FIRE-RESISTANT COPOLYMERS AND MOLDING MATERIALS
Patent Information
- Application Number
- DE502021005474
- Authority / Receiving Office
- DE · DE
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-12-17
- Filing Date
- 2021-12-17
- Publication Date
- 2024-10-31
- Estimated Expiration
- 2041-12-17
AI Technical Summary
Current flame-retardant materials for polystyrene, particularly those with high sulfur content, are ineffective due to their strong odor, yellow color, and limited flame retardancy, and often require additional additives, which can be harmful and environmentally persistent.
Development of copolymers and molding materials with covalently bound phosphorus and low sulfur content, which are inherently flame-retardant, odorless, and colorless, eliminating the need for additional flame retardant additives and avoiding harmful substances like antimony trioxide.
These materials exhibit excellent intrinsic flame retardancy, are environmentally compatible, and can be used in various applications without the drawbacks of traditional sulfur-based flame retardants, such as unpleasant odors and colors, while maintaining mechanical properties and thermal insulation.
Description
[0001] The present invention relates to flame-retardant styrene-based copolymers and molding materials and / or compositions with reactively bonded sulfur and a low sulfur content. Phosphorus compounds are also covalently bonded to these copolymers and molding compositions. The copolymers and molding compositions are characterized by being essentially colorless, odorless, and free of migrating flame-retardant additives. Furthermore, they are free of potentially carcinogenic antimony trioxide (ATO). The copolymers and molding compositions according to the invention exhibit very pronounced intrinsic flame retardancy and can therefore be used in the transportation / automotive, construction, and electrical and electronics industries.
[0002] The treatment of styrene homopolymers and copolymers with flame retardant additives is important for a wide range of applications, for example for polystyrene particle foams made of expandable polystyrene (EPS) or polystyrene extrusion foam boards (XPS) for insulating buildings, as well as for injection-molded parts made of HIPS, ABS, ASA, etc. for use as parts and components for consumer goods in the electrical and electronics sector.
[0003] Polymers composed of styrene monomers account for a total production volume of approximately 10% by weight of total global plastics production, making them the fourth largest group of the twenty plastics produced worldwide. Homopolystyrene (PS) is predominantly used as a packaging material in food packaging and disposable consumer goods. It is also used as particle foam or extruded foam in packaging and thermal insulation.
[0004] Polystyrene itself is highly flammable in the event of a fire and lacks flame-retardant properties. In fact, pure polystyrene bodies burn completely under most fire conditions and lack flame-retardant properties. Furthermore, heavy soot and smoke gases are produced in the event of a fire. Flame-retardant properties of the polymer can only be achieved through the addition of suitable flame-retardant additives. Due to the large surface area, intumescent and crust-forming flame-retardant systems are typically not sufficiently effective for foam applications. For this purpose, gas-phase active flame retardants such as brominated flame-retardant additives with suitable synergists (e.g., the thermal radical formers dicumyl peroxide, di-tert-butyl peroxide, or dicumyl) must be used, as described in WO 2006 / 082233 A1.Halogen-containing flame retardants are typically persistent in the environment and release corrosive gases such as hydrogen chloride or hydrogen bromide in the event of a fire. If these flame retardants are also low molecular weight, they are mobile within the plastic and tend to migrate out of it, accumulating in the environment and in living organisms.
[0005] WO 2007 / 058736 A1 describes that, due to its persistent, bioaccumulative, and toxic properties, hexabromocyclododecane, previously used in polystyrene foams, can be replaced with a polymeric and polybrominated flame retardant. Another alternative to the previously described flame-retardant polystyrene polymers is blending polystyrene with other, less flammable polymers. For example, WO 2013 / 028344 A1 describes that polystyrene can be blended with a halogenated polyphenylene ether (PPE) to achieve the necessary flame retardancy.
[0006] To adjust the mechanical properties of styrene polymers, styrene can be copolymerized with a wide variety of comonomers. Depending on the comonomers used, the products are the copolymers poly(acrylonitrile-butadiene-styrene) (ABS), poly(styrene-butadiene-styrene) (SBS), poly(styrene-acrylonitrile) (SAN), poly(acrylonitrile-styrene-acrylate) (ASA), poly(styrene-butadiene) rubber (SBR), high-impact polystyrene (HIPS), polystyrene acrylates such as polystyrene methyl acrylate (SMA) and polystyrene methyl methacrylate (SMMA), methyl acrylate-butadiene-styrene copolymer (MBS), methyl methacrylate-acrylonitrile-butadiene-styrene polymers (MABS), styrene-N-phenyl-maleimide copolymers (SPMI), and others.
[0007] The literature describes sulfur-containing flame retardant additives with high sulfur content (> 30%), which are used as flame retardant synergists for phosphorus-containing flame retardants in polystyrene foams. This is the case, for example, in the publications WO 2011 / 121001 A1 and WO 2012 / 089667 A1. However, these high-sulfur compounds are typically characterized by an intense odor and a strong, yellow to reddish-brown color, which limits or even prevents their use in many, particularly uncolored, plastics applications. Furthermore, the described flame retardant additives do not achieve sufficient flame retardancy in polystyrene foams when used alone and without other flame retardants. Furthermore, the publications only describe their use as an additive; the flammability of the pure materials is not mentioned.
[0008] Elemental sulfur as an additive flame retardant in homopolystyrene is also described in WO 2011 / 095540 A2, but its effectiveness is only achieved in combination with a phosphorus-containing flame retardant. Sulfur, when added individually as a flame retardant additive to polystyrene foams, remains virtually ineffective in terms of flame retardancy. Furthermore, the addition of elemental sulfur to the final product typically results in a pronounced yellowing, which is undesirable in many applications. Elemental sulfur also leads to the development of more or less pronounced sulfur odors during polymer processing and in the final product.
[0009] WO 2017 / 004186 A1 describes for the first time the flame-retardant effect of high-sulfur thermosets. These are said to be suitable for use as additives in polyurethane foams and as thermoset materials. However, these sulfur copolymers have a high sulfur content of at least 40 wt.%. Due to the high sulfur content and the associated unpleasant odor that high-sulfur materials typically emit due to their at least partially sulfidic structure, the use of these thermosets in many plastics applications is severely limited.
[0010] Furthermore, thermosetting materials cannot be used in typical applications for expanded polystyrene, as their foamability is either completely impossible or at least severely limited. The functionality of the material described in WO 2017 / 004186 A1 is based on the formation of a stable crust and on intumescence (foaming and bonding). For materials such as foamed polymers, which are characterized by a very large surface area relative to their mass, such flame retardant mechanisms do not provide sufficient protection to pass standardized fire tests. Test results regarding the fire behavior of these polymers are therefore also missing from WO 2017 / 004186 A1.
[0011] Furthermore, the publication by Ahmed Aziz et al.: "Copolymerisation of elemental sulfur with styrene", in Journal of Applied Polymer Science, Vol. 29, No. 4, of April 1, 1984, pages 1225-1239, describes the preparation of copolymers starting from the monomers styrene and sulfur, wherein the mass fraction of sulfur is less than 40%.
[0012] The working examples in EP 0509304 A1 also describe the preparation of copolymers starting from phosphate- and triazine-containing monomers, which, however, do not contain any sulfur.
[0013] WO 2011 / 095540 A2 describes fire-retardant molding compounds and processes for their production and their use.
[0014] Finally, WO 2011 / 121485 A1 describes sulfur-containing copolymers which, in contrast to the present copolymers, are composed of other monomer units and comprise other partial structures which have been subsequently published.
[0015] The object of the present invention is therefore to generate copolymers and / or molded materials, for example as semi-finished products or as components of cladding, insulating materials, which have a flame-retardant or fire-retardant property in combination with covalently bound, organic-phosphorus-containing comonomers and a low content of covalently bound sulfur, without the mandatory addition of further flame-retardant additives in order to achieve a sufficient fire-retardant effect.
[0016] This object is achieved according to the invention by the features of independent claims 1 and 5.
[0017] Due to the covalent bonding of the flame-retardant groups, the copolymers of the invention exhibit no leaching, no odor, and no inherent color, while simultaneously exhibiting very good intrinsic flame-retardant properties. They are also free of potentially carcinogenic antimony trioxide and can be produced cost-effectively using commercially available starting materials.
[0018] By copolymerizing styrene and its derivatives with additional phosphorus-containing monomers in the presence of small amounts of sulfur, novel thermoplastic copolymers and / or molding compounds have been discovered. These copolymers and / or molding materials or compounds, in addition to the covalently bound phosphorus, also contain an extremely low proportion of bound sulfur while simultaneously exhibiting intrinsic flame-retardant properties.
[0019] When preparing the present copolymers, a random distribution of the repeating units from the monomers used must be assumed. The number of repeating units "n" specified for a normal polymer chain is only partially applicable in this case, since the monomer units within the polymer chain do not follow a regular sequence. For this reason, the specification of a repeating unit "n" has been omitted in the following formulas 1 - 24. In the present case, it would therefore also be possible to define repeating units in the following formulas that can be in the range of n = 2 - 100,000. Nevertheless, the square brackets indicate a repeating sequence of the possible repeating units in accordance with the usual polymer chain representation according to the state of the art.Therefore, the notation "n" could be added to the square brackets in the following formulas (1) to (24), but this has been omitted for the reasons stated above. The representation of the copolymer composition of different monomers with " / " is chosen according to the IUPAC recommendation.
[0020] The copolymers formed according to formulas (6) to (15) and (17) to (24) according to the invention and / or molding compositions formed therefrom are flame-retardant and / or self-extinguishing and essentially colorless and / or odorless. Essentially colorless, as defined in the application, means the absence of any visible coloration. These correspond to the perceived RAL color types, including, by way of example but not exhaustively, RAL 1013 Pearl White, RAL 9001 Cream White, RAL 9003 Signal White, RAL 9010 Pure White, and / or RAL 9016 Traffic White.
[0021] Odourless in relation to the copolymers and moulding compounds can be understood as the olfactory perception of sulphidic compounds of less than 50 µg / m 3< air, or less than 5 µg / m 3< air (for example hydrogen sulphide, dimethyl sulphide, methyl mercaptan), or less than 0.5 µg / m 3< air (for example thiophenol, thiocresol, diphenyl sulphide, propyl mercaptan, ethyl mercaptan, crotyl mercaptan, amyl mercaptan, benzyl mercaptan, amyl mercaptan, allyl mercaptan), whereby the sulphidic compounds have a different odour threshold depending on their chemical structure and can be perceived differently by each individual.
[0022] Furthermore, the intrinsically flame-retardant copolymers are characterized by the fact that the phosphorus- or sulfur-containing groups are covalently bonded to the copolymer and cannot migrate from it.
[0023] A copolymer formed according to the invention from formulas (6) to (15) and (17) to (24) can form an individual component of a molding compound or be a co-component of a molding compound. By definition, the term molding compound refers to copolymer-containing workpieces that form a molding material for the production of molded articles, semi-finished products, or finished parts. By applying mechanical force and / or elevated temperatures of ≤ 250°C, the molding compound is processed into semi-finished products or finished parts using a processing method such as extrusion, compression molding, transfer molding, or injection molding in tools, followed by cooling.
[0024] For the purposes of this application, a semi-finished product is considered to be a prefabricated raw material or material or semi-finished product of the simplest form, which can generally consist of a single material or a single compound, such as a single copolymer according to the invention, but does not have to consist of only a single material or a single compound, such as a single copolymer according to the invention. Thus, it is possible for at least one copolymer according to the invention to form a workpiece or semi-finished product with at least one further copolymer and / or another polymer and / or another material, such as metal (e.g., aluminum and / or iron) and / or plastic (e.g., polyurethane and / or polycarbonate) and / or ceramics (e.g., kaolin and / or silicates and / or clay materials) and / or prepregs, BMC, or SMC.The molding compound or material can consist of a copolymer according to the invention and / or at least one further polymer and / or an additional copolymer according to the invention. The molding compound, the molding material or the molded body can also comprise a copolymer according to the invention and / or a further polymer and / or an additional copolymer according to the invention and / or another material such as metal (e.g. aluminum and / or iron) or plastic (e.g. polyurethane and / or polycarbonate) or ceramic (kaolin and / or silicates and / or clay materials) together for a semi-finished product. It is also possible for the molding compound, the molding material or the molded body to partially or completely surround the material or the workpiece as a coating or for the material or the workpiece to be embedded in the molding compound, the molding material or the molded body.
[0025] Semi-finished products include simple profiles, structural profiles, rods, tubes, and plates. Molded materials that have already been given an individual shape in a preparatory production step but are still intended for further production steps are further processed in a second step, for example, by forming in the next step, either into a finished part or initially into another semi-finished or finished product.
[0026] In this way, the semi-finished products are transformed into finished components, finished building elements (e.g. construction profiles, bricks or insulation materials) or finished building blocks.
[0027] The material and surface qualities are often optimized for specific applications and manufacturing processes. By way of example, but not exclusively, the copolymers formed according to the invention from formulas (6) to (15) and (17) to (24) can be individual components or co-components of a molding compound or molding material used as semi-finished products, for example, in the construction industry as insulating materials. The molding compound or molding material can thus contain a single copolymer or other polymers and / or copolymers and / or aggregates and / or additives, the properties of which are tailored to the desired application, such as in house or plant construction or automotive engineering.It is therefore possible for the molding materials or compounds to contain additional additives such as flame retardants such as melamine, melamine polyphosphate, melamine cyanurate, metal oxides, metal hydroxides, cyclotriphosphazenes, phosphates, phosphinates, phosphine oxides, hyphosphosphites, or expandable graphite. Suitable additives include additional halogen-free flame retardants such as Aflammit PCO 900, Exolit OP 930, Exolit OP 1312, DOPO, HCA-HQ, Cyagard RF-1241, Cyagard RF-1243, Fyrol PMP, Phoslite B85AX, Melapur 200, Melapur MC, and Budit 669.
[0028] In this context, compounds such as 2,4,8,10-tetraoxa-3,9-diphosphaspiro [5.5] undecane-3,9-dimethyl-3,9-dioxide (0.1 - 10 wt.%) or hexakisphenoxycyclotriphosphazene (0.5 - 20 wt.%) should also be mentioned as additives.
[0029] In the context of the present invention, the fire-retardant and / or self-extinguishing copolymers or the molding compounds or molding materials or semi-finished products have an optionally odor-neutral and / or color-neutral design.
[0030] A copolymer or a molding material formed from a molding compound has at least a flame-retardant or fire-retardant effect upon contact with a flame, or, depending on the substituents, is also self-extinguishing. The copolymers and / or molding compounds according to the invention are free of antimony trioxide and can be obtained free of halogen-containing components.
[0031] Compounds comprising copolymers or molding materials with a random monomer distribution of formulas (6) to (15) and (17) to (24) were found, with a statistical monomer distribution of monomer units with the mass fraction ω where ω(Sty) and ω(S) are 1. The sum of the mass fractions ω(Sty) and ω(S) is 1.
[0032] Furthermore, according to the invention, compounds comprising copolymers with a random monomer distribution of formulas (6) to (15) and (17) to (24) were found with a statistical monomer distribution of monomer units with the mass fraction ω with ω(Sty), ω(P), and ω(3), where ω(3) and ω(P) correspond to the mass fraction of the sulfur-containing and potentially phosphorus-containing repeating unit. The sum of the mass fractions in a copolymer with formulas (6) to (24) are each monomer units with the mass fractions ω with ω(Sty), ω(P), and ω(3) = 1.
[0033] The above applies to the following compounds of formula (6). In the structural formulas of the copolymers presented here, the indices "n" in the square brackets have also been omitted for the reasons described above. In the present case, it would therefore also be possible to define repeating units in the following formulas that can range from n = 3 to 100,000. Due to the random monomer distribution, the indication of "n" in the repeating units in formulas (6) to (24) has been omitted.
[0034] The copolymers of the invention are flame-retardant and / or self-extinguishing, either individually or as components of molding materials or compounds. Flame-retardant means that, after initial ignition, a copolymer or a molding material or compound comprising copolymers exhibits shorter afterburning times compared to homostyrene. Self-extinguishing means that an ignited copolymer or a molding material or compound extinguishes within five seconds after a burner flame is removed from the copolymer or the molding material or compound. These molding compounds can be obtained by physical blending with other polymers and copolymers in any desired ratio.
[0035] The copolymers and molding materials or compositions according to the invention do not have any halogen-containing substituents and are therefore halogen-free, which means they are environmentally friendly during production, use, disposal and in the event of fire.
[0036] Furthermore, fire-retardant molding materials or compounds for extrusion (or for pressing, casting or foaming) were found which comprise at least one fire-retardant copolymer with a sulfur content of less than 5%.
[0037] Due to the thermoplastic properties of the copolymers and / or molding compounds, a wide variety of applications can be served through a wide range of molding processes. Since foam bodies can also be produced from the copolymers and / or molding compounds, these can be used, for example, as thermal insulation materials.
[0038] The foams produced from the fire-retardant copolymers preferably have a density in the range from 5 to 200 kg / m 3< , particularly preferably in the range from 10 to 100 kg / m 3< and are preferably present in the foams to an extent of more than 80%, particularly preferably from 95 to 100%.
[0039] The polymer matrix of the fire-retardant copolymers, copolymer foams, or molding materials preferably consists of thermoplastic (co)polymers or polymer blends, especially styrene (co)polymers. The fire-retardant and expandable styrene (co)polymers (EPS) and styrene (co)polymer extrusion foams (XPS) according to the invention can be processed by mixing a blowing agent in the form of a low-boiling organic solvent such as n-hexane or pentane into the polymer melt and subsequent extrusion and granulation under pressure to form expandable granules (EPS), or by extrusion and relaxation using appropriately shaped dies to form foam sheets (XPS) or foam strands.
[0040] Expandable styrene (co)polymers (EPS) are understood to mean styrene (co)polymers containing a blowing agent. The EPS particle size is preferably in the range of 0.2 - 2 mm. Styrene (co)polymer foams are obtainable by prefoaming and sintering the corresponding expandable styrene (co)polymers (EPS). The styrene (co)polymer foams preferably have 2 to 15 cells per millimeter. A further polymer, in particular a styrene polymer, can be admixed to the copolymers according to the invention or to the copolymer-containing molding compositions according to the invention, e.g.Homopolystyrene, crystal-clear polystyrene (GPPS), impact-modified polystyrene (HIPS), styrene-methylstyrene copolymers, acrylonitrile-butadiene-styrene polymers (ABS), poly(styrene-butadiene-styrene) (SBS), styrene-acrylonitrile polymer (SAN), poly(styrene-butadiene) rubber (SBR), poly(acrylonitrile-styrene-acrylic ester) (ASA), polystyrene acrylates such as polystyrene methyl acrylate (SMA) and polystyrene methyl methacrylate (SMMA), methyl acrylate-butadiene-styrene copolymer (MBS), methyl methacrylate-acrylonitrile-butadiene-styrene polymers (MABS), styrene-N-phenylmaleimide copolymers (SPMI) or mixtures thereof or mixtures of the above-mentioned styrene (co)polymers with polyolefins such as polyethylene or polypropylene and polyphenylene ether (PPE).
[0041] Furthermore, a further polymer is also understood to mean a copolymer of styrene and / or phosphorus-containing comonomers, for example copolymers of styrene with at least one of the monomers of the formulae (25) to (38).
[0042] The molding compounds described are essentially colorless and / or odorless.
[0043] For the purposes of the application, "essentially colorless" means the absence of any visible coloration. These correspond to the perceived RAL color types, including, but not limited to, RAL 1013 Pearl White, RAL 9001 Cream White, RAL 9003 Signal White, RAL 9010 Pure White, and / or RAL 9016 Traffic White.
[0044] Odourless can be understood as the olfactory perception of sulphidic compounds of less than 50 µg / m 3< air, preferably less than 5 µg / m 3< air (for example hydrogen sulphide, dimethyl sulphide, methyl mercaptan), particularly preferably less than 0.5 µg / m 3< (for example thiophenol, thiocresol, diphenyl sulphide, propyl mercaptan, ethyl mercaptan, crotyl mercaptan, amyl mercaptan, benzyl mercaptan, amyl mercaptan, allyl mercaptan) air, whereby the sulphidic compounds have a different odour threshold depending on their chemical structure and can typically be perceived personally individually.
[0045] To improve their mechanical properties or temperature resistance, the styrene (co)polymers according to the invention can be admixed, optionally with the use of compatibilizers, with another polymer as a thermoplastic polymer, such as homopolystyrene (PS), polyamides (PA), polyolefins such as polypropylene (PP) or polyethylene (PE), polyacrylates such as polymethyl methacrylate (PMMA), polycarbonate (PC), polyesters such as polyethylene terephthalate (PET) or polybutylene terephthalate (PBT), polyethersulfones (PES), polyether ketones, or polyether sulfides (PES). Furthermore, blends with other polymers in the stated quantity ranges are also possible, for example with hydrophobically modified or functionalized polymers or oligomers, rubbers such as polyacrylates, or polydienes such as styrene-butadiene block copolymers, or biodegradable, aliphatic, or aliphatic / aromatic copolyesters.
[0046] Suitable compatibilizers include styrene copolymers modified with maleic anhydride, polymers containing epoxy groups, or organosilanes.
[0047] In the manufacturing process, polymer recyclates of the aforementioned thermoplastic polymers, in particular styrene (co)polymers and expandable styrene (co)polymers (EPS) can also be added to the styrene copolymers in amounts of up to 50 wt.%, in particular in amounts of 1 to 20 wt.%, without the flame-retardant or self-extinguishing properties of the copolymers and / or molding compounds being significantly changed.
[0048] For high-temperature-resistant copolymers and / or molding materials and / or foams, blends of SMA and SAN or SAN and SPMI are preferred. The proportion is selected according to the desired heat resistance. The acrylonitrile content in SAN is preferably 25 to 33 wt.%. The methacrylate content in SMA is preferably 25 to 30 wt.%.
[0049] The styrene (co)polymers or molding materials may contain auxiliaries and additives, for example flame retardants, fillers, nucleating agents, UV stabilizers, chain transfer agents, blowing agents, plasticizers, antioxidants, soluble and insoluble inorganic and / or organic dyes and pigments, e.g., infrared (IR) absorbers such as carbon black, graphite, or aluminum powder. The dyes and pigments are generally added in amounts ranging from 0.01 to 30 wt.%, preferably from 1 to 5 wt.%. For homogeneous and microdisperse distribution of the pigments in the styrene copolymer, it may be advantageous, particularly in the case of polar pigments, to use a dispersing agent such as organosilanes, epoxy-containing polymers, or maleic anhydride-grafted styrene polymers. Preferred plasticizers are mineral oils and phthalates, which can be used in amounts of 0.05 to 10 wt.% based on the styrene (co)polymer.
[0050] The amount of IR absorbers used depends on their type and effect. The styrene (co)polymer particle foams preferably contain 0.5 to 5 wt.%, particularly preferably 1 to 4 wt.% IR absorbers. Graphite, carbon black, or aluminum with an average particle size in the range of 1 to 50 µm are preferred as IR absorbers.
[0051] The preferred graphite has an average particle size of 1 to 50 µm, particularly 2.5 µm to 12 µm, a bulk density of 100 to 500 kg / m 3 , and a specific surface area of 5 to 20 m 2 / g. Natural graphite or ground synthetic graphite can be used. The graphite particles are preferably present in the styrene (co)polymer in amounts of 0.05 to 8 wt.%, particularly 0.1 to 5 wt.%.
[0052] The particularly preferred expandable styrene (co)polymers (EPS) or molding materials can be produced using different processes.
[0053] In one embodiment, athermanous particles and a nonionic surfactant are mixed with a melt of the styrene (co)polymer or molding material, preferably in an extruder. At the same time, the blowing agent is metered into the melt. Athermanous particles are defined as particles that are impermeable to infrared radiation (heat radiation).
[0054] The athermanous particles can also be incorporated into a melt of a blowing agent-containing styrene (co)polymer or molding material, using sieved edge fractions from a bead spectrum of blowing agent-containing polystyrene beads produced during suspension polymerization. The styrene (co)polymer melts or molding material polymer melts containing blowing agent and the athermanous particles are extruded and comminuted into blowing agent-containing granules. Since the athermanous particles can have a strong nucleating effect, rapid cooling under pressure is recommended after extrusion to prevent foaming. Therefore, underwater granulation under pressure in a closed system is advantageously carried out.
[0055] It is also possible to add a blowing agent to the styrene (co)polymers or molding materials containing the athermanous particles in a separate process step. The granules are then impregnated with the blowing agent, preferably in an aqueous suspension.
[0056] In all three cases, the finely divided, athermanous particles and the nonionic surfactant can be added directly to a styrene (co)polymer melt or molding material melt. The athermanous particles can also be added to the melt in the form of a concentrate in polystyrene. Preferably, however, the styrene (co)polymer granules and athermanous particles are fed together into an extruder, where the styrene (co)polymer is melted and mixed with the athermanous particles.
[0057] The expandable styrene (co)polymers (EPS) are particularly preferably produced by polymerizing styrene and, optionally, the copolymerizable monomers of the copolymers according to the invention in aqueous suspension and impregnating them with a blowing agent, wherein the polymerization is carried out in the presence of 0.1 to 5 wt. % graphite particles, based on the styrene (co)polymer, and a nonionic surfactant. Suitable nonionic surfactants include, for example, maleic anhydride copolymers (MA), e.g., of maleic anhydride and C(20)- to C(24)-olefin, polyisobutylene succinic anhydride (PIBSA), or their reaction products with hydroxypolyethylene glycol ester, diethylaminoethanol, or amines such as tridecylamine, octylamine, or polyetheramine, tetraethylenepentamine, or mixtures thereof. The molecular weights of the nonionic surfactant are preferably in the range from 500 to 3000 g / mol. They are usually used in amounts ranging from 0.01 to 2 wt.% based on the styrene (co)polymer.
[0058] The expandable styrene (co)polymers or molding materials containing athermanous particles can be processed into styrene (co)polymer foams with densities of 5 - 200 kg / m 3< , preferably of 7 to 100 kg / m 3< and in particular of 10 - 80 kg / m 3< .
[0059] For this purpose, the expandable particles are pre-foamed. This is usually done by heating the particles with steam in so-called pre-expanders. The pre-foamed particles are then welded into molded bodies. For this purpose, the pre-foamed particles are placed in non-gas-tight molds and exposed to steam. After cooling, the molded parts can be removed.
[0060] The foams produced from the inventive expandable copolymers or molding materials are characterized by excellent thermal insulation. This effect is particularly evident at low densities.
[0061] The foams or molded materials can be used for thermal insulation of buildings and building components, for thermal insulation of machines and household appliances, and as packaging materials.
[0062] To produce the expandable copolymers, the blowing agent can be mixed into the polymer melt. One possible process comprises the steps a) melt generation, b) mixing, c) cooling, d) conveying, and e) granulation. Each of these steps can be carried out using equipment or equipment combinations commonly used in plastics processing. Static or dynamic mixers, such as extruders, are suitable for mixing. The polymer melt can be taken directly from a polymerization reactor or produced directly in the mixing extruder or a separate melting extruder by melting polymer granules. The melt can be cooled in the mixing units or in separate coolers. Examples of suitable granulation methods include pressurized underwater granulation, granulation with rotating knives, and cooling by spraying atomized heat-control liquids or atomization granulation.Apparatus arrangements suitable for carrying out the process include: . a) Polymerization reactor - static mixer / cooler - granulator b) Polymerization reactor - extruder - granulator c) Extruder - static mixer - granulator d) Extruder - granulator
[0063] The blowing agent-containing copolymer melt is typically conveyed through the die plate at a temperature in the range of 140 to 300 °C, preferably in the range of 160 to 240 °C. Cooling to the glass transition temperature is not necessary.
[0064] The die plate is heated to at least the temperature of the blowing agent-containing copolymer melt. The die plate temperature is preferably in the range of 20 to 100 °C above the temperature of the blowing agent-containing copolymer melt. This prevents polymer deposits in the dies and ensures trouble-free pelletizing.
[0065] In order to obtain marketable granulate sizes, the diameter (D) of the nozzle bores at the nozzle outlet should be in the range of 0.2 to 1.5 mm, preferably in the range of 0.3 to 1.2 mm, particularly preferably in the range of 0.3 to 0.8 mm 10. This allows granulate sizes below 2 mm, especially in the range of 0.4 to 1.4 mm, to be specifically adjusted even after strand expansion.
[0066] Particularly preferred is a process for producing flame-retardant, expandable copolymers (EPS), which comprises the following steps: a) mixing an organic blowing agent into the polymer melt of the copolymers according to the invention and / or blends thereof by means of static or dynamic mixers at a temperature of at least 150°C, b) cooling the blowing agent-copolymer melt to a temperature range of 120 to 200°C, c) discharging through a nozzle plate with bores whose diameter at the nozzle outlet is at most 1.5 mm and d) granulating the blowing agent-containing melt directly behind the nozzle plate under water at a pressure in the range of 1 to 20 bar.
[0067] It is also possible to produce the copolymers and / or molding compositions according to the invention by suspension polymerization. In suspension polymerization, styrene, phosphorus-containing copolymers, and sulfur are preferred as monomers. However, up to 50% of the weight of the copolymers can be replaced by other ethylenically unsaturated monomers.
[0068] During suspension polymerization, conventional auxiliaries such as peroxide initiators, suspension stabilizers, blowing agents, chain transfer agents, expansion aids, nucleating agents, and plasticizers can be added. Blowing agents are added in amounts of 3 to 10 wt.%, based on the monomer(s). They can be added to the suspension before, during, or after polymerization. Suitable blowing agents are aliphatic hydrocarbons with 4 to 6 carbon atoms. It is advantageous to use inorganic Pickering dispersants such as magnesium pyrophosphate or calcium phosphate as suspension stabilizers.
[0069] Suspension polymerization produces bead-shaped, essentially round particles with an average diameter in the range of 0.2 to 2 mm. To improve processability, the finished, expandable copolymer beads and granules can be coated with conventional and well-known coating agents such as metal stearates, glycerol esters, and finely divided silicates, antistatic agents, or anti-sticking agents.
[0070] The EPS granules can be coated with glycerol monostearate (GMS, typically 0.25 wt%), glycerol tristearate (typically 0.25 wt%), finely divided silica (Aerosil R972, typically 0.12 wt%) and zinc stearate (typically 0.15 wt%) as well as antistatic agent.
[0071] The expandable copolymer particles can be processed into polystyrene foams with densities of 8 to 200 kg / m³, preferably 10 to 100 kg / m³. For this purpose, the expandable particles are pre-expanded. This is usually done by heating the particles with steam in so-called pre-expanders. The pre-expanded particles are then welded to form molded articles, semi-finished products, or molded articles. For this purpose, the pre-expanded particles are placed in non-gas-tight molds and exposed to steam. After cooling, the molded parts can be removed. Examples Synthesis of the monomers: Monomer (25): Hexakisallyloxy-cyclotriphosphazene
[0072]
[0073] Synthesized according to M. Dutkiewicz et al., Polymer Degradation and Stability 2018, 148, pages 10 - 18. Monomer (26): Diethyl-2-methacryloyloxy-ethyl phosphate
[0074] 2-Hydroxyethyl methacrylate (929 mg, 7.12 mmol), distilled triethylamine (741 mg, 7.32 mmol), and copper(I) chloride (11.38 mg, 0.11 mmol) were mixed in approximately 10 mL of peroxide-free diethyl ether, deoxygenated, and cooled in an ice bath. Diethyl chlorophosphate (1474 mg, 8.54 mmol) dissolved in 4 mL of diethyl ether was added dropwise. The mixture was stirred for 1 hour in an ice bath and for 48 h at room temperature, then filtered and the solvent evaporated.
[0075] 1< H-NMR (500 MHz, CDCl 3 ): 1.30 ppm (6 protons, -PO-CH 2 -CH 3 ), 1.93 (3 protons, -CH 3 acrylate), 4.10 (4 protons, -PO-CH 2 -CH 3 ), 4.26 and 4.35 (2 protons each, -O-CH 2 -CH 2 -O-), 5.59 and 6.14 (1 proton each, CH 2 =C-); Monomer (27): Diphenyl-2-methacryloyloxy-ethyl phosphate
[0076]
[0077] 2-Hydroxyethyl methacrylate (929 mg, 7.12 mmol), distilled triethylamine (741 mg, 7.32 mmol), and copper(I) chloride (11.38 mg, 0.11 mmol) were mixed in approximately 10 ml of peroxide-free diethyl ether, deoxygenated, and cooled in an ice bath. Diphenyl chlorophosphate (1860 mg, 7.12 mmol) dissolved in 4 ml of diethyl ether was added dropwise. The mixture was stirred for 1 hour in an ice bath and for 48 h at room temperature, then filtered and the solvent evaporated.
[0078] 1< H-NMR (500 MHz, CDCl 3 ): 1.91 ppm (3 protons, -CH 3 acrylate), 4.38 and 4.48 (2 protons each, -O-CH 2 -CH 2 -O-), 5.56 and 6.11 (1 proton each, CH 2 =C-), 7.22 and 7.33 (10 protons, aromatics) Monomer (28): Diphenyl-2-acryloyloxy-ethyl phosphate
[0079]
[0080] 2-Hydroxyethyl acrylate (826 mg, 7.12 mmol), distilled triethylamine (741 mg, 7.32 mmol), and copper(I) chloride (11.38 mg, 0.11 mmol) were mixed in approximately 10 ml of peroxide-free diethyl ether, deoxygenated, and cooled in an ice bath. Diphenyl chlorophosphate (1860 mg, 7.12 mmol) dissolved in 4 ml of diethyl ether was added dropwise. The mixture was stirred for 1 hour in an ice bath and for 48 h at room temperature, then filtered and the solvent evaporated.
[0081] 1< H-NMR (500 MHz, CDCl 3 ): 4.38 and 4.48 (2 protons each (-O-CH 2 -CH 2 -O-), 5.85, 6.08 and 6.41 (1 proton each, CH 2 =CH-), 7.23 and 7.34 (6 and 4 protons, aromatics) Monomer (29): Diphenyl methacryloyloxy butyl phosphate
[0082]
[0083] Hydroxybutyl methacrylate (2:1 isomer mixture) (1125 mg, 7.12 mmol), distilled triethylamine (741 mg, 7.32 mmol), and copper(I) chloride (11.38 mg, 0.11 mmol) were mixed in approximately 10 ml of peroxide-free diethyl ether, deoxygenated, and cooled in an ice bath. Diphenyl chlorophosphate (1860 mg, 7.12 mmol) dissolved in 4 ml of diethyl ether was added dropwise. The mixture was stirred for 1 hour in an ice bath and for 48 h at room temperature, then filtered and the solvent evaporated.
[0084] 1H-NMR (500 MHz, CDCl 3 ), δ (ppm): 0.92 / 0.96 (t, 6H, CH 3 ); 1.69 / 1.77 (q, 4H, CH2 ); 1.90 (s, 6H, CH3 ); 4.24 / 4.34 (m, 2H, -O-CH 2 -); 4.80 (d, 2H, CH2 ); 5.06 (q, 2H, CH); 5.52 (s, 1H, CH vinyl trans to carbonyl); 6.10 (s, 1H, CH vinyl cis to carbonyl); 7.20 / 7.32 (aromatic H). Monomer (30): Diphenyl-4-acryloyloxy-butyl phosphate
[0085]
[0086] 4-Hydroxybutyl acrylate (1025 mg, 7.12 mmol), distilled triethylamine (741 mg, 7.32 mmol), and copper(I) chloride (11.38 mg, 0.11 mmol) were mixed in approximately 10 ml of peroxide-free diethyl ether, deoxygenated, and cooled in an ice bath. Diphenyl chlorophosphate (1860 mg, 7.12 mmol) dissolved in 4 ml of diethyl ether was added dropwise. The mixture was stirred for 1 hour in an ice bath and for 48 h at room temperature, then filtered and the solvent evaporated.
[0087] 1< H-NMR (500 MHz, CDCl 3 ): 1.76 ppm (4 protons, -O-CH 2 -(CH 2 ) 2 -CH 2 -O-), 4.16 and 4.30 (2 protons each, -O-CH 2 -(CH 2 ) 2 -CH 2 -O-), 5.83, 6.11 and 6.36 (1 proton each, CH 2 =CH-), 7.22 and 7.33 (6+4 protons, aromatics) Monomer (31): Diethyl p-vinylbenzylphosphonate
[0088]
[0089] Potassium tert-butoxide (4.4 g, 39.3 mmol) was suspended in THF (40 mL, dry) at 0 °C under inert gas before diethyl phosphonate (5.4 g, 39.3 mmol) dissolved in THF (20 mL) was added dropwise. The mixture was stirred for 30 min before being added dropwise to a solution of chloromethylstyrene (3.0 g, 19.7 mmol), TBHQ (2-tert-butylhydroquinone), and TBAI (tetrabutylammonium iodide) in THF (20 mL) at 0 °C. After 18 hours at 20 °C under inert gas, the solids were separated and the solvent distilled off.
[0090] 1< H NMR (CDCl 3 , 500 MHz) δ (ppm): 1.21 (t, 6H, CH 2 -CH 3 ), 3.16 (d, 2H, CH 2 -P), 4.02 (m, 4H, PO-CH 2 ), 5.22 / 5.73 (d, 2H, CH=CH 2 ); 6.68 (dd, 1H, CH=CH 2 ); 7.24 - 7.34 (m, 4H aromatic).
[0091] IR (cm -1< ): 3025 (Ar-H), 2850-2953 (alkyl-H), 1600 (CH 2 =CH-Ar); 1512 (CC, Ar); 1250 (P=O), 1027 (POC); 957 (C=C), 854 (Ar-H). Monomer (32): Diphenyl-2-methacryloyloxy-ethylphosphinate
[0092]
[0093] 2-Hydroxyethyl methacrylate (2.0 g, 15.5 mmol) was stirred together with triethylamine (1.7 g, 16.5 mmol) and copper(I) chloride (0.06 g) in diethyl ether (20 mL) for 1 h at 0 °C under inert gas before diphenylphosphinic chloride (3.7 g, 15.8 mmol) dissolved in diethyl ether (5 mL) was added dropwise. After stirring for 24 h at 20 °C, the triethylammonium chloride was removed and the solvent distilled off.
[0094] 1< H NMR (CDCl 3 , 500 MHz) δ (ppm): 1.92 (s, 3H, α-CH 3 ), 4.25 (t, 2H, CH 2 -OP), 4.40 (t, 2H, O-CH 2 -CH 2 -), 5.58 / 6.05 (s, 2H, C=CH2), 7.42 - 7.78 (m, 10H aroma). Monomer (33): Dimethyl[(4-ethenylphenyl)methyl]phosphonate
[0095]
[0096] Potassium tert-butoxide (5.0 g, 44.1 mmol) was suspended in THF (40 mL, dry) at 0 °C under inert gas before dimethylphosphonate (4.9 g, 44.1 mmol) dissolved in THF (20 mL) was added dropwise. The mixture was stirred for 30 min before being added dropwise to a solution of chloromethylstyrene (3.4 g, 22.1 mmol), TBHQ (2-tert-butylhydroquinone), and TBAI (tetrabutylammonium iodide) in THF (20 mL) at 0 °C. After 18 hours at 20 °C under inert gas, the solids were separated and the solvent was distilled off.
[0097] 1< H NMR (CDCl 3 , 500 MHz) δ (ppm): 3.15 (d, 2H, CH 2 -P), 3.65 (d, 6H, PO-CH 3 ), 5.22 / 5.72 (d, 2H, CH=CH 2 ); 6.66 (dd, 1H, CH=CH 2 ); 7.22 - 7.34 (m, 4H arom.).
[0098] IR (cm -1< ): 3020 (Ar-H), 2850-2953 (alkyl-H), 1600 (CH 2 =CH-Ar); 1512 (CC, Ar); 1250 (P=O), 1027 (POC); 957 (C=C), 854 (Ar-H). Monomer (34): Dibutyl[(4-ethenylphenyl)methyl]phosphonate:
[0099]
[0100] Potassium tert-butoxide (5.0 g, 44.1 mmol) was suspended in THF (40 mL, dry) at 0 °C under inert gas before dibutylphosphonate (8.6 g, 44.1 mmol) dissolved in THF (20 mL) was added dropwise. The mixture was stirred for 30 min before being added dropwise to a solution of chloromethylstyrene (3.4 g, 22.1 mmol), TBHQ (2-tert-butylhydroquinone), and TBAI (tetrabutylammonium iodide) in THF (20 mL) at 0 °C. After 18 hours at 20 °C under inert gas, the solids were separated and the solvent was distilled off.
[0101] 1< H NMR (CDCl 3 , 500 MHz) δ (ppm): 0.89 (t, 6H, CH 3 ), 1.34 (sextet, 4H, CH 2 -CH 3 ), 1.56 (quintet, 4H, CH 2 -CH 2 -CH 3 ), 3.16 (d, 2H, CH 2 -P), 3.93 (m, 4H, PO-CH 2 ), 5.22 / 5.74 (d, 2H, CH=CH 2 ); 6.70 (dd, 1H, CH=CH 2 ); 7.24 - 7.34 (m, 4H arom.).
[0102] IR (cm -1< ): 3025 (Ar-H), 2850-2953 (alkyl-H), 1600 (CH2=CH-Ar); 1512 (CC, Ar); 1250 (P=O), 1027 (POC); 957 (C=C), 854 (Ar-H). Monomer (35): Diethyl-4-Acryloyloxy-Butyl Phosphate:
[0103]
[0104] 4-Hydroxybutyl acrylate (5.3 g, 37 mmol) was stirred together with triethylamine (3.8 g, 38 mmol) and copper(I) chloride (0.1 g) in diethyl ether (30 mL) for 1 h at 0 °C under inert gas before diethyl chlorophosphate (6.5 g, 38 mmol) dissolved in diethyl ether (10 mL) was added dropwise. After stirring for 24 h at 20 °C, the triethylammonium chloride was removed and the solvent distilled off.
[0105] 1< H-NMR (500 MHz, CDC! 3 ), δ(ppm): 1.33 (t, 6H, CH 3 ); 1.78 (q, 4H, CH2 ); 4.09 / 4.18 (m, 8H, -O-CH 2 -); 5.82 / 6.10 / 6.37 (3H, CH 2 =CH-) Monomer (36): Dimethyl-2-methacryloyloxy-ethylphosphonates:
[0106]
[0107] To a solution of 2-hydroxyethyl methacrylate (3.0 g, 23.0 mmol), triethylamine (2.5 g, 25 mmol), and 4-(dimethylamino)pyridine (60 mg, 0.5 mmol) in dichloromethane (10 mL) at 0 °C under inert gas, tosyl chloride (4.3 g, 22.6 mmol) dissolved in dichloromethane (15 mL) was added dropwise with stirring. After 6 hours, dimethylphosphonate (5.0 g, 45.8 mmol) dissolved in dichloromethane (20 mL) was added dropwise at 20 °C and stirred for 18 hours. The solids were separated, and the volatiles were removed.
[0108] 1< H NMR (CDCl 3 , 500 MHz) δ (ppm): 1.94 (s, 3H, α-CH 3 ), 3.12 (t, 2H, CH 2 -P), 3.7-4.30 (s, 6H, PO-CH 3 ), 5.58 / 6.05 (s, 2H, CH=CH 2 ).
[0109] IR (cm -1< ): 2961 (alkyl-H), 1717 (C=O), 1634 (C=C), 1456 (CH), 1362 (CP), 1262 (P=O), 1173 (CO), 1043 (POC), 977 (CH). Monomer (37): Diethyl-2-methacryloyloxy-ethylphosphonates:
[0110]
[0111] To a solution of 2-hydroxyethyl methacrylate (2.7 g, 20.5 mmol), triethylamine (2.1 g, 21 mmol), and 4-(dimethylamino)pyridine (60 mg, 0.5 mmol) in dichloromethane (10 mL) at 0 °C under inert gas, tosyl chloride (3.8 g, 20.1 mmol) dissolved in dichloromethane (15 mL) was added dropwise with stirring. After 6 hours, diethyl phosphonate (5.6 g, 40.7 mmol) dissolved in dichloromethane (20 mL) was added dropwise at 20 °C and stirred for 18 hours. The solids were separated, and the volatiles were removed.
[0112] 1< H NMR (CDCl 3 , 500 MHz) δ (ppm): 1.34 (t, 6H, CH 2 -CH 3 ), 1.94 (s, 3H, α-CH 3 ), 3.19 (t, 2H, CH 2 -P), 4.12 (q, 4H, PO-CH 2 ), 5.55 / 6.02 (s, 2H, CH=CH 2 ).
[0113] IR (cm -1< ): 2956 (alkyl-H), 1717 (C=O), 1634 (C=C), 1456 (CH), 1362 (CP), 1261 (P=O), 1173 (CO), 1043 (POC), 977 (CH). Monomer (38): Dibutyl-2-methacryloyloxy-ethylphosphonates:
[0114]
[0115] To a solution of 2-hydroxyethyl methacrylate (2.1 g, 16.4 mmol), triethylamine (1.7 g, 17 mmol), and 4-(dimethylamino)pyridine (40 mg, 0.3 mmol) in dichloromethane (10 mL) at 0 °C under inert gas, tosyl chloride (3.2 g, 16.6 mmol) dissolved in dichloromethane (15 mL) was added dropwise with stirring. After 6 hours, dibutylphosphonate (6.4 g, 33.0 mmol) dissolved in dichloromethane (20 mL) was added dropwise at 20 °C and stirred for 18 hours. The solids were collected, and the volatiles were removed.
[0116] 1< H NMR (CDCl 3 , 500 MHz) δ (ppm): 0.93 (t, 6H, CH 3 ), 1.39 (sextet, 4H, CH 2 -CH 3 ), 1.64 (quintet, 4H, CH 2 -CH 2 -CH 3 ), 1.95 (s, 3H, α-CH 3 ), 3.09 (m, 2H, CH 2 -P), 4.05 (m, 4H, PO-CH 2 ), 5.56 / 6.10 (s, 2H, CH=CH 2 ).
[0117] IR (cm -1< ): 2982 (alkyl-H), 1734 (C=O), 1639 (C=C), 1456 (CH), 1362 (CP), 1258 (P=O), 1173 (CO), 1017 (POC), 977 (CH). Synthesis of the copolymers: Materials used:
[0118] For the syntheses of the copolymers, styrene (99%, Acros Organics / stabilizer removed), sulfur (>99%, Alfa Aesar), divinylbenzene (Merck KGaA, containing 25 - 50% ethylstyrene), methacrylic acid allyl ester (98%, Sigma Aldrich, stab. with 50-185 ppm MEHQ), vinylphosphonic acid (97%, Sigma Aldrich), diphenyl(4-vinylphenyl)phosphine (97%, Sigma Aldrich) and the synthesized monomers of formulas (25) to (38) were used.
[0119] With regard to the following copolymer structures (6a) to (24a), the statements regarding the specification of repeating units apply analogously to formulas (6) to (24). Due to the random distribution of the monomer units within the copolymer, the specification of "n" as a repeating unit has been omitted. Copolymer (6): Poly(styrene-ran-diethyl-2-methacryloyloxy-ethylphosphate-ran-sulfur) Example (6a)
[0120] Synthesis of (6a):
[0121] Sulfur (310 mg, 1 wt%), styrene (30.98 g, 98 wt%), and monomer (26) (320 mg, 1 wt%) were mixed together and deoxygenated by three freeze-degassing cycles. The mixture was heated to 130 °C for 72 h. After dissolving in THF, the product was isolated by precipitation in methanol. EA: C 90.9%, H 8.4%, S 0.2%; TGA: Td 5%: 405 °C DCS: T g: 90.3 °C GPC (UV detector): Mn 32 kDa; Mw 62 kDa.
[0122] Compound (6a) exhibits particularly good flame-retardant properties. This is due to the presence of a high molecular weight in addition to the phosphorus-containing monomer unit. Copolymer (7): Poly(styrene-ran-diphenyl-2-methacryloyloxy-ethylphosphate-ran-sulfur) Example (7a)
[0123]
[0124] Compound (7a) exhibits particularly good flame-retardant properties. This is due to the presence of a high molecular weight in addition to the phosphorus-containing monomer unit. Synthesis of (7a):
[0125] Sulfur (1.5 g, 1 wt%), styrene (147 g, 98 wt%), and monomer (27) (1.5 g, 1 wt%) were mixed together and deoxygenated by three freeze-degassing cycles. The mixtures were heated to 130 °C for 72 h. After dissolving in THF, the product was isolated by precipitation in methanol. TGA: Td 5% (°C) = 325; DSC: T g (°C) = 96.7; GPC (UV detector): Mw (kDa) = 46; Mn (kDa) = 10. Copolymer (8): Poly(styrene- ran -diphenyl-2-acryloyloxy-ethylphosphate- ran -sulfur) Example (8a)
[0126] Synthesis of (8a):
[0127] Sulfur (1.5 g, 1 wt%), styrene (147 g, 98 wt%), and monomer (28) (1.5 g, 1 wt%) were mixed together and deoxygenated by three freeze-degassing cycles. The mixtures were heated to 130 °C for 72 h. After dissolving in THF, the product was isolated by precipitation in methanol. TGA: Td 5% (°C) = 325; DSC: T g (°C) = 94.2; GPC (UV detector): Mw (kDa) = 46; Mn (kDa) = 11.8.
[0128] Compound (8a) exhibits particularly good flame-retardant properties. This is due to the presence of a high molecular weight in addition to the phosphorus-containing monomer unit. Example (8b)
[0129] Synthesis of (8b):
[0130] Sulfur (1.6 g, 1 wt%), styrene (138.4 g, 94 wt%), and monomer (28) (10.0 g, 5 wt%) were mixed together and deoxygenated by three freeze-degassing cycles. The mixtures were heated to 130 °C for 72 hours. After dissolving in THF, the product was isolated by precipitation in methanol. TGA: Td 5% (°C) = 350; DSC: T g (°C) = 96.8; GPC (UV detector): Mw (kDa) =49.5; Mn (kDa) =7.3 Copolymer (9): Poly(styrene- ran -diphenyl-methacryloyloxy-n-butylphosphate- ran- sulfur) Example (9a)
[0131] Synthesis of (9a):
[0132] Sulfur (1.5 g, 1 wt%), styrene (147 g, 98 wt%), and monomer (29) (1.5 g, 1 wt%) were mixed together and deoxygenated by three freeze-degassing cycles. The mixtures were heated to 130 °C for 72 h. After dissolving in THF, the product was isolated by precipitation in methanol. TGA: Td 5% (°C) = 290; DSC: T g (°C) = 83.4; GPC: Mw (kDa) = 40; Mn (kDa) = 13.3. Copolymer (10): Poly(styrene- ran -diphenyl-4-acryloyloxy-butylphosphate- ran -sulfur) Example (10a)
[0133] Synthesis of (10a):
[0134] Sulfur (1.5 g, 1 wt%), styrene (147 g, 98 wt%), and monomer (30) (1.5 g, 1 wt%) were mixed together and deoxygenated by three freeze-degassing cycles. The mixtures were heated to 130 °C for 72 h. After dissolving in THF, the product was isolated by precipitation in methanol. TGA: Td 5% (°C) = 325; DSC: T g (°C) = 93.5; GPC (UV detector): Mw (kDa) = 51; Mn (kDa) = 12.1. Copolymer (11): Poly(styrene-ran-diphenyl-2-methacryloyloxy-ethylphosphinate-ran-sulfur) Example (11a)
[0135] Synthesis of (11a):
[0136] Sulfur (0.1 g, 1 wt%), styrene (9.8 g, 98 wt%), and monomer (32) (0.1 g, 1 wt%) were mixed together and deoxygenated by three freeze-degassing cycles. The mixtures were heated to 130 °C for 72 hours. After dissolving in THF, the product was isolated by precipitation in methanol. GPC (UV detector): Mw (kDa) =34.0; Mn (kDa) =3.3 Copolymer (14): Poly(styrene- ran -diethyl p-vinylbenzylphosphonate- ran -sulfur) Example (14a)
[0137] Synthesis of (14a):
[0138] Sulfur (0.1 g, 1 wt%), styrene (9.8 g, 98 wt%), and monomer (31) (0.1 g, 1 wt%) were mixed together and deoxygenated by three freeze-degassing cycles. The mixtures were heated to 130 °C for 72 h. After dissolving in THF, the product was isolated by precipitation in methanol. GPC (UV detector): Mw (kDa) = 14.6; Mn (kDa) = 2.5 Copolymer (16): Poly(styrene-ran-allyl-methacrylate-ran-sulfur) (not according to the invention) Example (16a)
[0139] where ω [AMA] corresponds to the mass fraction of the allyl methacrylate and Rv consists of vinyl or a covalent bond to another polymer of formula (1). Synthesis of (16):
[0140] Sulfur (0.01 g, 1 wt%), styrene (0.98 g, 98 wt%), allyl methacrylate (0.01 g, 1 wt%), and azodiisobutyronitrile (AIBN, 0.07 g) were mixed together and deoxygenated by three freeze-degassing cycles. The mixture was heated to 80 °C for 4 hours. After dissolving in THF, the product was isolated by precipitation in methanol. GPC (UV detector): Mw (kDa) = 22; Mn (kDa) = 6 Copolymer (17): Poly(styrene-ran-diethyl-4-methacryloyloxy-butylphosphate-ran-sulfur) Example (17a)
[0141] Synthesis of (17a):
[0142] Sulfur (0.01 g, 1 wt%), styrene (0.98 g, 98 wt%), and monomer (35) (0.01 g, 1 wt%) were mixed together and deoxygenated by three freeze-degassing cycles. The mixtures were heated to 130 °C for 72 hours. After dissolving in THF, the product was isolated by precipitation in methanol. TGA: Td 5% (°C) = 325; DSC: T g (°C) = 97.9; GPC (UV detector): Mw (kDa) =25.8; Mn (kDa) =5.3 Copolymer (18): Poly(styrene-ran-2-methacryloyloxy-methylphosphonate-ran-sulfur) Example 18a
[0143] Synthesis of (18a):
[0144] Sulfur (0.01 g, 1 wt%), styrene (0.98 g, 98 wt%), monomer (36) (0.01 g, 1 wt%), and azodiisobutyronitrile (AIBN, 70 mg, 5 mol% on styrene) were mixed together and deoxygenated by three freeze-degassing cycles. The mixture was heated to 80 °C for 40 hours. After dissolving in THF, the product was isolated by precipitation in methanol. GPC (UV detector): Mw (kDa) = 16.2; Mn (kDa) = 3.9; IR (P=O, 1247 cm-1): detectable Copolymer (19): Poly(styrene-ran-2-methacryloyloxy-methylphosphonate-ran-sulfur) Example (19a)
[0145] Synthesis of (19a):
[0146] Sulfur (0.01 g, 1 wt%), styrene (0.98 g, 98 wt%), monomer (37) (0.01 g, 1 wt%) and azodiisobutyronitrile (AIBN, 70 mg, 5 mol% on styrene) were mixed together and deoxygenated by three freeze-degassing cycles.
[0147] The mixture was heated to 80 °C for 40 hours. After dissolving in THF, the product was isolated by precipitation in methanol. GPC (UV detector): Mw (kDa) = 8.7; Mn (kDa) = 2.9; IR (P=O, 1247 cm -1 < ): detectable Copolymer (20): Poly(styrene-ran-2-methacryloyloxy-butylphosphonate-ran-sulfur) Example (20a)
[0148] Synthesis of (20a):
[0149] Sulfur (0.01 g, 1 wt%), styrene (0.98 g, 98 wt%), monomer (38) (0.01 g, 1 wt%), and azodiisobutyronitrile (AIBN, 70 mg, 5 mol% based on styrene) were mixed together and deoxygenated by three freeze-degassing cycles. The mixture was heated to 80 °C for 40 hours. After dissolving in THF, the product was isolated by precipitation from methanol. GPC (UV detector): Mw (kDa) = 13.8; Mn (kDa) = 3.6; Copolymer (21): Poly(styrene-ran-dimethyl [(4-ethenylphenyl)methyl]phosphonate-ran-sulfur) Example (21a)
[0150] Synthesis of (21a):
[0151] Sulfur (0.01 g, 1 wt%), styrene (0.98 g, 98 wt%), monomer (33) (0.01 g, 1 wt%), and azodiisobutyronitrile (AIBN, 70 mg, 5 mol% based on styrene) were mixed together and deoxygenated by three freeze-degassing cycles. The mixture was heated to 80 °C for 40 hours. After dissolving in THF, the product was isolated by precipitation from methanol. GPC (UV detector): Mw (kDa) = 6.0; Mn (kDa) = 3.6 IR (P=O, 1247 cm-1): detectable Copolymer (22): Poly(styrene-ran-dibutyl[(4-ethenylphenyl)methyl]phosphonate-ran-sulfur) Example (22a)
[0152] Synthesis of (22a):
[0153] Sulfur (0.01 g, 1 wt%), styrene (0.98 g, 98 wt%), monomer (34) (0.01 g, 1 wt%), and azodiisobutyronitrile (AIBN, 15.6 mg, 5 mol% based on styrene) were mixed together and deoxygenated by three freeze-degassing cycles. The mixture was heated to 80 °C for 40 hours. After dissolving in THF, the product was isolated by precipitation in methanol. GPC (UV detector): Mw (kDa) = 15.0; Mn (kDa) = 3.0 IR (P=O, 1247 cm -1 < ): detectable Copolymer (23): Poly(styrene-ran-vinylphosphonic acid-ran-sulfur) Example (23a)
[0154] Synthesis of (23a):
[0155] Sulfur (0.2 g, 1 wt%), styrene (19.6 g, 98 wt%), vinylphosphonic acid (0.2 g, 1 wt%), and azodiisobutyronitrile (AIBN, 1.3 g, 5 mol% based on styrene) were mixed together and deoxygenated by three freeze-degassing cycles. The mixture was heated to 80 °C for 15 hours. After dissolving in THF, the product was isolated by precipitation in methanol. GPC (UV detector): Mw (kDa) = 28.7; Mn (kDa) = 7.7 Copolymer (24): Poly(styrene-ran-diphenyl(4-vinylphenyl)phosphine-ran-sulfur) Example (24a)
[0156] Synthesis of (24a):
[0157] Sulfur (0.2 g, 1 wt%), styrene (19.6 g, 98 wt%), diphenylphosphinostyrene (0.2 g, 1 wt%), and azodiisobutyronitrile (AIBN, 1.3 g, 5 mol% based on styrene) were mixed together and deoxygenated by three freeze-degassing cycles. The mixture was heated to 80 °C for 15 hours. After dissolving in THF, the product was isolated by precipitation in methanol. GPC (UV detector): Mw (kDa) = 17.9; Mn (kDa) = 6.9 Production of fire-retardant molding compounds
[0158] Polymers and additives used for the production of fire-retardant molding materials or compounds: Polymer / aggregate Type and manufacturer Abbreviation Polystyrene Polystyrene 158K, BASF SE, Ludwigshafen, Germany PS 2,4,8,10-Tetraoxa-3,9-diphosphaspiro [5.5] undecane-3,9-dimethyl-3,9-dioxide Aflammit PCO 900, Thor GmbH, Speyer, Germany P1 Hexakisphenoxycyclotriphosphazene aber GmbH, Karlsruhe, Germany P2 Production of foam bodies for fire testing VB1:
[0159] First, 20 g of PS was dissolved in dichloromethane. The solution was then poured into a 20 cm x 10 cm aluminum mold and dried at room temperature (RT) for 24 h. The dried polymer was removed from the aluminum mold and foamed with steam in a perforated stainless steel mold for 20 min. The foamed test specimen was dried for 24 h at 50 °C until constant mass was reached. The resulting test specimens had a density of approximately 70 kg / m³. VB2:
[0160] First, 20 g of PS and 0.5 g of P1 were dissolved in dichloromethane. The solution was then poured into a 20 cm x 10 cm aluminum mold and dried at room temperature (RT) for 24 h. The dried compound was removed from the aluminum mold and foamed with steam in a perforated stainless steel mold for 20 min. The foamed test specimen was dried for 24 h at 50 °C until constant mass was reached. The resulting test specimens had a density of approximately 70 kg / m³. VB3:
[0161] First, 20 g of PS and 0.95 g of P2 were dissolved in dichloromethane. The solution was then poured into a 20 cm x 10 cm aluminum mold and dried at room temperature (RT) for 24 h. The dried compound was removed from the aluminum mold and foamed with steam in a perforated stainless steel mold for 20 min. The foamed test specimen was dried for 24 h at 50 °C until constant mass was reached. The resulting test specimens had a density of approximately 70 kg / m³. EB1:
[0162] First, 20 g of (2a) were dissolved in dichloromethane. The solution was then poured into a 20 cm x 10 cm aluminum mold and dried at room temperature (RT) for 24 h. The dried copolymer was removed from the aluminum mold and foamed with steam in a perforated stainless steel mold for 20 min. The foamed test specimen was dried to constant mass at 50 °C for 24 h. The resulting test specimens had a density of approximately 70 kg / m³. EB2:
[0163] First, 20 g of (2a) and 0.95 g of P2 were dissolved in dichloromethane. The solution was then poured into a 20 cm x 10 cm aluminum mold and dried at room temperature (RT) for 24 h. The dried compound was removed from the aluminum mold and foamed with steam in a perforated stainless steel mold for 20 min. The foamed test specimen was dried for 24 h at 50 °C until constant mass was reached. The resulting test specimens had a density of approximately 70 kg / m³. EB3:
[0164] First, 20 g of (2b) were dissolved in dichloromethane. The solution was then poured into a 20 cm x 10 cm aluminum mold and dried at room temperature (RT) for 24 h. The dried copolymer was removed from the aluminum mold and foamed with steam in a perforated stainless steel mold for 20 min. The foamed test specimen was dried for 24 h at 50 °C until constant mass was reached. The resulting test specimens had a density of approximately 70 kg / m³. EB4:
[0165] First, 20 g of (2b) and 0.5 g of P1 were dissolved in dichloromethane. The solution was then poured into a 20 cm x 10 cm aluminum mold and dried at room temperature (RT) for 24 h. The dried compound was removed from the aluminum mold and foamed with steam in a perforated stainless steel mold for 20 min. The foamed test specimen was dried for 24 h at 50 °C until constant mass. The resulting test specimens had a density of approximately 70 kg / m³. EB5:
[0166] First, 20 g of (3a) were dissolved in dichloromethane. The solution was then poured into a 20 cm x 10 cm aluminum mold and dried at room temperature (RT) for 24 h. The dried copolymer was removed from the aluminum mold and foamed with steam in a perforated stainless steel mold for 20 min. The foamed test specimen was dried to constant mass at 50 °C for 24 h. The resulting test specimens had a density of approximately 70 kg / m³. EB6:
[0167] First, 20 g of (4a) were dissolved in dichloromethane. The solution was then poured into a 20 cm x 10 cm aluminum mold and dried at room temperature (RT) for 24 h. The dried copolymer was removed from the aluminum mold and foamed with steam in a perforated stainless steel mold for 20 min. The foamed test specimen was dried to constant mass at 50 °C for 24 h. The resulting test specimens had a density of approximately 70 kg / m³. EB7:
[0168] First, 20 g of (4b) were dissolved in dichloromethane. The solution was then poured into a 20 cm x 10 cm aluminum mold and dried at room temperature (RT) for 24 h. The dried copolymer was removed from the aluminum mold and foamed with steam in a perforated stainless steel mold for 20 min. The foamed test specimen was dried to constant mass at 50 °C for 24 h. The resulting test specimens had a density of approximately 70 kg / m³. EB8:
[0169] First, 20 g of (6a) were dissolved in dichloromethane. The solution was then poured into a 20 cm x 10 cm aluminum mold and dried at room temperature (RT) for 24 h. The dried copolymer was removed from the aluminum mold and foamed with steam in a perforated stainless steel mold for 20 min. The foamed test specimen was dried to constant mass at 50 °C for 24 h. The resulting test specimens had a density of approximately 70 kg / m³. EB9:
[0170] First, 20 g of (7a) were dissolved in dichloromethane. The solution was then poured into a 20 cm x 10 cm aluminum mold and dried at room temperature (RT) for 24 h. The dried copolymer was removed from the aluminum mold and foamed with steam in a perforated stainless steel mold for 20 min. The foamed test specimen was dried to constant mass at 50 °C for 24 h. The resulting test specimens had a density of approximately 70 kg / m³. EB10:
[0171] First, 20 g of (8a) were dissolved in dichloromethane. The solution was then poured into a 20 cm x 10 cm aluminum mold and dried at room temperature (RT) for 24 h. The dried copolymer was removed from the aluminum mold and foamed with steam in a perforated stainless steel mold for 20 min. The foamed test specimen was dried to constant mass at 50 °C for 24 h. The resulting test specimens had a density of approximately 70 kg / m³. EB11:
[0172] First, 20 g of (9a) were dissolved in dichloromethane. The solution was then poured into a 20 cm x 10 cm aluminum mold and dried at room temperature (RT) for 24 h. The dried copolymer was removed from the aluminum mold and foamed with steam in a perforated stainless steel mold for 20 min. The foamed test specimen was dried to constant mass at 50 °C for 24 h. The resulting test specimens had a density of approximately 70 kg / m³. EB12:
[0173] First, 20 g of (10a) were dissolved in dichloromethane. The solution was then poured into a 20 cm x 10 cm aluminum mold and dried at room temperature (RT) for 24 h. The dried copolymer was removed from the aluminum mold and foamed with steam in a perforated stainless steel mold for 20 min. The foamed test specimen was dried to constant mass at 50 °C for 24 h. The resulting test specimens had a density of approximately 70 kg / m³. EB13:
[0174] First, 20 g of (14a) were dissolved in dichloromethane. The solution was then poured into a 20 cm x 10 cm aluminum mold and dried at room temperature (RT) for 24 h. The dried copolymer was removed from the aluminum mold and foamed with steam in a perforated stainless steel mold for 20 min. The foamed test specimen was dried to constant mass at 50 °C for 24 h. The resulting test specimens had a density of approximately 70 kg / m³.
[0175] EB14: First, 20 g of (11a) were dissolved in dichloromethane. The solution was then poured into a 20 cm x 10 cm aluminum mold and dried at room temperature (RT) for 24 h. The dried copolymer was removed from the aluminum mold and foamed with steam in a 5-hole stainless steel mold for 20 min. The foamed test specimen was dried to constant mass at 50 °C for 24 h. The resulting test specimens had a density of approximately 70 kg / m³.
[0176] EB15: First, 20 g of (2c) were dissolved in dichloromethane. The solution was then poured into a 20 cm x 10 cm aluminum mold and dried at room temperature (RT) for 24 h. The dried copolymer was removed from the aluminum mold and foamed with steam in a perforated stainless steel mold for 20 min. The foamed test specimen was dried to constant mass at 50 °C for 24 h. The resulting test specimens had a density of approximately 70 kg / m³.
[0177] EB16: First, 20 g of (4c) were dissolved in dichloromethane. The solution was then poured into a 20 cm x 10 cm aluminum mold and dried at room temperature (RT) for 24 h. The dried copolymer was removed from the aluminum mold and foamed with steam in a perforated stainless steel mold for 20 min. The foamed test specimen was dried to constant mass at 50 °C for 24 h. The resulting test specimens had a density of approximately 70 kg / m³.
[0178] EB17: First, 20 g of (8b) were dissolved in dichloromethane. The solution was then poured into a 20 cm x 10 cm aluminum mold and dried at room temperature (RT) for 24 h. The dried copolymer was removed from the aluminum mold and foamed with steam in a perforated stainless steel mold for 20 min. The foamed test specimen was dried to constant mass at 50 °C for 24 h. The resulting test specimens had a density of approximately 70 kg / m³. Carrying out fire tests Screening test:
[0179] A 5 cm x 10 cm x 1 cm strip of the foam body is held for a few seconds in a 2 cm high propane flame with an energy of approximately 50 kW. As soon as the sample ignites, but no later than 5 seconds later, it is removed from the flame, and the flammability and self-extinguishing properties of the sample are recorded.
[0180] Flame retardant means that after an initial ignition, the copolymer bodies or molding compounds have shorter afterburning times compared to homopolystyrene.
[0181] Self-extinguishing in the screening test is understood as the following behavior: The sample body made of copolymers or molding compounds ignited by the flame of the burner extinguishes within 5 s after the burner flame has been removed from the sample body. Fire test according to DIN 4102-2 (B2):
[0182] A 20 cm x 10 cm x 1 cm sample is exposed to flame for 15 s using a burner with an energy of approximately 50 kW and a flame height of 2 cm, positioned at a vertical distance of 1 cm from the underside of the sample. The afterburning time, flame height, self-extinguishing, and burning dripping behavior of the sample are recorded. Elemental analysis (EA):
[0183] The elemental composition of the copolymers was measured using a vario MICRO cube (Elementar Analysesysteme GmbH, Langenselbold). The calibration of the measurement method was performed using sulfanilamide. Gel permeation chromatography (GPC):
[0184] The molecular weight and molecular weight distribution of the samples were measured using a GPC analysis system from Shimadzu (Kyoto, Japan) consisting of a degasser (DGU-20A 3R ), two pumps (LC-20AD), an autosampler (SIL-20A HT ), a column oven (CTO-20A, 30°C), a diode array detector (SPD-M20A, 30°C), a refractive index detector (RID-20A, 30°C), a control unit (CBM-20A) and a column set (PSS Polymer Standard Services GmbH, Mainz - one guard column SDV 50x8 mm, 5 µm, two separation columns SDV 300x8 mm, 5 µm, 1000 Å, one separation column SDV 300x8 mm, 5 µm, 100,000 Å). Calibration was performed using polystyrene standards. Melt viscosity:
[0185] The melt viscosity was measured using the MeltFloW basic plus (Karg Industrietechnik, Krailing) according to ISO 1133. Foam quality:
[0186] Various aspects were considered in assessing foam quality: (a) Cellularity of the polymer foams (size and uniformity of the cells). The foam bodies were tested and classified according to the following criteria: -- Large cells (> 5 mm) highly irregular; - Large cells (> 5 mm) irregular; 0 Medium-sized cells (5 mm - 1 mm) irregular; + Small cells (< 1 mm) irregular; ++ small cells (< 1 mm) regularly. (b) Phase separation and agglomerate formation. The foam bodies were tested and classified according to the following criteria: 0 >10 agglomerates and phase separations per foam body; + >0 - <10 agglomerates and phase separations per foam body; ++ No agglomerates and phase separations per foam body.
[0187] "The assessment of the quality of the foam bodies, the elemental composition, the molecular weights and distributions as well as the thermal characteristics of the synthesized copolymers are presented in the following Tables 1, 2 and 3. The fire test results according to DIN 4102-2 (B2) are summarized in Tables 4 (screening test) and 5 (small burner test). Table 1: Assessment of foam body quality sample (a) Cellularity (b) Phase separation & agglomerates (6a) ++ ++ (7a) ++ ++ (8a) ++ ++ (9a) ++ + (10a) ++ + (14a) ++ ++ Table 2: Elemental composition of the synthesized copolymers: sample C (%) 1< H (%) 1< S (%) 1< N (%) 1< (6a) 90,9 8,40 0,20 0,00 1< percentage elemental composition determined by elemental analysis, Table 3: Molecular weights and distributions, thermal characteristics and viscosity of the copolymers: sample Mn 1< (kDa) Mw 1< (kDa) Ð 1< Td 5% 2< (°C) Tg 3< (°C) (6a) 32 62 1,94 405 90 (7a) 10 46 4,60 325 96,7 (8a) 11,8 46 3,90 325 94,2 (9a) 13,3 40 3,08 290 83,4 (10a) 12,1 51 4,21 325 93,5 1< average molecular weights and their molecular weight distribution determined by GPC, 2< decomposition temperature at 5% mass loss determined by TGA, 3< onset of the glass transition temperature determined by DSC. Table 4: Fire test results:Screening test according to DIN 4102-2 (B2): Example composition Proportion of (co)polymer (phr 1< ) Proportion P1 or P2 (phr 1< ) Self-extinguishing (yes / no) VB1 PS 100 - no VB2 PS + P1 100 2,50 no VB3 PS + P2 100 4,75 no EB8 (6a) 100 - Yes EB9 (7a) 100 - Yes EB10 (8a) 100 - Yes EB11 (9a) 100 - Yes EB12 (10a) 100 - Yes EB13 (14a) 100 - Yes EB14 (11a) 100 - Yes 1< parts per hundred rubber Table 5: Small burner test according to DIN 4102-2 (B2): Example composition Proportion of (co)polymer (phr 1< ) Proportion P1 or P2 (phr 1< ) Flame height (cm) Afterburn time (s) VB1 PS 100 - > 15 31 VB2 PS + P1 100 2,50 > 15 35 VB3 PS + P2 100 4,75 > 15 22 EB8 (6a) 100 - 11 13 EB10 (8a) 100 - 8 5 EB17 (8b) 100 - 9 3 EB12 (10a) 100 - 6 0 1< parts per hundred rubber
Claims
1. A fire-retardant copolymer having a statistical monomer distribution of monomer units having the compositions (mass fractions) ω with ω(Sty), ω(P) and ω(S), wherein ω(S) and ω(P) represent a mass fraction of the sulfurous and phosphorous repeating units and the sum of the mass fractions ω(Sty), ω(P) and ω(S) is equal to 1, selected from the group of formulas (6) to (15) and (17) to (24), comprising wherein the copolymer comprises covalently bonded phosphorus compounds and has a sulfur content of less than 40% within the fire-retardant copolymer.
2. The fire-retardant copolymer according to claim 1, characterized in that the copolymer is colorless and / or odorless, wherein the colorlessness is determined by comparing the colors according to RAL 1013 Oyster white, RAL 9001 Cream, RAL 9003 Signal white, RAL 9010 Pure white and / or RAL 9016 Traffic white and / or the odorlessness is within the detection limit of sulfide compounds within the range of less than 50 µg / m3 of air.
3. The fire-retardant copolymer according to any of claims 1 or 2, characterized in that the copolymer has shorter afterburn times after initial ignition compared to homopolystyrene or is extinguished within 5s after ignition.
4. The fire-retardant copolymer according to any of claims 1 to 3, further containing additional phosphorus-containing additives.
5. A fire-retardant molding material comprising at least one fire-retardant copolymer, having a statistical monomer distribution of monomer units having the compositions (mass fractions) ω with ω(Sty), ω(P) and ω(S), wherein ω(S) and ω(P) represent a mass fraction of the sulfurous and phosphorous repeating units and the sum of the mass fractions ω(Sty), ω(P) and ω(S) is equal to 1, selected from a group of compounds of formulas (6) to (15) and (17) to (24), comprising wherein the copolymer comprises covalently bonded phosphorus compounds and has a sulfur content of less than 40% within the fire-retardant copolymer, the fire-retardant molding material comprising at least one further polymer and / or at least one additional copolymer selected from the group of formulas (6) to (15) and (17) to (24) and / or a material in addition to the fire-retardant copolymer.
6. The fire-retardant molding material according to claim 5, wherein the fire-retardant molding material comprises a material made of metal or plastic or prepregs or ceramics.
7. The fire-retardant molding material according to claim 5 or 6, wherein the copolymer content is more than 10% by weight of the molding material.
8. The fire-retardant molding material according to any of claims 5 to 7, wherein the molding material comprises homopolymeric polystyrenes (PS) or expandable styrene polymers (EPS) or extruded foam sheets (XPS) as a further polymer.
9. The fire-retardant molding material according to any of claims 5 to 8, wherein the molding material has shorter afterburn times after initial ignition compared to homopolystyrene and is therefore flame-retardant or the molding material is extinguished within 5s after ignition and is therefore self-extinguishing.
10. The fire-retardant molding material according to any of claims 5 to 9, wherein the molding material is colorless and / or odorless and the colorlessness is determined by comparing the colors according to RAL 1013 Oyster white, RAL 9001 Cream, RAL 9003 Signal white, RAL 9010 Pure white and / or RAL 9016 Traffic white and / or the odorlessness is within the detection limit of sulfide compounds within the range of less than 50 µg / m3 of air.
11. The fire-retardant molding material according to any of claims 5 to 10, wherein the molding compound contains at least one IR absorber, in particular graphite, carbon black or aluminum having an average particle size within the range of 1 to 50 µm.
12. A method for producing fire-retardant molding materials according to any of claims 5 to 11, comprising the steps: a. mixing an organic blowing agent into a polymer melt comprising at least one fire-retardant copolymer having or not having further phosphorus-containing additives by means of static and / or dynamic mixers at a temperature of at least 150°C, b. cooling the blowing agent-containing polymer melt to a temperature of at least 120°C, c. discharging through a nozzle plate having holes whose diameter at the nozzle outlet is at most 1.5 mm and d. granulating the blowing agent-containing melt directly behind the nozzle plate under water at a pressure within the range of 1 to 20 bar.
13. A method for producing fire-retardant molding materials according to any of claims 5 to 11, comprising the steps: a. polymerization, b. adding an organic blowing agent before, during and / or after the polymerization and c. separating the expandable, blowing agent-containing copolymers by means of sieving.
14. The method for producing the fire-retardant copolymers or molding materials according to claim 13, wherein the molding materials being obtained by means of suspension polymerization.
15. Use of fire-retardant copolymers or molding materials according to any of claims 1 to 11 as an individual or co-component of insulating material for buildings or as a structural part and component in the electrical and electronics sector.