http: / / www.blasformen.com / In blow molding, the first process step involves drawing in plastic granules through a heated extruder, compressing them, degassing them, heating them, plasticizing them, and homogenizing them into a plastic strand. In the next step, the plastic mass is fed into a die head flanged to the extruder. There, the plastic melt is formed into a tube that exits vertically downwards from a nozzle. The tube diameter is adapted to the product to be manufactured using mandrel and nozzle standards of different sizes that are flanged to the die head. The tube thickness and the resulting weight of the blow-molded parts are predetermined by selecting different diameter differences between the mandrel and nozzle.

[0109] Injection molding is characterized by the fact that the raw material, i.e., the thermoplastic molding compound to be processed containing the components to be used according to the invention, preferably in granular form, is melted (plasticized) in a heated cylindrical cavity and injected as a molding compound under pressure into a temperature-controlled cavity. After the compound has cooled (solidified), the injection-molded part is demolded.

[0110] A distinction is made 1. Plasticizing / melting 2. Injection phase (filling process) 3. Holding pressure phase (due to thermal contraction during crystallization) 4. Demolding.

[0111] An injection molding machine consists of a clamping unit, the injection unit, the drive, and the control system. The clamping unit includes fixed and movable mold clamping plates, a face plate, and the columns and drive of the movable mold clamping plate (toggle joint or hydraulic clamping unit).

[0112] An injection unit comprises the electrically heated cylinder, the screw drive (motor, gear), and the hydraulics for moving the screw and injection unit. The injection unit's task is to melt, meter, inject, and repress the powder or granules (due to contraction). The problem of melt backflow within the screw (leakage flow) is solved by non-return valves.

[0113] In the injection mold, the incoming melt of the molding compound to be processed, which contains the components used according to the invention, is then dissolved and cooled, thus producing the component to be manufactured. Two mold halves are always required for this. Injection molding distinguishes between the following functional complexes: Gate system Mold-forming inserts Ventilation Machine and force absorption Demolding system and motion transmission Tempering

[0114] In contrast to injection molding, extrusion involves the continuous strand of the molding compound used according to the invention being fed into the extruder. The extruder is a machine for manufacturing products based on thermoplastic moldings. A distinction is made between single-screw extruders and twin-screw extruders, as well as their respective subgroups: conventional single-screw extruders, feed-effect single-screw extruders, counter-rotating twin-screw extruders, and co-rotating twin-screw extruders.

[0115] Extrusion systems for producing profiles consist of: extruder, profile tool, calibration, cooling section, caterpillar and roller take-off, separating device and tipping chute.

[0116] The present invention consequently also relates to products, preferably molded parts, molded bodies or semi-finished products, obtainable by extrusion or injection molding of the molding compositions according to the invention containing at least components a), b) and c) and optionally d) and optionally e).

[0117] The present invention relates to the use of electrically insulating but thermally conductive products, preferably molded parts, molded bodies or semi-finished products, produced by extrusion or injection molding from molding compositions containing at least components a), b) and c) and optionally d) and optionally e), for electrical or electronic components. These products according to the invention can preferably be used in the automotive, electrical, electronics, telecommunications, solar, information technology, computer industries, in the household, sports, medicine or in the entertainment industry. In particular, products according to the invention can be used for applications in which improved thermal conduction and good mechanical properties are necessary. For such applications, use for molded parts in electrical engineering and in vehicles, in particular components in motor vehicles (MVs) is preferred.

[0118] The present invention therefore also relates to the use of the thermoplastic molding compositions according to the invention for producing molded parts and semi-finished products and, in turn, products to be produced therefrom with increased thermal conductivity, preferably molded parts for motor vehicles. Examples:

[0119] The individual components a), b), c), and optionally d), and optionally e) were mixed in a twin-screw extruder of the ZSK 26 Compounder type from Coperion Werner & Pfleiderer (Stuttgart, Germany) at a temperature of approximately 270 °C, extruded as a strand into a water bath, cooled to pelletizable temperature, and pelletized. The pellets were dried at 120 °C in a vacuum drying cabinet for 4 hours.

[0120] The granules were then processed on an Arburg SG370-173732 injection molding machine at melt temperatures ranging from 270 to 300°C and mold temperatures ranging from 80 to 100°C into shoulder bars (4 mm thick according to ISO 528), flat bars (80 mm x 10 mm x 4 mm), and sheets measuring 60 mm x 40 mm x 2 mm. The sheets were then milled to dimensions of 12.7 mm x 12.7 mm x 2 mm.

[0121] The mechanical properties of the products manufactured from the molding compounds were determined by tensile testing according to ISO 527 and impact testing according to ISO 180-1U; thermal conductivity was determined on plates measuring 12.7 mm x 12.7 mm x 2 mm according to ISO 22007-4.

[0122] The wear behaviour of processing machines, hereinafter referred to as "abrasion", in particular extruders and injection moulding machines, was determined based on the wear test of the DKI Darmstadt ( Publication FG Kunststoffe, project number 12245 - New wear equipment, Project No. AiF 12245N (DKI 18 / 0-87), Duration 01.12.1999 to 28.02.2003)The abrasion was measured gravimetrically based on the material removal caused by the injection molding of 100 shots (1 shot = 3D) of a polyester-based composition at an injection speed of v = 30 mm / s and a screw diameter of D = 35 mm, at a melt temperature of 270°C, caused by a nozzle consisting of two metal plates (steel: 1.2738) with the dimensions 12 x 12 mm and a slot width of 0.4 mm. Materials used:

[0123] Component a): PBT, linear with a viscosity number determined in a 0.5 wt.% solution in a phenol / o-dichlorobenzene mixture (1 / 1) at 25°C, according to ISO1628 of 94 ml / g.

[0124] Component b): monomodal aluminum oxide CT 3000 SG from Almatis GmbH, surface-treated with 3-aminopropyltriethoxysilane, with a d50 value of 0.5 µm and a BET surface area of ​​7.8 m 2 / g. Phosphite stabilizer: Hostanox ®< P-EPQ from Clariant GmbH Talc: Microtalcum Mistron ®< R10 from Imerys Montan wax ester: Licowax ®< E from Clariant GmbH Surface treatment with 3-aminopropyltriethoxysilane

[0125] The aminosilane was applied to the aluminum oxide in the manner described in WO 2009 / 156342 A1, by first placing 0.6 g of 3-aminopropyltriethoxysilane per 100 g of Al 2 O 3 in deionized water (DE = fully demineralized water) to form silanol (DE = 250 ml of deionized water per 100 g of Al 2 O 3 ) and stirring at 25 °C (room temperature) for 30 minutes. The aluminum oxide was then added, the suspension was stirred at 80 °C, the surface-treated aluminum oxide was filtered off with suction, and washed with deionized water. The surface-treated aluminum oxide was then dried for 5 hours at temperatures of approximately 120 °C, and then annealed for 30 minutes at 200 °C.

[0126] The Table 1The composition shown was processed as described above, with the data being in weight percent. Table 1 Ingredient Example 1 polyester 49,5 aminosilane-treated aluminum oxide 50 Phosphite stabilizer 0,1 Microtalc 0,1 Montan wax esters 0,3 Measurement result Impact strength IZOD unnotched [kJ / m 2< ] 41 Elongation at break [%] 2,3 Thermal conductivity perpendicular to the flow direction of the specimen [W / mK] 0,5 Thermal conductivity in the flow direction of the specimen [W / mK] 0,6 Abrasion [mg] 25 Abrasion test

[0127] The abrasion test was carried out according to the specification in the Publication FG Kunststoffe, "New and further development of model testing methods for corrosive / abrasive wear in plastics processing", Project No. AiF 12245N (DKI 18 / 0-87), duration 01.12.1999 to 28.02.2003 (see description) was carried out, and by differential weighing the metal plates before and after the test, a material removal of 25 mg was determined for Example 1. A material removal of only 25 mg represents low abrasion. For the purposes of this invention, abrasion with material removal of <200 mg is considered acceptable.

[0128] The mechanical properties with an elongation at break of 2.3% measured according to ISO527 on freshly molded test specimens and an impact strength of 41 kJ / mol measured according to ISO180-1U on freshly molded test specimens are good mechanical properties in the sense of the present invention and exceed the requirements set out in the task of 1.5% elongation at break measured according to ISO527 on freshly molded test specimens at 150 parts by mass of aluminum oxide based on 100 parts by mass of polyester and an impact strength of 18 kJ / m 2< measured according to ISO180-1U on freshly molded test specimens at 150 parts by mass of aluminum oxide based on 100 parts by mass of polyester significantly and a deterioration that does not occur compared to the prior art.

[0129] The thermal conductivity of 0.5 W / mK measured perpendicular to the flow direction of the test specimen according to ISO 22007-4 and 0.6 W / mK measured in the flow direction of the test specimen according to ISO 22007-4 are acceptable thermal conductivities in the sense of the present invention and exceed the requirements of at least 0.4 W / mK set out in the task of the present invention.

Claims

1. Compositions, moulding materials producible therefrom and articles of manufacture based thereupon containing a) 100 parts by mass of at least one polyester, b) 70 to 600 parts by mass of aluminium oxide surface-treated with at least one aminosilane and / or epoxysilane, c) 0.017 to 12.5 parts by mass of at least one phosphite stabilizer.

2. Compositions and moulding materials producible therefrom and articles of manufacture based thereupon according to Claim 1, characterized in that for the surface treatment of component b) at least one aminosilane of general empirical formula         (RO)3-Si-(CH2)n-X is employed, wherein R represents an organic radical selected from the group consisting of methyl, ethyl, isopropyl and methoxymethyl, n represents an integer from 0 to 12 (end values included), and X represents a radical NR1R2 and R1 and R2 each independently of one another represent hydrogen, a C1-C6-alkyl radical or a C6-C9-cycloalkyl radical.

3. Compositions and moulding materials and articles of manufacture producible therefrom according to Claim 1 or 2, characterized in that for the surface-treatment of the aluminium oxide at least one aminosilane from the group of 3-aminopropyltriethoxysilane, 3-aminopropyltrimethoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, N-(2-aminoethyl)-3-aminopropyltriethoxysilane, 3-(N-cyclohexylamino)propyltrimethoxysilane and diethylaminomethyltriethoxysilane is employed.

4. Compositions and moulding materials producible therefrom and articles of manufacture based thereupon according to Claim 1, characterized in that for the surface treatment of the aluminium oxide at least one epoxysilane of general empirical formula         E-R3-Si(R4)a-(OR5)3-a is employed, wherein E represents a glycidyl group, a glycidyloxy group or an epoxycyclohexyl group or a mixture thereof, R3 represents a C1-C4-alkylene group, R4 and R5 each independently represent C1-C4-alkyl groups and a represents 0, 1 or 2.

5. Compositions and moulding materials producible therefrom and articles of manufacture based thereupon according to either of Claims 1 or 4, characterized in that for the surface treatment of the aluminium oxide at least one epoxysilane from the group of 2-(3,4-epoxycyclohexyl)-ethyltrimethoxysilane, (3-glycidoxypropyl)trimethoxysilane, (3-glycidoxypropyl)methyldiethoxysilane, 5,6-epoxyhexyltriethoxysilane, 2-(3,4-epoxycyclohexyl)ethylmethyldiethoxysilane, (3-glycidoxypropyl)triethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltriethoxysilane and (3-glycidoxypropyl)methyldimethoxysilane is employed.

6. Compositions and moulding materials producible therefrom and articles of manufacture based thereupon according to one or more of Claims 1 to 5, characterized in that at least one phosphite stabilizer from the group of tris(2,4-ditert-butylphenyl)phosphite, bis(2,4-di-tert-butylphenyl)pentaerythritol diphosphite, bis(2,6-di-ter-butyl-4-methylphenyl)pentaerythritol diphosphite, bis(2,4-dicumylphenyl)pentaerythritol diphosphite, tris(nonylphenyl)phosphite, (2,4,6-tri-t-butylphenol)2-butyl-2-ethyl-1,3-propanediol phosphite, tetrakis(2,4-di-tert-butylphenyl)-1,1-biphenyl-4,4'-diylbisphosphonite and polymeric phosphorus acid esters containing oxetane groups of which 50% or more of all molecules contain at least four monomers from the group of a di- or polyhydric phenol and / or ester of phosphorous acid is employed.

7. Compositions and moulding materials producible therefrom and articles of manufacture based thereupon according to one or more of Claims 1 to 6, characterized in that they additionally contain d) 0.001 to 10 parts by mass of at least one demoulding agent.

8. Compositions and moulding materials producible therefrom and articles of manufacture based thereupon according to one or more of Claims 1 to 6, characterized in that they additionally contain d) 0.001 to 10 parts by mass of at least one nucleating agent, preferably talc.

9. Compositions and moulding materials producible therefrom and articles of manufacture based thereupon according to one or more of Claims 1 to 6, characterized in that they additionally contain d) 0.001 to 10 parts by mass of at least one nucleating agent and at least one demoulding agent, wherein talc is preferably employed as the nucleating agent.

10. Compositions and moulding materials producible therefrom and articles of manufacture based thereupon according to Claims 7 and 9, characterized in that long-chain fatty acids, salts thereof and also ester derivatives or amide derivatives thereof, montan wax esters and salts thereof and low molecular weight polyethylene / polypropylene waxes in oxidized and non-oxidized form are employed as demoulding agents.

11. Compositions and moulding materials producible therefrom and articles of manufacture based thereupon according to Claim 10, characterized in that esters or amides of saturated or unsaturated aliphatic carboxylic acids having 8 to 40 carbon atoms with aliphatic saturated alcohols or amines having 2 to 40 carbon atoms are employed as demoulding agents.

12. Compositions and moulding materials and articles of manufacture producible therefrom according to one or more of Claims 1 to 11, characterized in that α-Al2O3 is employed as component b).

13. Compositions and moulding materials and articles of manufacture producible therefrom according to one or more of Claims 1 to 12, characterized in that an aluminium oxide having a monomodal particle size distribution is employed as component b).

14. Process for reducing the abrasiveness of thermally conductive, electrically insulating polyester compositions and moulding materials producible therefrom, characterized in that aluminium oxide which has been surface-treated with at least one aminosilane and / or epoxysilane is contacted with a polyester composition.

15. Use of aluminium oxide surface-treated with at least one aminosilane and / or epoxysilane for reducing abrasion in processing machinery in the processing of polyester compositions and polyester moulding materials based thereupon.