AMINOFUNCTIONAL POLYBUTADIENS WITH COMB-CONTINUOUS POLYETHER RESIDUES AND METHOD FOR THEIR PREPARATION
Patent Information
- Application Number
- DE502022002085
- Authority / Receiving Office
- DE · DE
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-02-17
- Filing Date
- 2022-02-09
- Publication Date
- 2024-11-21
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Current methods for producing polyether-modified polybutadienes are limited by the availability of only a few triblock structures and lack a simple manufacturing process, particularly for linear polybutadienes with lateral amino-functional groups, which restricts the chemical structure variation and accessibility of these polymers.
A process involving the reaction of polybutadiene with an epoxidizing reagent to form epoxy-functional polybutadiene, followed by reaction with an amino-functional compound to create hydroxy- and amino-functional polybutadiene, and subsequent reaction with an epoxy-functional compound to produce polyether-modified amino-functional polybutadiene, allowing for direct alkoxylation and variation in polyether chain length and structure.
This process enables the modification of linear polybutadienes with comb-positioned polyether residues, providing a wide range of structural diversity and accessibility to linear polyether-modified amino-functional polybutadienes, free from residual epoxy groups and free polyether components, with controlled chain length and monomer sequence.
Description
[0001] The invention relates to a process for producing polyether-modified amino-functional polybutadienes and to polyether-modified amino-functional polybutadienes that can be produced by this process.
[0002] Polybutadienes with pendant polyether residues are known and are produced according to the state of the art, for example, by reacting reactive, functionalized polybutadienes with polyethers. For example, Q. Gao et al. describe amphiphilic polymer comb structures in Macromolecular Chemistry and Physics (2013), 214(15), 1677-1687, which are produced by grafting polyethylene glycol to a polybutadiene main chain. According to JP 2011038003, polybutadienes functionalized with maleic anhydride units are reacted with amino-terminated polyethers. This results in maleinized polybutadienes with comb-shaped polyether residues, which are attached via an amide or imide group. In a similar process, according to J. Wang, Journal of Applied Polymer Science (2013), 128(4), 2408-2413, polyethylene glycols are added to polybutadienes with a high proportion of 1,2-butadiene monomer units to form an ester linkage.High-molecular-weight graft polymers with a comb structure are obtained by the process disclosed in JP 2002105209 through the addition of epoxidized polybutadienes with OH-functional polyethers. H. Decher et al., according to Polymer International (1995), 38(3), 219-225, utilize the addition of isocyanate-terminated polyethylene glycols to hydroxy-functional polybutadienes.
[0003] Furthermore, processes for the production of polyether-modified polybutadienes are known in which hydroxy-functional polybutadienes are reacted with epoxy compounds. For example, the alkoxylation of OH-terminated polybutadienes is known from the prior art.
[0004] US 4994621 A, for example, describes the alkoxylation of hydroxy-terminated polybutadienes with ethylene oxide and propylene oxide in the presence of tetramethylammonium hydroxide. The use of hydroxy-terminated polybutadienes in the alkoxylation leads exclusively to polyether-polybutadiene-polyether triblock structures. According to EP 2003156 A1, this block structure is responsible for the poor miscibility with other reaction components in the production of polyurethanes.
[0005] In addition to the alkoxylation of hydroxy-terminated polybutadienes, the alkoxylation of pendant hydroxy-functional polybutadienes is also known. For example, Q. Gao et al. describe in Macromolecular Chemistry and Physics (2013), 214(15), 1677-1687 the preparation of a pendant polyether-modified polybutadiene by alkoxylation of a pendant hydroxy-functional polybutadiene with ethylene oxide. The pendant hydroxy-functional polybutadiene used in this process is initially prepared by epoxidation of a polybutadiene, subsequent reaction of the epoxidized polybutadiene with a lithium polybutadiene compound, and finally protonation of the reaction product with HCl and methanol. This process leads to a polybutadiene with both pendant polyether residues and pendant polybutadiene residues.According to the process disclosed in the not yet published document PCT / EP2020 / 083013, polybutadienes modified with polyether residues in the comb position are prepared by alkoxylation of laterally hydroxy-functional polybutadienes which were previously obtained by ring-opening of epoxy-functional polybutadienes with preferably alcohols.
[0006] The chemical modification of polybutadienes by epoxidation and subsequent epoxy ring opening by reaction with amines is known. JP 63288295 discloses the reaction of epoxy-functional polybutadienes with dimethylamine and the subsequent protonation of the amine functions with acetic acid. The process according to JP 57205596 comprises, in addition to the epoxy ring opening with dimethylamine, the further quaternization of the amine functions with epichlorohydrin. A process for the epoxy ring opening of hydrogenated polybutadienes with amines is disclosed in DE 2554093. DE 2943879, DE 2732736, and JP 49055733 describe the addition of diethanolamine. JP 48051989 also describes the addition of diethanolamine followed by a crosslinking reaction in the presence of dibenzoyl peroxide.JP 53117030, DE 2734413, and DE 2943879 describe the addition of ethanolamine; JP 05117556 describes the reaction with diisopropanolamine; EP 0351135, EP 0274389, and DE 3305964 describe the reaction of the epoxy groups with dimethylamine. DD 296286 discloses the addition of primary and secondary amines containing 4 to 20 carbon atoms to epoxidized polybutadienes in polar solvents. Further alkoxylation of the amino-functional polybutadienes is not disclosed in any of these documents.
[0007] Therefore, no process is known from the prior art for the preparation of preferably linear amino-functional polybutadienes with pendant polyether chains by a simple, direct alkoxylation reaction of pendant amino-functional polybutadienes with alkylene oxides, wherein the pendant amino-functional polybutadienes are prepared from epoxy-functional polybutadienes by a ring-opening reaction with amines.
[0008] Polybutadienes and modified polybutadienes are widely used as reactive components or formulation ingredients, for example, to make polymers hydrophobic or flexible and to improve their mechanical properties. However, the application possibilities of polyether-modified polybutadienes are currently often limited by the restriction to a few available triblock structures. There is currently no way to vary the chemical structure of polyether-modified polybutadienes within wide limits. Furthermore, there is no simple manufacturing process for such polymers.
[0009] The object of the present invention was to overcome at least one disadvantage of the prior art.
[0010] The particular objective was to provide an improved process for the production of preferably linear polybutadienes that are comb-modified (laterally, sideways) with polyether residues via an amino group. Furthermore, the process should enable very simple access to preferably linear polybutadienes with sideways polyether residues. Furthermore, the polyether-modified polybutadienes should be obtainable by direct alkoxylation of sideways amino-functional polybutadienes. A further objective was to provide suitable sideways amino-functional polybutadienes as precursors and chain initiators for the alkoxylation.
[0011] Surprisingly, it has now been found that a process for producing polyether-modified amino-functional polybutadienes solves this problem, which comprises the following steps: a) reacting at least one polybutadiene (A) with at least one epoxidation reagent (B) to form at least one epoxy-functional polybutadiene (C); b) reacting the at least one epoxy-functional polybutadiene (C) with at least one amino-functional compound (D) to form at least one hydroxy- and amino-functional polybutadiene (E); c) reacting the at least one hydroxy- and amino-functional polybutadiene (E) with at least one epoxy-functional compound (F) to form at least one polyether-modified amino-functional polybutadiene (G).
[0012] Surprisingly, it was further found that, in particular, polybutadienes with a high proportion of 1,4-units and a low content of vinylic 1,2-units can be converted into pendant hydroxy- and amino-functional polybutadienes after epoxidation with hydrogen peroxide by ring opening with primary or secondary amines and subsequently alkoxylated with alkylene oxides.
[0013] The object of the present invention is therefore achieved by the subject matter of the independent claims. Advantageous embodiments of the invention are specified in the subordinate claims, the examples, and the description.
[0014] The subject matter of the invention is described below by way of example, without intending to limit the invention to these exemplary embodiments. Where ranges, general formulas, or classes of compounds are specified below, these are intended to encompass not only the corresponding ranges or groups of compounds explicitly mentioned, but also all subranges and subgroups of compounds that can be obtained by removing individual values (ranges) or compounds. If documents are cited within the scope of this description, their entire content is intended to be part of the disclosure of the present invention.
[0015] Unless otherwise stated, mean values given below are numerical averages. Unless otherwise stated, measured values, parameters, or material properties given below that are determined by measurement are measured at 25 °C and preferably at a pressure of 101325 Pa (standard pressure).
[0016] The number-average molecular weight M n , the weight-average molecular weight M w and the polydispersity (M w / M n ) are preferably determined in the context of the present invention by means of gel permeation chromatography (GPC), as described in the examples, unless explicitly stated otherwise.
[0017] If numerical ranges are specified below in the form "X to Y," where X and Y represent the limits of the numerical range, this is equivalent to the statement "from at least X up to and including Y," unless otherwise stated. Therefore, range specifications include the range limits X and Y, unless otherwise stated.
[0018] The terms lateral, lateral and comb are used synonymously.
[0019] Wherever molecules or molecular fragments have one or more stereocenters or can be distinguished into isomers due to symmetries or can be distinguished into isomers due to other effects, such as restricted rotation, all possible isomers are included in the present invention.
[0020] The following formulas (1) to (5) describe compounds or radicals that are composed of repeating units, such as repeating fragments, blocks, or monomer units, and can have a molecular weight distribution. The frequency of the repeating units is indicated by indices. The indices used in the formulas are to be regarded as statistical averages (numerical averages), unless explicitly stated otherwise. The index numbers used as well as the value ranges of the stated indices are understood as averages of the possible statistical distribution of the actual structures present and / or their mixtures, unless explicitly stated otherwise. The various fragments or repeating units of the compounds described in the following formulas (1) to (5) can be statistically distributed.Statistical distributions are constructed in blocks with any number of blocks and any sequence, or are subject to a randomized distribution; they can also be constructed alternately, or form a gradient across the chain, if one is present; in particular, they can also form all mixed forms in which groups of different distributions can follow one another. The following formulas include all permutations of repeating units. Therefore, if compounds such as polybutadienes (A), epoxy-functional polybutadienes (C), hydroxy- and amino-functional polybutadienes (E), polyether-modified amino-functional polybutadienes (G) or polyether-modified amino-functional polybutadienes (K) containing end-capped polyether radicals are described within the scope of the present invention, which can have different units multiple times, these can be both disordered, e.g.statistically distributed, or occur in an ordered manner in these compounds. The information on the number or relative frequency of units in such compounds is to be understood as a mean (numerical average) averaged over all corresponding compounds. Special designs may result in the statistical distributions being restricted by the embodiment. For all areas not affected by the restriction, the statistical distribution remains unchanged.
[0021] A first subject of the invention is thus a process for the preparation of one or more polyether-modified amino-functional polybutadienes, comprising the steps: a) reacting at least one polybutadiene (A) with at least one epoxidation reagent (B) to form at least one epoxy-functional polybutadiene (C); b) reacting the at least one epoxy-functional polybutadiene (C) with at least one amino-functional compound (D) to form at least one hydroxy- and amino-functional polybutadiene (E); c) reacting the at least one hydroxy- and amino-functional polybutadiene (E) with at least one epoxy-functional compound (F) to form at least one polyether-modified amino-functional polybutadiene (G).
[0022] It is preferred that the method according to the invention further comprises at least one of the following steps: d) reacting the at least one polyether-modified amino-functional polybutadiene (G) with at least one end-capping reagent (H) to form at least one polyether-modified amino-functional polybutadiene (K) containing end-capped polyether radicals; e) lightening the color of the at least one polyether-modified amino-functional polybutadiene (G) or (K); f) converting at least some of the amino groups of the at least one polyether-modified amino-functional polybutadiene (G) or (K) to quaternary ammonium groups by means of an acid and / or a quaternization reagent.
[0023] Steps a), b), c), d), e), and f) are carried out in the specified order, whereby one or more of steps d), e), and f) may be omitted. The steps may follow one another directly. However, the process may also include further upstream steps, intermediate steps, or downstream steps, such as purification of the reactants, intermediates, and / or final products.
[0024] The polybutadienes (E) prepared from the epoxy-functional polybutadienes (C) by epoxide ring opening with amines are characterized by having both amino groups and hydroxy groups on the side. Depending on the reaction conditions in step c), the addition of the epoxy-functional compounds (F) occurs at the amino groups, at the hydroxy groups, or preferably at both reactive groups.
[0025] It is preferred to use stabilizers or antioxidants during the process according to the invention to stabilize the reactants, intermediates, and products in order to avoid unwanted polymerization reactions of the double bonds. Suitable for this purpose are, for example, the sterically hindered phenols known to the person skilled in the art, commercially available, for example, as Anox®< 20, Irganox®< 1010 (BASF), Irganox®< 1076 (BASF), and Irganox®< 1135 (BASF).
[0026] It is further preferred to carry out one or more or all process steps under an inert atmosphere, e.g., under nitrogen. The unmodified reactants, i.e., the at least one polybutadiene (A), as well as the polyether-modified finished products according to the invention, i.e., the at least one polyether-modified polybutadiene (G) or (K), should preferably be stored in the absence of air, if possible.
[0027] The process according to the invention makes it possible for the first time to modify linear polybutadienes with comb-shaped polyether residues by simple direct alkoxylation of the pendant amino and hydroxy groups. The chain length and monomer sequence in the polyether residue can be varied within a wide range. The average number of polyether residues bound to the polybutadiene can be specifically adjusted by the degree of epoxidation and the functionalization with amino and hydroxy groups, opening up a wide structural diversity for the hydroxy- and amino-functional polybutadienes (E).
[0028] The amino-functional polybutadienes obtainable according to the invention with comb-shaped polyether radicals are preferably essentially free of residual epoxy groups. The process product according to the invention preferably contains essentially no free polyether moieties. Preferably, the polyethers are chemically bonded to the polybutadiene via a nitrogen atom and / or an oxygen atom. Step a)
[0029] In step a) of the process according to the invention, at least one polybutadiene (A) is reacted with at least one epoxidation reagent (B) to form at least one epoxy-functional polybutadiene (C).
[0030] In this reaction, double bonds of the polybutadiene (A) are converted into epoxy groups. Various methods for the epoxidation of polybutadienes with, for example, percarboxylic acids and hydrogen peroxide are known to the person skilled in the art and are disclosed, for example, in CN 101538338, JP 2004346310, DD 253627 and WO 2016 / 142249 A1. Particularly suitable for the preparation of the epoxy-functional polybutadienes (C) with a high proportion of 1,4-units is performic acid, which is also in situ can be formed from formic acid in the presence of hydrogen peroxide. The epoxidation preferably takes place in a solvent such as toluene or chloroform, which is removed by distillation after the reaction and washing out of any peroxide residues.
[0031] Polybutadienes (A) are polymers of buta-1,3-diene. The polymerization of the buta-1,3-diene monomers occurs primarily via 1,4- and / or 1,2-linkage. A 1,4-linkage leads to so-called 1,4- trans -units and / or 1.4- cis -units, which are collectively also referred to as 1,4-units. A 1,2-linkage leads to so-called 1,2-units. The 1,2-units carry a vinyl group and are also referred to as vinylic 1,2-units. In the context of the present invention, the 1,2-units are also referred to as "(X)", the 1,4- trans -units with "(Y)" and the 1.4- cis- Units designated with "(Z)":
[0032] The double bonds contained in the units are analogously referred to as 1,4- trans -double bonds, 1,4 -cis- Double bonds or 1,2-double bonds or 1,2-vinyl double bonds. The 1,4 -trans- Double bonds and 1,4- cis -Double bonds are also collectively referred to as 1,4-double bonds.
[0033] The polybutadienes (A) are therefore unmodified polybutadienes. The polybutadienes (A) and their preparation processes are known to those skilled in the art. They are preferably prepared by radical, anionic, or coordinative chain polymerization.
[0034] Free-radical chain polymerization is preferably carried out as an emulsion polymerization. This leads to a statistical occurrence of the three aforementioned units. At low reaction temperatures (approx. 5 °C), the proportion of vinyl groups decreases. Initiation is preferably carried out with potassium peroxodisulfate and iron salts or with hydrogen peroxide.
[0035] In anionic chain polymerization, the chain polymerization is preferably initiated with butyllithium. The resulting polybutadiene (A) contains about 40% 1,4- cis -units and 50% 1.4 -trans- units.
[0036] In the coordinative chain polymerization, Ziegler-Natta catalysts are preferably used, in particular stereospecific Ziegler-Natta catalysts, which lead to a polybutadiene (A) with a high proportion of 1,4- cis -units.
[0037] During the polymerization of 1,3-butadiene, branched polybutadienes (A) can also be formed through side or subsequent reactions, such as a subsequent reaction of the double bonds of the resulting 1,2- and 1,4-units of the polybutadiene. However, the polybutadienes (A) used according to the invention are preferably linear, i.e., unbranched polybutadienes. It is also possible for the polybutadienes to contain small amounts of units other than 1,2-units, 1,4- trans -units or 1.4- cis- units. However, it is preferred that the mass fraction of the sum of 1,2-units, 1,4- trans -units and 1.4- cis-units is at least 80%, preferably at least 90%, in particular at least 99%, based on the total mass of the at least one polybutadiene (A), i.e. based on the total mass of all polybutadienes (A) used.
[0038] For the process according to the invention, preference is given to using polybutadienes (A) which have 0% to 80% 1,2-units and 20% to 100% 1,4-units, more preferably 0% to 30% 1,2-units and 70% to 100% 1,4-units, even more preferably 0% to 10% 1,2-units and 90% to 100% 1,4-units, and most preferably 0% to 5% 1,2-units and 95% to 100% 1,4-units, based on the sum of 1,2-units and 1,4-units.
[0039] It is therefore preferred that of the double bonds of all polybutadienes (A) used, 0% to 80% are 1,2-vinyl double bonds and 20% to 100% are 1,4-double bonds, more preferably 0% to 30% are 1,2-vinyl double bonds and 70% to 100% are 1,4-double bonds, even more preferably 0% to 10% are 1,2-vinyl double bonds and 90% to 100% are 1,4-double bonds, most preferably 0% to 5% are 1,2-vinyl double bonds and 95% to 100% are 1,4-double bonds.
[0040] For the preparation of the products according to the invention, polybutadienes (A) of the formula (1) are preferably used. with a content of 0% to 80% 1,2-vinyl double bonds (index x) and 20% to 100% 1,4-double bonds, more preferably 0% to 30% 1,2-vinyl double bonds and 70% to 100% 1,4-double bonds, even more preferably with 0% to 10% 1,2-vinyl double bonds and 90% to 100% 1,4-double bonds, most preferably with 0% to 5% 1,2-vinyl double bonds and 95% to 100% 1,4-double bonds. The ratio of 1,4-trans double bonds (index y) and 1,4-cis double bonds (index z) is arbitrary.
[0041] The indices x, y, and z represent the number of butadiene units in the polybutadiene (A). These are numerical averages (number averages) across all polybutadiene polymers of the at least one polybutadiene (A).
[0042] The average molecular weight and polydispersity of the polybutadienes (A) used according to formula (1) is arbitrary.
[0043] It is preferred that the number-average molar mass M n of the at least one polybutadiene (A) is from 200 g / mol to 20,000 g / mol, more preferably from 500 g / mol to 10,000 g / mol, most preferably from 700 g / mol to 5,000 g / mol.
[0044] Alternatively, it is preferred that the number-average molar mass M n of the at least one polybutadiene (A) is from 2100 g / mol to 20,000 g / mol, more preferably from 2200 g / mol to 10,000 g / mol, most preferably from 2300 g / mol to 5000 g / mol.
[0045] It is further preferred that the at least one polybutadiene (A) has a number average of 5 to 360, more preferably 10 to 180, most preferably 15 to 90 units selected from the group consisting of 1,2-units, 1,4- cis -units and 1.4- trans -units.
[0046] Alternatively, it is preferred that the at least one polybutadiene (A) has a number average of 35 to 360, more preferably 40 to 180, most preferably 45 to 90 units selected from the group consisting of 1,2-units, 1,4- cis -units and 1.4- trans -units.
[0047] It is further preferred that the viscosity of the polybutadienes (A) used is 50 to 50,000 mPas, more preferably 100 to 10,000 mPas, most preferably 500 to 5,000 mPas (determined according to DIN EN ISO 3219:1994-10).
[0048] The most preferred polybutadienes are the products Polyvest ®< 110 and Polyvest ®< 130, commercially available from Evonik Industries AG / Evonik Operations GmbH, with the following typical characteristics: Polyvest ®< 110: approx. 1% 1,2-vinyl double bonds, approx. 24% 1,4- trans -Double bonds, approx. 75% 1,4-cis-double bonds, number average molar mass M n approx. 2600 g / mol, viscosity (20 °C) 700-860 mPas (according to DIN EN ISO 3219:1994-10), Polyvest ®< 130: approx. 1 % 1,2-vinyl double bonds, approx. 22 % 1,4- trans -Double bonds, approx. 77% 1,4-cis -double bonds, number average molar mass M n approx. 4600 g / mol, viscosity (20 °C) 2700-3300 mPas (according to DIN EN ISO 3219:1994-10).
[0049] The most preferred polybutadienes continue to be the products Lithene ultra AL and Lithene ActiV 50 available from Synthomer PLC with the following typical characteristics: Lithene ultra AL: approx. 40% 1,2-vinyl double bonds, approx. 60% 1,4-double bonds, Lithene ActiV 50: approx. 70% 1,2-vinyl double bonds, approx. 30% 1,4-double bonds.
[0050] The degree of epoxidation is determined quantitatively, for example, using 13< C-NMR spectroscopy or epoxy number titration (determination of the epoxy equivalent according to DIN EN ISO 3001:1999) and can be adjusted in a targeted and reproducible manner via the process conditions, in particular via the amount of hydrogen peroxide used in relation to the amount of double bonds in the polybutadiene.
[0051] In step a) of the process according to the invention, >0% (i.e. from >0% to 100%) of all double bonds of the at least one polybutadiene (A) are epoxidized.
[0052] It is preferred that in step a) of the process according to the invention from >0% to <100%, more preferably from >0% to 70%, even more preferably from 1% to 50%, even more preferably from 2% to 40%, even more preferably from 3% to 30% and most preferably from 4% to 20% of all double bonds of the at least one polybutadiene (A) are epoxidized.
[0053] In principle, all epoxidizing agents known to the person skilled in the art can be used as the epoxidizing reagent (B). It is preferred that the epoxidizing reagent (B) is selected from the group of peroxycarboxylic acids (percarboxylic acids, peracids), preferably from the group consisting of meta- Chloroperbenzoic acid, peracetic acid (peracetic acid) and peroxyformic acid (performic acid), especially peroxyformic acid (performic acid). The peroxycarboxylic acids are preferably in situ formed from the corresponding carboxylic acid and hydrogen peroxide.
[0054] It is most preferred that the at least one epoxidation reagent (B) contains performic acid, which is preferably in situ formed from formic acid and hydrogen peroxide.
[0055] The epoxidation of the at least one polybutadiene (A) occurs randomly distributed throughout the polybutadiene chain, preferentially at the 1,4-double bonds. Epoxidation of the 1,2-double bonds can also occur and also occurs at these bonds, randomly distributed throughout the polybutadiene chain. However, epoxidation of the 1,2-double bonds is disadvantaged compared to epoxidation of the 1,4-double bonds. The reaction product thus contains epoxy-functional polybutadiene polymers that differ from one another in their degree of epoxidation. All stated degrees of epoxidation are therefore to be understood as average values. Step b)
[0056] In step b) of the process according to the invention, the at least one epoxy-functional polybutadiene (C) is reacted with at least one amino-functional compound (D) to form at least one hydroxy- and amino-functional polybutadiene (E).
[0057] In this reaction, an addition reaction of the at least one amino-functional compound (D) to the at least one epoxy-functional polybutadiene (C) takes place. The reaction thus occurs with the formation of one or more covalent bonds between the at least one amino-functional compound (D) and the at least one epoxy-functional polybutadiene (C). The reaction preferably comprises (at least ideally) a reaction step in which a nucleophilic attack of at least one amino group of the at least one amino-functional compound (D) on at least one epoxy group of the at least one epoxy-functional polybutadiene (C) occurs, with ring opening of this at least one epoxy group.
[0058] It is preferred that the at least one amino-functional compound (D) is selected from compounds having at least one primary and / or at least one secondary amino group, since primary and secondary amino groups are particularly easily added to the epoxide groups of the polybutadiene. Within the scope of the present invention, ammonia is also included among these amino-functional compounds (D). However, it is more preferred that the at least one amino-functional compound (D) is selected from organic compounds having at least one primary and / or at least one secondary amino group. It is even more preferred that the at least one amino-functional compound (D) is selected from organic compounds having 1 to 22 carbon atoms and at least one primary and / or at least one secondary amino group.It is even more preferred that the at least one amino-functional compound (D) is selected from organic compounds having 1 to 12 carbon atoms and at least one primary and / or at least one secondary amino group. It is further preferred that the amino-functional compound (D) has precisely one primary or secondary amino group. This makes it possible to reduce or prevent undesired crosslinking reactions. It is further preferred that the amino-functional compound (D) is not an aromatic amine, in particular not a primary aromatic amine, since some primary aromatic amines are known to be human carcinogens. For the purposes of the present invention, an aromatic amine is understood to mean those amines in which the nitrogen atom of at least one amino group is bonded to a carbon atom which in turn is part of an aromatic ring system.
[0059] It is further preferred that the at least one amino-functional compound (D) is selected from the group consisting of ammonia, alkylamines, cycloalkylamines, dialkylamines, monoalkanolamines, and dialkanolamines. The aliphatic radicals bonded to the nitrogen can also carry aromatic radicals or heteroatoms such as nitrogen or oxygen. It is therefore further preferred that the at least one amino-functional compound (D) is selected from the group consisting of diamines, polyamines, polyetheramines, and hydroxy-functional aliphatic amines. More preferably, the at least one amino-functional compound (D) is selected from the group consisting of alkylamines, cycloalkylamines, dialkylamines, monoalkanolamines, dialkanolamines, and trialkanolamines, each having 1 to 22 carbon atoms and having exactly one primary or secondary amino group.More preferably, the at least one amino-functional compound (D) is selected from the group consisting of alkylamines, monoalkanolamines, dialkanolamines and trialkanolamines, each having 1 to 12 carbon atoms and exactly one primary or secondary amino group. Most preferably, the at least one amino-functional compound (D) is selected from the group consisting of butylamine, isobutylamine, hexylamine, octylamine, 2-ethylhexylamine, decylamine, laurylamine, ethanolamine, isopropanolamine, diethanolamine, diisopropanolamine, N-methylethanolamine, N-methylisopropanolamine, 2-amino-2-methyl-1-propanol, 2-amino-2-ethyl-1,3-propanediol, tris(hydroxymethyl)aminomethane (TRIS, 2-amino-2-(hydroxymethyl)propane-1,3-diol), morpholine, piperidine, cyclohexylamine, N,N-dimethylaminopropylamine (DMAPA), and benzylamine. Any desired mixtures of these amines can also be used.In the context of the present invention, the term "trialkanolamines" refers only to those trialkanolamines which carry primary and / or secondary amino groups, such as tris(hydroxymethyl)aminomethane.
[0060] The molar ratio of the NH groups of the at least one amino-functional compound (D) to the epoxy groups of the at least one epoxy-functional polybutadiene (C) can be varied within a wide range. However, it is preferred to use the at least one amino-functional compound (D) and the at least one epoxy-functional polybutadiene (C) in such a molar ratio of NH groups to epoxy groups that the most quantitative conversion of all epoxy groups is achieved. It is therefore preferred that in step b), the total number of NH groups of all amino-functional compounds (D) to the total number of epoxy groups of all epoxy-functional polybutadienes (C) is from 0.8:1 to 20:1, more preferably from 0.9:1 to 10:1, even more preferably from 1:1 to 5:1, most preferably from 1:1 to 3:1. The excess of compound (D) can be removed after the reaction, e.g. by distillation, and reused if required.In this context, it should be noted that an ammonia molecule has exactly three NH groups, a primary amino group has exactly two, and a secondary amino group has exactly one.
[0061] Epoxy ring opening with amines can optionally be carried out in a solvent such as ethanol, propanol, isopropanol, or THF. Avoiding solvents is preferred.
[0062] Preferably, the reaction takes place in the presence of at least one catalyst. The catalyst can be homogeneously soluble in the reaction mixture, added as an aqueous solution, or heterogeneously distributed as a solid.
[0063] It is preferred that the catalyst is selected from the group consisting of Lewis acids and Brønsted acids; more preferably from the group consisting of water, phenols, alcohols, carboxylic acids, ammonium compounds, phosphonium compounds, and lithium bromide; even more preferably from the group consisting of carboxylic acids, phenols, ammonium compounds, phosphonium compounds, and lithium bromide; even more preferably from the group consisting of carboxylic acids, phenol, and lithium bromide, most preferably lithium bromide. The catalyst is optionally homogeneously soluble in the reaction mixture, can be added as an aqueous solution, or is heterogeneously distributed therein as a solid.
[0064] The type and amount of catalyst used are selected so that the at least one amino-functional compound (D) is added to the epoxy groups of the at least one epoxy-functional polybutadiene (C) as quickly and quantitatively as possible. Lithium bromide, as a solid or dissolved in water, is preferably used in a mass fraction of 0.05% to 15.0%, preferably 0.2% to 10.0%, most preferably 0.5% to 7.0%, based on the mass of the at least one amino-functional compound (D).
[0065] The reaction of the at least one epoxy-functional polybutadiene (C) with the at least one amino-functional compound (D), optionally in the presence of a catalyst, is preferably carried out at 50 °C to 250 °C, more preferably at 80 °C to 200 °C.
[0066] The components are stirred for several hours until the epoxide groups are as completely converted as possible. The presence of epoxide groups can be determined either by NMR spectroscopy or by known methods of epoxide number titration (as described in the examples).
[0067] The reaction conditions in step b) are preferably selected such that more than 90% of the epoxide groups generated in step a) undergo ring opening. It is most preferred that no epoxide groups are detectable in the product of step b), i.e., in the at least one hydroxy- and amino-functional polybutadiene (E).
[0068] After the reaction, any excess amino-functional compounds (D) as well as any solvent, water and the catalyst are preferably removed by distillation and precipitated salts are filtered off if necessary.
[0069] From each epoxy group of an epoxy-functional polybutadiene (C) a repeating unit of the formula (2a), (2b) or (2c) results after ring opening by an amino-functional compound (D) of the formula A 1 -NH-A 2 :
[0070] In formulas (2a), (2b) and (2c), the radicals A 1 and A 2 are preferably each independently of one another organic radicals which may carry further amine or hydroxyl groups, or hydrogen radicals. The radicals A 1 and A 2 can thus contain heteroatoms such as nitrogen and oxygen and can also be bridged to one another via an organic radical, as is the case, for example, with morpholine or piperidine. The amino-functional compound (D) of the formula A 1 -NH-A 2 can also be ammonia. In the case of ammonia, both A 1 and A 2 are hydrogen radicals. If, for example, ethanolamine is used as the amino-functional compound (D), in formulas (2a), (2b) and (2c), the radical A 1 is, for example, a hydroxyethyl radical and the radical A 2 is then a hydrogen radical, i.e. A 2 = H. Each reacted epoxide group results in at least one pendant OH group.
[0071] When a primary amine as compound (D) is reacted with an epoxide group of an epoxy-functional polybutadiene (C), a secondary amino group with a reactive hydrogen on the nitrogen atom is always formed. This secondary amino group can add to another epoxide group via the NH group in a subsequent reaction, thus linking two epoxy-functional polybutadienes (C). The reaction conditions in step b) are preferably selected so that this linking reaction is largely suppressed.
[0072] In the case of the polybutadienes (A) preferred according to the invention with a predominant proportion of 1,4-units, the repeating units of the formulas (2a), (2b) and (2c) predominate those of the formula (2a).
[0073] It is preferred that the at least one hydroxy- and amino-functional polybutadiene (E) has 20% to 100%, more preferably 70% to 100%, even more preferably 90% to 100%, most preferably 95% to 100% repeat units of the formula (2a) based on the total number of all repeat units of the formulas (2a), (2b) and (2c).
[0074] The proportion of repeating units of formulas (2a), (2b) and (2c) taken together is >0% (i.e. from >0% to 100%) based on the total number of all repeating units of the at least one hydroxy- and amino-functional polybutadiene (E).
[0075] The degree of amination is accordingly >0% (i.e. from >0% to 100%).
[0076] It is preferred that the proportion of repeating units of formulas (2a), (2b) and (2c) taken together is from >0% to <100%, more preferably from >0% to 70%, even more preferably from 1% to 50%, even more preferably from 2% to 40%, even more preferably from 3% to 30% and most preferably from 4% to 20%, based on the total number of all repeating units of the at least one hydroxy- and amino-functional polybutadiene (E).
[0077] It is accordingly preferred that the degree of amination is from >0% to <100%, more preferably from >0% to 70%, even more preferably from 1% to 50%, even more preferably from 2% to 40%, even more preferably from 3% to 30% and most preferably from 4% to 20%.
[0078] Upon complete conversion in step b), the degree of amination of the hydroxy- and amino-functional polybutadiene (E) corresponds to the degree of epoxidation of the corresponding epoxy-functional polybutadiene (C). Step c)
[0079] In step c) of the process according to the invention, the at least one hydroxy- and amino-functional polybutadiene (E) is reacted with at least one epoxy-functional compound (F) to form at least one polyether-modified amino-functional polybutadiene (G).
[0080] The at least one hydroxy- and amino-functional polybutadiene (E) from step b) serves in step c) as a starting compound (starter) for the reaction with the at least one epoxy-functional compound (F). With ring opening and preferably in the presence of a suitable catalyst, the at least one epoxy-functional compound (F) (hereinafter also referred to simply as "monomer" or "epoxide monomer" or "epoxide") is added to the NH and / or OH groups of the at least one hydroxy- and amino-functional polybutadiene (E) in a polyaddition reaction. This leads to the formation of amino-functional polybutadienes with comb-positioned (pendent) polyether chains, i.e., to the formation of the at least one polyether-modified amino-functional polybutadiene (G). The monomers are preferably added to (at least substantially) all OH groups and to (at least substantially) all NH groups.Preferably, the polyether-modified aminofunctional polybutadiene (G) is a linear polybutadiene that is comb-modified (laterally) with polyether residues. Thus, it is preferred that the polyether-modified aminofunctional polybutadiene (G) has a linear polybutadiene backbone and lateral polyether residues.
[0081] The reaction in step c) is preferably an alkoxylation reaction, i.e., a polyaddition of alkylene oxides to the at least one hydroxy- and amino-functional polybutadiene (E). However, the reaction in step c) can also be carried out with glycidyl compounds as an alternative or in addition to the alkylene oxides.
[0082] It is therefore preferred that the at least one epoxy-functional compound used in step c) is selected from the group of alkylene oxides, more preferably from the group of alkylene oxides having 2 to 18 carbon atoms, even more preferably from the group of alkylene oxides having 2 to 8 carbon atoms, most preferably from the group consisting of ethylene oxide, propylene oxide, 1-butylene oxide, cis -2-Butylene oxide, trans -2-butylene oxide, isobutylene oxide and styrene oxide; and / or that the at least one epoxy-functional compound used in step c) is selected from the group of glycidyl compounds, more preferably from the group of monofunctional glycidyl compounds, most preferably from the group consisting of phenyl glycidyl ether, o-cresyl glycidyl ether, tert-butylphenyl glycidyl ether, allyl glycidyl ether, butyl glycidyl ether, 2-ethylhexyl glycidyl ether, C 12 / C 14 fatty alcohol glycidyl ether and C 13 / C 15 fatty alcohol glycidyl ether.
[0083] The monomers can be added individually in pure form, alternately one after the other in any dosing sequence, or simultaneously mixed. The sequence of monomer units in the resulting polyether chain is thus subject to a blockwise distribution, a random distribution, or a gradual distribution in the final product.
[0084] The process according to the invention builds up pendant polyether chains on the polybutadiene, which are characterized by the fact that they can be produced in a targeted and reproducible manner with regard to structural composition and molecular weight.
[0085] The sequence of monomer units can be varied within wide limits by changing the order of addition.
[0086] The molar masses of the pendant polyether residues can be varied within wide limits according to the process according to the invention and can be controlled in a targeted and reproducible manner via the molar ratio of the added monomers with respect to the NH and OH groups of the at least one hydroxy- and amino-functional polybutadiene (E) from step b) provided.
[0087] The polyether-modified amino-functional polybutadienes (G) prepared according to the invention are preferably characterized in that they contain radicals B bonded to the polybutadiene skeleton via an amino and / or ether group according to formulas (3a), (3b) and (3c),
[0088] The radicals A 1 and A 2 are each independently organic radicals, preferably having 1 to 22, most preferably 1 to 12, carbon atoms, where the radicals A 1 and A 2 may be covalently bonded to one another. The radicals A 1 and A 2 may contain heteroatoms, preferably nitrogen and oxygen.
[0089] The indices k1 and k2 in the formulas (3a), (3b) and (3c) are each independently integers from 0 to 8, preferably from 0 to 6, most preferably from 0 to 4. Furthermore, the indices I1 and I2 in the formulas (3a), (3b) and (3c) are each independently integers and are each independently either 0 or 1. The radicals B formed by alkoxylation can thus be k1-fold or k2-fold bonded to the radicals A1 and A2, respectively, wherein the chemical bonding takes place via a nitrogen atom or an oxygen atom which is part of A1 and A2. However, the radicals B formed by alkoxylation can also be directly bonded to the nitrogen atom shown. If in formulas (2a), (2b) or (2c) the radical A 1 or A 2 is a hydrogen radical, then in formulas (3a), (3b) or (3c) the index I1 or I2 is equal to 0 and k1 or k2 is equal to 1, ieThe corresponding radical A 1 or A 2 is nonexistent in formulas (3a), (3b), and (3c), and instead, a polyether radical B is directly bonded to the nitrogen atom shown. An NH group in formulas (2a), (2b), or (2c) is thus replaced by an NB group. If in formulas (2a), (2b) or (2c) the radical A 1 or A 2 is an organic radical, then in formulas (3a), (3b) or (3c) the index I1 or I2 is 1. If in formulas (2a), (2b) or (2c) both A 1 and A 2 are hydrogen radicals, then in formulas (3a), (3b) or (3c) the indices I1 and I2 are 0 and k1 and k2 are 1, i.e. the radicals A 1 and A 2 in formulas (3a), (3b) and (3c) are non-existent and the polyether radicals B are directly bonded to the nitrogen atom shown. The two NH groups in formulas (2a), (2b) or (2c) are each replaced by an NB group.
[0090] For example, if in step b) a primary alkylamine is used as the amino-functional compound (D) and the alkyl radical does not contain any other groups reactive towards epoxides, such as OH or NH groups, then I1 = 1, k1 = 0, I2 = 0 and k2 = 1 applies.
[0091] If, for example, the primary amine ethanolamine is used as the amino-functional compound (D) in step b), then A 1 is a divalent radical of the formula -CHzCHzO-, which in this representation is bonded on the left via the carbon atom to the nitrogen atom of the amino group and on the right via the oxygen atom to a radical B, ie I1 = 1, k1 = 1, I2 = 0 and k2 = 1.
[0092] If, for example, the primary amine tris(hydroxymethyl)aminomethane (TRIS, 2-amino-2-(hydroxymethyl)propane-1,3-diol) is used as the amino-functional compound (D) in step b), then A 1 is, for example, a tetravalent radical of the formula -C(CH 2 O-) 3 , which in this representation is bonded on the left via the carbon atom to the nitrogen atom of the amino group and on the right via the three oxygen atoms to one radical B each (and thus to a total of three radicals B), ie, for example, I1 = 1, k1 = 3, I2 = 0 and k2 = 1.
[0093] If, for example, the secondary amine diethanolamine is used as the amino-functional compound (D) in step b), then A 1 and A 2 are divalent radicals of the formula -CHzCHzO-, which in this representation are bonded on the left via the carbon atom to the nitrogen atom of the amino group and on the right via the oxygen atom to a radical B, ie the following applies: I1 =1 , k1 = 1, I2 = 1 and k2 = 1.
[0094] If, for example, the secondary amine N-methylethanolamine is used as the amino-functional compound (D) in step b), then A 1 is a methyl group and A 2 is a divalent radical of the formula -CHzCHzO-, which in this representation is bonded on the left via the carbon atom to the nitrogen atom of the amino group and on the right via the oxygen atom to the radical B, ie the following applies: I1 = 1, k1 = 0, I2 = 1 and k2 = 1.
[0095] If, for example, the secondary amine piperidine is used as the amino-functional compound (D) in step b), then A 1 and A 2 are covalently bonded to one another and together form the divalent radical -CH 2 CH 2 CH 2 CH 2 CH 2 -, which in this representation is bonded to the nitrogen atom of the amino group on both the left and right sides, ie: I1 = 1, k1 = 0, I2 = 1 and k2 = 0.
[0096] Thus, the alkoxylation reaction preferably results in exactly one pendant radical B from (at least almost) each pendant OH and NH group of the at least one hydroxy- and amino-functional polybutadiene (E). The radical B is in turn composed of one or more monomers, preferably of several monomers, of the at least one epoxy-functional compound (F) used. It is possible, although less preferred, that the alkoxylation reaction does not result in a pendant radical B from every OH or NH group of the hydroxy- and amino-functional polybutadiene (E), but rather only a portion, but preferably the majority, of the OH and NH groups are converted in step c).
[0097] For the purposes of the invention, in principle, all alkoxylation catalysts known to the person skilled in the art can be used, e.g., basic catalysts such as alkali metal hydroxides, alkali metal alkoxides, amines, guanidines, amidines, phosphorus compounds such as triphenylphosphine, as well as Brønsted acid and Lewis acid catalysts such as SnCl 4 , SnCl 2 , SnF 2 , BF 3 and BF 3 complexes, as well as double metal cyanide (DMC) catalysts. The addition of a catalyst can be omitted if necessary.
[0098] Before the epoxy is added, i.e., before the addition of the at least one epoxy-functional compound (F), the reactor partially filled with the starter and optionally the catalyst is rendered inert, e.g., with nitrogen. This is achieved, for example, by repeatedly and alternately evacuating and supplying nitrogen. It is advantageous to evacuate the reactor to below 200 mbar after the final introduction of nitrogen. The addition of the first amount of epoxy monomer thus preferably takes place in the evacuated reactor. The monomers are added with stirring and, if necessary, cooling to dissipate the released reaction heat and maintain the preselected reaction temperature.The starter used is at least one hydroxy- and amino-functional polybutadiene (E) or a polyether-modified amino-functional polybutadiene (G) already prepared according to the process according to the invention can also be used as starter, as described further below.
[0099] In a special embodiment, the addition of a catalyst can be omitted at the start of the monomer addition. This is the case, for example, if the amino groups bonded to the polybutadiene are sufficiently reactive. If, for example, a sufficient number of nucleophilic NH functions are present on the polybutadiene, the initiator itself catalyzes the alkoxylation reaction. The reaction rate generally decreases with the polyether chain length. To achieve higher molecular weight polyether residues B, it may be necessary or beneficial to add one of the aforementioned catalysts at a later stage of the alkoxylation reaction. DMC catalysis
[0100] Zinc / cobalt DMC catalysts are preferably used, especially those containing zinc hexacyanocobaltate(III). The DMC catalysts described in US 5,158,922, US 20030119663, and WO 01 / 80994 are preferably used. The catalysts can be amorphous or crystalline.
[0101] It is preferred that the catalyst concentration is from >0 wppm to 1000 wppm, more preferably from >0 wppm to 700 wppm, most preferably from >10 wppm to 500 wppm based on the total mass of the resulting products.
[0102] Preferably, the catalyst is added only once to the reactor. The reactor should preferably be clean, dry, and free of basic impurities that could inhibit the DMC catalyst. The catalyst quantity should preferably be adjusted to ensure sufficient catalytic activity for the process. The catalyst can be added as a solid or in the form of a catalyst suspension. If a suspension is used, the initiator is particularly suitable as a suspending agent.
[0103] To initiate the DMC-catalyzed reaction, it may be advantageous to first activate the catalyst with a portion of the at least one epoxy-functional compound (F), preferably selected from the group of alkylene oxides, in particular with propylene oxide and / or ethylene oxide. Once the alkoxylation reaction has begun, continuous monomer addition can begin.
[0104] The reaction temperature in the case of a DMC-catalyzed reaction in step c) is preferably from 60 °C to 200 °C, more preferably from 90 °C to 160 °C and most preferably from 100 °C to 140 °C.
[0105] The internal pressure of the reactor in the case of a DMC-catalyzed reaction in step c) is preferably from 0.02 bar to 100 bar, more preferably from 0.05 bar to 20 bar, most preferably from 0.1 bar to 10 bar (absolute).
[0106] Most preferably, a DMC-catalyzed reaction in step c) is carried out at a temperature of 100 °C to 140 °C and a pressure of 0.1 bar to 10 bar.
[0107] The reaction can be carried out in a suitable solvent, for example, to reduce the viscosity. After the epoxide addition is complete, a post-reaction preferably follows to complete the conversion. The post-reaction can be carried out, for example, by continuing the reaction under reaction conditions (i.e., maintaining the temperature, for example) without adding reactants. The DMC catalyst usually remains in the reaction mixture.
[0108] Unreacted epoxides and any other volatile components can be removed after the reaction by vacuum distillation, steam or gas stripping, or other deodorization methods. The finished product is then filtered at <100 °C to remove any turbidity. Basic catalysis
[0109] As an alternative to the DMC catalysts, basic catalysts can also be used in step c). Particularly suitable are alkali metal alkoxides such as sodium methoxide and potassium methoxide, which are added as solids or in the form of their methanolic solutions. Furthermore, all alkali metal hydroxides, in particular sodium hydroxide and / or potassium hydroxide, can be used, both as solids and, for example, as aqueous or alcoholic solutions. Furthermore, basic nitrogen compounds, preferably amines, guanidines, and amidines, most preferably tertiary amines such as trimethylamine and triethylamine, can also be used according to the invention.
[0110] It is preferred to use the basic catalysts in a concentration of >0 mol% to 100 mol%, more preferably from >0 mol% to 50 mol%, most preferably from 3 mol% to 40 mol%, based on the sum of the OH and NH groups of the starter.
[0111] The reaction temperature in the case of a base-catalyzed reaction in step c) is preferably from 80 °C to 200 °C, more preferably from 90 °C to 160 °C and most preferably from 100 °C to 160 °C.
[0112] The internal pressure of the reactor in the case of a base-catalyzed reaction in step c) is preferably from 0.2 bar to 100 bar, more preferably from 0.5 bar to 20 bar, most preferably from 1 bar to 10 bar (absolute).
[0113] Most preferably, the base-catalyzed reaction in step c) is carried out at a temperature of 100 °C to 160 °C and a pressure of 1 bar to 10 bar.
[0114] The reaction can optionally be carried out in a suitable solvent. After the epoxide addition, a post-reaction preferably follows to complete the reaction. The post-reaction can be carried out, for example, by continuing the reaction under reaction conditions without the addition of reactants. Unreacted epoxides and any other volatile components can be removed after the reaction by vacuum distillation, steam or gas stripping, or other deodorization methods. Volatile catalysts, such as volatile amines, are removed in the process.
[0115] To neutralize the basic crude products, acids such as phosphoric acid or sulfuric acid, or carboxylic acids such as acetic acid and lactic acid, are added. Aqueous phosphoric acid and lactic acid are preferred. The amount of each acid used depends on the amount of basic catalyst previously used. The basic polybutadiene with pendant polyether radicals is stirred in the presence of the acid, preferably at 40 °C to 95 °C, and then dry-distilled in a vacuum distillation at <100 mbar and 80 °C to 130 °C. The neutralized product is then filtered, preferably at <100 °C, to remove precipitated salts.
[0116] It is preferred that the end products according to the invention have a water content of <0.2% (expressed as mass fraction based on the total mass of the end product) and an acid number of <0.5 mg KOH / g and are practically phosphate-free. Products as starters
[0117] It is not always possible to achieve the desired molar mass of the final product in a single reaction step, especially the alkoxylation step. Particularly when long polyether side chains are desired and / or the initiator from step b), i.e., the at least one hydroxy- and amino-functional polybutadiene (E), has a high functionality of OH and NH groups, large amounts of epoxy monomers must be added. The reactor geometry sometimes does not permit this. The polyether-modified amino-functional polybutadienes (G) prepared according to the invention from step c) each bear an OH group at the end of their pendant polyether radicals and are therefore suitable as initiators for the synthesis of higher molecular weight subsequent products. Within the meaning of the invention, they represent precursors and starting compounds for the synthesis of polybutadienes with longer polyether radicals.The reaction of the at least one epoxy-functional compound (F) in step c) can therefore be carried out in several sub-steps.
[0118] According to the invention, a product prepared by DMC catalysis according to step c) can be alkoxylated either by DMC catalysis or by using one of the aforementioned basic or acidic catalysts by further addition of epoxy monomers. Optionally, additional DMC catalyst can be added, for example, to increase the reaction rate during chain extension.
[0119] Likewise, a product from step c) prepared under base catalysis can be alkoxylated to higher molecular weights either under basic conditions, acidic conditions, or using DMC catalysis. Neutralization is advantageously omitted in step c) if the intention is to further react the basic precursor with monomers under base catalysis. Optionally, additional basic catalyst can be added, for example, to increase the reaction rate during chain extension. Optional step d)
[0120] In an optional further step d), the at least one polyether-modified aminofunctional polybutadiene (G) is reacted with at least one endcapping reagent (H) to form at least one polyether-modified aminofunctional polybutadiene (K) containing end-capped polyether radicals. The B radicals of the polyether-modified polybutadiene (G), which have terminal hydroxyl groups, are further reacted terminally to form ester, ether, urethane, and / or carbonate groups. The endcapping of polyethers is known to the person skilled in the art, for exampleesterification with carboxylic acids or carboxylic anhydrides, in particular acetylation with the aid of acetic anhydride, etherification with halogenated hydrocarbons, in particular methylation with methyl chloride according to the principle of Williamson ether synthesis, urethanization by reaction of the OH groups with isocyanates, in particular with monoisocyanates such as stearyl isocyanate, and carbonation by reaction with dimethyl carbonate and diethyl carbonate. Optional step e)
[0121] In an optional step e), the color of the at least one polyether-modified aminofunctional polybutadiene (G) or (K) is lightened. If the optional step e) follows the optional step d), the color of the at least one polyether-modified aminofunctional polybutadiene (K) containing end-capped polyether radicals is lightened. If, however, the optional step d) is omitted, the optional step e) follows step c) of the process according to the invention, and the color of the at least one polyether-modified aminofunctional polybutadiene (G) is lightened. The lightening can be achieved, for example, by the addition of activated carbon, preferably in a suitable solvent, or by treatment with hydrogen peroxide. Optional step f)
[0122] In an optional step f), at least some of the amino groups of the at least one polyether-modified amino-functional polybutadiene (G) or (K) are reacted with an acid or a quaternization reagent such as alkyl and benzyl halides, dimethyl sulfate, chloroacetic acid, or sodium chloroacetate to form quaternary ammonium groups. Step f) can be carried out either after step c) or after the optional step d) or after the optional step e). After quaternization, the products can be dissolved or dispersed, for example, in water or organic solvents. reactors
[0123] In principle, any suitable reactor type that allows the reaction and any heat of reaction to be controlled can be used for the process according to the invention. The reaction can be conducted continuously, semi-continuously, or batchwise in a manner known in process engineering and can be flexibly adapted to the existing production facilities. In addition to conventional stirred tank reactors, jet loop reactors with a gas phase and internal heat exchanger tubes, as described in WO 01 / 062826, can also be used. Gas-phase-free loop reactors can also be used. Polyether-modified aminofunctional polybutadienes
[0124] The present invention further relates to amino-functional polybutadienes modified with polyether residues in a comb-position (lateral, side-position) as can be prepared by the process according to the invention.
[0125] A further subject of the invention is therefore a polyether-modified amino-functional polybutadiene (G) or (K) obtainable by the process according to the invention.
[0126] Preferably, the polyether-modified aminofunctional polybutadiene (G) or (K) is a linear polybutadiene that is comb-modified (laterally, pendently) with polyether residues. It is therefore preferred that the polyether-modified aminofunctional polybutadiene (G) or (K) has a linear polybutadiene backbone and pendent polyether residues.
[0127] The invention also further relates to a polyether-modified amino-functional polybutadiene (G) or (K), which is preferably obtainable by the process according to the invention, characterized in that the polyether-modified amino-functional polybutadiene (G) or (K) contains repeating units selected from the group consisting of the divalent radicals includes; where A 1 and A 2 are each independently organic radicals, preferably having 1 to 22 carbon atoms, most preferably having 1 to 12 carbon atoms, where the radicals A 1 and A 2 may be covalently bonded to one another, B is each independently a radical of the formula (4a), preferably each independently of one another is a radical of the formula (4b), most preferably each independently of the other is a radical of formula (4c), R 1< is each independently of one another a monovalent hydrocarbon radical having 1 to 16 carbon atoms; preferably, each independently of one another, is an alkyl radical having 1 to 16 carbon atoms or a phenyl radical; most preferably, each independently of one another, is a methyl radical, an ethyl radical or a phenyl radical; R 2< is a radical of the formula -CH 2 -OR 3<; R 3< is each independently of one another a monovalent hydrocarbon radical having 3 to 18 carbon atoms; preferably, each independently of one another, is an allyl radical, a butyl radical, an alkyl radical having 8 to 15 carbon atoms or a phenyl radical which may be substituted by monovalent radicals selected from hydrocarbon radicals having 1 to 4 carbon atoms; most preferably, a tert-butylphenyl radical or an o-cresyl radical; R 4< is each independently of one another a monovalent organic radical having 1 to 18 carbon atoms or hydrogen, preferably hydrogen; and k1 and k2 are each independently integers from 0 to 8, preferably from 0 to 6, most preferably from 0 to 4; I1 and I2 are integers and are each independently either 0 or 1; m, n, o, p and q are each independently rational numbers from 0 to 300, preferably from 0 to 200, most preferably from 0 to 100, with the proviso that the sum of m, n, o, p and q is greater than 1, preferably greater than 5, most preferably greater than 10; the sum of all repeating units (U), (V) and (W) divided by the sum of all repeating units (U), (V), (W), (X), (Y) and (Z) is >0%; and any permutation of the repeating units (U), (V), (W), (X), (Y) and (Z) and of the repeating units in the radical B is included.
[0128] The radicals R 1< , R 2< , R 3< and R 4< can each independently be linear or branched, saturated or unsaturated, aliphatic or aromatic, substituted or unsubstituted.
[0129] The general spelling with R = R 1< or R 2< in formula (4a) or R = CH 3 in formulas (4b) and (4c) represents both a unit of the formula as well as one for a unit of the formula , but preferably for a unit of the formula
[0130] The general spelling in formula (4a) represents both a unit of the formula as well as one for a unit of the formula but preferably for a unit of the formula
[0131] It is further preferred that the radical R 4< is each independently selected from the group consisting of monovalent hydrocarbon radicals having 1 to 18 carbon atoms, acyl radicals -C(=O)R 5< , urethane radicals -C(=O)NH-R 6< , carbonate radicals -C(=O)OR 7< and hydrogen; more preferably, R 4< is each independently selected from the group consisting of alkyl radicals having 1 to 18 carbon atoms, alkylene radicals having 1 to 18 carbon atoms, acyl radicals -C(=O)R 5< , urethane radicals -C(=O)NH-R 6< , carbonate radicals -C(=O)OR 7< and hydrogen; most preferably, R 4< is hydrogen; where the term "hydrogen" is intended to represent a hydrogen radical / a hydrogen radical.
[0132] R 5< is each independently an alkyl or alkenyl radical having 1 to 18 carbon atoms, preferably having 1 to 10 carbon atoms, most preferably a methyl radical.
[0133] R 6< is each independently an alkyl or aryl radical having 1 to 18 carbon atoms, preferably having 6 to 18 carbon atoms.
[0134] R 7< is each independently an alkyl radical having 1 to 18 carbon atoms, preferably having 1 to 2 carbon atoms.
[0135] According to the invention, the sum (the total number) of all repeating units (U), (V) and (W) divided by the sum (the total number) of all repeating units (U), (V), (W), (X), (Y) and (Z) of the at least one polyether-modified amino-functional polybutadiene (G) or (K) is >0%, i.e. from >0% to 100%.
[0136] Conversely, this means that the sum (the total number) of all repeating units (X), (Y) and (Z) divided by the sum (the total number) of all repeating units (U), (V), (W), (X), (Y) and (Z) of the at least one polyether-modified amino-functional polybutadiene (G) or (K) is <100% (i.e. <100% to 0%).
[0137] This means that >0% (i.e. from >0% to 100%) of the total repeat units (U), (V), (W), (X), (Y) and (Z) are polyether modified.
[0138] This also means that <100% (i.e. from <100% to 0%) of the total repeat units (U), (V), (W), (X), (Y) and (Z) are not polyether modified.
[0139] This further means that the polyether-modified amino-functional polybutadiene (G) or (K) comprises at least one repeating unit selected from the group consisting of (U), (V) and (W).
[0140] It is preferred that the sum (the total number) of all repeating units (U), (V) and (W) divided by the sum (the total number) of all repeating units (U), (V), (W), (X), (Y) and (Z) of the at least one polyether-modified amino-functional polybutadiene (G) or (K) is preferably from >0% to <100%, more preferably from >0% to 70%, more preferably from 1% to 50%, more preferably from 2% to 40%, more preferably from 3% to 30%, most preferably from 4% to 20%.
[0141] This means that preferably from >0% to <100%, more preferably from >0% to 70%, more preferably from 1% to 50%, more preferably from 2% to 40%, more preferably from 3% to 30%, most preferably from 4% to 20% of the total of the repeat units (U), (V), (W), (X), (Y) and (Z) are polyether-modified.
[0142] It is further preferred that the sum (the total number) of all repeating units (X), (Y) and (Z) divided by the sum (the total number) of all repeating units (U), (V), (W), (X), (Y) and (Z) of the at least one polyether-modified amino-functional polybutadiene (G) or (K) is from <100% to >0%, more preferably from <100% to 30%, even more preferably from 99% to 50%, even more preferably from 98% to 60%, even more preferably from 97% to 70%, most preferably from 96% to 80%.
[0143] This means that preferably from <100% to >0%, more preferably from <100% to 30%, even more preferably from 99% to 50%, even more preferably from 98% to 60%, even more preferably from 97% to 70%, most preferably from 96% to 80% of the total of the repeat units (U), (V), (W), (X), (Y) and (Z) are not polyether modified.
[0144] It is preferred that the mass fraction of all repeat units (U), (V), (W), (X), (Y) and (Z) taken together, based on the total mass of the polyether-modified amino-functional polybutadiene (G) or (K), is at least 80%, more preferably at least 90%, even more preferably at least 99%, most preferably 100%.
[0145] It is preferred that the polyether-modified amino-functional polybutadiene (G) or (K) consists essentially or entirely of the repeating units (U), (V), (W), (X), (Y) and (Z).
[0146] It is preferred that the polyether-modified amino-functional polybutadiene (G) or (K) is a polybutadiene of formula (5) equipped with pendant polyether radicals, wherein the proportion of the polyether-modified repeating units listed in formula (5) based on the sum of all repeating units listed in formula (5) is >0% (i.e. from >0% to 100%), more preferably from >0% to <100%, even more preferably from >0% to 70%, even more preferably from 1% to 50%, even more preferably from 2% to 40%, even more preferably from 3% to 30%, most preferably from 4% to 20%, the proportion being calculated according to [(d+e+f) / (a+b+c+d+e+f)] * 100%.
[0147] This means that the proportion of the non-polyether-modified repeating units listed in formula (5) based on the sum of all repeating units listed in formula (5) is <100% (i.e. from <100% to 0%), preferably from <100% to >0%, more preferably from <100% to 30%, even more preferably from 99% to 50%, even more preferably from 98% to 60%, even more preferably from 97% to 70%, most preferably from 96% to 80%, where the proportion is calculated according to [(a+b+c) / (a+b+c+d+e+f)] * 100%.
[0148] The repeating units with indices a, b, c, d, e, and f are randomly distributed throughout the polybutadiene chain. All index values given are therefore to be understood as averages.
[0149] It is preferred that the mass fraction of all repeating units with the indices a, b, c, d, e and f taken together, based on the total mass of the polyether-modified amino-functional polybutadiene (G) or (K), is at least 80%, more preferably at least 90%, even more preferably at least 99%, most preferably 100%.
[0150] It is preferred that the polyether-modified amino-functional polybutadiene (G) or (K) consists essentially or entirely of the repeating units with the indices a, b, c, d, e and f.
[0151] It is further preferred that the polyether-modified amino-functional polybutadienes (G) or (K) are characterized in that 0% to 80%, more preferably 0% to 30%, even more preferably 0% to 10% and most preferably 0% to 5% of the double bonds present are 1,2-vinyl double bonds and 20% to 100%, more preferably 70% to 100%, even more preferably 90% to 100% and most preferably 95% to 100% of the double bonds present are 1,4-double bonds.
[0152] Preferred within the meaning of the invention are therefore compounds of the formula (5) with a content of 0% to 80% 1,2-vinyl double bonds (index a) and 20% to 100% 1,4-double bonds (sum of indices b and c), more preferably with 0% to 30% 1,2-vinyl double bonds and 70% to 100% 1,4-double bonds, even more preferably with 0% to 10% 1,2-vinyl double bonds and 90% to 100% 1,4-double bonds and most preferably 0% to 5% 1,2-vinyl double bonds and 95% to 100% 1,4-double bonds, based on the total number of repeating units containing double bonds (sum of a + b + c). The ratio of 1,4- trans -double bonds (index b) and 1,4- cis -double bonds (index c) is arbitrary.
[0153] Most preferred are compounds of formula (5) with a content of >95% of repeating units with index d based on the sum of the repeating units d + e + f. The ratio of the repeating units e and f to each other is arbitrary.
[0154] The number-average molar mass M n , weight-average molar mass M w and polydispersity of the polybutadiene moiety of the polyether-modified amino-functional polybutadiene (G) or (K) are arbitrary. The polybutadiene moiety is understood to mean the part of the polyether-modified amino-functional polybutadiene (G) or (K) that originates from the polybutadiene (A) used in the process. In formula (5), the polybutadiene moiety of the polyether-modified amino-functional polybutadiene (G) or (K) is understood to mean the part of the polymer that results from the polyether-modified amino-functional polybutadiene (G) or (K) less the radicals [B] k1 (A 1 ) l1 -N-(A 2 ) l2 -[B] k2 and BO. This also applies accordingly to the above-mentioned polyether-modified amino-functional polybutadiene (G) or (K) comprising repeating units selected from the group consisting of the divalent repeating units (U), (V), (W), (X), (Y) and (Z).
[0155] It is preferred that the number-average molar mass M n of the polybutadiene part of the polyether-modified polybutadiene (G) or (K) is from 200 g / mol to 20,000 g / mol, more preferably from 500 g / mol to 10,000 g / mol, most preferably from 700 g / mol to 5,000 g / mol.
[0156] Alternatively, it is preferred that the number-average molar mass M n of the polybutadiene part of the polyether-modified polybutadiene (G) or (K) is from 2100 g / mol to 20000 g / mol, more preferably from 2200 g / mol to 10000 g / mol, most preferably from 2300 g / mol to 5000 g / mol.
[0157] The number-average molar mass M n of the polybutadiene part is defined as the number-average molar mass M n of the underlying polybutadiene (A).
[0158] It is further preferred that the polyether-modified amino-functional polybutadiene (G) or (K) has a number average of 5 to 360, preferably 10 to 180, most preferably 15 to 90 repeating units, wherein the repeating units are selected from the group consisting of (U), (V), (W), (X), (Y) and (Z).
[0159] Alternatively, it is preferred that the polyether-modified amino-functional polybutadiene (G) or (K) has a number average of 35 to 360, preferably 40 to 180, most preferably 45 to 90 repeating units, wherein the repeating units are selected from the group consisting of (U), (V), (W), (X), (Y) and (Z).
[0160] Most preferred are those polyether-modified amino-functional polybutadienes (G) and (K) which are derived from the above-described polybutadienes (A) Polyvest ®< 110 and Polyvest ®< 130 from Evonik Industries AG / Evonik Operations GmbH as well as Lithene ultra AL and Lithene ActiV 50 from Synthomer PLC.
[0161] The molar mass and polydispersity of the B residues are arbitrary. However, it is preferred that the average molar mass of the B residues be from 30 g / mol to 20,000 g / mol, more preferably from 50 g / mol to 10,000 g / mol, even more preferably from 100 g / mol to 5,000 g / mol, and most preferably from 150 g / mol to 1,000 g / mol. The average molar mass of the B residues can be calculated from the initial weight of the monomers used, based on the number of OH and NH groups in the hydroxy- and amino-functional polybutadiene (E) used. Thus, for example, if 40 g of ethylene oxide are used and the total amount of all OH and NH groups in the hydroxy- and amino-functional polybutadiene (E) used together is 0.05 mol, the average molar mass of the B residue is 800 g / mol.
[0162] The polyether-modified amino-functional polybutadienes (G) and (K) are liquid, pasty or solid depending on their composition and molecular weight.
[0163] The number-average molar mass (M n ) of the polyether-modified amino-functional polybutadienes (G) or (K) is preferably from 1000 g / mol to 50000 g / mol, more preferably from 1500 g / mol to 40000 g / mol, even more preferably from 2000 g / mol to 30000 g / mol, most preferably from 3000 g / mol to 10000 g / mol.
[0164] Their polydispersity (M w / M n ) is variable within wide ranges. The polydispersity of the at least one polyether-modified polybutadiene (G) or (K) is preferably from 1.5 to 10, more preferably from 2 to 8, most preferably from 3 to 5.
[0165] In the examples listed below, the present invention is described by way of example, without the invention, the scope of which emerges from the entire description and the claims, being intended to be limited to the embodiments mentioned in the examples. Examples: General methods: Gel permeation chromatography (GPC):
[0166] GPC measurements to determine the polydispersity (M w / M n ), the weight-average molecular weight (M w ), and the number-average molecular weight (M n ) of the epoxy-functional polybutadienes (C) were performed under the following measurement conditions: column combination SDV 1000 / 10000 Å (length 65 cm), temperature 30 °C, THF as mobile phase, flow rate 1 ml / min, sample concentration 10 g / L, RI detector, and analysis against a polypropylene glycol standard. GPC measurements to determine the polydispersity (M w / M n ), the weight-average molecular weight (M w ), and the number-average molecular weight (M n ) of the polybutadienes (A) can be performed in the same way.
[0167] GPC measurements to determine the polydispersity (M w / M n ), the weight-average molar mass (M w ), and the number-average molar mass (M n ) of the polyether-modified amino-functional polybutadienes (G) according to the invention were carried out under the following measurement conditions: Jordi DVB 500 Å column combination (length 30 cm), Jordi DVB mixed bed (length 30 cm), temperature 30 °C, THF / triethylamine as mobile phase, flow rate 0.4 ml / min, sample concentration 3 g / L, RI detector, and analysis against a polystyrene standard. The GPC measurements to determine the polydispersity (M w / M n ), the weight-average molar mass (M w ), and the number-average molar mass (M n ) of the end-capped polyether-modified amino-functional polybutadienes (K) can be carried out in the same way. Determination of the content of 1,4-cis, 1,4-trans and 1,2-units in polybutadiene:
[0168] The content of 1,4-cis, 1,4-trans, and 1,2-units can be determined using 1< H NMR spectroscopy. This method is familiar to those skilled in the art. Determination of the content of epoxy groups in epoxy-functional polybutadiene (C) (epoxide content, degree of epoxidation):
[0169] The epoxy group content was determined using 13< C NMR spectroscopy. A Bruker Avance 400 NMR spectrometer was used. The samples were dissolved in deuterochloroform. The epoxy content is defined as the proportion of epoxidized butadiene units in mol% relative to the total number of repeat units contained in the sample. This corresponds to the number of epoxy groups in the epoxy-functional polybutadiene (C) divided by the number of double bonds in the polybutadiene used (A). Determination of the acid number:
[0170] The acid number determination was carried out using a titration method based on DIN EN ISO 2114. Synthesis examples: Step a), Production of epoxidized polybutadienes Example A1:
[0171] To produce an epoxidized polybutadiene, a polybutadiene of formula (1) with the structure x=1%, y=24%, and z=75% was used (Polyvest ®< 110). According to the state of the art, 1500 g of Polyvest ®< 110 and 146.3 g of concentrated formic acid in 1500 g of chloroform were placed at room temperature in a 5-liter reactor under a nitrogen atmosphere. Subsequently, 540 g of 30% H 2 O 2 solution (30 wt.% H 2 O 2 based on the total mass of the aqueous solution) were slowly added dropwise, and the solution was heated to 50 °C for 7 hours. After the reaction, the mixture was cooled to room temperature, the organic phase was separated, and washed four times with distilled H 2 O. Excess chloroform and residual water were distilled off. A total of 1481 g of product was obtained, which was treated with 1000 ppm of Irganox ®< 1135 and stored under nitrogen. Analysis by 13< C NMR revealed a degree of epoxidation of approximately 15.8% of the double bonds.The analysis by GPC showed: M w =4690 g / mol; M n =1982 g / mol; M w / M n = 2.4. Step b), Production of aminofunctional polybutadienes Example B1:
[0172] The epoxidized polybutadiene prepared in Example A1 was used to produce an amino-functional polybutadiene with a degree of amination of approximately 15.8%. The degree of amination is the number of amino groups in the amino-functional polybutadiene divided by the number of double bonds in the polybutadiene used in step a). For the preparation, 800 g of the epoxidized polybutadiene were placed in a 1-liter four-necked flask under a nitrogen atmosphere with 136.3 g of ethanolamine and 6.8 g of lithium bromide and heated to 180°C with stirring. The mixture was stirred at this temperature for 15 hours. The viscosity increased during the reaction. After the reaction was complete, volatile components were removed by distillation at 180°C and 20 mbar. The product was cooled to 60°C. 908 g of a yellowish product were obtained and stored under nitrogen.The evaluation by 13< C-NMR showed complete conversion of all epoxide groups, resulting in a degree of amination of approximately 15.8%. Step c), Alkoxylation of aminofunctional polybutadienes Example C1:
[0173] 151 g of the hydroxy- and amino-functional polybutadiene prepared in Example B1 were placed in a 1.5-liter autoclave under nitrogen and heated to 115 °C with stirring. The reactor was evacuated to an internal pressure of 30 mbar to remove any volatile components by distillation. 15.9 g of ethylene oxide were added over 5 minutes at 115 °C. The internal reactor pressure rose to a maximum of 3.4 bar (absolute) and decreased continuously over the course of the reaction. After 5.5 hours, a constant pressure of 0.6 bar (absolute) was reached. At 115 °C and 20 mbar, volatile components were removed, the reactor was depressurized to atmospheric pressure with N2, and the reaction mixture was cooled to 40 °C. Subsequently, 26.9 g of 30% sodium methoxide solution (30 wt.% sodium methoxide in methanol based on the total mass of the solution) were added, the reactor contents were inerted with nitrogen and heated to 115 °C while stirring.The internal reactor pressure was reduced to 20 mbar, and methanol was removed by distillation. 164.7 g of ethylene oxide were added at 115 °C over 1.5 h with stirring and cooling at a maximum internal pressure of 3.4 bar. During the post-reaction of 3 h at 115 °C, the internal pressure fell continuously until constant pressure reached 0.5 bar (absolute). Volatile components, such as residual ethylene oxide, were distilled off under vacuum. The product was cooled to below 80 °C, neutralized with 14.9 g of 90% lactic acid (90 wt.% lactic acid in water based on the total mass of the solution) to an acid number of 0.1 mg KOH / g, mixed with 1000 ppm of Irganox ®< 1135, and drained. 317 g of a viscous, orange-red, slightly cloudy polyether-modified aminofunctional polybutadiene were drained and stored under nitrogen. The total amount of ethylene oxide corresponded to an average of 3.8 ethylene oxide units per reactive NH / OH group. GPC analysis showed M w = 19.484 g / mol; M n = 4474 g / mol; M w / M n = 3.45. Example C2:
[0174] 181 g of the aminated polybutadiene prepared in Example B1 were placed in a 1.5-liter autoclave under nitrogen and heated to 115 °C with stirring. The reactor was evacuated to an internal pressure of 30 mbar to remove any volatile components by distillation. 25.2 g of propylene oxide were added over 5 minutes at 115 °C. The internal reactor pressure rose to a maximum of 2.4 bar (absolute) and decreased continuously over the course of the reaction. After 4.5 hours, a constant pressure of 0.7 bar (absolute) was reached. At 115 °C and 20 mbar, volatile components were removed, the reactor was depressurized to atmospheric pressure with N2, and the reaction mixture was cooled to 40 °C. Subsequently, 32.2 g of 30% sodium methoxide solution (30 wt.% sodium methoxide in methanol based on the total mass of the solution) were added, the reactor contents were inerted with nitrogen and heated to 115 °C while stirring.The internal reactor pressure was reduced to 20 mbar, and methanol was removed by distillation. 260 g of propylene oxide were added at 115 °C over 1.5 h with stirring and cooling at a maximum internal pressure of 2.9 bar. During the post-reaction of 2 h at 115 °C, the internal pressure fell continuously until constant pressure reached 0.3 bar (absolute). Volatile components, such as residual propylene oxide, were distilled off under vacuum. The product was cooled to below 80 °C, neutralized with 17.9 g of 90% lactic acid (90 wt.% lactic acid in water based on the total mass of the solution) to an acid number of 0.1 mg KOH / g, mixed with 1000 ppm of Irganox ®< 1135, and drained. 421 g of a viscous, orange, slightly cloudy polyether-modified aminofunctional polybutadiene were drained and stored under nitrogen. The total amount of propylene oxide corresponded to an average of 3.8 propylene oxide units per reactive NH / OH group. GPC analysis showed M w = 25.386 g / mol; M n = 5226 g / mol; M w / M n = 4.86. Example C3: (Stoichiometry: 5 EO / 5 PO per reactive NH / OH group)
[0175] 197 g of the aminated polybutadiene prepared in Example B1 were placed in a 1.5-liter autoclave under nitrogen and heated to 115 °C with stirring. The reactor was evacuated to an internal pressure of 30 mbar to remove any volatile components by distillation. 27.4 g of propylene oxide were added over 5 minutes at 115 °C. The internal pressure in the reactor rose to a maximum of 2.3 bar (absolute) and decreased continuously over the course of the reaction. After 4 hours, a constant pressure of 0.7 bar (absolute) was reached. At 115 °C and 20 mbar, volatile components were removed, the reactor was depressurized to atmospheric pressure with N2, and the reaction mixture was cooled to 40 °C. Subsequently, 17.6 g of 30% sodium methoxide solution (30 wt.% sodium methoxide in methanol based on the total mass of the solution) were added, the reactor contents were inerted with nitrogen and heated to 115 °C while stirring.The internal reactor pressure was reduced to 20 mbar, and methanol was removed by distillation. A mixture of 382 g of propylene oxide and 310 g of ethylene oxide was added at 115 °C over 6 h with stirring and cooling at a maximum internal pressure of 3.2 bar. During the post-reaction of 2.5 h at 115 °C, the internal pressure fell continuously until constant pressure reached 0.4 bar (absolute). Volatile components such as residual propylene oxide and ethylene oxide were distilled off under vacuum. The product was cooled to below 80 °C, neutralized with 30% phosphoric acid (30 wt.% phosphoric acid in water based on the total mass of the solution) to an acid number of 0.1 mg KOH / g, mixed with 500 ppm of Irganox ®< 1135, and drained through a filter. 881 g of a viscous, orange, clear polyether-modified aminofunctional polybutadiene was drained and stored under nitrogen.The total amount of ethylene oxide and propylene oxide corresponded to an average of 5 ethylene oxide units and 5 propylene oxide units per reactive NH / OH group. Analysis by GPC showed: M w = 32,145 g / mol; M n = 8,349 g / mol; M w / M n = 3.85.
Claims
1. Process for preparing one or more polyether-modified amino-functional polybutadienes, comprising the steps of: a) reacting at least one polybutadiene (A) with at least one epoxidizing reagent (B) to give at least one epoxy-functional polybutadiene (C); b) reacting the at least one epoxy-functional polybutadiene (C) with at least one amino-functional compound (D) to give at least one hydroxy- and amino-functional polybutadiene (E); c) reacting the at least one hydroxy- and amino-functional polybutadiene (E) with at least one epoxy-functional compound (F) to give at least one polyether-modified amino-functional polybutadiene (G).
2. Process according to Claim 1, further comprising at least one of the following steps of: d) reacting the at least one polyether-modified amino-functional polybutadiene (G) with at least one endcapping reagent (H) to give at least one polyether-modified amino-functional polybutadiene (K) containing end-capped polyether radicals; e) lightening the colour of the at least one polyether-modified amino-functional polybutadiene (G) or (K); f) converting at least some of the amino groups of the at least one polyether-modified amino-functional polybutadiene (G) or (K) to quaternary ammonium groups by means of an acid and / or a quaternizing reagent.
3. Process according to either of Claims 1 and 2, characterized in that, of the double bonds of all the polybutadienes (A) used, 0% to 80% are 1,2 vinyl double bonds and 20% to 100% are 1,4 double bonds, preferably 0% to 30% are 1,2 vinyl double bonds and 70% to 100% are 1,4 double bonds, more preferably 0% to 10% are 1,2 vinyl double bonds and 90% to 100% are 1,4 double bonds, most preferably 0% to 5% are 1,2 vinyl double bonds and 95% to 100% are 1,4 double bonds.
4. Process according to any of Claims 1 to 3, characterized in that the number-average molar mass Mn of the at least one polybutadiene (A) is from 200 g / mol to 20 000 g / mol, preferably from 500 g / mol to 10 000 g / mol, most preferably from 700 g / mol to 5000 g / mol, determined as specified in the description.
5. Process according to any of Claims 1 to 4, characterized in that from >0% to <100%, preferably from >0% to 70%, more preferably from 1% to 50%, even more preferably from 2% to 40%, even more preferably from 3% to 30% and most preferably from 4% to 20% of the double bonds of the at least one polybutadiene (A) are epoxidized.
6. Process according to any of Claims 1 to 5, characterized in that the at least one epoxidizing reagent (B) contains performic acid which is preferably formed in situ from formic acid and hydrogen peroxide.
7. Process according to any of Claims 1 to 6, characterized in that the at least one amino-functional compound (D) is selected from compounds having at least one primary and / or at least one secondary amino group; preferably from organic compounds having at least one primary and / or at least one secondary amino group; more preferably from organic compounds having 1 to 22 carbon atoms and at least one primary and / or at least one secondary amino group; even more preferably from organic compounds having 1 to 12 carbon atoms and at least one primary and / or at least one secondary amino group; most preferably from the group consisting of butylamine, isobutylamine, hexylamine, octylamine, 2-ethylhexylamine, decylamine, laurylamine, ethanolamine, isopropanolamine, diethanolamine, diisopropanolamine, N-methylethanolamine, N-methylisopropanolamine, 2-amino-2-methyl-1-propanol, 2-amino-2-ethyl-1,3-propanediol, tris(hydroxymethyl)aminomethane tris(hydroxymethyl)aminomethane (TRIS, 2-amino-2-(hydroxymethyl)propane-1,3-diol), morpholine, piperidine, cyclohexylamine, N,N-dimethylaminopropylamine (DMAPA) and benzylamine.
8. Process according to any of Claims 1 to 7, characterized in that, in step b), the total number of NH groups in all the amino-functional compounds (D) to the total number of epoxy groups in all the epoxy-functional polybutadienes (C) is from 0.8:1 to 20:1, more preferably from 0.9:1 to 10:1, even more preferably from 1:1 to 5:1, most preferably from 1:1 to 3:1.
9. Process according to any of Claims 1 to 8, characterized in that a catalyst is used in step b), preferably selected from the group consisting of Lewis acids and Bronsted acids; more preferably from the group consisting of water, phenols, alcohols, carboxylic acids, ammonium compounds, phosphonium compounds and lithium bromide; even more preferably from the group consisting of carboxylic acids, phenols, ammonium compounds, phosphonium compounds and lithium bromide, even more preferably from the group consisting of carboxylic acids, phenol and lithium bromide, most preferably lithium bromide.
10. Process according to any of Claims 1 to 9, characterized in that the at least one epoxy-functional compound used in step c) is selected a. from the group of the alkylene oxides having 2 to 18 carbon atoms, preferably from the group of the alkylene oxides having 2 to 8 carbon atoms, most preferably selected from the group consisting of ethylene oxide, propylene oxide, 1-butylene oxide, cis-2-butylene oxide, trans-2-butylene oxide, isobutylene oxide and styrene oxide, and / or b. from the group of the glycidyl compounds, preferably from the group of the monofunctional glycidyl compounds, most preferably from the group consisting of phenyl glycidyl ether, o-cresyl glycidyl ether, tert-butylphenyl glycidyl ether, allyl glycidyl ether, butyl glycidyl ether, 2-ethylhexyl glycidyl ether, C12 / C14 fatty alcohol glycidyl ether and C13 / C15 fatty alcohol glycidyl ether.
11. Process according to any of Claims 1 to 10, characterized in that an alkoxylation catalyst is used in step c); preferably selected from the group consisting of alkali metal hydroxides, alkali metal alkoxides, amines, guanidines, amidines, phosphines, SnCl4, SnCl2, SnF2, BF3, BF3 complexes and double metal cyanide (DMC) catalysts; more preferably selected from the group consisting of Zn / Co double metal cyanide catalysts, amines, guanidines, amidines, alkali metal hydroxides and alkali metal alkoxides; most preferably selected from the group consisting of alkali metal alkoxides.
12. Polyether-modified amino-functional polybutadiene (G) or (K) obtainable by a process according to any of Claims 1 to 11.
13. Polyether-modified amino-functional polybutadiene (G) or (K), preferably according to Claim 12, characterized in that the polyether-modified amino-functional polybutadiene (G) or (K) comprises repeating units selected from the group consisting of the divalent radicals where A1 and A2 are in each case independently organic radicals, preferably having 1 to 22 carbon atoms, most preferably having 1 to 12 carbon atoms, where the radicals A1 and A2 may be covalently bonded to each other, B is in each case independently a radical of the formula (4a), preferably is in each case independently a radical of the formula (4b), most preferably is in each case independently a radical of the formula (4c), R1 is in each case independently a monovalent hydrocarbon radical having 1 to 16 carbon atoms; preferably is in each case independently an alkyl radical having 1 to 16 carbon atoms or a phenyl radical; most preferably is in each case independently a methyl radical, an ethyl radical or a phenyl radical; R2 is a radical of the formula -CH2-O-R3; R3 is in each case independently a monovalent hydrocarbon radical having 3 to 18 carbon atoms; preferably is in each case independently an allyl radical, a butyl radical, an alkyl radical having 8 to 15 carbon atoms or a phenyl radical that may be substituted by monovalent radicals selected from hydrocarbon radicals having 1 to 4 carbon atoms; most preferably is a tert-butylphenyl radical or an o-cresyl radical; R4 is in each case independently a monovalent organic radical having 1 to 18 carbon atoms or hydrogen, preferably hydrogen; and k1 and k2 are in each case independently integers from 0 to 8, preferably from 0 to 6, most preferably from 0 to 4; 11 and 12 are integers and in each case independently either 0 or 1; m, n, o, p and q are in each case independently rational numbers from 0 to 300, preferably from 0 to 200, most preferably from 0 to 100, with the proviso that the sum total of m, n, o, p and q is greater than 1, preferably greater than 5, most preferably greater than 10; the sum total of all repeating units (U), (V) and (W) divided by the sum total of all repeating units (U), (V), (W), (X), (Y) and (Z) is >0%; including every permutation of the repeating units (U), (V), (W), (X), (Y) and (Z) and of the repeating units in the radical B.
14. Polyether-modified amino-functional polybutadiene (G) or (K) according to Claim 12 or 13, characterized in that the sum total of all repeating units (U), (V) and (W) divided by the sum total of all repeating units (U), (V), (W), (X), (Y) and (Z) is from >0% to <100%, preferably from >0% to 70%, more preferably from 1% to 50%, even more preferably from 2% to 40%, even more preferably from 3% to 30%, most preferably from 4% to 20%.
15. Polyether-modified polybutadiene (G) or (K) according to at least one of Claims 12 to 14, characterized in that the polybutadiene is of the formula (5) where the proportion of the polyether-modified repeating units shown in formula (5), based on the sum total of all repeating units shown in formula (5), is >0%, preferably from >0% to <100%, more preferably from >0% to 70%, even more preferably from 1% to 50%, even more preferably from 2% to 40%, even more preferably from 3% to 30%, most preferably from 4% to 200, where the proportion is calculated as [(d+e+f) / (a+b+c+d+e+f)]*100%.
16. Polyether-modified amino-functional polybutadiene (G) or (K) according to at least one of Claims 12 to 15, characterized in that 0% to 80%, preferably 0% to 30%, more preferably 0% to 10%, most preferably 0% to 5% of the double bonds present are 1,2 vinyl double bonds, and 20% to 100%, preferably 70% to 100%, more preferably 90% to 100%, most preferably 95% to 100% of the double bonds present are 1,4 double bonds.
17. Polyether-modified amino-functional polybutadiene (G) or (K) according to any of Claims 12 to 16, characterized in that - the number-average molar mass (Mn) of the polybutadiene part is from 200 g / mol to 20 000 g / mol, preferably from 500 g / mol to 10 000 g / mol, most preferably from 700 g / mol to 5000 g / mol; and / or - the average molar mass of the radical B is from 30 g / mol to 20 000 g / mol, preferably from 50 g / mol to 10 000 g / mol, more preferably from 100 g / mol to 5000 g / mol, most preferably from 150 g / mol to 1000 g / mol; and / or - the number-average molar mass (Mn) of the polyether-modified amino-functional polybutadiene (G) or (K) is preferably from 1000 g / mol to 50 000 g / mol, more preferably from 1500 g / mol to 40 000 g / mol, even more preferably from 2000 g / mol to 30 000 g / mol, most preferably from 3000 g / mol to 10 000 g / mol, determined in each case as specified in the description.