METHOD FOR PRODUCING A POWDER BASED ON A NICKEL BASE ALLOY

DE502020009375D1Active Publication Date: 2024-10-17VDM METALS INTERNATIONAL GMBH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
DE502020009375
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-06-26
Filing Date
2020-07-01
Publication Date
2024-10-17
Estimated Expiration
2040-07-01

AI Technical Summary

Technical Problem

Current methods for producing nickel-based powders for additive manufacturing lack efficiency in achieving the desired properties of corrosion resistance, mechanical strength, and high-temperature strength, while also being cost-effective and meeting specific particle size, shape, and flowability requirements.

Method used

A process for producing nickel-based alloy powders involving vacuum induction melting, followed by closed atomization in a system with a controlled dew point and gas flow, resulting in spherical particles with tailored composition and properties, including a specific range of particle sizes and low porosity, optimized for additive manufacturing.

Benefits of technology

The process yields powders with enhanced mechanical properties, improved flowability, and reduced residual porosity, enabling the production of components with superior corrosion resistance and high-temperature strength, suitable for additive manufacturing and other processing techniques like HIP.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The invention relates to a method for producing a powder from a nickel-based alloy.

[0002] WO 2015 / 110668 A2 describes a process for producing iron-based powders which are atomized using a centrifuge, with the following process steps: providing an alloy having a melting point above 1040°C, melting the composition, atomizing the molten composition using a centrifuge or a rotating atomizing device.

[0003] DE 10 2015 016 729 A discloses a process for producing metallic semi-finished products from an alloy with more than 50% nickel, comprising the following process steps: an electrode is produced by VIM, the electrode is subjected to a heat treatment in a furnace in order to reduce stresses and overaging in the temperature range between 400 and 1250°C for a period of 10 to 336 hours, the electrode is cooled in air or in the furnace, depending on the dimension, in particular depending on the diameter, to a temperature between room temperature and less than 1250°C, in particular less than 900°C, the cooled electrode is then remelted by VAR at a remelting rate of 3.0 to 10 kg / minute to form a VAR ingot, the VAR ingot is heat treated in a furnace in the temperature range between 400 and 1250°C for a period of 10 to 336 hours, the VAR ingot is cooled in air or in the furnace, depending on the dimension, in particular depending on the diameter, to a temperature between room temperature and less than 1.250°C, in particular less than 900°C, cooled, the VAR block is remelted again at a remelting rate of 3.0 to 10 kg / minute, the remelted VAR block is subjected to heat treatment in the temperature range between 400 and 1250°C for a period of 10 to 336 hours, the VAR block is then brought to the desired product shape and dimensions by hot and / or cold forming.

[0004] EP 1 377 690 B1 discloses a process for producing a nickel-based superalloy which is substantially free from positive and negative segregation, the process comprising the following: Pouring an alloy that is a nickel-base superalloy into a casting mold; annealing and overaging the alloy by heating the alloy to at least 1200°F (649°C) for a period of at least 10 hours; electroslag remelting the alloy at a melting rate of at least 8 lbs / min (3.63 kg / min); placing the alloy in a heating furnace within 4 hours of complete solidification; holding the alloy in the heating furnace at a first temperature of 600°F (316°C) to 1800°F (982°C) for a period of at least 10 hours; raising the furnace temperature from the first temperature to a second temperature of at least 2125°F (1163°C) in such a manner as to avoid thermal stresses within the alloy; holding at the second temperature for a period of at least 10 hours;Vacuum arc remelting a VAR electrode of the alloy at a melting rate of 8 to 11 lbs / min (3.63 to 5 kg / min) to produce a VAR ingot. ;

[0005] It is well known that Ni and Ni-Co alloys are used to produce components with special properties regarding corrosion resistance and good mechanical properties, such as strength, heat resistance and fracture toughness.

[0006] The invention is based on the object of providing a method for producing a powder for the additive manufacturing of components that exhibits the advantageous properties of Ni and Ni-Co alloys and is cost-effective to produce. Furthermore, the powder described above can be used, if required, for the production of components by hot isostatic pressing (HIP) or conventional sintering and extrusion processes. Furthermore, a process combination of additive manufacturing and subsequent HIP treatment is possible. The post-processing steps for HIP components described below for additive manufacturing can be applied. It is important to meet the specific requirements regarding particle size distribution, particle shape, and flowability of the powder.

[0007] This object is achieved by a process for producing a powder from a nickel-based alloy, wherein the contents (in wt.%) are defined as follows: C max. 0.5% S max. 0.15%, in particular max. 0.03% N max. 0.25% Cr 14 - 35%, especially 17 - 28% Ni Rest (> 38%) Mn max. 4% Si max. 1.5% Mon > 0 - 22 % Ti ≤ 4%, in particular ≤ 3.25% Nb up to 6.0% Cu up to 3%, especially up to 0.5% Fe ≤ 50 % P max. 0.05%, in particular max. 0.04% AI up to 3.15%, in particular up to 2.5% Mg max. 0.015% V max. 0.6% Zr max. 0.12%, in particular max. 0.1% W up to 4.5%, especially up to max. 3% Co up to 28% B ≤ 0,125 % O > 0,00001 - 0,1 % and manufacturing-related impurities, where: Ni + Fe + Co 56 - 80% Nb + Ta ≤ 6.0%, by melting an alloy in a VIM furnace, keeping the liquid melt for 5 minutes to 2 hours for homogenization, setting a closed atomization system with a supplied gas to a dew point of -10°C to 120°C, blowing the melt through a nozzle into a gas stream with a gas flow rate of 2 m³ / min to 150 m³ / min, collecting the solidified powder particles in a gas-tight container, wherein the particles have a particle size of 5 µm to 250 µm, the particles of the powder are spherical, the powder has gas inclusions of 0.0 to 4% pore area (pores > 1 µm) in relation to the total area of ​​​​evaluated objects, the powder has a bulk density of 2 to the density of the alloy of approx. 8 g / cm 3<, the powder is packed hermetically under a protective gas atmosphere with argon.

[0008] Advantageously, the powder alloy should have the following composition (in wt%): C max. 0.25% S max. 0.03% N >0 - 0,15 % Cr 17 - 28%, especially 17 - 24% Ni Rest (38-72%) Mn max. 2%, in particular max. 1% Si max. 1.2%, in particular ≤ 0.5% Mon > 0 - 21, especially 2.5 - 21% Ti > 0 - < 3,25 % Nb > 0 - 5,5 % Cu max. 3%, especially up to 0.5% Fe > 0 - 38 % P max. 0.04% Al >0 - 0,8 % Mg max. 0.015% V max. 0.4% Zr max. 0.1% W up to 0.5% Co ≤ 10% B ≤ 0,01 % Pb max. 0.001%, in particular max. 0.0005% See max. 0.0005%, in particular max. 0.0003% Bi max. 0.00005%, in particular max. 0.00003% O > 0,00001 - 0,1 % Nb + Ta >0 - 5,5% and manufacturing-related impurities, where: Ni + Fe + Co 57 - 77%.

[0009] Furthermore, it is possible to compose the powder alloy for specific applications as follows: C >0 - 0.1%, especially >0 - 0.08% S max. 0.015% N >0 - 0,03 % Cr 17-24 % Ni Rest (> 50 - 63%) Mn max. 1.0%, in particular max. 0.5% Si max. 0.5% Mon 2,8 - 16,5 % Ti >0 - 1,15 % Nb > 0 - ≤ 5,5 % Cu max. 0.5% Fe > 0 - 25 % P max. 0.015% Al 0,1 - 0,6 % Mg max. 0.015% V max. 0.2% Zr max. 0.1% W up to 0.2%, especially >0 - 0.2% Co ≤ 2.5%, in particular ≤ 1.0% B ≤ 0,01 % Pb max. 0.001%, in particular max. 0.0005% See max. 0.0005%, in particular max. 0.003% Bi max. 0.0005%, in particular max. 0.0003% O > 0,00001 - 0,1 % Nb + Ta >0 - 5,5 % Al + Ti < 1,2 % and manufacturing-related impurities, where: Ni + Fe + Co 59 - 72%.

[0010] The following initial production steps are conceivable: A master alloy block with a defined chemical analysis is produced by melting in a VIM furnace, VIM / ESU, VIM / ESU / VAR, VIM / VAR, VOD, or VLF with, if necessary, subsequent remelting in ESU and / or VAR depending on the purity requirements of the material. A master alloy block is cut into small pieces by sawing. The master alloy pieces are melted in a VIM furnace, or alloying elements of a defined weight are melted in a VIM according to the chemical analysis, or the combination of master alloy material, process-related scrap (including scrap from customers such as recycled powders, support structures, or defective components), and new alloying elements in a ratio of 0 to 100%. The exact ratio is considered in each case, taking qualitative, economic, and ecological aspects into account. It can be advantageous if the master alloy block is subjected to surface treatment (e.g.,This allows defects to be removed that cannot be eliminated by further remelting and could be detrimental to later applications. Furthermore, the use of optional master alloys ensures compliance with the highest quality standards regarding the chemical purity of the powder, which can only be guaranteed through prior remelting processes. The liquid melt is held for 5 minutes to 2 hours for homogenization.

[0011] The following further processing steps can follow the alternative initial production steps: the closed atomization system is set with argon gas to a dew point of -10°C to -120°C, preferably in the range of -30°C to -100°C, the melt is blown through a nozzle into an argon gas stream with a gas flow rate of 2 m³ / min to 150 m³ / min, the solidified powder particles are collected in a gas-tight container, the particles have a particle size of 5µm to 250µm, with preferred ranges being between 5 and 150µm, or 10 and 150µm, the powder particles are spherical, the powder has gas inclusions of 0.0 to 4% pore area (pores > 1µm) in relation to the total area of ​​​​evaluated objects, with preferred ranges being 0.0 to 2%. The amount of gas inclusions in the powder allows for minimal residual porosity in the manufactured parts. The powder has a bulk density of 2 to the alloy density of approximately.8 g / cm 3< , with preferred ranges being values ​​of 4 to 5 g / cm 3<, the powder is packaged hermetically under a protective gas atmosphere with argon. .

[0012] The powder is preferably produced in a vacuum inert gas atomization (VIGA) system. In this system, the alloy is melted in a vacuum induction melting furnace (VIM) and fed into a pouring funnel, which leads to a gas nozzle where the molten metal is atomized into metal particles using inert gas at high pressures of 5 to 100 bar. The melt is heated in the crucible at temperatures between 5 and 400 °C above the melting point. The metal flow rate during atomization is 0.5 to 80 kg Imin and the gas flow rate is 2 to 150 m³ / min. Due to the rapid cooling, the metal particles solidify into spherical shapes (particles). The inert gas used during atomization can contain 0.01 to 100% nitrogen, if required. The gas phase is then separated from the powder in a cyclone, and the powder is then packaged.

[0013] Alternatively, the powder can be produced using the so-called EIGA process instead of VIGA. In this process, a prefabricated alloy block in the form of a rotating electrode is melted contactlessly by an induction coil. The melt drips from the electrode directly into the gas stream of a gas nozzle.

[0014] The alloy ingot for EIGA can be produced using the VIM, ESR, VAR, VOD, or VLF melting processes, and combinations thereof, and can optionally undergo hot forming processes such as forging and rolling. It is advantageous to clean the ingot's surface by treatment such as grinding and / or peeling before use in the EIGA process.

[0015] The inert gas used in powder production can be either argon or a mixture of argon with 0.01 to 100% nitrogen. Possible limitations of the nitrogen content may include: 0.01 to 80% 0.01 to 50% 0.01 to 30% 0.01 to 20% 0.01 to 10% 0.01 to 10% 0.1 to 5% 0.5 to 10% 1 to 5% 2 to 3%

[0016] Alternatively, the inert gas can be helium.

[0017] The inert gas preferably has a purity of at least 99.996 vol.%. In particular, the nitrogen content should be between 0.0 and 10 ppmv, the oxygen content between 0.0 and 4 ppmv, and the H2O content should be ≤ 5 ppmv.

[0018] In particular, the inert gas preferably has a purity of at least 99.999 vol.%. In particular, the nitrogen content should be between 0.0 and 5 ppmv, the oxygen content between 0.0 and 2 ppmv, and the H2O content should be ≤ 3 ppmv. The dew point in the system is in the range of -10 to -120°C. It is preferably in the range of -30 to -100°C.

[0019] The pressure during powder atomization can preferably be 10 to 80 bar.

[0020] The parts and components, or layers on parts and components, manufactured using additive manufacturing are constructed from layer thicknesses ranging from 5 to 500 µm and, immediately after production, have a textured microstructure with grains elongated in the build direction and an average grain size of 2 µm to 1000 µm. The preferred range is between 5 µm and 500 µm.

[0021] Parts and components, or coatings on parts and components, produced using additive manufacturing can optionally be subjected to solution annealing in the temperature range from 700°C to 1250°C for 0.1 min to 70 h, optionally under a protective gas such as argon or hydrogen, followed by cooling in air, in a moving annealing atmosphere, or in a water bath. The surface can then be cleaned or machined by pickling, blasting, grinding, turning, peeling, or milling. This machining can be carried out partially or entirely even before annealing.

[0022] Parts and components, or coatings on parts and components, produced using additive manufacturing can be subjected to homogenization, stress relief, solution hardening, and / or precipitation hardening annealing. Heat treatments can be performed under a protective gas, such as argon or hydrogen, if necessary, followed by cooling in a furnace, in a protective gas, in air, in a moving annealing atmosphere, or in a water bath.

[0023] The parts and components, or coatings on parts and components, produced using additive manufacturing have an average grain size of 2 µm to 2000 µm after annealing. The preferred range is between 20 µm and 500 µm.

[0024] The parts and components, or layers on parts and components, produced by additive manufacturing from the powder produced according to the invention are preferably to be used in areas in which the material is also used as a wrought or cast alloy with related analysis.

[0025] Additive manufacturing also includes terms such as generative manufacturing, rapid technology, rapid tooling, rapid prototyping or the like.

[0026] In general, a distinction is made between: 3D printing with powders, selective laser sintering and selective laser melting, laser cladding, selective electron beam welding.

[0027] The abbreviations used here are defined as follows: VIMVacuum Induction Melting VIGAVacuuminert gas atomization system VARVacuum Arc Remelting VODVaccum Oxygen Decaburization VLFVaccum Ladle Furnace EIGAElectrode Induction Melting Gas Atomization

[0028] Advantageous further developments of the method according to the invention can be found in the subclaims.

[0029] The particle size range of the powder is between 5 and 250 µm, with preferred ranges being between 5 and 150 µm, or 10 and 150 µm.

[0030] The powder has gas inclusions of 0.0 to 4% pore area (pores > 1 µm) in relation to the total area of ​​evaluated objects, with preferred ranges being 0.0 to 2% 0.0 to 0.5% 0.0 to 0.2% 0.0 to 0.1% 0.0 to 0.05%

[0031] The powder has a bulk density of 2 to the density of the alloy of approximately 8 g / cm 3< , whereby preferred ranges can be the following values. 4-5 g / cm 3< 2-8 g / cm 3< 2-7 g / cm 3< 3-6 g / cm 3<

[0032] The amount of gas inclusions in the powder allows for low residual porosity in the manufactured parts.

[0033] Compared to the state of the art, the centrifuge process is omitted, thus optimizing the plant's operating time. The subsequent refinement processes optimize the quality of the powder for additive manufacturing.

[0034] It can be advantageous if the block is subjected to surface treatment (e.g., brushing, grinding, pickling, cutting, peeling, etc.) before cutting. This can remove defects that cannot be eliminated by further remelting and could be detrimental to later applications.

[0035] The process according to the invention can be applied to any Ni or Ni-Co base alloy.

[0036] The following presents an alloy composition that can be produced as a powder using the process parameters according to the invention. All values ​​are in wt. %: C max. 0.5% S max. 0.150%, in particular max. 0.03% Cr 17-32%, especially 17-26% Ni 45-72%, especially 45-71% Mn max. 1% Si max. 1% Mon > 0-10 % Ti max. 3.25%, in particular max. 2.7% Nb max. 5.5% Cu max. 5%, in particular max. 0.5% Fe max. 25% Al max. 3.15%, in particular max. 2.5% V max. 0.6% Zr max. 0.12%, in particular max. 0.1% Co max. 28% O 0,00001-0,1 % and manufacturing-related impurities.

[0037] In addition, the following elements may be present (in % by weight): Nb+Ta max. 6% B max. 0.02%, in particular max. 0.006% See max. 0.0005% Bi max. 0.00005% Pb max. 0.002% P max. 0.03%, in particular max. 0.02%

[0038] The following elements can advantageously be adjusted as follows (data in wt.%): C 0.015 - 0.5%; especially 0.015 - 0.2% S max. 0.1%, in particular max. 0.02% Cr 17-25% Ni 45-58 % Mn max. 0.6% Si max. 0.4% Mon 0-6,1 % Ti 0,1-2,7 % Al max. 1.7% Co max. 13%

[0039] To improve the mechanical properties, the elements boron and carbon can also be adjusted as follows: C 0,015 - 0,5 % B 0,006 - 0,125 %

[0040] It is also advantageous if the sum C + B is between 0.1875 and 0.530%, between 0.156 and 0.625%, especially between 0.16 and 0.6%, and the C / B ratio is between 12 and 18.

[0041] The following is an example of a powder made of a Ni alloy based on Alloy 718 (data in wt.%): C max. 0.08% S max. 0.015% Cr 17-21 % Ni 50-55 % Mn max. 0.35% Si max. 0.35% Mon 2,8-3,3 % Ti 0,65-1, 15 % Nb 4,75-5,5 % Cu max. 0.3% Fe 6-25 % P max. 0.015% Al 0,2-0,8 % Co max. 1% B max. 0.006% Ta max. 0.05% O 0,00001-0,1 % Pb max. 0.001%, in particular max. 0.0005% See max. 0.0005%, in particular max. 0.0003% Bi max. 0.00005%, in particular max. 0.00003%

[0042] Alternatively, this alloy can also have higher Ni contents (values ​​in wt.%). C max. 0.1% S max. 0.03%, in particular max. 0.02% Cr 17-32%, especially 17-30% Ni 58-79, especially 58 - 72% Nb max. 4.1%, in particular max. 0.6% Fe max. 18% C max. 0.1% S max. 0.02% Mn max. 1% Si max. 1% Mon > 0-10 % Ti max. 3.25%, in particular max. 2.7% Cu max. 0.5% Al max. 3.15% V max. 0.6% Zr max. 0.1% Co max. 15%, especially max. 7% O 0,00001-0,1 % and optionally (in % by weight): B max. 0.008%, in particular max. 0.006% See max. 0.0005% Bi max. 0.00005% Pb max. 0.002% P max. 0.03%, in particular max. 0.02%

[0043] Further restrictions are conceivable as follows (in % by weight): C 0,01-0,04 % Mn max. 0.5% Si max. 0.5% Cu max. 0.2%

[0044] And optionally (in % by weight): Mon 8-10 %

[0045] Optionally, the oxygen content of the produced alloy can be 0.00001 - 0.1%, 0.0001 - 0.1%, 0.001 - 0.1%, 0.001 - 0.002% or 0.0015 - 0.002%.

[0046] Optionally, the oxygen content can also be adjusted as follows: 0.00001 - 0.1 0.00002 - 0.1 0.00005 - 0.1 0.00008 - 0.1 0.0001 - 0.1 0.0002 - 0.1 0.0005 - 0.1 0.0008 - 0.1 0.001 - 0.1 0.002 - 0.1 0.005 - 0.1 0.008 - 0.1 0.010 - 0.1 0.00001 - 0.10 0.00001 - 0.08 0.00001 - 0.05 0.00001 - 0.03 0.00001 - 0.02

[0047] The nitrogen content must be less than or equal to 0.100% to ensure the manufacturability and usability of the alloy. Excessively high nitrogen content leads to the formation of nitrides, which negatively affect the alloy's properties. Too low a nitrogen content increases costs. Therefore, the nitrogen content should be ≥ 0.00001%. The following limitations on the nitrogen content are conceivable: 0.00001 - 0.1 0.00002 - 0.1 0.00005 - 0.1 0.00008 - 0.1 0.0001 - 0.1 0.0002 - 0.1 0.0005 - 0.1 0.0008 - 0.1 0.001 - 0.1 0.002 - 0.1 0.005 - 0.1 0.008 - 0.1 0.010 - 0.1 0.00001 - 0.10 0.00001 - 0.08 0.00001 - 0.05 0.00001 - 0.03 0.00001 - 0.02

[0048] Both in powder and in fabricated components (3D-printed samples), the particle sizes of nitrides, carbides, and / or carbonitrides are very small (approximately < 8 µm). In some cases, the above-mentioned particles may not be present or may only become visible after heat treatment. Small particle sizes of N-containing precipitates have a positive effect on high-temperature properties and low-cycle fatigue (LCF), as N-containing precipitates act as crack initiation sites in conventionally produced alloys.

[0049] The argon content must be less than or equal to 0.08% to ensure the manufacturability and usability of the alloy. Argon cannot be dissolved in the y-matrix, so it can negatively impact the mechanical properties of the component, as argon inclusions can act as crack initiation sites. An excessively low argon content increases costs. The argon content is therefore ≥ 0.0000001% (≥ 1 ppb). The following limitations on the argon content are conceivable, including the argon content from both powder production and component manufacturing: 0.0000001 - 0.05 0.0000002 - 0.05 0.0000001 - 0.005 0.0000001 - 0.002 0.0000001 - 0.001

[0050] The process according to the invention should preferably be applicable for the following alloys: Alloy 601 Alloy 602 CA and its variant MCA Alloy 2120 MoN Alloy B2 Alloy C 276 Crofer 22 APU Crofer 22 H

[0051] Table 1 shows exemplary analysis ranges of the above-mentioned alloys. Table 1 Alloy 601 Alloy 602 CA / MCA FM 602 Alloy 617 (B / OCC) FM 617 Alloy 625 FM 625 Alloy 690 Alloy 699XA C 0,03-0,1 0,15-0,25 0,15-0,25 0,05-0,08 0,05-0,15 -0,03 -0,1 -0,05 0,005-0,12 S -0,015 -0,01 -0,008 -0,01 -0,015 -0,01 N -0,05 Cr 21-25 24-26 24-26 21-23 20-24 21-23 20-23 27-31 26-30 Ni 58-63 59-66 59-66 45-58 50-61 58-71 58-71 58-66 62-72 Mn -1 -0,5 -0,5 -0,5 -1 -0,5 -0,5 -0,5 -0,5 Si -0,5 -0,5 -0,5 -0,3 -1 -0,4 -0,5 -0,5 -0,5 Mon 8-10 8-10 8-10 8-10 Ti 0,5 0,1-0,2 0,1-0,2 0,25-0,5 -0,6 -0,4 -0,4 -0,6 Nb -0,6 3-4,1 -0,5 Cu -0,5 0,1 -0,1 -0,5 -0,5 -0,5 -0,5 Fe -18 8-11 8-11 -1,5 -3 -5 -5 7-11 -2,5 P -0,02 -0,02 -0,012 -0,03 -0,01 -0,02 Al 1-1,7 1,8-2,4 1,8-2,4 0,8-1,3 0,8-1,5 -0,4 -0,4 2-3 Mg Ca V -0,6 Zr 0,01-0,1 0,01-0,1 -0,1 W -0,5 Co -1 11-13 10-15 -1 B -0,006 0,001-0,005 -0,008 Ni + Co Nb + Ta 3,2-3,8 3,2-3,8 3,2-3,8 Additional elements Alloy 617 and its variants 617 B and 617 OCC Alloy 625 Alloy 690 Alloy 699XA Alloy 718 and its variants Alloy 780 Alloy 788 Alloy 80A Alloy 81 Alloy X-750 Alloy C-263 Alloy K-500 Waspaloy FM 625 FM 617 and FM 602 Alloy 31 Alloy 31 Plus Alloy 25 Alloy 28 Alloy 33 Alloy 59 Alloy 188 Alloy 310 L Alloy 330 Alloy 333 Alloy 400 Alloy 600 + 600 L Ally 800 + 800 H, HP, L Alloy 825 + 825 CTP Alloy 925 Alloy 926 Alloy 718 Alloy 718 CTP FM 718 Alloy 780 Alloy 788 Waspaloy Alloy C-263 Alloy 80A Alloy 81 C -0,08 -0,045 -0,08 -0,1 0,04-0,1 0,02-0,1 0,04-0,08 0,04-0,1 -0,08 S -0,015 -0,01 -0,015 -0,01 -0,03 -0,007 -0,015 -0,02 N -0,03 Cr 17-21 17-21 17-21 16-20 18-21 18-21 19-21 18-21 28-32 Ni 50-55 50-55 50-55 26-62 51-69 49,6-62,5 50-55 65-79 59-66 Mn -0,35 -0,35 -0,3 -0,5 -1 -1 -0,6 -1 -0,7 Si -0,35 -0,35 -0,3 -0,3 -0,5 -0,75 -0,4 -1 -0,7 Mon 2,8-3,3 2,8-3,3 2,8-3,3 2-4 3,5-5 5,6-6,1 -0,5 Ti 0,65-1,15 0,8-1,15 0,7-1,1 0,1-1 1,8-2,7 2,75-3,25 1,9-2,4 1,8-2,7 1,5-2,1 Nb 4,75-5,5 Nb+Ta 4,8-5,5 Cu -0,3 -0,23 -0,3 -0,5 -0,2 -0,5 -0,2 -0,2 -0,25 Fe 6-25 12-24 -24 -10 8-15 -2 -0,7 -1,5 -1,5 P -0,015 -0,01 -0,015 -0,03 -0,02 -0,03 -0,015 Al 0,2-0,8 0,4-0,6 0,2-0,8 1-3 1-1,8 1,2-1,6 0,3-0,6 1-1,8 -1,2 Mg -0,01 -1 Ca -0,01 V Zr -0,05 0,02-0,12 0,01-0,1 W Co -1 -1 15-28 3-7 12-15 19-21 Ol. Mar B -0,006 -0,006 -0,006 -0,02 -0,008 0,003-0,01 -0,005 -0,006 Ni + Co Nb + Ta 4,87-5,2 4-6 Additional elements C Alloy K-500 Alloy X-750 Alloy 31 Plus ®< Alloy 28 Alloy 31 Alloy 33 Alloy 59 Alloy 188 S -0,18 -0,08 ≤ 0.01 < 0.015 ≤ 0.015 ≤ 0.015 ≤ 0.01 0.05 to 0.15 N -0,01 -0,01 ≤ 0.01 ≤ 0.01 ≤ 0.01 ≤ 0.01 ≤ 0.01 ≤ 0.015 Cr 0.1 to 0.25 0.04 to 0.07 0.15 to 0.25 0.35 to 0.6 Ni 14-17 26.0 to 27.0 26 to 28 26 to 28 31 to 35 22 to 24 20 to 24 Mn 63-70 70-77,5 33.5 to 35.0 30 to 32 30 to 32 30 to 33 57 to 63 20 to 24 Yes -1,5 -1 1.0 to 4.0 ≤ 2 ≤ 2 ≤ 2 ≤ 0.5 ≤ 1.25 Mo -0,5 -0,5 ≤ 0.10 ≤ 0.7 ≤ 0.3 ≤ 0.5 ≤ 0.1 0.2 to 0.4 Ti 6.0 to 7.0 3 to 4 6 to 7 0.5 to 2 15 to 16.5 Nb 0,35-0,85 2,25-2,75 Cu 0,7-1,2 Fe 27-33 -0,5 0.5 to 1.5 1 to 1.4 1 to 1.4 0.3 to 1.2 5 0.5 P 0,5-2 5-9 22.5 to 33.5 32 to 40 29 to 37 26 to 38 ≤ 1.5 ≤ 3 Al -0,02 ≤ 0.02 ≤ 0.02 ≤ 0.02 ≤ 0.02 ≤ 0.015 ≤ 0.015 Mg 2,3-3,15 0,4-1 ≤ 0.3 0.1 to 0.4 ≤ 0.2 Ca V Zr W Co 13 to 16 B -1 ≤ 0.3 Ni + Co ≤ 0.01 Nb + Ta Weitere Elemente / additional elements 0,7-1,2 C Alloy 310L Alloy 330 Alloy 333 Alloy 400 Alloy 600 Alloy 600 L Alloy 800 Alloy 800 H Alloy 800 HP S ≤ 0.02 ≤ 0.15 0.03 to 0.06 ≤ 0.15 0.05 to 0.1 ≤ 0.025 ≤ 0.1 0.06 to 0.10 0.06 to 0.1 N 5 0.005 ≤ 0.015 ≤ 0.02 ≤ 0.015 ≤ 0.01 ≤ 0.01 ≤ 0.01 ≤ 0.01 Cr Ni 24 to 25 15 to 17 24 to 26 14 to 17 14 to 17 19.0 to 21.5 19 to 21 19 to 22 Mn 20 to 21 33 to 37 44 to 47 ≥ 63 ≥ 72 ≥ 72 30.0 to 32.0 30 to 32 30 to 32 Yes ≤ 1 ≤ 2 1.2 to 2 ≤ 2 ≤ 1 ≤ 1 0.5 to 1.0 0.5 to 1 0.5 to 1 Mo 5 0.15 1 to 2 0.8 to 1.2 ≤ 0.5 ≤ 0.5 ≤ 0.5 0.2 to 0.6 0.2 to 0.6 0.2 to 0.6 Ti 5 0.1 2.5 to 3.5 Nb 0.1 to 0.2 S 0.3 ≤ 0.3 0.20 to 0.5 0.2 to 0.6 0.3 to 0.6 Cu Fe ≤ 0.5 28 to 34 ≤ 0.5 ≤ 0.5 ≤ 0.5 ≤ 0.5 ≤ 0.5 P 42 to 51 13 to 22 1 to 2.5 6 to 10 6 to 10 41 to 47 43 to 50 43 to 50 Al ≤ 0.02 ≤ 0.045 ≤ 0.02 ≤ 0.015 5 0.015 5 0.015 ≤ 0.015 Mg ≤ 0.5 ≤ 0.3 ≤ 0.3 0.20 to 0.40 0.2 to 0.6 0.3 to 0.6 Ca V Zr W Co 2.5 to 3.5 B 2.5 to 3.5 Ni + Co ≤ 0.006 Nb + Ta Weitere Elemente / additional elements Al + Ti max. 1.0 % Al + Ti max 0.7% Al + Ti 0.85% - 1.2% C Alloy 800 L Alloy 825 Alloy 825 CTP Alloy 925 Alloy 926 Alloy 2120 MoN Alloy B-2 S ≤ 0.025 ≤ 0.025 ≤ 0.015 ≤ 0.03 ≤ 0.020 ≤ 0.01 ≤ 0.01 N ≤ 0.01 ≤ 0.015 ≤ 0.005 ≤ 0.03 ≤ 0.010 ≤ 0.01 ≤ 0.01 Cr ≤ 0.03 0.15 to 0.25 0.02 to 0.15 Ni 20 to 22 19.5 to 23.5 21 to 23 19.5 to 22.5 20.0 to 21.0 20.0 to 23.0 0.4 to 1 Mn 32 to 34 38 to 46 39 to 43 42 to 46 24.00 to 26.00 58 64 to 72 Yes 0.5 to 1 ≤ 1 0.5 to 0.9 ≤ 1 51.00 ≤ 0.50 ≤ 1 Mo ≤ 0.7 ≤ 0.5 0.2 to 0.5 ≤ 0.5 ≤ 0.50 ≤ 0.1 ≤ 0.08 Ti 2.5 to 3.5 4.5 to 6.5 2.5 to 3.5 6.0 to 7.0 18.5 to 21.0 26 to 30 Nb 0.35 to 0.6 0.6 to 1.2 1.9 to 2.4 Cu ≤ 0.15 ≤ 0.5 Fe ≤ 0.5 1.5 to 3 1.6 to 2.3 1.5 to 3 0.5 to 1.5 ≤ 0.5 ≤ 0.5 P 41 to 47 20 to 38 20 to 38 ≥ 22 ≤ 1.5 1.6 to 2 Al ≤ 0.015 ≤ 0.02 ≤ 0.03 ≤ 0.030 ≤ 0.015 ≤ 0.02 Mg 0.15 to 0.4 ≤ 0.2 0.06 to 0.25 0.1 to 0.5 ≤ 0.4 Ca 0.006 to 0.015 v Zr W Co ≤ 0.3 B ≤ 1 ≤ 0.5 ≤ 0.3 ≤ 1 Ni + Co 0.002 to 0.004 Nb + Ta Weitere Elemente / additional elements Al + Ti 1.0% C Alloy C-263 Alloy C-276 Crofer 22 APU Crofer 22 H NeutroShield S 0.04 to 0.08 ≤ 0.01 ≤ 0.03 ≤ 0.03 ≤ 0.08 N ≤ 0.007 ≤ 0.01 ≤ 0.020 ≤ 0.006 ≤ 0.030 Cr ≤ 0.04 ≤ 0.10 Ni 19.0 to 21.0 15 to 16.5 20.0 to 24.0 20 to 24 18.00 to 20.00 Mn 50 to 55 51 to 63 ≤ 0.5 12.00 to 15.00 Yes ≤ 0.6 ≤ 1 0.30 to 0.80 ≤ 0.8 ≤ 2.00 Mo ≤ 0.4 ≤ 0.08 ≤ 0.50 0.1 to 0.6 Ti 5.6 to 6.1 15 to 17 Nb 1.90 to 2.40 0.03 to 0.20 0.02 to 0.2 Cu 0.2 to 1 Fe ≤ 0.2 ≤ 0.50 ≤ 0.5 P ≤ 0.7 4 to 7 ≥ 73 70 to 79 R Al ≤ 0.015 ≤ 0.02 ≤ 0.050 ≤ 0.05 ≤ 0.045 Mg 0.30 to 0.60 ≤ 0.50 ≤ 0.1 Ca V Zr ≤ 0.3 W Co 3 to 4.5 1 to 3 B 19.0 to 21.0 ≤ 2.5 ≤ 0.2 Ni + Co ≤ 0.005 0.20 to 2.25 Nb + Ta Weitere Elemente / additional elements Ag: max, 0.0005; Zr: max. 0.02? Al+Ti: 2.40 - 2.80; Ni: Rest. Si 0.75 % (max) Pb, Ag, Zr: Determination only on request.

[0052] Powders with a particle size of 5µm to 250µm are achieved.

[0053] A particle size that is too small below 5 µm impairs the flow behavior and should therefore be avoided; a particle size that is too large above 250 µm impairs the behavior during additive manufacturing.

[0054] A bulk density that is too low, less than 2 g / cm², impairs the performance during additive manufacturing. The maximum possible bulk density of approximately 8 g / cm³ is determined by the density of the alloy.

[0055] The oxygen content must be less than or equal to 0.100% to ensure the manufacturability and usability of the alloy. An oxygen content that is too low increases costs. Therefore, the oxygen content is ≥ 0.0001%. Powders produced using this process can be used in additive manufacturing to build components that exhibit the properties of the underlying alloys.

[0056] In addition, the powder described above can also be used to manufacture components using hot isostatic pressing (HIP) or conventional sintering and extrusion processes. A combination of additive manufacturing and subsequent HIP treatment is also possible. The post-processing steps for HIP components described below for additive manufacturing can be applied.

[0057] The powder produced using this process, as well as components manufactured from this powder (3D-printed samples), are free of nitrides, carbides, and / or carbonitriding. If nitrides or carbides are present, they have a particle size of < 100 nm, particularly < 50 nm.

[0058] After heat treatment of components manufactured from this powder (3D-printed samples) for homogenization, diffusion annealing at temperatures above 900°C, especially above 1000°C, ideally above 1100°C, for more than 1 hour, nitrides, carbides, and / or carbonitrides may occur in the manufactured components (3D-printed samples). These have particle sizes of <8µm or <5µm, ideally <1µm, and especially <500nm. The process according to the invention is explained by way of example as follows:

[0059] The following melts were produced using the process according to the invention and manufactured as powder (data in wt.%): Batch P10030 P10036 P10038 P10039 P10046 P10049 P10057 P10153 P10154 P10155 C 0,022 0,027 0,025 0,026 0,028 0,023 0,033 0,002 0,002 0,003 S 0,0005 0,0005 0,0006 0,0005 0,0007 0,0006 0,001 0,002 0,002 0,002 N 0,007 0,008 0,006 0,008 0,005 0,008 0,007 0,004 0,004 0,003 Cr 18,33 18,38 17,94 18,35 17,94 18,95 18,56 22,46 22,48 22,72 Ni 53,07 53,24 52,33 53,24 53,32 52,2 53,44 60,91 60,71 60,5 Mn 0,04 0,03 0,18 0,1 0,03 0,11 0,03 0,2 0,19 0,18 Si 0,06 0,05 0,18 0,08 0,04 0,16 0,06 0,01 0,01 0,01 Mon 2,98 3,03 2,96 3,01 3,05 3,13 2,98 15,43 15,42 15,48 Ti 0,93 0,93 1,28 0,98 0,9 0,92 0,95 0,01 0,01 0,01 Nb 5,28 5,37 5,18 5,09 5,41 5,61 5,39 0,01 0,01 0,01 Cu 0,03 0,02 0,14 0,05 0,02 0,03 0,03 0,01 0,01 0,01 Fe 18,52 18,18 17,66 18,01 18,55 17,63 17,82 0,52 0,66 0,67 P 0,009 0,008 0,039 0,013 0,007 0,011 0,007 0,002 0,002 0,002 Al 0,55 0,58 0,8 0,6 0,52 0,53 0,46 0,24 0,31 0,22 Mg 0,001 0,001 0,011 0,005 0,001 0,002 0,001 0,001 0,001 0,001 Ca 0,001 0,001 0,002 0,004 0,001 0,004 0,001 0,001 0,001 0,001 V 0,02 0,02 0,18 0,06 0,02 0,13 0,02 0,16 0,15 0,15 Zr 0,01 0,01 0,05 0,05 0,01 0,03 0,01 - - - W 0,03 0,03 0,19 0,09 0,06 0,06 0,02 0,01 0,01 0,01 Co 0,1 0,08 0,84 0,22 0,07 0,44 0,08 0,01 0,01 0,01 B 0,004 0,004 0,007 0,004 0,004 0,01 0,004 0,001 0,001 0,001 Table 2 Batch P10156 P10157 P10207 P10208 P10209 P10210 P10211 P10212 P10213 P10214 P10215 C 0,003 0,002 0,002 0,002 0,002 0,002 0,002 0,002 0,003 0,002 0,002 S 0,002 0,002 0,003 0,003 0,003 0,003 0,003 0,003 0,003 0,003 0,003 N 0,004 0,005 0,003 0,005 0,004 0,004 0,003 0,006 0,005 0,002 0,003 Cr 22,78 22,66 22,8 22,65 22,95 22,66 22,5 22,54 22,43 22,46 22,49 Ni 60,27 60,19 60,4 60,34 60,27 60,36 60,82 60,4 61,01 60,89 60,59 Mn 0,19 0,18 0,22 0,22 0,2 0,18 0,19 0,18 0,19 0,15 0,17 Si 0,01 0,01 0,04 0,01 0,03 0,02 0,02 0,02 0,01 0,02 0,02 Mon 15,71 16,02 15,5 15,64 15,47 15,68 15,39 15,77 15,39 15,39 15,68 Ti 0,01 0,01 0,01 0,01 0,01 0,01 0,01 0,01 0,01 0,01 0,01 Nb 0,01 0,01 0,01 0,01 0,01 0,01 0,01 0,01 0,01 0,01 0,01 Cu 0,01 0,01 0,01 0,01 0,01 0,01 0,01 0,01 0,01 0,01 0,01 Fe 0,61 0,45 0,61 0,61 0,53 0,53 0,53 0,52 0,44 0,52 0,51 P 0,002 0,002 0,002 0,002 0,002 0,002 0,002 0,002 0,002 0,002 0,002 Al 0,22 0,28 0,22 0,24 0,27 0,26 0,28 0,26 0,26 0,29 0,27 Mg 0,001 0,001 0,001 0,001 0,001 0,001 0,001 0,001 0,001 0,001 0,001 Ca 0,001 0,001 0,001 0,001 0,001 0,001 0,001 0,001 0,001 0,001 0,001 V 0,14 0,14 0,14 0,14 0,13 0,14 0,14 0,15 0,14 0,14 0,15 Zr - - - - - - - - - - - W 0,01 0,01 0,01 0,01 0,01 0,02 0,01 0,01 0,01 0,01 0,01 Co 0,01 0,01 0,01 0,08 0,09 0,1 0,07 0,09 0,06 0,08 0,06 B 0,001 0,001 0,001 0,001 0,001 0,001 0,001 0,001 0,001 0,001 0,001

[0060] Table 2 shows the chemical compositions of the powders produced using the process according to the invention: Both powder and manufactured components (3D-printed samples) were free of nitrides and carbides.

[0061] After annealing at a temperature of 1100°C for 1 hour followed by quenching in water, particles such as nitrides, carbides, and / or carbonitrides were present in the manufactured components (3D-printed samples). These particles had a diameter of less than 1µm.

Claims

1. Method for producing a nickel-base alloy powder, wherein the contents (in % by weight) are defined as follows: Cmax. 0.5%Smax. 0.15%, in particular max. 0.03%Nmax. 0.25%Cr14 - 35%, in particular 17 - 28%Niremainder (> 38%)Mnmax. 4%Simax. 1.5%Mo> 0 - 22%Ti≤ 4%, in particular ≤ 3.25%Nbup to 6.0%Cuup to 3%, in particular up to 0.5%Fe≤ 50%Pmax. 0.05%, in particular max. 0.04%Alup to 3.15%, in particular up to 2.5%Mgmax. 0.015%Vmax. 0.6%Zrmax. 0.12%, in particular max. 0.1%Wup to 4.5%, in particular up to max. 3%Coup to 28%B≤ 0.125%O> 0.00001 - 0.1% and production-related impurities, wherein: Ni + Fe + Co 56 - 80% Nb + Ta ≤ 6.0% by - melting an alloy in a VIM furnace, - holding the liquid melt from 5 min to 2 hours for homogenisation, - setting a closed atomisation system with a supplied gas to a dew point from -10 °C to 120 °C, - blowing the melt through a nozzle into a gas stream with a gas flow rate from 2 qm3 / min to 150 qm3, - collecting the solidified powder particles in a sealed, gas-tight container, wherein - the particles have a particle size from 5 µm to 250 µm, - the particles of the powder are spherical, - the powder has gas inclusions from 0.0 to 4% pore area (pores > 1 µm) as a proportion of the total area of evaluated objects, - the powder has a bulk density from 2 up to the density of the alloy of approx. 8 g / cm3, - the powder is packed airtight under the protective gas atmosphere with argon.

2. Method according to Claim 1 with the following composition (in % by weight): Cmax. 0.25%Smax. 0.03%N> 0-0.15%Cr17-28%, in particular 17 - 24%Niremainder (38 - 72%)Mnmax. 2%, in particular max. 1%Simax. 1.2%, in particular ≤ 0.5%Mo> 0 - 21, in particular 2.5-21%Ti> 0 - < 3.25%Nb> 0 - 5.5%Cumax 3%, in particular up to 0.5%Fe> 0 - 38%Pmax. 0.04%Al> 0 - 0.8%Mgmax. 0.015%Vmax. 0.4%Zrmax. 0.1%Wup to 0.5%Co≤ 10%B≤ 0.01%Pbmax. 0.001%, in particular max. 0.0005%Semax.0.0005%, in particular max. 0.0003%Bimax 0.00005%, in particular max. 0.00003%O> 0.00001 - 0.1%Nb + Ta> 0 - 5.5% and production-related impurities, wherein: Ni +Fe + Co 57 - 77%.

3. Method according to Claim 1 or 2 with the following composition (in % by weight): C> 0 - 0.1%, in particular > 0 - 0.08%Smax 0.015%N> 0 - 0.03%Cr17 - 24%Niremainder (> 50 - 63%)Mnmax. 1.0%, in particular max. 0.5%Simax. 0.5%Mo2.8 - 16.5%Ti> 0 - 1.15%Nb> 0 - ≤ 5.5%Cumax. 0.5%Fe> 0 - 25%Pmax. 0.015%Al0.1 - 0.6%Mgmax. 0.015%Vmax. 0.2%Zrmax. 0.1%Wup to 0.2% in particular> > 0 - 0.2%Co≤ 2.5%, in particular ≤ 1.0%B≤ 0.01%Pbmax. 0.001%, in particular max. 0.0005%Semax. 0.0005%, in particular max.0.003%Bimax. 0.0005%, in particular max. 0.0003%O> 0.00001 - 0.1%Nb + Ta> 0 - 5.5%Al + Ti< 1.2% and production-related impurities, wherein: Ni + Fe + Co 59-72%.

4. Method according to any one of Claims 1 to 3, wherein the alloy is first produced as a master alloy with a defined chemical analysis by melting in the VIM furnace, VIM / ESR, VIM / ESR / VAR, VIM / VAR VOD or VLF, with subsequent remelting in the ESU and / or VAR as necessary, - the master alloy block is cut into small pieces by sawing, - the pieces of the master alloy are melted in a VIM furnace.

5. Method according to any one of Claims 1 to 4, characterized in that an inert gas is used as the supplied gas.

6. Method according to any one of Claims 1 to 5, characterized in that argon is used as the supplied gas.

7. Method according to any one of Claims 1 to 6, characterized in that the gas stream into which the melt is atomised consists of argon.

8. Method according to any one of Claims 1 to 7, characterized in that the gas stream into which the melt is atomised consists of nitrogen.

9. Method according to any one of Claims 1 to 8, characterized in that the gas stream into which the melt is atomised consists of a mixture of nitrogen and argon.

10. Method according to any one of claims 1 to 9, characterized in that the atomisation of the melt takes place at a rate of 0.5 to 80 kg / min.

11. Use of a powder produced according to a method according to any one of Claims 1 to 10 for the additive manufacture of components or parts.

12. Use of a powder produced according to a method according to any one of Claims 1 to 10 for the additive manufacture of layers on components or parts.

13. Use of a powder produced according to a method according to any one of Claims 1 to 10 for the manufacture of turbine components.

14. Use of a powder produced according to a method according to any one of Claims 1 to 10 for the manufacture of components for the oil and gas and chemical process industries.

15. Use of a powder produced according to a method according to any one of Claims 1 to 10 for the manufacture of valves or flanges.