POLYCARBONATE COMPOSITIONS CONTAINING TITANIUM DIOXIDE AND A TITANIUM DIOXIDE COATING ENSOURCING GLASS PLATES
Patent Information
- Application Number
- DE502021005274
- Authority / Receiving Office
- DE · DE
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-11-30
- Filing Date
- 2021-11-25
- Publication Date
- 2024-10-17
- Estimated Expiration
- 2041-11-25
AI Technical Summary
Conventional titanium dioxide-containing polycarbonate compositions for high reflection applications face challenges such as degradation of the polycarbonate matrix, melt instabilities, and increased costs due to high titanium dioxide requirements, along with undesirable color casts and non-linear reflection curves from optical brighteners.
Incorporating glass platelets with a titanium dioxide coating in low concentrations (0.001% to 0.25% by weight) into polycarbonate compositions, which enhance reflection without significantly affecting flow behavior or introducing color casts, thereby maintaining the brilliance and processability of the materials.
The use of glass platelets with a titanium dioxide coating significantly improves reflection values while maintaining the thermal and mechanical properties of the polycarbonate compositions, reducing the need for excessive titanium dioxide and avoiding color distortions, thus achieving enhanced reflectance without compromising processing stability.
Description
[0001] The invention relates to titanium dioxide-containing, polycarbonate-based compositions with high reflectivity. The invention also relates to improving the reflectivity of titanium dioxide-containing compositions. Furthermore, the present invention relates to molded parts made from these compositions, for example for housings or housing parts or other elements in the renewable energy and information technology sectors, e.g., for panels and switches for automotive interior lighting and, in particular, for reflectors of lighting units such as LED lamps or LED arrays, as well as automotive headlights and rear lights or indicators.
[0002] It is known from the state of the art to add titanium dioxide to plastics such as polycarbonate to improve reflection.
[0003] CN 109867941 A, for example, describes a reflective polycarbonate material which contains titanium dioxide, a liquid silicone and other polymeric components.
[0004] TW 200743656 A discloses flame-retardant, halogen-free, reflective polycarbonate compositions containing, in addition to titanium dioxide, inorganic fillers such as clay or silica as well as other organic components such as optical brighteners, perfluoroalkylene compounds and metal salts of aromatic sulfur compounds.
[0005] US2012220708 relates to a polycarbonate resin composition consisting of (A) an aromatic polycarbonate resin; (B) titanium oxide having an average particle diameter of 0.05 to 6 µm; and (C) (C-1) lustrous particles having an average particle diameter of 10 µm or more and less than 60 µm, and (C-2) lustrous particles having an average particle diameter of 60 to 300 µm, wherein the lustrous particles (C) comprise at least one selected from the group consisting of mica, metal particles, metal sulfide particles, particles having a surface coated with a metal or a metal oxide, and glass flakes having a surface coated with a metal or a metal oxide.
[0006] The reflection values achieved with conventional compositions are increasingly failing to meet market expectations. There is a demand for components, such as reflectors, with increasingly higher reflection values in order to maximize the energy used.
[0007] However, achieving high reflectance levels requires large amounts of titanium dioxide. This is a disadvantage because titanium dioxide can lead to degradation of the polycarbonate matrix, which can cause melt instabilities and a decrease in the viscosity of the compound, which also impairs its thermal and mechanical properties.
[0008] The amount of titanium dioxide also has a very significant impact on the price of polycarbonate compositions, so it is desirable to increase the reflectance by means other than adding even larger amounts of titanium dioxide.
[0009] Optical brighteners, which could be added, have the disadvantage that they lead to a non-linear reflection curve when used, which can result in a blue color cast of the material, which is perceived as disturbing.
[0010] The object of the present invention was therefore to provide titanium dioxide-containing, polycarbonate-based compositions with improved reflection and corresponding molded parts made from these compositions, wherein the compositions, with improved reflection, should preferably not have significantly poorer flow behavior during processing and / or should also be without any disturbing color cast.
[0011] Surprisingly, it was found that titanium dioxide-containing polycarbonate-based compositions exhibit increased reflectance values when glass flakes comprising a titanium dioxide coating are present in very low concentrations. Amounts as low as 0.5 wt.% lead to a noticeable deterioration in reflection. Furthermore, depending on the glass flakes used, distinct glittering, shiny effects or metallic-looking surfaces can be observed. Such glass flakes are typically used in amounts of several weight percent to act as effect pigments in transparent or opaque plastics. Other common applications for glass flakes are found in the cosmetics industry, for example, in lipsticks, eyeliners, or face powders. They are also used as an effect pigment in printing inks for bottle or can coating.
[0012] When used in polycarbonate compositions containing titanium dioxide as a white pigment, it is important that the glass flakes have a low intrinsic color and are compatible with the polycarbonate matrix. Excessively high intrinsic color leads to an increase in the yellowness index and thus to a reduction in reflection. Incompatibility with the polycarbonate matrix leads to polymer degradation during compounding as well as during thermoplastic processing such as injection molding or extrusion, which is also associated with an undesirable increase in the yellowness index and a change in the rheological properties. Furthermore, the thermal and mechanical properties of the components deteriorate.
[0013] According to the invention, to surprisingly increase reflection, glass flakes comprising a titanium dioxide coating are used in a very low concentration of 0.001 to 0.25 wt. %, preferably 0.004 to 0.2 wt. %, more preferably 0.004 to 0.1 wt. %, particularly preferably 0.006 to 0.010 wt. %. The concentration of the glass flakes comprising a titanium dioxide coating (hereinafter referred to as glass flakes) is so low that their effect pigment character is not visually apparent, and the brilliant white appearance of the injection-molded articles remains unadulterated. The flow behavior of the compositions is not significantly affected, and the good processability in injection molding is maintained.
[0014] Thermoplastic compositions according to the invention are therefore those containing A) 44 wt% to 96.999 wt% aromatic polycarbonate, B) 3.0 wt% to 30.0 wt% titanium dioxide and C) glass flakes comprising a titanium dioxide coating, characterized in that the amount of component C is 0.001 wt.% to 0.25 wt.%, the amounts being based on the total weight of the thermoplastic composition.
[0015] The weight percentages below also refer to the total weight of the respective thermoplastic composition, unless otherwise stated.
[0016] Thermoplastic compositions preferred according to the invention contain A) 44.8 wt% to 95.996 wt% aromatic polycarbonate, B) 4.0 wt% to 25 wt% titanium dioxide and C) 0.004 wt% to 0.2 wt% glass flakes comprising a titanium dioxide coating, where the quantities given refer to the total weight of the thermoplastic composition.
[0017] In principle, the compositions according to the invention can also contain one or more blend partners. Examples of thermoplastic polymers suitable as blend partners include polystyrene, styrene copolymers, aromatic polyesters such as polyethylene terephthalate (PET), PET-cyclohexanedimethanol copolymer (PETG), polyethylene naphthalate (PEN), polybutylene terephthalate (PBT), cyclic polyolefins, poly- or copolyacrylates, poly- or copolymethacrylates such as poly- or copolymethyl methacrylates (such as PMMA), as well as copolymers with styrene such as transparent polystyreneacrylonitrile (PSAN), thermoplastic polyurethanes, and / or polymers based on cyclic olefins (e.g., TOPAS®, a commercial product from Ticona).
[0018] Further preferred thermoplastic compositions consist of A) 44.8 wt.% to 95.996 wt.% aromatic polycarbonate, B) 4.0 wt.% to 25 wt.% titanium dioxide and C) 0.004 wt.% to 0.2 wt.% glass flakes comprising a titanium dioxide coating, D) 0 to 30 wt.% of one or more further additives other than components B and C, E) optionally one or more blend partners, where the quantities given refer to the total weight of the thermoplastic composition.
[0019] Even more preferred thermoplastic compositions consist of A) 44.8 wt.% to 95.996 wt.% aromatic polycarbonate, B) 4.0 wt.% to 25 wt.% titanium dioxide and C) 0.004 wt.% to 0.2 wt.% glass flakes comprising a titanium dioxide coating, D) 0 to 30 wt.% of one or more further additives other than components B and C, where the quantities given refer to the total weight of the thermoplastic composition.
[0020] Thermoplastic compositions particularly preferred according to the invention consist of A) 64.8 wt% to 95.996 wt% aromatic polycarbonate, B) 4.0 wt% to 25 wt% titanium dioxide and C) 0.004 wt% to 0.2 wt% glass flakes comprising a titanium dioxide coating, D) 0 to 10 wt% of one or more other additives different from components B and C, where the quantities given refer to the total weight of the thermoplastic composition.
[0021] Particularly preferred thermoplastic compositions consist of A) 76.99 wt.% to 94.994 wt.%, in particular 76.99 wt.% to 94.993 wt.%, aromatic polycarbonate, B) 5 wt.% to 20 wt.% titanium dioxide and C) 0.006 wt.% to 0.010 wt.% glass flakes comprising a titanium dioxide coating, D) 0 to 3 wt.%, in particular 0.01 to 3 wt.%, of one or more other additives different from components B and C, where the quantities given refer to the total weight of the thermoplastic composition.
[0022] In the context of the present invention, the stated % by weight of components A, B, C and optionally D - unless explicitly stated otherwise - are each based on the total weight of the composition. It is understood that all components contained in a composition according to the invention, i.e. the amounts of components A, B, C, optionally D, and optionally further components, together make up 100 % by weight. In addition to components A, B, C and optionally D, the composition can in principle contain further components, provided that the aforementioned core properties of the compositions according to the invention are retained. For example, the compositions can contain one or more further thermoplastics as blend partners (component E), which are not covered by any of components A to D. However, the compositions described above very particularly preferably contain no further components, but rather the amounts of components A, B, C and optionallyD, particularly in the described preferred embodiments, add up to 100 wt. %, i.e., the compositions consist of components A, B, C, and optionally D. It is further understood that the titanium dioxide according to component B is considered separately from the titanium dioxide coating of the glass flakes. The titanium dioxide of the coating of the glass flakes is not included in the quantitative range of component B.
[0023] It is also understood that the components used may contain common impurities, for example, resulting from their manufacturing processes. It is preferable to use components that are as pure as possible. It is further understood that these impurities may also be present in a closed formulation of the composition. The impurities are part of the total weight of the respective component.
[0024] The invention also relates to the improvement of the reflectance, preferably determined according to ASTM E 1331-2015 at a layer thickness of 2 mm, of titanium dioxide-containing polycarbonate compositions by the addition of glass flakes comprising a titanium dioxide coating. The improvement in reflectance refers to the corresponding compositions without glass flakes comprising a titanium dioxide coating. "Improvement in reflectance" is understood to mean any increase in the reflectance value. The improvement in reflectance preferably occurs while maintaining the flowability and gloss of the reference composition. Particularly preferably, the material does not have a glittering or metallic-looking surface.
[0025] The reflection of the compositions in which the reflection is further improved by the addition of component C is preferably at least 95%, more preferably at least 95.5%, determined according to ASTM E 1331-2015 at a layer thickness of 2 mm before the addition of component C
[0026] The features mentioned as preferred etc. for the composition according to the invention naturally also apply to the use according to the invention. Therefore, 0.006 to 0.10 wt.% of the glass platelets are preferably used to improve reflection.
[0027] The individual components of the compositions according to the invention are explained in more detail below: Component A
[0028] "Aromatic polycarbonate" or simply "polycarbonate" in the context of the invention refers to both aromatic homopolycarbonates and aromatic copolycarbonates. The polycarbonates can be linear or branched in a known manner. Mixtures of polycarbonates can also be used according to the invention.
[0029] Compositions according to the invention contain, as component A, at least 44% by weight, preferably at least 44.8% by weight, more preferably at least 64.8% by weight, even more preferably at least 76.99% by weight, of aromatic polycarbonate. A proportion of at least 44% by weight, preferably at least 64.8% by weight, of aromatic polycarbonate in the total composition means, according to the invention, that the composition is based on aromatic polycarbonate. A single polycarbonate or a mixture of several polycarbonates may be present.
[0030] The polycarbonates contained in the compositions are prepared in a known manner from dihydroxyaryl compounds, carbonic acid derivatives, optionally chain terminators and branching agents.
[0031] Details of the production of polycarbonates have been documented in numerous patents published over the past 40 years. Examples include Schnell, "Chemistry and Physics of Polycarbonates," Polymer Reviews, Volume 9, Interscience Publishers, New York, London, Sydney 1964; D. Freitag, U. Grigo, PR Müller, H. Nouvertné, BAYER AG, "Polycarbonates" in Encyclopedia of Polymer Science and Engineering, Volume 11, Second Edition, 1988, pages 648-718; and finally, U. Grigo, K. Kirchner, and PR Müller, "Polycarbonates" in Becker / Braun, Kunststoff-Handbuch, Volume 3 / 1, Polycarbonates, Polyacetals, Polyesters, Cellulose Esters, Carl Hanser Verlag Munich, Vienna 1992, pages 117 to 299.
[0032] Aromatic polycarbonates are produced, for example, by reacting dihydroxyaryl compounds with carbonic acid halides, preferably phosgene, and / or with aromatic dicarboxylic acid dihalides, preferably benzenedicarboxylic acid dihalides, by the interfacial process, optionally using chain terminators and optionally using trifunctional or more than trifunctional branching agents. Production via a melt polymerization process is also possible by reacting dihydroxyaryl compounds with, for example, diphenyl carbonate.
[0033] Dihydroxyaryl compounds suitable for the production of polycarbonates are, for example, hydroquinone, resorcinol, dihydroxydiphenyls, bis-(hydroxyphenyl)-alkanes, bis-(hydroxyphenyl)-cycloalkanes, bis-(hydroxyphenyl)-sulfides, bis-(hydroxyphenyl)-ethers, bis-(hydroxyphenyl)-ketones, bis-(hydroxyphenyl)-sulfones, bis-(hydroxyphenyl)-sulfoxides, α-α'-bis-(hydroxyphenyl)-diisopropylbenzenes, phthalimidines derived from isatin or phenolphthalein derivatives, as well as their nuclear alkylated, nuclear arylated and nuclear halogenated compounds.
[0034] Preferred dihydroxyaryl compounds are 4,4'-dihydroxydiphenyl, 2,2-bis-(4-hydroxyphenyl)-propane (bisphenol A), 2,4-bis-(4-hydroxyphenyl)-2-methylbutane, 1,1-bis-(4-hydroxyphenyl)-p-diisopropylbenzene, 2,2-bis-(3-methyl-4-hydroxyphenyl)-propane, dimethyl bisphenol A, bis-(3,5-dimethyl-4-hydroxyphenyl)-methane, 2,2-bis-(3,5-dimethyl-4-hydroxyphenyl)-propane, bis-(3,5-dimethyl-4-hydroxyphenyl)-sulfone, 2,4-bis-(3,5-dimethyl-4-hydroxyphenyl)-2-methylbutane, 1,1-Bis-(3,5-dimethyl-4-hydroxyphenyl)-p-diisopropylbenzene and 1,1-bis-(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane, as well as the bisphenols (I) to (III) in which R' is each C 1 to C 4 alkyl, aralkyl or aryl, preferably methyl or phenyl, most preferably methyl.
[0035] Particularly preferred bisphenols are 2,2-bis-(4-hydroxyphenyl)-propane (bisphenol A), 2,2-bis-(3,5-dimethyl-4-hydroxyphenyl)-propane, 1,1-bis-(4-hydroxyphenyl)-cyclohexane, 1,1-bis-(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane, 4,4'-dihydroxydiphenyl and dimethyl-bisphenol A as well as the bisphenols of the formulas (I), (II) and (III).
[0036] These and other suitable dihydroxyaryl compounds are described, for example, in US 3 028 635 A, US 2 999 825 A, US 3 148 172 A, US 2 991 273 A, US 3 271 367 A, US 4 982 014 A and US 2 999 846 A, in DE 1 570 703 A, DE 2 063 050 A, DE 2 036 052 A, DE 2 211 956 A and DE 3 832 396 A, in FR 1 561 518 A, in the monograph "H. Schnell, Chemistry and Physics of Polycarbonates, Interscience Publishers, New York 1964" and in JP 62039 / 1986 A, JP 62040 / 1986 A and JP 105550 / 1986 A.
[0037] In the case of homopolycarbonates, only one dihydroxyaryl compound is used; in the case of copolycarbonates, several dihydroxyaryl compounds are used.
[0038] Suitable carbonic acid derivatives include phosgene or diphenyl carbonate.
[0039] Suitable chain terminators that can be used in the production of polycarbonates are monophenols. Examples of suitable monophenols include phenol itself, alkylphenols such as cresols, p-tert-butylphenol, cumylphenol, and mixtures thereof.
[0040] Preferred chain terminators are phenols that are mono- or polysubstituted by C1 to C30 alkyl radicals, linear or branched, preferably unsubstituted, or by tert-butyl. Particularly preferred chain terminators are phenol, cumylphenol, and / or p-tert-butylphenol.
[0041] The amount of chain terminator to be used is preferably 0.1 to 5 mol%, based on the moles of dihydroxyaryl compounds used. The chain terminators can be added before, during, or after the reaction with a carbonic acid derivative.
[0042] Suitable branching agents are the tri- or more than trifunctional compounds known in polycarbonate chemistry, in particular those with three or more than three phenolic OH groups.
[0043] Suitable branching agents are, for example, 1,3,5-tri-(4-hydroxyphenyl)benzene, 1,1,1-tri-(4-hydroxyphenyl)ethane, tri-(4-hydroxyphenyl)phenylmethane, 2,4-bis-(4-hydroxyphenylisopropyl)phenol, 2,6-bis-(2-hydroxy-5'-methylbenzyl)-4-methylphenol, 2-(4-hydroxyphenyl)-2-(2,4-dihydroxyphenyl)propane, tetra-(4-hydroxyphenyl)methane, tetra-(4-(4-hydroxyphenylisopropyl)phenoxy)methane and 1,4-bis-((4',4"-dihydroxytriphenyl)methyl)benzene and 3,3-bis-(3-methyl-4-hydroxyphenyl)-2-oxo-2,3-dihydroindole.
[0044] The amount of branching agents to be used optionally is preferably 0.05 mol% to 2.00 mol%, based on moles of dihydroxyaryl compounds used.
[0045] The branching agents can either be added together with the dihydroxyaryl compounds and the chain terminators in the aqueous alkaline phase or dissolved in an organic solvent before phosgenation. In the case of the transesterification process, the branching agents are used together with the dihydroxyaryl compounds.
[0046] Particularly preferred polycarbonates are the homopolycarbonate based on bisphenol A, the copolycarbonates based on 1,1-bis-(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane and 4,4'-dihydroxydiphenyl as well as the copolycarbonates based on the two monomers bisphenol A and 1,1-bis-(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane, as well as the dihydroxyaryl compounds of the formulas (I), (II) and (III) in which R' is each C 1 - to C 4 -alkyl, aralkyl or aryl, preferably methyl or phenyl, most preferably methyl, derived homo- or copolycarbonates, in particular with bisphenol A.
[0047] Also preferred are copolycarbonates for the preparation of which diphenols of the general formula (1a) were used: where R 5< represents hydrogen or C 1 to C 4 alkyl, C 1 to C 3 alkoxy, preferably hydrogen; Methoxy or methyl, R 6< , R 7< , R 8< and R 9< each independently of one another represent C 1 - to C 4 -alkyl or C 6 - to C 12 -aryl, preferably methyl or phenyl, Y represents a single bond, SO 2 -, -S-, -CO-, -O-, C 1 - to C 6 -alkylene, C 2 - to C 8 -alkylidene, C 6 - to C 12 -arylene, which may optionally be condensed with further aromatic rings containing heteroatoms or represents a C 5 - to C 6 -cycloalkylidene radical which may be mono- or polysubstituted by C 1 - to C 4 -alkyl, preferably a single bond, -O-, isopropylidene or represents a C 5 - to C 6 -cycloalkylidene radical which may be mono- or polysubstituted by C 1 - to C 4 -alkyl, V represents oxygen, C 2 - to C 6 -alkylene or C 3 - to C 6 -alkylidene, preferably oxygen or C 3 -alkylene, p, q and r each independently represent 0 or 1 when q = 0,W stands for a single bond when q = 1 and r = 0, W stands for oxygen, C 2 - to C 6 -alkylene or C 3 - to C 6 -alkylidene, preferably oxygen or C 3 -alkylene when q = 1 and r = 1, W and V each independently stand for C 2 - to C 6 -alkylene or C 3 - to C 6 -alkylidene, preferably C 3 -alkylene, Z stands for a C 1 - to C 6 -alkylene, preferably C 2 -alkylene, o stands for an average number of repeating units of 10 to 500, preferably 10 to 100, and m stands for an average number of repeating units of 1 to 10, preferably 1 to 6, more preferably 1.5 to 5. It is also possible to use diphenols in which two or more siloxane blocks of the general formula (1a) are linked to one another via terephthalic acid and / or isophthalic acid to form ester groups.
[0048] Particularly preferred are (poly)siloxanes of the formulas (2) and (3) where R1 is hydrogen, C1 to C4 alkyl, preferably hydrogen or methyl and particularly preferably hydrogen, R2 independently of one another is aryl or alkyl, preferably methyl, X is a single bond, -SO2-, -CO-, -O-, -S-, C1 to C6 alkylene, C2 to C5 alkylidene or C6 to C12 arylene, which may optionally be condensed with further aromatic rings containing heteroatoms, X is preferably a single bond, C1 to C5 alkylene, C2 to C5 alkylidene, C5 to C12 cycloalkylidene, -O-, -SO- -CO-, -S-, -SO2-, particularly preferably X is a single bond, isopropylidene, C5 to C12 cycloalkylidene or oxygen, and very particularly preferably isopropylidene, n is an average number of 10 to 400, preferably 10 and 100, particularly preferably 15 to 50 and m represents an average number from 1 to 10, preferably from 1 to 6 and particularly preferably from 1.5 to 5.
[0049] Likewise preferably, the siloxane block can be derived from the following structure preferred (Va) or where a in formula (IV), (V) and (VI) represents an average number from 10 to 400, preferably 10 to 100 and particularly preferably 15 to 50.
[0050] It is also preferred that at least two identical or different siloxane blocks of the general formulas (IV), (V) or (VI) are linked to one another via terephthalic acid and / or isophthalic acid to form ester groups.
[0051] It is also preferred if in formula (1a) p = 0, V is C 3 -alkylene, r = 1, Z is C 2 -alkylene, R 8< and R 9< are methyl, q = 1, W is C 3 -alkylene, m = 1, R 5< is hydrogen or C 1 - to C 4 -alkyl, preferably hydrogen or methyl, R 6< and R 7< are each independently of one another C 1 - to C 4 -alkyl, preferably methyl and o is 10 to 500.
[0052] Copolycarbonates with monomer units of formula (IV) and in particular their preparation are described in WO 2015 / 052106 A2.
[0053] The thermoplastic polycarbonates, including the thermoplastic aromatic polyester carbonates, preferably have weight-average molecular weights M w of 15,000 g / mol to 40,000 g / mol, more preferably up to 34,000 g / mol, particularly preferably from 17,000 g / mol to 33,000 g / mol, in particular from 19,000 g / mol to 32,000 g / mol, determined by gel permeation chromatography, calibrated against bisphenol A polycarbonate standards using dichloromethane as the eluent, calibration with linear polycarbonates (from bisphenol A and phosgene) of known molar mass distribution from PSS Polymer Standards Service GmbH, Germany, calibration according to method 2301-0257502-09D (from 2009 in German) from Currenta GmbH & Co. OHG, Leverkusen. The eluent is dichloromethane. Column combination made of cross-linked styrene-divinylbenzene resins. Analytical column diameter: 7.5 mm; length: 300 mm. Column material particle sizes: 3 µm to 20 µm.Solution concentration: 0.2 wt%. Flow rate: 1.0 ml / min. Solution temperature: 30°C. UV and / or RI detection is used.
[0054] For the incorporation of additives, component A is preferably used in the form of powders, granules or mixtures of powders and granules. Component B
[0055] Compositions according to the invention contain 3.0 wt.% to 30.0 wt.%, preferably 4.0 wt.% to 25 wt.%, particularly preferably 5.0 wt.% to 20 wt.%, very particularly preferably 5.0 wt.% to 20.0 wt.%, in particular 5.0 wt.% to 15 wt.%, extremely preferably 10 to 13 wt.%, of titanium dioxide.
[0056] The titanium dioxide according to component B does not include titanium dioxide used as a coating on the glass flakes.
[0057] The titanium dioxide according to component B of the compositions according to the invention preferably has an average particle size D 50 , determined by scanning electron microscopy (STEM), of 0.1 to 5 µm, preferably 0.2 µm to 0.5 µm. However, the titanium dioxide can also have a different particle size, e.g., an average particle size D 50 , determined by scanning electron microscopy (STEM), of ≥ 0.5 µm, approximately 0.65 to 1.15 µm.
[0058] The titanium dioxide preferably has a rutile structure.
[0059] The titanium dioxide used in the invention is a white pigment, Ti(IV)Oz. Colored titanium dioxides contain significant amounts of elements such as Sb, Ni, and Cr in addition to titanium, resulting in a color impression other than "white." It is understood that the white pigment titanium dioxide may also contain traces of other elements as impurities. However, these amounts are so small that they do not impart any color cast to the titanium dioxide.
[0060] Suitable titanium dioxides are preferably those produced by the chloride process, hydrophobized, specially post-treated, and suitable for use in polycarbonate. In principle, uncoated titanium dioxide or a mixture of both can be used instead of coated titanium dioxide in compositions according to the invention. However, the use of coated titanium dioxide is preferred.
[0061] Possible surface modifications of titanium dioxide include inorganic and organic modifications. These include, for example, surface modifications based on aluminum or polysiloxane. An inorganic coating can contain 0.0 wt.% to 5.0 wt.% silicon dioxide and / or aluminum oxide. An organic-based modification can contain 0.0 wt.% to 3.0 wt.% of a hydrophobic wetting agent. The titanium dioxide preferably has an oil absorption number, determined according to DIN EN ISO 787-5:1995-10, of 12 to 18 g / 100 g titanium dioxide, more preferably of 13 to 17 g / 100 g titanium dioxide, and particularly preferably of 13.5 to 15.5 g / 100 g titanium dioxide.
[0062] Particularly preferred is titanium dioxide with the standard designation R2 according to DIN EN ISO 591-1:2001-08, which is stabilized with aluminum and / or silicon compounds and has a titanium dioxide content of at least 96.0 wt.%. Such titanium dioxides are available under the brand names Kronos 2233 and Kronos 2230. Component C
[0063] Component C of the compositions according to the invention is a glass platelet comprising a titanium dioxide coating. "Glass platelet comprising a titanium dioxide coating" means that the titanium dioxide coating is considered part of the glass platelet, i.e., unless explicitly stated otherwise, size specifications refer to the particles according to component C in their entirety, i.e., to the glass cores together with their titanium dioxide coating. The glass platelets used are splinter-shaped, with a thickness significantly less than a length. The glass platelets preferably have the smoothest possible surface.
[0064] The coating could, in principle, be based on various oxides, for example, various iron oxides such as Fe 2 O 3 or Fe 3 O 4 . However, these have an intense inherent color and are therefore unsuitable for highly reflective white compounds. For such applications, only a titanium dioxide coating of the glass flakes is used.
[0065] The glass flakes - based purely on the glass, without titanium dioxide coating - preferably contain 59 wt.% to 65 wt.% SiO2, 8 wt.% to 15 wt.% Al2O3, 20 wt.% to 30 wt.% calcium oxide CaO and 1 wt.% to 5 wt.% magnesium oxide MgO. The glass composition is preferably free of boric acid and other borates as well as free of zinc compounds. More preferably, a total of > 0 to less than 2 wt.% lithium oxide, sodium oxide and potassium oxide is contained, as well as 0 to 5 wt.% titanium dioxide. Even more preferably, essentially no barium oxide, strontium oxide or zirconium oxide is contained. Very particularly preferably, 47 wt.% ≤ SiO2 - Al2O3 ≤ 57 wt.% Suitable glass flakes and their production are described in particular in EP 1829833 A1.
[0066] The surfaces of the glass cores are coated with one or more metal oxides, with titanium dioxide being part of the coating. It is understood that component C in a thermoplastic composition according to the invention can also be a mixture of one or more types of glass flakes comprising a titanium dioxide coating.
[0067] Rutile-type titanium dioxide is particularly preferred. The thickness of the TiO2 coating is preferably thin enough to reflect a neutral white color.
[0068] The particle size distributions of the glass flakes can be determined using scanning electron microscopy (SEM). During the evaluation, the equivalent circular diameter (ECD) is calculated. The equivalence refers to the area of a particle projected onto a substrate. The ECD value is the diameter of a circle with an area equal to the area of the particle. The ECD of the individual glass flakes is preferably between 0.5 µm and 250 µm, more preferably between 1 µm and 200 µm, particularly preferably between 20 µm and 175 µm, and most preferably between 30 µm and 150 µm. The average ECD (D50 value, determined by scanning electron microscopy (STEM)) is preferably between 5 µm and 25 µm. The aspect ratio (length:width) is preferably between 1 and 5, more preferably between 1.5 and 4, particularly preferably between 2 and 3.
[0069] The thickness of the glass platelets comprising a titanium dioxide coating, determined by scanning electron microscopy, is preferably in the range from 0.3 µm to 12 µm, more preferably from 0.4 µm to 10 µm, even more preferably from 0.5 µm to 6 µm, particularly preferably between 1 µm and 3 µm, most preferably between 1.0 and 2.0 µm.
[0070] Scanning electron microscopy in combination with energy-dispersive X-ray spectrometry can be used to determine the thickness of the titanium dioxide coating on the glass platelets. The glass platelets are homogeneously coated with titanium dioxide. "Homogeneous" here means that the coating is approximately the same thickness over the entire surface of the glass, with "approximately" preferably meaning a maximum deviation at any individual point of ± 20%, more preferably ± 10%, even more preferably ± 5% from the average thickness of the surface coating. The thickness of the coating is preferably between 50 nm and 400 nm, preferably between 80 nm and 350 nm, and particularly preferably between 100 nm and 300 nm, most preferably between 120 nm and 200 nm.
[0071] The proportion of the glass platelets comprising a titanium dioxide coating in the total polycarbonate-based composition is 0.001 wt.% to 0.25 wt.%, preferably 0.001 wt.% to 0.15 wt.%, more preferably 0.004 wt.% to 0.1 wt.%, even more preferably 0.004 wt.% to 0.10 wt.%, particularly preferably 0.005 wt.% to 0.02 wt.%, most preferably 0.006 wt.% to 0.010 wt.%. Component D
[0072] In addition, optional further additives are present, preferably up to 30 wt.%, more preferably up to 10.0 wt.%, even more preferably 0.01 wt.% to 6.0 wt.%, particularly preferably 0.1 wt.% to 3.0 wt.%, very particularly preferably 0.2 wt.% to 1.0 wt.%, in particular up to 0.5 wt.% of other customary additives ("further additives"). The group of further additives does not include titanium dioxide, as this is already described as component B. Likewise, the group of further additives does not include glass flakes comprising a titanium dioxide coating according to component C.
[0073] Such further additives, as are usually added to polycarbonates, are in particular thermal stabilizers, flame retardants, antioxidants, mold release agents, anti-drip agents, such as polytetrafluoroethylene (Teflon) or SAN-encapsulated PTFE (e.g. Blendex 449), UV absorbers, IR absorbers, impact modifiers, antistatic agents, optical brighteners, fillers other than components B and C, e.g. talc, quartz, light scattering agents, hydrolysis stabilizers, compatibilizers, inorganic pigments other than component B and / or additives for laser marking, in particular in the amounts customary for polycarbonate-based compositions. Such additives are described, for example, in EP-A 0 839 623, WO-A 96 / 15102, EP-A 0 500 496, or in the "Plastics Additives Handbook," Hans Zweifel, 5th Edition 2000, Hanser Verlag, Munich. These additives can be added individually or in mixtures.It goes without saying that only additives, and only in such quantities, may be added if they do not have a significant negative impact on the inventive effect of improved reflection. Carbon black, for example, is preferably not included. Furthermore, an improvement in reflection must be observed compared to corresponding reference compositions that differ from the inventive composition only in that they do not contain glass flakes according to component C.
[0074] The additives are preferably selected from the group of thermal stabilizers, flame retardants, antioxidants, mold release agents, anti-drip agents, UV absorbers, IR absorbers, impact modifiers, antistatic agents, optical brighteners, fillers other than components B and C, light scattering agents, hydrolysis stabilizers, transesterification inhibitors, compatibilizers, and / or laser marking additives. If additives are present, one or more of these additives can represent component D in a composition according to the invention.
[0075] The further additives are particularly preferably those from the group consisting of flame retardants, anti-drip agents, UV absorbers, thermal stabilizers, antioxidants, antistatic agents, mold release agents, impact modifiers, transesterification inhibitors.
[0076] The compositions further preferably contain at least one flame retardant selected from the group of alkali, alkaline earth, ammonium salts of aliphatic or aromatic sulfonic acid, sulfonamide and sulfonimide derivatives, or combinations thereof.
[0077] For the purposes of the invention, "derivatives" are understood here and elsewhere to mean compounds whose molecular structure contains a different atom or group of atoms instead of a hydrogen atom or functional group, or in which one or more atoms / groups of atoms have been removed. The parent compound is thus still recognizable.
[0078] Compositions according to the invention particularly preferably comprise, as flame retardants, one or more compounds selected from the group consisting of sodium or potassium perfluorobutane sulfate, sodium or potassium perfluoromethanesulfonate, sodium or potassium perfluorooctane sulfate, sodium or potassium 2,5-dichlorobenzenesulfate, sodium or potassium 2,4,5-trichlorobenzenesulfate, sodium or potassium diphenylsulfonesulfonate, sodium or potassium 2-formylbenzenesulfonate, sodium or potassium (N-benzenesulfonyl)benzenesulfonamide or mixtures thereof.
[0079] Sodium or potassium perfluorobutane sulfate, sodium or potassium perfluorooctane sulfate, sodium or potassium diphenylsulfonesulfonate, or mixtures thereof are preferably used. Potassium perfluoro-1-butanesulfonate, which is commercially available, including as Bayowet®< C4 from Lanxess, Leverkusen, Germany, is particularly preferred.
[0080] The amounts of alkali, alkaline earth and / or ammonium salts of aliphatic or aromatic sulfonic acid, sulfonamide and sulfonimide derivatives in the composition, if used, are preferably in total 0.05 wt.% to 0.5 wt.%, more preferably 0.06 wt.% to 0.3 wt.%, particularly preferably 0.06 wt.% to 0.2 wt.%, most preferably 0.065 wt.% to 0.12 wt.%.
[0081] Additional or alternatively included, preferred additives are thermal stabilizers.
[0082] Phosphorus-based stabilizers selected from the group of phosphates, phosphites, phosphonites, phosphines, and mixtures thereof are particularly suitable as thermal stabilizers. Mixtures of different compounds from one of these subgroups, e.g., two phosphites, can also be used.
[0083] Phosphorus compounds with the oxidation number +III, in particular phosphines and / or phosphites, are preferably used as thermal stabilizers.
[0084] Particularly preferred thermal stabilizers are triphenylphosphine, tris-(2,4-di-tert-butylphenyl)phosphite (Irgafos ®< 168), tetrakis-(2,4-di-tert-butylphenyl)-[1,1-biphenyl]-4,4'-diylbisphosphonite, octadecyl 3-(3,5-di-tert-butyl-4-hydroxyphenyl)-propionate (Irganox ®< 1076), bis-(2,4-dicumylphenyl)-pentaerythritol diphosphite (Doverphos ®< S-9228), bis-(2,6-di-tert-butyl-4-methylphenyl)-pentaerythritol diphosphite (ADK STAB PEP-36).
[0085] They are used alone or in a mixture, e.g. Irganox ®< B900 (mixture of Irgafos ®< 168 and Irganox ®< 1076 in a ratio of 4:1) or Doverphos ®< S-9228 with Irganox ®< B900 or Irganox ®< 1076.
[0086] The thermal stabilizers are preferably used in amounts of up to 1.0 wt.%, more preferably 0.003 wt.% to 1.0 wt.%, even more preferably 0.005 wt.% to 0.5 wt.%, particularly preferably 0.01 wt.% to 0.2 wt.%.
[0087] Preferred additives also include special UV stabilizers that have the lowest possible transmission below 400 nm and the highest possible transmission above 400 nm. Particularly suitable ultraviolet absorbers for use in the composition according to the invention are benzotriazoles, triazines, benzophenones, and / or arylated cyanoacrylates.
[0088] Particularly suitable ultraviolet absorbers are hydroxybenzotriazoles, such as 2-(3',5'-bis-(1,1-dimethylbenzyl)-2'-hydroxy-phenyl)-benzotriazole (Tinuvin ®< 234, BASF SE, Ludwigshafen), 2-(2'-hydroxy-5'-(tert.-octyl)-phenyl)-benzotriazole (Tinuvin ®< 329, BASF SE, Ludwigshafen), bis-(3-(2H-benzotriazolyl)-2-hydroxy-5-tert.-octyl)methane (Tinuvin ®< 360, BASF SE, Ludwigshafen), 2-(4,6-diphenyl-1,3,5-triazin-2-yl)-5-(hexyloxy)-phenol (Tinuvin ®< 1577, BASF SE, Ludwigshafen), 2-(5chloro-2H-benzotriazol-2-yl)-6-(1,1-dimethylethyl)-4-methyl-phenol (Tinuvin ®< 326, BASF SE, Ludwigshafen), as well as benzophenones such as 2,4-dihydroxybenzophenone (Chimasorb ®< 22, BASF SE, Ludwigshafen) and 2-hydroxy-4-(octyloxy)-benzophenone (Chimassorb ®< 81, BASF SE, Ludwigshafen), 2,2-Bis[[(2-cyano-1-oxo-3,3-diphenyl-2-propenyl)oxy]-methyl]-1,3-propanediyl ester (9CI) (Uvinul 3030, BASF SE, Ludwigshafen), 2-[2-Hydroxy-4-(2-ethylhexyl)oxy]phenyl-4,6-di(4-phenyl)phenyl-1,3,5-triazine (Tinuvin 1600, BASF SE, Ludwigshafen), tetraethyl-2,2'-(1,4-phenylene-dimethylidene)-bismalonate (Hostavin B-Cap, Clariant AG) or N-(2-ethoxyphenyl)-N'-(2-ethylphenyl)-ethanediamide (Tinuvin 312, CAS No. 23949-66-8, BASF SE, Ludwigshafen).
[0089] Particularly preferred specific UV stabilizers are Tinuvin 360, Tinuvin 329, Tinuvin 326, Tinuvin 1600, Tinuvin 312, Uvinul 3030 and / or Hostavin B-Cap, with Tinuvin 329 and Tinuvin 360 being very particularly preferred.
[0090] Mixtures of the ultraviolet absorbers mentioned can also be used.
[0091] If UV absorbers are included, the composition preferably contains ultraviolet absorbers in an amount of up to 0.8 wt.%, preferably 0.05 wt.% to 0.5 wt.%, more preferably 0.08 wt.% to 0.4 wt.%, most preferably 0.1 wt.% to 0.35 wt.%, based on the total composition.
[0092] The compositions according to the invention may also contain phosphates or sulfonic acid esters as transesterification inhibitors. Triisooctyl phosphate is preferably present as the transesterification inhibitor. Triisooctyl phosphate is preferably used in amounts of 0.003 wt.% to 0.05 wt.%, more preferably 0.005 wt.% to 0.04 wt.%, and particularly preferably 0.01 wt.% to 0.03 wt.%, based on the total composition.
[0093] Examples of impact modifiers suitable as additives include: acrylate core-shell systems such as ABS or MBS or butadiene rubbers (Paraloid grades from DOW Chemical Company); olefin-acrylate copolymers such as Elvaloy® grades from DuPont; and silicone acrylate rubbers such as Metablen® grades from Mitsubishi Rayon Co., Ltd.
[0094] Most preferably, at least one further additive selected from the group consisting of heat stabilizers, mold release agents, antioxidants, impact modifiers, flame retardants, and anti-drip agents is present, in particular in an amount of 0 to 3 wt.%. Mixtures of two or more of the aforementioned additives may also be present.
[0095] The compositions according to the invention are preferably free from optical brighteners.
[0096] Most preferably, at least one additive from the group consisting of heat stabilizers, flame retardants, and impact modifiers is present in the compositions according to the invention. Additional additives from the group of further additives according to component D may also be present, but this is not required.
[0097] As a further additive, at least one anti-drip agent may be included, preferably in an amount of 0.05 wt.% to 1.5 wt.%, in particular 0.1 wt.% to 1.0 wt.%.
[0098] The compositions according to the invention, containing components A to C and optionally D and blending partners, are prepared using conventional incorporation methods by combining, mixing, and homogenizing the individual components, with homogenization preferably taking place in the melt under the action of shear forces. Optionally, the combining and mixing takes place before melt homogenization using powder premixes.
[0099] Premixes of granules or granules and powders with components B, C and, if applicable, D, with the polycarbonate or with the blend partner, if present, can also be used.
[0100] Premixes prepared from solutions of the mixture components in suitable solvents may also be used, optionally by homogenisation in solution and subsequent removal of the solvent.
[0101] In particular, the components of the composition according to the invention can be introduced into the polycarbonate, optionally into the polycarbonate with blend partner, by known methods or as a masterbatch.
[0102] The use of masterbatches is preferred for incorporating components B to D, individually or in a mixture.
[0103] In this context, the composition according to the invention can be combined, mixed, homogenized, and then extruded in conventional devices such as screw extruders (e.g., twin-screw extruders, ZSK), kneaders, Brabender or Banbury mills. After extrusion, the extrudate can be cooled and comminuted. Individual components can also be premixed, and then the remaining starting materials can be added individually and / or in a mixed form.
[0104] The merging and mixing of a premix in the melt can also take place in the plasticizing unit of an injection molding machine. In this case, the melt is transferred directly into a molded body in the subsequent step.
[0105] Thermoplastic compositions preferred according to the invention contain A) 44.9 wt% to 95.996 wt% aromatic polycarbonate, B) 4.0 wt% to 25 wt% titanium dioxide and C) 0.004 wt% to 0.1 wt% of glass flakes comprising a titanium dioxide coating, wherein the glass flakes comprising a titanium dioxide coating have a D50 value, determined by scanning electron microscopy, between 5 µm and 25 µm, an average aspect ratio, determined by scanning electron microscopy, between 1 and 5 and a thickness, determined by scanning electron microscopy, between 1 µm and 3 µm, where the quantities given refer to the total weight of the thermoplastic composition.
[0106] Thermoplastic compositions particularly preferred according to the invention consist of A) 64.9 wt.% to 95.996 wt.% aromatic polycarbonate, B) 4.0 wt.% to 25 wt.% titanium dioxide and C) 0.004 wt.% to 0.1 wt.% glass flakes comprising a titanium dioxide coating, wherein the glass flakes comprising a titanium dioxide coating have a D50 value, determined by means of scanning electron microscopy, between 5 µm and 25 µm, an average aspect ratio, determined by means of scanning electron microscopy, between 2 and 3 and a thickness, determined by means of scanning electron microscopy, between 1.0 µm and 2 µm and wherein the average thickness of the titanium dioxide coating, determined by means of scanning electron microscopy in combination with energy-dispersive X-ray spectrometry, is 100 nm to 300 nm, in particular 120 nm to 200 nm, D) 0 to 10 wt.-% of one or more further additives different from components B and C, selected from the group of heat stabilizers, flame retardants, antioxidants, mold release agents, anti-dripping agents, UV absorbers, IR absorbers, impact modifiers, antistatic agents, optical brighteners, fillers different from components B and C, light scattering agents, inorganic pigments different from component B, hydrolysis stabilizers, transesterification inhibitors, compatibilizers and / or additives for laser marking. where the quantities given refer to the total weight of the thermoplastic composition.
[0107] Very particularly preferred compositions according to the invention consist of A) 76.99 wt.% to 89.994 wt.% aromatic polycarbonate, B) 10 wt.% to 13 wt.% titanium dioxide and C) 0.006 wt.% to 0.01 wt.% glass flakes comprising a titanium dioxide coating, wherein the glass flakes comprising a titanium dioxide coating have a D50 value, determined by means of scanning electron microscopy, between 5 µm and 25 µm, an average aspect ratio, determined by means of scanning electron microscopy, between 2 and 3 and a thickness, determined by means of scanning electron microscopy, between 1.0 µm and 2 µm and wherein the average thickness of the titanium dioxide coating, determined by means of scanning electron microscopy in combination with energy-dispersive X-ray spectrometry, is 100 nm to 300 nm, in particular 120 nm to 200 nm, D) 0 up to 10 wt.-% of one or more further additives different from components B and C, selected from the group of heat stabilizers, flame retardants, antioxidants, mold release agents, anti-dripping agents, UV absorbers, IR absorbers, impact modifiers, antistatic agents, optical brighteners, fillers different from components B and C, light scattering agents, inorganic pigments different from component B, hydrolysis stabilizers, transesterification inhibitors, compatibilizers and / or additives for laser marking. where the quantities given refer to the total weight of the thermoplastic composition.
[0108] The compositions according to the invention preferably have a melt volume flow rate (MVR) of 3 to 40 cm 3 / (10 min), more preferably of 6 to 30 cm 3 / (10 min), even more preferably of 8 to 25 cm 3 / (10 min), particularly preferably of 9 to 24 cm 3 / (10 min), determined according to ISO 1133:2012-3 (test temperature 300°C, mass 1.2 kg). The compositions according to the invention are preferably used for the production of molded parts.
[0109] The molded parts are preferably produced by injection molding, extrusion, or from solution in a casting process. The compositions according to the invention can be processed in the usual way on conventional machines, for example extruders or injection molding machines, into any desired shaped articles, such as films, sheets, or bottles.
[0110] The composites or molded parts made from the composites appear "bright white" to the observer. The coated glass flakes demonstrate good compatibility with the polycarbonate matrix. This is reflected in the consistently high melt stability of the compounds.
[0111] The compositions according to the invention are suitable for producing multilayer systems. Here, the polycarbonate-containing composition is applied in one or more layers to a molded article made of a plastic or serves itself as a substrate layer to which one or more further layers are applied. Application can occur simultaneously with or immediately after the molding of the molded article, for example, by back-injection molding of a film, coextrusion, or multi-component injection molding. However, application can also occur on the finished molded base body, for example, by lamination with a film, overmolding of an existing molded article, or by coating from a solution.
[0112] The compositions according to the invention are suitable for the production of components in the lighting sector, such as reflectors for lamps, in particular LED lamps or LED arrays, in the automotive sector, for example headlight and taillight reflectors, parts for indicators, panels, switches or frames, and for the production of frames or frame parts or housings or housing parts in the EE (electrical / electronic) and IT sectors. Due to the very good reflection values, the compositions according to the invention are preferably used for the production of reflectors. These and other molded parts consisting of the compositions according to the invention or comprising them - e.g. in the case of multi-component injection molding - including molded parts which have a layer of a multi-layer system or layers of multi-layer systems orRepresent an element of an above-mentioned component or are such a component, made of ("consisting of") these compositions according to the invention, are also subject of this application. The compositions according to the invention can also be used in the form of filaments, granules, or powder as material in 3D printing.
[0113] The embodiments described above for the compositions according to the invention also apply - where applicable - to the use according to the invention of component C, i.e. the use for improving reflection.
[0114] The following examples are intended to illustrate the invention. Examples 1. Description of raw materials and test methods
[0115] The polycarbonate compositions described in the following examples were produced by compounding on a Berstorff ZE 25 extruder with a throughput of 10 kg / h. The melt temperature was 275 °C.
[0116] Component A1: Linear polycarbonate based on bisphenol A with a melt volume-flow rate (MVR) of 19 cm³ / (10 min) (according to ISO 1133:2012-03, at a test temperature of 300°C and a load of 1.2 kg). The product contains 250 ppm triphenylphosphine as component D1. Component A2: Linear polycarbonate based on bisphenol A in powder form with a melt volume flow rate MVR of 19 cm 3 < / (10 min) (according to ISO 1133:2012-03, at a test temperature of 300°C and a load of 1.2 kg).
[0117] Component B: Titanium dioxide Kronos 2230 from Kronos Titan GmbH, Leverkusen.
[0118] Component C1:Titanium dioxide (rutile-type) coated glass flakes Metashine Microglass GT 1020RS from Nippon Sheet Glass Co., Ltd. D50 value: 6.2 µm. Average aspect ratio: 2.31. The thickness of the glass flakes (without coating) is approximately 1.3 µm, and the thickness of the titanium dioxide layer is 149 nm. The total thickness of the titanium dioxide-coated glass flakes is approximately 1.6 µm.
[0119] Component C2: Titanium dioxide (rutile-type) coated glass flakes Metashine Microglass GT 1080RS from Nippon Sheet Glass Co., Ltd. D50 value: 23.2 µm. Average aspect ratio: 2.89. The thickness of the glass flakes (without coating) is approximately 1.6 µm, and the thickness of the titanium dioxide layer is 164 nm. The total thickness of the titanium dioxide-coated glass flakes is approximately 1.9 µm.
[0120] Component D1: Triphenylphosphine, commercially available from BASF SE, Ludwigshafen.
[0121] The determination of the Melt volume flow rate (MVR)The test was carried out according to ISO 1133:2012-03 (at a test temperature of 300 °C, mass 1.2 kg) using a Zwick 4106 tester from Zwick Roell. Additionally, the MVR was measured after 20 minutes of preheating (IMVR20'). This is a measure of melt stability under increased thermal stress.
[0122] The determination of the Ash content was carried out according to DIN 51903:2012-11 (850°C, hold for 30 min).
[0123] The total reflection spectrum was measured using a spectrophotometer based on ASTM E 1331-04. The total transmission spectrum was measured using a spectrophotometer based on ASTM E 1348-15.
[0124] From the transmission or reflection spectrum thus obtained, the visual transmission Ty (according to illuminant D65, observer 10°) or the visual reflection Ry (according to illuminant D65, observer 10°) calculated according to ASTM E 308-08. This also applies to the Color values L*a*b*.
[0125] The Shinewas determined according to ASTM D 523-14 (2018).
[0126] The Yellowness Index (YI) was determined according to ASTM E 313-10 (observer: 10° / illuminant: D65).
[0127] Inventive experiments are designated "E" in the following table, comparative experiments are designated "V". Table 1: Example V-1 E-2 E-3 E-4 V-5 V-6 component component % by weight % by weight % by weight % by weight % by weight % by weight A1 80,000 80,000 80,000 80,000 80,000 80,000 A2 8,000 7,994 7,992 7,990 7,500 7,000 B 12,000 12,000 12,000 12,000 12,000 12,000 C1 0,006 0,008 0,010 0,500 1,000 Test Condition Standard / Unit Ash content (average) 850°C / 0.5h % 11,92 11,99 12,02 11,92 12,41 12,73 MVR 300 °C; 1.20 kg; 7 min cm3< / [10min] 24,2 24,0 24,8 25,0 25,3 23,9 MVR 300 °C; 1.20 kg; 20 min cm3< / [10min] 27,6 26,4 26,3 27,2 25,9 28,1 Delta MVR / IMVR20' 3,4 2,4 1,5 2,2 0,6 4,2 Test Condition transmission PELambda950, photometer sphere 0° / diffuse; D65; 10° Sample thickness (ro) mm 1 1 1 1 1 1 L* (ro) ASTM E308 3,16 3,57 3,8 4,04 2,89 2,28 a* (ro) ASTM E 308 4,72 4,59 4,54 4,37 4,72 5,17 b* (ro) ASTM E308 16,24 16,2 16,25 16,27 16,11 15,9 Transmission (ro) [%] ASTM D 1003 / ISO 13468 0,45 0,48 0,5 0,52 0,43 0,39 reflection Hunter Ultra-ScanPRO, diffuse / 8°; D65; 10° ASTM E 1331 with gloss Sample thickness (ro) mm 2 2 2 2 2 2 L* (ro) 98,37 98,42 98,45 98,45 98,34 98,26 a* (ro) -0,62 -0,62 -0,62 -0,62 -0,61 -0,61 b* (ro) 2,12 2,14 2,14 2,13 2,13 2,16 Reflection (ro) % 95,83 95,96 96,04 96,04 95,77 95,58 Yellowness Index (ro) 3,46 3,47 3,49 3,46 3,48 3,54 Gloss 60° (red) 102 102 101 101 96 92
[0128] The addition of small amounts of C1 glass flakes leads to a significant improvement in reflection (E-2 to E-4 compared to V-1). Flowability and gloss remain at the same level. Transmission is slightly improved.
[0129] An amount of 0.5 wt.% of component C1 has an opposite effect (V-5 and V-6): the reflection is significantly deteriorated. Table 2: Example V-7 E-8 E-9 E-10 V-11 V-12 component % by weight Weight % Weight % Weight % Weight % Weight % A1 80,000 80,000 80,000 80,000 80,000 80,000 A2 8,000 7,994 7,992 7,990 7,500 7,000 B 12,000 12,000 12,000 12,000 12,000 12,000 C2 0,006 0,008 0,010 0,500 1,000 Test Condition Standard / Unit Ash content (average) 850°C / 0.5h % 11,96 12,04 11,72 11,76 12,38 12,74 MVR 300 °C; 1.20 kg; 7 min cm3< / [10min] 24,7 23,1 23,7 24,8 24,7 26,3 MVR cm3< / [10min] 26,5 27 26,5 26,3 27,4 33,9 Delta MVR / IMVR20' 300 °C; 1.20 kg; 20 mm 1,8 3,9 2,8 1,5 2,7 7,6 Test Condition transmission PELambda950, photometer sphere 0° / diffuse; D65; 10° Sample thickness (ro) mm 1 1 1 1 1 1 L* (ro) ASTM E 308 2,74 3,13 3,1 3,56 2,26 1,71 a* (ro) ASTM E 308 4,86 4,7 4,68 4,66 5,12 5,37 b* (ro) ASTM E 308 15,99 16,31 16,18 16,7 16,19 15,82 Transmission (ro) [%] ASTM D 1003 / ISO 13468 0,42 0,45 0,45 0,48 0,39 0,36 reflection Hunter Ultra-ScanPRO, diffuse / 8°; D65; 10° ASTM E 1331 with gloss Sample thickness (ro) mm 2 2 2 2 2 2 L* (ro) 98,31 98,37 98,39 98,4 98,26 98,14 a* (ro) -0,6 -0,61 -0,61 -0,61 -0,59 -0,57 b* (ro) 2,07 2,12 2,12 2,14 2,13 2,17 Reflection (ro) % 95,69 95,85 95,9 95,93 95,56 95,28 Yellowness Index (ro) 3,38 3,46 3,46 3,5 3,49 3,59 Gloss 60° (red) 100 100 100 100 97 93
[0130] The addition of small amounts of glass flakes C2 leads to a significant improvement in reflection (E-8 to E-10 compared to V-7). However, an amount of 10% by weight of glass flakes has the opposite effect (V-11 and V-12): Reflection is significantly reduced. Table 3: Example V-13 E-14 E-5 E-16 E-17 component % by weight % by weight % by weight % by weight % by weight A1 80,000 80,000 80,000 80,000 80,000 A2 5,000 4,994 4,900 4,800 4,750 B 15,000 15,000 15,000 15,000 15,000 C2 0,006 0,100 0,200 0,250 Test Condition Standard / Unit Ash content (average) 850°C / 0.5h % 14,24 14,97 15,15 15,28 15,13 MVR 300 °C; 1.20 kg; 7 min cm 3< / [1 0 min] 19,3 25 24,7 20,7 19,3 MVR 300 °C; 1.20 kg; 20 min cm3< / [10min] 19,9 28 25,4 24,1 19,7 Delta MVR / IMVR20' 0,6 3 0,7 3,4 0,4 Test Condition transmission PELambda950, photometer sphere 0° / diffuse; D65; 10° Sample thickness (ro) mm 1 1 1 1 1 L* (ro) ASTM E 308 -2,46 -1,28 -0,56 -0,22 -0,86 a* (ro) ASTM E 308 4,61 5,12 4,87 4,66 4,65 b* (ro) ASTM E 308 11,44 13,99 13,91 13,58 12,5 Transmission (ro) [%] ASTM D 1003 / ISO 13468 0,16 0,2 0,24 0,25 0,22 reflection Hunter Ultra-ScanPRO, diffuse / 8°; D65; 10° ASTM E 1331 with gloss Sample thickness (ro) mm 2 2 2 2 2 L* (ro) 97,93 98,3 98,35 98,4 98,27 a* (ro) -0,57 -0,62 -0,62 -0,63 -0,58 b* (ro) 1,56 2 1,96 1,9 1,63 Reflexion (ro) % 94,74 95,68 95,80 95,91 95,58 Yellowness-Index (ro) 2,46 3,22 3,15 3,04 2,57 Glanz60° (ro) 102 101 101 100 100
Claims
1. Thermoplastic composition, containing A) 44% by weight to 96.999% by weight of aromatic polycarbonate, B) 3.0% by weight to 30.0% by weight of titanium dioxide and C) glass flakes comprising a titanium dioxide coating, characterized in that the amount of component C is 0.001% by weight to 0.25% by weight, wherein the reported amounts are in each case based on the total weight of the thermoplastic composition.
2. Thermoplastic composition according to Claim 1, containing A) 44.8% by weight to 95.996% by weight of aromatic polycarbonate, B) 4.0% by weight to 25% by weight of titanium dioxide and C) 0.004% by weight to 0.2% by weight of glass flakes comprising a titanium dioxide coating, wherein the reported amounts are in each case based on the total weight of the thermoplastic composition.
3. Thermoplastic composition according to either of the preceding claims, wherein the glass flakes comprising a titanium dioxide coating are shard-shaped.
4. Thermoplastic composition according to any of the preceding claims, wherein the titanium dioxide of the coating of the glass flakes is of the rutile type.
5. Thermoplastic composition according to any of the preceding claims, wherein the aromatic polycarbonate present is exclusively bisphenol A-based polycarbonate.
6. Thermoplastic composition according to any of the preceding claims, consisting of A) 64.8% by weight to 95.996% by weight of aromatic polycarbonate, B) 4.0% by weight to 25% by weight of titanium dioxide and C) 0.004% by weight to 0.2% by weight of glass flakes comprising a titanium dioxide coating, D) 0% to 10% by weight of one or more further additive(s) distinct from components Band C, wherein the reported amounts are in each case based on the total weight of the thermoplastic composition.
7. Thermoplastic composition according to any of the preceding claims, containing 0.006% by weight to 0.010% by weight of component C.
8. Thermoplastic composition according to any of the preceding claims, consisting of A) 76.99% by weight to 94.994% by weight of aromatic polycarbonate, B) 5% by weight to 20% by weight of titanium dioxide and C) 0.006% by weight to 0.010% by weight of glass flakes comprising a titanium dioxide coating, D) 0% to 3% by weight of one or more further additive (s) distinct from components Band C, wherein the reported amounts are in each case based on the total weight of the thermoplastic composition.
9. Thermoplastic composition according to any of the preceding claims, wherein at least one additive from the group of heat stabilizers, flame retardants, impact modifiers and transesterification inhibitors is present in the composition as a further additive.
10. Thermoplastic composition according to any of the preceding claims, wherein the glass flakes have a D50 value determined by scanning electron microscopy between 5 µm and 25 µm, an average aspect ratio determined by scanning electron microscopy between 1 and 5 and a thickness determined by scanning electron microscopy between 1 µm and 3 µm.
11. Thermoplastic composition according to any of the preceding claims, wherein the average thickness of the titanium dioxide coating of the glass flakes determined by scanning electron microscopy in conjunction with energy dispersive X-ray spectrometry is between 50 nm and 400 nm.
12. Moulding made of a thermoplastic composition according to any of the preceding claims.
13. Moulding according to Claim 12, wherein the moulding is a reflector or part of a reflector.
14. Use of 0.001% by weight to 0.25% by weight, based on the total composition after addition of the glass flakes, of glass flakes comprising a titanium dioxide coating for improving the reflectance of titanium dioxide-containing polycarbonate compositions, wherein the reflectance is determined by the method specified in the description.
15. Use according to Claim 14, wherein the amount of glass flakes comprising a titanium dioxide coating is 0.006% to 0.010% by weight.