LOW DIELECTRIC LOSS POLYAMIDE MOLDING COMPOTE

DE502021005397D1Active Publication Date: 2024-10-31EMS CHEM AG
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
DE502021005397
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-06-22
Filing Date
2021-06-21
Publication Date
2024-10-31
Estimated Expiration
2041-06-21

AI Technical Summary

Technical Problem

Current glass fiber-reinforced thermoplastic molding compounds with low relative permittivity and low dielectric loss factor have limitations in mechanical properties and metallizability, particularly when used in injection molding processes, leading to issues with injection shrinkage and warping, and are not easily metallizable after partial irradiation.

Method used

A thermoplastic molding compound comprising a mixture of polyamide, polyphenylene ether, and glass filler with specific boron oxide and alkaline oxide content, combined with an LDS additive, which allows for low relative permittivity and dielectric loss factor, improved mechanical properties, and ease of metallization after partial laser irradiation.

Benefits of technology

The solution achieves a relative permittivity of less than 3.0 and a dielectric loss factor of less than 0.008, along with mechanical properties such as a tensile modulus of elasticity of at least 4000 MPa and breaking stress of at least 70 MPa, and enables successful metallization of molded parts with copper deposition in multiple areas.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader
Need to check novelty before this filing date? Find Prior Art

Description

TECHNICAL FIELD

[0001] The present invention relates to glass fiber-reinforced thermoplastic molding compounds based on polyamides and polyphenylene ethers with low relative permittivity and low dielectric loss factors, as well as molded articles made from these molding compounds and their uses. The molding compounds additionally contain an LDS additive, and molded articles produced therefrom can be selectively metallized after partial irradiation. STATE OF THE ART

[0002] Plastic molding compounds with low relative permittivity and low dielectric loss factor are advantageously used in the manufacture of housings, housing parts or other components of devices that communicate via electromagnetic waves with a frequency of 0.3 to 300 GHz, since their use can avoid significant impairment of the transmission and reception properties of these devices.

[0003] Devices that communicate via such electromagnetic waves are used in a variety of areas, such as telecommunications, entertainment electronics or in the home, in particular transmitting and receiving devices, mobile phones, tablets, laptops, navigation devices, surveillance cameras, cameras, sensors, dive computers, audio systems, remote controls, loudspeakers, headphones, radios, televisions, kitchen appliances, door or gate openers, control devices for central locking systems in vehicles, keyless-go vehicle keys, temperature measuring or temperature display devices, measuring devices and control devices.

[0004] The polyamide molding compounds described in EP3330319A1 are said to have a relative permittivity of no more than 3.5 at a frequency of 2.45 GHz. In addition to a specific mixture of aliphatic and amorphous or microcrystalline polyamides, the molding compounds contain a glass filler consisting of glass with an alkali oxide and alkaline earth oxide content of 0 to 12 wt.%, as well as additives. All worked examples and comparative examples, regardless of composition, exhibit a relative permittivity of greater than 3.2. No information is provided regarding the dielectric loss factor and metallizability.

[0005] EP 3 560 987 A1 describes a glass fiber-reinforced molding compound with high tensile strength and impact resistance combined with a low dielectric constant and low dielectric loss factor. The molding compound contains 10 to 90 wt.% glass fibers and 90 to 10 wt.% of a plastic, with the glass fiber composition being specified in more detail. Compared to E-glass, the described glass fiber contains significantly less alkaline earth oxide but a higher boron oxide content, reducing the dielectric constant to 4.8 and the dielectric loss factor to 0.0015, each determined at 10 GHz. As the disclosed examples show, the improved dielectric properties can also be transferred to polyamide molding compounds. However, for a molding compound made of PA6 and 50 wt.% glass fibers, a relative permittivity of 3.39 and a dielectric loss factor of 0.0109 are determined at best. No information is given on the metallizability of the molding compounds.

[0006] EP2291444 describes laser-directly structurable (LDS) molding compounds with a high dielectric constant of at least 4 and a low dielectric loss factor of at most 0.01. The molding compounds contain a base resin, an LDS additive, and a ceramic filler with a dielectric constant ≥ 25. The examples show molding compounds based on polyamides and polyphenylene ethers, which have a dielectric constant in the range of 4.1 to 6.8. However, the dielectric loss factor of the molding compounds described in the examples is not disclosed.

[0007] US2016 / 355679A1 also describes laser-directly structurable molding compounds. OBJECT OF THE INVENTION

[0008] Based on this, one object of the present invention was to provide thermoplastic molding compounds that, in addition to a low relative permittivity of less than 3.0 and a low dielectric loss factor of less than 0.008, are also readily processable by injection molding and, in particular, exhibit good injection shrinkage and warpage behavior. Furthermore, the thermoplastic molding compounds should have good mechanical properties; preferably, the molding compounds should have a breaking stress of at least 70 MPa and a tensile modulus of elasticity of at least 4000 MPa. Furthermore, the molding compounds should be readily metallizable after partial laser irradiation.

[0009] This object is achieved by the thermoplastic molding compositions according to claim 1, which consist of the following components: (A) A mixture of at least one polyamide (A1), at least one polyphenylene ether (A2) and optionally a compatibilizer (A3) and optionally an olefinic and / or vinyl aromatic polymer (A4); (B) 10 to 60 wt.% glass filler, the glass composition of which comprises at least 10.0 wt.% boron oxide and at most 15 wt.% for the sum of magnesium oxide and calcium oxide; (C) 1 to 8 wt.% LDS additive; (D) 0 to 5 wt.% additives other than components (A), (B) and (C); wherein the mixture (A) consists of 80 to 100 wt. % of a mixture (M) of components (A1), (A2) and (A3) and 0 to 20 wt. % of component (A4), in each case based on the sum of components (M) and (A4), and wherein the sum of components (M) and (A4) amounts to 100 wt. % of the mixture (A); and wherein the mixture (M) consists of 36 to 92 wt. % of component (A2), 8 to 60 wt. % of component (A1) and 0 to 4 wt. % of component (A3), in each case based on the sum of components (A1) to (A3), and wherein the sum of components (A1) to (A3) amounts to 100 wt. % of the mixture (M); and wherein the sum of components (A) to (D) amounts to 100 wt. % of the molding composition.

[0010] Dependent claims 2 to 12 relate to advantageous embodiments of the thermoplastic molding compositions according to the invention. Furthermore, according to claim 13, molded articles made from the thermoplastic molding composition according to the invention are provided, and claims 14 and 15 relate to specific molded articles.

[0011] Regarding the composition of mixture (A), it follows from the above information that components (A1) to (A3) together make up 80 to 100 wt.% of mixture (A), and the content of component (A4) in mixture (A) is 0 to 20 wt.%. The mixture of components (A1), (A2), and (A3) is referred to as component (M). Besides components (A1) to (A4), mixture (A) contains no other components.

[0012] The thermoplastic molding compound according to the invention and molded parts produced therefrom exhibit a relative permittivity of less than 3.0 and a dielectric loss factor (DVF) of less than 0.008. The relative permittivity and DVF are measured according to IEC 61189-2-721 (2015) on 80 x 80 x 3 mm plates using a split-post dielectric resonator (SPDR) from QWED, Poland, at a measurement frequency of 2.45 GHz and a temperature of 23 °C.

[0013] Good mechanical properties are understood to mean that the molding compound according to the invention has a tensile modulus of elasticity of at least 4000 MPa, preferably at least 5000 MPa, and / or a stress at break of at least 70 MPa, preferably at least 75 MPa, and / or an elongation at break of at least 1.5%, preferably at least 1.8%. The tensile modulus of elasticity, the stress at break, and the elongation at break are determined according to ISO 527 (2012).

[0014] For the purposes of the invention, readily metallizable means that injection-molded parts (sheet 60 x 60 x 2 mm) made from the thermoplastic molding compound according to the invention can be sufficiently metallized after partial irradiation with an Nd:YAG laser (FOBA DP50 laser, wavelength = 1064 nm, irradiation width = 50 µm, speed = 4 m / s) in a copper plating bath. For this purpose, 16 adjacent, 10 x 10 mm areas on the molded part surface are irradiated during laser structuring, with both the pulse frequency (5, 6, 7, and 8 kHz) and the current intensity (24 to 25.5 amperes) of the laser being varied. The cleaned molded parts are then metallized in a reductive copper plating bath (MacDermid MID-Copper 100 B1) for 20–30 minutes. Sufficiently metallized here means that copper is deposited in at least 14 areas with an average thickness of at least 3 µm. PRESENTATION OF THE INVENTION

[0015] Surprisingly, it was found that the above-described task is solved by a thermoplastic molding compound consisting of: (A) A mixture of at least one polyamide (A1), at least one polyphenylene ether (A2) and optionally a compatibilizer (A3) and optionally an olefinic and / or vinyl aromatic polymer (A4); (B) 10 to 60 wt.% glass filler, the glass composition of which comprises at least 10.0 wt.% boron oxide and at most 15 wt.% for the sum of magnesium oxide and calcium oxide; (C) 1 to 8 wt.% LDS additive, different from components (A), (B) and (C); (D) 0 to 5 wt.% additives; wherein the mixture (A) consists of 80 to 100 wt. % of a mixture (M) of components (A1), (A2) and (A3) and 0 to 20 wt. % of component (A4), in each case based on the sum of components (M) and (A4), and wherein the sum of components (M) and (A4) amounts to 100 wt. % of the mixture (A); and wherein the mixture (M) consists of 36 to 92 wt. % of component (A2), 8 to 60 wt. % of component (A1) and 0 to 4 wt. % of component (A3), in each case based on the sum of components (A1) to (A3), and wherein the sum of components (A1) to (A3) amounts to 100 wt. % of the mixture (M); and wherein the sum of components (A) to (D) amounts to 100 wt. % of the molding composition.

[0016] The content of the mixture (A) in the molding compound is the difference between the sum of the contents (B) to (D) and 100 wt.% of the total molding compound.

[0017] The mixture (A) is preferably present in the molding composition in a proportion of 34 to 82.9 wt.%, particularly preferably 39 to 78.8 wt.%, based on the total weight of the molding composition (sum of A to D).

[0018] The proportion of component (B) is preferably in the range from 15 to 55% by weight, particularly preferably in the range from 18 to 52% by weight, in each case based on the sum of (A) to (D).

[0019] The proportion of component (C) is preferably in the range from 2 to 6 wt.%, particularly preferably in the range from 3 to 5 wt.%, in each case based on the sum of (A) to (D).

[0020] The proportion of component (D) is preferably in the range from 0.1 to 5 wt.%, particularly preferably in the range from 0.2 to 4 wt.%, in each case based on the sum of (A) to (D).

[0021] As the studies conducted show, glass fiber-reinforced molding compounds whose polymer matrix consists exclusively of polyamides exhibit excessively high relative permittivity and dielectric loss factors, even when so-called "low DK glass fibers" are used as the reinforcing fibers. In contrast, molding compounds with a matrix of polyphenylene ethers exhibit excessive warpage, particularly excessive shrinkage values, and are significantly more difficult to process. A molding compound whose polymer component is formed by a 1:1 mixture of polyamide and polyphenylene ether and which is reinforced with glass fibers consisting of E-glass also exhibits excessively high permittivity and dielectric loss, especially in the presence of an LDS additive with a high relative permittivity. DEFINITIONS OF TERMS

[0022] For the purposes of the present invention, the term "polyamide" (abbreviation PA) is understood as a generic term that encompasses homopolyamides and copolyamides. The chosen notations and abbreviations for polyamides and their monomers correspond to those defined in ISO standard 16396-1 (2015(D)). The abbreviations used therein are used synonymously with the IUPAC names of the monomers in the following, in particular the following abbreviations for monomers occur: T or TPS for terephthalic acid, I or IPS for isophthalic acid, MACM for bis(4-amino-3-methyl-cyclohexyl)methane (also known as 3,3'-dimethyl-4,4'-diaminodicyclohexylmethane, CAS No. 6864-37-5), PACM for bis(4-aminocyclohexyl)methane (also known as 4,4'-diaminodicyclohexylmethane, CAS No. 1761-71-3), TMDC for bis(4-amino-3,5-dimethyl-cyclohexyl)methane (also known as 3,3',5,5'-tetramethyl-4,4'-diaminodicyclohexylmethane, CAS No. 65962-45-0).The abbreviation HMDA is used below for 1,6-hexanediamine (also known as hexamethylenediamine).

[0023] Compared to semi-crystalline polyamides, amorphous polyamides exhibit no or only a very low, barely detectable heat of fusion. In differential scanning calorimetry (DSC) according to ISO 11357 (2013) at a heating rate of 20 K / min, amorphous polyamides preferably exhibit a heat of fusion of less than 5 J / g, more preferably a maximum of 3 J / g, and most preferably between 0 and 1 J / g. Due to their amorphous nature, amorphous polyamides do not have a melting point.

[0024] In addition to a glass transition temperature, microcrystalline polyamides also have a melting point. However, their morphology is such that the crystallites are so small that a 2 mm thick sheet made from them is still transparent, i.e., its light transmission is at least 90% and its haze is at most 3%, measured according to ASTM D 1003-13 (2013). In differential scanning calorimetry (DSC) according to ISO 11357 (2013) at a heating rate of 20 K / min, microcrystalline polyamides preferably exhibit a latent heat of fusion of 5 to 25 J / g, more preferably 5 to 22 J / g, and most preferably 5 to 20 J / g.

[0025] Semi-crystalline polyamides have, in addition to a glass transition temperature, a pronounced melting point and, in differential scanning calorimetry (DSC) according to ISO 11357 (2013) at a heating rate of 20 K / min, preferably show a heat of fusion of more than 25 J / g, particularly preferably more than 30 J / g, most preferably from 30 to 80 J / g. Relative permittivity and dielectric loss factor

[0026] The permittivity (ε) is an indicator of the behavior of molecules when placed in an electric field. It is linked to the relative permittivity (ε r ) and the permittivity of the vacuum (ε 0 ) via the relationship ε = ε r · ε 0 . The relative permittivity (ε r ) is a material-dependent quantity and is the quotient of the permittivity (ε) and the permittivity of the vacuum (ε 0 ). In addition to the type of material, the relative permittivity (ε r ) also depends on the frequency of the electric field and the temperature.

[0027] The dielectric loss factor indicates the size of the losses in electrical components such as capacitors or in the propagation of electromagnetic waves in material, e.g. plastic molding compounds. Loss here refers to the energy that is converted electrically or electromagnetically and dissipated, for example, as heat. These losses dampen the electromagnetic wave. To illustrate the loss factor more precisely, consider a capacitor connected to a voltage source with a sinusoidal voltage curve over time. A phase shift ϕ occurs between voltage and current in such a capacitor. An ideal capacitor with no losses whatsoever has a phase shift of ϕ = 90°. In a real, lossy capacitor, the phase shift by the loss angle δ is less than 90°; the dielectric loss factor (DVF) corresponds to tan δ.The dielectric loss factor is therefore a measure of the amount of energy an insulating material absorbs in an alternating field and converts into heat loss. Materials with a high loss factor are unsuitable as insulating materials or housing materials for high-frequency applications. The relative permittivity and the dielectric loss factor are preferably determined according to IEC 61189-2-721 (2015). Component (A)

[0028] The thermoplastic molding composition according to the invention comprises, as polymer component, a mixture (A) consisting of at least one polyamide (A1), at least one polyphenylene ether (A2) and optionally a compatibilizer (A3) and optionally an olefinic and / or vinylaromatic polymer (A4).

[0029] The mixture (A) consists of 80 to 100 wt.% of a mixture (M) of components (A1) to (A3) and 0 to 20 wt.% of component (A4), in each case based on the sum of components (M) and (A4), the sum of components (M) and (A4) being 100 wt.% of the mixture (A).

[0030] The mixture (M) consists of 36 to 92 wt.% of component (A2), 8 to 60 wt.% of component (A1), 0 to 4 wt.% of component (A3), in each case based on the sum of components (A1) to (A3).

[0031] Component (A1) is preferably present in the mixture (M) in a proportion of 10 to 48 percent by weight, particularly preferably 10 to 45 percent by weight, based on the sum of (A1) to (A3).

[0032] Component (A2) is preferably present in the mixture (M) in a proportion of 48 to 89.9 percent by weight, particularly preferably 52 to 89.8 percent by weight, based on the sum of (A1) to (A3).

[0033] Component (A3) is preferably present in the mixture (M) in a proportion of 0.1 to 4 percent by weight, particularly preferably 0.2 to 3 percent by weight, based on the sum of (A1) to (A3).

[0034] Component (A4) is preferably present in mixture (A) in a proportion of 0 to 20 percent by weight, based on the sum of (M) and (A4). More preferably, mixture (A) is free of component (A4). This means that mixture (A) particularly preferably consists exclusively of components (A1) to (A3). Component (A1)

[0035] One embodiment of the present invention provides that aliphatic polyamides are preferred as component (A1). Particular preference is given to selecting aliphatic polyamides from the group consisting of PA 46, PA 6, PA 66, PA 6 / 66, PA 10, PA 11, PA 12, PA 516, PA 610, PA 612, PA 614, PA 616, PA 618, PA 1010, PA 1012, PA 1014, PA 1016, PA 1018, PA 1212, and mixtures thereof. Particular preference is given to aliphatic polyamides with an N / C ratio (N = nitrogen / C = carbon) of greater than or equal to 8, since these polyamides have lower water absorption and thus their dielectric properties change less in humid environments. Particularly preferred are the aliphatic polyamides PA 610, PA 612, PA 1010, PA12 and PA 616.

[0036] According to a further embodiment of the present invention, amorphous or microcrystalline polyamides are preferred as component (A1).Insbesondere bevorzugt ausgewählt sind amorphe oder mikrocristalline Polyamide aus der Gruppe bestehend aus PA 6I / 6T, PA MACM9, PA MACM10, PA MACM12, PA MACM13, PA MACM14, PA MACM16, PA MACM17, PA MACM18, PA PACM10, PA PACM12, PA PACM13, PA PACM14, PA PACM16, PA PACM17, PA PACM18, PA TMDC10, PA TMDC12, PA TMDC13, PA TMDC14, PA TMDC16, PA TMDC17, PA TMDC18, PA MACM10 / 10, PA MACMI / 12, PA MACMT / 12, PA 6I / MACMI / MACMT, PA MACMI / MACMT / 12, PA MACMI / MACMT / MACM12, PA MACMI / MACMT / MACM12 / 12, PA 6I / 6T / MACMI / MACMT / 12, PA 6I / 6T / MACMI, PA MACMI / MACM36, PA MACMT / MACM36, PA MACMI / MACM12, PA MACMT / MACM12, PA MACM6 / 11 PA MACM10 / 10, PA MACM12 / PACM12, PA MACM14 / PACM14, PA MACM18 / PACM18 and Mischungen daraus, wobei PA 6I / 6T, PA MACM12, PA MACM14, PA TMDC12, PA TMDC14, PA MACMI / 12, PA 6I / 6T / MACMI / MACMT, PA MACMI / MACMT / 12, PA MACMI / MACMT / MACM12, PA 6I / 6T / MACMI / MACMT / 12, PA MACM10 / 10, PA MACM12 / PACM12, PA MACM14 / PACM14, PA MACM18 / PACM18 und Mischungen daraus.PA 6I / 6T, PA MACM12, PA MACMI / 12, PA MACMI / MACMT / 12, PA MACMI / MACMT / MACM12, PA MACM12 / PACM12 and mixtures are very particularly preferred.

[0037] According to a further preferred embodiment, semi-crystalline, semi-aromatic polyamides are preferred as component (A1). The semi-crystalline, semi-aromatic polyamides preferably have a glass transition temperature in the range from 90 to 150°C, preferably in the range from 110 to 140°C, and in particular in the range from 115 to 135°C. The melting point of the semi-crystalline, semi-aromatic polyamides is in the range from 255 to 330°C, preferably in the range from 270 to 325°C, and in particular in the range from 280 to 320°C. The semi-crystalline, semi-aromatic polyamides of component (A1) preferably have enthalpies of fusion, determined by DSC according to ISO 11357 (2013), in the range from 25 to 80 J / g, preferably in the range from 30 to 70 J / g.

[0038] Preferred semi-aromatic, semi-crystalline polyamides are (a): Dicarboxylic acids: 30 to 100 mol%, in particular 50 to 100 mol% of terephthalic acid and 0 to 70 mol%, in particular 0 to 50 mol% of at least one aliphatic dicarboxylic acid having 6 to 16 carbon atoms, and / or 0 to 70 mol%, in particular 0 to 50 mol% of at least one cycloaliphatic dicarboxylic acid having 8 to 20 carbon atoms, and / or 0 to 50 mol% of isophthalic acid, in each case based on the total amount of the dicarboxylic acids, (b): Diamines: 80 to 100 mol% of at least one aliphatic diamine having 4-18 carbon atoms, preferably having 6 to 12 carbon atoms and 0 to 20 mol% of at least one cycloaliphatic diamine, preferably having 6 to 20 carbon atoms, such as PACM, MACM, IPDA and / or 0 to 20 mol% of at least one araliphatic diamine, such as MXDA and PXDA, based on the total amount of diamines, and optionally (c): aminocarboxylic acids and / or lactams: each having 6 to 12 carbon atoms.

[0039] According to a preferred embodiment, the semi-crystalline, semi-aromatic polyamide of component (A1) is formed on the basis of at least 55 mol%, in particular at least 65 mol% of terephthalic acid and at least 80 mol%, preferably at least 90 mol%, in particular at least 95 mol% of aliphatic diamines having 4 to 18 carbon atoms, preferably having 6-12 carbon atoms, and optionally further aliphatic, cycloaliphatic and aromatic dicarboxylic acids and also lactams and / or aminocarboxylic acids.

[0040] According to a further preferred embodiment, the aliphatic dicarboxylic acids mentioned, for example, of the semi-aromatic polyamide of component (A1), which can be used in addition to terephthalic acid, are selected from the group consisting of adipic acid, suberic acid, azelaic acid, sebacic acid, undecanedioic acid, dodecanedioic acid, brassylic acid, tetradecanedioic acid, pentadecanedioic acid, hexadecanedioic acid, octadecanedioic acid, and dimer fatty acid (36 carbon atoms). Particular preference is given to adipic acid, sebacic acid, and dodecanedioic acid. Dicarboxylic acids that are preferably used in addition to terephthalic acid are accordingly isophthalic acid, adipic acid, sebacic acid, and dodecanedioic acid, or a mixture of such dicarboxylic acids. Polyamides (A1) based exclusively on terephthalic acid as the dicarboxylic acid are particularly preferred.

[0041] According to a further preferred embodiment, the said aliphatic diamines of the semi-aromatic polyamide of component (A1) are selected from the group consisting of 1,4-butanediamine, 1,5-pentanediamine, 1,6-hexanediamine, 1,7-heptanediamine, 1,8-octanediamine, 1,9-nonanediamine, methyl-1,8-octanediamine, 1,10-decanediamine, 1,11-undecanediamine, 1,12-dodecanediamine, or a mixture of such diamines, with 1,6-hexanediamine, 1,10-decanediamine, 1,12-dodecanediamine, or a mixture of such diamines being preferred, and with 1,6-hexanediamine and 1,10-decanediamine being particularly preferred. In addition to the aliphatic diamines, cycloaliphatic and / or araliphatic diamines can be replaced in a concentration of 0 to 20 mol%, based on the total amount of diamines.

[0042] Furthermore, the polyamides (A1) are preferably formed from the following components: (a): Dicarboxylic acids: 50 to 100 mol% terephthalic acid, 0 to 50 mol% of an aliphatic dicarboxylic acid, preferably having 6 to 12 carbon atoms, and / or a cycloaliphatic dicarboxylic acid having preferably 8 to 20 carbon atoms, and / or isophthalic acid, in each case based on the total content of dicarboxylic acids present; (b): Diamines: 80 to 100 mol% of at least one aliphatic diamine having 4 to 18 carbon atoms, preferably having 6 to 12 carbon atoms, based on the total content of diamines present, 0 to 20 mol% cycloaliphatic diamines, preferably having 6 to 20 carbon atoms, such as PACM, MACM, IPDA and / or araliphatic diamines, such asMXDA and PXDA, wherein in the high-melting polyamides the percentage molar content of dicarboxylic acids is 100% and the percentage molar content of diamines is 100%, and optionally from: (c): aminocarboxylic acids and / or lactams, containing lactams preferably having 6 to 12 carbon atoms, and / or aminocarboxylic acids preferably having 6 to 12 carbon atoms. .

[0043] While components (a) and (b) are preferably used in substantially equimolar amounts, the concentration of (c) is preferably at most 30% by weight, preferably at most 20% by weight, in particular at most 15% by weight, in each case based on the sum of (a) to (c).

[0044] Suitable cycloaliphatic dicarboxylic acids are cis- and / or trans-cyclohexane-1,4-dicarboxylic acid and / or cis- and / or trans-cyclohexane-1,3-dicarboxylic acid (CHDA). The above-mentioned, generally used aliphatic diamines can be replaced by other diamines in minor amounts of not more than 20 mol%, preferably not more than 15 mol%, and in particular not more than 10 mol%, based on the total amount of diamines. Examples of cycloaliphatic diamines that can be used include cyclohexanediamine, 1,3-bis(aminomethyl)cyclohexane (BAC), isophoronediamine (IPDA), norbornanedimethylamine, 4,4'-diaminodicyclohexylmethane (PACM), 2,2-(4,4'-diaminodicyclohexyl)propane (PACP), and 3,3'-dimethyl-4,4'-diaminodicyclohexylmethane (MACM). Examples of araliphatic diamines include m-xylylenediamine (MXDA) and p-xylylenediamine (PXDA).

[0045] In addition to the dicarboxylic acids and diamines described, lactams and / or aminocarboxylic acids can also be used as polyamide-forming components (component (c)). Suitable compounds include, for example, caprolactam (CL), α,ω-aminocaproic acid, α,ω-aminononanoic acid, α,ω-aminoundecanoic acid (AUA), laurolactam (LL), and α,ω-aminododecanoic acid (ADA). The concentration of the aminocarboxylic acids and / or lactams used together with components (A1a) and (A1b) is at most 20 wt. %, preferably at most 15 wt. %, and particularly preferably at most 12 wt. %, based on the sum of components (A1a) to (A1c). Lactams or α,ω-amino acids having 4, 6, 7, 8, 11, or 12 C atoms are particularly preferred. These are the lactams pyrrolidin-2-one (4 C atoms), ε-caprolactam (6 C atoms), enanthlactam (7 C atoms), capryllactam (8 C atoms), laurolactam (12 C atoms) respectively.the α,ω-amino acids 1,4-aminobutanoic acid, 1,6-aminohexanoic acid, 1,7-aminoheptanoic acid, 1,8-aminooctanoic acid, 1,11-aminoundecanoic acid, and 1,12-aminododecanoic acid. In a particularly preferred embodiment, component (A1) is free of caprolactam or aminocaproic acid or free of any aminocarboxylic acid or any lactam.

[0046] To control the molar mass, the relative viscosity or the flowability or the MVR, regulators in the form of monocarboxylic acids or monoamines can be added to the batch and / or the precondensate (before post-condensation).Aliphatic, cycloaliphatic or aromatic monocarboxylic acids or monoamines suitable as regulators are acetic acid, propionic acid, butyric acid, valeric acid, caproic acid, lauric acid, stearic acid, 2-ethylhexanoic acid, cyclohexanoic acid, benzoic acid, 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propanoic acid, 3,5-di-tert-butyl-4-hydroxybenzoic acid, 3-(3-tert-butyl-4-hydroxy-5-methylphenyl)propanoic acid, 2-(3,5-di-tert-butyl-4-hydroxybenzylthio)acetic acid, 3,3-bis(3-tert-butyl-4-hydroxyphenyl)butanoic acid, butylamine, pentylamine, hexylamine, 2-ethylhexylamine, n-octylamine, n-dodecylamine, n-tetradecylamine, n-Hexadecylamine, stearylamine, cyclohexylamine, 3-(cyclohexylamino)-propylamine, methylcyclohexylamine, dimethylcyclohexylamine, benzylamine, 2-phenylethylamine, 2,2,6,6-tetramethylpiperidin-4-amine, 1,2,2,6,6-pentamethylpiperidin-4-amine, 4-amino-2,6-di-tert-butylphenol, etc. The regulators can be used individually or in combination.Other monofunctional compounds that can react with an amino or acid group, such as anhydrides, isocyanates, acid halides, or esters, can also be used as regulators. The typical amount of regulators used is between 10 and 200 mmol per kg of polymer.

[0047] Specific representatives of the partially crystalline, partially aromatic polyamides (A1) are: PA 4T / 4I, PA 4T / 6I, PA 5T / 5I, PA 6T / 6, PA 6T / 6I, PA 6T / 6I / 6, PA 6T / 66, 6T / 610, 6T / 612, PA 6T / 10T, PA 6T / 10I, PA 9T, PA 10T, PA 12T, PA 10T / 10I, PA10T / 106, PA10T / 610, PA10T / 612, PA10T / 66, PA10T / 6, PA10T / 1010, PA10T / 1012, PA10T / 12, PA10T / 11, PA 6T / 9T, PA 6D / 12D, PA 6T / 10T / 6I, PA 6T / 6I / 6, PA 6T / 6I / 12, and mixtures thereof. The partially aromatic polyamide of component (A1) is particularly preferably selected from the group: PA 6T / 6I, PA 6T / 10T, PA 6T / 10T / 6I, and mixtures thereof. Polyamides (A1) containing 6T units, in particular at least 10 wt.% of 6T units, are preferred.

[0048] According to the invention, the following partially aromatic copolyamides are particularly preferred as polyamides (A1): Semi-crystalline polyamide 6T / 6I with 55 to 75 mol% hexamethylene terephthalamide units and 25 to 45 mol% hexamethylene isophthalamide units; semi-crystalline polyamide 6T / 6I with 62 to 73 mol% hexamethylene terephthalamide units and 25 to 38 mol% hexamethylene isophthalamide units; semi-crystalline polyamide produced from at least 50 mol% terephthalic acid and at most 50 mol% isophthalic acid, in particular from 100 mol% terephthalic acid, and a mixture of at least two diamines selected from the group consisting of hexamethylenediamine, nonanediamine, methyloctanediamine and decanediamine; semi-crystalline polyamide, made from 70-100 mol% terephthalic acid and 0-30 mol% isophthalic acid and a mixture of hexamethylenediamine and dodecanediamine;Semi-crystalline polyamide produced from at least 50 mol% terephthalic acid and at most 50 mol% dodecanedioic acid and a mixture of at least two diamines selected from the group consisting of hexamethylenediamine, nonanediamine, methyloctanediamine, and decanediamine; semi-crystalline polyamide 6T / 10T with 10 to 60 mol%, preferably 10 to 40 mol% hexamethylene terephthalamide (6T) and 40 to 90 mol%, preferably 60 to 90 mol% decamethylene terephthalamide (10T) units; semi-crystalline polyamide 6T / 10T / 6I with 50 to 90 mol%, preferably 50-70 mol% of hexamethylene terephthalamide (6T) units, and 5 to 45 mol%, preferably 10-30 mol% of hexamethylene isophthalamide (6I) units and 5 to 45 mol%, preferably 20-40 mol% of decamethylene terephthalamide (10T) units; ;

[0049] The polyamides (A1) have a solution viscosity η rel , measured according to ISO 307 (2007) on solutions of 0.5 g of polymer in 100 ml of m-cresol at a temperature of 20 °C, preferably in the range from 1.3 to 2.7, particularly preferably in the range from 1.4 to 2.3 and especially preferably in the range from 1.5 to 2.0. Component (A2)

[0050] The polyphenylene ethers used in the invention are known per se. They are prepared by conventional methods from phenols disubstituted in the ortho position by alkyl groups by oxidative coupling (see US Patents 3,661,848, 3,378,505, 3,306,874, 3,306,875, and 3,639,656). Catalysts based on heavy metals such as copper, manganese, or cobalt in combination with other substances such as secondary amines, tertiary amines, halogens, or combinations thereof are typically used for their production.

[0051] Suitable polyphenylene ethers include, for example, poly(2,6-dimethyl-1,4-phenylene) ether, poly(2,6-diethyl-1,4-phenylene) ether, poly(2-methyl-6-ethyl-1,4-phenylene) ether, poly(2-methyl-6-propyl-1,4-phenylene) ether, poly(2,6-dipropyl-1,4-phenylene) ether, poly(2-ethyl-6-propyl-1,4-phenylene) ether, or copolymers, such as those containing 2,3,6-trimethylphenol, as well as polymer blends. Poly(2,6-dimethyl-1,4-phenylene) ether is preferred, optionally in combination with 2,3,6-trimethylphenol units. The polyphenylene ethers can be used in the form of homopolymers, copolymers, graft copolymers, block copolymers, or ionomers.

[0052] Suitable polyphenylene ethers generally have an intrinsic viscosity preferably in the range of 0.1 to 0.6 dl / g, measured in chloroform at 25°C. This corresponds to a molecular weight Mn (number average) of 3,000 to 40,000 g / mol and a weight average molecular weight Mw of 5,000 to 80,000 g / mol. It is possible to use a combination of a high-viscosity and a low-viscosity polyphenylene ether. The ratio of the two different viscosities depends on the viscosities and the desired physical properties.

[0053] To improve the compatibility between component (A1) and component (A2), in a preferred embodiment, the polyphenylene ethers used are modified such that they preferably contain covalently bonded carbonyl, carboxyl, carboxylic acid, acid anhydride, acid amide, acid imide, carboxylic acid ester, carboxylate, amino, hydroxyl, epoxy, oxazoline, urethane, urea, lactam, or halobenzyl groups. For this purpose, the unmodified polyphenylene ethers (A2) are preferably modified with α,β-unsaturated dicarbonyl compounds, amide groups, or lactam group-containing monomers having a polymerizable double bond (A3), optionally in combination with free-radical initiators (A3), such as peroxides, in particular dibenzoyl peroxide, as described, for example, in EP0654505A1. Component (A3)

[0054] To improve the compatibility of components (A1) and (A2), compatibilizers in the form of functional compounds can be used that interact with the polyphenylene ether, the polyamide, or both. The interaction can be chemical (e.g., by grafting) and / or physical (e.g., by influencing the surface properties of the dispersed phase).

[0055] In a preferred embodiment of the invention, the compatibilizer additionally comprises a free-radical initiator, which is preferably an organic peroxide or an azo compound. This means that in this embodiment, the compatibilizer is graft-polymerized in the presence of a free-radical initiator.

[0056] In a particularly preferred embodiment, the compatibilizer is used without a radical initiator.

[0057] The compatibilizers may be functional compounds containing at least one carboxylic acid, carboxylic anhydride, epoxy, ester, amide or imide group, preferably in combination with olefinic double bonds. Examples include maleic acid, maleic anhydride, fumaric acid, acrylic acid, methacrylic acid, methylmaleic acid, methylmaleic anhydride, itaconic acid, itaconic anhydride, butenylsuccinic acid, butenylsuccinic anhydride, tetrahydrophthalic acid, tetrahydrophthalic anhydride N-phenylmaleimide, citric acid, malic acid and 2-hydroxynonadecane-1,2,3-tricarboxylic acid, the mono- or diesters of the acids mentioned with C1 to C12 alcohols such as methanol or ethanol, the mono- or diamides of the acids mentioned, which may optionally be substituted on the nitrogen with alkyl or aryl radicals with up to 12 C atoms and the salts with alkali or alkaline earth metals such as calcium and potassium.Maleic acid, fumaric acid, maleic anhydride, and citric acid are particularly preferred. The compatibilizer can be added alone or in combination with an optional free-radical initiator, either directly during blend preparation or the polyphenylene ether and / or polyamide can be functionalized with the compatibilizer in a separate step.

[0058] Suitable radical initiators include, for example, 1,1-di-tert-butylperoxy-3,3,5-trimethylcyclohexane, tert-butylperoxyisopropyl carbonate, tert-butylperoxy-3,3,5-trimethylhexoate, tert-butyl peracetate, tert-butyl perbenzoate, n-butyl 4,4-di-tert-butylperoxyvalerate, 2,2-di-tert-butylperoxybutane, dicumyl peroxide, tert-butylcumyl peroxide, 1,3-bis(tert-butylperoxyisopropyl)benzene, di-tert-butyl peroxide, and azoisobutyronitrile. An organic peroxide is preferred as the radical initiator, with dicumyl peroxide being particularly preferred.

[0059] Component (A3) accordingly comprises a compatibilizer or a mixture of compatibilizer and free-radical initiator. The compatibilizer and free-radical initiator are present in a total amount of 0 to 4 wt.%, preferably 0.1 to 4 wt.%, and particularly preferably 0.2 to 3 wt.%, based on the sum of (A1) to (A3). The free-radical initiator is preferably present in a range of 0 to 1 wt.%, particularly preferably 0.05 to 0.8 wt.%, based on the sum of (A1) to (A3).

[0060] In a preferred embodiment, the compatibilizer is graft polymerized without the addition of a radical initiator, ie component (A3) is preferably free of radical initiator. Component (A4)

[0061] The mixtures (A) according to the invention can contain, in addition to the polyamide (A1), the polyphenylene ether (A2) and the optional compatibilizer (A3), 0 to 20% by weight of vinyl aromatic and / or olefinic polymers (A4).

[0062] The olefinic polymer is a homo- or co-polyolefin, particularly preferably polymers based on ethylene, propylene and butylene or their copolymers as well as copolymers with other α-olefinic monomers, in particular 1-pentene, 1-hexene, 1-heptene, 1-octene and 1-decene.

[0063] The vinylaromatic polymer is preferably polystyrene or copolymers of styrene with other monomers that have at least one olefinic double bond, such as the α-olefins ethylene, propylene, and butylene, or acrylic acid or acrylic esters, or butadiene. Particular preference is given to block copolymers with at least one block formed from vinylaromatic monomers (Block A) and at least one block formed from olefinic monomers (Block B), such as those found, for example, in styrene block copolymers.

[0064] The olefinic and / or vinyl aromatic polymers used as constituents of component (A4) may be or contain a natural rubber, polybutadiene, polyisoprene, polyisobutylene, a copolymer of butadiene and / or isoprene with styrene or styrene derivatives and other comonomers, a hydrogenated copolymer and / or a copolymer formed by grafting or copolymerizing with acid anhydrides, (meth)acrylic acid and its esters.The polymers (A4) may also be a graft rubber with a crosslinked elastomeric core consisting of butadiene, isoprene or alkyl acrylates and having a graft shell of polystyrene, a non-polar or polar olefin homo- and copolymer such as ethylene-propylene, ethylene-propylene-diene and ethylene-octene or ethylene-vinyl acetate rubber or a non-polar or polar olefin homo- and copolymer formed by grafting or copolymerization with acid anhydrides, (meth)acrylic acid and their esters. The polymers (A4) may also be a carboxylic acid-functionalized copolymer such as poly(ethene-co-(meth)acrylic acid) or poly(ethene-co-1-olefin-co-(meth)acrylic acid), wherein the 1-olefin is an alkene or an unsaturated (meth)acrylic acid ester having more than 4 atoms, including those copolymers in which the acid groups are partially neutralized with metal ions.

[0065] Component (A4) is advantageously selected from the group consisting of polystyrene, polybutadiene-polystyrene graft copolymer, styrene-ethylene-butylene-styrene block copolymers (SEBS), styrene-ethylene-propylene-styrene block copolymers (SEPS), styrene-butadiene-styrene block copolymers (SBS), styrene-styrene-butadiene-styrene block copolymers (SSBS), ethylene / propylene copolymers, ethylene / propylene / diene copolymers (EPDM), polyethylene (PE), polypropylene (PP), polybutadiene (PB), poly-4-methylpentene, ethylene-propylene copolymers, ethylene-butene copolymer, ethylene-methylhexadiene copolymers, propylene-methylhexadiene copolymers, ethylene-octene copolymer, Ethylene-propylene-butene copolymers, ethylene-propylene-hexene copolymers, ethylene-propylene-methylhexadiene copolymers, poly-(ethylene vinyl acetate) (EVA), ethylene-ethyl acrylate copolymer (EEA), ethylene-hexene copolymer, ethylene-propylene-diene terpolymers, and mixtures of these polymer materials.These polymers (A4) are particularly preferably grafted with acrylic acid, methacrylic acid or maleic anhydride, the degree of grafting being 0.1 to 4.0 percent by weight based on the grafted polymer (A4).

[0066] It is further preferred that the mixture (A) contains, as component (A4), at least one vinylaromatic polymer and optionally at least one polyolefin. It is particularly preferred if the mixture (A) contains at least 5 percent by weight, in particular at least 10 percent by weight, based in each case on the total amount of (A), of a vinylaromatic polymer.

[0067] Preferably, the olefinic and / or vinylaromatic polymers (A4) are selected from the group consisting of styrene-ethylene-butylene-styrene block copolymers (SEBS), styrene-ethylene-propylene-styrene block copolymers (SEPS), styrene-butadiene-styrene block copolymers (SBS), styrene-styrene-butadiene-styrene block copolymers (SSBS), polyethylene (PE), polypropylene (PP), polybutadiene (PB), poly-4-methylpentene, ethylene-propylene copolymers, ethylene-butene copolymer, ethylene-methylhexadiene copolymers, propylene-methylhexadiene copolymers, ethylene-octene copolymer, ethylene-propylene-butene copolymers, ethylene-propylene-hexene copolymers, ethylene-propylene-methylhexadiene copolymers, Poly(ethylene vinyl acetate) (EVA), ethylene ethyl acrylate copolymer (EEA), ethylene hexene copolymer, ethylene propylene diene terpolymers, and mixtures of these polymer materials.

[0068] Furthermore, it is preferred if the olefinic and / or vinylaromatic polymers (A4) of the molding composition are grafted with carboxylic acid or carboxylic acid anhydride groups, wherein the grafting is particularly preferably carried out with acrylic acid, methacrylic acid or maleic anhydride and / or the degree of grafting is preferably 0.1 to 4.0 percent by weight, particularly preferably 0.4 to 2.5 percent by weight and especially preferably 0.5 to 2.0 percent by weight, in each case based on the grafted polymer (A4).

[0069] Component (B)is a glass-based filler present in the polyamide molding compound at 10 to 60 wt.%. The fillers can be fibrous or particulate, individually or in a mixture. Component (B) can therefore contain fibrous fillers (reinforcing agents) or particulate fillers, or even a mixture of reinforcing agents and particulate fillers. For the purposes of the invention, the terms glass-based filler, glass filler, or glass filler are used synonymously.

[0070] According to the invention, a glass filler (B) based on glass is used, the glass composition of which comprises at least 10 wt.% boron oxide and at most 15 wt.% for the sum of magnesium oxide and calcium oxide, based on the composition of the glass.

[0071] According to a preferred embodiment of the present invention, the glass filler is based on glass whose glass composition comprises 2 to 14 wt.%, particularly preferably 4 to 12 wt.% for the sum of the magnesium oxide and calcium oxide contents, based on the composition of the glass.

[0072] According to a further preferred embodiment of the present invention, the glass filler is based on glass whose glass composition comprises 12 to 24 wt.%, particularly preferably 15 to 22 wt.%, boron oxide, based on the composition of the glass.

[0073] The glass filler is preferably selected from the group consisting of fibers, ground fibers, particles, flakes, spheres, hollow spheres, and mixtures thereof, particularly preferably consisting of fibers, particles, flakes, and mixtures thereof. The glass filler is particularly preferably a glass fiber. A glass fiber with a non-circular cross-section and an axial ratio of the major to the minor cross-sectional axis in the range of 2 to 6, particularly preferably 3 to 5, is particularly preferably used as component (B).

[0074] The glass filler can be surface-treated. This can be done with a suitable sizing or adhesion promoter system. Systems based on fatty acids, waxes, silanes, titanates, polyamides, urethanes, polyurethanes, polyhydroxyethers, epoxies, nickel, or combinations or mixtures thereof can be used for this purpose. Preferably, the glass filler is surface-treated with aminosilanes, epoxysilanes, polyamides, or mixtures thereof.

[0075] If fibers are selected as the glass filler for component (B), the glass fibers are preferably selected from the group consisting of chopped fibers, continuous fibers, and mixtures thereof, wherein the fibers may have a circular or non-circular cross-section. Non-circular or non-round glass fibers are also referred to as flat glass fibers and may have an oval, elliptical, angular, rectangular, or nearly rectangular cross-sectional area.

[0076] The chopped glass fibers preferably have a fiber length of 1 to 25 mm, preferably 1.5 to 20 mm, particularly preferably 2 to 12 mm and most particularly preferably 2 to 8 mm.

[0077] The cut glass fibers preferably have a diameter of 5 to 20 µm, preferably 5 to 15 µm and particularly preferably 6 to 12 µm.

[0078] If the glass fibers are used as continuous fibers (roving), they preferably have a diameter of maximum 20 µm, preferably maximum 18 µm, particularly preferably 5 to 17 µm.

[0079] For flat glass fibers, the aspect ratio, i.e., the ratio of the main cross-sectional axis to the secondary cross-sectional axis, is 2 to 8, preferably 2 to 6, particularly preferably 3 to 5. The cross-sectional axes of the flat glass fibers are 3 to 40 µm long. The length of the secondary cross-sectional axis is preferably 3 to 20 µm, particularly preferably 4 to 10 µm, and the length of the main cross-sectional axis is 6 to 40 µm, particularly preferably 12 to 30 µm.

[0080] Mixtures of fibers with circular (round) and non-circular (flat) cross-sections can also be used to reinforce the polyamide molding compositions according to the invention.

[0081] If glass spheres or glass particles are selected as the glass filler (B), their mean volumetric diameter (D50) is preferably 0.3 to 100 µm, particularly preferably 5 to 80 µm and especially preferably 17 to 70 µm, measured by laser diffraction according to ASTM B 822-10 (2010).

[0082] Furthermore, the glass filler has a relative permittivity of preferably at most 7, particularly preferably at most 5 and a dielectric loss factor of preferably at most 0.0040 and particularly preferably at most 0.0030, determined using a glass plate (80 x 80 x 3 mm) made of the glass of the glass filler according to IEC 61189-2-721 (2015) with a split post dielectric resonator (SPDR) from QWED, Poland at a frequency of 2.45 GHz and a temperature of 23 °C.

[0083] According to a preferred embodiment of the present invention, component (B) is present in the polyamide molding composition preferably in an amount of 15 to 55% by weight, particularly preferably in an amount of 18 to 52% by weight, these amounts being based on the sum of components (A) to (D).

[0084] According to a preferred embodiment of the present invention, component (B) consists exclusively of a glass filler selected from the group consisting of glass fibers, ground glass fibers, glass particles, glass flakes, glass spheres, hollow glass spheres, or combinations of the aforementioned, wherein the glass filler consists of glass in which the sum of the magnesium oxide and calcium oxide contents is in the range from 2 to 14 wt.% and the boron oxide (B 2 O 3 ) content is in the range from 12 to 24 wt.%, in each case based on the composition of the glass. Particularly preferably, the glass filler is formed entirely from glass fibers.

[0085] In a particularly preferred embodiment, component (B) is selected as a glass filler, particularly preferably as a glass fiber, the glass of which comprises the following composition: 52.0 to 57.0 wt.% silicon dioxide, 13.0 to 17.0 wt.% aluminum oxide, 15.0 to 22.0 wt.% boron oxide, 2.0 to 6.0 wt.% magnesium oxide, 2.0 to 6.0 wt.% calcium oxide, 1.0 to 4.0 wt.% titanium dioxide, 0 to 1.5 wt.% fluorine, 0 to 0.6 wt.% alkali oxides.

[0086] Preferably, the proportion of Component (C) in the range of 2 to 6 wt.%, preferably in the range of 3 to 5 wt.%, in each case based on the molding composition (sum of components (A) to (D)).

[0087] Component (C) is preferably an LDS additive with an absorption coefficient for UV, VIS or IR radiation that is different from zero and which, under the action of electromagnetic radiation, preferably as laser radiation, forms metal nuclei that facilitate and / or enable and / or improve the deposition of metal layers for producing conductor tracks at the irradiated locations on the molded part surface in a chemical metallization process, wherein the LDS additive preferably has an absorption capacity in the visible and infrared radiation range with an absorption coefficient of at least 0.05, preferably at least 0.1 and in particular at least 0.2, and / or that an absorber is preferably provided that transfers the radiation energy to the LDS additive.

[0088] Component (C) is preferably an LDS additive having an average particle size (D50) in the range of 50 - 10,000 nanometers, preferably 200 to 5,000 nanometers and particularly preferably 300 to 4,000 nanometers, and / or an aspect ratio of at most 10, in particular of at most 5. The D50 value given as a measure of the particle size is a measure of the average particle size, with 50 volume percent of the sample being finer and the other 50% of the sample being coarser than the D50 value (median).

[0089] Component (C) is preferably an LDS (Laser Direct Structuring) additive selected from the group of metal oxides, in particular so-called spinels with the general chemical formula AB 2 O 4 , where A stands for a metal cation with valence 2 and B stands for a metal cation with valence 3. The metal cation A is preferably selected from the group consisting of magnesium, copper, cobalt, zinc, tin, iron, manganese and nickel and combinations thereof, and the metal cation B is preferably selected from the group consisting of manganese, nickel, copper, cobalt, tin, titanium, iron, aluminum and chromium and combinations thereof.

[0090] The LDS additive is particularly preferably a copper iron spinel, a copper-containing magnesium aluminum oxide, a copper-chromium-manganese mixed oxide, a copper-manganese-iron mixed oxide, optionally in each case with oxygen vacancies, or salts and oxides of copper, such as in particular copper(I) oxide, copper(II) oxide, basic copper phosphates, copper sulfate, and metal complex compounds, in particular chelate complexes of copper, tin, nickel, cobalt, silver and palladium or mixtures of such systems, and / or in particular selected from the following group: copper-chromium-manganese mixed oxides, copper-manganese-iron mixed oxides, copper chromium oxide, copper tungstate, zinc iron oxide, cobalt chromium oxide, cobalt aluminum oxide, magnesium aluminum oxide, and mixtures and / or surface-treated and / or oxygen-defect-containing forms thereof. Possible systems are those described in WO-A-2000 / 35259 or in Kunststoffe 92 (2002) 11, 2-7.

[0091] Also preferred as component (C) is an LDS (Laser Direct Structuring) additive selected from the group of metal oxides, mixed metal oxides, metal hydroxide oxides, and metal sulfide oxides based on tin. Particular preference is given to tin oxide and doped tin oxide, wherein the doping can be carried out with antimony, bismuth, molybdenum, aluminum, titanium, silicon, iron, copper, silver, palladium, and cobalt. Tin oxide doped with antimony, titanium, or copper is particularly preferred. Furthermore, mixtures of tin oxide and at least one other metal oxide, in particular antimony oxide, are preferred as LDS additives. As further metal oxides, both colorless, highly refractive metal oxides, such as, in particular, titanium dioxide, antimony(III) oxide, zinc oxide, tin oxide, and / or zirconium dioxide, and colored metal oxides such as, for example, chromium oxide, nickel oxide, copper oxide, cobalt oxide, and in particular iron oxide (Fe2O3, Fe3O4), are used.Particularly preferred is the mixture of tin oxide and antimony(III) oxide.

[0092] The doped tin oxides or metal oxide mixtures or tin oxide are preferably formed as layers on platelet-shaped substrates, in particular layered silicates, such as synthetic or natural mica, talc, kaolin, glass flakes, or silicon dioxide flakes. Mica or mica flakes are particularly preferred as substrates for the metal oxides. Platelet-shaped metal oxides such as platelet-shaped iron oxide, aluminum oxide, titanium dioxide, silicon dioxide, LCPs (liquid crystal polymers), holographic pigments, or coated graphite flakes are also suitable as substrates.

[0093] Particularly preferred are LDS additives based on mica, where the mica surface is coated with metal-doped tin oxides. Antimony-doped tin oxide is particularly preferred. Examples of commercially available LDS additives according to the present invention are: Lazerflair LS820, LS825, LS830, and Minatec 230 A-IR from Merck; Stanostat CP40W, Stanostat CP15G, or Stanostat CP5C from Keeling & Walker; and Fabulase 322S, 330, 350, and 352 from Budenheim.

[0094] The most preferred LDS additives are copper chromite, copper tungstate, copper phosphate hydroxide, and antimony-doped tin oxide, the latter preferably used in combination with mica. Copper tungstate is especially preferred.

[0095] The thermoplastic molding composition according to the invention contains 0 to 5 wt.% of at least one additive as Component (D), which is different from components (A), (B) and (C).

[0096] According to a preferred embodiment, the molding composition according to the invention contains 0.1 to 5 wt.% and preferably 0.2 to 4 wt.%, based on the sum of components (A) to (D), of at least one additive as component (D).

[0097] According to a preferred embodiment, the additives of components (D) are selected from the group consisting of stabilizers, age inhibitors, antioxidants, antiozonants, processing stabilizers, processing aids, viscosity modifiers, light stabilizers, UV stabilizers, UV absorbers, inorganic heat stabilizers, in particular based on copper halides and alkali halides, organic heat stabilizers, optical brighteners, crystallization accelerators, crystallization retarders, flow aids, lubricants, glidants, mold release agents, colorants, in particular dyes, inorganic pigments, organic pigments, marking substances and mixtures thereof.

[0098] According to a particularly preferred embodiment, the molding composition according to the invention contains at least one processing aid as component (D), this being present preferably in a proportion of 0 to 2 wt.%, particularly preferably from 0.1 to 2.0 wt.%, particularly preferably from 0.1 to 1.5 wt.% and most preferably from 0.2 to 1.0 wt.%, in each case based on the total weight of components (A) to (D). Preference is given to Al, alkali metal, alkaline earth metal salts, esters or amides of fatty acids having 10 to 44 C atoms and preferably having 14 to 44 C atoms, with the metal ions Na, Mg, Ca and Al being preferred and Ca or Mg being particularly preferred. Particularly preferred metal salts are magnesium stearate, calcium stearate and calcium montanate and also aluminum stearate. The fatty acids can be mono- or divalent.Examples include pelargonic acid, palmitic acid, lauric acid, margaric acid, dodecanedioic acid, behenic acid and the particularly preferred stearic acid, capric acid and montanic acid (mixture of fatty acids with 30 to 40 C atoms).

[0099] According to a further preferred embodiment, the molding composition according to the invention contains as component (D) at least one heat stabilizer, this being preferably present in a proportion of 0 to 3% by weight, particularly preferably of 0.1 to 2.0% by weight, in each case based on the total weight of components (A) to (D).

[0100] According to a preferred embodiment, the heat stabilizers are selected from the group consisting of: Compounds of mono- or divalent copper, e.g. salts of mono- or divalent copper with inorganic or organic acids or mono- or divalent phenols, the oxides of mono- or divalent copper, or the complex compounds of copper salts with ammonia, amines, amides, lactams, cyanides or phosphines, preferably Cu(I) or Cu(II) salts of hydrohalic acids, hydrocyanic acids or the copper salts of aliphatic carboxylic acids. Particularly preferred are the monovalent copper compounds CuCl, CuBr, CuI, CuCN and Cu2O, as well as the divalent copper compounds CuCl2, CuSO4, CuO, copper(II) acetate or copper(II) stearate. Advantageously, the copper compounds are used in combination with other metal halides, in particular alkali halides, such as NaI, Cl, NaBr, KBr, wherein the molar ratio of metal halide to copper halide is 0.5 to 20, preferably 1 to 10 and particularly preferably 3 to 7. Stabilizers based on secondary aromatic amines, these stabilizers preferably being present in an amount of 0.1 to 2, preferably 0.2 to 0.5 wt.%, stabilizers based on sterically hindered phenols, these stabilizers preferably being present in an amount of 0.1 to 1.5, preferably 0.2 to 0.6 wt.%, and phosphites and phosphonites, as well as mixtures of the above-mentioned stabilizers.

[0101] Examples of stabilizers based on secondary aromatic amines which can be used according to the invention are adducts of phenylenediamine with acetone (Naugard A), adducts of phenylenediamine with linolene, Naugard 445, N,N'-dinaphthyl-p-phenylenediamine, N-phenyl-N'-cyclohexyl-p-phenylenediamine or mixtures thereof.

[0102] In principle, all compounds with a phenolic structure that have at least one sterically demanding group on the phenolic ring are suitable as sterically hindered phenols. Preferred examples of stabilizers based on sterically hindered phenols that can be used according to the invention are N,N'-hexamethylene-bis-3-(3,5-di-tert-butyl-4-hydroxyphenyl)-propionamide, bis-(3,3-bis-(4'-hydroxy-3'-tert-butylphenyl)-butanoic acid) glycol ester, 2,1'-thioethylbis-(3-(3,5-di-tert-butyl-4-hydroxyphenyl)-propionate, 4-4'-butylidene-bis-(3-methyl-6-tert-butylphenol), triethylene glycol 3-(3-tert-butyl-4-hydroxy-5-methylphenyl)-propionate, or mixtures of two or more of these stabilizers.

[0103] Bevorzugte Phosphite und Phosphonite sind Triphenylphosphit, Diphenylalkylphosphit, Phenyldialkylphosphit, Tris(nonylphenyl)phosphit, Trilaurylphosphit, Trioctadecylphosphit, Distearylphentaerythritoldiphosphit, Tris(2,4-di-tert-butylphenyl)phosphit, Diisodecylpentaerythritoldiphosphit, Bis(2,4-di-tert-butylphenyl)pentaerythritoldiphosphit, Bis(2,6-di-tert-butyl-4-methylphenyl)-pentaerythritoldiphosphit, Diisodecyloxypentaerythritoldiphosphit, Bis(2,4-di-tert-butyl-6-methylphenyl)pentaerythritoldiphosphit, Bis(2,4,6-tris-(tert-butylphenyl))pentaerythritol-diphosphit, Tristearylsorbitoltriphosphit, Tetrakis(2,4-di-tert-butylphenyl)-4,4'-biphenylendiphosphonit, 6-Isooctyloxy-2,4,8,10-tetra-tert-butyl-12H-dibenz-[d,g]-1,3,2-dioxaphosphocin, 6-Fluoro-2,4,8,10-tetra-tert-butyl- 12-methyl-dibenz[d,g]-1,3,2-dioxaphosphocin, Bis(2,4-di-tert- butyl-6-methylphenyl)methylphosphit und Bis(2,4-di-tert-butyl-6-methylphenyl)ethylphosphit.In particular, tris[2-tert-butyl-4-thio(2'-methyl-4'-hydroxy-5'-tert-butyl)-phenyl-5-methyl]phenyl phosphite and tris(2,4-di-tert-butylphenyl) phosphite (Irgafos 168) are preferred.

[0104] A preferred embodiment of the heat stabilizer consists in the combination of organic heat stabilizers, in particular Irgafos 168 and Irganox 1010 or HOSTANOX O 3 P (bis[3,3-bis-(4'hydroxy-3'-tert-butylphenyl) butanoic acid glycol ester) and SANDOSTAB P-EPQ (tetrakis(2,4-di-tert-butylphenyl)-4,4'-biphenyl diphosphonite). Heat stabilization based exclusively on Cul and Kl is particularly preferred.

[0105] Examples of oxidation retarders and heat stabilizers include phosphites and other amines (e.g. triacetonediamine), hydroquinones, various substituted representatives of these groups and mixtures thereof in concentrations of up to 1 wt.%, based on the weight of components (A) to (D).

[0106] UV stabilizers, which are generally used in amounts of up to 2% by weight, based on the weight of the molding compound, include various substituted resorcinols, salicylates, benzotriazoles, triazines and benzophenones.

[0107] Inorganic pigments such as titanium dioxide, ultramarine blue, iron oxide, carbon black and / or graphite, as well as organic pigments such as phthalocyanines, quinacridones, perylenes, and dyes such as nigrosine and anthraquinones, can be added as colorants. However, it is preferred that the molding composition according to the invention contains neither carbon black nor graphite, ie, the molding composition according to the invention is preferably free of carbon black and graphite.

[0108] In a particularly preferred embodiment, the thermoplastic molding composition according to the invention consists of: (A) 34 to 82.9 wt.% of a mixture of at least one polyamide (A1), at least one polyphenylene ether (A2), and a compatibilizer (A3); (B) 15 to 55 wt.% of glass fiber, the glass composition of which comprises 12 to 24 wt.% boron oxide and 2 to 14 wt.% for the sum of magnesium oxide and calcium oxide; (C) 2 to 6 wt.% LDS additive selected from the group consisting of copper chromium oxide, copper tungstate, copper oxide, copper hydroxide phosphate, tin hydroxide phosphate, tin phosphate, copper phosphate, basic copper phosphates, and tin phosphates, or mixtures thereof, preferably selected as copper tungstate; (D) 0.1 to 5 wt.% of additives other than (A), (B), and (C); wherein the mixture (A) consists of 52 to 89.8 wt.% of component (A2), 10 to 45 % by weight of component (A1), to 0.2 to 3 wt. % of component (A3), in each case based on the sum of components (A1) to (A3), wherein the sum of components (A1) to (A3) results in 100 wt. % of the mixture (A) and wherein the sum of components (A) to (D) results in 100 wt. % of the molding composition.

[0109] The molding compounds according to the invention have good mechanical properties, can be easily metallized after irradiation and are characterized by a low relative permittivity of less than 3.0 and a low dielectric loss factor of less than 0.008.

[0110] A preferred variant for producing the molding composition according to the invention comprises preparing the mixture comprising components (A1) to (A4) in a first step. For this purpose, components (A2), (A3), and optionally (A4) can first be metered into the feed of an extruder and mixed at a temperature in the range from 220 to 340°C. By means of a side feeder, component (A1) can then be introduced into the melt mixture formed from components (A2), (A3), and optionally (A4) in a barrel of the extruder downstream of the feed. Alternatively, components (A1) to (A4) can also be metered into the feed of an extruder and mixed in the extruder at a temperature of 220 to 340°C. In both variants, components (C) and / or (D) can additionally be included, with these components preferably being metered into the feed.In a second extrusion step, the mixture (A) and the components (C) and (D) or the mixture of (A), (C) and (D) can then be metered into the feed of the extruder and melted at a temperature of 220 - 340 °C, while component (B) is then fed via a side feeder into a barrel of the extruder downstream of the feed and mixed with the existing melt.

[0111] Another preferred production process for the molding compound involves metering components (A1) to (A4), (C), and (D) into the feed of an extruder and melting and mixing them in a first extruder section at a temperature of 220 to 340 °C. Component (B) is then introduced into the melt via a side feeder and mixed with the remaining components in a second extruder section. The molding compound is then discharged and, after cooling, granulated. Underwater granulation is preferred for high filler contents.

[0112] Furthermore, the invention comprises a shaped body which contains the above-described thermoplastic molding composition according to the invention or which preferably consists of this molding composition.

[0113] This molded body preferably comprises components, housings or housing parts of devices that communicate with electromagnetic waves with a frequency of 0.3 to 300 GHz.

[0114] In particular, the shaped bodies are selected from the group consisting of components, housings or housing parts of transmitting and receiving devices, mobile phones, tablets, laptops, navigation devices, surveillance cameras, photo cameras, sensors, diving computers, audio systems, remote controls, loudspeakers, headphones, radios, televisions, household appliances, kitchen appliances, door or gate openers, operating devices for central locking in vehicles, keyless-go vehicle keys, temperature measuring or temperature display devices, measuring devices and control devices. WAYS OF IMPLEMENTING THE INVENTION Measurement methods:

[0115] The following measurement methods were used in this application: Relative viscosity

[0116] The relative viscosity was determined according to ISO 307 (2007) at 20 °C. For this purpose, 0.5 g of polymer granules were weighed into 100 ml of m-cresol. The relative viscosity (RV) was calculated using RV = t / t0 based on Section 11 of the standard. Glass transition temperature (Tq) and melting point (Tm)

[0117] The glass transition temperature and melting point were determined on granules according to ISO 11357-2 and -3 (2013). Differential scanning calorimetry (DSC) was performed for each of the three heating cycles at a heating rate of 20 K / min. After the first heating cycle, the sample was cooled at a rate of 20 K / min, and the melting point was determined during the subsequent heating cycle (second heating cycle). The sample was then quenched in dry ice, and the glass transition temperature (Tg) was determined during the third heating cycle. The temperature at the peak maximum was given as the melting point. The midpoint of the glass transition range, which was given as the glass transition temperature (Tg), was determined using the half-height method. Tensile modulus of elasticity

[0118] The determination of the tensile modulus of elasticity was carried out according to ISO 527 (2012) at 23°C with a tensile speed of 1 mm / min on an ISO tensile test specimen (type A1, mass 170 x 20 / 10 x 4) manufactured according to the standard: ISO / CD 3167 (2003). Breaking stress and elongation

[0119] The determination of stress and elongation at break was carried out according to ISO 527 (2012) at 23°C with a tensile speed of 5 mm / min for reinforced materials on an ISO tensile bar, type A1 (dimensions 170 x 20 / 10 x 4 mm), manufactured according to ISO / CD 3167 (2003). Relative permittivity and dielectric loss factor (DVF)

[0120] The relative permittivity εr and the dielectric loss factor (DVF) are measured according to IEC 61189-2-721 (2015) on 80 x 80 x 3 mm film-cast plates using a split-post dielectric resonator (SPDR) from QWED, Poland (a brochure including measurement information is available at www.qwed.eu). The measurement frequency is 2.45 GHz, and the measurement temperature is 23 °C. Spray shrinkage

[0121] The plates (type D2, 60 x 60 x 2 mm, film gate) were manufactured for the determination of injection shrinkage according to ISO 294-3 (2002) and Amendment 1 (2006). Injection shrinkage was determined according to ISO 294-4 (2001) after storage of the plates for 14 days under standard conditions (23 °C, 50% relative humidity) in relation to the mold cavity size, both longitudinally and transversely to the flow direction of the molding melt. The arithmetic mean value from measurements on five plates is given. The ratio of injection shrinkage longitudinally and transversely to the flow direction of the molding melt is also referred to below as warpage. Laser structuring and metallization:

[0122] To evaluate the metallization behavior, injection-molded parts (60 x 60 x 2 mm plate) were structured using an Nd:YAG laser and subsequently metallized in a copper plating bath without electrolysis. During laser structuring, 18 adjacent 10 x 10 mm areas on the part surface were irradiated. Laser structuring was performed using a FOBA DP50 laser at a wavelength of 1064 nm and an irradiation width of approximately 50 µm at a speed of 4 m / s. Both the pulse frequency and the laser current were varied. For the specific pulse frequencies of 5, 6, 7, and 8 kHz, the laser diode current was set to 24.0, 24.5, 25.0, and 25.5 amperes, respectively. Following laser structuring, the molded parts were subjected to a cleaning process to remove laser process residues. The molded parts were successively passed through ultrasonic baths containing surfactant and deionized water.The cleaned molded parts were then metallized in a reductive copper plating bath (MacDermid MID-Copper 100 B1) for 20 - 30 minutes.

[0123] Assessment of metallization: o: in fewer than 14 areas, copper was deposited with an average thickness of at least 3 µm; +: in 14 or 15 areas, copper was deposited with an average thickness of at least 3 µm; ++: In all 16 areas, copper was deposited with an average thickness of at least 3 µm;

[0124] In the context of the invention, sufficiently metallized means that copper is deposited in at least 14 areas with an average thickness of at least 3 µm. Dyeability:

[0125] F: The molding compounds can be colored in other colors besides black, such as yellow, orange, red, or blue. S: The molding compounds are black and cannot be colored in other colors. Glass composition of the glass filler

[0126] The glass composition of the glass filler, in particular the glass fibers, was determined using the following methods: inductively coupled plasma optical emission spectrometry (ICP OES) according to DIN 51086-2:2004, titrimetric determination of the boron oxide content according to ISO 21078-1:2008, X-ray fluorescence fusion method according to ISO 12677:2003, fluorine determination after pyrohydrolysis according to DIN 51084:2008. Production of polyamide molding compounds

[0127] For the inventive examples B1 to B9 and for the comparative example VB4, the various mixtures (A) were first prepared. For this purpose, the respective amounts of polyphenylene ether (A2) and compatibilizer (A3) were metered into the feed zone of a Werner & Pfleiderer ZSK 25 twin-screw extruder according to Tables 2 and 3, and the polyamide component (A1) was introduced into the melt via a side feeder 6 barrel zones before the exit. The temperature of the first barrel was set to 70 °C, that of the remaining barrels for the examples with polyamide 1 to 260 to 290 °C and for the examples with polyamide 2 to 290 to 320 °C. A speed of 300 rpm and a throughput of 10 kg / h were used, and atmospheric degassing was performed. The strands were cooled in a water bath, cut and the resulting granules were dried at 100 °C for 24 h in vacuum (30 mbar).The dried granules of mixture (A), the polyamides, or polyphenylene ethers were then blended with the additives (C) and (D) to form a dry blend in the ratios specified in Tables 2 and 3. This mixture was homogenized using a tumble mixer for approximately 20 minutes. The molding compounds were produced on a Werner & Pfleiderer ZSK 25 twin-screw extruder in the ratios specified in Tables 2 and 3. The dry blend was metered into the feed via a dosing scale. The glass fibers (B) were metered into a side feeder via a dosing scale, which conveyed the glass fibers (B) into the melt six housing units upstream of the die. The temperature of the first housing was set to 80 °C, that of the remaining housings to 260 to 280 °C for examples B1 to B3, B7, B8, VB1 and VB2 and to 280 to 310 °C for examples B4 to B6, B9, VB3 and VB4.A speed of 250 rpm and a throughput of 15 kg / h were used, and the material was degassed atmospherically. The strands were cooled in a water bath, cut, and the resulting granules were dried at 110 °C for 24 h under vacuum (30 mbar) to a water content below 0.1 wt.%. Production of the test specimens

[0128] The test specimens were produced on an Arburg Allrounder 420 C 1000-250 injection molding machine. Cylinder temperatures ranged from 260 °C to 280 °C and a mold temperature of 80 °C were used for examples B1 - B3, B7, B8, VB1, and VB2, and cylinder temperatures ranged from 290 °C to 320 °C and a mold temperature of 120 °C were used for examples B4 - B6, B9, VB3, and VB4. Unless otherwise stated, the test specimens were used in a dry state; for this purpose, they were stored for at least 48 hours after injection molding at room temperature in a dry environment, i.e., over silica gel. Table 1: Materials used in the examples and comparative examples Components Description Manufacturer Polyamide-1 (component A1) Polyamide 12 made from laurolactam, RV = 1.90, Tm = 178 °C EMS-CHEMIE AG, Switzerland Polyamide-2 (component A1) Polyamide 10T / 6T made from 1,6-hexanediamine, 1,10-decanediamine and terephthalic acid RV = 1.78, Tm = 295 °C EMS-CHEMIE AG, Switzerland Polyphenylene ether (component A2) IUPIACE PX100F, Poly(oxy-2,6-dimethyl-1,4-phenylene), CAS No.: 25134-01-4; RV = 1.12 Mitsubishi Engineering Plastics Corporation, Japan MAH (component A3) Maleic anhydride, CAS No.: 108-31-6 (compatibility agent) Lanxess, Germany Glass fiber type 1 (component B, glass fiber according to the invention) NITTOBO CNG3PA-820, flat glass fiber, length = 3 mm, major cross-sectional axis 28 mm, minor cross-sectional axis 7 mm, aspect ratio of the cross-sectional axes = 4, glass composition: Mg oxide + Ca oxide = 8.3 wt%, boron oxide = 19.4 wt%, RP = 4.8, DVF = 0.0015 Nitto Boseki Co., LTD., Japan Glass fiber type 2 (non-inventive glass fiber) NITTOBO CSG3PA-820, flat glass fiber, length = 3 mm, major cross-sectional axis 28 mm, minor cross-sectional axis 7 mm, aspect ratio of the cross-sectional axes = 4, glass composition: Mg oxide + Ca oxide = 23.6 wt%, boron oxide = 6.1 wt%, RP = 6.8, DVF = 0.0035 Nitto Boseki Co., LTD., Japan LDS-1 (component C) SHEPHERD BLACK 30C965, copper chromite (CuCr 2 O 4 ) with an average particle size D50 of 0.6 µm The Shepherd Color Company, USA LDS-2 (component C) SHEPHERD EX1815, CAS No. 13587-35-4 Copper tungstate (CuWO 4 ) with an average particle size D50 of 1.1 µm The Shepherd Color Company, USA Stabilizer (component D) Mixture of Clariant Products AG, Switzerland D1: HOSTANOX O 3 P, Bis[3,3-bis-(4'hydroxy-3'-tert-butyl-phenyl) butanoic acid glycol ester, CAS No.: 32509-66-3 D2: SANDOSTAB P-EPQ, tetrakis(2,4-di-tert-butylphenyl)-4,4'- biphenyl diphosphonite, CAS no. 119345-01-6 D3: HOSTAVIN N 30 P, HALS (Hindered Amine Light Stabilizer), CAS No.: [202483-55-4 in the ratio 4 : 1 : 2 (D1 : D2 : D3) Processing aids (component D) Magnesium Stearate AV Baerlocher GmbH, Germany RP: Relative permittivity; DVF: Dielectric loss factor Table 2: Results Unit B1 B2 B3 B4 B5 B6 B7 Mixture (A) % by weight 1)< 75.1 75.1 75.1 75.1 75.1 75.1 65.1 Polyamide-1 (A1) % by weight 2)< 10 30 45 30 Polyamide-2 (A1) % by weight 2)< 10 30 45 Polyphenylene ether (A2) % by weight 2)< 88 68 53 88 68 53 68 MAH (A3) % by weight 2)< 2 2 2 2 2 2 2 Fiber optic type 1 (B) % by weight 1)< 20.0 20.0 20.0 20.0 20.0 20.0 30 Fiber optic type 2 % by weight 1)< LDS-1 (C) % by weight 1)< 4.0 4.0 4.0 4.0 4.0 4.0 4.0 Stabilization (D) % by weight 1)< 0.7 0.7 0.7 0.7 0.7 0.7 0.7 Processing aids % by weight 1)< 0.2 0.2 0.2 0.2 0.2 0.2 0.2 Tensile modulus of elasticity MPa 5900 5720 5400 6220 6430 6440 6800 Breaking stress MPa 78 83 87 101 94 101 89 Elongation at break % 1.9 2.1 2.5 2.1 1.9 2.1 1.9 Spray shrinkage, longitudinal % 0.64 0.71 0.57 0.48 0.56 0.534 0.28 Spray shrinkage, transverse % 0.75 0.82 0.69 0.58 0.61 0.64 0.35 Delay - 1.17 1.15 1.21 1.21 1.09 1.21 1.25 Relative permittivity - 2.8 2.8 2.8 2.8 2.9 2.9 2.9 DVF - 0.006 0.006 0.007 0.005 0.006 0.007 0.007 Metallizability ++ ++ ++ + + + ++ Dyeability S S S S S S S 1)< based on the sum of components (A) to (D) 2)< based on the sum of components (A1) to (A3); A4 = 0 wt.% 3)< Warpage = ratio of injection shrinkage transverse to longitudinal Table 3: Results Unit B8 B9 VB1 VB2 VB3 VB4 Mixture (A) % by weight 1)< 75.1 75.1 75.1 75.1 75.1 75.1 Polyamide-1 (A1) % by weight 2)< 30 0 100 0 Polyamide-2 (A1) % by weight 2)< 30 0 0 100 49 Polyphenylene ether (A2) % by weight 2)< 68 68 100 0 0 49 MAH (A3) % by weight 2)< 2 2 0 0 0 2 Fiber optic type 1 (B) % by weight 1)< 20.0 20.0 20.0 20.0 20.0 Fiber optic type 2 % by weight 1)< 20.0 LDS-1 (C) % by weight 1)< 4.0 4.0 4.0 4.0 LDS-2 (C) % by weight 1)< 4.0 4.0 Stabilization (D) % by weight 1)< 0.7 0.7 0.7 0.7 0.7 0.7 Processing aids % by weight 1)< 0.2 0.2 0.2 0.2 0.2 0.2 Tensile modulus of elasticity MPa 5860 6430 5900 5400 6500 6440 Breaking stress MPa 86 101 96 89 110 101 Elongation at break % 1.9 2.0 2.3 4.8 2.9 2.1 Spray shrinkage, longitudinal % 0.59 0.66 0.50 0.58 0.65 0.534 Spray shrinkage, transverse % 0.7 0.79 0.82 0.66 0.75 0.64 Delay - 1.19 1.20 1.64 1.14 1.15 1.21 Relative permittivity - 2.8 2.8 2.8 3.0 3.1 3.1 DVF - 0.007 0.007 0.004 0.013 0.012 0.009 Metallizability ++ + + ++ + + Dyeability F F S S S S ' based on the sum of components (A) to (D) 2)< based on the sum of components (A1) to (A3); A4 = 0 wt.% 3)< Warpage = ratio of injection shrinkage transverse to longitudinal

Claims

1. A thermoplastic molding composition consisting of: A Mixture of at least one polyamide A1, at least one polyphenylene ether A2 and optionally a compatibilizer A3 and optionally an olefinic and / or vinylaromatic polymer A4; B 10 to 60% by weight of glass filler, the glass composition of which comprises at least 10% by weight of boron oxide and at most 15% by weight for the sum of magnesium oxide and calcium oxide; C 1 to 8% by weight of LDS additive; D 0 to 5% by weight of additives other than components A, B and C; wherein 80 to 100% by weight of mixture A consists of a mixture M of components A1, A2 and A3 and 0 to 20% by weight of component A4, each based on the sum of components M and A4, and wherein the sum of components M and A4 gives 100% by weight of mixture A; and where the mixture M consists of from 36 to 92% by weight of component A2, from 8 to 60% by weight of component A1 and from 0 to 4% by weight of component A3, in each case based on the sum of components A1 to A3, and where the sum of components A1 to A3 gives 100% by weight of the mixture M; and the sum of components A to D being 100% by weight of the molding composition.

2. A thermoplastic molding composition according to claim 1, wherein component A1 is present in the mixture M in a proportion of from 10 to 48% by weight, particularly preferably from 10 to 45% by weight, based on the sum of components A1 to A3; and component A2 is present in the mixture M in a proportion of from 48 to 89.9 percent by weight, particularly preferably from 52 to 89.8 percent by weight, based on the sum A1 to A3; and component A3 is present in the mixture M in a proportion of from 0.1 to 4% by weight, particularly preferably from 0.2 to 3% by weight, based on the sum A1 to A3; and / or the mixture A consists exclusively of components A1 to A3.

3. A thermoplastic molding composition according to one of the preceding claims, <b>characterized in that the glass filler B is based on glass whose composition contains 2 to 14% by weight, particularly preferably 4 to 12% by weight for the sum of the magnesium oxide and calcium oxide contents, based on the composition of the glass; and / or 12 to 24% by weight, particularly preferably 15 to 22% by weight, of boron oxide, based on the composition of the glass; or 52.0 to 57.0% by weight of silica, 13.0 to 17.0% by weight of aluminum oxide, 15.0 to 21.5% by weight of boron oxide, 2.0 to 6.0% by weight of magnesium oxide, 2.0 to 6.0% by weight of calcium oxide, 1.0 to 4.0% by weight of titanium dioxide, 0 to 1.5% by weight of fluorine, 0 to 0.6% by weight of alkali oxides.

4. A thermoplastic molding composition according to claim 3, characterized in that the glass filler B is selected from the group consisting of fibers, ground fibers, particles, flakes, spheres, hollow spheres or combinations of the foregoing; or as glass fibers; or as glass fibers having a non-circular cross-section and an axis ratio of major to minor cross-sectional axis in the range of from 2 to 6, preferably from 3 to 5.

5. A thermoplastic molding composition according to any one of the preceding claims, characterized in that the at least one polyamide A1 is selected as aliphatic polyamide from the group consisting of PA 46, PA 6, PA 66, PA 6 / 66, PA 10, PA 11, PA 12, PA 516, PA 610, PA 612, PA 614, PA 616, PA 618, PA 1010, PA 1012, PA 1014, PA 1016, PA 1018, PA 1212 and mixtures thereof, PA 610, PA 612, PA 1010, PA12 and PA 616 being preferred; and / or semi-crystalline partially aromatic polyamide selected from the group consisting of: PA 4T / 4I, PA 4T / 6I, PA 5T / 5I, PA 6T / 6, PA 6T / 6I, PA 6T / 6I / 6, PA 6T / 66, 6T / 610, 6T / 612, PA 6T / 10T, PA 6T / 10I, PA 9T, PA 10T, PA 12T, PA 10T / 10I, PA10T / 106, PA10T / 610, PA10T / 612, PA10T / 66, PA10T / 6, PA10T / 1010, PA10T / 1012, PA10T / 12, PA10T / 11, PA 6T / 9T, PA 6T / 12T, PA 6T / 10T / 6I, PA 6T / 6I / 6, PA 6T / 6I / 12 and mixtures thereof, PA 6T / 6I, PA 6T / 10T, PA 6T / 10T / 6I being preferred; and / or amorphous or microcrystalline polyamide selected from the group consisting of: PA 6I / 6T, PA MACM9, PA MACM10, PA MACM12, PA MACM13, PA MACM14, PA MACM16, PA MACM17, PA MACM18, PA PACM10, PA PACM12, PA PACM13, PA PACM14, PA PACM16, PA PACM17, PA PACM18, PA TMDC10, PA TMDC12, PA TMDC13, PA TMDC14, PA TMDC16, PA TMDC17, PA TMDC18, PA MACM10 / 10, PA MACMI / 12, PA MACMT / 12, PA 6I / MACMI / MACMT, PA MACMI / MACMT / 12, PA MACMI / MACMT / MACM12, PA MACMI / MACMT / MACM12 / 12, PA 6I / 6T / MACMI / MACMT / 12, PA 6I / 6T / MACMI, PA MACMI / MACM36, PA MACMT / MACM36, PA MACMI / MACM12, PA MACMT / MACM12, PA MACM6 / 11 PA MACM 10 / 10, PA MACM 12 / PACM 12, PA MACM 14 / PACM 14, PA MACM18 / PACM18, and mixtures thereof, wherein PA 6I / 6T, PA MACM12, PA MACM14, PA TMDC12, PA TMDC14, PA MACMI / 12, PA 6I / 6T / MACMI / MACMT, PA MACMI / MACMT / 12, PA MACMI / MACMT / MACM12, PA 6I / 6T / MACMI / MACMT / 12, PA MACM10 / 10, PA MACM12 / PACM12, PA MACM14 / PACM14, PA MACM18 / PACM18, and mixtures thereof.

6. A thermoplastic molding composition according to any one of the preceding claims, characterized in that the at least one polyphenylene ether of component A2 is selected from the group consisting of poly(2,6-dimethyl-1,4-phenylene) ether, poly(2,6-diethyl-1,4-phenylene) ether, poly(2-methyl-6-ethyl-1,4-phenylene) ether, poly(2-methyl-6-propyl-1,4-phenylene) ether, poly(2,6-dipropyl-1,4-phenylene) ether, poly(2-ethyl-6-propyl-1,4-phenylene) ether or copolymers or mixtures thereof.

7. A thermoplastic molding composition according to any one of the preceding claims, characterized in that component A3 is selected as a compatibilizer; or a mixture of a compatibilizer and a free radical initiator; and / or a compatibilizer selected from the group consisting of maleic acid, maleic anhydride, fumaric acid, acrylic acid, methacrylic acid, methylmaleic acid, methylmaleic anhydride, itaconic acid, itaconic anhydride, butenylsuccinic acid, butenylsuccinic anhydride, tetrahydrophthalic acid, tetrahydrophthalic anhydride N-phenylmaleimide, citric acid, malic acid and 2-hydroxynonadecane-1,2,3-tricarboxylic acid, the mono- or diesters of the acids mentioned with C1- to C12-alcohols such as methanol or ethanol, the mono- or diamides of the acids mentioned, which may be substituted on the nitrogen with alkyl or aryl radicals having up to 12 carbon atoms, the salts with alkali or alkaline earth metals such as calcium and potassium and mixtures thereof; and / or a radical initiator selected from the group consisting of 1,1-di-tert-butyl-peroxy-3,3,5-trimethylcyclohexane, tert-butyl-peroxy-isopropyl-carbonate, tert-butyl-peroxy-3,3,5-trimethylhexoate, tert-butyl-peracetate, tert-butyl perbenzoate, 4,4-di-tert-butyl peroxy-valeric acid n-butyl ester, 2,2-di-tert-butyl peroxy-butane, dicumyl peroxide, tert-butyl cumyl peroxide, 1,3-bis(tert-butyl peroxyisopropyl) benzene, di-tert-butyl peroxide and mixtures thereof.

8. A thermoplastic molding composition according to any one of the preceding claims, characterized in that the olefinic and / or vinylaromatic polymers A4 are selected from the group consisting of: styrene-ethylene-butylene-styrene block copolymers, styrene-ethylene-propylene-styrene block copolymers, styrene-butadiene-styrene block copolymers, styrene-styrene-butadiene-styrene block copolymers, polyethylene, polypropylene, polybutadiene, poly-4-methylpentene, ethylene-propylene copolymers, ethylene-butene copolymer, ethylene-methylhexadiene copolymers, propylene-methylhexadiene copolymers, ethylene-octene copolymer, ethylene-propylene-butene copolymers, ethylene-propylene-hexene copolymers, ethylene-propylene-methylhexadiene copolymers, poly(ethylene-vinyl acetate), ethylene-ethyl acrylate copolymer, ethylene-hexene copolymer, ethylene-propylene-diene terpolymers, and mixtures of these polymer materials; and / or are grafted with carboxylic acid or carboxylic acid anhydride groups; and / or are grafted with acrylic acid, methacrylic acid or maleic anhydride, the degree of grafting being 0.1 to 4.0, preferably 0.4 to 2.5 and particularly preferably 0.5 to 2.0 percent by weight, based on the grafted polymer A4.

9. A thermoplastic molding composition according to one of the preceding claims, <b>characterized in that, that component C contains or is entirely formed by at least one LDS additive based on the copper and / or tin selected from the following group: metal oxide, metal phosphate, preferably basic metal phosphate and / or metal hydroxide phosphate, preferably component (C) contains or is entirely formed by at least one LDS additive selected from the following group: Tin oxide; metal or metal oxide doped tin oxide; antimony doped tin oxide; metal oxide coated mica; antimony doped tin oxide coated mica; mixture of tin oxide and antimony oxide and optionally other metal oxides; spinels; copper chromium oxide; copper tungstate, copper oxide; copper hydroxide; copper hydroxide phosphate; copper phosphate; basic copper phosphates; copper-tin phosphate; basic copper-tin phosphate; tin phosphate; basic tin phosphate; antimony-doped tin oxide, preferably in combination with mica; or mixtures and combinations thereof.

10. A thermoplastic molding composition according to any one of the preceding claims, characterized in that the LDS additive of component C is selected from the group consisting of copper chromium oxide, copper tungstate, copper oxide, copper hydroxide phosphate, tin hydroxide phosphate, tin phosphate, copper phosphate, basic copper phosphates and tin phosphates, or mixtures thereof; or as copper tungstate.

11. A thermoplastic molding composition according to any one of the preceding claims, characterized in that the additives of components D are selected from the group consisting of stabilizers, anti-aging agents, antioxidants, antiozonants, processing stabilizers, processing aids, viscosity modifier, light stabilizers, UV stabilizers, UV absorbers, inorganic heat stabilizers, in particular based on copper halides and alkali halides, organic heat stabilizers, optical brighteners, crystallization accelerators, crystallization retarders, flow aids, lubricants, slip agents, mold release agents, coloring agents, in particular dyes, inorganic pigments, organic pigments, marking agents and mixtures thereof.

12. A thermoplastic molding composition according to one of the preceding claims, characterized in that the proportion of component A is present in a range from 34 to 82.9% by weight, preferably from 39 to 78.8% by weight, based on the sum of components A to D; and / or component B is present in a range from 15 to 55% by weight, preferably from 18 to 52% by weight, based on the sum of components A to D; and / or component C is present in the range from 2 to 6% by weight, preferably in the range from 3 to 5% by weight, based on the sum of components A to D; and / or component D is present in the range from 0.1 to 5% by weight, preferably from 0.2 to 4% by weight, based on the sum of components A to D.

13. A molded article comprising a molding composition according to any one of claims 1 to 12, or preferably consisting of said molding composition.

14. A molded article according to claim 13, characterized in that the molded article is selected from components, housings or housing parts of devices communicating with electromagnetic waves having a frequency of 0.3 to 300 GHz.

15. A molded article according to claim 14, characterized in that the article is selected from the group consisting of components, housings or housing parts of transmitting and receiving devices, cell phones, tablets, laptops, navigation devices, surveillance cameras, photo cameras, sensors, diving computers, audio systems, remote controls, loudspeakers, headphones, radio sets, television sets, household appliances, kitchen appliances, door or gate openers, operating devices for the central locking system in vehicles, keyless-go vehicle keys, temperature measuring or temperature indicating devices, measuring devices and control devices.