PLASTIC COMPOSITION, USE OF THE PLASTIC COMPOSITION AND METHOD FOR MAKING A MOLDED BODY

DE502022001918D1Active Publication Date: 2024-11-07DIPROMAT GMBH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
DE502022001918
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Filing Date
2022-12-23
Publication Date
2024-11-07
Estimated Expiration
2042-12-23

AI Technical Summary

Technical Problem

Polyolefin plastics exhibit significant shrinkage during molding processes, leading to dimensional inconsistencies and stress in moldings, which complicates production and reduces economic efficiency, especially when switching between different plastic compositions or molding processes.

Method used

A plastic composition comprising at least one polyolefin and a thermoplastic elastomer with a diene-based block A and an alpha-methylstyrene-based block B, combined with 10% to 70% by weight of flat glass fibers, which reduces shrinkage by up to 95% compared to pure polyolefin, ensuring low distortion and high dimensional stability.

Benefits of technology

The solution enables the production of moldings with minimal distortion and high dimensional stability, allowing for shorter cooling times, increased production efficiency, and improved mechanical properties such as impact strength, making it suitable for various molding processes including 3D printing.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The invention relates to a plastic composition, the use of the plastic composition and a method for producing a molded body.

[0002] Polyolefins, such as polypropylene (PP) or polyethylene (PE), are among the most versatile plastics used in plastic compounds. As commodity plastics, polyolefin compounds are molded into a wide variety of shapes using a range of forming processes.

[0003] Injection molding is a particularly relevant shaping process. In injection molding, a molded part is formed from a plastic compound, for example, polyolefin, which is injected into a mold cavity. The molten plastic compound is held in the mold cavity for a sufficient period to solidify and conform to its shape. The cooling phase, i.e., the time required to cool the plastic compound and remove the molded part, is a crucial factor for production time and thus for manufacturing efficiency. The properties of the plastic compound, such as thermal expansion and compressibility, determine the extent to which the molten plastic compound undergoes dimensional changes during the cooling phase. These dimensional changes occurring during the cooling phase are referred to as shrinkage, specifically processing shrinkage.

[0004] Other relevant shaping processes include extrusion and printing processes of additive manufacturing. Well-known processes include granular printing, powder printing, and filament printing. These processes are also referred to as 3D printing. In powder printing, a powder bed consisting of particles of a plastic composition, for example, a polyolefin, is prepared. The plastic composition is selectively melted by the application of energy, causing the particles in contact to fuse together. After a cooling phase, another layer of powder is applied to the existing powder bed and selectively melted in the same way. This process is repeated until a finished object is obtained.In filament printing or granular printing, a plastic compound in the form of a filament or granules is melted in a print head and arranged along a specific contour, where it then solidifies. The desired shape is obtained by layering several of the plastic compound on top of each other.

[0005] One disadvantage of polyolefin plastic compositions, however, is that they exhibit significant shrinkage after solidification in most molding processes. Polypropylene homopolymer is known to shrink by up to 2%. The shrinkage problem is further exacerbated by the fact that polyolefins exhibit a shrinkage differential in the longitudinal and transverse directions, which depends on the molding process.

[0006] The longitudinal direction is understood to be the spatial extent of the molded part, preferably starting at the gate point, which runs along an introduced anisotropy of polymer chains, particularly the amorphous regions, and / or fibers, along the flow direction of the molten polymer composition. In other words, polymer chains and / or fibers in a molded part are at least partially oriented longitudinally. The transverse direction is the spatial extent of the molded part that preferably runs perpendicular to the longitudinal direction.

[0007] The difference in shrinkage between the longitudinal and transverse directions not only results in molded parts with smaller dimensions, but also creates stresses within the molded parts, leading to warpage. This is due to a reduction in the anisotropy of the polymer chains and / or fibers, with greater shrinkage occurring in the longitudinal direction due to the higher orientation. For thermoplastic polymer compositions with glass fiber reinforcement, this observation is reversed. Shrinkage is lower in the direction of the glass fibers and higher perpendicular to them.

[0008] This means that in forming processes where tight dimensional tolerances are critical, the mold, for example, the tool cavity, must be adapted to the specific polyolefin composition and the specific forming process to ensure that the resulting molded part has precisely the required dimensions. Shrinkage is particularly problematic when a mold is specifically designed for a particular plastic composition and / or forming process, but the plastic composition is to be changed. While it is possible to partially compensate for this problem by increasing the cooling time, this reduces the production volume and thus the overall cost-effectiveness of the process.

[0009] In light of the aforementioned problem, there is a need for a plastic composition that exhibits low shrinkage even during short cooling phases. Furthermore, it is desirable that this plastic composition possesses improved mechanical properties such as high impact strength and notched impact strength, as well as high heat deflection temperature (HDT).

[0010] EP 3 212 713 B2 describes how low shrinkage of a polypropylene plastic composition can be achieved by adding a predominantly amorphous propylene-ethylene copolymer to a crystalline isotactic homopolymer. This results in a heterophase polypropylene plastic composition, and it is shown that the longitudinal dimensions of the samples exhibit lower shrinkage, between 0.96% and 1.05%, compared to samples in the reference examples. US 7,893,171 B2, in turn, describes a reduction in the difference between longitudinal and transverse shrinkage by adding a nucleating agent such as talc. More uniform shrinkage in all spatial directions reduces warpage in the final product.

[0011] WO 2020 / 058313 A1 discloses a mixture intended to achieve optimized notched impact strength and volumetric shrinkage. D3 does not contain 10-70 wt% flat fibers and does not have a ratio of "{shrinkage (polyolefin) - shrinkage (composition)} / shrinkage (polyolefin) ≥ 30%". D3 exhibits lower notched impact strength.

[0012] The object of the invention is to provide an improved plastic composition, wherein the plastic composition is used to produce a molded body that exhibits particularly low shrinkage. Furthermore, it is an object of the invention to provide a use for the improved plastic composition and a method for producing an improved molded body, wherein the improved molded body comprises the improved plastic composition.

[0013] The problem is solved by providing a plastic composition, in particular according to one of claims 1 to 12, wherein the plastic composition contains at least one polyolefin and at least one thermoplastic elastomer, wherein the at least one thermoplastic elastomer is a copolymer comprising at least one diene-based block A and at least one alpha-methylstyrene-based block B, wherein the ratio of the difference between the shrinkage of the polyolefin and the shrinkage of the plastic composition to the shrinkage of the polyolefin is at least 30%, wherein the shrinkages are determined in accordance with DIN ISO 294-4 ("Plastics - Injection molding of thermoplastic specimens - Part 4: Determination of processing shrinkage (ISO 294-4:2018); German version EN ISO 294-4:2019", issue date: 2019-04), wherein the plastic composition contains reinforcing fibers in an amount of 10 wt.% to 70 wt.%.-%, in each case based on the total weight of the plastic composition, containing the reinforcing fibers comprising glass fibers designed as flat fibers.

[0014] Furthermore, the problem is solved by providing a use of the plastic composition according to one of claims 1 to 10 in injection molding, extrusion or additive manufacturing.

[0015] Furthermore, the problem is solved by providing a method according to claim 14 for producing a molded body, wherein the method comprises at least the following steps: Providing a plastic composition according to any one of claims 1 to 9, and shaping the provided plastic composition into a molded body.

[0016] Shrinkage is preferably understood to mean shrinkage in the longitudinal direction and / or shrinkage in the transverse direction. Furthermore, shrinkage is preferably understood to mean processing shrinkage. Processing shrinkage is defined as the ratio of the difference between the mold dimensions and the molded part dimensions after 16 hours of storage in standard climate conditions (temperature: 23 °C, relative humidity: 50%) to the mold dimensions, expressed as a percentage. The molded part dimensions immediately after the molding process can be the molded part dimensions in the liquid state and can be determined by the mold dimensions.

[0017] In other words, the ratio of the difference between the shrinkage of the polyolefin and the shrinkage of the plastic composition to the shrinkage of the polyolefin can be calculated using the following equation (1): Δ % = PO − K PO

[0018] Here, PO represents the shrinkage of the polyolefins and K the shrinkage of the plastic composition, each expressed as a percentage. The result is the percentage difference Δ% of the shrinkage, which represents the degree to which the shrinkage of the plastic composition is improved compared to that of the polyolefin.

[0019] For example, if a polyolefin has a shrinkage of 2% and a corresponding plastic composition according to the invention has a shrinkage of 1.4%, the percentage difference is 30%. However, if the plastic composition has a shrinkage of 0.1% compared to the aforementioned polyolefin with a shrinkage of 2%, the percentage difference is 95%.

[0020] According to the invention, it is also possible to provide a molded body comprising the plastic composition according to claim 1, a use of the molded body, and a method for producing the plastic composition according to claim 1.

[0021] The present invention makes it possible to provide a plastic composition that can be used to manufacture molded parts. These molded parts exhibit high dimensional stability due to very low shrinkage, both longitudinally and transversely. This applies to plastic compositions with and without reinforcing fibers. In particular, for plastic compositions with reinforcing fibers, shrinkage perpendicular to the fiber can be reduced to a minimum. In other words, the plastic composition enables the production of molded parts with minimal distortion.

[0022] This offers the advantage that cycle times in molding processes can be shortened by reducing cooling time, thereby increasing the number of molded parts produced per unit of time. This allows molding processes to be made more economically efficient. Additionally, the process duration is significantly reduced if only a specific number of molded parts are to be produced. Thus, energy-intensive processes, such as keeping the plastic composition in a molten state, are only necessary for a shorter period, which also reduces the overall cost of the process.

[0023] Furthermore, the molded parts obtained from the plastic composition exhibit improved mechanical properties in addition to low shrinkage. Through the addition of the thermoplastic elastomer, as specified in claim 1, the molded parts, particularly those produced in bulk, exhibit very high impact strength and very high notched impact strength. Thus, robust molded parts for demanding applications can be obtained, thereby increasing the application possibilities of molded parts produced in high volumes.

[0024] Furthermore, the improved properties of the plastic composition make it possible to use it in a variety of processes. In 3D printing processes such as extrusion-deposition processes with granules, powder, or filament, the molten polymer is deposited onto a flat build plate made of epoxy resin, glass, or metal. If a plastic composition exhibits significant warpage, low heat resistance, or insufficient toughness, it will detach from the build plate, making printing impossible. However, the plastic composition according to the invention possesses the necessary combination of high heat resistance, high toughness, and low shrinkage to enable good build plate adhesion and warp-free parts.

[0025] Semicrystalline thermoplastics offer the advantage over amorphous thermoplastics of being stronger, harder, and tougher due to the formation of regular structures. Furthermore, they exhibit higher heat resistance and better chemical resistance. They thus display advantageous resistance to mechanical and chemical stresses. In contrast, amorphous thermoplastics are easier to process and, due to the lack of crystallization, exhibit less shrinkage. The described polymer composition now makes it possible to combine the aforementioned advantageous properties of semicrystalline thermoplastics with those of amorphous thermoplastics.

[0026] Further advantageous embodiments of the invention are specified in the dependent claims.

[0027] The polyolefin is preferably a semi-crystalline thermoplastic. The polyolefin can be linear or branched.

[0028] Furthermore, the polyolefin can be a homopolymer or a copolymer. In particular, the polyolefin can be a copolymer selected from the group consisting of statistical copolymer, gradient copolymer, alternating copolymer, block copolymer, graft copolymer, or mixtures thereof.

[0029] In a preferred embodiment, the polyolefin is selected from the group consisting of polypropylene (PP), in particular polypropylene homopolymer (PPH), polypropylene copolymer (PPC), or polypropylene random copolymer (PPR), polyethylene (PE), in particular high-density polyethylene (HDPE), low-density polyethylene (LDPE), linear low-density polyethylene (LLDPE), very low-density polyethylene (VLDPE), or medium-density polyethylene (MDPE), ethylene vinyl acetate copolymer (EVA), ethylene ethyl acrylate copolymer (EEA), ethylene butyl acrylate copolymer (EBA) and their copolymers and mixtures thereof.

[0030] The polyolefin is preferably selected from the group consisting of PP, in particular PPH, PPC, or PPR, PE, in particular HDPE, LDPE, LLDPE, VLDPE, or MDPE, and their copolymers and mixtures thereof.

[0031] Preferably, the polyolefin is selected from the group consisting of PPH, PPC, or PPR, and their copolymers and mixtures thereof. Even more preferably, the polyolefin is a PPH.

[0032] In a preferred embodiment, the plastic composition contains the polyolefin in an amount selected from the range of 25 wt.% to 99 wt.%, preferably from 35 wt.% to 96 wt.%, from 40 wt.% to 75 wt.%, in each case based on the total weight of the plastic composition.

[0033] In a preferred embodiment, the polyolefin has a glass transition temperature selected from the range of -100 °C to 100 °C, preferably from -80 °C to 50 °C, and more preferably from -70 °C to 30 °C.

[0034] The glass transition temperature is determined using methods known from the prior art by employing a dynamic-mechanical analysis at a frequency of 11 Hz in train mode as a function of temperature.

[0035] According to a preferred embodiment, the glass transition temperature is determined by means of dynamic mechanical analysis according to the method described in ISO 6721-11:2019-06 (“Plastics - Determination of dynamic mechanical properties - Part 11: Glass transition temperature”, issue date: 2019-06).

[0036] In a preferred embodiment, the plastic composition contains the thermoplastic elastomer in an amount of up to 75 wt.%, preferably up to 70 wt.%, more preferably up to 60 wt.%, and even more preferably up to 50 wt.%, in each case based on the total weight of the plastic composition.

[0037] The inventors have determined that above the specified amount of thermoplastic elastomer, the resistance of the plastic composition to oils and greases may decrease.

[0038] Furthermore, the plastic composition preferably contains the thermoplastic elastomer in an amount of at least 1 wt.%, preferably at least 4 wt.%, and more preferably at least 10 wt.%, in each case based on the total weight of the plastic composition.

[0039] Even the aforementioned minimal amount of thermoplastic elastomer ensures that the advantageous properties of reduced shrinkage and improved impact strength, as well as notched impact strength, obtained through the thermoplastic elastomer are enabled for the plastic composition.

[0040] The thermoplastic elastomer is preferably a block copolymer, particularly with a block sequence selected from the group consisting of AB, ABA, or BAB, or a graft copolymer. Preferably, in the graft copolymer, at least one block A is grafted onto at least one block B, or at least one block B is grafted onto at least one block A. According to a variation of the invention, the thermoplastic elastomer is a mixture of the aforementioned copolymers.

[0041] In a preferred embodiment, the at least one block A is selected from the group consisting of butadiene, isoprene, and combinations thereof. In a particularly preferred embodiment, the at least one block A is based on 1,3-butadiene.

[0042] The at least one block A is preferably at least partially hydrogenated. More preferably, the at least one block A is hydrogenated to at least 80%, more preferably to at least 95%, and even more preferably to 100%.

[0043] Preferably, the at least one block A of the thermoplastic elastomer has a glass transition temperature of at most 100 °C, more preferably at most 50 °C, and more preferably at most 30 °C. Alternatively or additionally, the glass transition temperature of the at least one block A of the thermoplastic elastomer may have a value selected from a range of -100 °C to 100 °C, more preferably from -80 °C to 50 °C, and even more preferably from -70 °C to 30 °C. The glass transition temperature is determined as described above by using a dynamic mechanical analysis.

[0044] In a preferred embodiment, the proportion of at least one block B in the thermoplastic elastomer is selected from a range of 15 wt.% to 45 wt.%, preferably 20 wt.% to 40 wt.%, and more preferably 30 wt.% to 32 wt.%, in each case based on the total weight of the thermoplastic elastomer. In a particularly preferred embodiment, the proportion of at least one block B in the thermoplastic elastomer is 31 wt.% based on the total weight of the thermoplastic elastomer.

[0045] In a preferred embodiment, the at least one block B of the thermoplastic elastomer has a glass transition temperature in the range of 120 °C to 230 °C, preferably from 140 °C to 215 °C, and more preferably from 160 °C to 170 °C. The glass transition temperature is determined as described above by means of a dynamic-mechanical analysis.

[0046] In particular, due to the high glass transition temperature of at least one block B, a crystallization process begins very quickly, preferably immediately, after the forming process when a molten plastic composition according to the invention cools, and the plastic composition solidifies, thereby enabling very low shrinkage.

[0047] In a preferred embodiment of the thermoplastic elastomer, the thermoplastic elastomer is a block copolymer, wherein block A is based on 1,3-butadiene, wherein at least one block A is hydrogenated to at least 80%, more preferably at least 95%, and more preferably 100%, and wherein the at least one block B is selected from a range of 15 wt.% to 45 wt.%, more preferably from 20 wt.% to 40 wt.%, more preferably from 30 wt.% to 32 wt.%, and more preferably from 31 wt.%, in each case based on the total weight of the thermoplastic elastomer, and wherein the thermoplastic elastomer has a glass transition temperature from a range of 120 °C to 230 °C, more preferably from 140 °C to 215 °C, and more preferably from 160 °C to 170 °C.

[0048] According to a preferred embodiment, the thermoplastic elastomer has a melt flow index value at 230 °C and a load of 2.16 kg selected from a range of 3 g / 10 min to 7 g / 10 min, preferably from 5 g / 10 min to 6 g / 10 min, in particular according to the method described in DIN EN ISO 1133-1:2012-03 (“Plastics - Determination of melt mass flow rate (MFR) and melt volume flow rate (MVR) of thermoplastics - Part 1: General test method (ISO 1133-1:2011); German version EN ISO 1133-1:2011”, Publication date: 2012-03).

[0049] An advantage of the above range of the melt flow index of the thermoplastic elastomer is that it corresponds to the order of magnitude of the melt flow index relevant for the plastic composition according to the invention. Thus, the processability of the plastic composition in the molten state is not negatively affected by the addition of the thermoplastic elastomer.

[0050] In a preferred embodiment, the ratio of the difference between the longitudinal shrinkage of the polyolefin and the longitudinal shrinkage of the plastic composition to the longitudinal shrinkage of the polyolefin has a value of at least 30%, at least 40%, and at least 50%, wherein the shrinkages are determined in accordance with DIN ISO 294-4.

[0051] Further preferably, the ratio of the difference between the longitudinal shrinkage of the polyolefin and the longitudinal shrinkage of the plastic composition to the longitudinal shrinkage of the polyolefin has a value selected from a range of 30% to 100%, more preferably from 35% to 98%, even more preferably from 40% to 90%, and even more preferably from 50% to 80%, wherein the shrinkages are determined in accordance with DIN ISO 294-4.

[0052] The percentage values ​​listed in the two preceding paragraphs correspond to the percentage difference in the longitudinal direction Δ% L and can be determined by the following equation (2): Δ% L = PO L − K L PO L

[0053] PO L corresponds to the value of the shrinkage of the polyolefin in the longitudinal direction and KL to the value of the shrinkage of the plastic composition in the longitudinal direction, each given in percent.

[0054] In a further preferred embodiment, the ratio of the difference between the shrinkage of the polyolefin in the transverse direction and the shrinkage of the plastic composition to the shrinkage of the polyolefin in the transverse direction has a value of at least 30%, at least 40%, at least 50%, wherein the shrinkages are determined in accordance with DIN ISO 294-4.

[0055] Further preferably, the ratio of the difference between the shrinkage of the polyolefin in the transverse direction and the shrinkage of the plastic composition in the longitudinal direction to the shrinkage of the polyolefin in the transverse direction has a value selected from a range of 30% to 100%, more preferably from 35% to 98%, even more preferably from 40% to 90%, and even more preferably from 50% to 80%, wherein the shrinkages are determined in each case according to DIN ISO 294-4.

[0056] The percentage values ​​listed in the two preceding paragraphs correspond to the percentage difference in the transverse direction Δ% Q and can be determined by the following equation (2): Δ % Q = PO Q − K Q PO Q

[0057] POQ corresponds to the value of the shrinkage of the polyolefin in the longitudinal direction and KQ to the value of the shrinkage of the plastic composition in the longitudinal direction, each given in percent.

[0058] Typically, unfilled semi-crystalline thermoplastics exhibit shrinkage values ​​in the longitudinal and / or transverse direction according to DIN EN ISO 294-4 between 1% and 2.5%, preferably between 1% and 2%, with shrinkage in the longitudinal direction being more pronounced.

[0059] In a further preferred embodiment, the plastic composition has a longitudinal shrinkage value selected from a range of 0% to 0.7%, preferably 0.1% to 0.5%, or more preferably 0.2% to 0.3%, according to the method described in DIN EN ISO 294-4. Additionally or alternatively, the plastic composition has a transverse shrinkage value selected from a range of 0% to 0.7%, preferably 0.1% to 0.5%, or more preferably 0.2% to 0.3%, according to the method described in DIN EN ISO 294-4.

[0060] Due to the low shrinkage, especially the low shrinkage in the longitudinal and transverse directions, it is possible to provide molded parts with very low distortion.

[0061] Thus, it is possible that the plastic composition in the form of a plate-shaped injection-molded body with dimensions of width: 150 mm, length: 100 mm and height: 2 mm has a value for warpage selected from a range of 0 mm to 10 mm, preferably from 0.01 mm to 7 mm, more preferably from 0.1 mm to 3.5 mm.

[0062] To determine the warpage, the plate-shaped injection molded part is placed on a flat surface. One corner of the part is then pressed onto the surface in succession, bringing it into contact with the surface. The maximum possible distance between the diagonally opposite corners of the plate-shaped injection molded part, perpendicular to the plane defined by the surface, is measured.

[0063] The low warpage of the plastic composition allows for the production of molded parts with high dimensional accuracy. Combined with the good chemical resistance of semi-crystalline thermoplastics, this makes it possible, for example, to produce precisely fitting pipes and conduits for solid, liquid, and / or gaseous media without the risk of corrosion from the media or leakage at the joints.

[0064] In a further preferred embodiment, the plastic composition has a Charpy impact strength value according to the method described in DIN EN ISO 179-1:2010-11 ("Plastics - Determination of Charpy impact properties - Part 1: Non-instrumented impact test (ISO 179-1:2010); German version EN ISO 179-1:2010", issue date: 2010-11) of at least 16 kJ / m², preferably selected from the range of 16 kJ / m² to 100 kJ / m², more preferably from 25 kJ / m² to 80 kJ / m², and even more preferably from 30 kJ / m² to 65 kJ / m².

[0065] In a further preferred embodiment, the plastic composition has a Charpy impact strength value according to the method described in DIN EN ISO 179-1:2010-11 of at least 16 kJ / m², preferably selected from the range of 16 kJ / m² to 100 kJ / m², more preferably from 30 kJ / m² to 85 kJ / m², and even more preferably from 40 kJ / m² to 65 kJ / m².

[0066] In a further preferred embodiment, the plastic composition has a value for notched impact strength according to Izod as described in DIN EN ISO 180:2020-03 (“Plastics - Determination of Izod impact strength (ISO 180:2019); German version EN ISO 180:2019”, issue date: 2020-03) of at least 16 kJ / m², preferably selected from the range of 16 kJ / m² to 100 kJ / m², more preferably from 30 kJ / m² to 85 kJ / m², and even more preferably from 40 kJ / m² to 65 kJ / m².

[0067] The aforementioned impact strength and non-concrete impact strength values ​​ensure that the plastic composition according to the invention exhibits outstanding resistance to mechanical stress. This resistance is achieved through the addition of the thermoplastic elastomer.

[0068] Specimens that do not break into two pieces, bend, and / or elastically rebound after impact testing, despite a notch, are designated as "NB" (non-broken). In a preferred embodiment, specimens that do not break during the determination of notched impact strength and impact strength at a load of less than 80 kJ / m² are designated as "NB".

[0069] In a further preferred embodiment, the plastic composition has a heat deflection temperature (HDT) value according to Method B of DIN EN ISO 75-1:2020-06 ("Plastics - Determination of heat deflection temperature - Part 1: General test method (ISO 75-1:2020); German version EN ISO 75-1:2020", Publication date: 2020-06) and DIN EN ISO 75-2:2013-08 ("Plastics - Determination of heat deflection temperature - Part 2: Plastics and hard rubber (ISO 75-2:2013); German version EN ISO 75-2:2013", Publication date: 2013-08) of at least 60 °C, preferably selected from the range of 60 °C to 200 °C, more preferably from 80 °C to 180 °C, and even more preferably from 130 °C to 165 °C. The heat deflection temperature determined according to method B is abbreviated as HDT-B in the following.

[0070] In method B, a force of 0.45 N / mm² per area is applied to the specimen using weights and / or springs.

[0071] A key advantage is that the plastic composition, even with a proportion of, for example, 15 wt.% to 20 wt.% thermoplastic elastomer, exhibits high heat resistance, particularly in addition to its high toughness. This is surprising, as the addition of a conventional elastomer would typically result in a reduction of the heat resistance. The high heat resistance, especially in combination with the low warpage, achieves the beneficial effect of making the plastic composition very well suited for 3D printing processes, as it prevents detachment from the build plate during the process.

[0072] The plastic composition contains reinforcing fibers: 10 wt.% to 70 wt.%, based on the total weight of the plastic composition, wherein the reinforcing fibers comprise flat glass fibers.

[0073] In particular, the plastic composition contains reinforcing fibers in an amount of 10 to 70 wt.%, preferably up to 50 wt.%, and more preferably up to 40 wt.%, based on the total weight of the plastic composition. Furthermore, the plastic composition can contain reinforcing fibers selected from the range of 10 wt.% to 70 wt.%, preferably from 10 wt.% to 50 wt.%, and more preferably from 15 wt.% to 40 wt.%, in each case based on the total weight of the plastic composition.

[0074] The quantity of reinforcing fibers described above ensures that the shrinkage of the plastic composition is reduced by the glass fibers without significantly impairing the processability of the plastic composition.

[0075] The flat fibers preferably have a thickness-to-width form factor selected from a range of 1:1.5 to 1:5, preferably 1:2 to 1:4, more preferably 1:2.5 to 1:3.5.

[0076] The use of glass fibers offers the advantage that shrinkage can be further reduced cost-effectively. In particular, the use of flat fibers offers the advantage that not only is overall shrinkage reduced, but also, due to the form factor described above, the orientation of the fibers is reduced. Flat fibers thus preferably exhibit a statistical distribution of orientation. This further reduces the difference between shrinkage in the longitudinal and transverse directions.

[0077] In a preferred embodiment, the plastic composition does not contain any mineral fillers, and glass is not a mineral filler within the meaning of the invention.

[0078] Fillers are defined as materials that have a weight fraction of over 5% based on the total weight of the plastic composition and are present undissolved in the plastic composition.

[0079] Mineral fillers include, for example, silicates, sulfates, carbonates, or mixtures thereof. Preferably, the plastic composition does not contain layered silicates such as talc, chalk, rock flour, or mixtures thereof.

[0080] In a preferred embodiment, the plastic composition does not include any filler, in particular a mineral filler, with a thickness-to-width ratio of less than 1:1.5, preferably less than 1:1.3.

[0081] Mineral fillers are commonly used to minimize the shrinkage of plastic compounds because they reduce the differences between longitudinal and transverse shrinkage. However, mineral fillers reduce overall shrinkage to a lesser extent compared to, for example, reinforcing fibers. Therefore, to achieve a noticeable effect relative to the total weight of the plastic compound, mineral fillers must be used in large proportions. Even with high proportions of mineral fillers below 0.7% to 1.5% in either the longitudinal and / or transverse direction, shrinkage is usually not reduced. This slight improvement in shrinkage, however, leads to several negative properties. For instance, mineral fillers typically have a higher density compared to polymers, resulting in heavier final products.Furthermore, they exhibit poor toughness and impact strength and reduce the scratch resistance of the plastic composition.

[0082] It is also possible that the plastic composition includes at least one additive selected individually or in combination from the group consisting of stabilizer, light stabilizer, flame retardant, hydrophobic agent, plasticizer, antioxidant, colorant, pigment, antistatic agent, silicone oils, demolding agent or release agent.

[0083] Additives are defined as materials that constitute less than 5% by weight of the total weight of the plastic composition. Additives can be dissolved or undissolved within the plastic composition.

[0084] Preferably, the plastic composition comprises at least one additive selected from a proportion of up to 5 wt%, preferably up to 3 wt%, and more preferably up to 2 wt%, based on the total weight of the plastic composition. The addition of additives allows desired properties of the plastic composition to be adjusted without negatively affecting its mechanical properties. In a preferred embodiment, the plastic composition has the following composition, wherein the components of the plastic composition are selected to total 100 wt%: Polyolefin: 30% to 96% by weight, Thermoplastic elastomer: 4% by weight to 70% by weight, Reinforcing fiber: 10 wt.% to 50 wt.%, Additives: 0 wt.% to 3 wt.%, preferred: Polyolefin: 40% to 75% by weight, Thermoplastic elastomer: 10 wt.% to 60 wt.% Reinforcing fiber: 15% to 40% by weight, Additives: 0 wt.% to 2 wt.%.

[0085] In a preferred embodiment of the composition described above, the polyolefin is a PP, preferably PPH. In a further preferred embodiment, the polyolefin is a PE, preferably an HDPE, LDPE, LLDPE, VLDPE or MDPE.

[0086] In a preferred embodiment of the composition described above, the thermoplastic elastomer is a block copolymer wherein block A is based on 1,3-butadiene, wherein at least one block A is hydrogenated to at least 80%, more preferably at least 95%, and more preferably 100%, and wherein the at least one block B is selected from a range of 15 wt.% to 45 wt.%, more preferably from 20 wt.% to 40 wt.%, more preferably from 30 wt.% to 32 wt.%, and more preferably from 31 wt.%, in each case based on the total weight of the thermoplastic elastomer, and wherein the thermoplastic elastomer has a glass transition temperature from a range of 120 °C to 230 °C, more preferably from 140 °C to 215 °C, and more preferably from 160 °C to 170 °C.

[0087] In a preferred embodiment of the composition described above, the reinforcing fibers are glassy flat fibers, in particular with a shape factor of thickness to width selected from a range of 1:1.5 to 1:5, preferably from 1:2 to 1:4, more preferably from 1:2.5 to 1:3.5.

[0088] In a particularly preferred embodiment, the plastic composition contains the thermoplastic elastomer in an amount selected from the range of 1 wt.% to 75 wt.%, preferably from 4 wt.% to 70 wt.%, more preferably from 10 wt.% to 60 wt.%, the polyolefin in an amount selected from the range of 25 wt.% to 99 wt.%, preferably from 35 wt.% to 96 wt.%, from 40 wt.% to 75 wt.%, and flat glass fibers in an amount selected from the range of 10 wt.% to 70 wt.%, preferably from 10 wt.% to 50 wt.%, each based on the total weight of the plastic composition, wherein the proportions of the composition are selected such that they total 100 wt.%.-% of the plastic composition, wherein the thermoplastic elastomer is a block copolymer, wherein the at least one block A is based on 1,3-butadiene, wherein the at least one block A is hydrogenated to at least 80%, more preferably to 100%, and wherein the at least one block B is selected from a range of 15 wt.% to 45 wt.%, preferably from 20 wt.% to 40 wt.%, more preferably from 31 wt.%, in each case based on the total weight of the thermoplastic elastomer, and wherein the thermoplastic elastomer has a glass transition temperature from a range of 120 °C to 230 °C, preferably from 140 °C to 215 °C, more preferably from 160 °C to 170 °C, and wherein the polyolefin is a polypropylene homopolymer.

[0089] In a further particularly preferred embodiment, the plastic composition contains the thermoplastic elastomer in an amount selected from the range of 1 wt.% to 75 wt.%, preferably from 4 wt.% to 70 wt.%, more preferably from 10 wt.% to 60 wt.%, the polyolefin in an amount selected from the range of 25 wt.% to 99 wt.%, more preferably from 35 wt.% to 96 wt.%, from 40 wt.% to 75 wt.%, in each case based on the total weight of the plastic composition, wherein the proportions of the composition are selected such that they together constitute 100 wt.% of the plastic composition, wherein the thermoplastic elastomer is a block copolymer, wherein the at least one block A is based on 1,3-butadiene, wherein the at least one block A is hydrogenated to at least 80%, more preferably to 100%, and wherein the at least one block B is selected from a range of 15 wt.% to 45 wt.%, more preferably from 20 wt.% to 40 wt.%.-%, further preferably 31 wt%, in each case based on the total weight of the thermoplastic elastomer, and wherein the thermoplastic elastomer has a glass transition temperature in the range of 120 °C to 230 °C, preferably from 140 °C to 215 °C, further preferably from 160 °C to 170 °C, and wherein the polyolefin is a polypropylene homopolymer.

[0090] The plastic composition is preferably provided by supplying and mixing the respective components, in particular at least the polyolefin and / or the thermoplastic elastomer, each in a dosage form selected from the group consisting of powder, grits, pellets, granules (preferably cylindrical granules, cube granules, cylindrical granules, lenticular granules, or splinter granules), and filament. The mixing of the polyolefin and the thermoplastic elastomer can be carried out by means of an extruder (in particular a twin-screw extruder), a kneader (in particular a roller kneader), a static mixer, a dynamic mixer, an injection molding machine, or a combination thereof, whereby the plastic composition is obtained. According to a preferred embodiment, the mixing is carried out on an injection molding machine with a dynamic mixer or with a static mixer.

[0091] Furthermore, it is possible that an optional manufacturing process, in particular a forming process, a separation process, or a coating process, is carried out after mixing. This allows the dosage form of the plastic composition to be adapted and optimized for the intended use.

[0092] In a preferred embodiment, the plastic composition is in a dosage form selected from the group consisting of powder, grits, crumbs, pellets, granules, and filaments. The granules can be in the form of cylindrical granules, cube granules, cylindrical granules, lenticular granules, or splinter granules.

[0093] The plastic composition can be used in a variety of manufacturing processes, in particular injection molding, extrusion, granulation, printing, especially filament printing, powder printing and / or granule printing, in particular the plastic composition is formed into the molded body when the above processes are carried out.

[0094] A molded body comprising the plastic composition can be used in a wide variety of technically demanding fields. It is particularly favored in power tools, automotive engineering, electrical engineering, aerospace, shipbuilding, power plants, chemical industry plants, medical technology, electromobility, and / or refrigeration systems.

[0095] The plastic composition may be in the form of a molded body. Preferably, the molded body is an injection-molded part, an extrudate, or a printed part.

[0096] Furthermore, it is possible that the molded body exists as a conduit, pipe, connecting element, body part, dashboard, drill housing, housings and shafts for the construction industry, rotor, bearing, casing, gear or nozzle.

[0097] The invention is explained below by way of example using several embodiments and the accompanying drawing. The embodiments shown are only examples and are therefore not to be understood as limiting. Fig. 1 shows a thermogram for determining the glass transition temperature.

[0098] Fig. 1Figure 1 shows a thermogram for determining the glass transition temperature, the data sets of which were generated using dynamic mechanical analysis at a frequency of 11 Hz in tensile mode. Specifically, the glass transition temperature was determined using dynamic mechanical analysis according to the method described in ISO 6721-11:2019-06. The left y-axis shows the base-10 logarithm of the Young's modulus (log(E') in 10⁻⁵ N / cm²) as a function of temperature T in °C. The right y-axis shows the dimensionless loss angle (tan δ) as a function of temperature T in °C, which describes the damping properties. The black arrows on the measurement curves indicate the corresponding axes.

[0099] The unfilled circles and triangles show the profile of a conventional styrene-ethylene-butylene-styrene (SEBS). This thermoplastic elastomer is a copolymer and has a styrene-based block and an ethylene-butylene-based block.

[0100] The filled circles and triangles show the profile of a thermoplastic elastomer, where the thermoplastic elastomer was a copolymer and comprised at least one diene-based block A and one alpha-methylstyrene (AMS)-based block B. For the diene of block A, the following was observed in Fig. 1 The thermoplastic elastomer shown is 100% hydrogenated 1,3-butadiene, with the proportion of at least one block B being 31 wt% based on the total weight. This polymer was thus a thermoplastic elastomer of the subgroup thermoplastic styrene block copolymers (TPS) based on alpha-methylstyrene and is referred to below and in the legend of the Fig. 1 referred to as TPS-AMS.

[0101] The in Fig. 1 The thermoplastic elastomer shown exhibited a melt flow index value at 230 °C and a load of 2.16 kg selected from a range of 5.6 g / 10 min, in particular according to the method described in DIN EN ISO 1133-1:2012-03.

[0102] The thermogram revealed two significant temperature-dependent changes in the logarithmically plotted Young's modulus for each type of thermoplastic elastomer (see triangular symbols). Furthermore, two temperature-dependent changes in the damping properties (tan δ) were also evident for each type (see circular symbols).

[0103] The glass transition temperatures of the respective polymer blocks could be determined from the respective maxima of tan δ. Both thermoplastic elastomers exhibited a maximum at approximately -30 °C, which can be attributed to the block based on polyolefins. Furthermore, both thermoplastic elastomers exhibited another maximum at higher temperatures, which could be attributed to the glass transition temperature of the block based on styrene in the case of conventional SEBS and on alpha-methylstyrene in the case of the thermoplastic elastomer of the inventive polymer composition.

[0104] From the curve's progression Fig. 1 It was determined that the styrene-based block of conventional SEBS thus exhibited a glass transition temperature of approximately 100 °C. The block of the thermoplastic elastomer based on alpha-methylstyrene of the plastic composition according to the invention showed, Fig. 1a glass transition temperature of 160 °C to 170 °C.

[0105] Table 1 shows essential material parameters of polyolefins that are available and can be used as conventional plastic compositions. Table 2 further shows essential material parameters of a glass fiber-reinforced plastic composition of a polyolefin, which has 30 wt.% reinforcing fibers in the form of glass fibers with a spherical cross-section, based on the total weight of the plastic composition. The polyolefins shown in Tables 1 and 2 are intended to serve as comparative examples for the plastic compositions according to the invention. The abbreviation "na" represents values ​​that were not available. Table 1: Conventional plastic compositions based on polypropylene homopolymer (PPH) as polyolefin (PO) and their properties as a reference material and / or starting material for the plastic composition according to the invention. PO1 PO2 PO3 PO4 PO5 Type of PO PPH PPH PPH PPH PPH Melting flow index / g / 10 min 3,1 6,0 23 48 12 Shrinkage / % 1,2 / 1,5 1 / 1,1 0,9 / 1 1 / 1 1 / 1,11 Charpy impact strength / kJ / m² 4 3,5 3 3 3,3 Impact strength (Charpy) / kJ / m² < 145 140 91 87 115 Heat deflection temperature (HDT-B) / °C 115 55 105 105 110 Table 2: Conventional plastic composition comprising reinforcing fibers (round fibers) based on polypropylene homopolymer (PPH) as polyolefin (PO) and their properties as a reference material and / or starting material for the plastic composition according to the invention. POG1 Type of PO PPH Percentage of reinforcing fibers / wt.% 30 Shrinkage / % 0,2 / 0,8 Distortion / mm 16,45 Impact strength (Izod) / kJ / m²< 10,4 Charpy impact strength / kJ / m² 10 Impact strength (Charpy) / kJ / m² < 48,4 Heat deflection temperature (HDT-B) / °C 159

[0106] Tables 3 and 4 show essential material parameters of plastic compositions A1 to A4 and B1 to B7, which comprised at least one polyolefin and at least one thermoplastic elastomer according to claim 1. In plastic compositions A1 to A4 and B1 to B5, the polyolefin was a polypropylene homopolymer (PPH). In plastic compositions B6 and B7, the polyolefin was a mixture of polypropylene homopolymer (PPH) at 85 wt.% and linear low-density polyethylene (LLDPE) at 15 wt.%. The thermoplastic elastomer was a thermoplastic styrene block copolymer and contained at least one diene-based block A and at least one alpha-methylstyrene-based block B. In this specific case, the plastic composition comprised the TPS-AMS, which is shown in thermogram of Fig. 1The plastic compositions A1 to A4 according to Table 3 contained the thermoplastic elastomer in a proportion of between 25 wt.% and 60 wt.%, respectively, based on the total weight of the plastic composition.

[0107] The plastic compositions B1 to B7 according to Table 4 contained the thermoplastic elastomer in a proportion of between 5 wt% and 25 wt%, based on the total weight of the plastic composition. Additionally, the plastic compositions B1 to B7 contained reinforcing fibers in the form of flat glass fibers, with the proportion of reinforcing fibers varying between 15 wt% and 20 wt%, based on the total weight of the plastic composition.

[0108] The melt flow indices of the plastic compositions described in Tables 1 to 4 were determined at 230 °C and a load of 2.16 kg, in particular according to the method described in DIN EN ISO 1133-1:2012-03.

[0109] Plastic compositions with a melt flow index greater than 3 g / 10 min are particularly well-suited for extrusion and / or injection molding processes due to their lower viscosity. Plastic compositions used in injection molding and extrusion processes are subjected to stresses that lead to increased orientation of the polymer chains. This orientation, in turn, results in increased shrinkage. Such plastic compositions typically exhibit shrinkage of up to 2% in both the longitudinal and transverse directions, which translates into reduced dimensional accuracy of the molded parts. Plastic compositions with a melt flow index greater than 3 g / 10 min are also very well-suited for printing processes, such as filament printing.

[0110] The longitudinal and transverse shrinkages were determined using the method described in DIN ISO 294-4, where the initial dimensions of an injection-molded plate were as follows: width: 61 mm, length: 61 mm, height: 2 mm.

[0111] The distortion of the respective plastic composition was determined on a plate with the initial dimensions of width: 150 mm, length 100 mm, height: 2 mm as explained above.

[0112] The notched impact strengths and Charpy impact strengths of the plastic compositions according to Tables 1 to 4 were determined at 23 °C using the respective method described in DIN EN ISO 179-1:2010-11.

[0113] The Izod impact strengths were determined at 23 °C using the method described in DIN EN ISO 180:2020-03.

[0114] The abbreviation "NB" was chosen for the determination of impact strength and notched impact strength for specimens that did not break into two pieces, bend, and / or spring back elastically after impact testing, despite a notch. In a preferred embodiment, specimens that did not break during the determination of notched impact strength and impact strength at a load of less than 80 kJ / m² were classified as "NB".

[0115] The heat deflection temperature (HDT) according to Method B was determined in accordance with DIN EN ISO 75-1:2020-06 and DIN EN ISO 75-2:2013-08 and is abbreviated as HDT-B. In Method B, a force of 0.45 N / mm² per area is applied to the specimen using weights and / or springs.

[0116] The plastic compositions A1 to A4 and B1 to B7 were provided by supplying and mixing the respective components, in particular at least the polyolefin and / or the thermoplastic elastomer, as granules, powder, flakes or crumbs.

[0117] The polyolefin and the thermoplastic elastomer were mixed using a twin-screw extruder and a roller kneader, resulting in the plastic compositions A1 to A4 and B1 to B7.

[0118] The plastic compositions obtained, A1 to A4 and B1 to B7, were in granular form.

[0119] Subsequently, molded bodies in the form of test specimens were formed from the plastic composition in order to determine the parameters specified in Tables 3 and 4. Table 3: Plastic compositions containing at least polypropylene homopolymer (PPH) as polyolefin (PO) and TPS-AMS (na: not available). A1 A2 A3 A4 Type of PO PPH PPH PPH PPH Percentage of TPS-AMS / wt.% 60 40 30 25 Melting flow index / g / 10 min 12 12 3,1 3,1 Shrinkage / % 0,4 / 0,5 0,7 / 0,7 0,5 / 0,6 0,6 / 0,9 Impact strength (Izod) / kJ / m²< 55 60 63 60 Charpy impact strength / kJ / m² n / a 81 NB 70 Impact strength (Charpy) / kJ / m² < NB NB NB NB Heat resistance (HDT-B) / °C 61 66 73 n / a use Injection molding Injection molding Filament printing, granule printing, extrusion Filament printing, granule printing, extrusion Table 4: Plastic compositions according to the invention, containing polypropylene homopolymer (PPH) and / or linear low-density polyethylene as polyolefin (PO) and TPS-AMS, wherein the plastic compositions additionally contained reinforcing fibers (flat fibers) (na: not available). B1 B2 B3 B4 B5 B6 B7 Type of PO PPH PPH PPH PPH PPH PPH / LLDPE PPH / LLDPE Percentage of TPS-AMS / wt% 5 10 15 15 20 15 20 Percentage of reinforcing fibers / wt.% 50 50 50 30 50 25 15 Shrinkage / % 0,1 / 0,4 0,1 / 0,3 0 / 0,05 0 / 0,3 0,1 / 0,3 0,2 / 0,4 0,2 / 0,4 Distortion / mm 0,25 0,18 0,03 n / a n / a 3,08 3,5 Impact strength (Izod) / kJ / m²< 18 23 26 26 28 36 34 Charpy impact strength / kJ / m² < 19 22 25 26 28 39 33 Impact strength (Charpy) / kJ / m² < 73 80 75 73 70 88 76 Heat resistance (HDT-B) / °C 162 161 158 158 158 141 134 use Injection molding Injection molding Injection molding Injection molding Injection molding Extrusion Extrusion

[0120] The parameters shown in Tables 3 and 4 demonstrate that the plastic compositions according to the invention exhibited very low shrinkage. The measured shrinkage of plastic compositions A1 to A4 was only 0.4% to 0.7% in the longitudinal direction and 0.5% to 0.9% in the transverse direction.

[0121] Thus, the measured shrinkages were lower than the typical shrinkages expected above for semi-crystalline thermoplastics. Rather, they were within the range considered typical for the shrinkage of amorphous thermoplastics.

[0122] The addition of reinforcing fibers further reduced the shrinkage of the plastic composition. This is evident from the shrinkage values ​​determined for plastic compositions B1 to B7. Plastic compositions B6 and B7, which contained polyolefin mixtures of PPH and LLDPE, exhibited the highest values ​​of the plastic compositions listed in Table 4, at 0.2% in the longitudinal direction and 0.4% in the transverse direction. The proportion of thermoplastic elastomer was 15% or 20% by weight, and the proportion of flat glass fibers was 25% or 15% by weight, respectively, based on the total weight of the plastic composition. It should be noted, however, that plastic compositions B6 and B7 also exhibited the highest impact strength values ​​within the group of plastic compositions B1 to B7.Particularly noteworthy are the plastic compositions B3 and B4, in which no longitudinal shrinkage was measurable. These plastic compositions each contained 15 wt% thermoplastic elastomer and 50 wt% or 30 wt% glass fibers, respectively, based on the total weight of the plastic composition. In the transverse direction, shrinkage was only 0.05% and 0.3%, respectively.

[0123] The following comparison is made between the plastic compositions according to the invention in Tables 3 and 4 and the conventional plastic compositions.

[0124] Here, the plastic compositions A1 and A2 of Table 3 were based on the polyolefin of the plastic composition PO5 of Table 1, with the plastic compositions A1 and A2 additionally including the thermoplastic elastomer according to Fig. 1exhibited the following characteristics: The plastic compositions A3 and A4 of Table 3 were based on the polyolefin of the plastic composition PO1 of Table 1, with plastic compositions A3 and A4 additionally including the thermoplastic elastomer according to Fig. 1 exhibited.

[0125] The plastic compositions A1, A2, A3, and A4 all exhibited reduced shrinkage in both the longitudinal and transverse directions compared to the plastic compositions PO1 and PO5, which consisted solely of a polyolefin. According to equations (2) and (3), longitudinal shrinkage could be reduced by at least 30% to 60%, while transverse shrinkage could be reduced by at least 36% to 55%.

[0126] In other words, the plastic compositions according to the invention, comprising a polyolefin and the thermoplastic elastomer, wherein the thermoplastic elastomer was a thermoplastic styrene block copolymer having at least one diene-based block A and at least one alpha-methylstyrene-based block B, exhibited reduced shrinkage compared to plastic compositions containing only the polyolefin. Table 5: Comparison of a conventional plastic composition with plastic compositions according to the invention with respect to shrinkage in the longitudinal direction and in the transverse direction, calculated according to equations (2) and (3). A1 / PO5 A2 / PO5 A3 / PO1 A4 / PO1 Shrinkage ratio (longitudinal direction) 60% 30% 58% 50% Shrinkage ratio (transverse direction) 55% 36% 50% 47%

[0127] Table 6 shows, for comparison, the shrinkage of plastic compositions with glass reinforcing fibers. For this purpose, the inventive plastic compositions B3, B4 and B5 from Table 4 and the plastic composition PPG1 from Table 2 were used, with plastic compositions B3, B4 and B5 additionally including the thermoplastic elastomer according to Fig. 1 exhibit.

[0128] The plastic compositions B3, B4 and B5 all exhibit reduced shrinkage in the longitudinal and transverse directions compared to the plastic composition PPG1, which consists only of a glass fiber reinforced polyolefin. Table 6: Comparison of the reduction in shrinkage in the longitudinal and transverse directions of a conventional glass fiber reinforced plastic composition with plastic compositions according to the invention, wherein these have reinforcing fibers. Values ​​calculated according to equations (2) and (3). B3 / PPG1 B4 / PPG1 B5 / PPG1 Shrinkage ratio (longitudinal direction) 100 % 100 % 50 % Ratio (transverse direction) 94 % 63 % 63 %

[0129] Comparing the warpage of plastic composition B3 and PPG1 reveals that, in addition to shrinkage, the warpage of plastic composition B3 (0.03 mm) was more than an order of magnitude lower than that of plastic composition PPG1 (16.45 mm), or virtually non-existent. This was surprising, as the reinforcing fibers in plastic composition PPG1 were expected to exhibit less warpage compared to an unreinforced plastic composition.

[0130] Furthermore, the heat deflection temperature (HDT-B) of the plastic compositions B3, B4, and B5 differed by only 1 °C from that of PPG1, with a value of 158 °C. This high value, or rather the small difference, was surprising, since the plastic compositions contained the thermoplastic elastomer at a proportion of 15 wt.% or 20 wt.% by weight of the total weight of the plastic composition, and a reduction in heat deflection temperature would have been expected with the addition of a conventional elastomer. Instead, it showed that the heat deflection temperature (HDT-B) was almost independent of the addition of the thermoplastic elastomer.

[0131] The parameters shown in Tables 3 and 4 also clearly demonstrate that components made from the compositions according to the invention exhibited very good properties. For example, they were very impact-resistant and notched-impact-resistant, especially compared to conventional plastic compositions.

[0132] In summary, as described above, the plastic composition according to the invention made it possible to produce molded parts that exhibited high dimensional stability due to very low shrinkage, both longitudinally and transversely, as well as low distortion, particularly compared to conventional plastic compositions. This was likely due to the high glass transition temperature of the thermoplastic elastomer according to claim 1, which resulted in very rapid crystallization and solidification after injection of the molten plastic composition. Furthermore, in addition to low shrinkage, the molded parts obtained from the plastic composition exhibited improved mechanical properties such as high impact strength and high notched impact strength, which were also attributable to the addition of the thermoplastic elastomer.Thus, it was possible to obtain a plastic composition that exhibited the advantageous properties of semi-crystalline thermoplastics, as well as the easy processability and low shrinkage typical of amorphous thermoplastics.

[0133] Naturally, the listed design variants can be combined in any way and do not represent a limitation.

Claims

1. Polymer composition containing at least one polyolefin and at least one thermoplastic elastomer, wherein the at least one thermoplastic elastomer is a copolymer having at least one diene-based block A and at least one alpha-methylstyrene-based block B, wherein the ratio of the difference between the shrinkage of the polyolefin and the shrinkage of the polymer composition to the shrinkage of the polyolefin has at least a value of 30%, where the shrinkages are determined to DIN ISO 294-4, wherein the polymer composition contains reinforcing fibres in an amount of 10% by weight to 70% by weight, based in each case on the total weight of the polymer composition, where the reinforcing fibres comprise glass fibres configured as flat fibres.

2. Polymer composition according to Claim 1, characterized in that the reinforcing fibres are glass fibres.

3. Polymer composition according to Claim 1 or 2, characterized in that the glass fibres are flat fibres that preferably have a form factor of thickness to width from a range from 1:1.5 to 1:5.

4. Polymer composition according to any of the preceding claims, characterized in that the polyolefin is selected from the group consisting of polypropylene (PP), especially polypropylene homopolymer (PPH), polypropylene copolymer (PPC), or polypropylene random copolymer (PPR), polyethylene (PE), in particular high-density polyethylene (HDPE), low-density polyethylene (LDPE), linear low-density polyethylene (LLDPE), very low-density polyethylene (VLDPE), or medium-density polyethylene (MDPE), ethylene-vinyl acetate copolymer (EVA), ethylene-ethyl acrylate copolymer (EEA), ethylene-butyl acrylate copolymer (EBA) and copolymers and mixtures thereof.

5. Polymer composition according to any of the preceding claims, characterized in that the thermoplastic elastomer has a glass transition temperature from a range from 120°C to 230°C.

6. Polymer composition according to any of the preceding claims, characterized in that the diene-based block A has been at least partly hydrogenated.

7. Polymer composition according to any of the preceding claims, characterized in that the block A is selected from the group consisting of butadiene, isoprene and combinations thereof.

8. Polymer composition according to any of the preceding claims, characterized in that the proportion of the block B in the thermoplastic elastomer is within a range from 150 by weight to 45% by weight, based in each case on the total weight of the thermoplastic polymer.

9. Polymer composition according to any of the preceding claims, characterized in that the polymer composition contains the thermoplastic elastomer in an amount of up to 75% by weight, based on the total weight of the polymer composition.

10. Polymer composition according to any of the preceding claims, characterized in that the polymer composition is in a presentation form selected from the group consisting of powder, grit, crumbs, pellets and filaments.

11. Polymer composition according to any of the preceding claims, characterized in that the polymer composition takes the form of a shaped body.

12. Polymer composition according to any of the preceding claims, characterized in that the shaped body is an injection moulding, an extrudate or a printed shaped body.

13. Use of the polymer composition according to any of Claims 1 to 10 in injection moulding, extrusion or additive manufacturing.

14. Process for producing a shaped body, wherein the process comprises at least the following steps: - providing a polymer composition according to any of Claims 1 to 10, - forming the polymer composition provided to a shaped body.