POLYBUTYLENE SUCCINATE AND POLYBUTYLENE SUCCINATE CO-ADIPATE COMPOSITE MATERIAL AND THE COMPOSTABLE ITEM CONTAINING THIS

DE502020009619D1Active Publication Date: 2024-11-14SPC SUNFLOWER PLASTIC COMPOUND GMBH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
DE502020009619
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-04-04
Filing Date
2020-03-27
Publication Date
2024-11-14
Estimated Expiration
2040-03-27

AI Technical Summary

Technical Problem

Current biodegradable plastics, such as polybutylene succinate and polybutylene succinate-co-adipate, lack optimal mechanical properties and biodegradability at low temperatures, making them unsuitable for compostable disposable items that require specific degradation rates.

Method used

A composite material or compound comprising a polymer blend of polybutylene succinate and polybutylene succinate-co-adipate, with varying mass ratios, is developed to enhance mechanical properties and biodegradability, allowing for tailored degradation rates by adjusting the proportion of each polymer in the blend.

Benefits of technology

The composite material exhibits improved toughness, strength, and biodegradability, enabling the production of compostable disposable items that can decompose within desired time frames, from short-term to long-term, depending on the blend ratio.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The present invention relates to a disposable article comprising or consisting of a composite material or compound comprising a polymer mixture or polymer blend comprising polybutylene succinate and polybutylene succinate co-adipate, as well as one or more filler components, as well as to a method for producing the aforementioned composite material or compound or the aforementioned disposable article. The invention also relates to the use of the composite material or compound for producing a disposable article, in particular a compostable one.

[0002] Polybutylene succinate is a plastic made from 1,4-butanediol and succinic acid. Polybutylene succinate has extremely useful mechanical properties quite similar to polyethylene, such as a low modulus of elasticity and high toughness. Polybutylene succinate is also known to be biodegradable, but the conditions required for this, such as the temperatures required for extensive biodegradation within a practically usable period of approximately three months, and certainly no more than a year, are not optimal for extensive use as a compostable material.

[0003] For some time now, a copolymer of polybutylene succinate, polybutylene succinate-co-adipate (also referred to as "poly(butylene succinate-co-adipate)" or "poly(1,4-butylene adipate-co-1,4-butylene succinate)"), has been investigated for use as a compostable plastic. This copolymer of polybutylene succinate contains monomer units formed from esters of succinic acid residues with butanediol residues, as well as monomer units formed from esters of adipic acid residues with butanediol residues. Polybutylene succinate-co-adipate exhibits similar mechanical properties to polybutylene succinate, but, for example, a lower tensile strength. However, it is known that polybutylene succinate-co-adipate is more biodegradable than polybutylene succinate (see, for example, M. Puchalski et al., Polymers 2018, 10, 251-262).Further information on the structures and properties of polybutylene succinate and polybutylene succinate-co-adipate can also be found in the book "Synthetic Biodegrable Polymers", B. Rieger et al., Springer Science & Business Media, 2012.

[0004] The prior art already contains proposals for combining polybutylene succinate or polybutylene succinate-co-adipate with other polymeric compounds to modify their properties for specific applications. Examples include combinations with starch, polylactic acid (polylactide), or poly(butylene adipate-co-terephthalate).

[0005] Document WO 99 / 45067 A1 relates to a polylactic acid composition and a film made therefrom. Document JP 2007 002011 A discloses biodegradable polymer films. Examples 4 and 13 disclose compositions containing a 50 / 50 blend of PBS and PBSA, talc (Example 4), and calcium carbonate (Example 13), respectively.

[0006] It was a primary object of the present invention to provide a disposable article comprising a material which has excellent mechanical properties (in particular high toughness, strength and tensile strength) and good formability, combined with particularly good biodegradability, even at comparatively low temperatures, approximately ≤ 50 °C, and which is excellently suited for the production of compostable articles such as disposable articles, or of articles which are degradable in the medium or long term.A further, specific, object of the present invention was to provide methods for the production of such a disposable article. It has now surprisingly been found that the primary object as well as further objects and / or sub-objects of the present invention are achieved by a disposable article as defined in the appended claims, comprising or consisting of a composite material or compound comprising as polymer component a polymer mixture or a polymer blend comprising. Polybutylene succinate and polybutylene succinate-co-adipate.

[0007] Our own investigations have shown that a polymer mixture or polymer blend comprising the two components polybutylene succinate and polybutylene succinate-co-adipate can be excellently processed into compounds or composite materials that are easy to shape. The properties of the polymer mixture or polymer blend can be advantageously and specifically varied in a practice-relevant manner by varying the proportions of polybutylene succinate or polybutylene succinate-co-adipate. Furthermore, our own investigations have found that a composite material or compound made from the aforementioned polymer mixture or polymer blend, or an article or disposable article made from it, is significantly more biodegradable than a homopolymer of polybutylene succinate (or a composite material or compound made from this homopolymer) considered for comparison.

[0008] The invention, as well as preferred combinations of preferred parameters, properties, and / or components of the present invention, are defined in the appended claims. Preferred aspects of the present invention are also specified or defined in the following description and in the examples.

[0009] For the purposes of the present invention and as is customary in the art, a polymer mixture or polymer blend is understood to be a physical mixture of two or more (in the case of the present invention, in particular two) base polymers. This preferably results in a mixture in which the two base polymers are molecularly distributed or microscopically dispersed. Such a polymer mixture or polymer blend is therefore also referred to as a "polymer alloy." Preferably, no new chemical bonds are formed between the base polymers involved in such a polymer mixture or polymer blend. The properties of such a polymer mixture or polymer blend may nevertheless differ from the properties or the purely additive properties of the base polymers involved. The polymer mixture or polymer blend used hereThe polymer blend used here can be produced in a manner known per se to those skilled in the art, for example by compounding the base polymers involved, polybutylene succinate and polybutylene succinate-co-adipate. In this text, the terms "polymer mixture" and "polymer blend" are used synonymously.

[0010] A polymer mixture or corresponding polymer blend as described above is preferred and used in the disposable article according to the invention, wherein the mass ratio of the polybutylene succinate (hereinafter also referred to as "PBS") present in the polymer mixture or polymer blend to the polybutylene succinate-co-adipate (hereinafter also referred to as "PBSA") present in the polymer mixture or polymer blend is in the range from 10:90 to 90:10, preferably from 20:80 to 80:20, more preferably from 30:70 to 70:30, particularly preferably from 40:60 to 60:40 and very particularly preferably from 45:55 to 55:45. In a particularly preferred embodiment of the present invention, the mass ratio of the PBS present in the above-mentioned polymer mixture or the above-mentioned polymer blend to the PBSA present in the polymer mixture or the polymer blend is 50:50 (or 1:1).

[0011] By varying the mass ratios of the PBS present in the polymer mixture or in the polymer blend to the PBSA present in the polymer mixture or in the polymer blend, preferably within the ranges specified above, the biodegradation rate or the composting rate of the polymer mixture or the corresponding polymer blend used in the disposable article according to the invention or of a composite material or compound containing this polymer mixture or this polymer blend (or of an article containing the aforementioned materials) can be adjusted and specifically tailored to the respective desired intended use of the polymer mixture or the polymer blend.

[0012] For example, a polymer mixture or a polymer blend in which the mass ratio of the PBS present therein to the PBSA present therein is 30:70 is biodegraded more quickly than a polymer mixture or a polymer blend in which the mass ratio of the PBS present therein to the PBSA present therein is 50:50, so that such a polymer mixture or such a polymer blend is suitable as a starting material, in particular for the production of articles or disposable articles which are intended to decompose after a relatively short time, such as disposable plant pots.

[0013] On the other hand, for example, a polymer mixture or a polymer blend in which the mass ratio of the PBS present therein to the PBSA present therein is 70:30, is biodegraded more slowly than a polymer mixture or a polymer blend in which the mass ratio of the PBS present therein to the PBSA present therein is 50:50, so that such a polymer mixture or such a polymer blend is particularly suitable as a starting material for the production of articles or disposable articles which are intended to decompose after a relatively long period of time, such as browsing protection on trees.

[0014] Therefore, a polymer mixture or a corresponding polymer blend used in the disposable article according to the invention or a polymer mixture or a polymer blend described as preferred in this text is also preferred, wherein the mass ratio of the polybutylene succinate present in the polymer mixture or the polymer blend to the polybutylene succinate-co-adipate present in the polymer mixture or the polymer blend is: in the range from 10:90 to 40:60, preferably from 10:90 to 35:65 and particularly preferably from 20:80 to 35:65, or in the range from 90:10 to 60:40, preferably from 90:10 to 65:35 and particularly preferably from 80:20 to 65:35.

[0015] A polymer mixture or a corresponding polymer blend described above used in the disposable article according to the invention is preferred (or a polymer mixture or a polymer blend described as preferred in this text), wherein the polybutylene succinate structural components (monomers) of formula I and / or (preferably "and") the polybutylene succinate-co-adipate comprises structural components of the formula II includes.

[0016] The structural components of formula II represent combinations of two comonomers (each enclosed in square brackets), which are (i) based on residues of 1,4-butanediol and succinic acid linked by an ester bond, and (ii) based on residues of 1,4-butanediol and adipic acid linked by an ester bond. The comonomer, which is based on residues of 1,4-butanediol and succinic acid linked by an ester bond, corresponds to the above-mentioned structural component (monomer) of formula (I).

[0017] The polybutylene succinate to be used in the disposable article according to the invention and the polybutylene succinate-co-adipate to be used in the disposable article according to the invention can each be present independently of one another (depending on the respective manufacturing conditions used) in a linear polymer structure or copolymer structure (unbranched) or in a branched polymer structure or copolymer structure.

[0018] Also preferred is a polymer mixture or polymer blend described above used in the disposable article according to the invention (or a corresponding polymer mixture or polymer blend described as preferred in this text), wherein the polybutylene succinate present in the polymer mixture or polymer blend and / or the polybutylene succinate-co-adipate present in the polymer mixture or polymer blend are each independently a weight-average molecular weight M w in the range from 50,000 to 150,000, preferably in the range from 75,000 to 140,000, and / or a melt flow rate MFR in the range from 0.5 to 50 g / 10 min, preferably from 1 to 40 g / 10 min, determined according to DIN EN ISO 1133-1:2011, method A.

[0019] The aforementioned melt mass flow rate (MFR) is preferably determined in the context of the present invention at a temperature of 190 °C and a test load of 2.16 kg. Preferably, all melt mass flow rates (MFR) specified in the context of this invention are determined according to DIN EN ISO 1133-1:2011, Method A, and at a temperature of 190 °C and a test load of 2.16 kg.

[0020] The present invention particularly relates to a disposable article comprising or consisting of a composite material or compound comprising as polymer component polybutylene succinate (as described or defined above) and polybutylene succinate-co-adipate (as described or defined above), and / or (preferably "or") a polymer mixture or polymer blend according to the invention described above (or a polymer mixture or polymer blend according to the invention described as preferred in this text), in a total amount in the range from 30 to 75% by mass, preferably from 35 to 70% by mass, based on the total mass of the composite material or compound, and organic and inorganic filler components as defined below and in the appended claims.

[0021] With regard to preferred embodiments of a composite material or compound mentioned above used in the disposable article according to the invention, the explanations given above for the polymer mixture or the corresponding polymer blend used in the disposable article according to the invention, in particular concerning possible preferred embodiments and possible or preferred combinations, apply accordingly (where appropriate, analogously), and vice versa.

[0022] The mass ratio of the polybutylene succinate present in the above-mentioned polymer component of the composite material or compound to the polybutylene succinate-co-adipate present in the polymer component of the composite material or compound is accordingly preferably also in the range from 10:90 to 90:10, more preferably from 20:80 to 80:20, particularly preferably from 30:70 to 70:30, very particularly preferably from 40:60 to 60:40 and even more preferably from 45:55 to 55:45.

[0023] In general, within the context of the present invention, the term "a polybutylene succinate present in the polymer component of the composite material or compound according to the invention" refers to both a polybutylene succinate present separately (individually) in the composite material or compound (used in the disposable article according to the invention) and a polybutylene succinate present in the composite material or compound (used in the disposable article according to the invention) in the form of a polymer mixture or polymer blend (i.e., as a base polymer component of a polymer mixture or polymer blend). The same applies to the term "a polybutylene succinate co-adipate present in the polymer component of the composite material or compound according to the invention."

[0024] In a preferred embodiment of the present invention, the mass ratio of the polybutylene succinate present in the above-mentioned polymer component of the composite material or compound to the polybutylene succinate-co-adipate present in the polymer component of the composite material or compound is in the range from 10:90 to 40:60, preferably from 10:90 to 35:65 and particularly preferably from 20:80 to 35:65, or in the range from 90:10 to 60:40, preferably from 90:10 to 65:35 and particularly preferably from 80:20 to 65:35.

[0025] As stated above, a composite material or compound used in the disposable article according to the invention, wherein the mass ratio of the polybutylene succinate present in the polymer component to the polybutylene succinate co-adipate present in the polymer component is in the range from 10:90 to 40:60, preferably from 10:90 to 35:65 and particularly preferably from 20:80 to 35:65, is preferably suitable for the production of relatively rapidly biodegradable articles or disposable articles.

[0026] In contrast, a composite material or compound used in the disposable article according to the invention, wherein the mass ratio of the polybutylene succinate present in the polymer component to the polybutylene succinate co-adipate present in the polymer component is in the range from 90:10 to 60:40, preferably from 90:10 to 65:35 and particularly preferably from 80:20 to 65:35, is preferably suitable for the production of relatively slowly biodegradable articles or disposable articles.

[0027] The weight-average molar mass M w of the polybutylene succinate present in the above-mentioned polymer component of the composite material or compound is preferably in the range from 50,000 to 150,000, preferably from 75,000 to 140,000. The weight-average molar mass M w of the polybutylene succinate-co-adipate present in the polymer component of the composite material or compound according to the invention is likewise preferably in the range from 50,000 to 150,000, preferably in the range from 75,000 to 140,000.

[0028] The melt mass flow rate MFR of the polybutylene succinate present or to be used in the above-mentioned polymer component of the composite material or compound is preferably in the range from 0.5 to 50 g / 10 min, particularly preferably from 1 to 40 g / 10 min. The melt mass flow rate MFR of the polybutylene succinate-co-adipate present or to be used in the polymer component of the composite material or compound according to the invention is likewise preferably in the range from 0.5 to 50 g / 10 min, particularly preferably from 1 to 40 g / 10 min.

[0029] In a further preferred embodiment of the present invention, the polybutylene succinate present in the above-mentioned polymer component of the composite material or compound and / or the polybutylene succinate-co-adipate present in the polymer component of the composite material or compound, each independently of one another, has a melt mass flow rate MFR of in the range of ≥ 0.5 to ≤ 3.5 g / 10 min, preferably in the range of ≥ 1 to ≤ 3 g / 10 min, and / or (preferably "or") in the range of > 3.5 g / 10 min to ≤ 12 g / 10 min, preferably in the range of ≥ 4 g / 10 min to ≤ 10 g / 10 min, and / or (preferably "or") in the range of > 12 g / 10 min to ≤ 50 g / 10 min, preferably in the range of ≥ 15 g / 10 min to ≤ 35 g / 10 min.

[0030] Our own investigations have shown that the processing properties of the composite material or compound according to the invention can be specifically influenced by the selection and combination of polybutylene succinate and / or polybutylene succinate-co-adipate, which each have melt mass flow rates MFR in the ranges specified above: For example, a composite material or compound used in the disposable article according to the invention, in which the polybutylene succinate present in its polymer component and / or (in particular "and") the polybutylene succinate-co-adipate present in its polymer component, in each case independently of one another, has a melt mass flow rate MFR in the range of ≥ 0.5 to ≤ 3.5 g / 10 min, preferably in the range of ≥ 1 to ≤ 3 g / 10 min, is excellently suited for processing by thermoforming, film extrusion, blown film extrusion and / or extrusion blow molding.

[0031] A composite material or compound used in a disposable article according to the invention, wherein the polybutylene succinate present in its polymer component and / or (in particular "and") the polybutylene succinate-co-adipate present in its polymer component, each independently of one another, has a melt mass flow rate MFR in the range of > 3.5 g / 10 min to ≤ 12 g / 10 min, preferably in the range of ≥ 4 g / 10 min to ≤ 10 g / 10 min, is particularly suitable for processing in the foam extrusion process.

[0032] A composite material or compound used in a disposable article according to the invention, wherein the polybutylene succinate present in its polymer component and / or (in particular "and") the polybutylene succinate-co-adipate present in its polymer component, each independently of one another, has a melt mass flow rate MFR in the range of > 12 g / 10 min to ≤ 50 g / 10 min, preferably in the range of ≥ 15 g / 10 min to ≤ 35 g / 10 min, is excellently suited for processing by injection molding.Likewise excellently suited for processing by injection molding is a composite material or compound used in a disposable article according to the invention, wherein the polybutylene succinate present in its polymer component has a melt mass flow rate MFR in the range from > 12 g / 10 min to ≤ 50 g / 10 min, preferably from ≥ 15 g / 10 min to ≤ 35 g / 10 min, and wherein the polybutylene succinate-co-adipate present in its polymer component has a melt mass flow rate MFR in the range from ≥ 0.5 g / 10 min to ≤ 10 g / 10 min, preferably from ≥ 1 g / 10 min to ≤ 5 g / 10 min.Furthermore, a composite material or compound used in a disposable article according to the invention is excellently suited for processing by injection molding, wherein the polybutylene succinate present in its polymer component has a melt mass flow rate MFR in the range from ≥ 0.5 g / 10 min to ≤ 10 g / 10 min, preferably from ≥ 1 g / 10 min to ≤ 5 g / 10 min, and wherein the polybutylene succinate-co-adipate present in its polymer component has a melt mass flow rate MFR in the range from > 12 g / 10 min to ≤ 50 g / 10 min, preferably from ≥ 15 g / 10 min to ≤ 35 g / 10 min.

[0033] Preferably, within the scope of the present invention, in a composite material or compound used in a disposable article according to the invention (or in a corresponding polymer mixture or a polymer blend), its processing properties or the material properties of an article or disposable article produced therefrom can be specifically adjusted by adding to its polymer component: (i) selecting a suitable or preferred mass ratio of the polybutylene succinate present therein to the polybutylene succinate-co-adipate present therein and simultaneously (ii) selecting polybutylene succinate and / or polybutylene succinate-co-adipate with suitable or preferred melt mass flow rates MFR in each case.

[0034] In many cases, a composite material or compound described above used in a disposable article according to the invention is also preferred (or a composite material or compound described as preferred in this text), wherein the mass ratio of the polybutylene succinate present in the polymer component of the composite material or compound to the polybutylene succinate-co-adipate present in the polymer component of the composite material or compound is in the range from 10:90 to 40:60, preferably from 10:90 to 35:65 and particularly preferably from 20:80 to 35:65, and the polybutylene succinate present in the polymer component of the composite material or compound and / or (preferably "and") the polybutylene succinate-co-adipate present in the polymer component of the composite material or compound, in each case independently of one another, has a melt mass flow rate MFR in the range from ≥ 0.5 to ≤ 3.5 g / 10 min, preferably in the range from ≥ 1 to ≤ 3 g / 10 min.

[0035] Likewise, in many cases, a composite material or compound described above used in a disposable article according to the invention (or a composite material or compound described as preferred in this text) is preferred, wherein the mass ratio of the polybutylene succinate present in the polymer component of the composite material or compound to the polybutylene succinate-co-adipate present in the polymer component of the composite material or compound is in the range from 90:10 to 60:40, preferably from 90:10 to 65:35 and particularly preferably from 80:20 to 65:35, and the polybutylene succinate present in the polymer component of the composite material or compound and / or (preferably "and") the polybutylene succinate-co-adipate present in the polymer component of the composite material or compound, in each case independently of one another, has a melt mass flow rate MFR in the range from > 12 g / 10 min to ≤ 50 g / 10 min, preferably in the range from ≥ 15 g / 10 min to ≤ 35 g / 10 min.

[0036] One or more particulate and / or fibrous, cellulose-containing materials are considered as organic filler components usable in a disposable article according to the invention. One or more particulate inorganic materials selected from the group consisting of calcium carbonate, clay minerals, and silicates are considered as inorganic filler components usable in a disposable article according to the invention.

[0037] Our own investigations have shown that the at least one particulate and / or fibrous cellulose-containing material usable in a disposable article according to the invention as an organic filler component (in particular the cellulose-containing materials indicated below as preferred) contributes in a particular way to the mechanical property profile of the composite material or compound according to the invention, or of articles produced therefrom.

[0038] By varying the mass fraction of the at least one particulate and / or fibrous, cellulose-containing material as an organic filler component in the composite material or compound used in a disposable article according to the invention, it is possible, for example, to produce rather thin-walled articles from the corresponding composite material or compound - for example, if a total amount of at least one cellulose-containing material in the range of 5 to 35 mass%, based on the total mass of the composite material or compound, is used. Alternatively, in many cases, rather thick-walled articles (e.g., urns) can also be produced - for example, if a total amount of at least one cellulose-containing material in the range of 25 to 50 mass%, based on the total mass of the composite material or compound, is used.By varying the content of the composite material or compound of at least one particulate and / or fibrous, cellulose-containing material usable according to the invention as an organic filler component, the mechanical properties of the composite material or compound, or the mechanical properties of an article according to the invention produced from the composite material or compound, can therefore be advantageously controlled or adjusted.

[0039] Furthermore, our own investigations have shown that the at least one particulate inorganic material usable according to the invention as an inorganic filler component (in particular the particulate inorganic materials specified below as preferred) contributes in a particular way to the ductility properties and / or the oxygen barrier effect of the composite material or compound according to the invention, or of articles produced therefrom. For example, our own investigations have shown that an exemplary article according to the invention, consisting of a composite material or compound used according to the invention, had an oxygen transmission rate of <0.01 cm 3 / article*day*bar, while a corresponding article containing no inorganic fillers had an oxygen transmission rate of 0.1 cm 3 / article*day*bar.

[0040] Thus, a composite material or compound, or an article made therefrom, with a low content of at least one particulate inorganic material - for example, containing a total amount of at least one particulate inorganic material in the range of 3 to 10 mass%, based on the total mass of the composite material or compound - exhibits comparatively high ductility (plastic deformability), low brittleness, and a relatively low barrier effect against oxygen. In contrast, a composite material or compound used in a disposable article according to the invention exhibitsa disposable article made therefrom, with a higher content of at least one particulate inorganic material - for example containing a total amount of at least one particulate inorganic material in the range of 12.5 to 25% by mass, based on the total mass of the composite material or compound, has a comparatively low ductility, a comparatively higher brittleness and a comparatively higher barrier effect against oxygen. By varying the content of the at least one particulate inorganic material that can be used according to the invention as an inorganic filler component in the composite material or compound according to the invention, the ductility properties and / or the barrier properties against oxygen of the composite material or compound, respectively, can therefore be advantageously improved.which control or adjust the ductility properties and / or the barrier properties against oxygen of a disposable article according to the invention made from the composite material or compound according to the invention.

[0041] If, for example, disposable items such as coffee capsules are to be produced from the composite material or compound, it has often proven advantageous to use a higher content (see above) of at least one particulate inorganic material (e.g. kaolin) in the corresponding composite material or compound, because in this way such coffee capsules are better suited for their intended use and can, for example, be pierced more easily.

[0042] A composite material or compound used in a disposable article according to the invention (or a composite material or compound used accordingly and described as preferred in this text) comprises as filler components at least one particulate and / or fibrous, cellulose-containing material (preferably as an organic filler component) and at least one particulate inorganic material (preferably as an inorganic filler component) selected from the group consisting of calcium carbonate, clay minerals and silicates.

[0043] A disposable article according to the invention comprises a composite material or a compound (or a composite material or a compound described above or below as preferred) comprising C1) as polymer component polybutylene succinate and polybutylene succinate-co-adipate, and / or a polymer mixture or a polymer blend described above (or a polymer mixture or a polymer blend described as preferred in this text), as defined in the appended claims, in a total amount in the range from 30 to 75% by mass, preferably from 35 to 70% by mass, based on the total mass of the composite material or compound, and C2) as first filler component (preferably as organic filler component) at least one particulate and / or fibrous, cellulose-containing material, in a total amount in the range from 3 to 50% by mass, preferably from 3.5 to 47.5% by mass, particularly preferably from 5 to 45% by mass, based on the total mass of the composite material or compound.

[0044] Also preferred is a disposable article according to the invention as described above, comprising a composite material or a compound (or a composite material or a compound described above or below as preferred), wherein the particulate and / or fibrous, cellulose-containing material comprises one or more natural fibers and / or one or more regenerated cellulose fibers and / or is selected from the group consisting of cellulose, wood, flax, hemp, sunflower seed shells, bamboo, jute, kenaf, ramie, coconut fibers, fibers from stems of the broom plant, fibers from stems of the hop plant, fibers from leaves and infructescences of cattail reeds and mixtures thereof, wherein preferably the particulate, cellulose-containing material is selected from the group consisting of wood, flax, hemp, sunflower seed shells (preferably flour from sunflower seed shells) and mixtures thereof.

[0045] Particularly preferred is a composite material or compound as described above and used in a disposable article according to the invention (or a composite material or compound described above or below as preferred), wherein the particulate, cellulose-containing material comprises flour from sunflower seed shells. Sunflower seed shells are generated in large quantities as an industrial waste product, for example in food production. The use as an organic filler component in the composite material or compound used in the disposable article according to the invention therefore combines the advantages that (i) an otherwise unused waste product is put to industrial use and that such a filler component is not only (ii) biodegradable, but that its decomposition also additionally (iii) produces valuable, biodegradable degradation products.

[0046] In the context of the present invention and as is customary in the art, regenerated cellulose fibers are understood to be fibers produced from naturally occurring, renewable, cellulose-containing raw materials through chemical processes. These are primarily cellulose derivatives from wood. In the context of the present invention, regenerated cellulose fibers preferably include the materials (or fibers made from the materials) viscose, modal, lyocell, and cupro, particularly preferably lyocell.

[0047] Viscose fibers are synthetic fibers (regenerated fibers) that are industrially produced using the well-known viscose process, a widely used wet spinning technique. The starting raw material for the viscose process is cellulose, predominantly in the form of wood, from which the highly pure cellulose is extracted using various processes.

[0048] Like viscose fibers, modal fibers are also made 100 percent from cellulose, but unlike other regenerated fibers, they are primarily made from beechwood. The raw material is debarked beechwood, which is then shredded to separate the lignin. By modifying the manufacturing process, modal fibers achieve greater fiber strength and improved fiber properties than other cellulose fibers. Modal fibers also have higher moisture absorption and dry quickly.

[0049] Lyocell is a well-known, industrially produced regenerated cellulose fiber made from cellulose, produced using the well-known direct solvent process. It is used primarily for the production of textiles and nonwovens. Lyocell fibers exhibit high dry and wet strength, are soft, and absorb moisture very well.

[0050] Cupro, also known as copper silk or copper fiber, is a textile fiber made from regenerated cellulose. Its properties are comparable to those of viscose. Cupro fibers are primarily used for textile linings because they are breathable, hygroscopic, and do not build up static electricity. Furthermore, fabrics made from them have a silky, soft feel and are smooth and shiny. Cupro is typically produced using the copper oxide-ammonia process (Cuoxam process).

[0051] A composite material or compound used in a disposable article according to the invention described above (or a corresponding composite material or compound described as preferred in this text) additionally comprises C3) as a second filler component, at least one particulate inorganic material selected from the group consisting of calcium carbonate, clay minerals, and silicates, in a total amount in the range of 12.5 to 25 mass%, based on the total mass of the composite material (as defined in the appended claims). and preferably C4) further additives and / or auxiliaries, preferably selected from the group consisting of adhesion promoters (preferably maleic anhydride), waxes, lubricants, antioxidants, and light stabilizers, preferably in a total amount in the range of 0.1 to 10 mass%, more preferably 0.2 to 5 mass%, based on the total mass of the composite material.

[0052] Furthermore, it was found that particulate inorganic material, preferably with a high average aspect ratio of its particles, as a second filler component imparts particularly good strength properties to the composite material or compound according to the invention or to the articles produced therefrom, such as disposable articles.

[0053] Therefore, a disposable article according to the invention as described above is also preferred, comprising a composite material or compound as described above or a composite material or compound described as preferred in this text, wherein the at least one particulate inorganic material and / or the second filler component C3) comprise or comprises at least one particulate inorganic material, which is selected from the group consisting of calcium carbonate, talc, talc, kaolin, iron mica, wollastonite mica, muscovite mica, phlogopite mica and mixtures thereof, and is preferably selected from the group consisting of talc, kaolin, iron mica, wollastonite mica, muscovite mica, phlogopite mica and mixtures thereof and / or whose particles have an average aspect ratio of ≥ 5:1, preferably of ≥ 7:1 and particularly preferably of ≥ 10:1.

[0054] In the context of the present invention (as is customary in the art), the "aspect ratio" is preferably understood to mean the ratio between the length (height) and the (smallest) lateral dimension of a particle under consideration.

[0055] In the context of the present invention, the "average aspect ratio" is preferably understood (as is customary in the art) to mean the mean value of the aspect ratios of a plurality of particles present in a sample. For the purposes of the present invention, the average aspect ratio is preferably determined by dynamic image analysis of a plurality of particles, preferably using an automated particle sizer such as the Analysette 28 ImageSizer particle sizer from Fritsch GmbH, Germany.

[0056] The present invention thus relates in particular to a disposable article according to the invention described above, comprising or consisting of a composite material or compound (or a composite material or compound described above or below as preferred) comprising C1) as polymer component, polybutylene succinate and polybutylene succinate-co-adipate, and / or a polymer mixture or a polymer blend described above (or a polymer mixture or polymer blend described as preferred in this text), in a total amount in the range from 30 to 75% by mass, particularly preferably from 35 to 70% by mass, based on the total mass of the composite material or compound, wherein preferably the mass ratio of the polybutylene succinate present in the polymer mixture or polymer blend to the polybutylene succinate-co-adipate present in the polymer mixture or polymer blend is in the range from 10:90 to 90:10, preferably from 20:80 to 80:20, more preferably from 30:70 to 70:30, particularly preferably from 40:60 to 60:40 and very particularly preferably from 45:55 to 55 : 45; C2) as the first filler component (preferably as an organic filler component) at least one particulate and / or fibrous,Cellulose-containing material, preferably selected from the group consisting of cellulose, wood, flax, hemp, sunflower seed shells, bamboo, jute, kenaf, ramie, coconut fibers, fibers from stems of the broom plant, fibers from stems of the hop plant, fibers from leaves and fruiting heads of cattail reeds and mixtures thereof, preferably in a total amount in the range of 3 to 50% by mass, preferably from 3.5 to 47.5% by mass, particularly preferably from 5 to 45% by mass, based on the total mass of the composite material or compound, C3) as a second filler component at least one particulate inorganic material selected from the group consisting of calcium carbonate, clay minerals and silicates, in a total amount in the range of 12.5 to 25% by mass, based on the total mass of the composite material, and preferably C4) further additives and / or auxiliaries, preferably selected from the group consisting of adhesion promoters, (preferably maleic anhydride),Waxes, lubricants, antioxidants and light stabilizers, preferably in a total amount in the range of 0.1 to 10 mass%, preferably 0.2 to 5 mass%, based on the total mass of the composite material.

[0057] The disposable article of the present invention is preferably compostable.

[0058] With regard to preferred embodiments of a disposable article according to the invention mentioned above, the explanations given above for the polymer mixture or polymer blend described above and / or for the composite material or compound described above, in particular concerning (in each case) possible preferred embodiments and (in each case) possible or preferred combinations, apply accordingly (where appropriate, analogously), and vice versa.

[0059] The disposable article specified above is - due to its content of PBS and PBSA - generally excellently biodegradable and preferably compostable according to the criteria of DIN EN 13432: 2000-12.

[0060] Disposable articles within the meaning of the present invention preferably comprise coffee capsules.

[0061] The present invention further relates to the use of a composite material or compound described above (or a corresponding composite material or compound described as preferred in this text) for or in the production of a, preferably compostable, disposable article.

[0062] With regard to preferred embodiments of a use according to the invention mentioned above for or in the production of a disposable article, the explanations given above for the disposable article according to the invention, for the polymer mixture or polymer blend described above and / or for the composite material or compound described above apply accordingly (where appropriate, analogously), and vice versa.

[0063] The present invention also relates to a process for producing a composite material or compound as described above, comprising the steps V1) Producing or providing a polymer mixture or polymer blend as described above (or a polymer mixture or polymer blend described as preferred in this text), and / or (preferably "or") polybutylene succinate and / or (preferably "and") polybutylene succinate-co-adipate, V2) Producing or providing at least one particulate and / or fibrous, cellulose-containing material as the first filler component, as described above or as preferred, V3) Producing or providing at least one particulate inorganic material as the second filler component, as described above or as preferred, V4) Combining the polymer mixture or polymer blend from step V1) and / or (preferably "or") the polybutylene succinate and / or (preferably "and") the polybutylene succinate-co-adipate from step V1) with the at least one particulate and / or fibrous,Cellulose-containing material from step V2) and additionally with the at least one particulate inorganic material from step V3), preferably comprising a compounding step, particularly preferably comprising a melt extrusion step, so that the or a composite material or the or a compound results.

[0064] With regard to preferred embodiments of the method according to the invention for producing a composite material or compound mentioned above, the explanations given above for the use of a polymer mixture or a polymer blend described above for or in the production of a composite material or compound, the use according to the invention for or in the production of a disposable article, for the disposable article according to the invention, for the polymer mixture or the polymer blend described above and / or for the composite material or compound described above apply accordingly (where appropriate, analogously), and vice versa.

[0065] In step V1) of the above-specified inventive method for producing a composite material or compound, a polymer mixture or polymer blend described above (or a polymer mixture or polymer blend designated as preferred in this text) can be produced or provided, i.e. said polymer mixture or polymer blend can be used to produce the composite material or compound. Likewise, in step V1) (or in separate sub-steps of step V1) of the above-specified inventive method, polybutylene succinate and polybutylene succinate-co-adipate can be produced or provided separately as individual substances or polymer constituents, so that a mixture of the two polymers (or the polymer and the copolymer) with one another (and with the specified further constituents) only takes place in step V4).However, in step V1) of the above-specified inventive process, a polymer mixture or polymer blend described above can also be produced or provided and, in addition, optionally (i) either polybutylene succinate can be produced or provided separately as an individual substance or polymer component, or (ii) polybutylene succinate-co-adipate can be produced or provided separately as an individual substance or polymer component, or (iii) polybutylene succinate and polybutylene succinate-co-adipate can both be produced or provided separately as individual substances or polymer components. In this way, the polymer components produced or provided in step V1) are at least partially mixed with one another (and with the specified further components) only in step V4).

[0066] In step V4) of the above-specified process according to the invention for producing a composite material or compound, the above-specified constituents (polymer mixture or polymer blend from step V1) and / or polybutylene succinate and / or polybutylene succinate-co-adipate from step V1), at least one particulate and / or fibrous, cellulose-containing material from step V2) and at least one particulate inorganic material from step V3)) are preferably additionally combined with further additives and / or auxiliaries, preferably selected from the group consisting of adhesion promoters (preferably maleic anhydride), waxes, lubricants, antioxidants and light stabilizers.

[0067] The present invention further relates to a method for producing a disposable article, comprising the steps V5) Producing or providing a composite material or compound comprising, as polymer components, polybutylene succinate and polybutylene succinate-co-adipate and / or an above-mentioned polymer mixture or polymer blend according to the invention (or a polymer mixture or polymer blend described as preferred in this text) and one or more organic and / or inorganic filler components, wherein the production or provision of a composite material or compound is carried out by providing an above-described composite material or compound (or a composite material or compound described as preferred in this text) and / or (preferably "or") producing a composite material or compound according to an above-described process according to the invention (or according to an inventive process described as preferred in this text);and V6) molding the composite material or compound, preferably comprising at least one step selected from the group consisting of extrusion, preferably comprising film extrusion, blown film extrusion, extrusion blow molding, and foam extrusion; injection molding, deep drawing, and / or thermoforming.

[0068] With regard to preferred embodiments of the method according to the invention for producing a disposable article mentioned above, the explanations given above for the composite material or compound produced or producible by a method according to the invention mentioned above, the method according to the invention for producing a composite material or compound, the use described above of a polymer mixture or polymer blend described above for or in the production of a composite material or compound, the use according to the invention for or in the production of a disposable article, for the disposable article according to the invention, for the polymer mixture or polymer blend described above and / or for the composite material or compound described above apply, in particular with regard to (in each case) possible preferred embodiments and (in each case) possible orpreferred combinations, accordingly (if appropriate), and vice versa.

[0069] The present invention is explained in more detail below with reference to the figure and by way of examples. The following examples are intended to describe and explain the invention in more detail without limiting its scope. Figure:

[0070] Fig. 1:In Fig. 1 The test results comparing the composting rates of articles according to the invention and those not according to the invention as well as of cellulose (cf. Example 9, Table 1) are shown graphically. Examples: Example 1: Preparation of a polymer mixture or polymer blend usable in a disposable article according to the invention

[0071] 5.41 kg of polybutylene succinate of the type BioPS ™< FZ 71 PM (PTT MCC Biochem Co. Ltd, MFR = 22 g / 10 min) are mixed with 5.41 kg of polybutylene succinate-co-adipate of the type BioPS ™< FD 92 PM (PTT MCC Biochem Co. Ltd, MFR = 4 g / 10 min) and compounded together in a twin-screw extruder at a temperature in the range of 140 °C in the feed and melting zone and 180 °C downstream (whereby the melt temperature at the die plate may be higher), so that a polymer mixture or a polymer blend according to the invention is produced. Example 2: Production of a composite material or compound usable in a disposable article according to the invention

[0072] A polymer mixture or polymer blend prepared as above (see Example 1) is mixed with 6 kg of sunflower seed shell flour, 3 kg of powdered kaolin, and 180 g of maleic anhydride-based adhesion promoter, and the mixed components are compounded or mixed in a twin-screw extruder at a temperature in the range of 140 °C in the feed and melting zone and 180 °C downstream (whereby the melt temperature at the die plate may be higher), so that a composite material or a compound according to the invention (hereinafter referred to as "VM-E1") is produced that can be used in a disposable article according to the invention. Example 3: Production of a composite material or compound usable in a disposable article according to the invention by separate addition of polybutylene succinate and polybutylene succinate-co-adipate (1)

[0073] 5.41 kg of polybutylene succinate of the type BioPS™< FZ 71 PM (for details see Example 1) are mixed with 5.41 kg of polybutylene succinate co-adipate of the type BioPS™< FD 92 PM (for details see Example 1), 6 kg of sunflower seed shell flour, 3 kg of powdered kaolin and 180 g of maleic anhydride-based adhesion promoter, and the mixed components are compounded or mixed in a twin-screw extruder at a temperature in the range of 140 °C in the feed and melting zone and 180 °C downstream (whereby the melt temperature at the die plate may be higher), so that a composite material according to the invention or a compound according to the invention (hereinafter referred to as "VM-E2") is produced. Example 4: Production of a composite material or compound usable in a disposable article according to the invention by separate addition of polybutylene succinate and polybutylene succinate-co-adipate (2)

[0074] 3.25 kg of polybutylene succinate of the type BioPS™< FZ 71 PM (for details see Example 1) are mixed with 7.57 kg of polybutylene succinate co-adipate of the type BioPS™< FD 72 PM (PTT MCC Biochem Co. Ltd, MFR = 22 g / 10 min), 6 kg of sunflower seed shell flour, 3 kg of powdered kaolin and 180 g of adhesion promoter based on maleic anhydride and the mixed components are compounded in a twin-screw extruder at a temperature in the range of 140 °C in the feed and melting zone and 180 °C downstream (whereby the melt temperature at the die plate may be higher) so that a composite material according to the invention or a compound according to the invention (hereinafter referred to as "VM-E3") is produced. Example 5: Preparation of a non-inventive comparative composite material or comparative compound

[0075] 10.82 kg of polybutylene succinate of the type BioPS™< FZ 71 PM (for details see Example 1) are mixed with 6 kg of sunflower seed shell flour, 3 kg of powdered kaolin and 180 g of maleic anhydride-based adhesion promoter, and the mixed components are compounded in a twin-screw extruder at a temperature in the range of 140 °C in the feed and melting zone and 180 °C downstream (whereby the melt temperature at the die plate may be higher), so that a non-inventive comparative composite material or comparative compound (hereinafter referred to as "VM-V1") is produced. Example 6: Production of a disposable article according to the invention (1)

[0076] 2 kg of a composite material or compound (VM-E2) produced according to Example 3 above are injection molded at a temperature of 185 to 195 °C into disposable plant pots (diameter: 12 cm, height: 12 cm, mass: 42 g, each per individual article or plant pot). Disposable plant pots are obtained as disposable articles according to the invention (hereinafter referred to as "A-E1"). Example 7: Production of a disposable article according to the invention (2)

[0077] 2 kg of a composite material or compound (VM-E3) produced according to Example 4 above are injection molded at a temperature of 185 to 195 °C into disposable plant pots (diameter: 12 cm, height: 12 cm, mass: 42 g, each per individual article or plant pot). Disposable plant pots are obtained as disposable articles according to the invention. Example 8: Production of a non-inventive comparative article

[0078] 2 kg of a non-inventive composite material or compound produced according to Example 5 above are injection molded at a temperature of 185 to 195 °C into disposable plant pots (diameter: 12 cm, height: 12 cm, mass: 42 g, each per individual article or plant pot). Disposable plant pots are obtained as non-inventive comparison articles or comparison disposable articles (hereinafter referred to as "A-V1"). Example 9: Comparison of the composting rates of articles according to the invention and non-inventive articles and of cellulose

[0079] A disposable plant pot according to the invention (A-E1, starting weight: 42 g) produced according to Example 6 above, a non-inventive comparison disposable plant pot (A-V1, starting weight: 42 g) produced according to Example 8 above, and cellulose ("Z", comparison, powder as used for thin-layer chromatography) were finely ground and added to a simulated garden compost at 28 °C. Composting rates were determined according to DIN EN ISO 14855-1:2013-04 by analyzing the carbon dioxide (CO 2 ) released during composting.

[0080] For this purpose, the amount of carbon dioxide released during composting was determined over an observation period, compared to the amount of carbon dioxide released during the decomposition of the cellulose, and thus the relative degradation rate of the samples (A-E1 or A-V1) compared to the degradation rate of the cellulose (reference) was determined.

[0081] The composting progress values ​​for items A-E1 and A-V1, as well as for cellulose, determined as above, were each expressed as "% of the theoretically possible total carbon dioxide amount" and plotted against the number of days elapsed since the start of the experiment as composting rates in Table 1 below. A graphical representation of the results is shown in Figure 1.

[0082] Sampling for the non-inventive comparative article A-V1 was discontinued after 110 days because a significant stagnation of carbon dioxide formation caused by biological degradation was observed.

[0083] After 117 days from the start of the experiment, fresh simulated garden compost was added to the test mixtures of article A-E1 and the cellulose reference to compensate for the declining microbial activity. Table 1 : Determination of composting rates Days since start of trial Z [% CO 2 formation] A-V1 [% CO 2 formation] A-E1 [% CO 2 formation] 0 . / . . / . . / . 5 23,8 1,5 1,9 10 35,3 2,6 4,4 20 57,9 5,5 13,8 30 75,8 8,1 22,9 40 84,0 10,5 30,5 53 88,1 12,7 36,9 90 91 16,4 50,9 105 92,1 16,7 54,5 120 93,7 No data found 58,1 159 94,9 No data found 69,8 202 96,0 No data found 78,4 245 96,9 No data found 83,0 299 97,7 No data found 86,1 330 97,8 No data found 87,7

[0084] The data in Table 1 above show that CO2 formation through biodegradation is significantly slower for the non-inventive comparative article A-V1 than for the inventive article A-E1 or for cellulose. Already after 80 days from the start of the test, a significantly slower biodegradation was observed for the non-inventive comparative article A-V1. At the time the test was terminated after 110 days (see also above), only approximately 16% by mass of the organic components (comprising the polybutylene succinate and the sunflower seed shells) of the non-inventive comparative article A-V1 had actually been biodegraded.

[0085] From the data in Table 1 above, it is also evident that the mass loss due to biodegradation for the inventive article A-E1 is indeed slower than for cellulose, but that at the end of the test (after 365 days) the mass loss due to biodegradation for the inventive article A-E1 was approximately 90% by mass of the organic components (comprising the polybutylene succinate, polybutylene succinate-co-adipate and the sunflower seed shells) of the inventive article A-E1 and thus reached > 90% of the corresponding value for cellulose.

[0086] From this result, it can be concluded that the increase in the composting rate as well as the increase in the proportion of composted mass for the inventive article A-E1 compared to the non-inventive comparative article A-V1 is due to the additional content of polybutylene succinate-co-adipate in the inventive article A-E1 and that the extent of this increase in the composting rate as well as the extent of this increase in the proportion of composted mass was higher than would have been expected for a purely additive effect of the additional content of polybutylene succinate-co-adipate in the inventive article A-E1 (in addition to the polybutylene succinate used in the non-inventive comparative article A-V1).

Claims

1. Single-use article, preferably coffee capsule, comprising or consisting of a composite material or compound as claimed in either of claims 5 and 6, comprising C1) as polymer constituent polybutylene succinate and polybutylene succinate-co-adipate, and / or a polymer mixture or a polymer blend, comprising - polybutylene succinate and - polybutylene succinate-co-adipate, wherein the mass ratio of the polybutylene succinate present in the polymer mixture to the polybutylene succinate-co-adipate present in the polymer mixture is in the range from 10:90 to 90:10, in a total amount in the range from 30% to 75% by mass based on the total mass of the composite material or compound, C2) as first filler constituent at least one particulate and / or fibrous, cellulose-containing material, in a total amount in the range from 3% to 50% by mass based on the total mass of the composite material or compound, and C3) as second filler constituent at least one particulate inorganic material selected from the group consisting of calcium carbonate, clay minerals and silicates, in a total amount in the range from 12.5% to 25% by mass based on the total mass of the composite material.

2. Single-use article as claimed in claim 1, wherein the mass ratio of the polybutylene succinate present in the polymer constituent to the polybutylene succinate-co-adipate present in the polymer constituent is in the range from 20:80 to 80:20, preferably from 30:70 to 70:30, especially preferably from 40:60 to 60:40 and most preferably from 45:55 to 55:45.

3. Single-use article as claimed in either of the preceding claims, wherein - the polybutylene succinate comprises structural constituents of the formula I and / or - the polybutylene succinate-co-adipate comprises structural constituents of the formula II 4. Single-use article as claimed in any of the preceding claims, wherein the polybutylene succinate present in the polymer constituent and / or the polybutylene succinate-co-adipate present in the polymer constituent each independently have - a melt flow rate MFR in the range from 0.5 to 50 g / 10 min, preferably from 1 to 40 g / 10 min, determined to DIN EN ISO 1133-1:2011, Method A.

5. Single-use article as claimed in any of the previous claims, wherein - the polymer constituent C1) is present in a total amount in the range from 35% to 70% by mass, based on the total mass of the composite material or compound, and - the first filler constituent C2) is present in a total amount in the range from 3.5% to 47.5% by mass, preferably from 5% to 45% by mass, based on the total mass of the composite material or compound.

6. Single-use article as claimed in any of the previous claims, wherein the particulate and / or fibrous cellulose-containing material - comprises one or more natural fibers and / or one or more regenerated cellulose fibers and / or - is selected from the group consisting of cellulose, wood, flax, hemp, sunflower seed shells, bamboo, jute, kenaf, ramie, coconut fibers, fibers from stems of the gorse plant, fibers from stems of the hop plant, fibers from leaves and infructescences of bulrushes, and mixtures thereof, wherein the particulate and / or fibrous cellulose-containing material is selected from the group consisting of wood, flax, hemp, sunflower seed shells, and mixtures thereof.

7. Single-use article as claimed in any of the previous claims, wherein the composite material or compound additionally comprises C4) further additives and / or auxiliaries, preferably selected from the group consisting of adhesion promoters, waxes, lubricants, antioxidants and light stabilizers, preferably in a total amount in the range from 0.1% to 10% by mass, preferably from 0.2% to 5% by mass, based on the total mass of the composite material.

8. Single-use article as claimed in any of the previous claims, wherein the at least one particulate inorganic material and / or the second filler constituent C3) comprise(s) at least one particulate inorganic material, - selected from the group consisting of calcium carbonate, talcum, talc, kaolin, iron mica, wollastonite mica, muscovite mica, phlogopite mica and mixtures thereof, and preferably selected from the group consisting of talc, kaolin, iron mica, wollastonite mica, muscovite mica, phlogopite mica and mixtures thereof and / or - the particles of which have an average aspect ratio of ≥ 5:1, preferably of ≥ 7:1 and more preferably of ≥ 10:1.

9. Single-use article as claimed in any of the previous claims, preferably compostable, wherein the single-use article is a coffee capsule.

10. The use of a composite material or compound as defined in any of the claims 1 to 8 for or in the production of a preferably compostable single-use article, preferably a coffee capsule.

11. A process for producing a composite material or compound as defined in any of the claims 1 to 8, comprising the steps of V1) producing or providing - a polymer mixture or polymer blend comprising polybutylene succinate and polybutylene succinate-co-adipate as defined in any of claims 1 to 5, and / or - polybutylene succinate and / or polybutylene succinate-co-adipate, V2) producing or providing at least one particulate and / or fibrous, cellulose-containing material as first filler constituent as defined in any of claims 1, 5 or 6, V3) producing or providing at least one particulate inorganic material as second filler constituent as defined in any of claims 1 or 8, V4) combining - the polymer mixture or polymer blend from step V1) and / or - the polybutylene succinate and / or polybutylene succinate-co-adipate from step V1), with the at least one particulate and / or fibrous, cellulose-containing material from step V2) and additionally with the at least one particulate inorganic material from step V3), preferably comprising a step of compounding, more preferably comprising a step of melt extrusion, so as to result in the or a composite material or the or a compound.

12. A process for producing a single-use article, comprising the steps of V5) producing or providing a composite material or compound comprising, as polymer constituent, - polybutylene succinate and polybutylene succinate-co-adipate and / or - a polymer mixture or polymer blend as defined in any of claims 1 to 5, and one or more organic and inorganic filler constituents, where the producing or providing of a composite material or compound is executed by - providing a composite material or compound as defined in any of claims 1 to 8 and / or - producing a composite material or compound by a process as claimed in claim 11; and V6) forming the composite material or compound, preferably comprising at least one step selected from the group consisting of - extrusion, preferably comprising film extrusion, blown film extrusion, extrusion blow molding and foam extrusion; - injection molding, - deep drawing and / or - thermoforming.